Analytical method of lithium composite oxide

By analyzing lithium composite oxides through chemical calculations and experiments, the structure and efficiency of substituted lithium composite oxides are clarified, resulting in improved positive electrode materials for lithium ion secondary batteries with enhanced safety and performance.

JP2024159898AActive Publication Date: 2024-11-08SEMICON ENERGY LAB CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024139946
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-01-31
Filing Date
2024-08-21
Publication Date
2024-11-08
Estimated Expiration
2040-01-22

AI Technical Summary

Technical Problem

Existing methods fail to clarify the structure of lithium composite oxides with substituted elements, hindering improvements in capacity, cycle characteristics, charge/discharge characteristics, reliability, safety, and cost of lithium ion secondary batteries.

Method used

A method involving chemical calculations and experiments to analyze the substitution positions of Ni and Mg atoms in lithium composite oxides, using the GGA+U(DFT-D2) method to determine stabilization energy and cation occupancy, combined with measurements to evaluate the crystal structure and charge/discharge efficiency.

Benefits of technology

Enables detailed analysis of lithium composite oxide structures, leading to the development of positive electrode active material particles with reduced deterioration, enhancing the safety and performance of power storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159898000001_ABST
    Figure 2024159898000001_ABST
Patent Text Reader

Abstract

To provide an analytical method of lithium composite oxide.SOLUTION: Disclosed is an analytical method of substitution sites of Ni atom and Mg atom in a compound represented by a chemical formula Li(1-x-y)Co(1-a-b)Ni(x+a)Mg(y+b)O2, wherein the analytical method includes: a first calculation step of calculating a stabilization energy obtained when Ni atom and Mg atom are replaced by a desired Li atom or Co atom included in LiCoO2 crystal; a second calculation step of calculating a stabilization energy of the compound represented by the chemical formula on changing cation occupancy in Li sites; and a first measurement step of measuring the first charge-discharge efficiency and the n-th charge-discharge efficiency of the compound represented by the chemical formula. Here, n is an integer of 2 or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] One embodiment of the present invention relates to a method for analyzing a lithium composite oxide, or to an object or a manufacturing method. Alternatively, the present invention relates to a process, a machine, a manufacture, or a composition of matter. One embodiment of the present invention relates to a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, or an electronic device, or a manufacturing method thereof.

[0002] In this specification, the term "power storage device" refers to elements and devices in general that have a power storage function, including, for example, storage batteries (also called secondary batteries) such as lithium ion secondary batteries, lithium ion capacitors, and electric double layer capacitors.

[0003] In addition, in this specification, electronic devices refer to devices in general that have a power storage device, and electro-optical devices that have a power storage device, information terminal devices that have a power storage device, and the like are all electronic devices. [Background technology]

[0004] In recent years, various types of power storage devices, such as lithium-ion secondary batteries, lithium-ion capacitors, and air batteries, have been actively developed. In particular, the demand for high-output, high-capacity lithium-ion secondary batteries has rapidly expanded in conjunction with the development of the semiconductor industry, and they are now indispensable in the modern information society as a rechargeable energy source, as they are used in portable information terminals, such as mobile phones, smartphones, and notebook computers, portable music players, digital cameras, medical equipment, and next-generation clean energy automobiles, such as hybrid electric vehicles (HEVs), electric vehicles (EVs), and plug-in hybrid electric vehicles (PHEVs).

[0005] Therefore, in order to improve the cycle characteristics and increase the capacity of lithium ion secondary batteries, improvements in the positive electrode active material have been investigated (Patent Document 1 and Patent Document 2).

[0006] Furthermore, characteristics required of power storage devices include safety in various operating environments and improved long-term reliability. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2012-018914 A [Patent Document 2] JP 2016-076454 A [Non-patent literature]

[0008] [Non-Patent Document 1] Toyoki Okumura et al, “Correlation of lithium ion distribution and X-ray absorption near-edge structure in O3- and O2-lithium cobalt oxides from first-principle calculation”, Journal of Materials Chemistry, 2012, 22, p.17340-17348 [Non-Patent Document 2] Motohashi, T. et al, “Electronic phase diagram of the layered cobalt oxide system LixCoO2(0.0≦x≦1.0)”, Physical Review B, 80(16);165114 Summary of the Invention [Problem to be solved by the invention]

[0009] There is a demand for improvements in various aspects of lithium ion secondary batteries and the positive electrode active materials used therein, such as capacity, cycle characteristics, charge / discharge characteristics, reliability, safety, and cost. ODevelopment is underway of a lithium composite oxide LiMO2 (where M is two or more metals including Co) in which part of the O2 is replaced with a different element.

[0010] However, because the amount of the above-mentioned substitution elements is so small, a method for clarifying the structure of lithium composite oxides has not yet been developed. If the structure of lithium composite oxides could be clarified, it would be helpful in materials development and elucidation of the mechanisms behind charge / discharge characteristics and reliability.

[0011] In view of the above, an object of one embodiment of the present invention is to provide a method for analyzing a lithium composite oxide. Another object of one embodiment of the present invention is to provide positive electrode active material particles that are less deteriorated. Another object of one embodiment of the present invention is to provide a new positive electrode active material particle. Another object of one embodiment of the present invention is to provide a power storage device that is less deteriorated. Another object of one embodiment of the present invention is to provide a power storage device that is highly safe. Another object of one embodiment of the present invention is to provide a new power storage device.

[0012] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that it is possible to extract problems other than these from the description of the specification, drawings, and claims. [Means for solving the problem]

[0013] One aspect of the present invention is a compound of formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b)A method for analyzing the substitution positions of Ni atoms and Mg atoms in a compound represented by O2. In the chemical formula, x + y < 1 and a + b < 1, and x, y, a, and b each independently represent a real number from 0 to 1. A first calculation step of calculating the stabilization energy of a compound represented by the chemical formula obtained when Ni atoms and Mg atoms are each independently substituted for any Li atom or Co atom contained in the LiCoO2 crystal; a second calculation step of calculating the stabilization energy of a compound represented by the chemical formula when the cation occupancy of the Li site is changed; and a first measurement step of measuring the initial charge-discharge efficiency and the charge-discharge efficiency at the nth time (n is an integer of 2 or more) of a compound represented by the chemical formula. It is a method for analyzing the substitution positions of Ni atoms and Mg atoms.

[0014] In the above configuration, the measurement step includes at least a step of preparing a sample and a step of performing mechanical measurement. By combining calculation and measurement, the validity of the calculation result and the phenomenon predicted from the calculation result can be evaluated, so detailed analysis can be performed.

[0015] Also, in the above configuration, it is preferable to use the GGA+U(DFT-D2) method in the first calculation step and the second calculation step.

[0016] Also, in the above configuration, it is preferable to perform the calculation by changing the cation occupancy in the range of at least 80% or more and 100% or less.

[0017] Also, in the above configuration, it is preferable that n = 2.

[0018] Also, in the above configuration, in the above chemical formula, it is preferable that 0 < x + a ≤ 0.015 and 0 < y + b ≤ 0.06.

[0019] Also, in the above configuration, when Ni atoms and Mg atoms are substituted for the same type of atoms in the LiCoO2 crystal during the second calculation step, it is preferable to further include a step of calculating the stabilization energy when the same type of atoms are present in the same layer and in different layers in the LiCoO2 crystal, respectively. Effect of the Invention

[0020] According to one embodiment of the present invention, a method for analyzing a lithium composite oxide can be provided. Further, a positive electrode active material particle that is less deteriorated can be provided. Further, a novel positive electrode active material particle can be provided. Further, a power storage device that is less deteriorated can be provided. Further, a highly safe power storage device can be provided. Further, a novel power storage device can be provided. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a diagram illustrating an example of the crystal structure of LiCoO2. [Diagram 2] 2A and 2B are diagrams illustrating examples of the crystal structure of a lithium composite oxide. [Diagram 3] FIG. 3 is a diagram illustrating an example of a method for producing a positive electrode active material. [Figure 4] FIG. 4 is a diagram illustrating the crystal structure and magnetism of a conventional positive electrode active material. [Diagram 5] FIG. 5 is a diagram illustrating the crystal structure and magnetism of the positive electrode active material. [Figure 6] 6A and 6B are cross-sectional views of an active material layer in which a graphene compound is used as a conductive assistant. [Figure 7] 7A and 7B are diagrams illustrating a coin-type secondary battery. [Figure 8] 8A and 8B are diagrams for explaining a cylindrical secondary battery, FIG. 8C is a perspective view of a battery module, and FIG. 8D is a top view of the battery module. [Figure 9] 9A and 9B are diagrams illustrating an example of a secondary battery. [Figure 10] 10A1, 10A2, 10B1, and 10B2 are diagrams illustrating examples of a secondary battery. [Figure 11] 11A and 11B are diagrams illustrating an example of a secondary battery. [Figure 12] 12A and 12B are diagrams illustrating an example of a secondary battery. [Figure 13]FIG. 13 is a diagram illustrating an example of a secondary battery. [Figure 14] 14A, 14B, and 14C are diagrams illustrating a laminated type secondary battery. [Figure 15] 15A and 15B are diagrams illustrating a laminated type secondary battery. [Figure 16] FIG. 16 is a diagram showing the external appearance of a secondary battery. [Figure 17] FIG. 17 is a diagram showing the external appearance of a secondary battery. [Figure 18] 18A, 18B, and 18C are diagrams illustrating a method for producing a secondary battery. [Figure 19] FIG. 19A is a top view of a bendable secondary battery, FIG. 19B1 is a cross-sectional view taken along dashed line C1C2, FIG. 19B2 is a cross-sectional view taken along dashed line C3C4, FIG. 19C is a cross-sectional view taken along dashed line A1A2, and FIG. 19D is a cross-sectional view taken along dashed line B1B2 when bent. [Figure 20] FIG. 20A is a perspective view of a secondary battery, and FIG. 20B is a perspective view of the secondary battery. [Figure 21] Figure 21A is an oblique view of an electronic device, Figure 21B is an oblique view of an electronic device, Figure 21C is an oblique view of a secondary battery, Figure 21D is an oblique view of an electronic device, Figure 21E is an oblique view of a secondary battery, and Figures 21F and 21G are oblique views illustrating an example of an electronic device. [Figure 22] 22A is a top view of the electronic device in an open state, FIG. 22B is a top view of the electronic device in a closed state, and FIG. 22C is a diagram illustrating a block diagram of the electronic device. [Figure 23] FIG. 23 is a diagram illustrating an example of an electronic device. [Figure 24] 24A, 24B, and 24C are diagrams illustrating an example of an electronic device. [Diagram 25] FIG. 25 is a diagram for explaining calculation results of stabilization energy according to the embodiment. [Figure 26] FIG. 26 is a diagram for explaining the calculation results of the stabilization energy according to the embodiment. [Figure 27]FIG. 27 is a diagram illustrating the charge / discharge efficiency according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be easily understood by those skilled in the art that the form and details of the present invention can be modified in various ways. Furthermore, the present invention is not to be interpreted as being limited to the description of the embodiments shown below.

[0023] In addition, in crystallography, crystal planes and directions are expressed by adding a superscript bar to the numbers, but in this specification and elsewhere, due to restrictions on notation in applications, crystal planes and directions are expressed by adding a - (minus sign) before the numbers instead of adding a bar above them. Also, individual directions showing directions within a crystal are expressed with [ ], collective directions showing all equivalent directions with < >, individual faces showing crystal faces with ( ), and collective faces with equivalent symmetry with {}.

[0024] (Embodiment 1) Development of lithium composite oxides in which a part of LiCoO2 is replaced with a different element as a positive electrode material is underway. Since the content of the replacement element is small, it is difficult to analyze the crystal structure of lithium composite oxides. The inventors have found that the analysis of the crystal structure can be performed efficiently and in more detail by analyzing the crystal structure through a combination of chemical calculations and experiments.

[0025] [Calculation of stabilization energy for different substitution positions] When a metal element is doped into LiCoO2, it is expected that it will substitute for the Li site or Co site in the LiCoO2 crystal, but it is currently difficult to analyze by measurement which site has been substituted. Furthermore, when there are multiple metal elements to be doped, the situation becomes even more complicated because each of the doped metals can substitute for the Li site or the Co site. Therefore, it is effective to use chemical calculations to determine the stabilization energy of the crystal structure due to the arrangement of each cation site, thereby estimating the site that the doped metal will substitute. Below, we will look at an example of a lithium composite oxide in which LiCoO2 is doped with Mg and Ni, with the chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) The method for analyzing the substitution position of the doping element in the lithium composite oxide is explained by taking the calculation of the substance represented by O2 as an example. Note that in the above chemical formula, x+y<1 and a+b<1.

[0026] It is preferable that the experimenter creates an outline of the crystal model and uses a computer to perform various calculations. By creating an outline of the crystal model, the experimenter can clarify the crystal conditions and the relationships between various parameters, allowing for detailed analysis to be performed later. In addition, since the amount of calculation is enormous, the calculation results can be obtained quickly by processing using a computer. In the following calculation example, it is assumed that the crystal structure of LiCoO2 (R-3m(O3)) is created by the experimenter and various calculations are performed using a computer.

[0027] [Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) Calculation example of O2 stabilization energy] By creating a model in which LiCoO2, which has the crystal structure of R-3m(O3), which is the basic structure of LiCoO2, is doped with Mg and Ni, and calculating the stabilization energy, (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b)It is possible to analyze the crystal structure of O2. Figure 1 shows a crystal model of R-3m(O3), which is the basic structure of LiCoO2. Figure 1 shows the crystal structure of LiCoO2 (total number of atoms: 192), which consists of 48 Li atoms, 48 ​​Co atoms, and 96 oxygen atoms.

[0028] Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) O2 is a compound that uses Mg and Ni as substitution elements for the metal elements (Li and / or metal) that LiCoO2 has. Here, the combination of the substitution sites of the Mg and Ni can be considered in several crystal models as shown below. When Li in the same Li layer is replaced with Mg and Ni When Li in different Li layers is replaced with Mg and Ni When Co in the same Co layer is replaced by Mg and Ni When Co in different Co layers is replaced by Mg and Ni When Li in the Li layer is replaced with Mg and Co in the Co layer is replaced with Ni When Li in the Li layer is replaced with Ni, and Co in the Co layer is replaced with Mg

[0029] Figures 2A and 2B show examples of the substitution positions of Mg and Ni in a LiCoO2 crystal. Figure 2A shows the case where Li in the same Li layer is substituted with Mg and Ni, and Figure 2B shows the case where Li in a different Li layer is substituted with Mg and Ni.

[0030] Here, by calculating the stabilization energy of the crystal structure for each combination of the above substitution sites, Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) It is possible to analyze what kind of crystal structure O2 can take. The stabilization energy can be estimated from the following formula. Here, we consider a model in which a Li atom or a Co atom in LiCoO2 (total number of atoms: 192) consisting of 48 Li atoms, 48 ​​Co atoms, and 96 oxygen atoms is replaced by one Mg atom and one Ni atom.

