Composite laminate heater and method for manufacturing the same
The composite laminate heater integrates polypropylene into textile meshes with heat-generating fibers and optional aluminum layers, addressing the issue of layer peeling and achieving stable, efficient heating for various applications.
Patent Information
- Application Number
- JP2024073871
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-30
- Publication Date
- 2024-11-08
AI Technical Summary
Existing methods struggle to integrate polypropylene layers effectively to form a composite laminate heater with sufficient shape stability and heat-generating capabilities, as polypropylene sheets tend to peel off when stacked and thermocompressed.
A composite laminate heater is designed with multiple layers, including a planar heat-generating layer and film layers, where polypropylene is infiltrated and fixed into the mesh structure of textiles, and electrodes are connected to heat-generating fibers, allowing for uniform heating and easy voltage application, with optional aluminum layers for radiation reflection and insulation.
The laminate heater achieves excellent shape stability and uniform heating, with improved corrosion resistance and thermal efficiency, suitable for applications in automobiles and heated surfaces like toilet seats.
Smart Images

Figure 2024159738000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite laminate heater and a method for making the same. [Background technology]
[0002] Conventionally, a method of manufacturing a component by infiltrating resin into fibers has been known as a decorative molding technique for resin (for example, Patent Document 1). Patent Document 1 discloses a veneer sheet in which a nonwoven fabric mainly made of fibers capable of maintaining its shape at a temperature higher than the melting point of the resin film is interposed between the back surface of the veneer and the resin film, and the resin film is configured as if it were FRP, and an application product of the veneer sheet. PET fiber is given as an example of the nonwoven fabric, and a propylene film is given as an example of the resin film. In the veneer sheet described in Patent Document 1, the nonwoven fabric and the base resin are firmly bonded to each other by exerting an anchor effect between them.
[0003] Patent Document 2 discloses a sheet heating element in which a matrix resin is impregnated into a carbon fiber sheet having electrodes formed on both ends of continuous carbon fiber. Patent Document 2 mentions polyolefin resin, and specifically introduces an example in which polycarbonate resin is used as the matrix resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Re-tabled publication No. 2013-190839 [Patent Document 2] Patent Publication No. 2021-12814 Summary of the Invention [Problem to be solved by the invention]
[0005] Polypropylene is not only low-cost to procure, but also has excellent chemical resistance, and has the potential for application in a variety of applications. The inventors of the present invention have been working on the production of an integrated laminate using only polypropylene as the resin to be infiltrated into the fibers of a nonwoven fabric. However, it is common knowledge in the molding field that even if multiple sheets made of polypropylene are stacked and thermocompressed, the layers derived from the sheets peel off from the product, and it is not possible to firmly integrate the entire product as a member made only of polypropylene.
[0006] Patent Document 1 lists a propylene film as an example of a resin film. However, the nonwoven fabric is impregnated with resin in order to bond the veneer sheet to the veneer, and only a single layer is formed for bonding. Therefore, even if the above-mentioned conventional technology is used, it is not easy to impregnate polypropylene into fibers that can generate heat by electric current and integrate them.
[0007] The present invention has been made in consideration of the above circumstances, and aims to provide a composite laminate heater having excellent shape stability due to the stacked layers being integrated together, and a manufacturing method thereof. [Means for solving the problem]
[0008] (1) In order to achieve the above object, the present invention takes the following measures. That is, the composite laminate heater of the present invention comprises a plurality of composite layers formed by infiltrating and bonding polypropylene into the mesh structure of a sheet-like textile, and a sheet-like heat generating fiber, a pair of electrodes connected to the heat generating fiber, and polypropylene infiltrated and bonded into the mesh structure of the heat generating fiber, the sheet-like heat generating layer being provided between adjacent textiles in the plurality of composite layers, the plurality of composite layers and the sheet-like heat generating layer being laminated, and the polypropylene in the plurality of composite layers and the sheet-like heat generating layer being filled into the mesh structure and integrated. By integrating the laminated layers in this way, a composite laminate heater with excellent shape stability is obtained.
[0009] (2) The composite laminate heater of the present invention comprises a film layer made of polypropylene, a composite layer having a sheet-like textile and polypropylene infiltrated and fixed into the mesh of the textile, and a sheet-like heat generating fiber, a pair of electrodes connected to the heat generating fiber, and polypropylene infiltrated and fixed into the mesh structure of the heat generating fiber, and a planar heat generating layer provided between the film layer and the composite layer, the film layer and the composite layer being laminated, and the polypropylene contained in the film layer and the composite layer being integrated. By integrating the laminated layers in this way, a composite laminate heater with excellent shape stability can be obtained.
[0010] (3) In the composite laminate heater described in (1) or (2) above, the pair of electrodes are connected to the opposing edges of the heat generating fiber. This allows for uniform heating over the entire surface of the composite laminate heater. Also, by embedding the electrodes, it becomes easier to connect to terminals that apply voltage.
[0011] (4) The composite laminate heater described in (1) above is characterized by further comprising an aluminum layer provided on one of the main surfaces of the plurality of composite layers, which reflects radiation from the heat-generating fiber and amplifies heating on the other side.
[0012] (5) In the composite laminate heater described in (4) above, the aluminum layer is formed by laminating a plurality of aluminum foils, and a gap is formed between the plurality of aluminum foils. The gap formed between the plurality of aluminum foils can increase the reflectance of radiation.
[0013] (6) In the composite laminate heater described in (5) above, a resin layer having holes that do not overlap each other is formed between the plurality of aluminum foils. The holes that do not overlap each other ensure a gap between the aluminum foils.
[0014] (7) The composite laminate heater described in (2) above is characterized by further comprising an aluminum layer provided on one of the main surfaces of the laminate of the film layer and the composite layer, which reflects radiation from the heat-generating fiber and amplifies heating on the other side.
[0015] (8) In the composite laminate heater described in (7) above, the aluminum layer is formed by laminating a plurality of aluminum foils, and a gap is formed between the plurality of aluminum foils. The gap generated between the plurality of aluminum foils can increase the reflectance of radiation.
[0016] (9) In the composite laminate heater described in (8) above, a resin layer having holes that do not overlap each other is formed between the plurality of aluminum foils. The holes that do not overlap each other ensure a gap between the aluminum foils.
[0017] (10) The composite laminate heater according to (1) or (2) above is characterized in that it further comprises a coating layer made of polypropylene and covering the composite layer, thereby improving corrosion resistance against cleaning agents such as hydrochloric acid.
