Gas barrier coating agent, multilayer body, and method for producing the same
A gas barrier coating agent using a water-soluble polysaccharide and metal salt, cured with active energy rays, addresses the challenges of maintaining barrier properties and transparency under high humidity, enhancing packaging material performance.
Patent Information
- Application Number
- JP2024065761
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-04-15
- Publication Date
- 2024-11-08
AI Technical Summary
Existing packaging materials face challenges in maintaining gas barrier properties under high humidity conditions, transparency, and adhesion to substrates while using environmentally friendly raw materials, and they often require high-temperature treatments that reduce productivity.
A gas barrier coating agent comprising a water-soluble polysaccharide with an anionic hydrophilic group and ethylenically unsaturated double bond, combined with a metal salt having a similar ligand, is applied to substrates and cured using active energy rays, forming a laminate with improved barrier properties, adhesion, and transparency.
The coating agent achieves excellent gas barrier properties under high humidity, maintains substrate adhesion, and ensures transparency, making it suitable for use as a top coat in packaging materials without the need for high-temperature treatments.
Smart Images

Figure 2024159574000001 
Figure 2024159574000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a gas barrier coating agent and a laminate. [Background technology]
[0002] Packaging materials used for packaging foods, medicines, etc. are required to prevent deterioration of the contents. The deterioration of the contents is mainly caused by oxygen that permeates the packaging material or other gases that react with the contents. Therefore, packaging materials used for packaging foods, medicines, etc. are required to have a property that does not allow gases such as oxygen to permeate, that is, so-called gas barrier properties. In particular, in the case of food packaging, it is expected that extending the expiration date or best-before date will lead to a reduction in the large amount of waste generated from ordinary households and commercial facilities such as supermarkets and convenience stores (Non-Patent Document 1).
[0003] To impart barrier properties to packaging materials, it is effective to use metals such as aluminum or inorganic materials including alumina, silica, etc., in the barrier layer. Specifically, high gas barrier properties are ensured by forming a laminate with an aluminum foil laminated structure, or by forming an inorganic layer on a plastic film substrate by a vacuum process such as CVD or deposition. However, it is desirable to eliminate the process of laminating aluminum foil from the viewpoint of energy saving and recyclability, while a structure including an inorganic layer has problems such as resistance caused by defects such as cracks.
[0004] In response to these problems, gas barrier films made of flexible gas barrier polymers with relatively high gas barrier properties and laminates using these as substrate films have been proposed. Conventionally, polymers containing hydrogen-bonding groups in the molecule, such as poly(meth)acrylic acid, ethylene-vinyl alcohol copolymers, or mixtures of these, have been used as oxygen barrier polymers (Patent Documents 1 and 2). However, while gas barrier materials made of these polymers have very good oxygen barrier properties under dry conditions, they have problems in that their oxygen barrier properties are significantly reduced under high humidity conditions due to their hydrophilicity, and the films have poor resistance to water friction and hot water. Naturally, it is practically difficult to use such films with low water resistance as the outermost layer (top coat) of packaging materials.
[0005] In order to solve these problems, it is known that the polyvalent metal compound is contained in the substrate itself, or that a polycarboxylic acid polymer layer and a polyvalent metal compound-containing layer are adjacently laminated on the substrate, and a polyvalent metal salt of the polycarboxylic acid polymer is obtained by an interlayer reaction (Patent Documents 3 and 4). It has been shown that the gas barrier packaging material obtained in this way has high oxygen gas barrier properties even under high humidity. However, the gas barrier packaging materials described in Patent Documents 3 and 4 require heat treatment at 150°C or higher, immersion treatment in a crosslinking agent, or retort treatment, which reduces productivity. Furthermore, in order to achieve high barrier properties, it is necessary to form a layer containing a high concentration of polyvalent metal salt in an insoluble state, which causes a problem of reduced transparency.
[0006] In recent years, growing interest in environmental issues has led to active development of products that proactively utilize biomass raw materials and biodegradable materials, and it can be said that there is a very large social need for similar products in the field of packaging materials. As a gas barrier material with high hydrogen bonding properties derived from natural materials to replace poly(meth)acrylic acid and polyvinyl alcohol derived from petroleum raw materials, polysaccharides that have many hydrogen bonding groups and anionic hydrophilic groups in the molecule have been reported by subjecting cellulose raw materials, which exist in abundance in nature, to TEMPO oxidation treatment or sulfuric acid treatment (Patent Documents 5 and 6). Patent Document 6 In the paper, a water-soluble nanocellulose coating film is formed on an undercoat layer containing a metal salt in combination with a crosslinking agent or a layered inorganic compound to achieve a relatively high oxygen barrier property under high humidity conditions, but the barrier property is not sufficient and the transparency is low. Furthermore, modified cellulose is relatively expensive, and it is difficult to increase the solid content when solubilizing it due to issues with viscosity and storage stability, which results in low productivity during printing and coating.
[0007] As mentioned above, no oxygen barrier coating agent that uses environmentally friendly raw materials, has gas barrier properties and transparency under high humidity, has substrate adhesion, and also has sufficient water resistance and can be used as a top coat has yet been reported. [Prior art documents] [Non-patent literature]
[0008] [Non-Patent Document 1] Molding and Processing Vol. 34 No. 4 2022 [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 157830 / 1983 [Patent Document 2] Patent No. 3203287 [Patent Document 3] JP 2019-178130 A [Patent Document 4] JP 2003-171419 A [Patent Document 5] JP 2016-159576 A [Patent Document 6] JP 2021-113244 A Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention provides a gas barrier coating agent which, when applied to a substrate such as a general-purpose substrate such as a polyethylene terephthalate (PET) film, a polypropylene (OPP, CPP) film, or paper, can be cured by exposure to active energy rays such as ultraviolet light or an electron beam to produce a laminate which exhibits excellent gas barrier properties even under high humidity conditions and which also has transparency, water friction resistance, and adhesion to substrates. [Means for solving the problem]
[0011] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by a gas barrier coating agent for packaging materials, which comprises (A) a water-soluble polysaccharide, (B) a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond, and a molecular weight of 50 or more and less than 300, and (C) a metal salt having, as a ligand, a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond, and a molecular weight of 50 or more and less than 300, and thus completed the present invention.
[0012] That is, the present invention relates to a gas barrier coating agent comprising (A) a water-soluble polysaccharide, (B) a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond, and having a molecular weight of 50 or more and less than 300, and (C) a metal salt having, as a ligand, a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond, and having a molecular weight of 50 or more and less than 300.
[0013] The present invention also relates to the gas barrier coating agent, wherein the water-soluble polysaccharide (A) contains chitosan.
[0014] The present invention also relates to the gas barrier coating agent, wherein the central metal of the metal salt (C) contains at least one selected from the group consisting of zinc, calcium, magnesium, and aluminum.
[0015] The present invention also provides a gas barrier coating agent having a solid content of 100% by mass, which contains a water-soluble polysaccharide. The content of the class (A) is 20 to 70 mass %, The content of the compound (B) is 10 to 60 mass %, The content of the metal salt (C) is 10 to 70 mass%. The present invention relates to the gas barrier coating agent.