[0031] <When two Li sites are substituted by one Mg and one Ni> (Equation 1) ΔE = [E_total{(Li 46 Mg1Ni1Co 48 O 96 ) + 2×E_atom(Li)} - {E_total(Li 48 Co 48 O 96 ) + E_atom(Mg) + E_atom(Ni)} ··· (Equation 1)

[0032] <When one Li site is substituted by one Mg and one Co site is substituted by one Ni> (Equation 2) ΔE = [E_total{(Li 47 Mg1Ni1Co 47 O 96 ) + E_atom(Li) + E_atom(Co)} - {E_total(Li 48 Co 48 O 96 ) + E_atom(Mg) + E_atom(Ni)} ··· (Equation 2)

[0033] <When two Co sites are substituted by one Mg and one Ni> (Equation 3) ΔE = [E_total{(Li 48 Mg1Ni1Co 46 O 96 ) + 2×E_atom(Co)} - {E_total(Li 48 Co 48 O 96 ) + E_atom(Mg) + E_atom(Ni)} ··· (Equation 3)

[0034] The symbols in the above Equations 1 to 3 are as follows. · ΔE: Stabilization energy. · E_total(Li 46 Mg1Ni1Co 48 O 96): Energy of a model in which two Li atoms are replaced with one Mg atom and one Ni atom in a LiCoO2 crystal (total number of atoms: 192). ·E_total(Li 47 Mg1Ni1Co 47 O 96 ): Energy of a model in which one Li atom is replaced with one Mg atom and one Co atom is replaced with one Ni atom in a LiCoO2 crystal (total number of atoms: 192). ·E_total(Li 48 Mg1Ni1Co 46 O 96 ): Energy of a model in which two Co atoms are replaced with one Mg atom and one Ni atom in a LiCoO2 crystal (total number of atoms: 192). ·E_total(Li 48 Co 48 O 96 ): Energy of a LiCoO2 crystal model (total number of atoms: 192). E_atom(Li): Energy of one Li atom. E_atom(Co): Energy of one Co atom. E_atom(Mg): Energy of one Mg atom. E_atom(Ni): Energy of one Ni atom.

[0035] By calculating and comparing the stabilization energy for each combination of Mg and Ni substitution sites, the stable crystal structure can be estimated. The smaller the stabilization energy value calculated from formulas (1) to (3), the more stable the crystal model is. (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) This indicates that O2 is the most likely option.

[0036] The above calculation can be performed using the LDA+U method, the GGA+U (DFT-D2) method, etc., but it is preferable to use the GGA+U (DFT-D2) method. The GGA+U (DFT-D2) method can estimate the van der Waals forces more accurately than the LDA+U method, and therefore can estimate the stabilization energy more accurately.

[0037] The stabilization energy is also influenced by the position where the atom is substituted. For example, in FIG. 2A, when Mg is substituted at the Li(a) site and Ni is substituted at the Li(b) site (first nearest neighbor), and when Mg is substituted at the Li(a) site and Ni is substituted at the Li(c) site (second nearest neighbor), the stabilization energy may change, even though Li in the same Li layer is substituted with Mg and Ni. Therefore, when calculating the stabilization energy, it is preferable to perform calculations taking into account not only the layer of the substituted atoms but also the positional relationship of the substituted atoms. In addition, when analyzing which layer Mg and Ni are substituted in, it is preferable to calculate and compare the stabilization energies of the first to third nearest neighbors in each of the crystal models to be compared among the six crystal models shown above. It is more preferable to calculate and compare the stabilization energies of the first to fourth nearest neighbors.

[0038] In the above formula, the calculation is performed using a model with 192 atoms in the crystal, but the user of the present invention can consider the tendency of the calculation result by extending it to a bulk crystal. In addition, since it is expected that the same tendency will be observed when a model with a different number of atoms is used, the tendency of the calculation result can be applied to a model with a different number of atoms. For example, if the stabilization energy of a model in which Li in the same Li layer is replaced by Mg and Ni is lower than the stabilization energy of a model in which Co in the same Co layer is replaced by Mg and Ni, this result is expected to show the same tendency in a bulk crystal or a model with a different number of atoms, and the tendency of the calculation result can be applied.

[0039] As mentioned above, by calculating and comparing the stabilization energies of each crystal model, Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b)It is possible to analyze what crystal structures O₂ can take. Note that the calculation and comparison of the above stabilization energy estimate the state of the lithium composite oxide when the occupancy of the cation site is 100%, but the calculation is performed without considering the behavior and changes in the crystal structure when using the lithium composite oxide as the positive electrode. When treating the lithium composite oxide as a positive electrode material, it is preferable to consider the behavior during charge and discharge. By considering the behavior during charge and discharge, more detailed analysis can be performed.

[0040] [Calculation of Stabilization Energy When Changing the Cation Occupancy of the Li Site] When using a lithium composite oxide as the positive electrode material of a secondary battery, in order to estimate what changes occur in the crystal structure of the lithium composite oxide due to charge and discharge of the secondary battery, there is a method of calculating the stabilization energy when Li in the lithium composite oxide is extracted, that is, the stabilization energy when changing the cation occupancy of the Li site. The extraction of Li from the lithium composite oxide assumes the behavior that occurs at the positive electrode when charging the secondary battery. Therefore, the stabilization energy when Li in the lithium composite oxide is extracted estimates the stabilization energy during charging.

[0041] The calculation formula used for calculating the stabilization energy when changing the cation occupancy of the Li site is shown below.

[0042] <When 2 Li Sites are Substituted with 1 Mg and 1 Ni> (Equation 4) ΔE C =[E C _total{(Li 46-z Mg1Ni1Co 48 O 96 ) + z × E_atom(Li)} - {E_total(Li 48 Co 48 O 96 ) + E_atom(Mg) + E_atom(Ni)} ··· (Equation 4)

[0043] <When one Li site is substituted by one Mg and one Co site is substituted by one Ni> (Equation 5) ΔE C =[E C _total{(Li 47-z Mg1Ni1Co 47 O 96 ) + z × E_atom(Li) + E_atom(Co)} - {E_total(Li 48 Co 48 O 96 ) + E_atom(Mg) + E_atom(Ni)} ··· (Equation 5)

[0044] <When two Co sites are substituted by one Mg and one Ni> (Equation 6) ΔE C =[E C _total{(Li 48-z Mg1Ni1Co 46 O 96 ) + z × E_atom(Li) + 2 × E_atom(Co)} - {E_total(Li 48 Co 48 O 96 ) + E_atom(Mg) + E_atom(Ni)} ··· (Equation 6)

[0045] The symbols in the above Equations 4 to 6 are as follows. The explanations of the symbols similar to those used in Equations 1 to 3 are omitted.

[0046] ·ΔE C : Stabilization energy when the cation occupancy of the Li site is changed. ·E C _total(Li 46-z Mg1Ni1Co 48 O 96 ): Energy when z Li are withdrawn in the model where two Li in LiCoO2 crystal (total 192 atoms) are substituted by one Mg and one Ni. Here, z is an integer satisfying 0 ≦ z ≦ 46. ·E C _total(Li 47-z Mg1Ni1Co 47 O 96): Energy of a model in which one Li atom is replaced with one Mg atom and one Co atom is replaced with one Ni atom in a LiCoO2 crystal (total number of atoms: 192). Note that z is an integer that satisfies 0≦z≦47. E C _total(Li 48-z Mg1Ni1Co 46 O 96 ): The energy when z Li atoms are extracted from a LiCoO2 crystal (total number of atoms: 192) in which two Co atoms are replaced with one Mg atom and one Ni atom. z is an integer satisfying the condition 0≦z≦48.

[0047] In the above formulas 4 to 6, z represents the number of extracted Li. Therefore, changing the value of z is equivalent to changing the cation occupancy rate of the Li site in the lithium composite oxide crystal. ΔE C Calculate ΔE for the cation occupancy of the Li site or the value of z. C By plotting this, the stabilization energy during charging can be estimated.

[0048] As shown in Figure 1, LiCoO2 crystals have a structure in which Li ions and Co ions are stacked alternately. Therefore, as the number of cations on the Li site decreases, the energy (E C _total(Li 46-z Mg1Ni1Co 48 O 96 ), E C _total(Li 47-z Mg1Ni1Co 47 O 96 ) and E C _total(Li 48-z Mg1Ni1Co 46 O 96 )), the effect of van der Waals forces between the Co layers is considered to be large. C In order to calculate, it is preferable to use a functional that takes into account van der Waals forces, and the above-mentioned GGA + U (DFT-D2) is ΔE CThe functional can be suitably used for the calculation of . As other functionals, OPTB88, DFT-D3, DFT-TS, etc. can also be used. The functionals that can be used in one embodiment of the present invention are not limited to these.

[0049] The cation occupancy is changed from at least 80% to 100%. C It is preferable to plot the above-mentioned. More preferably, it is 50% or more and 100% or less, and further preferably, it is 0% or more and 100% or less. By using this configuration, it is possible to grasp the phenomenon that occurs during charging.

[0050] By creating this plot, the crystal structure of the lithium composite oxide can be analyzed from both the above-mentioned ΔE and ΔEc. In the above example, the substitution positions of Ni atoms and Mg atoms when Mg and Ni are added to LiCoO2 can be analyzed.

[0051] In formulas 4 to 6, the value of z is changed during calculation, so that multiple calculations (up to 48 in the above example) must be performed for one model, which may increase the calculation cost. On the other hand, ΔE calculated by formulas 1 to 3 requires only a small number of relationships between Mg and Ni atoms (up to roughly the fourth nearest neighbors) for one model, so the calculation cost is low. Therefore, after calculating ΔE and examining appropriate models, ΔEc is calculated only for the appropriate models, and the above-mentioned plot is created, so that the crystal structure or the substitution positions of Ni and Mg atoms can be analyzed efficiently.

[0052] Here, ΔE C When plotting, ΔE C It is expected that a graph of the relationship will be obtained in which the relationship also increases. When the graph is created for multiple models, the relationship between the magnitude of each model may be reversed depending on the value of z. For example, when the cation occupancy rate is in the range of 95% to 100%, the ΔE C ΔE of Model B CHowever, in the range of cation occupancy of 0% or more and less than 95%, the ΔE C is the ΔE of Model B C If the calculation result is greater than , when the cation occupancy is in the range of 95% to 100%, Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) O2 is expected to have a structure of model A, but when the cation occupancy is in the range of 0% or more and less than 95%, it is expected to have a structure of model B. In other words, it is expected that a change in the crystal structure occurs due to charging. In order to analyze such phenomena caused by charging, it is preferable to carry out the following measurements.

[0053] [Measurement of first charge / discharge efficiency and second charge / discharge efficiency] The charge / discharge efficiency of a secondary battery is approximately 100% if the appropriate electrodes are selected, provided that there is no deterioration of the electrode materials and electrolyte, no short circuit, and no deposition of metallic lithium. If the charge / discharge efficiency is below 100% despite the absence of the above-mentioned deterioration factors, a change in the crystal structure of the positive electrode material during charging or discharging can be estimated. In addition, since the charge / discharge efficiency is calculated from the ratio of the discharge capacity and the charge capacity, if the energy given during charging is used for purposes other than the extraction of Li, the charge / discharge efficiency decreases. Therefore, if a change occurs in the crystal model of the positive electrode material, a decrease in the charge / discharge efficiency can be observed. Therefore, by measuring the charge / discharge efficiency, the change in the crystal model of the lithium composite oxide can be analyzed.

[0054] When analyzing the change in the crystal model more accurately, it is preferable that the above-mentioned deterioration factors are few. Therefore, it is preferable to measure the first charge / discharge efficiency. In addition, when the crystal model changes, the phenomenon occurring in the crystal can be analyzed in more detail by analyzing whether the change is reversible or irreversible. Therefore, it is more preferable to measure not only the first charge / discharge efficiency but also the second charge / discharge efficiency. If the second measurement has the same result as the first, it can be estimated that the phenomenon occurring in the crystal is reversible. On the other hand, if the second measurement is different from the first measurement, for example, the first charge / discharge efficiency is less than 100% while the second charge / discharge efficiency is 100%, it can be estimated that the phenomenon occurring in the crystal is irreversible and occurs only in the first measurement. In this way, a more detailed analysis can be performed by comparing the first and second charge / discharge efficiencies.

[0055] If the deterioration factors are few, the charge / discharge efficiency may be compared between the first and third or later cycles. The charge / discharge efficiency may also be compared between any number of cycles, such as the second and third or later cycles. However, if the phenomenon occurring in the crystal is irreversible, the phenomenon may only be observed the first time. Therefore, it is preferable to measure the first charge / discharge efficiency. In addition, it is more preferable to compare the first and second cycles when the deterioration factors are taken into consideration.

[0056] Also, the chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) To measure the charge-discharge efficiency of a compound represented by the formula LiO2, it is first necessary to synthesize the compound. Next, a battery cell is made using the synthesized compound, and then the charge-discharge efficiency of the battery cell is measured. These steps are necessary to measure the charge-discharge efficiency. (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) If you are performing measurements that are not related to charging / discharging or electrolytes, such as XRD measurements of O2, you do not need to create a battery cell. (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b)When measuring a compound represented by O2, at least a step of synthesizing the compound and a step of measuring the properties of the compound are required. When measuring the charge-discharge efficiency, a step of fabricating a battery cell is further required. Note that other steps may be included for the measurement.

[0057] By combining and analyzing the measurements of ΔE, ΔEc, and charge-discharge efficiency described in this embodiment, the crystal structure and substitution position of the lithium composite oxide can be accurately analyzed. It is a feature of the present invention to perform calculations efficiently using a plurality of calculation methods and further perform analysis by combining measurements. By combining calculations and measurements, the validity of the calculation results and the phenomena predicted from the calculation results can be evaluated, so that detailed analysis can be performed. In particular, for the chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) The compound represented by O2 has particularly good properties when 0 < x + a ≤ 0.015 and 0 < y + b ≤ 0.06. However, since the mixing amounts of Mg and Ni are small, it is currently difficult to analyze the detailed crystal structure only by measurement. Therefore, the analysis method of one aspect of the present invention can be preferably used. Further, based on the analysis results obtained from the calculations and measurements, by performing analysis again by calculation and measurement, a more accurate analysis can be performed. Therefore, the calculations and measurements shown in this embodiment may be repeated. Also, further analysis may be performed based on the results obtained from the calculations and measurements shown in this embodiment.

[0058] Also, although the measurement of charge-discharge efficiency has been described as an example of measurement, as the measurement of one aspect of the present invention, dQ / dV measurement, XRD measurement, magnetization measurement, Li NMR measurement, etc. can also be used. The measurement of one aspect of the present invention is not limited to these.

[0059] This embodiment can be used in appropriate combination with other embodiments.

[0060] (Embodiment 2) Using FIG. 3, the chemical formula Li (1-x-y)Co (1-a-b) Ni (x+a) Mg (y+b) An example of a method for producing the compound represented by O2 will be described.

[0061] As shown in step S11 of FIG. 3, first, lithium fluoride, which is a fluorine source, and magnesium fluoride, which is a magnesium source, are prepared as materials for the mixture 902. Lithium fluoride is preferable because it has a relatively low melting point of 848°C and is easily melted in the annealing step described below. Lithium fluoride can be used as both a lithium source and a fluorine source. Magnesium fluoride can be used as both a fluorine source and a magnesium source.

[0062] In this embodiment, lithium fluoride LiF is prepared as the fluorine source and the lithium source, and magnesium fluoride MgF2 is prepared as the fluorine source and the magnesium source (step S11 in FIG. 3). The molar ratio of lithium fluoride LiF and magnesium fluoride MgF2 is preferably LiF:MgF2=u:1 (0≦u≦1.9), more preferably LiF:MgF2=x:1 (0.1≦u≦0.5), and even more preferably LiF:MgF2=u:1 (u=near 0.33).

[0063] If the next mixing and grinding step is performed in a wet manner, a solvent is prepared. As the solvent, a ketone such as acetone, an alcohol such as ethanol or isopropanol, ether, dioxane, acetonitrile, N-methyl-2-pyrrolidone (NMP), etc. can be used. It is more preferable to use an aprotic solvent that is less likely to react with lithium. In this embodiment, acetone is used (see step S11 in FIG. 3).

[0064] Next, the materials of the mixture 902 are mixed and pulverized (step S12 in FIG. 3). Mixing can be performed in a dry or wet manner, but the wet method is preferred because it allows for finer pulverization. For example, a ball mill, a bead mill, etc. can be used for mixing. When using a ball mill, it is preferable to use zirconia balls, for example, as the media. It is preferable to thoroughly perform this mixing and pulverization process to finely pulverize the mixture 902.