[0018] (11) The method for producing a composite laminate heater of the present invention is characterized by including the steps of: preparing a plurality of prepreg sheets having a nonwoven fabric and polypropylene impregnated in the nonwoven fabric; stacking the prepreg sheets with a sheet-shaped heat generating fiber and a pair of electrodes connected to the heat generating fiber sandwiched therebetween to form a first laminate; and heat pressing the first laminate at a predetermined temperature or higher and at a predetermined pressure or higher. As a result, the stacked layers are integrated together to obtain a high-strength composite laminate heater with excellent shape stability.
[0019] (12) The method for producing a composite laminate heater of the present invention is characterized by including the steps of: preparing a plurality of prepreg sheets and a sheet-like textile having a woven fabric and polypropylene impregnated in the woven fabric, sandwiching a sheet-like heat generating fiber and a pair of electrodes connected to the heat generating fiber between the prepreg sheets and the textile to form a second laminate, and hot pressing the second laminate at a predetermined temperature or higher and at a predetermined pressure or higher. As a result, the laminated layers are integrated together to obtain a high-strength composite laminate heater with excellent shape stability.
[0020] (13) The method for producing a composite laminate heater of the present invention is characterized by including the steps of sandwiching a sheet-shaped heat generating fiber and a pair of electrodes connected to the heat generating fiber between a polypropylene film and a textile, alternately stacking the polypropylene film and the textile to form a laminate, and heat pressing the laminate at a predetermined temperature or higher and at a predetermined pressure or higher. This allows the stacked layers to be integrated together, resulting in a high-strength composite laminate heater with excellent shape stability. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a cross-sectional view showing a PP-FRP heater. [Diagram 2] 1(a) to 1(c) are cross-sectional views showing the steps of producing a prepreg. [Diagram 3] FIG. 2 is a perspective view showing a process of stacking prepregs and thermocompression bonding them. [Figure 4] 4(a) to 4(d) are cross-sectional views showing the molding and trimming steps, respectively. [Diagram 5] FIG. 2 is a perspective view showing a process of overlapping and thermocompression bonding a prepreg and a textile. [Figure 6] 1(a) and 1(b) are cross-sectional views showing a PP-FRP heater having an aluminum layer, a heat insulating layer, and an aluminum layer, respectively. [Figure 7] FIG. 2 is a perspective view showing the PP-FRP heater and the aluminum foil before bonding. [Figure 8] FIG. 11 is a cross-sectional view showing a composite laminate heater according to a fourth embodiment. [Figure 9] 1(a) and 1(b) are cross-sectional views showing the injection molding process. [Figure 10] 1A and 1B are cross-sectional views showing a PP-FRP member having an aluminum layer, a heat-insulating layer, and an aluminum layer, respectively. [Figure 11] FIG. 2 is a cross-sectional view showing the configuration of a buried heater. [Figure 12] 1(a) and 1(b) are a side cross-sectional view and a plan cross-sectional view, respectively, showing a stage in a manufacturing process of a buried heater. [Figure 13] This is a micrograph of the cut surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings.
[0023] [First embodiment] [Configuration of composite laminate heater (PP-FRP heater)] FIG. 1 is a cross-sectional view showing a PP-FRP heater 100. The form shown in FIG. 1 is one example, and the PP-FRP heater 100 is composed of composite layers 111-114 and a planar heating layer 130. PP-FRP (Fiber Reinforced Plastics) is a type of composite laminate, and is particularly excellent in shape stability. The planar heating layer 130 is composed of a heat generating fiber layer 131 and a pair of electrodes 132. The composite layers 111-114 and the planar heating layer 130 are laminated, and each of the composite layers 111-114 is formed of a textile and polypropylene that is infiltrated and fixed into the mesh of the textile. For the polypropylene, for example, those with melting points of 95°C, 120°C, and 150°C can be used depending on the temperature of the thermocompression bonding. In particular, amorphous materials are preferably used for hot melt.
[0024] In the composite layers 111-114 and the heat generating fiber layer 131, polypropylene exists continuously across the layers, and permeates into the meshes of the textile and heat generating fiber. Due to the anchor effect of the permeated polypropylene, the composite layers 111-114 and the heat generating fiber layer 131 are firmly bonded to the adjacent layers. In this way, a firmly integrated plate-shaped heater is formed.
[0025] The polypropylene preferably contains 5 wt% to 30 wt% of a tackifier, which is a tackifier resin, such as a petroleum-based tackifier, which makes it easier to prepare prepregs by hot melt.
[0026] As the polypropylene, one having a high melting point can be used. Such a high melting point polypropylene is a high shrinkage type material and can be used as a material for products requiring a high elastic modulus. For example, a high melting point polypropylene having a melting point of 150°C or higher is preferable. Such a high melting point polypropylene is preferably composed of 85 wt% to 95 wt% polypropylene and 5 wt% to 15 wt% tackifier.
[0027] Also, polypropylene with a low melting point can be used. Such low melting point polypropylene is a low shrinkage type and is slightly softer than high melting point polypropylene. It can be used for impregnation of synthetic fiber fabrics with low heat resistance such as polyethylene reinforced fiber. For example, low melting point polypropylene with a melting point of 100°C or less is preferable. Such low melting point polypropylene is preferably composed of 70wt% to 85wt% polypropylene and 15wt% to 30wt% tackifier.
[0028] It is preferable that the melting point of polypropylene is at least 160°C or less. This allows processing at low temperatures and enables bonding with components with different melting points. For example, a component with a surface decoration made of polypropylene with a high melting point can be formed and bonded to a PP-FRP heater.
[0029] It is preferable that all the textiles contained in each of the composite layers 111 to 114 are nonwoven fabrics or nonwoven fabrics and woven fabrics are alternately layered. The nonwoven fabric is preferably a spunbond nonwoven fabric, and particularly preferably a spunbond nonwoven fabric containing polyester. The nonwoven fabric may be a paper-based nonwoven fabric or felt containing polyester. The woven fabric may be a polyethylene-reinforced fiber woven fabric. When using polyester nonwoven fabric, the basis weight is preferably 30 g / m2 or more and 250 g / m2 or less. This makes it easier for the softened polypropylene to be impregnated.
[0030] The planar heating layer 130 is composed of a heat generating fiber layer 131 and a pair of electrodes 132. The heat generating fiber layer 131 has heat generating fiber and polypropylene. The polypropylene is infiltrated and fixed into the mesh structure of the heat generating fiber. The polypropylene infiltrated area into the heat generating fiber can obtain a sufficient integration effect even if it is only slightly deep from the surface. The pair of electrodes are connected to both ends of the heat generating fiber. It is preferable that the heat generating fiber is formed into a rectangular sheet, and the pair of electrodes are connected to both opposing edges of the sheet. This allows uniform heating over the entire surface of the PP-FRP heater. In addition, the electrodes are embedded, which makes it easier to connect to terminals that apply voltage.