[0016] The present invention also relates to the gas barrier coating agent for use in packaging materials.
[0017] The present invention also relates to a laminate having a gas barrier layer formed on a substrate using the gas barrier coating agent for packaging materials.
[0018] The present invention also provides a method for producing a laminate, the method comprising the steps of applying a gas barrier coating agent to a substrate to obtain a coated product, and irradiating the coated product with ultraviolet light or electron beams to form a gas barrier layer on the substrate, the method comprising the steps of: The present invention relates to a method for producing a laminate, wherein the gas barrier coating agent is a gas barrier coating agent comprising: a water-soluble polysaccharide (A); a compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond, and having a molecular weight of 50 or more and less than 300; and a metal salt (C) having, as a ligand, a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond, and having a molecular weight of 50 or more and less than 300. Effect of the Invention
[0019] The present invention makes it possible to provide a gas barrier coating agent which, when applied to a substrate and cured by exposure to active energy rays such as ultraviolet light or electron beams, can produce a laminate which exhibits excellent gas barrier properties even under high humidity conditions and which also has transparency, water abrasion resistance, and adhesion to substrates, even when a general-purpose substrate such as a polyethylene terephthalate (PET) film, polypropylene (OPP, CPP) film, or paper is used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The following examples are provided to explain the embodiments of the present invention in detail. However, the following examples are merely examples or representative examples of the embodiments of the present invention, and the present invention is not limited to these examples as long as they do not depart from the gist of the present invention.
[0021] The gas barrier coating agent of the present invention is characterized by comprising a water-soluble polysaccharide (A), a compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond, and having a molecular weight of 50 or more and less than 300, and a metal salt (C) having, as a ligand, a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond, and having a molecular weight of 50 or more and less than 300, and can be suitably used for packaging material applications.
[0022] [Water-soluble polysaccharide (A)] Polysaccharides are a general term for substances in which a large number of monosaccharide molecules are polymerized in a chain shape through glycosidic bonds. The water-soluble polysaccharides used in the present invention refer to compounds that dissolve when mixed with water or hot water in any ratio, or that stably exhibit a colloidal or suspended state in water. As chain polysaccharides, linear polysaccharides or branched polysaccharides may be used, but linear polysaccharides are preferred from the viewpoints of water solubility and viscosity when made into an aqueous solution. Examples of the linear water-soluble polysaccharides include anionic water-soluble polysaccharides such as amylose, chitin, chitosan, agarose, agar, dextran, hyaluronic acid, chondroitin sulfate, starch, inulin, cellulose, tuberose polysaccharide, quince seed extract, gellan gum, sodium alginate, pectin, carboxymethylcellulose, sodium chondroitin sulfate, hyaluronic acid, and carrageenan; hydroxyethyl cellulose, hydroxypropyl cellulose, guar gum, agarose, pullulan, locust bean gum, galactan, gum arabic, tara gum, tamarind seed gum, and agar. Among the above, chitosan is particularly preferred from the viewpoints of coatability and barrier properties. is preferred.
[0023] Chitosan can be obtained by treating chitin, which is abundant in the shells of crustaceans such as shrimp and crabs, with a strong base to deacetylate the acetamide groups contained in the molecular structure of chitin and convert them to amino groups. Since it takes a lot of energy and cost to completely carry out this deacetylation process, most chitosans on the market generally contain acetamide residues, and the quality specifications state that the deacetylation rate is 70% or more or 80% or more. In the present invention, it is assumed that chitosan with a similar deacetylation rate will be used, but this is not limited to the case if there is a compounding composition that can obtain a sufficient cured coating film.
[0024] The water-soluble polysaccharides described above tend to exhibit excellent oxygen barrier properties because they have multiple hydrogen-bonding functional groups in the molecule, i.e., hydroxyl groups, carboxyl groups, amino groups, sulfo groups, etc. In addition, because they are high molecular weight substances, they are suitable as binder resins in that they can impart coating suitability, wettability to substrates, adhesion, and flexibility that does not crack even when bent.
[0025] [Compound having an anionic hydrophilic group and an ethylenically unsaturated double bond] The compound having an anionic hydrophilic group and an ethylenically unsaturated double bond used in the present invention includes a compound (B) having a molecular weight of 50 or more and less than 300. The anionic hydrophilic group refers to a functional group from which more than half of the hydrogen ions are dissociated in water at pH 7, and examples thereof include a carboxyl group, a sulfonic acid group, a phosphonic acid group, a phosphinic acid group, and a phosphoric acid group. All of these groups have hydrogen bonding properties, thereby complementing the oxygen barrier properties of the water-soluble polysaccharide. Furthermore, since the monomer contains an ethylenically unsaturated double bond, it is possible to improve the coating strength and water resistance by crosslinking with thermal polymerization, photopolymerization, electron beams, etc., and to suppress the decrease in oxygen barrier properties under high humidity. When the water-soluble polysaccharide has a cationic hydrophilic group, for example, chitosan is suitable because it is modified by an ionic bond with an anionic monomer and becomes a reactive binder.
[0026] The compound having an anionic hydrophilic group and an ethylenically unsaturated double bond used in the present invention has a molecular weight of 50 or more and less than 300, and from the viewpoint of molecular mobility and reactivity derived from steric hindrance, the molecular weight is preferably 50 or more and less than 200, and more preferably 50 or more and less than 120. In addition, from the viewpoint of radical polymerization reactivity, the compound having an ethylenically unsaturated double bond is most preferably a (meth)acrylate compound.
[0027] Specific examples of the compound (B) include acrylic acid, methacrylic acid, cinnamic acid, crotonic acid, senecioic acid, tiglic acid, sorbic acid, itaconic acid, maleic acid, angelic acid, aconitic acid, citraconic acid, mesaconic acid, 3-cyclopentene-1-carboxylic acid, 2-methyl-4-pentenoic acid, 2-amino-4-pentenoic acid, 2-hydroxy-3-butenoic acid, trans-2-pentenoic acid, trans-3-hexenedioic acid, sulfoalkyl (meth)acrylate, 2-acrylamido-2-methylpropanesulfonic acid, 2-methacryloyloxyethyl acid phosphate, vinylsulfonic acid, styrenesulfonic acid, vinylphosphonic acid, cinnamylphosphonic acid, etc., and acrylic acid and methacrylic acid are more preferred, and acrylic acid is particularly preferred in terms of characteristics such as gas barrier properties and cost. The above compounds can be used alone or in combination of two or more.
[0028] [Metal salts] The metal salt used in the present invention includes a metal salt (C) having as a ligand a compound having a molecular weight of 50 or more and less than 300, which has an anionic hydrophilic group and an ethylenically unsaturated double bond. Examples of the central metal of the metal salt (C) include divalent or higher polyvalent metals such as magnesium (Mg), calcium (Ca), barium (Ba), zinc (Zn), copper (Cu), cobalt (Co), nickel (Ni), aluminum (Al), and iron (Fe). Among the above, zinc, calcium, magnesium, and aluminum are preferred. Metal salts using divalent or higher metals include: By using the binder resin water-soluble polysaccharide and an anionic hydrophilic group and an ethylenically unsaturated double bond-containing compound at the same time, crosslinking by thermal polymerization, photopolymerization, electron beam, etc. is made denser and curing properties are improved. This suppresses the intrusion of water and water vapor into the coating film, improving water resistance and gas barrier properties under high humidity. The metal salt may be used alone or in combination of two or more types. In addition, the compound having an anionic hydrophilic group and an ethylenically unsaturated double bond as a ligand and a molecular weight of 50 or more and less than 300 is synonymous with the aforementioned compound (B), and the compound as a ligand of the metal salt (C) and the aforementioned compound (B) may be the same or different.