[0065] The mixed and pulverized materials are collected (step S13 in FIG. 3) to obtain a mixture 902 (step S14 in FIG. 3).

[0066] The mixture 902 preferably has a D50 of, for example, 600 nm or more and 20 μm or less, and more preferably 1 μm or more and 10 μm or less. If the mixture 902 is finely pulverized in this way, when it is mixed with a composite oxide having lithium, a transition metal, and oxygen in a later process, the mixture 902 can be easily attached uniformly to the surface of the composite oxide particles. If the mixture 902 is attached uniformly to the surface of the composite oxide particles, it is preferable because it is easy to distribute halogen and magnesium thoroughly in the surface layer of the composite oxide particles after heating. If there is a region in the surface layer that does not contain halogen and magnesium, it may be difficult to obtain the pseudo-spinel type crystal structure described above in a charged state.

[0067] Next, a lithium source is prepared as shown in step S25. In step S25, a composite oxide having lithium, a transition metal, and oxygen that has been synthesized in advance is used.

[0068] For example, lithium cobalt oxide particles (product name: Cellseed C-10N) manufactured by Nippon Chemical Industry Co., Ltd. can be used as the pre-synthesized lithium cobalt oxide. This is lithium cobalt oxide with an average particle diameter (D50) of about 12 μm, and in impurity analysis by glow discharge mass spectrometry (GD-MS), the magnesium concentration and fluorine concentration are 50 ppm wt or less, the calcium concentration, aluminum concentration and silicon concentration are 100 ppm wt or less, the nickel concentration is 150 ppm wt or less, the sulfur concentration is 500 ppm wt or less, the arsenic concentration is 1100 ppm wt or less, and the concentration of other elements other than lithium, cobalt and oxygen is 150 ppm wt or less.

[0069] The composite oxide having lithium, a transition metal, and oxygen in step S25 preferably has a layered rock-salt type crystal structure with few defects and distortion. Therefore, it is preferable that the composite oxide has few impurities. If the composite oxide having lithium, a transition metal, and oxygen contains a large amount of impurities, it is highly likely that the composite oxide will have a crystal structure with many defects or distortion.

[0070] Next, the mixture 902 is mixed with a composite oxide having lithium, a transition metal, and oxygen (step S31 in FIG. 3). The ratio of the number of transition metal atoms TM in the composite oxide having lithium, a transition metal, and oxygen to the number of magnesium atoms MgMix1 in the mixture 902 is preferably TM:MgMix1=1:v (0.005≦v≦0.05), more preferably TM:MgMix1=1:v (0.007≦v≦0.04), and even more preferably about TM:MgMix1=1:0.02.

[0071] The mixing in step S31 is preferably performed under milder conditions than those in step S12 in order not to destroy the composite oxide particles. For example, the mixing is preferably performed under conditions of a lower rotation speed or shorter time than those in step S12. It can also be said that the dry method is a milder condition than the wet method. For example, a ball mill, a bead mill, etc. can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media, for example.

[0072] The mixed materials are collected (step S32 in FIG. 3) to obtain a mixture 903 (step S33 in FIG. 3).

[0073] Next, the mixture 903 is heated (step S34 in FIG. 3). This step is sometimes called annealing or second heating to distinguish it from the previous heating step.

[0074] The annealing is preferably performed at an appropriate temperature and time. The appropriate temperature and time vary depending on conditions such as the size and composition of the particles of the composite oxide having lithium, transition metal, and oxygen in step S25. If the particles are small, a lower temperature or a shorter time may be more preferable than if the particles are large.

[0075] For example, when the average particle size (D50) of the particles in step S25 is about 12 μm, the annealing temperature is preferably, for example, 600° C. or more and 950° C. or less. The annealing time is, for example, preferably 3 hours or more, more preferably 10 hours or more, and even more preferably 60 hours or more.

[0076] On the other hand, when the average particle size (D50) of the particles in step S25 is about 5 μm, the annealing temperature is preferably, for example, from 600° C. to 950° C. The annealing time is preferably, for example, from 1 hour to 10 hours, and more preferably about 2 hours.

[0077] The temperature drop time after annealing is preferably, for example, 10 hours or more and 50 hours or less.

[0078] When the mixture 903 is annealed, it is believed that the material with the low melting point of the mixture 902 (for example, lithium fluoride, melting point 848°C) melts first and distributes in the surface layer of the composite oxide particle. It is then assumed that the presence of this molten material lowers the melting points of other materials, causing the other materials to melt. For example, it is believed that magnesium fluoride (melting point 1263°C) melts and distributes in the surface layer of the composite oxide particle.

[0079] The diffusion of elements contained in the mixture 903 is faster in the surface layer and in the vicinity of the grain boundaries than in the interior of the composite oxide particles, so that the magnesium and halogen are concentrated in the surface layer and in the vicinity of the grain boundaries more than in the interior.

[0080] The annealed material is collected (step S35 in FIG. 3) to obtain a mixture 904 (step S36 in FIG. 3).

[0081] Next, as shown in step S50, the mixture 904 and the pulverized nickel hydroxide are mixed. Then, the mixed material is collected (step S51). The pulverized nickel hydroxide is previously subjected to step S15 in which nickel hydroxide is mixed with acetone and step S16 in which the nickel hydroxide is collected. By step S16, pulverized nickel hydroxide is obtained (step S17).

[0082] The materials mixed in step S50 are collected in step S51 to obtain a mixture 905 (step S52 in FIG. 3).

[0083] Next, the resulting mixture is heated (Step S53 in FIG. 3).

[0084] The heating time is preferably set to a holding time within the heating temperature range of 1 hour to 80 hours.

[0085] The heating temperature is less than 1000°C, preferably 700°C to 950°C, and more preferably about 850°C.

[0086] Moreover, the heating is preferably carried out in an atmosphere containing oxygen.

[0087] In this embodiment, the heating temperature is set to 850° C. and held for 2 hours, the temperature increase rate is set to 200° C. / h, and the oxygen flow rate is set to 10 L / min.

[0088] The heating temperature in step S53 is preferably lower than the heating temperature in step S34.

[0089] <Step S54, Step S55> Next, the cooled particles are collected (step S54 in FIG. 3). It is preferable to further sieve the particles. (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) A positive electrode active material 100A-1, which is an example of a compound represented by O2, can be produced (Step S55 in FIG. 3).

[0090] The positive electrode active material 100A-1 obtained by the above-mentioned method will be described.

[0091] [Positive electrode active material structure] Materials having a layered rock-salt crystal structure, such as lithium cobalt oxide (LiCoO2), are known to have a high discharge capacity and are excellent as positive electrode active materials for secondary batteries. An example of a material having a layered rock-salt crystal structure is a composite oxide represented by LiMO2. An example of element M is one or more selected from Co and Ni. Also, an example of element M is one or more selected from Al and Mg in addition to one or more selected from Co and Ni.

[0092] It is known that the strength of the Jahn-Teller effect in transition metal compounds varies depending on the number of electrons in the d orbital of the transition metal.

[0093] In a compound having nickel, distortion may easily occur due to the Jahn-Teller effect. Therefore, when charge and discharge are performed at a high voltage in LiNiO2, there is a concern that the crystal structure may collapse due to the distortion. In LiCoO2, it is suggested that the influence of the Jahn-Teller effect is small, and it may be more resistant to charge and discharge at a high voltage, which is preferable.

[0094] Using FIGS. 4 and 5, the positive electrode active material will be described. FIGS. 4 and 5 describe the case where cobalt is used as the transition metal included in the positive electrode active material.

[0095] Chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) The compound represented by O2 can reduce the shift of the CoO2 layer in repeated charge and discharge at a high voltage. Furthermore, the volume change can be reduced. Therefore, the compound can achieve excellent cycle characteristics. In addition, the compound can have a stable crystal structure in a charged state at a high voltage. Therefore, when the compound maintains a charged state at a high voltage, a short circuit is less likely to occur. In such a case, the safety is further improved, which is preferable. In particular, it is preferable that 0 < x + a ≦ 0.015 and 0 < y + b ≦ 0.06 because the characteristics are good.

[0096] In this compound, the change in the crystal structure and the volume difference per the same number of transition metal atoms in a fully discharged state and a state charged at a high voltage are small.

[0097] The crystal structure of the positive electrode active material 100A-1 before and after charge and discharge is shown in FIG. 5. The positive electrode active material 100A-1 is a composite oxide represented by the chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) O2.

[0098] The crystal structure at a charge depth of 0 (discharged state) in FIG. 5 is the same as that in FIG. 4, R-3m (O3). On the other hand, when the positive electrode active material 100A-1 is fully charged, it has a crystal structure different from the H1-3 type crystal structure. This structure is in the space group R-3m, and although it is not a spinel type crystal structure, ions of cobalt, magnesium, etc. occupy oxygen 6 coordination positions, and the arrangement of cations has a symmetry similar to that of the spinel type. Therefore, this structure is referred to as a pseudo-spinel type crystal structure in this specification. In the diagram of the pseudo-spinel type crystal structure shown in FIG. 5, lithium is omitted in order to explain the symmetry of the cobalt atom and the symmetry of the oxygen atom, but in reality, for example, 20 atomic % or less of lithium is present between the CoO2 layers with respect to cobalt. In addition, in both the O3 type crystal structure and the pseudo-spinel type crystal structure, it is preferable that magnesium is present dilutely between the CoO2 layers, that is, at the lithium site. In addition, halogen such as fluorine may be present randomly and dilutely at the oxygen site.

[0099] In addition, in the pseudospinel crystal structure, light elements such as lithium may occupy the oxygen tetracoordination site, and in this case too, the arrangement of ions has a symmetry similar to that of the spinel type.

[0100] It can also be said that the pseudo-spinel type crystal structure is a crystal structure similar to the CdCl2 type crystal structure, although it has random Li between the layers. This CdCl2 type-like crystal structure was observed when lithium nickel oxide was charged to a charge depth of 0.94 (Li 0.06 The crystal structure is close to that of lithium cobalt oxide (NiO2), but it is known that pure lithium cobalt oxide or layered rock salt type positive electrode active materials that contain a large amount of cobalt do not usually have this crystal structure.

[0101] The layered rock salt crystal and the anions of the rock salt crystal have a cubic close-packed structure (face-centered cubic lattice structure). It is presumed that the anions of the pseudo-spinel crystal also have a cubic close-packed structure. When they contact, there is a crystal plane where the orientation of the cubic close-packed structure formed by the anions is aligned. However, the space group of the layered rock salt crystal and the pseudo-spinel crystal is R-3m, which is different from the space group Fm-3m (the space group of a general rock salt crystal) and Fd-3m (the space group of a rock salt crystal with the simplest symmetry) of the rock salt crystal, so the Miller indices of the crystal planes that satisfy the above conditions are different between the layered rock salt crystal and the pseudo-spinel crystal and the rock salt crystal. In this specification, when the orientation of the cubic close-packed structure formed by the anions is aligned in the layered rock salt crystal, the pseudo-spinel crystal, and the rock salt crystal, it may be said that the crystal orientation is approximately the same.

[0102] In the positive electrode active material 100A-1, the change in the crystal structure when a large amount of lithium is released during charging at a high voltage is suppressed more than in the positive electrode active material 100C. For example, as shown by the dotted line in Figure 4, there is almost no displacement of the CoO2 layer in these crystal structures.

[0103] More specifically, the positive electrode active material 100A-1 has a high structural stability even when the charging voltage is high. For example, in the positive electrode active material 100C, there is a charging voltage region where the R-3m(O3) crystal structure can be maintained even at a charging voltage that results in an H1-3 crystal structure, for example, a voltage of about 4.6V based on the potential of lithium metal, and there is a region where the pseudo-spinel crystal structure can be maintained even at a higher charging voltage, for example, a voltage of about 4.65V to 4.7V based on the potential of lithium metal. When the charging voltage is further increased, the H1-3 crystal may finally be observed. In addition, when graphite is used as the negative electrode active material in a secondary battery, there is a charging voltage region where the R-3m(O3) crystal structure can be maintained even at a secondary battery voltage of 4.3V to 4.5V, and there is a region where the pseudo-spinel crystal structure can be maintained even at a higher charging voltage, for example, a region where the pseudo-spinel crystal structure can be maintained even at a higher charging voltage, for example, a region where the pseudo-spinel crystal structure can be maintained even at a higher charging voltage, for example, a region where the pseudo-spinel crystal structure can be maintained even at a voltage of 4.35V to 4.55V based on the potential of lithium metal.

[0104] Therefore, in the positive electrode active material 100A-1, the crystal structure is not easily destroyed even when the material is repeatedly charged and discharged at a high voltage.

[0105] In addition, the pseudospinel crystal structure can be expressed by the coordinates of cobalt and oxygen in the unit cell being Co(0,0,0.5), O(0,0,x), with 0.20≦x≦0.25.

[0106] Magnesium, which is present randomly and dilutely between the CoO2 layers, i.e., at the lithium sites, has the effect of suppressing the displacement of the CoO2 layers. Therefore, when magnesium is present between the CoO2 layers, it is easy to form a pseudo-spinel type crystal structure. Therefore, it is preferable that magnesium is distributed throughout the particles of the positive electrode active material 100A-1. In order to distribute magnesium throughout the particles, it is preferable to perform a heat treatment in the manufacturing process of the positive electrode active material 100A-1.

[0107] However, if the heat treatment temperature is too high, cation mixing occurs, increasing the possibility that magnesium will enter the cobalt site. If magnesium is present at the cobalt site, it will no longer be effective in maintaining the R-3m structure. Furthermore, if the heat treatment temperature is too high, there are concerns that it may have adverse effects such as reducing cobalt to a divalent state and evaporating lithium.

[0108] Therefore, it is preferable to add a halogen compound such as a fluorine compound to the lithium cobalt oxide before the heat treatment for distributing magnesium throughout the particles. The addition of the halogen compound lowers the melting point of the lithium cobalt oxide. Lowering the melting point makes it easier to distribute magnesium throughout the particles at a temperature where cation mixing is unlikely to occur. Furthermore, the presence of a fluorine compound is expected to improve corrosion resistance against hydrofluoric acid produced by decomposition of the electrolyte.

[0109] If the magnesium concentration is increased above a desired value, the effect of stabilizing the crystal structure may be reduced. This is believed to be because magnesium enters the cobalt site in addition to the lithium site. The number of magnesium atoms in the positive electrode active material of one embodiment of the present invention is preferably 0.001 times or more and 0.1 times or less than the number of cobalt atoms, more preferably greater than 0.01 and less than 0.04, and even more preferably about 0.02. The magnesium concentration shown here may be, for example, a value obtained by performing elemental analysis of the entire particle of the positive electrode active material using ICP-MS or the like, or may be based on the value of the raw material composition in the process of producing the positive electrode active material.

[0110] The number of nickel atoms in the positive electrode active material 100A-1 is preferably 7.5% or less of the number of cobalt atoms, more preferably 0.05% to 4%, and more preferably 0.1% to 2%. The nickel concentration shown here may be a value obtained by performing elemental analysis of the entire particles of the positive electrode active material using, for example, ICP-MS or the like, or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material.

[0111] A more detailed structure of positive electrode active material 100A-1 can be analyzed by the analysis method shown in the first embodiment.

[0112] ≪Particle size≫ If the particle size of the positive electrode active material 100A-1 is too large, problems such as difficulty in diffusing lithium, and excessive roughness of the surface of the active material layer when applied to a current collector occur. On the other hand, if the particle size is too small, problems such as difficulty in supporting the active material layer when applied to a current collector, and excessive reaction with the electrolyte occur. Therefore, the average particle size (D50: also called the median size) is preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 40 μm or less, and even more preferably 5 μm or more and 30 μm or less.