[0031] The heat generating fiber is formed by mixing organic fiber and carbon fiber. The organic fiber is, for example, cellulose or a mixture of cellulose and polyester. The carbon fiber preferably has a representative length of 3 mm or more and 6 mm or less. The carbon fiber is preferably contained in an amount of 10 wt % or more and 20 wt % or less relative to the organic fiber. The pair of electrodes 132 is a thin film having electrical conductivity. The pair of electrodes 132 is preferably a tape containing a metal, for example, an aluminum tape or a copper tape.
[0032] In the PP-FRP heater 100, the composite layers 111-114 have a four-layer structure, but may have other numbers of layers. A four-layer structure or more can improve the strength of the PP-FRP heater 100 and stabilize the shape. On the other hand, a structure of less than four layers makes it easier to mold.
[0033] [Manufacturing method for composite laminate heater (PP-FRP heater)] A method for manufacturing the PP-FRP heater 100 configured as above will be described. The PP-FRP heater 100 is manufactured through the steps of prepreg production, thermocompression bonding, preform molding, and trimming. Figures 2(a) to (c) are cross-sectional views each showing the steps of prepreg production.
[0034] First, a prepreg is prepared. For example, as shown in Fig. 2(a), a sheet-like nonwoven fabric 10 is placed with its surface horizontal, and then polypropylene 20, which has been softened by heating to a temperature above its softening point, is applied from above, infiltrated, and fixed to produce a prepreg 30. It is preferable to use a nonwoven fabric 10 having a thickness of 50 µm or more and 500 µm or less.
[0035] For coating, a device called a melter can be used as a hot melt coater. The example of the device shown in Fig. 2(a) is a sheet-fed coater, in which the nonwoven fabric 10 is fixed and a spray nozzle part M1 is moved over the entire nonwoven fabric 10 to coat the nonwoven fabric 10 with polypropylene 20, thereby producing a prepreg 30.
[0036] The example of the device shown in Figure 2(b) is a roll-to-roll continuous impregnation device. By fixing a spray nozzle part M2 and moving the nonwoven fabric 10 from roll R1 to roll R2, polypropylene 20 can be applied to the entire nonwoven fabric 10 to produce prepreg 30. In the above-mentioned applicator, it is preferable to move either the applicator side or the nonwoven fabric side at a constant speed relative to the other during application.
[0037] The example of the device shown in Fig. 2(c) is also a continuous impregnation device using rolls. A discharge-type nozzle part M3 is fixed, and polypropylene 20 is supplied to a position between rolls R3 and R4. The polypropylene 20 is infiltrated into the nonwoven fabric 10 that is sandwiched between the rolls R3 and R4 and fed out. Using such a continuous impregnation device can improve the production efficiency of the prepreg 30.
[0038] The heated and softened polypropylene may be stored in a container, and the sheet-shaped textile may be immersed in the container (so-called "dipping in a bath"). The polypropylene thus impregnated in the textile is cooled and hardened to form a prepreg. In this case, it is preferable to move the textile continuously at a constant speed by rotating a roller or the like to pass through the polypropylene.
[0039] The sheet-like prepreg thus obtained preferably has a thickness of 100 μm or more and 1500 μm or less, and more preferably has a thickness of 100 μm or more and 500 μm or less.
[0040] The obtained sheet-like prepregs 30 are stacked and arranged according to a predetermined design, with the heat generating material 37 sandwiched between any of them, to form a stack (first stack). The arranged stack is then heated and pressed for thermocompression bonding. The heat generating material 37 includes a heat generating fiber 38 and a pair of electrodes 132 connected to both ends of the heat generating fiber 38. FIG. 3 is a perspective view showing the process of stacking and thermocompression bonding the prepregs. In the example shown in FIG. 3, a stack 40a in which four prepregs 31 to 34 are stacked with the heat generating material 37 sandwiched therebetween is heated and pressed from above and below. As a result, a sheet-like laminate is formed.
[0041] Since the heat generating material 37 has a greater effect closer to the inside (heating side), it can be disposed, for example, between the first prepreg 31 and the second prepreg 32 from the inside. It is also preferable that the heat generating fiber 38 is embedded in the laminate and the end of the electrode 132 is exposed from the laminate. This allows the exposed end to be connected to a terminal of a power source.
[0042] The heat generating fiber is formed by mixing organic fiber and carbon fiber. The organic fiber is, for example, cellulose or a mixture of cellulose and polyester. The carbon fiber preferably has a representative length of 3 mm or more and 6 mm or less. The carbon fiber is preferably contained in an amount of 10% by weight or more and 20% by weight or less with respect to the organic fiber. For example, a paper made by mixing cut carbon fiber with paper, or a paper made by mixing cut PET with paper, can be used. A paper made by mixing natural fiber cellulose with carbon fiber and then papermaking the mixture may be used. The heat generating fiber may be composed of only carbon fiber. The heat generating fiber may be not only a nonwoven fabric but also a woven fabric. For example, the heat generating fiber may be a woven fabric made of a heater wire, and the heater wire may be a conductive wire itself, or may be a combined wire made of an insulating wire and one or more conductive wires wound around the insulating wire. The combined wire includes a covering wire formed by providing a conductive wire around an insulating wire, and a twisted wire formed by intertwining an insulating wire and a conductive wire. The woven fabric may be woven with the heater wires as warp and weft lines, or may be woven with only weft lines. The pair of electrodes 132 are thin films having electrical conductivity. The pair of electrodes 132 are preferably tapes containing metal, such as aluminum tape or copper tape. An electrode such as a conductive tape can be connected to the heat generating fiber by using a conductive adhesive or pressure sensitive adhesive.
[0043] The thermocompression is preferably performed by using a hydraulic heat press or a multi-stage press at a predetermined temperature or higher and a predetermined pressure or higher. The predetermined temperature is a temperature lower than the melting point and higher than the softening point of polypropylene. For example, it is preferable to heat to 140°C or higher and 160°C or lower. The predetermined pressure is preferably 1.5 MPa or higher and 2.5 MPa or lower. This allows the polypropylene to infiltrate and bond to the mesh in the textile, creating an anchor effect and firmly integrating the heater.
[0044] In this way, the prepreg is heat-pressed at a temperature higher than the softening point and lower than the melting point of polypropylene, so that the polypropylene that has infiltrated into the mesh is continuously integrated and firmly fixed into the mesh structure by the anchor effect. As a result, the PP-FRP heater 100 sheet is produced as a laminated sheet in which multiple nonwoven fabrics are firmly bonded by the polypropylene that has permeated throughout.