[0029] By forming a cured coating film (gas barrier layer) using a coating agent containing the above water-soluble polysaccharide (A), compound (B), and metal salt (C), it is possible to realize high levels of oxygen barrier properties, substrate adhesion, and water resistance. As for the content ratio of each component, the content ratio (mass%) of the water-soluble polysaccharide (A) is preferably 20 to 70 mass%, more preferably 30 to 60 mass%, in 100 mass% of the solid content of the gas barrier coating agent. The content ratio (mass%) of the compound (B) is preferably 10 to 60 mass%, more preferably 15 to 60 mass%, and even more preferably 20 to 50 mass%. The content ratio (mass%) of the metal salt (C) is preferably 10 to 70 mass%, more preferably 15 to 60 mass%, and even more preferably 20 to 50 mass%.
[0030] [solvent] The gas barrier coating agent of the present invention preferably contains a solvent. It is preferable to use water as the solvent to form an aqueous composition, but in order to improve the wettability of the substrate or to realize uniform dissolution or dispersion of each component, a small amount of an organic solvent (e.g., alcohols) may be added within a range that does not inhibit the polymerization reaction.
[0031] [Initiator] Since the gas barrier coating agent of the present invention has an ethylenically unsaturated double bond as a polymerizable group, a method of crosslinking by irradiation with ultraviolet light or electron beam to obtain a cured coating film is preferable. Electron beam irradiation is more preferable because it is possible to carry out a crosslinking reaction without using a polymerization initiator, but a polymerization initiator can be included as necessary. Representative examples of the polymerization initiator include a photopolymerization initiator and a thermal polymerization initiator. A photopolymerization initiator and a thermal polymerization initiator may be used in combination. The thermal polymerization initiator may be an azo compound or a peroxide that is activated by irradiation with ionizing radiation.
[0032] The polymerization reaction after applying the gas barrier coating agent to the substrate may be carried out after the solvent is sufficiently removed in an oven, or may be carried out in a wet state before drying. When the wet coating film is irradiated with ultraviolet light, it is preferable to include a photopolymerization initiator in the gas barrier coating agent. The photopolymerization initiator may be simply called a photoinitiator or a sensitizer. Examples of the photopolymerization initiator include acetophenones, benzophenones, Michler's ketones, benzils, benzoins, benzoin ethers, benzil dimethyl ketals, thioxanthones, and mixtures of two or more of these.
[0033] Preferable specific examples of the photopolymerization initiator include acetophenones such as acetophenone, 2,2-diethoxyacetophenone, m-chloroacetophenone, p-tert-butyltrichloroacetophenone, 4-dialkylacetophenone, and 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methylpropan-1-one; benzophenones; Benzophenones such as benzophenone; Michler's ketone such as Michler's ketone; benzils such as benzil and benzyl methyl ether; benzoins such as benzoin and 2-methylbenzoin Benzoins; Benzoin methyl ether, Benzoin ethyl ether, Benzoin isoprene Benzoin ethers such as benzoin propyl ether and benzoin butyl ether; Benzyl dimethyl ketals such as methyl ketal; thioxanes such as thioxanthone Tonnes; Propiophenone, Anthraquinone, Acetoin, Butyroin, Toluoin, Carbonyl compounds such as benzoyl benzoates, α-acyloxime esters; It is possible.
[0034] As a photopolymerization initiator, in addition to the above carbonyl compounds, tetramethylthiuram disulfide is also used. sulfur compounds such as thiuram disulfide, tetraethylthiuram disulfide, tetramethylthiuram monosulfide, thioxanthone, and 2-chlorothioxanthone; azobisisobutyronitrile Examples of suitable peroxides include azo compounds such as azoyl peroxide and azobis-2,4-dimethylvaleronitrile; and peroxides such as benzoyl peroxide and di-tert-butyl peroxide.
[0035] When these photopolymerization initiators are added to the gas barrier coating agent, they are usually added at a ratio of 0.001 to 10% by mass, preferably 0.01 to 5% by mass, based on the polymerizable compound containing the compound (B). Although it is not necessary to add a photopolymerization initiator, it is preferable to add a photopolymerization initiator in order to increase the polymerization efficiency when polymerization is performed by irradiation with ultraviolet light. When a hydrogen abstraction type photopolymerization initiator such as benzophenone is used, a part of the α,β-unsaturated carboxylic acid monomer is grafted to the plastic film used as the substrate, and the interlayer adhesion between the substrate and the ion-crosslinked polycarboxylic acid polymer film layer can be increased. Other general-purpose additives such as sensitizers and light stabilizers may be added together with the photopolymerization initiator.
[0036] When a wet coating film is heated to carry out thermal polymerization, the initiator dissociates thermally and acts as an initiator. It is preferable to use a thermal polymerization initiator that exerts a thermal polymerization effect. Examples of the thermal polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate; 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis[2-methyl-N-[1,1-bis(hydroxymethyl)ethyl]propionamide], 2,2'-azobis[2-methyl-N-[1,1-bis(hydroxymethyl)ethyl]propionamide], Azo polymerization initiators such as bis(4-methoxy-2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(methyl isobutyrate), 1,2'-azobis(N,N'-dimethyleneisobutylamidine) dihydrochloride, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide, 1,1'-azobis(cyclohexane-1-carbonitrile); hydroperoxides such as tert-alkyl hydroperoxides; di-tert-butyl peroxide, di Cumyl peroxide, lauroyl peroxide, benzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-hexyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, di-isopropyl peroxydicarbonate, di-tert-butyl peroxyisophthalate, 1,1',3,3'-tetramethylbutyl peroxy-2-ethylhexanoate, tert- Examples of the thermal polymerization initiator include peroxides such as butyl peroxybutyrate. When a thermal polymerization initiator is used, it is usually added at a ratio of 0.001 to 10% by mass, preferably 0.01 to 5% by mass, based on the solid content of the gas barrier coating agent.
[0037] [Sensitizer] In the gas barrier coating agent of the present invention, a sensitizer can be used in combination with the photopolymerization initiator. Examples of the sensitizer include amine-based sensitizers, anthracene-based sensitizers, and thioxanthone-based sensitizers. The sensitizers can be used alone or in combination of two or more kinds.
[0038] Examples of the amine sensitizer include trimethylamine, methyldimethanolamine, triethanolamine, p-diethylaminoacetophenone, ethyl p-dimethylaminobenzoate, isoamyl p-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, N,N-dimethylbenzylamine, and 4'-bis(diethylamino)benzophenone.