[0113] <Analysis method> Whether or not a certain positive electrode active material exhibits a pseudospinel crystal structure when charged at a high voltage can be determined by analyzing the positive electrode charged at a high voltage using XRD, electron beam diffraction, neutron beam diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR), etc. XRD is particularly preferable in that it can analyze the symmetry of transition metals such as cobalt contained in the positive electrode active material with high resolution, it can compare the degree of crystallinity and the orientation of the crystals, it can analyze the periodic distortion of the lattice and the crystallite size, and it can obtain sufficient accuracy even when the positive electrode obtained by disassembling the secondary battery is directly measured.

[0114] As described above, the positive electrode active material 100A-1 is characterized by a small change in crystal structure between a state charged at a high voltage and a discharged state. A material in which a crystal structure that changes greatly from a discharged state when charged at a high voltage accounts for 50 wt% or more is not preferable because it cannot withstand high-voltage charging and discharging. It is also important to note that the desired crystal structure may not be obtained by simply adding an impurity element. For example, even if lithium cobalt oxide containing magnesium and fluorine is common in that it is charged at a high voltage, there are cases in which the pseudo-spinel crystal structure accounts for 60 wt% or more, and cases in which the H1-3 crystal structure accounts for 50 wt% or more. In addition, at a predetermined voltage, the pseudo-spinel crystal structure may be almost 100 wt%, and if the predetermined voltage is further increased, the H1-3 crystal structure may occur. Therefore, it is preferable to analyze the crystal structure of the positive electrode active material 100A-1 by XRD or the like. It is also more preferable to perform the analysis using the analysis method described in the first embodiment. By using it in combination with the measurement of XRD or the like, a more detailed analysis can be performed.

[0115] However, when the positive electrode active material is charged or discharged at a high voltage, its crystal structure may change when it comes into contact with the air. For example, it may change from a pseudo-spinel crystal structure to an H1-3 crystal structure. Therefore, it is preferable to handle all samples in an inert atmosphere such as an argon atmosphere.

[0116] <Comparative example of positive electrode active material (LiCoO2)> The positive electrode active material (lithium cobalt oxide) shown in Fig. 4 is lithium cobalt oxide (LiCoO2) to which no halogen or magnesium is added, produced by a method described later. As described in Non-Patent Documents 1 and 2, etc., the crystal structure of the lithium cobalt oxide shown in Fig. 4 changes depending on the charge depth.

[0117] As shown in Figure 4, lithium cobalt oxide at a charge depth of 0 (discharged state) has a region with a crystal structure of space group R-3m, and there are three CoO2 layers in the unit cell. Therefore, this crystal structure is sometimes called an O3 type crystal structure. Note that a CoO2 layer is an octahedral structure in which cobalt is coordinated with six oxygen atoms, and the octahedral structure is continuous on a plane with edge sharing.

[0118] At a charge depth of 1, the crystal structure has the space group P-3m1, and there is one CoO2 layer in the unit cell. Therefore, this crystal structure is sometimes called the O1 type crystal structure.

[0119] Lithium cobalt oxide at a charge depth of about 0.88 has a crystal structure of space group R-3m. This structure can be said to be a structure in which a CoO2 structure such as P-3m1(O1) and a LiCoO2 structure such as R-3m(O3) are alternately stacked. Therefore, this crystal structure is sometimes called an H1-3 type crystal structure. In reality, the number of cobalt atoms per unit cell in the H1-3 type crystal structure is twice that of other structures. However, in FIG. 5 and other parts of this specification, the c-axis of the H1-3 type crystal structure is shown as half the unit cell in order to make it easier to compare with other structures.

[0120] As an example, as described in Non-Patent Document 3, the coordinates of cobalt and oxygen in the unit cell of the H1-3 type crystal structure can be expressed as Co(0,0,0.42150±0.00016), O1(0,0,0.27671±0.00045), and O2(0,0,0.11535±0.00045). O1 and O2 are oxygen atoms. Thus, the H1-3 type crystal structure is expressed by a unit cell using one cobalt and two oxygens. On the other hand, as described later, the pseudo-spinel type crystal structure of one embodiment of the present invention shown in FIG. 5 is preferably expressed by a unit cell using one cobalt and one oxygen. This indicates that the symmetry of cobalt and oxygen is different in the case of the pseudo-spinel structure and the case of the H1-3 type structure, and the pseudo-spinel structure has a smaller change from the O3 structure than the H1-3 type structure. The unit cell that is more preferably used to represent the crystal structure of the positive electrode active material may be selected, for example, so that the good of fitness (GOF) value is smaller in Rietveld analysis of XRD.

[0121] When lithium cobalt oxide is repeatedly charged at a high voltage of 4.6 V or higher based on the redox potential of lithium metal, or when it is repeatedly charged to a deep depth of charge of 0.8 or higher, and then discharged, it undergoes repeated changes in crystal structure (i.e., a non-equilibrium phase change) between the H1-3 crystal structure and the R-3m(O3) structure in the discharged state.

[0122] However, these two crystal structures have a large deviation in the CoO2 layer. As shown by the dotted line and arrow in Figure 4, in the H1-3 type crystal structure, the CoO2 layer is significantly deviated from R-3m(O3). Such a dynamic structural change can have a negative effect on the stability of the crystal structure.

[0123] Furthermore, the difference in volume is large: when compared per the same number of cobalt atoms, the difference in volume between the H1-3 crystal structure and the O3 crystal structure in the discharged state is more than 3.0%.

[0124] In addition, the structure in which the CoO2 layers such as P-3m1(O1) having the H1-3 type crystal structure are continuous is likely to be unstable.

[0125] Therefore, when high-voltage charge and discharge are repeated, the crystal structure of lithium cobalt oxide collapses. The collapse of the crystal structure causes deterioration of the cycle characteristics. This is considered to be because when the crystal structure collapses, the sites where lithium can stably exist decrease, and it becomes difficult for lithium to be inserted and removed.

[0126] (Embodiment 3) In this embodiment, an example of a material that can be used for a secondary battery having the positive electrode active material 100 shown in FIGS. 6A and 6B will be described. In this embodiment, a secondary battery in which a positive electrode, a negative electrode, and an electrolytic solution are wrapped in an exterior body will be described as an example. Note that the positive electrode active material 100 has the chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) The compound represented by O2 and the positive electrode active material 100A-1 can be used.

[0127] [Positive Electrode] The positive electrode has a positive electrode active material layer and a positive electrode current collector.

[0128] [Positive Electrode Active Material Layer] The positive electrode active material layer has positive electrode active material particles. Further, the positive electrode active material layer may have a conductive assistant and a binder.

[0129] As the positive electrode active material particles, the positive electrode active material 100 can be used. As the positive electrode active material 100, the lithium composite oxide described in the previous embodiment, for example, the chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) The compound represented by O2 and the positive electrode active material 100A-1 can be used. In the chemical formula, it is preferably 0 < x + a ≤ 0.015 and 0 < y + b ≤ 0.06. By using this compound, a secondary battery with less deterioration and high safety can be obtained.

[0130] The conductive assistant may be a carbon material, a metal material, a conductive ceramic material, or the like. A fibrous material may also be used as the conductive assistant. The content of the conductive assistant relative to the total amount of the active material layer is preferably 1 wt% to 10 wt%, more preferably 1 wt% to 5 wt%.

[0131] The conductive assistant can form an electrical conductive network in the electrode. The conductive assistant can maintain an electrical conductive path between the positive electrode active materials. By adding the conductive assistant to the active material layer, an active material layer having high electrical conductivity can be realized.

[0132] As the conductive assistant, for example, natural graphite, artificial graphite such as mesocarbon microbeads, carbon fiber, etc. can be used. As the carbon fiber, for example, mesophase pitch carbon fiber, isotropic pitch carbon fiber, etc. can be used. As the carbon fiber, carbon nanofiber, carbon nanotube, etc. can be used. Carbon nanotube can be produced by, for example, vapor phase growth method, etc. As the conductive assistant, for example, carbon material such as carbon black (acetylene black (AB) etc.), graphite (graphite) particles, graphene, fullerene, etc. can be used. As the conductive assistant, for example, metal powder or metal fiber such as copper, nickel, aluminum, silver, gold, etc., conductive ceramic material, etc. can be used.

[0133] In addition, a graphene compound may be used as the conductive assistant.

[0134] Graphene compounds may have excellent electrical properties, such as high electrical conductivity, and excellent physical properties, such as high flexibility and high mechanical strength. In addition, graphene compounds have a planar shape. Graphene compounds enable surface contact with low contact resistance. In addition, even if they are thin, they may have very high electrical conductivity, and a conductive path can be efficiently formed in the active material layer with a small amount. Therefore, by using a graphene compound as a conductive assistant, it is preferable to increase the contact area between the active material and the conductive assistant. In addition, it is preferable to reduce electrical resistance in some cases. Here, it is particularly preferable to use, for example, graphene or multi-graphene, graphene quantum dots, or reduced graphene oxide (hereinafter, RGO) as the graphene compound. Here, RGO refers to a compound obtained by reducing graphene oxide (GO: Graphene Oxide), for example.

[0135] When using active material particles having a small particle size, for example, active material particles having a size of 1 μm or less, the specific surface area of ​​the active material particles is large, and more conductive paths connecting the active material particles are required. In such a case, it is particularly preferable to use a graphene compound that can efficiently form conductive paths even in a small amount.

[0136] As an example, a cross-sectional configuration example in which a graphene compound is used as a conductive assistant in the active material layer 200 will be described below.

[0137] 6A shows a vertical cross-sectional view of an active material layer 200. The active material layer 200 includes a granular positive electrode active material 100, a graphene compound 201 as a conductive assistant, and a binder (not shown). Here, for example, graphene or multi-graphene may be used as the graphene compound 201. Here, the graphene compound 201 preferably has a sheet-like shape. The graphene compound 201 may be a sheet-like shape formed by partially overlapping a plurality of multi-graphenes or (and) a plurality of graphenes.

[0138] In the vertical cross section of the active material layer 200, as shown in Fig. 6A, sheet-like graphene compounds 201 are dispersed approximately uniformly inside the active material layer 200. In Fig. 6A, the graphene compounds 201 are typically represented by thick lines, but are actually thin films having a thickness corresponding to a single layer or multiple layers of carbon molecules. The multiple graphene compounds 201 are formed so as to wrap or cover the multiple granular positive electrode active materials 100, or to be attached to the surfaces of the multiple granular positive electrode active materials 100, and are therefore in surface contact with each other.

[0139] Here, a mesh-like graphene compound sheet (hereinafter referred to as a graphene compound net or graphene net) can be formed by bonding multiple graphene compounds together. When an active material is covered with a graphene net, the graphene net can also function as a binder that bonds the active materials together. Therefore, the amount of binder can be reduced or no binder can be used, and the ratio of the active material to the electrode volume or weight can be improved. In other words, the capacity of the power storage device can be increased.

[0140] Here, it is preferable to use graphene oxide as the graphene compound 201, mix it with an active material to form a layer that becomes the active material layer 200, and then reduce it. By using graphene oxide, which has extremely high dispersibility in a polar solvent, to form the graphene compound 201, it is possible to disperse the graphene compound 201 approximately uniformly inside the active material layer 200. Since the solvent is volatilized and removed from the dispersion medium containing the uniformly dispersed graphene oxide and the graphene oxide is reduced, the graphene compound 201 remaining in the active material layer 200 is dispersed to such an extent that it partially overlaps with each other and is in surface contact with each other, thereby forming a three-dimensional conductive path. Note that the reduction of the graphene oxide may be performed by, for example, heat treatment or using a reducing agent.

[0141] Therefore, unlike a granular conductive assistant such as acetylene black that makes point contact with the active material, the graphene compound 201 enables surface contact with low contact resistance, and therefore the electrical conductivity between the granular positive electrode active material 100 and the graphene compound 201 can be improved with a smaller amount than that of a normal conductive assistant. Thus, the ratio of the positive electrode active material 100 in the active material layer 200 can be increased. This can increase the discharge capacity of the power storage device.

[0142] As the binder, it is preferable to use a rubber material such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. Also, as the binder, fluororubber can be used.

[0143] Moreover, it is preferable to use, for example, a water-soluble polymer as the binder. For example, polysaccharides can be used as the water-soluble polymer. For example, cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, and regenerated cellulose, and starch can be used as the polysaccharide. It is even more preferable to use these water-soluble polymers in combination with the above-mentioned rubber material.

[0144] Alternatively, it is preferable to use materials such as polystyrene, polymethyl acrylate, polymethyl methacrylate (PMMA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene, polyisobutylene, polyethylene terephthalate, nylon, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, polyvinyl acetate, and nitrocellulose as the binder.

[0145] The binder may be used in combination of two or more of the above.

[0146] For example, a material having a particularly excellent viscosity adjusting effect may be used in combination with another material. For example, while rubber materials and the like have excellent adhesive strength and elasticity, it may be difficult to adjust the viscosity when mixed with a solvent. In such a case, it is preferable to mix the material with a material having a particularly excellent viscosity adjusting effect. For example, a water-soluble polymer may be used as a material having a particularly excellent viscosity adjusting effect. In addition, as a water-soluble polymer having a particularly excellent viscosity adjusting effect, the above-mentioned polysaccharides, for example, carboxymethylcellulose (CMC), methylcellulose, ethylcellulose, hydroxypropylcellulose, diacetylcellulose, cellulose derivatives such as regenerated cellulose, and starch may be used.

[0147] In addition, the solubility of cellulose derivatives such as carboxymethylcellulose is increased by converting them into salts such as sodium salts and ammonium salts of carboxymethylcellulose, and they are more likely to exhibit their effect as viscosity adjusters. The increased solubility can also increase the dispersibility of the active material and other components when preparing an electrode slurry. In this specification, the cellulose and cellulose derivatives used as electrode binders include their salts.

[0148] Water-soluble polymers stabilize the viscosity by dissolving in water, and can stably disperse active materials and other materials combined as binders, such as styrene-butadiene rubber, in an aqueous solution. In addition, since they have functional groups, they are expected to be easily and stably adsorbed onto the surface of active materials. In addition, many cellulose derivatives, such as carboxymethyl cellulose, have functional groups such as hydroxyl groups and carboxyl groups, and since they have functional groups, the polymers are expected to interact with each other and widely cover the surface of the active material.

[0149] When the binder covers the active material surface or contacts the surface to form a film, it is expected to function as a passive film and suppress the decomposition of the electrolyte. Here, the passive film is a film with no electrical conductivity or a film with extremely low electrical conductivity. For example, when a passive film is formed on the surface of the active material, it can suppress the decomposition of the electrolyte at the battery reaction potential. Moreover, it is more preferable that the passive film suppresses electrical conductivity and can conduct lithium ions.

[0150] <Positive electrode current collector> The positive electrode current collector may be made of a material having high electrical conductivity, such as metals such as stainless steel, gold, platinum, aluminum, and titanium, and alloys thereof. The material used for the positive electrode current collector is preferably one that does not dissolve at the potential of the positive electrode. Aluminum alloys to which elements that improve heat resistance, such as silicon, titanium, neodymium, scandium, and molybdenum, are added may be used. The positive electrode current collector may be made of a metal element that reacts with silicon to form silicide. Examples of metal elements that react with silicon to form silicide include zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, and nickel. The current collector may be in the form of a foil, plate (sheet), net, punched metal, or expanded metal. The current collector may be made of a material having a thickness of 5 μm to 30 μm.

[0151] [Negative electrode] The negative electrode includes a negative electrode active material layer and a negative electrode current collector. The negative electrode active material layer may include a conductive assistant and a binder.

[0152] <Negative electrode active material> As the negative electrode active material, for example, an alloy-based material or a carbon-based material can be used.