[0045] The PP-FRP heater 100 has excellent shape stability, and when heat-pressed at a temperature of 100°C to 150°C and a pressure of 2.5 MPa or less, the absolute value of the rate of change in length before and after pressing is 1% or less. In this way, the PP-FRP heater is less likely to change in dimensions before and after pressing. Therefore, the PP-FRP heater can be formed as designed, making it easy to apply.
[0046] After lamination by thermocompression, the PP-FRP heater 100 can be naturally cooled to stabilize its shape. Therefore, it is possible to mass-produce them simultaneously using a multi-stage press. A multi-stage press is a heat press machine that has a middle heat plate in addition to upper and lower heat plates, and has multiple openings as stages to sandwich the material. By sandwiching the material between multiple stages and applying pressure with a press while heating, multiple PP-FRP heaters can be formed at the same time. PP-FRP heaters have a composite layer structure in which polypropylene is infiltrated into the textile and fixed, and therefore have high strength.
[0047] The sheet of the PP-FRP heater 100 obtained in the above steps is then shaped and trimmed. Figures 4(a) to 4(d) are cross-sectional views showing the shaping and trimming steps. First, the laminate 41 is softened by heating. Then, as shown in Figure 4(a), the laminate 41 is placed between a male mold D1 and a female mold D2.
[0048] Next, the male mold D1 and the female mold D2 are clamped together as shown in FIG. 4(b). As a result, the laminate 41 is shaped. After clamping, the male mold D1 and the female mold D2 are opened as shown in FIG. 4(c), and the obtained molded body 42 is released. Then, as shown in FIG. 4(d), unnecessary parts are removed by trimming to obtain a molded body 43. Even after such molding, the change rate of length from the laminate 41 to the molded body 43 is within 1%, and the PP-FRP heater 100 has excellent shape stability. The obtained PP-FRP heater 100 is further cut as appropriate depending on the application. The PP-FRP heater 100 can be applied to various products using polypropylene as a surface layer material. For example, a PVB sheet can be sandwiched between sheet-like textiles such as nonwoven fabrics from both sides and compressed at 130°C or higher to be integrated, and then compressed to the PP-FRP heater 100 at 110°C. In this case, it is possible to prevent the polypropylene from seeping out onto the surface, and to widen the range of temperature options for thermocompression bonding.
[0049] [Second embodiment] In the above embodiment, only the prepregs are layered and thermocompression bonded, but the prepregs and textiles may be layered alternately and thermocompression bonded. Fig. 5 is a perspective view showing the process of thermocompression bonding the prepregs and textiles. The textiles layered alternately with the prepregs are woven fabrics or nonwoven fabrics.
[0050] In the example shown in Fig. 5, two prepregs 35-36 and two textiles 51-52 are alternately stacked to form a laminate 40b (second laminate) with a heat-generating material sandwiched between them, and the laminate 40b is thermocompression bonded. As a result, a sheet-like laminate is formed. Thermocompression bonding in this case can also be performed using the same equipment and under the same temperature conditions as in the first embodiment.
[0051] In this case, too, the prepreg and the textile are thermocompression bonded at a temperature higher than the softening point and lower than the melting point of polypropylene, so that the polypropylene in the prepreg also permeates into the mesh of the textile and is firmly fixed to the mesh by the anchor effect. As a result, the PP-FRP heater 100 sheet is produced as a laminated sheet in which the prepreg and the textile are bonded by the polypropylene that has permeated continuously.
[0052] [Third embodiment] In the above embodiment, the PP-FRP heater is formed only by the sheet in which the planar heating layer is embedded, but it may further include a layer having a heat insulating function on the outside (opposite the heating side). Figures 6(a) and (b) are cross-sectional views showing PP-FRP heaters 200a and 200b each including an aluminum layer, a heat insulating layer, and an aluminum layer.
[0053] In the PP-FRP heater 200a, an aluminum layer 250 is bonded to the outside of the PP-FRP heater 100. That is, the aluminum layer 250 is provided on one main surface side of a plurality of composite layers. This makes it possible to reflect radiation from the heat-generating fibers and amplify heating on the other side.
[0054] The aluminum layer 250 is preferably made of aluminum foil, and preferably has a plurality of aluminum foils. When a plurality of aluminum foils are used, gaps are generated between the aluminum foils, and the reflectance of the radiation generated from the heat generating fiber can be increased.
[0055] When a plurality of aluminum foils are laminated to form an aluminum layer, it is preferable that a resin layer having a plurality of holes that do not overlap each other is formed between the plurality of aluminum foils. This allows the voids generated between the plurality of aluminum foils to increase the reflectance of radiation and improve the heat insulating effect. The resin layer can be, for example, a resin film such as PET, which functions as a support for creating an air layer. The resin layer may be formed by stacking PP-FRP sheets.
[0056] The shape of the hole is preferably a circle, but may be a polygon such as a square. The hole diameter is preferably 2 mm or more and 18 mm or less. If the hole diameter is less than 2 mm, the adhesion of the aluminum foil is insufficient. If the hole diameter is greater than 18 mm, the adhesive will get into the aluminum foil and there will be no gaps. The aluminum foil may have a thickness of 1 μm or more and 1 mm or less. If it is thinner than 1 μm, sufficient reflection will not be obtained, and if it is thicker than 1 mm, the cost-effectiveness will be low. The aluminum foil may be adhered in sheet form or formed by vapor deposition.
[0057] The aluminum layer 250 and the composite layer 114 can be bonded together with an adhesive. A thermosetting resin can be used as the adhesive. For example, an adhesive having hot melt and heat curing properties, such as HM30 (manufactured by PANAC Corporation), is preferable. In this case, the adhesive can be cured at a temperature of 100°C or higher and 150°C or lower.
[0058] The PP-FRP heater 200b has a heat insulating layer 260 and an aluminum layer 250 bonded to the outside of the PP-FRP heater 100. The heat insulating layer 260 is made of a sheet-like material with low thermal conductivity. For example, a fibrous material containing voids, such as paper, is preferable. Paper mixed with inorganic particles with low thermal conductivity may also be used.
[0059] The PP-FRP heater 200a can be constructed by bonding an aluminum layer 250 to the outside of the PP-FRP heater 100. Fig. 7 is a perspective view showing the PP-FRP heater 100, aluminum foil 251, and resin sheet 252 before bonding.