[0039] Examples of the anthracene sensitizer include 9,10-dibutoxyanthracene, 9,10-diethoxyanthracene, 9,10-dipropoxyanthracene, and 9,10-bis(2-ethylhexyloxy)anthracene.
[0040] Examples of thioxanthone sensitizers include 2,4-diethylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, etc. Representative examples of commercially available products include amine sensitizers such as EPA (manufactured by Nippon Kayaku Co., Ltd.), anthracene sensitizers such as DBA and DEA (manufactured by Kawasaki Kasei Chemical Industries, Ltd.), and thioxanthone sensitizers such as DETX and ITX (manufactured by Lambson Co., Ltd.). The sensitizer is preferably a thioxanthone sensitizer.
[0041] [Resin (D)] The gas barrier coating agent in the present invention may contain a non-polymerizable resin to the extent that the performance such as gas barrier property and water resistance is not impaired, and an aqueous resin is preferable. By containing a non-polymerizable resin in the gas barrier coating agent, the flexibility of the coating material, wettability to the substrate, and the curing shrinkage of the coating film occurring during curing are alleviated, thereby suppressing curling of the substrate, and further improving adhesion to the substrate. Examples of the resin include acrylic resin, epoxy resin, polyurethane resin, polyurethane urea resin, (modified) styrene maleic anhydride copolymer, (modified) vinyl chloride vinyl acetate copolymer, (modified) vinyl chloride vinyl acetate maleic anhydride copolymer, ketone aldehyde resin, polyester resin, polypropylene resin, polylactic acid resin, cellulose acetate resin, cellulose acetate butyrate resin, esterified cellulose resin, butyral resin, etc. These resins can be used alone or in combination of two or more kinds.
[0042] [Crosslinker (E)] The gas barrier coating agent in the present invention may use a water-soluble or water-dispersible crosslinking agent for the purpose of improving gas barrier properties and water resistance under high humidity, and a crosslinking agent capable of reacting with functional groups such as hydroxyl groups, carboxyl groups, and amino groups in the molecules of compounds contained in the gas barrier coating agent is preferable. Typical examples of crosslinking agents capable of reacting with the functional groups include compounds having an isocyanate group, an epoxy group, a carbodiimide group, an oxazoline group, and the like, and metal chelates such as titanium and zirconium may also be used. These may be used alone or in combination of two or more.
[0043] Specific examples of the crosslinking agent (E) include water-dispersible isocyanates Duranate WB40-100 and Duranate WT20-100 manufactured by Asahi Kasei Corporation, water-soluble polyfunctional epoxy compounds Denacol EX-313 and Denacol EX-321 manufactured by Nagase ChemteX Corporation, carbodiimide compounds Carbodilite E-02 and Carbodilite E-05 manufactured by Nisshinbo Inc., oxazoline compounds WS-500 and K2020E manufactured by Nippon Shokubai Co., Ltd., titanium chelates Orgatix TC-300 and TC-310 manufactured by Matsumoto Fine Chemical Co., Ltd., and zirconium chelates ZC-126 and ZC-300 manufactured by Matsumoto Fine Chemical Co., Ltd.
[0044] The gas barrier coating agent of the present invention may contain other additives as necessary, such as a surface conditioner, an ultraviolet absorber, an antioxidant, a polymerization inhibitor, wax, and an inorganic compound.
[0045] [Surface conditioner] The surface conditioner is a material having a surface conditioner function such as leveling property and prevention of cissing. Examples of the surface conditioner include polyether-modified polydimethylsiloxane having an acrylic group, polyether-modified dimethylsiloxane, polyester-modified dimethylsiloxane having an acrylic group, polyether-modified polydimethylsiloxane, and polyester-modified polydimethylsiloxane. Silicone-based surface conditioners such as siloxane and aralkyl-modified polymethylalkylsiloxane are preferably used. Other examples include acrylic surface conditioners, fluorine-based surface conditioners, and acetylene glycol surface conditioners. These can be used alone or in combination of two or more, and are preferably present in an amount of 0.001% by mass or more and 2.0% by mass or less, and more preferably 0.01% by mass or more and 1.0% by mass or less, relative to 100% by mass of the total of components (A) to (C).
[0046] [Ultraviolet absorber] The ultraviolet absorber is used for the purpose of preventing deterioration of the laminate due to ultraviolet rays emitted from sunlight or lighting. For example, benzophenone-based, benzotriazole-based, triazine-based, etc. are mentioned, and many water-dispersed products for water-based applications are on the market. These can be used alone or in combination of two or more types, and are preferably 0.001% by mass or more and 1.0% by mass or less with respect to 100% by mass of the total of components (A) to (C).
[0047] [Antioxidants] The antioxidant is used for the purpose of preventing deterioration, similarly to the above-mentioned ultraviolet absorber, and examples thereof include hindered phenol-based antioxidants, hindered amine-based antioxidants, etc. These can be used alone or in combination of two or more kinds, and are preferably present in an amount of 0.001% by mass or more and 0.5% by mass or less relative to 100% by mass of the total of the components (A) to (C).
[0048] [Polymerization inhibitor] The gas barrier coating agent of the present invention may contain a polymerization inhibitor in order to improve storage stability. The polymerization inhibitor may be appropriately selected from known ones. Examples of the polymerization inhibitor include hindered phenols, hindered amines, quinones, nitrosamines, phenothiazines, and piperidine-1-oxyls. When a polymerization inhibitor is used, the content is preferably 0.001% by mass or more and 0.2% by mass or less with respect to 100% by mass of the total of the components (A) to (C) in order to achieve both storage stability and photocurability.
[0049] [wax] When the gas barrier coating agent of the present invention is water-based, the wax is preferably a water dispersion, that is, an emulsion. Examples of wax emulsions include wax emulsions containing polyolefin wax, paraffin wax, Sasol wax, etc. Polyolefin wax is a polymer or copolymer mainly composed of an olefin monomer. Paraffin wax is a petroleum wax consisting of a mixture of linear saturated hydrocarbons having 20 to 30 carbon atoms. Sasol wax is a synthetic wax consisting of almost saturated linear hydrocarbons produced by the Fischer-Tropsch method using carbon monoxide and hydrogen as raw materials. Wax emulsions containing one or more selected from polyolefin wax and paraffin wax are preferred, and wax emulsions containing polyolefin wax are more preferred. The wax emulsions containing the above waxes can be used alone or in combination of two or more.
[0050] [Inorganic compounds] The gas barrier coating agent of the present invention may further contain an inorganic compound for the purpose of imparting higher gas barrier properties. The inorganic compound is preferably in a plate-like form that is likely to exhibit a labyrinth effect, but this is not necessarily optimal from the viewpoint of coatability and stability over time, and the inorganic compound may be in a spherical or amorphous form. Examples of plate-like inorganic compounds that can be suitably used in the present invention include hydrated silicates (phyllosilicate minerals, etc.), kaolinite-serpentine clay minerals (halloysite, kaolinite, endelite, dickite, nacrite, etc., antigonium oxide, etc.), and the like. lite, chrysotile, etc.), pyrophyllite-talc family (pyrophyllite, talc, ke loray, etc.), smectite group clay minerals (montmorillonite, beidellite, nontronite, saponite, hectorite, sauconite, stevensite, etc.), vermiculite group Clay minerals (vermiculite, etc.), mica or mica group clay minerals (muscovite, phlogopite, etc.), Margarite, tetrasilylic mica, taeniolite, etc.), chlorite group (kukkeite, sudoite, clinochlore, chamosite, nimite, etc.), hydrotalcite, platelet sulfur Examples of the clay minerals include barium sulfate, boehmite, and aluminum polyphosphate. These minerals may be natural clay minerals or synthetic clay minerals.