[0153] As the negative electrode active material, an element capable of carrying out a charge / discharge reaction by alloying / dealloying reaction with lithium can be used. For example, a material containing at least one of silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium, indium, etc. can be used. Such elements have a larger capacity than carbon, and silicon in particular has a high theoretical capacity of 4200mAh / g. For this reason, it is preferable to use silicon as the negative electrode active material. Compounds containing these elements may also be used. For example, there are SiO, Mg2Si, Mg2Ge, SnO, SnO2, Mg2Sn, SnS2, V2Sn3, FeSn2, CoSn2, Ni3Sn2, Cu6Sn5, Ag3Sn, Ag3Sb, Ni2MnSb, CeSb3, LaSn3, La3Co2Sn7, CoSb3, InSb, SbSn, etc. Here, elements capable of undergoing charge / discharge reactions through alloying / dealloying reactions with lithium, and compounds containing such elements, are sometimes referred to as alloying materials.

[0154] In this specification, SiO refers to, for example, silicon monoxide. Alternatively, SiO x Here, x preferably has a value close to 1. For example, x is preferably 0.2 or more and 1.5 or less, and more preferably 0.3 or more and 1.2 or less.

[0155] Examples of the carbon-based material that can be used include graphite, easily graphitizable carbon (soft carbon), non-graphitizable carbon (hard carbon), carbon nanotubes, graphene, and carbon black.

[0156] Examples of graphite include artificial graphite and natural graphite. Examples of artificial graphite include mesocarbon microbeads (MCMB), coke-based artificial graphite, and pitch-based artificial graphite. Here, as the artificial graphite, spherical graphite having a spherical shape can be used. For example, MCMB may have a spherical shape, which is preferable. In addition, it is relatively easy to reduce the surface area of ​​MCMB, which may be preferable. Examples of natural graphite include flake graphite and spheroidized natural graphite.

[0157] When lithium ions are inserted into graphite (when lithium-graphite intercalation compounds are formed), graphite exhibits a low potential similar to that of lithium metal (0.05 V to 0.3 V vs. Li / Li + ) This allows lithium-ion secondary batteries to exhibit high operating voltages. Furthermore, graphite is preferred because it has the advantages of relatively high capacity per unit volume, relatively small volume expansion, low cost, and high safety compared to lithium metal.

[0158] In addition, titanium dioxide (TiO2), lithium titanium oxide (Li4Ti5O 12 ), lithium-graphite intercalation compound (Li x C6), niobium pentoxide (Nb2O5), tungsten oxide (WO2), molybdenum oxide (MoO2), and other oxides can be used.

[0159] In addition, the negative electrode active material is a composite nitride of lithium and transition metals, Li3N type structure Li 3-x M x N (M=Co, Ni, Cu) can be used. For example, Li 2.6 Co 0.4 N3 has a large charge / discharge capacity (900mAh / g, 1890mAh / cm 3 ) and is preferred.

[0160] When a composite nitride of lithium and a transition metal is used, lithium ions are contained in the negative electrode active material, and therefore it is preferable to combine it with a material that does not contain lithium ions, such as V2O5 or Cr3O8, as the positive electrode active material. Even when a material that contains lithium ions is used as the positive electrode active material, the composite nitride of lithium and a transition metal can be used as the negative electrode active material by first removing the lithium ions contained in the positive electrode active material.

[0161] In addition, materials that undergo a conversion reaction can also be used as the negative electrode active material. For example, transition metal oxides that do not form an alloy with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), and iron oxide (FeO), can be used as the negative electrode active material. Further examples of materials that undergo a conversion reaction include oxides such as Fe2O3, CuO, Cu2O, RuO2, and Cr2O3, and CoS 0.89 It also occurs in sulfides such as NiS and CuS, nitrides such as Zn3N2, Cu3N and Ge3N4, phosphides such as NiP2, FeP2 and CoP3, and fluorides such as FeF3 and BiF3.

[0162] As the conductive assistant and binder that the negative electrode active material layer can have, the same materials as the conductive assistant and binder that the positive electrode active material layer can have can be used.

[0163] <Negative electrode current collector> The negative electrode current collector may be made of the same material as the positive electrode current collector, but it is preferable that the negative electrode current collector is made of a material that does not form an alloy with carrier ions such as lithium.

[0164] [Electrolyte] The electrolytic solution has a solvent and an electrolyte. The solvent of the electrolytic solution is preferably an aprotic organic solvent, and for example, one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chloroethylene carbonate, vinylene carbonate, γ-butyrolactone, γ-valerolactone, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, 1,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), dimethyl sulfoxide, diethyl ether, methyl diglyme, acetonitrile, benzonitrile, tetrahydrofuran, sulfolane, sultone, etc., or two or more of these can be used in any combination and ratio.

[0165] In addition, by using one or more ionic liquids (room-temperature molten salts) that are flame-retardant and non-volatile as a solvent for the electrolyte, even if the internal temperature of the electricity storage device rises due to an internal short circuit or overcharging, the electricity storage device can be prevented from bursting or catching fire. The ionic liquid is composed of a cation and an anion, and includes an organic cation and an anion. Examples of the organic cation used in the electrolyte include aliphatic onium cations such as quaternary ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations, and aromatic cations such as imidazolium cations and pyridinium cations. Examples of the anion used in the electrolyte include monovalent amide anions, monovalent methide anions, fluorosulfonic acid anions, perfluoroalkylsulfonic acid anions, tetrafluoroborate anions, perfluoroalkylborate anions, hexafluorophosphate anions, and perfluoroalkylphosphate anions.

[0166] Examples of the electrolyte to be dissolved in the above-mentioned solvent include LiPF6, LiClO4, LiAsF6, LiBF4, LiAlCl4, LiSCN, LiBr, LiI, Li2SO4, and Li2B 10 Cl 10 , Li2B 12 Cl 12 Lithium salts such as LiCF3SO3, LiC4F9SO3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiN(CF3SO2)2, LiN(C4F9SO2)(CF3SO2), LiN(C2F5SO2)2, etc. can be used alone or in any combination and ratio of two or more of these.

[0167] The electrolyte used in the electricity storage device is preferably a highly purified electrolyte with a low content of granular waste and elements other than the constituent elements of the electrolyte (hereinafter, simply referred to as "impurities"). Specifically, the weight ratio of impurities to the electrolyte is preferably 1% or less, more preferably 0.1% or less, and even more preferably 0.01% or less.

[0168] In addition, additives such as vinylene carbonate, propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate)borate (LiBOB), and dinitrile compounds such as succinonitrile and adiponitrile may be added to the electrolyte solution. The concentration of the additive may be, for example, 0.1 weight % or more and 5 weight % or less with respect to the entire solvent.

[0169] Alternatively, a polymer gel electrolyte may be used in which a polymer is swollen with an electrolytic solution.

[0170] The use of a polymer gel electrolyte improves safety against leakage, etc. Also, it is possible to make the secondary battery thinner and lighter.

[0171] Examples of the polymer to be gelled include silicone gel, acrylic gel, acrylonitrile gel, polyethylene oxide gel, polypropylene oxide gel, and fluorine-based polymer gel. For example, polymers having a polyalkylene oxide structure such as polyethylene oxide (PEO), PVDF, polyacrylonitrile, and copolymers containing these can be used. For example, PVDF-HFP, which is a copolymer of PVDF and hexafluoropropylene (HFP), can be used. The polymer to be formed may also have a porous shape.

[0172] In addition, instead of the electrolyte, a solid electrolyte containing inorganic materials such as sulfides or oxides, or a solid electrolyte containing polymeric materials such as PEO (polyethylene oxide) can be used. When using a solid electrolyte, the installation of a separator or spacer becomes unnecessary. In addition, since the entire battery can be solidified, there is no risk of leakage, and safety is dramatically improved.

[0173] (Embodiment 4) In this embodiment, an example of the shape of a secondary battery including the positive electrode active material 100 described in the previous embodiment will be described. The description in the previous embodiment can be referred to for the material used in the secondary battery described in this embodiment.

[0174] [Coin-type secondary battery] First, an example of a coin-type secondary battery will be described. Fig. 7A is an external view of a coin-type (single-layer flat) secondary battery, and Fig. 7B is a cross-sectional view thereof.

[0175] In the coin-type secondary battery 300, a positive electrode can 301, which also serves as a positive electrode terminal, and a negative electrode can 302, which also serves as a negative electrode terminal, are insulated and sealed with a gasket 303 made of polypropylene or the like. The positive electrode 304 is formed of a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector. The negative electrode 307 is formed of a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode current collector.

[0176] In addition, the positive electrode 304 and the negative electrode 307 used in the coin-type secondary battery 300 each need only have an active material layer formed on one side.

[0177] Metals such as nickel, aluminum, and titanium that are corrosion-resistant to the electrolyte, or alloys of these metals and other metals (e.g., stainless steel, etc.) can be used for the positive electrode can 301 and the negative electrode can 302. In order to prevent corrosion by the electrolyte, it is preferable to coat them with nickel, aluminum, etc. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.

[0178] These negative electrode 307, positive electrode 304, and separator 310 are impregnated with an electrolyte, and as shown in FIG. 7B, positive electrode can 301 is placed at the bottom, and positive electrode 304, separator 310, negative electrode 307, and negative electrode can 302 are stacked in this order, and positive electrode can 301 and negative electrode can 302 are crimped together via gasket 303, to produce coin-type secondary battery 300.

[0179] By using the positive electrode active material particles described in the above embodiment for the positive electrode 304, the coin-type secondary battery 300 can be made less susceptible to deterioration and highly safe.

[0180] [Separator] The secondary battery preferably has a separator. The separator may be made of, for example, paper or other cellulose-containing fibers, nonwoven fabric, glass fiber, ceramics, or synthetic fibers using nylon (polyamide), vinylon (polyvinyl alcohol-based fibers), polyester, acrylic, polyolefin, or polyurethane. The separator is preferably processed into a bag shape and disposed so as to encase either the positive electrode or the negative electrode.

[0181] The separator may have a multi-layer structure. For example, an organic material film such as polypropylene or polyethylene may be coated with a ceramic material, a fluorine material, a polyamide material, or a mixture of these. As the ceramic material, for example, aluminum oxide particles or silicon oxide particles may be used. As the fluorine material, for example, PVDF or polytetrafluoroethylene may be used. As the polyamide material, for example, nylon or aramid (meta-aramid or para-aramid) may be used.

[0182] Coating with ceramic materials improves oxidation resistance, suppressing the deterioration of the separator during high-voltage charging and discharging, and improving the reliability of the secondary battery. Coating with fluorine-based materials also improves adhesion between the separator and electrodes, improving output characteristics. Coating with polyamide-based materials, especially aramid, improves heat resistance, improving the safety of the secondary battery.

[0183] For example, both sides of a polypropylene film may be coated with a mixture of aluminum oxide and aramid.Alternatively, the surface of the polypropylene film that contacts the positive electrode may be coated with a mixture of aluminum oxide and aramid, and the surface that contacts the negative electrode may be coated with a fluorine-based material.

[0184] By using a separator with a multi-layer structure, the safety of the secondary battery can be maintained even if the overall thickness of the separator is thin, and therefore the capacity per volume of the secondary battery can be increased.

[0185] [Cylindrical secondary battery] An example of a cylindrical secondary battery will be described with reference to Figures 8A to 8D. As shown in Figures 8A and 8B, a cylindrical secondary battery 600 has a positive electrode cap (battery lid) 601 on the top surface, and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap and the battery can (external can) 602 are insulated by a gasket (insulating packing) 610.

[0186] FIG. 8B is a schematic diagram showing a cross section of a cylindrical secondary battery. Inside a hollow cylindrical battery can 602, a battery element is provided in which a strip-shaped positive electrode 604 and a negative electrode 606 are wound with a separator 605 sandwiched therebetween. Although not shown, the battery element is wound around a center pin. One end of the battery can 602 is closed and the other end is open. For the battery can 602, metals such as nickel, aluminum, and titanium that are resistant to corrosion by the electrolyte, or alloys of these metals and other metals (e.g., stainless steel, etc.) can be used. In addition, it is preferable to coat the battery can 602 with nickel, aluminum, or the like to prevent corrosion by the electrolyte. Inside the battery can 602, the battery element in which the positive electrode, negative electrode, and separator are wound is sandwiched between a pair of opposing insulating plates 608 and 609. In addition, a nonaqueous electrolyte (not shown) is injected into the inside of the battery can 602 in which the battery element is provided. The non-aqueous electrolyte may be the same as that used in a coin-type secondary battery.

[0187] Since the positive and negative electrodes used in a cylindrical storage battery are wound, it is preferable to form an active material on both sides of the current collector. A positive electrode terminal (positive electrode current collector lead) 603 is connected to the positive electrode 604, and a negative electrode terminal (negative electrode current collector lead) 607 is connected to the negative electrode 606. Both the positive electrode terminal 603 and the negative electrode terminal 607 can be made of a metal material such as aluminum. The positive electrode terminal 603 is resistance-welded to a safety valve mechanism 612, and the negative electrode terminal 607 is resistance-welded to the bottom of the battery can 602. The safety valve mechanism 612 is electrically connected to the positive electrode cap 601 via a PTC element (Positive Temperature Coefficient) 611. The safety valve mechanism 612 cuts off the electrical connection between the positive electrode cap 601 and the positive electrode 604 when the rise in the internal pressure of the battery exceeds a predetermined threshold value. The PTC element 611 is a thermosensitive resistor whose resistance increases when the temperature rises, and the increase in resistance limits the amount of current to prevent abnormal heat generation. Barium titanate (BaTiO3)-based semiconductor ceramics can be used for the PTC element.

[0188] 8C, a plurality of secondary batteries 600 may be sandwiched between conductive plates 613 and 614 to form a module 615. The plurality of secondary batteries 600 may be connected in parallel, in series, or in parallel and then further in series. By forming a module 615 having a plurality of secondary batteries 600, a large amount of power can be extracted.

[0189] FIG. 8D is a top view of the module 615. To clarify the drawing, the conductive plate 613 is shown with a dotted line. As shown in FIG. 8D, the module 615 may have a conductor 616 that electrically connects the multiple secondary batteries 600. A conductive plate can be provided by overlapping the conductor 616. Also, a temperature control device 617 may be provided between the multiple secondary batteries 600. When the secondary battery 600 is overheated, it can be cooled by the temperature control device 617, and when the secondary battery 600 is too cold, it can be heated by the temperature control device 617. Therefore, the performance of the module 615 is less affected by the outside air temperature.

[0190] By using the positive electrode active material 100 described in the above embodiment for the positive electrode 604, the cylindrical secondary battery 600 can be made less susceptible to deterioration and highly safe.

[0191] [Structural example of power storage device] Another structural example of the power storage device will be described with reference to FIGS.

[0192] 9A and 9B are diagrams showing the external appearance of a power storage device. The power storage device has a circuit board 900 and a secondary battery 913. A label 910 is attached to the secondary battery 913. Furthermore, as shown in FIG. 9B, the power storage device has a terminal 951, a terminal 952, an antenna 914, and an antenna 915.

[0193] The circuit board 900 has a terminal 911 and a circuit 912. The terminal 911 is connected to a terminal 951, a terminal 952, an antenna 914, an antenna 915, and the circuit 912. Note that a plurality of terminals 911 may be provided, and each of the plurality of terminals 911 may be a control signal input terminal, a power supply terminal, or the like.

[0194] The circuit 912 may be provided on the back surface of the circuit board 900. The antennas 914 and 915 are not limited to being coil-shaped, and may be, for example, wire-shaped or plate-shaped. In addition, antennas such as planar antennas, aperture antennas, traveling wave antennas, EH antennas, magnetic field antennas, and dielectric antennas may be used. Alternatively, the antennas 914 and 915 may be flat conductors. This flat conductor can function as one of the conductors for electric field coupling. In other words, the antennas 914 and 915 may function as one of the two conductors of the capacitor. This allows power to be exchanged not only by electromagnetic fields and magnetic fields, but also by electric fields.