[0060] When two aluminum foils 251 are bonded to the PP-FRP heater 100 as shown in FIG. 7, a resin sheet 252 with staggered holes can be placed between the aluminum foils 251. The resin sheet 252 can be a polyethylene naphthalate sheet or a PP-FRP sheet. The holes are arranged in a staggered arrangement to generate gaps between the aluminum foils. The gaps can increase the reflectance of radiation. When a composite layer of PP-FRP with high shape stability is used, the holes can be prevented from shifting even when processed at a high temperature of 100° C. or higher. The PP-FRP heater 200b can also be formed by bonding each layer to the composite layer using an adhesive, as in the case of the PP-FRP heater 200a.
[0061] The thickness of the PP-FRP heater is preferably 60 μm or more and 1 mm or less. In the above example, the aluminum layer and the heat insulating layer are bonded to the composite layer, but the number of composite layers may be increased and the aluminum layer and the heat insulating layer may be embedded between the composite layers. A resin such as polypropylene may be injection molded on the outside (opposite side to the heating side) of the PP-FRP heater. A layer to be bonded made of a thermoplastic resin or a decorative layer made of one of wood, suede, and metal mesh may be bonded to the inside or outside of the PP-FRP heater via a bonding layer having PVB.
[0062] [Fourth embodiment] [Configuration of composite laminate heater] In the above embodiment, the composite laminate heater is composed of a composite layer and a sheet heating layer, but the composite laminate heater may also be composed of a film layer, a composite layer, a base resin layer and a sheet heating layer.
[0063] 8 is a cross-sectional view showing a composite laminate heater 300. The composite laminate heater 300 includes a main body layer 340 and a base resin layer 320. The main body layer 340 is composed of film layers 311 and 313, composite layers 312 and 314, and a sheet heating layer 130. The sheet heating layer 130 is provided between the film layer 311 and the composite layer 312. The film layers 311 and 313 and the composite layers 312 and 314 are laminated alternately.
[0064] The film layers 311 and 313 are layers formed by thermoplastic resin films being thermocompressed. The thickness is uniform because a certain percentage of the thermoplastic resin film having a uniform thickness is infiltrated into the fibers of the nonwoven fabric by thermocompression.
[0065] The composite layers 312, 314 are formed of a nonwoven fabric and a thermoplastic resin that is infiltrated and fixed into the mesh of the nonwoven fabric. The nonwoven fabric is preferably a spunbond nonwoven fabric, but may also be a paper-based nonwoven fabric containing polyester or a felt.
[0066] The composite layers 312, 314 are in contact with the film layers 311, 313, and the thermoplastic resin continuing from the film layers 311, 313 permeates into the mesh of the nonwoven fabric. The anchor effect firmly bonds the composite layers 312, 314 to the film layers 311, 313. This makes it possible to form a plate-like member that is firmly integrated with the thermoplastic resin.
[0067] Base resin layer 320 is formed from a thermoplastic resin by injection molding, and is in contact with composite layer 314. Composite layers 312, 314 are both fixed by infiltrating the thermoplastic resin into the mesh of the nonwoven fabric from both sides.
[0068] In the composite laminate heater 300, the main body layer 340 preferably has a four-layer structure composed of film layers 311, 313 and composite layers 312, 314. A four-layer structure or more can improve the strength of the composite laminate heater and stabilize its shape. On the other hand, a four-layer structure or less makes it easier to mold.
[0069] However, the main body layer may be a two-layer structure consisting of only a film layer and a composite layer, or may be a six-layer structure or more. In either case, the layer closest to the surface is the film layer, and the layer closest to the base resin layer is the composite layer.
[0070] The edge of the composite laminate heater 300 is preferably formed by covering the main body layer 340 with the base resin layer 320. This allows the edge 310a of the main body layer 340 to be covered with the base resin layer 320, enabling reliable circuit insulation. In this way, the heat generating fiber layer 131 and the electrodes 132 can be entirely buried without being exposed. This allows a structure in which only a portion of the electrodes 132 is exposed, or a non-contact current-carrying structure without an extraction electrode, preventing leakage current due to water penetration, etc.
[0071] When forming a composite laminate heater in this manner, it is preferable to use polypropylene as the thermoplastic resin. PVB (polyvinyl butyral) may also be used as the thermoplastic resin. PVB can be easily softened and can infiltrate into the gaps between fibers. It is preferable to add a plasticizer or the like to PVB and use it as hot-melt PVB. In that case, it is preferable to set the melting temperature to 120°C.
[0072] [Manufacturing method of composite laminate heater] A method for manufacturing the composite laminate heater 300 configured as above will be described. The composite laminate heater 300 is manufactured through the steps of thermocompression bonding, preform molding, trimming, and injection molding. The arrangement of each material when thermocompression bonding the thermoplastic resin film and the nonwoven fabric is the same as that in Fig. 5, except that the prepreg sheet is replaced with the thermoplastic resin film.
[0073] First, the thermoplastic resin film and the nonwoven fabric are arranged in layers according to a predetermined design and heat-pressed. For example, a layered body is formed by stacking the thermoplastic resin film, the nonwoven fabric, the thermoplastic resin film, and the nonwoven fabric in this order from the top. A planar heating layer is arranged between the thermoplastic resin film and the nonwoven fabric. Then, the layered body is heat-pressed from above and below to form a sheet-like laminate. The heat-pressing can be performed using a hydraulic heat press or a multi-stage press. When polypropylene is used as the thermoplastic resin, the layered body is pressed while being heated to a temperature below the melting point and above the softening point. Specifically, a temperature of 140°C to 160°C is preferable.
[0074] In this way, by performing heat compression bonding at a temperature higher than the softening point and lower than the melting point, the thermoplastic resin forming the film softens, infiltrates into the mesh of the nonwoven fabric, and is firmly fixed to the mesh by the anchor effect, resulting in a laminated sheet in which the thermoplastic resin film layer is firmly bonded to the composite layer having fibers.
[0075] When using a polypropylene film, it is preferable to use one having a thickness of 100 μm or more and 1500 μm or less, and more preferably to use one having a thickness of 100 μm or more and 500 μm or less. Also, it is preferable to use a nonwoven fabric having a thickness of 50 μm or more and 500 μm or less. As a result of the above-mentioned thermocompression bonding, a laminated sheet corresponding to the main body layer 340 of the composite laminate heater 300 is obtained.
[0076] Then, the steps of preform molding and trimming are performed. These steps are performed in the same manner as in the first embodiment, as shown in Figures 4(a) to 4(d). By removing unnecessary parts by trimming, the cut surface by trimming can be covered with injected thermoplastic resin by the subsequent injection molding.
[0077] 9(a) and (b) are cross-sectional views showing the injection molding process. As shown in FIG. 9(a), the preform 83 is placed in a female injection mold M12 with the thermoplastic resin film side facing up, and the female mold M12 is then moved toward a male injection mold M13. At the same time, the injection hole M15 of the injector is pressed against the injection molding hole M16 of the male mold M13.