[0051] <Method of manufacturing gas barrier coating agent> The gas barrier coating agent of the present invention may contain the above-mentioned water-soluble polysaccharide (A), the compound (B) having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 to less than 300, and the metal salt (C) having a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 to less than 300 as a ligand, and the manufacturing method is not particularly limited. Specific manufacturing methods include a method of mixing each raw material and water and dissolving it over time with a roller-type agitator, or a method of preparing a coating agent by stirring with a stirrer such as a homodisper, and any method may be used as long as a uniform solution without lumps is obtained, but from the above viewpoint, it is preferable to mix the water-soluble polysaccharide (A) and the metal salt (C) after preparing them in a water-soluble or dispersed state at any ratio. In addition, when the compound (B) having an anionic hydrophilic group is required (for example, chitosan) when the water-soluble polysaccharide (A) is made water-soluble, it is necessary to mix and dissolve it first and then mix it with the aqueous solution of the metal salt (C). When additives are added, it is desirable to dilute them with water or alcohol before use in order to prevent shock at the time of addition.
[0052] <Gas barrier laminate> The gas barrier laminate of the present invention has a gas barrier layer formed by applying the gas barrier coating agent of the present invention to one or both sides of a substrate and curing it as necessary, and can be suitably used for packaging material applications. [Base material] The substrate or film substrate is selected from the group consisting of resin sheets, paper, and aluminum sheets (aluminum foil). For example, the resin sheet may be a resin sheet formed from a polyester resin such as polyethylene terephthalate (PET) or polyethylene naphthalate (PEN), a polycarbonate resin, a polyarylate resin, an acrylic resin, a polyphenylene sulfide resin, a polystyrene resin, a vinyl resin, a vinyl chloride resin, a polyimide resin, an epoxy resin, or a polyolefin resin such as polyethylene, polypropylene, or polynorbornene. In addition, the substrate may be a laminate in which a metal is laminated on these sheets, for example, a laminate in which a metal is laminated on a polyethylene terephthalate (PET) sheet. Among the substrates, polypropylene, polyethylene terephthalate, polyethylene, etc. are preferable because a laminate sheet having good stretchability, translucency, and rigidity can be obtained. The substrate may contain one or more optional components within a range that does not impair the effects of the present invention. The substrate used in the present invention may contain an ultraviolet absorber, an antioxidant, an antistatic agent, a surfactant, a pigment, a fluorescent whitening agent, etc. The substrate may contain inorganic particles containing silica, calcium carbonate, titanium oxide, etc., or organic particles containing acrylic resin, styrene resin, etc.
[0053] [Method of applying gas barrier coating agent] The method of applying the gas barrier coating agent includes a printing method and is not particularly limited, and any known coating method can be used. Examples of the coating method include wire bar coating, die coat coating, cast coating, slot coating, omega coating, spiral coating, controlled seam coating, slot coating, dot coating, hot melt applicator coating, hot melt coater coating, blade coat coating, dip coating, and gravure coating. Examples of the coating method include a coating method, a microgravure coating method, a curtain spray coating method, a bead coating method, a hot melt roll coater coating method, and a spin coat coating method, and examples of the printing method include an inkjet printing method, a spray printing method, a roll coat printing method, a doctor roll printing method, a doctor blade printing method, a curtain coat printing method, a slit coat printing method, a screen printing method, a reverse printing method, a push coat printing method, and a slit coater printing method. After the oxygen barrier laminate is applied to the substrate by these methods, it may be heated and dried or dried under reduced pressure as necessary to remove the solvent or promote crosslinking. The drying conditions are not particularly limited as long as the substrate is not deteriorated depending on the film thickness, the substrate, and the selected organic solvent, but hot air heating at about 40 to 200°C is preferably used.
[0054] The thickness of the gas barrier coating agent layer (coated product) is not particularly limited, but is preferably a thin film in order to prevent cracks from occurring when the product is bent, and is preferably 0.1 to 200 μm in a dry state, more preferably 0.5 to 20 μm, and even more preferably 1.0 to 10.0 μm. The gas barrier coating agent layer formed here may be laminated in one or more layers on one or both sides of the substrate. When multiple gas barrier coating layers are provided, the compositions of the layers may be the same or different. For example, after applying the gas barrier coating agent to one side of the substrate, a drying process may be performed, and the same water vapor barrier layer may be formed in the same process to form two layers, or a different gas barrier coating agent may be formed to form three layers.
[0055] [Method of curing the gas barrier coating layer] The gas barrier coating agent of the present invention is most preferably applied by various coating methods, and then passed through an electron beam irradiator to obtain a cured coating film (gas barrier layer). In the case of electron beam irradiation, the irradiation dose varies depending on the film thickness and the desired degree of curing, but if the film thickness is 10 μm or less, it is desirable to irradiate with 10 to 100 kGy at an acceleration voltage of 80 to 150 kV, preferably 30 to 80 kGy at an acceleration voltage of 100 to 120 kV. After electron beam irradiation, heating can be performed as necessary to promote curing.
[0056] The gas barrier coating agent of the present invention is also suitable for obtaining a cured coating film by irradiation with ultraviolet light in addition to electron beam curing. When using the ultraviolet light irradiation method, it is necessary to add the above-mentioned photopolymerization initiator and photosensitizer to the gas barrier coating agent. For example, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, an excimer laser lamp, a xenon lamp, an ultraviolet light emitting diode (UV-LED), etc. can be used as the ultraviolet light irradiation means.
[0057] Among the ultraviolet irradiation means, UV-LED has the characteristics of narrow wavelength width of the ultraviolet light irradiated and easy miniaturization. Therefore, the irradiation wavelength and the usage method of UV-LED can be adjusted to some extent according to the characteristics of the photopolymerization initiator in the gas barrier coating agent. The peak wavelength of the UV-LED used is preferably 280 to 420 nm, and particularly preferably 320 to 400 nm.
[0058] When using an ultraviolet ray irradiation means (ultraviolet lamp) other than UV-LED as the ultraviolet ray irradiation means, a metal halide lamp is preferably used from the viewpoint of efficiently emitting ultraviolet rays in the UV-A region and allowing the irradiation light to reach the inside of the ink coating sufficiently. Note that it can also be used in combination with the above-mentioned UV-LED.
[0059] The maximum illuminance of the ultraviolet light is preferably 80 mW / cm2 or more, more preferably 120 mW / cm2 or more. The integrated light amount during irradiation varies depending on the type and content of the polymerizable monomer and photopolymerization initiator, but is preferably 100 mJ / cm2 or more. It is preferable to set the exposure dose to 150 mJ / cm2 or more, and more preferable to set the exposure dose to 200 mJ / cm2 or more.