[0195] The line width of the antenna 914 is preferably larger than the line width of the antenna 915. This allows the amount of power received by the antenna 914 to be increased.

[0196] The power storage device includes a layer 916 between the antenna 914 and the antenna 915 and the secondary battery 913. The layer 916 has a function of shielding, for example, an electromagnetic field generated by the secondary battery 913. The layer 916 can be formed using, for example, a magnetic material.

[0197] The structure of the power storage device is not limited to that shown in FIG.

[0198] For example, as shown in Fig. 10A1 and Fig. 10A2, an antenna may be provided on each of a pair of opposing surfaces of the secondary battery 913 shown in Fig. 9A and Fig. 9B. Fig. 10A1 is an external view of the pair of surfaces as viewed from one side, and Fig. 10A2 is an external view of the pair of surfaces as viewed from the other side. Note that the description of the power storage device shown in Fig. 9A and Fig. 9B can be used as appropriate for the same parts as those of the power storage device shown in Fig. 9A and Fig. 9B.

[0199] 10A1, an antenna 914 is provided on one of a pair of surfaces of a secondary battery 913 with a layer 916 sandwiched therebetween, and as shown in Fig. 10A2, an antenna 915 is provided on the other of the pair of surfaces of the secondary battery 913 with a layer 917 sandwiched therebetween. The layer 917 has a function of shielding, for example, an electromagnetic field caused by the secondary battery 913. The layer 917 can be made of, for example, a magnetic material.

[0200] By using the above structure, the size of both antenna 914 and antenna 915 can be increased.

[0201] Alternatively, as shown in Fig. 10B1 and Fig. 10B2, a separate antenna may be provided on each of a pair of opposing surfaces of the secondary battery 913 shown in Fig. 9A and Fig. 9B. Fig. 10B1 is an external view of the pair of surfaces as viewed from one side, and Fig. 10B2 is an external view of the pair of surfaces as viewed from the other side. Note that the description of the power storage device shown in Fig. 9A and Fig. 9B can be used as appropriate for the same parts as those of the power storage device shown in Fig. 9A and Fig. 9B.

[0202] As shown in Fig. 10B1, antennas 914 and 915 are provided on one of a pair of surfaces of a secondary battery 913 with a layer 916 interposed therebetween, and as shown in Fig. 10B2, antenna 918 is provided on the other of the pair of surfaces of the secondary battery 913 with a layer 917 interposed therebetween. The antenna 918 has a function of performing data communication with an external device, for example. For example, an antenna having a shape applicable to the antennas 914 and 915 can be applied to the antenna 918. As a communication method between the power storage device and another device via the antenna 918, a response method that can be used between the power storage device and another device, such as NFC, can be applied.

[0203] 11A, a display device 920 may be provided on the secondary battery 913 shown in FIGS. 9A and 9B. The display device 920 is electrically connected to a terminal 911 via a terminal 919. Note that the label 910 does not need to be provided on the portion where the display device 920 is provided. Note that the description of the power storage device shown in FIGS. 9A and 9B can be appropriately applied to the same portions as those of the power storage device shown in FIGS. 9A and 9B.

[0204] For example, an image indicating whether charging is in progress, an image indicating the amount of stored power, etc. may be displayed on the display device 920. For example, electronic paper, a liquid crystal display device, an electroluminescence (EL) display device, etc. can be used as the display device 920. For example, the use of electronic paper can reduce the power consumption of the display device 920.

[0205] 11B, a sensor 921 may be provided in the secondary battery 913 shown in FIGS. 9A and 9B. The sensor 921 is electrically connected to a terminal 911 via a terminal 922. Note that the description of the power storage device shown in FIGS. 9A and 9B can be used as appropriate for the same parts as those of the power storage device shown in FIGS. 9A and 9B.

[0206] The sensor 921 may have a function of measuring, for example, displacement, position, speed, acceleration, angular speed, rotation speed, distance, light, liquid, magnetism, temperature, chemical substances, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor, or infrared ray. By providing the sensor 921, for example, data indicating the environment in which the power storage device is placed (such as temperature) can be detected and stored in the memory in the circuit 912.

[0207] Further, a structural example of the secondary battery 913 will be described with reference to FIGS.

[0208] A secondary battery 913 shown in FIG. 12A has a wound body 950 in which terminals 951 and 952 are provided inside a housing 930. The wound body 950 is impregnated with an electrolyte inside the housing 930. The terminal 952 contacts the housing 930, and the terminal 951 does not contact the housing 930 by using an insulating material or the like. Note that in FIG. 12A, the housing 930 is illustrated separately for convenience, but in reality, the wound body 950 is covered by the housing 930, and the terminals 951 and 952 extend outside the housing 930. The housing 930 can be made of a metal material (e.g., aluminum) or a resin material.

[0209] As shown in Fig. 12B, the housing 930 shown in Fig. 12A may be formed of a plurality of materials. For example, the secondary battery 913 shown in Fig. 12B has a housing 930a and a housing 930b bonded together, and a wound body 950 is provided in the area surrounded by the housings 930a and 930b.

[0210] The housing 930a can be made of an insulating material such as organic resin. In particular, by using a material such as organic resin on the surface on which the antenna is formed, it is possible to suppress shielding of the electric field by the secondary battery 913. Note that if the shielding of the electric field by the housing 930a is small, antennas such as antenna 914 and antenna 915 may be provided inside the housing 930a. The housing 930b can be made of, for example, a metal material.

[0211] 13 shows the structure of the wound body 950. The wound body 950 has a negative electrode 931, a positive electrode 932, and a separator 933. The wound body 950 is a wound body in which the negative electrode 931 and the positive electrode 932 are stacked with the separator 933 sandwiched therebetween, and the laminated sheet is wound. Note that the stack of the negative electrode 931, the positive electrode 932, and the separator 933 may be stacked a plurality of times.

[0212] 9 via one of the terminal 951 and the terminal 952. The positive electrode 932 is connected to the terminal 911 shown in FIG.

[0213] By using the positive electrode active material particles described in the above embodiment for the positive electrode 932, the secondary battery 913 which is less susceptible to deterioration and has high safety can be provided.

[0214] [Laminated secondary battery] Next, examples of laminated secondary batteries will be described with reference to Figures 14 to 19. If the laminated secondary battery has a flexible configuration, and is mounted in an electronic device having at least a flexible portion, the secondary battery can be bent in accordance with the deformation of the electronic device.

[0215] A laminated secondary battery 980 will be described with reference to Fig. 14. The laminated secondary battery 980 has a wound body 993 shown in Fig. 14A. The wound body 993 has a negative electrode 994, a positive electrode 995, and a separator 996. The wound body 993 is formed by stacking the negative electrode 994 and the positive electrode 995 with the separator 996 sandwiched therebetween, in the same manner as the wound body 950 described in Fig. 13, and winding the laminated sheet.

[0216] The number of layers of the negative electrode 994, the positive electrode 995, and the separator 996 may be appropriately designed according to the required capacity and element volume. The negative electrode 994 is connected to a negative electrode current collector (not shown) via one of the lead electrodes 997 and 998, and the positive electrode 995 is connected to a positive electrode current collector (not shown) via the other of the lead electrodes 997 and 998.

[0217] As shown in Fig. 14B, a film 981 serving as an exterior body and a film 982 having a recess are bonded together by thermocompression or the like to form a space, and the above-mentioned wound body 993 is stored in the space, thereby producing a secondary battery 980 as shown in Fig. 14C. The wound body 993 has lead electrodes 997 and 998, and is impregnated with an electrolyte solution between the film 981 and the film 982 having a recess.

[0218] For example, a metal material such as aluminum or a resin material can be used for the film 981 and the film 982 having the recesses. If a resin material is used as the material for the film 981 and the film 982 having the recesses, the film 981 and the film 982 having the recesses can be deformed when an external force is applied, and a flexible storage battery can be produced.

[0219] Although an example in which two films are used is shown in FIG. 14B and FIG. 14C, a space may be formed by folding one film, and the above-mentioned wound body 993 may be housed in the space.

[0220] By using the positive electrode active material particles described in the above embodiment for the positive electrode 995, the secondary battery 980 can be made less susceptible to deterioration and highly safe.

[0221] In addition, in FIG. 14, an example of a secondary battery 980 having a wound body in a space formed by a film that serves as an outer casing is described. However, as shown in FIG. 15, for example, a secondary battery may also be used that has a plurality of rectangular positive electrodes, separators, and negative electrodes in a space formed by a film that serves as an outer casing.

[0222] 15A includes a positive electrode 503 having a positive electrode current collector 501 and a positive electrode active material layer 502, a negative electrode 506 having a negative electrode current collector 504 and a negative electrode active material layer 505, a separator 507, an electrolyte 508, and an exterior body 509. The separator 507 is disposed between the positive electrode 503 and the negative electrode 506 provided in the exterior body 509. The interior of the exterior body 509 is filled with the electrolyte 508. The electrolyte solution described in Embodiment 2 can be used as the electrolyte solution 508.

[0223] 15A, the positive electrode current collector 501 and the negative electrode current collector 504 also serve as terminals for obtaining electrical contact with the outside. Therefore, the positive electrode current collector 501 and the negative electrode current collector 504 may be arranged so as to be partially exposed to the outside from the exterior body 509. Alternatively, the positive electrode current collector 501 and the negative electrode current collector 504 may not be exposed to the outside from the exterior body 509, but may be exposed to the outside by using a lead electrode and ultrasonically bonding the lead electrode to the positive electrode current collector 501 or the negative electrode current collector 504.

[0224] In the laminated secondary battery 500, the exterior body 509 may be a three-layer laminate film having a highly flexible thin metal film such as aluminum, stainless steel, copper, nickel, etc., provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, polyamide, etc., and further having an insulating synthetic resin film such as a polyamide-based resin, polyester-based resin, etc., provided on the thin metal film as the outer surface of the exterior body.

[0225] 15B shows an example of the cross-sectional structure of a laminated secondary battery 500. For simplicity, Fig. 15A shows an example formed of two current collectors, but in reality, the battery is formed of a plurality of electrode layers.

[0226] In FIG. 15B, the number of electrode layers is 16 as an example. Even if the number of electrode layers is 16, the secondary battery 500 has flexibility. FIG. 15B shows a structure of 16 layers in total, including 8 layers of negative electrode collector 504 and 8 layers of positive electrode collector 501. FIG. 15B shows a cross section of the negative electrode lead-out portion, in which 8 layers of negative electrode collector 504 are ultrasonically bonded. Of course, the number of electrode layers is not limited to 16, and may be more or less. When the number of electrode layers is large, a secondary battery having a larger capacity can be obtained. Also, when the number of electrode layers is small, a secondary battery that can be made thin and has excellent flexibility can be obtained.

[0227] 16 and 17 show an example of an external view of a laminated secondary battery 500. In FIG. 16 and FIG. 17, a positive electrode 503, a negative electrode 506, a separator 507, an exterior body 509, a positive electrode lead electrode 510, and a negative electrode lead electrode 511 are provided.

[0228] FIG. 18A shows an external view of a positive electrode 503 and a negative electrode 506. The positive electrode 503 has a positive electrode current collector 501, and a positive electrode active material layer 502 is formed on the surface of the positive electrode current collector 501. The positive electrode 503 has a region where the positive electrode current collector 501 is partially exposed (hereinafter referred to as a tab region). The negative electrode 506 has a negative electrode current collector 504, and a negative electrode active material layer 505 is formed on the surface of the negative electrode current collector 504. The negative electrode 506 has a region where the negative electrode current collector 504 is partially exposed, that is, a tab region. The areas and shapes of the tab regions of the positive electrode and the negative electrode are not limited to the example shown in FIG. 18A.

[0229] [Method of manufacturing laminated secondary battery] Here, an example of a method for producing the laminate type secondary battery whose external view is shown in FIG. 16 will be described with reference to FIGS. 18B and 18C.

[0230] First, the negative electrode 506, the separator 507, and the positive electrode 503 are laminated. FIG. 18B shows the laminated negative electrode 506, the separator 507, and the positive electrode 503. Here, an example is shown in which five pairs of negative electrodes and four pairs of positive electrodes are used. Next, the tab regions of the positive electrodes 503 are bonded to each other, and the positive electrode lead electrode 510 is bonded to the tab region of the outermost positive electrode. For example, ultrasonic welding or the like may be used for the bonding. Similarly, the tab regions of the negative electrodes 506 are bonded to each other, and the negative electrode lead electrode 511 is bonded to the tab region of the outermost negative electrode.

[0231] Next, the negative electrode 506 , the separator 507 and the positive electrode 503 are placed on the exterior body 509 .

[0232] Next, as shown in Fig. 18C, exterior body 509 is folded at the portion indicated by the dashed line. After that, the outer periphery of exterior body 509 is joined. For the joining, for example, thermocompression bonding or the like may be used. At this time, a region (hereinafter referred to as an inlet) that is not joined is provided in a part (or one side) of exterior body 509 so that electrolyte 508 can be introduced later.

[0233] Next, electrolytic solution 508 is introduced into the inside of exterior body 509 through an inlet provided in exterior body 509. The introduction of electrolytic solution 508 is preferably performed under a reduced pressure atmosphere or an inert atmosphere. Finally, the inlet is joined. In this manner, secondary battery 500, which is a laminated type secondary battery, can be produced.

[0234] By using the positive electrode active material particles described in the above embodiment for the positive electrode 503, the secondary battery 500 can be made less susceptible to deterioration and highly safe.

[0235] [Bendable secondary battery] Next, an example of a bendable secondary battery will be described with reference to FIGS.

[0236] FIG. 19A shows a schematic top view of a bendable battery 250. FIG. 19B1, FIG. 19B2, and FIG. 19C are schematic cross-sectional views taken along the chain lines C1-C2, C3-C4, and A1-A2 in FIG. 19A, respectively. The battery 250 has an exterior body 251, and a positive electrode 211a and a negative electrode 211b housed inside the exterior body 251. A lead 212a electrically connected to the positive electrode 211a and a lead 212b electrically connected to the negative electrode 211b extend outside the exterior body 251. In addition to the positive electrode 211a and the negative electrode 211b, an electrolyte (not shown) is enclosed in the area surrounded by the exterior body 251.

[0237] The positive electrode 211a and the negative electrode 211b of the battery 250 will be described with reference to Fig. 20. Fig. 20A is a perspective view illustrating the stacking order of the positive electrode 211a, the negative electrode 211b, and the separator 214. Fig. 20B is a perspective view showing the lead 212a and the lead 212b in addition to the positive electrode 211a and the negative electrode 211b.

[0238] 20A, battery 250 has a plurality of rectangular positive electrodes 211a, a plurality of rectangular negative electrodes 211b, and a plurality of separators 214. Positive electrode 211a and negative electrode 211b each have a protruding tab portion and a portion other than the tab. A positive electrode active material layer is formed on one surface of positive electrode 211a in the portion other than the tab, and a negative electrode active material layer is formed on one surface of negative electrode 211b in the portion other than the tab.

[0239] The positive electrode 211a and the negative electrode 211b are stacked so that the surfaces of the positive electrode 211a on which the positive electrode active material layer is not formed and the surfaces of the negative electrode 211b on which the negative electrode active material layer is not formed are in contact with each other.

[0240] Furthermore, a separator 214 is provided between the surface of the positive electrode 211a on which the positive electrode active material is formed and the surface of the negative electrode 211b on which the negative electrode active material is formed. In Fig. 20, the separator 214 is indicated by a dotted line for ease of viewing.

[0241] 20B, the multiple positive electrodes 211a and the lead 212a are electrically connected at a joint 215a, and the multiple negative electrodes 211b and the lead 212b are electrically connected at a joint 215b.

[0242] Next, exterior body 251 will be described with reference to FIGS. 19B1, 19B2, 19C, and 19D.