[0078] Then, the injection screw M11 is rotated clockwise to inject the raw material P1 for the base resin layer in the tank T1 into the space defined by the preform 83 and the male injection mold M13. That is, the thermoplastic resin is injection molded onto one main surface that forms the surface of the laminate sheet and the other main surface that is formed of the nonwoven fabric on the opposite side.
[0079] The molten thermoplastic resin, which is the raw material P1 of the base resin layer, is heated and melted by an injection molding machine M10, and injected into a female mold M12 to which a preform molded body 83 is attached, and is fixed by infiltrating into the gaps between the fibers of the nonwoven fabric layer. At this time, the thermoplastic resin infiltrates into the gaps between the fibers of the nonwoven fabric, and the adhesion between the preform molded body 83 and the base resin layer 320 becomes stronger due to the shrinkage of the raw material P1 when it is cooled and solidified.
[0080] Then, as shown in FIG. 9(b), after the injection-molded base resin layer 320 cools and solidifies, the injector and the male mold M13 for injection molding are separated from the female mold M12, and the composite laminate heater 300 is taken out. The obtained composite laminate heater 300 is appropriately cut according to the application. The obtained composite laminate heater 300 can be applied to various products using thermoplastic resin as a surface layer material. Note that the composite laminate heater 300 can also be provided with an aluminum layer or a heat insulating layer on the outer layer, like the PP-FRP heater 100. In that case, it is also possible to omit the base resin layer 320 and provide an aluminum layer or a heat insulating layer.
[0081] [Automotive applications] Composite laminate heaters including the above-mentioned PP-FRP heaters are effective as heaters to be installed inside automobiles. For example, they can be installed below the steering wheel (at the driver's feet) to heat the interior of the vehicle. Composite laminate heaters are easy to handle because the heat-generating fiber is integrated with the composite resin, and the heater installation process can be omitted. In addition, because they are manufactured using textiles, they are strong, have excellent shape stability, and are easy to incorporate into mass production. They also have high thermal efficiency and are excellent in terms of power saving. They are particularly useful for electric vehicles (EVs).
[0082] [Application to toilet seats] The composite laminate heater can also be used in toilet seats. The toilet seat is a so-called heated toilet seat, and the surface temperature can be maintained at about 40°C by passing an electric current through the heat-generating fiber. Because the composite laminate heater uses heat-generating fiber, it has higher thermal efficiency than toilet seats that use conventional heater wires. In addition, heated toilet seats with a surface formed from polypropylene, which has excellent resistance to hydrochloric acid, can be washed as is. A planar heating layer can be provided directly under the composite layer on the surface to facilitate heat conduction to the surface. The surface may further be provided with a surface material that has been treated to be pleasant to the touch, such as with a raised nap.
[0083] [others] The composite laminate heater can also be used by adhering to a composite laminate of PP film and nonwoven fabric, or a composite laminate of a resin film such as PMMA, PET, PC, etc., and nonwoven fabric. In that case, PVB resin may be used as an adhesive to bond the resin film to the nonwoven fabric. Furthermore, ABS resin, PP, PC, PMMA, or other resin may be injection molded on the back side as the base resin.
[0084] [Fifth embodiment] In the above embodiment, the layer having a heat insulating function is adhered to the composite layer in which the planar heating layer 130 is embedded, but the layer having a heat insulating function may be adhered only to the PP-FRP member, that is, to a composite layer without the planar heating layer 130. Figures 10(a) and (b) are cross-sectional views showing PP-FRP heat insulating members 400a and 400b each having an aluminum layer and a heat insulating layer and an aluminum layer.
[0085] In the PP-FRP heat insulating member 400a, an aluminum layer 250 is provided on one side of the composite layers 111-114. The aluminum layer 250 is adhered to the composite layers 111-114 with an adhesive, as in the third embodiment. The aluminum layer 250 is preferably made of a plurality of aluminum foils. The adhesion between the aluminum layer 250 and the composite layers 111-114 and the configuration of the aluminum layer 250 are the same as in the third embodiment.
[0086] In the PP-FRP insulation member 400b, a thermal insulation layer 260 and an aluminum layer 250 are provided on one side of the composite layers 111-114. The thermal insulation layer 260 is adhered to the composite layers 111-114, and the aluminum layer 250 is further adhered to the thermal insulation layer 260. In this case, too, the adhesion and configuration of the thermal insulation layer 260 and the aluminum layer 250 are similar to those in the third embodiment.
[0087] [Application to wall materials, etc.] Such PP-FRP heat insulating members 400a, 400b can be used as flat building materials. For example, by using the PP-FRP heat insulating members 400a, 400b as a wall material inside a house, the inside of the room can be kept warm and cold at the bottom can be prevented. In this case, the thickness of the PP-FRP heat insulating members 400a, 400b is preferably 60 μm or more and 2 mm or less, and more preferably 60 μm or more and 1 mm or less. When using the PP-FRP heat insulating members 400a, 400b as a wall material, it is preferable to use a non-flammable material such as a non-flammable polyester woven fabric as the textile. Alternatively, inorganic or organic flame-retardant particles such as aluminum hydroxide, halogen-based or antimony trioxide may be mixed with polypropylene.
[0088] It can also be used for toilet seats and decorative components. PP-FRP heat insulation components can also be used as a backer for composite laminates. Composite laminates can be made of resin films such as PP, PMMA, PET, PC, etc., and nonwoven fabric. PVB resin can be used as an adhesive to bond the resin film and nonwoven fabric. ABS resin, PP, PC, PMMA, or other resins can be injection molded on the back side as the base resin.
[0089] [Sixth embodiment] As mentioned above, some composite laminate heaters can be manufactured using hot melt prepregs (PP-FRP heaters) or by compression bonding using PP film, but it is also possible to manufacture embedded heaters by completely embedding these composite laminate heaters in polypropylene.
[0090] FIG. 11 is a cross-sectional view showing the configuration of an embedded heater 500. As shown in FIG. 11, the embedded heater 500 includes a covering portion 510 and a PP-FRP heater 100. The covering portion 510 is made of polypropylene, and the PP-FRP heater 100 is embedded therein. The PP-FRP heater 100 is covered without any gaps by the covering portion 510, and only the electrode 132 is taken out to the outside of the covering portion 510. The heater can be heated by applying a voltage from here. By providing the covering portion 510, it is possible to improve corrosion resistance against cleaning agents such as hydrochloric acid.