[0060] When the gas barrier layer of the present invention uses an electron beam or ultraviolet curing method, the usual method is to obtain a cured coating film by a coating step, a solvent drying step, and then an electron beam or ultraviolet irradiation step, but if the binder resin used has a high molecular weight, molecular mobility is restricted, so the degree of crosslinking may be improved by prioritizing the polymerization reaction in a wet state. In other words, by limiting the solvent drying step to a pre-drying step in which a certain amount of solvent remains, irradiating with electron beams or ultraviolet rays, and then completely drying, a more highly crosslinked coating film can be obtained, and the barrier properties and water resistance may be improved.
[0061] In addition to the substrate and the gas barrier layer, the gas barrier laminate may have an optional organic or inorganic layer, and examples of the optional layer include an anchor coat layer, a printing ink layer, an adhesive layer, a topcoat layer, and an overcoat layer. One or more of these layers may be included. The optional layer is not particularly limited, but may be formed directly on the substrate layer, or may be formed via a gas barrier layer. For example, a protective layer and an adhesive layer may be provided on the gas barrier layer as necessary from the viewpoint of protecting the oxygen barrier composition layer or improving the abrasion resistance. The anchor coat layer is preferably formed between the gas barrier layer and the substrate layer, and the topcoat layer is preferably formed on the gas barrier layer formed via the substrate. The thickness of the laminate when the optional layer is provided is not particularly limited, but is preferably 0.1 to 200 μm in a dry state, more preferably 0.5 to 20 μm, and even more preferably 1.0 to 10.0 μm.
[0062] The method for laminating the organic layer or inorganic layer is not particularly limited. For example, the organic layer or inorganic layer may be laminated by a wet process such as coating, or may be laminated from above by film, extrusion processing, or lamination, or may be a laminate including a layer formed by a vacuum process such as vapor deposition or CVD. Examples of materials for the organic layer include polyvinyl alcohol, polyolefins (polyethylene, polypropylene, poly-4-methyl-1-pentene, polybutene, etc.), cyclic olefin polymers, polyesters (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyamides (nylon-6, nylon-66, polymetaxylene adipamide, etc.), polyphenylene sulfide, polyethyleneimine, polyimides, etc. These may be used alone or in combination of two or more. Examples of materials for the inorganic layer include metals and semi-metals such as chromium, zinc, cobalt, aluminum, tin, and silicon, or oxides, nitrides, nitride oxides, sulfides, and phosphides of the aforementioned metals and semi-metals such as silica, alumina, titanium oxide, zinc oxide, and silicon nitride. These may be used alone or in combination of two or more. When one or more oxygen barrier composition layers and one or more organic or inorganic layers are included on one or both sides of the substrate, the order of stacking these layers is arbitrary.
[0063] The laminate of the present invention may further have a heat-sealable heat-adhesive layer as necessary. By having the heat-adhesive layer, the laminate can be sealed by heat sealing, and can be suitably used for packaging material applications.
[0064] The laminate of the present invention can be used as a multi-layer packaging material for protecting foods, medicines, etc. When used as a multi-layer packaging material, the layer structure can be changed depending on the contents, the environment of use, and the form of use. There are no particular limitations on the applications, but the laminate of the present invention can be suitably used for foods, daily necessities, electronic materials, medical applications, and the like, which require high barrier properties. EXAMPLES
[0065] Specific examples of the present invention will be described below together with comparative examples. In the following examples and comparative examples, "parts" and "%" represent "parts by mass" and "% by mass", respectively.
[0066] <Preparation of metal salt (C) aqueous solution> [Calcium acrylate aqueous solution] 10 parts calcium hydroxide powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade, 0.135 mol ) and 64 parts of ion-exchanged water were placed in a 225 ml mayonnaise bottle (mayo bottle) and mixed lightly using a homodisper to the extent that no lumps were formed. While stirring, 20 parts (0.278 mol) of acrylic acid were gradually added dropwise so that the temperature in the system did not rise above 50°C due to an exothermic reaction. The addition of acrylic acid caused the mixture to change from a cloudy dispersed state to a transparent liquid, and stirring was continued for approximately 10 minutes to terminate the reaction. After filtration with a #200 filter cloth, the mixture was diluted with ion-exchanged water so that the solid content was 30.0%. Exchanged water was added to obtain an aqueous solution of calcium acrylate. The molecular weight of acrylic acid was 72.1 g / mol.
[0067] [Magnesium acrylate aqueous solution] Put 10 parts of magnesium hydroxide powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade, 0.171 mol) and 74 parts of ion-exchanged water into a 225 ml mayonnaise bottle and mix with a homodisper until no lumps form. While stirring, 25 parts (0.347 mol) of acrylic acid was gradually added dropwise so that the temperature in the system would not rise to 50°C or higher due to an exothermic reaction. The mixture changed from a cloudy dispersion state to a transparent liquid upon addition of acrylic acid, and stirring was continued for about 10 minutes to terminate the reaction. After filtering with a #200 mesh filter cloth, the solid content was adjusted to 30.0%, and the acrylic acid was added dropwise. An aqueous solution of magnesium acrylate was obtained.
[0068] [Zinc acrylate aqueous solution] 10 parts of zinc oxide powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade, 0.123 mol) and ion 60 parts of acrylic acid were placed in a 225 ml mayonnaise bottle and mixed lightly with a homodisper until no lumps formed. While stirring, 18.2 parts (0.253 mol) of acrylic acid were gradually added dropwise so that the temperature in the system did not rise above 50°C due to an exothermic reaction. The addition of acrylic acid caused the mixture to change from a cloudy dispersion state to a transparent liquid, and stirring was continued for about 10 minutes to terminate the reaction. After filtering with a #200 mesh filter cloth, the solid content was adjusted to 30.0%, and the acrylic acid was added. Thus, an aqueous zinc acid solution was obtained.
[0069] [2-acrylamido-2-methylpropanesulfonic acid zinc aqueous solution] 5.0 parts of zinc oxide powder (FUJIFILM Wako Pure Chemical Industries, Ltd., special grade, 0.061 mol) and 60 parts of ion-exchanged water were placed in a 225 ml mayonnaise bottle and mixed lightly with a homodisper to the extent that no lumps were formed. While stirring, 25.7 parts (0.124 mol) of 2-acrylamido-2-methylpropanesulfonic acid was gradually added dropwise so that the temperature in the system did not exceed 50°C due to an exothermic reaction. The addition of 2-acrylamido-2-methylpropanesulfonic acid changed the cloudy dispersion state to a transparent liquid, and stirring was continued for about 10 minutes to terminate the reaction. After filtration with a #200 mesh filter cloth, the solid content was adjusted to 30.0%, and the 2-acrylamido An aqueous solution of zinc amido-2-methylpropanesulfonate was obtained. The molecular weight of 2-acrylamido-2-methylpropanesulfonic acid was 207.3 g / mol.