[0243] The exterior body 251 has a film-like shape and is folded in two to sandwich the positive electrode 211a and the negative electrode 211b. The exterior body 251 has a folded portion 261, a pair of sealing portions 262, and a sealing portion 263. The pair of sealing portions 262 are provided to sandwich the positive electrode 211a and the negative electrode 211b, and can also be called side seals. The sealing portion 263 has a portion overlapping the lead 212a and the lead 212b, and can also be called a top seal.

[0244] It is preferable that exterior body 251 has a corrugated shape in which ridge lines 271 and valley lines 272 are alternately arranged in the portions overlapping with positive electrode 211a and negative electrode 211b. In addition, it is preferable that seal portion 262 and seal portion 263 of exterior body 251 are flat.

[0245] Fig. 19B1 is a cross section taken at a portion overlapping with ridge line 271, and Fig. 19B2 is a cross section taken at a portion overlapping with valley line 272. Fig. 19B1 and Fig. 19B2 both correspond to widthwise cross sections of battery 250 and positive electrode 211a and negative electrode 211b.

[0246] Here, the distance between the ends of the positive electrode 211a and the negative electrode 211b in the width direction, i.e., the ends of the positive electrode 211a and the negative electrode 211b, and the seal portion 262 is defined as the distance La. When the battery 250 is deformed, such as by bending, the positive electrode 211a and the negative electrode 211b are deformed so as to be displaced from each other in the length direction, as described below. At that time, if the distance La is too short, the exterior body 251 and the positive electrode 211a and the negative electrode 211b may rub strongly against each other, and the exterior body 251 may be damaged. In particular, if the metal film of the exterior body 251 is exposed, the metal film may be corroded by the electrolyte. Therefore, it is preferable to set the distance La as long as possible. On the other hand, if the distance La is made too large, the volume of the battery 250 increases.

[0247] Moreover, it is preferable that the distance La between the positive electrode 211a and the negative electrode 211b and the seal portion 262 is increased as the total thickness of the stacked positive electrode 211a and negative electrode 211b is increased.

[0248] More specifically, when the total thickness of the laminated positive electrode 211a and negative electrode 211b is taken as thickness t, the distance La is preferably 0.8 to 3.0 times, more preferably 0.9 to 2.5 times, and even more preferably 1.0 to 2.0 times, of the thickness t. By setting the distance La in this range, a compact battery with high reliability against bending can be realized.

[0249] Furthermore, when the distance between the pair of seal portions 262 is distance Lb, it is preferable to set distance Lb sufficiently larger than the width of positive electrode 211a and negative electrode 211b (here, width Wb of negative electrode 211b). As a result, even if positive electrode 211a and negative electrode 211b come into contact with exterior body 251 when battery 250 is repeatedly deformed, such as by bending, parts of positive electrode 211a and negative electrode 211b can be displaced in the width direction, so that rubbing between positive electrode 211a and negative electrode 211b and exterior body 251 can be effectively prevented.

[0250] For example, it is preferable that the difference between the distance La between the pair of seal portions 262 and the width Wb of the negative electrode 211b is 1.6 to 6.0 times, preferably 1.8 to 5.0 times, and more preferably 2.0 to 4.0 times the thickness t of the positive electrode 211a and the negative electrode 211b.

[0251] In other words, it is preferable that the distance Lb, the width Wb, and the thickness t satisfy the relationship of the following formula 7.

[0252]

number

[0253] Here, a satisfies the range of 0.8 to 3.0, preferably 0.9 to 2.5, and more preferably 1.0 to 2.0.

[0254] 19C is a cross section including lead 212a, and corresponds to a cross section in the longitudinal direction of battery 250, positive electrode 211a, and negative electrode 211b. As shown in FIG. 19C, it is preferable to have a space 273 between exterior body 251 and the ends of positive electrode 211a and negative electrode 211b in the longitudinal direction at bent portion 261.

[0255] Fig. 19D shows a schematic cross-sectional view of the bent battery 250. Fig. 19D corresponds to the cross section taken along the line B1-B2 in Fig. 19A.

[0256] When the battery 250 is bent, a part of the exterior body 251 located on the outside of the bend is stretched, and another part located on the inside is deformed so as to contract. More specifically, the part located on the outside of the exterior body 251 is deformed so that the wave amplitude becomes smaller and the wave period becomes larger. On the other hand, the part located on the inside of the exterior body 251 is deformed so that the wave amplitude becomes larger and the wave period becomes smaller. In this way, the deformation of the exterior body 251 relieves the stress applied to the exterior body 251 due to bending, so that the material constituting the exterior body 251 itself does not need to expand or contract. As a result, the exterior body 251 is not damaged, and the battery 250 can be bent with a small force.

[0257] 19D, when the battery 250 is bent, the positive electrode 211a and the negative electrode 211b are displaced relative to each other. At this time, since one end of the multiple stacked positive electrodes 211a and negative electrodes 211b on the seal portion 263 side is fixed by the fixing member 217, the multiple stacked positive electrodes 211a and negative electrodes 211b are displaced such that the amount of displacement increases toward the bent portion 261. This relieves the stress applied to the positive electrodes 211a and negative electrodes 211b, and the positive electrodes 211a and negative electrodes 211b themselves do not need to expand or contract. As a result, the battery 250 can be bent without damaging the positive electrodes 211a and negative electrodes 211b.

[0258] Furthermore, by providing space 273 between positive electrode 211a and negative electrode 211b and exterior body 251, when bent, positive electrode 211a and negative electrode 211b located on the inside can shift relative to exterior body 251 without coming into contact with the exterior body 251.

[0259] 19 and 20 is a battery that is unlikely to suffer damage to the exterior body, the positive electrode 211a, the negative electrode 211b, etc., even when repeatedly bent and stretched, and the battery characteristics are unlikely to deteriorate. By using the positive electrode active material particles described in the previous embodiment for the positive electrode 211a of the battery 250, it is possible to obtain a secondary battery that is even less prone to deterioration and has a high level of safety.

[0260] (Embodiment 5) In this embodiment, an example in which a secondary battery which is one embodiment of the present invention is mounted on an electronic device will be described.

[0261] First, an example of mounting the bendable secondary battery described in part of the third embodiment in an electronic device is shown in Fig. 21. Examples of electronic devices to which the bendable secondary battery is applied include television devices (also called televisions or television receivers), computer monitors, digital cameras, digital video cameras, digital photo frames, mobile phones (also called mobile phones or mobile phone devices), portable game machines, personal digital assistants, audio playback devices, and large game machines such as pachinko machines.

[0262] Furthermore, a secondary battery having a flexible shape can be incorporated into the inner or outer wall of a house or building, or along the curved surface of the interior or exterior of an automobile.

[0263] 21A shows an example of a mobile phone. The mobile phone 7400 includes a display unit 7402 built into a housing 7401, operation buttons 7403, an external connection port 7404, a speaker 7405, a microphone 7406, and the like. The mobile phone 7400 includes a secondary battery 7407.

[0264] FIG. 21B shows a state in which the mobile phone 7400 is bent. When the mobile phone 7400 is deformed by an external force and bent as a whole, the secondary battery 7407 provided inside is also bent. FIG. 21C shows the state of the bent secondary battery 7407 at that time. The secondary battery 7407 is a thin storage battery. The secondary battery 7407 is fixed in a bent state. The secondary battery 7407 has a lead electrode 7408 electrically connected to a current collector 7409.

[0265] FIG. 21D shows an example of a bangle-type display device. The portable display device 7100 includes a housing 7101, a display unit 7102, an operation button 7103, and a secondary battery 7104. FIG. 21E shows a bent state of the secondary battery 7104. When the secondary battery 7104 is bent and worn on the user's arm, the housing is deformed, and the curvature of part or all of the secondary battery 7104 changes. The degree of bending at any point of the curve is expressed by the value of the radius of the corresponding circle, and the reciprocal of the radius of curvature is called the curvature. Specifically, part or all of the main surface of the housing or the secondary battery 7104 changes within a range of the radius of curvature of 40 mm or more and 150 mm or less. If the radius of curvature of the main surface of the secondary battery 7104 is within a range of 40 mm or more and 150 mm or less, high reliability can be maintained.

[0266] 21F shows an example of a wristwatch-type portable information terminal 7200. A portable information terminal 7200 includes a housing 7201, a display portion 7202, a band 7203, a buckle 7204, operation buttons 7205, an input / output terminal 7206, and the like.

[0267] The portable information terminal 7200 can execute various applications such as mobile telephone, e-mail, document browsing and creation, music playback, Internet communication, and computer games.

[0268] The display surface of the display portion 7202 is curved, and display can be performed along the curved display surface. The display portion 7202 is also provided with a touch sensor, and can be operated by touching the screen with a finger, a stylus, or the like. For example, an application can be started by touching an icon 7207 displayed on the display portion 7202.

[0269] The operation button 7205 can have various functions, such as time setting, power on / off operation, wireless communication on / off operation, silent mode activation / cancellation, power saving mode activation / cancellation, etc. For example, the function of the operation button 7205 can be freely set by an operating system built into the mobile information terminal 7200.

[0270] The mobile information terminal 7200 can also perform short-distance wireless communication according to a communication standard. For example, the mobile information terminal 7200 can communicate with a wireless headset to enable hands-free calling.

[0271] The portable information terminal 7200 also includes an input / output terminal 7206, and can directly exchange data with other information terminals via a connector. Charging can also be performed via the input / output terminal 7206. Note that charging may be performed by wireless power supply without using the input / output terminal 7206.

[0272] The secondary battery of one embodiment of the present invention is included in the display portion 7202 of the portable information terminal 7200. For example, the secondary battery 7104 shown in FIG. 21E can be incorporated in a curved state inside the housing 7201 or in a bendable state inside the band 7203.

[0273] The portable information terminal 7200 preferably has a sensor. For example, it is preferable to mount a human body sensor such as a fingerprint sensor, a pulse sensor, or a body temperature sensor, a touch sensor, a pressure sensor, an acceleration sensor, or the like, as the sensor.

[0274] 21G illustrates an example of an armband-type display device. The display device 7300 includes a display portion 7304 and a secondary battery of one embodiment of the present invention. The display device 7300 can also include a touch sensor in the display portion 7304 and can function as a portable information terminal.

[0275] The display surface of the display portion 7304 is curved, and display can be performed along the curved display surface. In addition, the display device 7300 can change the display state by short-range wireless communication according to a communication standard.

[0276] The display device 7300 also includes an input / output terminal, and can directly exchange data with other information terminals via a connector. Charging can also be performed via the input / output terminal. Note that charging may be performed by wireless power supply without using the input / output terminal.

[0277] Next, an example of a tablet terminal that can be folded in two is shown in Fig. 22A and Fig. 22B. The tablet terminal 9600 shown in Fig. 22A and Fig. 22B has a housing 9630a, a housing 9630b, a movable part 9640 that connects the housings 9630a and 9630b, a display part 9631, a display mode changeover switch 9626, a power switch 9627, a power saving mode changeover switch 9625, a fastener 9629, and an operation switch 9628. By using a flexible panel for the display part 9631, a tablet terminal having a wider display part can be obtained. Fig. 22A shows the tablet terminal 9600 in an open state, and Fig. 22B shows the tablet terminal 9600 in a closed state.

[0278] The tablet terminal 9600 also includes a power storage unit 9635 inside the housing 9630a and the housing 9630b. The power storage unit 9635 passes through the movable portion 9640 and is provided across the housings 9630a and 9630b.

[0279] A part of the display portion 9631 can be a touch panel area, and data can be input by touching the displayed operation keys. Also, keyboard buttons can be displayed on the display portion 9631 by touching a position on the touch panel where a keyboard display switching button is displayed with a finger or a stylus.

[0280] Furthermore, the display mode changeover switch 9626 can change the display orientation, such as portrait or landscape, and can select black and white or color display. The power saving mode changeover switch 9625 can optimize the display brightness according to the amount of external light during use detected by an optical sensor built into the tablet terminal 9600. The tablet terminal may be equipped with not only an optical sensor, but also other detection devices such as a gyro, an acceleration sensor, or other sensors that detect tilt.

[0281] 22B shows a tablet terminal in a closed state, which includes a housing 9630, a solar cell 9633, and a charge / discharge control circuit 9634 including a DC-DC converter 9636. In addition, a secondary battery according to one embodiment of the present invention is used as a power storage unit 9635.

[0282] Note that the tablet terminal 9600 can be folded in two, and therefore can be folded so that the housing 9630a and the housing 9630b overlap each other when not in use. By folding, the display portion 9631 can be protected, and therefore durability of the tablet terminal 9600 can be improved. In addition, the power storage unit 9635 using the secondary battery of one embodiment of the present invention has a high capacity and favorable cycle characteristics, and therefore a tablet terminal that can be used for a long period of time can be provided.

[0283] In addition, the tablet terminal shown in Figures 22A and 22B can have a function to display various information (still images, videos, text images, etc.), a function to display a calendar, date or time on the display unit, a touch input function to perform touch input operations or edit information displayed on the display unit, and a function to control processing using various software (programs), etc.

[0284] A solar cell 9633 attached to the surface of the tablet terminal can supply power to a touch panel, a display unit, a video signal processor, or the like. Note that the solar cell 9633 can be provided on one or both sides of the housing 9630, and a configuration can be adopted in which the power storage unit 9635 can be efficiently charged.

[0285] The configuration and operation of the charge / discharge control circuit 9634 shown in Fig. 22B are described with reference to a block diagram in Fig. 22C. Fig. 22C shows a solar cell 9633, a power storage unit 9635, a DCDC converter 9636, a converter 9637, switches SW1 to SW3, and a display unit 9631. The power storage unit 9635, the DCDC converter 9636, the converter 9637, and the switches SW1 to SW3 correspond to the charge / discharge control circuit 9634 shown in Fig. 22B.

[0286] First, an example of operation in the case where power is generated by the solar cell 9633 using external light will be described. The power generated by the solar cell is stepped up or stepped down by a DC-DC converter 9636 to a voltage for charging a power storage unit 9635. When power from the solar cell 9633 is used for the operation of the display unit 9631, a switch SW1 is turned on, and the converter 9637 steps up or steps down the voltage to a voltage required for the display unit 9631. When no display is to be performed on the display unit 9631, SW1 is turned off and SW2 is turned on to charge the power storage unit 9635.

[0287] Note that the solar cell 9633 is shown as an example of a power generating means, but is not particularly limited thereto, and may be configured to charge the power storage unit 9635 using other power generating means such as a piezoelectric element (piezo element) or a thermoelectric conversion element (Peltier element). For example, a non-contact power transmission module that transmits and receives power wirelessly (non-contact) for charging, or a combination with other charging means may be used.

[0288] FIG. 23 illustrates an example of another electronic device. In FIG. 23, a display device 8000 is an example of an electronic device using a secondary battery 8004 according to one embodiment of the present invention. Specifically, the display device 8000 corresponds to a display device for receiving a TV broadcast and includes a housing 8001, a display unit 8002, a speaker unit 8003, a secondary battery 8004, and the like. The secondary battery 8004 according to one embodiment of the present invention is provided inside the housing 8001. The display device 8000 can receive power from a commercial power source, and can also use power stored in the secondary battery 8004. Thus, even when power cannot be supplied from a commercial power source due to a power outage or the like, the display device 8000 can be used by using the secondary battery 8004 according to one embodiment of the present invention as an uninterruptible power source.

[0289] The display unit 8002 can be a liquid crystal display device, a light-emitting device having a light-emitting element such as an organic EL element in each pixel, an electrophoretic display device, a semiconductor display device such as a DMD (Digital Micromirror Device), a PDP (Plasma Display Panel), or an FED (Field Emission Display).

[0290] The display device includes all display devices for displaying information, such as display devices for receiving TV broadcasts, display devices for personal computers, display devices for advertisements, and the like.