[0091] Such an embedded heater 500 can be produced by placing a composite laminate heater in hollow molds M22 and M23, injecting polypropylene resin into the hollow of the molds M22 and M23, and hardening it. Figures 12(a) and 12(b) are a side cross-sectional view and a plan cross-sectional view, respectively, showing a scene in the manufacturing process of the embedded heater 500. As shown in Figures 12(a) and 12(b), first, a plate-shaped PP-FRP heater 100 is fixed in the mold M22 in a state where it is raised from the bottom of the mold by a plurality of supports M22a. At that time, the electrodes 132 of the PP-FRP heater 100 are exposed from the hollow. Note that the dashed line 12b shown in Figure 12(a) and the dashed line 12a shown in Figure 12(b) show the cross sections shown in Figures 12(b) and 12(A), respectively.
[0092] It is preferable to provide holes 105 that communicate with the front and back of the main surface of the PP-FRP heater 100. Because a planar heater is used, the effect on the heater's function is limited even if holes are provided. The support portions M22a are formed in a protrusion shape, and providing four of them, for example, allows the PP-FRP heater 100 to be stably supported.
[0093] The polypropylene is melted in advance and injected into the mold from the injection port M23a. The temperature of the melted polypropylene is 200°C or higher and 250°C or lower, and preferably 220°C. The type of polypropylene used has a melting point of 140°C or higher and 150°C or lower. The melting point of polypropylene increases as the length of its molecular chain increases and as the amount of plasticizer and tackifier added decreases.
[0094] It is preferable to inject polypropylene from vertically above, and if the polypropylene has a suitable degree of fluidity when melted, it will pass through the outer periphery and holes 105 of the PP-FRP heater 100 and reach every corner vertically below inside the hollow. The embedded heater 500 can be formed by gradually cooling the polypropylene after filling. It is preferable to seal the recesses left behind after the support portions M22a are removed.
[0095] In the above example, the PP-FRP heater 100 is used as the composite laminate heater, but a composite laminate heater 300 that can be manufactured by pressure bonding using a PP film may also be used. The composite laminate heater used in this case may be the composite laminate heater 300 itself, or may not have the base resin layer 320. In the above example, a polypropylene covering layer is provided by injection molding to cover the composite laminate heater, but a covering layer may be provided using a heat-shrinkable polypropylene film.
[0096] [Application to toilet seats] The embedded heater is suitable for use in toilet seats. The toilet seat is a so-called heated toilet seat, and the surface temperature can be maintained at about 40°C by passing an electric current through the heat-generating fibers. The heated toilet seat, whose surface is formed with a polypropylene covering that has excellent resistance to hydrochloric acid, can be washed as is. The surface may further be provided with a surface layer that has been treated to be pleasant to the touch, such as with a raised nap.
[0097] [Experiment 1] A prepreg was prepared by heating and softening hot melt polypropylene (HMPP) with added tackifier, and applying the softened polypropylene to a nonwoven fabric made of spunbond polyester. For the nonwoven fabric, Toray Industries, Inc.'s nonwoven fabric N2070-6S was used. For convenience, the prepreg using hot melt polypropylene (PP 80 wt%, tackifier 20 wt%) with a low melting point (95°C) is called "prepreg 2". The obtained prepreg was used to layer materials in the following combinations. [Table 1]
[0098] The black nonwoven fabric is denser and harder than normal nonwoven fabrics. Toray Industries, Inc.'s nonwoven fabric G2200-BKO was used as the black nonwoven fabric. The coarse white nonwoven fabric is less dense than normal nonwoven fabrics. Toray Industries, Inc.'s nonwoven fabric D5100 was used as the coarse white nonwoven fabric.
[0099] A square with a side length of approximately 100 mm was drawn on the surface of the overlapping sample with a 0.5 mm felt tip pen, and the length of each side was measured twice and averaged. The length was measured to the nearest 0.01 mm using a digital caliper (same below). Each sample was pressed for 1 minute using a hydraulic heat press to perform thermocompression bonding. When thermocompression bonding of laminate sample 3, a 15 mm spacer was inserted to prevent the sample from becoming too flat and crushed, which deviates from the purpose of bonding.
[0100] After the thermocompression bonding, the length of each side of the square was measured twice and the results were averaged. The change in the length of the square was within 1% for all of the laminate samples 1 to 3 obtained as PP-FRP members. The measurement results are shown in the table below. [Table 2]
[0101] Next, a prepreg using hot melt polypropylene with a high melting point (155°C) (PP 90wt%, tackifier 10wt%) and a prepreg using hot melt polypropylene with a low melting point (95°C) were laminated, and the sample was sandwiched between nonwoven fabric at both ends and heat-pressed. For convenience, the prepreg using hot melt polypropylene with a high melting point (155°C) is called "prepreg 1". The materials were layered in the following combinations. [Table 3]
[0102] A square with sides of approximately 100 mm was drawn with a felt tip pen on the surface of the overlapping sample, and the length of each side was measured twice and averaged. Each sample was thermocompression bonded by pressing it for one minute using a hydraulic heat press. After thermocompression bonding, the length of each side of the square was measured twice and averaged. For both laminate samples 4 and 5 obtained as PP-FRP components, the change in the length of the square was within 1%. The measurement results are shown in the table below. [Table 4]
[0103] Next, a sample was laminated with a prepreg made of hot-melt polypropylene with a high melting point (155°C) and a nonwoven fabric, and the laminate was heat-pressed. The materials were laminated in the following combinations: [Table 5]
[0104] A square with sides of approximately 100 mm was drawn with a felt tip pen on the surface of the overlapping sample, and the length of each side was measured twice and averaged. Each sample was thermocompression bonded by pressing it for one minute using a hydraulic hot press. After thermocompression bonding, the length of each side of the square was measured twice and averaged. For both laminate samples 6 and 7 obtained as PP-FRP components, the change in the length of the square was within 1%. The measurement results are shown in the table below. [Table 6]
[0105] As described above, the change in length before and after thermocompression was within 1% for all laminate samples, demonstrating extremely excellent shape stability. In particular, when prepregs using low-melting-point hot-melt polypropylene were laminated and thermocompression was performed at a relatively low temperature of 120°C or less, the change was 0.4% or less. These results show that not only is the PP-FRP component stable in shape during manufacture, but that the manufactured PP-FRP component also has an extremely excellent shape stability, with a change rate of more than 1% when hot-pressed at temperatures between 100°C and 150°C and at a pressure of 2.5 MPa or less.