[0070] [Water-based polyurethane solution] Into a four-necked 2000 ml flask equipped with a reflux condenser, a dropping funnel, a gas inlet tube, a stirrer, and a thermometer, 240 parts of PTG-2000SN (manufactured by Hodogaya Chemical Co., Ltd., polytetramethylene glycol having a number average molecular weight of 2000), 24 parts of PEG2000 (polyethylene glycol having a number average molecular weight of 2000), 35 parts of dimethylol butanoic acid (manufactured by HighChem Co., Ltd.), 75 parts of isophorone diisocyanate (manufactured by Evonik Degussa Japan Co., Ltd.), MEK (methyl ketone), and 10 parts of dimethylol butanoic acid (manufactured by HighChem Co., Ltd.). The mixture was charged with 94 parts of ethyl ethyl ketone (ethyl ethyl ketone) and substituted with dry nitrogen. The temperature was gradually raised to 85°C under stirring and allowed to react for 5 hours. Next, while cooling, a mixed solution of 8.9 parts of 28% ammonia water, 900 parts of ion-exchanged water, and 119 parts of isopropyl alcohol was gradually dropped into the solvent-based polyurethane resin to neutralize it and make it water-soluble. Thereafter, the solvent was distilled off under reduced pressure, and the distillate was replaced with ion-exchanged water to obtain an aqueous polyurethane resin solution (PU-1) with a solid content of 24%. PU-1 has 6.4% structural units derived from polyethylene glycol, a weight average The molecular weight was 30,000, the glass transition temperature was -80°C, and the acid value was 35 mgKOH / g.
[0071] <Preparation of gas barrier coating agent> [Example 1] Put 10 parts of chitosan powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Chitosan 10), 110 parts of ion-exchanged water, and 10 parts of acrylic acid into a 225 ml mayonnaise bottle, close the lid, and stir for 2 hours using a roller stirrer. The chitosan was dissolved by stirring for 30 minutes. After removing the small amount of insoluble matter using a filter cloth, 33.3 parts of the calcium acrylate aqueous solution was added and stirred again with the roller stirrer for 30 minutes to obtain a transparent, viscous gas barrier coating agent.
[0072] [Examples 2 to 15, 17, and 18] A gas barrier coating agent was obtained in the same manner as in Example 1, except that the compounds and their amounts shown in Table 1 were changed.
[0073] [Example 16] In a 450 ml mayonnaise bottle, 10 parts of high molecular weight chitosan powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Chitosan 100), 250 parts of ion-exchanged water, 5 parts of acrylic acid, and 5 parts of Light Ester P-1M (manufactured by Kyoeisha Chemical Co., Ltd.) were placed, and the bottle was covered and stirred for 2 hours with a roller stirrer to dissolve the chitosan. After removing the remaining insoluble matter using a filter cloth, 20 parts of zinc acrylate aqueous solution were placed and stirred again for 30 minutes with a roller stirrer. 2 parts of aluminum acrylate powder (manufactured by Asada Chemical Industry Co., Ltd.) and 80 parts of glass beads (5 μm) were added, and the dispersion was completed by shaking and stirring for 1 hour with a wet media disperser Scandex. The glass beads were removed with a filter cloth to obtain a gas barrier coating agent.
[0074] [Comparative Examples 1 to 4] Coating agents were obtained in the same manner as in Example 1, except that the compounds and their amounts shown in Table 1 were changed.
[0075] [Comparative Example 5] 10 parts of ethylene-vinyl alcohol copolymer (PVOH) powder (Kuraray Co., Ltd., AQ-4104) and 200 parts of ion-exchanged water were placed in a 450 ml mayonnaise bottle, the bottle was covered, and the bottle was placed in a 95°C oven and heated for 1 hour. After returning to room temperature, 10 parts of acrylic acid were added, the mixture was stirred with a roller stirrer, and filtered using a filter cloth. 33.3 parts of a 30% aqueous zinc acrylate solution was added, and the mixture was stirred again with the roller stirrer for 30 minutes to obtain a coating agent.
[0076] [Comparative Example 6] 10 parts of water-based polyurethane (PU-1), 20 parts of ion-exchanged water, and 5 parts of Carbodilite E-02 (manufactured by Nisshinbo Co., Ltd.) were placed in a 225 ml mayonnaise bottle, and the mixture was stirred and mixed using a homodisper to obtain a coating agent.
[0077] [Comparative Example 7] 10 parts of polyacrylic acid (manufactured by Wako Pure Chemical Industries, Ltd., average molecular weight 25,000), 40 parts of ion-exchanged water, and 5 parts of Denacol EX-313 (manufactured by Nagase ChemteX Corporation) were placed in a 225 ml mayonnaise bottle, and the mixture was stirred and mixed using a homodisper to obtain a coating agent.
[0078] [Table 1]
[0079] [Table 2]
[0080] The abbreviations and properties of the raw materials listed in Tables 1 and 2 are as follows. The compound amounts listed in the tables are expressed as solid amounts.
[0081] (Water-soluble polysaccharide (A)) Chitosan 10: Fujifilm Wako Pure Chemical Industries, Ltd., low molecular weight product, deacetylation rate 80.0 mol% or more Chitosan 100: Fujifilm Wako Pure Chemical Industries, Ltd., high molecular weight product, deacetylation rate 80. 0mol% or more Guar gum: white powder, product name Guapack PF-20 MP Gokyo Food & Chemical Co., Ltd. Xanthan gum: white powder, product name: Labolgum GS-C MP Gokyo Food & Chemical Co., Ltd.
[0082] (Compound Having Anionic Hydrophilic Group and Ethylenically Unsaturated Double Bond) Acrylic acid: Fujifilm Wako Pure Chemical Industries, molecular weight 72.1 g / mol Methacrylic acid: Fujifilm Wako Pure Chemical Industries, molecular weight 86.1 g / mol AAmSA (2-acrylamido-2-methylpropanesulfonic acid): Fujifilm Wako Pure Chemical Industries, molecular weight 207.3 g / mol Light Ester P-1M: 2-Methacryloyloxyethyl Acid Phosphate, Kyoei Manufactured by Sha Kagaku Co., Ltd., molecular weight 210g / mol Light Ester P-2M: 2-Methacryloyloxyethyl Acid Phosphate, Kyoei Manufactured by Sha Kagaku Co., Ltd., molecular weight 322g / mol *The molecular weight of Light Ester P-1M and Light Ester P-2M is calculated from the chemical structure of the main component.
[0083] (Metal Salts (C)) Calcium acrylate: 30% calcium acrylate aqueous solution prepared above Magnesium acrylate: 30% magnesium acrylate aqueous solution prepared above Zinc acrylate: 30% zinc acrylate aqueous solution prepared above AAmSA zinc: 30% zinc 2-acrylamido-2-methylpropanesulfonate prepared above Aluminum acrylate: white powder, manufactured by Wako Pure Chemical Industries, Ltd.
[0084] (Resin (D)) Ethylene-vinyl alcohol copolymer (EVOH): AQ-4104 (Kuraray Co., Ltd.) Water-based polyurethane (PU-1): Water-based polyether polyurethane resin prepared above, solid content 24%, average molecular weight 30,000, acid value 35 mgKOH / g
[0085] (Crosslinking agent (E)) Carbodilite E-02: Carbodiimide crosslinking agent, manufactured by Nisshinbo Co., Ltd., carbodiimide equivalent 445g / eq. solid content 40% Denacol EX-313: Glycerol polyglycidyl ether (epoxy crosslinker), Nagase ChemteX Corporation, epoxy equivalent 141g / eq.
[0086] [Laminated body production] In Examples 1 to 18 and Comparative Examples 1 to 7, the prepared samples were applied to a PET substrate (Toyobo Co., Ltd. E-5102, film thickness 25 μm) using a Mayer bar. The number of the Mayer bar was selected so that the applied film thickness was within 3 to 5 μm when measured at multiple locations. After application, the coating was dried in a drying oven at 75° C. for 3 minutes to remove the solvent, and cured using an electron beam irradiator EC250 / 15 / 180L manufactured by Iwasaki Electric Co., Ltd. at an acceleration voltage of 110 kV and an electron beam dose of 70 kGy to prepare laminates as shown in Tables 1 and 2, which were used as samples for evaluating the physical properties of the coating film.
[0087] <Oxygen permeability measurement> The oxygen transmission rate was measured under conditions of a temperature of 23° C. and a relative humidity of 65% and a temperature of 23° C. and a relative humidity of 90% for the laminates obtained in Examples 1 to 18 and Comparative Examples 1 to 7. Here, RH indicates relative humidity. The oxygen permeability was measured using the MOCON oxygen permeability measuring device OX-TRAN2 / 22. The measurement was performed by the isostatic method in accordance with JIS K 7126. The measurement area of the laminate set in the measurement cell was 50 cm. 2 The oxygen barrier required for general packaging materials is an oxygen transmission rate of 1cc / m at a temperature of 23°C and a relative humidity of 65%. 2 If the humidity is less than 20cc / m2, the performance is sufficient, and in addition, it is excellent enough to suppress the deterioration of the barrier property under high humidity conditions. 2 Barrier films with oxygen permeability of 100% or more per day atm are marked as OVER because the reproducibility of oxygen permeability is low. The oxygen permeability measured under normal humidity and high humidity were evaluated according to the following criteria, and the evaluation results are shown in Tables 1 and 2. (Oxygen permeability at normal humidity) A: Excellent 1.0cc / m 2 ·day·atm Less than B: Good 1.0cc / m 2 ·day · atm or more 5.0cc / m 2 ·da Less than y·atm C: Practical level 5.0cc / m 2 ·day · atm or more 20.0cc / m 2 d Less than ay·atm D: Defective 20.0cc / m 2 ·day · atm or more (Oxygen permeability under high humidity conditions) A: Excellent 3.0cc / m 2 ·day·atm Less than B: Good 3.0cc / m 2 ·day · atm or more 10.0cc / m2 ·day Less than ATM C: Practical level 10.0cc / m 2 ·day · atm or more 20.0cc / m 2 ·day·less than atm D: Defective 20.0cc / m 2 ·day · atm or more
[0088] <Water friction resistance> The laminates obtained in Examples 1 to 18 and Comparative Examples 1 to 7 were used to evaluate water abrasion resistance. A cotton swab sufficiently moistened with water was rubbed from one side from the uncoated substrate portion to the coated portion a certain number of times, and the degree of dissolution of the coated edge, the degree of swelling of the rubbed portion, and the degree of scraping of the laminate surface were visually evaluated. The evaluation was based on the following criteria and is shown in Tables 1 and 2. (Evaluation Criteria) A: Excellent - No change in appearance even after rubbing 200 times or more B: Good. After rubbing 200 times, there are changes in appearance such as swelling and scraping of the coating surface. C: Practical level. Edge melting occurs after 100 to 200 cycles. D: Poor: The edge or entire rubbing area melted and the substrate was exposed after less than 100 times.
[0089] <Adhesion to substrate> Adhesion to substrates was evaluated using the laminates obtained in Examples 1 to 18 and Comparative Examples 1 to 7. Measurements were performed by applying an adhesive tape (cellophane tape (width 12 mm) manufactured by Nichiban Co., Ltd.) to the coated surface and peeling it off at an angle of 180 degrees, and the area percentage of the coating film remaining on the coated substrate side was measured according to the following criteria, and the evaluation results are shown in Tables 1 and 2. (Evaluation Criteria) A: Excellent, no peeling B: Good, peeling (less than 40%) C: Practical level, peeling (40% to less than 90%) D: Poor, peeling (90% or more)
[0090] <haze> Regarding the transparency of the laminates obtained in Examples 1 to 18 and Comparative Examples 1 to 7, the turbidity value (haze value) was measured using a spectroscopic haze meter SH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) according to the following criteria: The evaluation results are shown in Tables 1 and 2 in accordance with the standards. (Evaluation Criteria) A: Excellent Haze value is less than 3.0% B: Good Haze value is 3.0% or more and less than 6.0% C: Practical level Haze value is 6.0% or more and less than 10.0% D: Defective Haze value is 10.0% or more
[0091] As shown in Table 1, the coating material of the example was exposed to mild humidity conditions of 23°C and 65% RH. It was also shown that the film not only exhibits excellent oxygen barrier properties, but also prevents the deterioration of barrier properties under high humidity conditions of 23°C and 90% RH. It also achieved high levels of substrate adhesion, transparency, and water resistance, and was shown to be suitable for use as a top coating for packaging materials.< / haze>
Claims
1. water-soluble polysaccharide (A), (B) a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more and less than 300; and a metal salt (C) having, as a ligand, a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more and less than 300. A gas barrier coating agent comprising:
2. 2. The gas barrier coating agent according to claim 1, wherein the water-soluble polysaccharide (A) comprises chitosan.
3. 2. The gas barrier coating agent according to claim 1, wherein the central metal of the metal salt (C) comprises at least one metal selected from the group consisting of zinc, calcium, magnesium, and aluminum.
4. Based on 100% by mass of the solid content of the gas barrier coating agent, The content of the water-soluble polysaccharide (A) is 20 to 70% by mass, The content of compound (B) is 10 to 60% by mass, The content of the metal salt (C) is 10 to 70 mass%.
2. The gas barrier coating agent according to claim 1.
5. 2. The gas barrier coating agent according to claim 1, which is for use in packaging materials.
6. A laminate having a gas barrier layer formed on a substrate using the gas barrier coating agent according to any one of claims 1 to 5.
7. A method for producing a laminate, comprising the steps of: applying a gas barrier coating agent to a substrate to obtain a coated product; and irradiating the coated product with ultraviolet light or electron beams to form a gas barrier layer on the substrate, The gas barrier coating agent is water-soluble polysaccharide (A), (B) a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more and less than 300; and a metal salt (C) having, as a ligand, a compound having an anionic hydrophilic group and an ethylenically unsaturated double bond and a molecular weight of 50 or more and less than 300. A method for producing a laminate, the gas barrier coating agent comprising the steps of:
Citation Information
Patent Citations
Oriented film laminate and manufacture thereof
JP1985157830A
Gas barrier resin composition and gas barrier film formed from the same
JP2003171419A
Gas barrier laminate and manufacturing method therefor
JP2016159576A
Amyloid β decomposition discharge promoter
JP2019178130A
Gas barrier molding and method for producing the same
JP2021113244A