[0106] [Experiment 2] For comparison, a 100% polypropylene (PP) film with a thickness of 0.5 mm was heat-treated for 1 minute. The heat treatment was performed under the following temperature, pressure and measurement conditions. Before heat treatment, a square with approximately 100 mm on each side was drawn on the surface of the sample with a felt tip pen, and the length of each side was measured twice and averaged. In addition, after heat treatment, the length of each side of the square was measured twice and averaged to calculate the rate of change. [Table 7]
[0107] It was found that the shape of polypropylene film samples 4 and 6 changed when a pressure of 2 MPa was applied at a temperature above the softening point. The rate of change exceeded 1%, indicating that sufficient shape stability could not be obtained even if a laminate was made by compressing polypropylene films.
[0108] [Experiment 3] The PP-FRP member obtained in Experiment 1 was cut and the cut surface was observed under a microscope. Figure 13 is a micrograph of the cut surface. As shown in Figure 13, it can be seen that a PP-FRP member 700 has been formed in which a composite layer 711 derived from a prepreg and a composite layer 712 derived from a nonwoven fabric are laminated. It can be seen that polypropylene 711b that has infiltrated into nonwoven fabric 711a is continuously integrated.
[0109] [Experiment 4] A planar heating layer was placed between the first and second layers of a four-layer composite, a PEN sheet with a 5mm hole was sandwiched between aluminum foil, and this laminate was attached to the fourth layer to create a composite laminate heater. There was no misalignment in the position of the holes in the resin layer between the aluminum foils of the resulting composite laminate heater. When a current of 12V and 4A was applied to the resulting composite laminate heater, the temperature of the surface on the first layer side immediately rose to 60°C. There was almost no increase in temperature on the reverse surface.
[0110] On the other hand, as a comparative example, a heat generating material was sandwiched between the first and second sheets of four polypropylene films, which were then thermocompressed, and a PEN sheet with a 5 mm hole was sandwiched between aluminum foils, and this laminate was adhered to the fourth sheet. The heater obtained as the comparative example had an uneven shape and wrinkles on the surface. In addition, the position of the resin hole between the aluminum foils was shifted by 1 mm or more. When a current of 12 V and 4 A was passed through the heater of the comparative example, the surface temperature rose. [Explanation of symbols]
[0111] 10. Nonwoven Fabrics 20 Polypropylene 30~36 Prepreg 37 Heat generating materials 38 Heat-generating Fibers 40a, 40b Superimposed body 41 Laminate 42-43 Molded body 51~52 Textile 100 PP-FRP heater 105 holes 111~114 Composite layer 130 Planar heating layer 131 Heat generating fiber layer 132 Electrode 200a, 200b PP-FRP heater 211~212 Composite layer 231 Conductor 250 Aluminum Layer 251 Aluminum foil 252 Resin Sheet 260 Insulation Layer 300 Composite Laminated Heater 400a, 400b PP-FRP insulation material 200 Composite Materials 340 Main Layer 310a edge 311, 313 Film layer 312, 314 composite layer 320 Base resin layer 500 Buried heater 510 Covering part 700 PP-FRP materials 711 Composite layer 711a Non-woven fabric 711b Polypropylene 712 Composite layer M1~M3 Nozzle part R1~R4 Role M10 injection molding machine M11 injection screw M12 female mold M13 Male mold M15 injection hole M16 injection molding hole T1 Tank P1 raw material M22, M23 molds M22a support part M23a ejection port
Claims
1. A plurality of composite layers formed by infiltrating and bonding polypropylene into the mesh structure of a sheet-like textile; a sheet-shaped heating layer including a sheet-shaped heating fiber, a pair of electrodes connected to the heating fiber, and polypropylene infiltrated and fixed in the mesh structure of the heating fiber, the sheet-shaped heating layer being provided between adjacent textiles in the plurality of composite layers; A composite laminate heater characterized in that the multiple composite layers and the sheet heating layer are laminated, and the polypropylene in the multiple composite layers and the sheet heating layer is filled into a mesh structure to be integrated.
2. A film layer formed of polypropylene; a composite layer having a sheet-like textile and polypropylene infiltrated and bonded to the mesh of the textile; a sheet-shaped heat generating layer provided between the film layer and the composite layer, the sheet-shaped heat generating layer having a heat generating fiber, a pair of electrodes connected to the heat generating fiber, and polypropylene infiltrated and fixed in the mesh structure of the heat generating fiber; A composite laminate heater, characterized in that the film layer and the composite layer are laminated together, and the polypropylene contained in the film layer and the composite layer are integrated together.
3. 3. The composite laminate heater according to claim 1, wherein the pair of electrodes are connected to opposite edges of the heat generating fiber.
4. 2. The composite laminate heater according to claim 1, further comprising an aluminum layer provided on one main surface side of said plurality of composite layers.
5. 5. The composite laminate heater according to claim 4, wherein the aluminum layer is formed by laminating a plurality of aluminum foils, and gaps are provided between the plurality of aluminum foils.
6. 6. The composite laminate heater according to claim 5, wherein a resin layer having holes that do not overlap each other is formed between the plurality of aluminum foils.
7. 3. The composite laminate heater according to claim 2, further comprising an aluminum layer provided on one main surface side of the laminate of said film layer and said composite layer.
8. 8. The composite laminate heater according to claim 7, wherein the aluminum layer is formed by laminating a plurality of aluminum foils, and gaps are formed between the plurality of aluminum foils.
9. 9. The composite laminate heater according to claim 8, wherein a resin layer having holes that do not overlap each other is formed between the plurality of aluminum foils.
10. 3. The composite laminate heater according to claim 1, further comprising a cover layer made of polypropylene and covering said composite layer.
11. Providing a plurality of prepreg sheets having a nonwoven fabric and polypropylene impregnated into the nonwoven fabric; a step of stacking the prepreg sheets with a sheet-shaped heat generating fiber and a pair of electrodes connected to the heat generating fiber sandwiched therebetween to form a first laminate; and heat pressing the first laminate at a predetermined temperature or higher and at a predetermined pressure or higher.
12. Providing a plurality of prepreg sheets and sheet-like textiles having a woven fabric and polypropylene impregnated into the woven fabric; a step of alternately stacking the prepreg sheet and the textile with a sheet-like heat generating fiber and a pair of electrodes connected to the heat generating fiber sandwiched therebetween to form a second laminate; and heat pressing the second laminate at a predetermined temperature or higher and at a predetermined pressure or higher.
13. a step of sandwiching a sheet-shaped heat generating fiber and a pair of electrodes connected to the heat generating fiber between a polypropylene film and a textile, and alternately stacking the polypropylene film and the textile to form a laminate; and heat pressing the laminate at a predetermined temperature or higher and at a predetermined pressure or higher.
Citation Information
Patent Citations
Planar heating element and manufacturing method of the same
JP2021012814A