[0291] 23, a stationary lighting device 8100 is an example of an electronic device using a secondary battery 8103 according to one embodiment of the present invention. Specifically, the lighting device 8100 includes a housing 8101, a light source 8102, a secondary battery 8103, and the like. FIG. 23 illustrates an example in which the secondary battery 8103 is provided inside a ceiling 8104 on which the housing 8101 and the light source 8102 are provided, but the secondary battery 8103 may be provided inside the housing 8101. The lighting device 8100 can receive power from a commercial power source or can use power stored in the secondary battery 8103. Thus, even when power cannot be supplied from a commercial power source due to a power outage or the like, the lighting device 8100 can be used by using the secondary battery 8103 according to one embodiment of the present invention as an uninterruptible power source.

[0292] Note that although Figure 23 shows an example of a stationary lighting device 8100 provided on a ceiling 8104, the secondary battery of one embodiment of the present invention can also be used in a stationary lighting device provided on a surface other than the ceiling 8104, such as a side wall 8105, a floor 8106, or a window 8107, or can also be used in a tabletop lighting device.

[0293] An artificial light source that artificially obtains light using electric power can be used as the light source 8102. Specifically, examples of the artificial light source include discharge lamps such as incandescent lamps and fluorescent lamps, and light-emitting elements such as LEDs and organic EL elements.

[0294] 23, an air conditioner including an indoor unit 8200 and an outdoor unit 8204 is an example of an electronic device using a secondary battery 8203 according to one embodiment of the present invention. Specifically, the indoor unit 8200 includes a housing 8201, an air outlet 8202, a secondary battery 8203, and the like. FIG. 23 illustrates an example in which the secondary battery 8203 is provided in the indoor unit 8200, but the secondary battery 8203 may be provided in the outdoor unit 8204. Alternatively, the secondary battery 8203 may be provided in both the indoor unit 8200 and the outdoor unit 8204. The air conditioner can receive power from a commercial power source or can use power stored in the secondary battery 8203. In particular, when a secondary battery 8203 is provided in both the indoor unit 8200 and the outdoor unit 8204, even when power cannot be supplied from a commercial power source due to a power outage or the like, the air conditioner can be used by using the secondary battery 8203 of one embodiment of the present invention as an uninterruptible power source.

[0295] Note that although FIG. 23 illustrates an example of a separate-type air conditioner including an indoor unit and an outdoor unit, a secondary battery according to one embodiment of the present invention can also be used in an integrated air conditioner that has the functions of an indoor unit and an outdoor unit in a single housing.

[0296] 23, an electric refrigerator-freezer 8300 is an example of an electronic device using a secondary battery 8304 according to one embodiment of the present invention. Specifically, the electric refrigerator-freezer 8300 includes a housing 8301, a refrigerator door 8302, a freezer door 8303, a secondary battery 8304, and the like. In FIG. 23, the secondary battery 8304 is provided inside the housing 8301. The electric refrigerator-freezer 8300 can receive power from a commercial power source or can use power stored in the secondary battery 8304. Thus, even when power cannot be supplied from the commercial power source due to a power outage or the like, the electric refrigerator-freezer 8300 can be used by using the secondary battery 8304 according to one embodiment of the present invention as an uninterruptible power source.

[0297] Also, by storing power in the secondary battery during time periods when electronic devices are not used, particularly during time periods when the ratio of the amount of power actually used to the total amount of power that can be supplied by the commercial power source (called the power usage rate) is low, it is possible to prevent the power usage rate from increasing outside of the above time periods. For example, in the case of an electric refrigerator-freezer 8300, power is stored in the secondary battery 8304 during the night when the temperature is low and the refrigerator door 8302 and the freezer door 8303 are not opened or closed. Then, during the daytime when the temperature is high and the refrigerator door 8302 and the freezer door 8303 are opened and closed, the secondary battery 8304 is used as an auxiliary power source, thereby making it possible to keep the daytime power usage rate low.

[0298] In addition to the electronic devices described above, the secondary battery of one embodiment of the present invention can be mounted on any electronic device. According to one embodiment of the present invention, a secondary battery with less deterioration and high safety can be obtained. Therefore, by mounting the secondary battery of one embodiment of the present invention on the electronic device described in this embodiment, the electronic device can have a longer life and a higher safety. This embodiment can be implemented in appropriate combination with other embodiments.

[0299] (Embodiment 6) In this embodiment, an example in which a secondary battery according to one embodiment of the present invention is mounted on a vehicle will be described.

[0300] By installing a secondary battery in a vehicle, next-generation clean energy vehicles such as hybrid electric vehicles (HEV), electric vehicles (EV), and plug-in hybrid electric vehicles (PHEV) can be realized.

[0301] FIG. 24 illustrates an example of a vehicle using a secondary battery according to one embodiment of the present invention. An automobile 8400 illustrated in FIG. 24A is an electric automobile using an electric motor as a power source for running. Alternatively, it is a hybrid automobile that can use an electric motor and an engine as a power source for running. By using one embodiment of the present invention, a vehicle with a long cruising distance can be realized. In addition, the automobile 8400 includes a secondary battery. The secondary battery can not only drive the electric motor 8406, but also supply power to a light-emitting device such as a headlight 8401 or a room light (not shown).

[0302] The secondary battery can also supply power to display devices such as a speedometer and a tachometer included in the automobile 8400. The secondary battery can also supply power to semiconductor devices such as a navigation system included in the automobile 8400.

[0303] The automobile 8500 shown in FIG. 24B can charge the secondary battery of the automobile 8500 by receiving power supply from an external charging facility by a plug-in method, a non-contact power supply method, or the like. FIG. 24B shows a state in which a secondary battery 8024 mounted on the automobile 8500 is being charged from a ground-mounted charging device 8021 via a cable 8022. When charging, the charging method and connector standards may be appropriately performed by a predetermined method such as CHAdeMO (registered trademark) or Combo. The charging device 8021 may be a charging station installed in a commercial facility, or may be a home power source. For example, the secondary battery 8024 mounted on the automobile 8500 can be charged by an external power supply using plug-in technology. Charging can be performed by converting AC power to DC power via a conversion device such as an ACDC converter.

[0304] Although not shown, a power receiving device may be mounted on a vehicle, and charging may be performed by supplying power contactlessly from a ground power transmitting device. In the case of this contactless power supply method, by incorporating a power transmitting device in a road or an exterior wall, charging may be performed not only while the vehicle is stopped but also while the vehicle is moving. This contactless power supply method may also be used to transmit and receive power between vehicles. Furthermore, a solar cell may be provided on the exterior of the vehicle, and a secondary battery may be charged while the vehicle is stopped or moving. An electromagnetic induction method or a magnetic field resonance method may be used for such contactless power supply.

[0305] 24C is an example of a two-wheeled vehicle using the secondary battery of one embodiment of the present invention. A scooter 8600 shown in FIG. 24C includes a secondary battery 8602, a side mirror 8601, and a turn signal light 8603. The secondary battery 8602 can supply electricity to the turn signal light 8603.

[0306] 24C, the secondary battery 8602 can be stored in the under-seat storage 8604. The secondary battery 8602 can be stored in the under-seat storage 8604 even if the under-seat storage 8604 is small.

[0307] According to one embodiment of the present invention, a secondary battery with little deterioration and high safety can be obtained. Therefore, by mounting the secondary battery on a vehicle, it is possible to suppress a decrease in cruising distance, acceleration performance, and the like. In addition, a vehicle with high safety can be obtained. In addition, the secondary battery mounted on the vehicle can also be used as a power supply source other than the vehicle. In this case, for example, it is possible to avoid using a commercial power source during peak power demand. If it is possible to avoid using a commercial power source during peak power demand, it is possible to contribute to energy saving and reduction of carbon dioxide emissions. In addition, since the secondary battery with little deterioration and high safety can be used for a long period of time, it is possible to reduce the amount of rare metals used, including cobalt.

[0308] This embodiment mode can be implemented in appropriate combination with other embodiment modes. EXAMPLES

[0309] In this embodiment, the chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) The analysis of the substitution positions of Ni and Mg atoms in the compound represented by O2 will be described below.

[0310] [Calculation of stabilization energy (ΔE) for different substitution positions] Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) O2 is LiC O This is a compound in which Mg and Ni are added as substitution elements to O2. Here, one Mg atom and one Ni atom are LiC O When replacing the metal atom of O2, the combination of substitution sites can be the combinations mentioned above. The combinations are shown again below. When Li in the same Li layer is replaced with Mg and Ni, condition (A) When Li in different Li layers is replaced with Mg and Ni, condition (B) When Co in the same Co layer is replaced by Mg and Ni, condition (C) When Co in different Co layers is replaced by Mg and Ni, condition (D) When Li in the Li layer is replaced by Mg and CoNi in the Co layer, condition (E) When Li in the Li layer is replaced by Ni and Co in the Co layer is replaced by Mg, condition (F)

[0311] For the above combinations of substitution sites, the stabilization energy ΔE was calculated for each combination in which Ni and Mg are from the first to the third or fourth nearest neighbors using the above formulas 1 to 3. The calculation conditions for LiCoO2 are shown in Table 1, and the calculation results of ΔE are shown in FIG. 25. Note that (A) to (E) in FIG. 25 represent the calculation results under the above conditions (A) to (E). Since the ionic radius of Mg ions is larger than that of Co ions, it is expected that large energy is required for Mg to be substituted at the Co site. Therefore, the stabilization energy of condition (F) is expected to be large.

[0312] In Table 1, VSAP stands for Vienna Ab initio Simulation Package (purchased from VASP Software GmbH).

[0313] [Table 1]

[0314] From Figure 25, it was found that the stabilization energy of conditions (A), (B) and (E) tended to be low, while conditions (C) and (D) had high stabilization energy and were unstable conditions. This suggests that Mg and Ni are difficult to substitute for the Co site. On the other hand, condition (E) had the lowest stabilization energy, suggesting that Ni at the Co site is stabilized by the presence of Mg substituted for the Li site. In addition, conditions (A) and (B) had the same degree of stabilization energy, suggesting that the stabilization energy was slightly higher than that of condition (E).

[0315] [Stabilization energy (ΔE C ) calculation] To estimate the energy change during charging, ΔE C From Figure 25, the chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) The crystal structure of the compound represented by O2 is likely to be under conditions (A), (B) and (E). Therefore, for conditions (B) and (E), ΔE C The ΔE C The calculation cost was reduced by using the above equation.

[0316] As shown in Figure 26, under condition (E), as the cation occupancy rate of the Li site decreases, ΔE CIn addition, when the Li site occupancy rate is 100%, which is the state before charging, condition (E) has a higher ΔE than condition (B). C is smaller than that of condition (B) when the Li site occupancy is 98% or less. C It was also found that condition (B) has a minimum point when the occupancy rate of the Li sites is 96%. This suggests that condition (B) is more stable when charging begins.

[0317] From these results, the chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) In the compound represented by O2, Mg is substituted for the Li site and Ni is substituted for the Co site immediately after synthesis, but it is suggested that Ni moves to the Li site by charging, and the instability is alleviated. In other words, it is suggested that the substitution position of Ni changes before and after charging. In other words, it is suggested that the phenomenon of "Ni moving from the Co site to the Li site by charging" occurs.

[0318] [Charge / discharge efficiency measurement] In order to confirm whether the phenomenon of Ni migrating from the Co site to the Li site by charging actually occurs, (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) A compound represented by O2 was prepared, and the charge / discharge efficiency of a secondary battery using the compound was measured.

[0319] <Chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) Preparation of the compound represented by O2> As the positive electrode active material 100A-1, referring to the flow shown in FIG. 3, (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b)A compound represented by the formula O2 was prepared. As described later, Samples 1 to 3 were prepared by changing the amount of nickel hydroxide Ni(OH)2 mixed. Two similar samples were prepared for each sample, and the charge-discharge efficiency of Samples 1 to 3 was measured twice.

[0320] First, a mixture 902 containing magnesium and fluorine was prepared (steps S11 to S14). LiF and MgF2 were weighed out so that the molar ratio of LiF:MgF2 was 1:3, and acetone was added as a solvent to perform wet mixing and pulverization. Mixing and pulverization were performed in a ball mill using zirconia balls at 400 rpm for 12 hours. The processed material was collected and used as the mixture 902.

[0321] Next, nickel hydroxide, which is a metal source, was mixed with acetone to prepare finely powdered nickel hydroxide (steps S15 to S17).

[0322] Next, lithium cobalt oxide was prepared as a composite oxide containing lithium and cobalt. More specifically, Cellseed C-10N manufactured by Nippon Chemical Industry Co., Ltd. was prepared (step S25).

[0323] Next, in step S31, the atomic weight of magnesium in the mixture 902 was weighed out so that the atomic weight of cobalt in the lithium cobalt oxide was 2.0 mol%. Mixing was performed by a dry method. Mixing was performed in a ball mill using zirconia balls at 150 rpm for 1 hour.

[0324] Next, the mixture 903 was placed in an alumina crucible and annealed in a muffle furnace in an oxygen atmosphere at 850°C for 60 hours (step S34). The alumina crucible was covered during annealing. The oxygen flow rate was 10 L / min. The temperature was increased at 200°C / hr, and decreased over 10 hours or more. The material after the heat treatment was collected and sieved (step S35), and the mixture 904 was obtained (step S36).

[0325] Next, nickel hydroxide, which is a metal source, was mixed with acetone to prepare finely powdered nickel hydroxide (steps S15 to S17).

[0326] Next, in step S50, the atomic weight of nickel in the nickel hydroxide was weighed out to be w mol% relative to the sum of the atomic weights of cobalt and nickel in the mixture 903. w differs for each sample, as shown in Table 2 below. The weighed mixture 903 and nickel hydroxide were mixed. Mixing was performed in a dry manner. Mixing was performed in a ball mill using zirconia balls at 150 rpm for 1 hour.

[0327] [Table 2]

[0328] Next, the treated material was collected to obtain a mixture 905 (steps S51 and S52).

[0329] Next, the mixture 905 was placed in an alumina crucible and annealed in a muffle furnace in an oxygen atmosphere at 850°C for 60 hours (step S53). During annealing, the alumina crucible was covered with a lid. The oxygen flow rate was 10 L / min. The temperature was increased at 200°C / hr, and decreased over 10 hours or more. The material after the heat treatment was collected and sieved (step S54), and Samples 1 to 3 were obtained (step S55).

[0330] <Battery cell production> Next, each of the samples 1 to 3 obtained above was used as a positive electrode active material to fabricate a positive electrode. The positive electrode active material, AB, and PVDF were mixed in a ratio of active material:AB:PVDF=95:3:2 (weight ratio) and the slurry was applied to a current collector. NMP was used as the solvent for the slurry.

[0331] After the slurry was applied to the current collector, the solvent was evaporated. Then, pressure was applied at 210 kN / m, and then pressure was applied at 1467 kN / m. A positive electrode was obtained by the above process. The amount of the positive electrode loaded was about 7 mg / cm. 2 The electrode density was set to 3.8 g / cc.

[0332] Using the prepared positive electrode, a coin-type battery cell of the CR2032 type (diameter 20 mm, height 3.2 mm) was produced.

[0333] Lithium metal was used as the counter electrode.

[0334] The electrolyte used in the electrolytic solution was 1 mol / L lithium hexafluorophosphate (LiPF6), and the electrolytic solution was a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) at a volume ratio of EC:DEC = 3:7. For the secondary batteries used to evaluate the charge / discharge efficiency, 2 wt% vinylene carbonate (VC) was added to the electrolytic solution.

[0335] The separator was made of polypropylene having a thickness of 25 μm.

[0336] The positive electrode can and the negative electrode can were made of stainless steel (SUS).

[0337] <Measurement of charge / discharge efficiency> The first and second charge / discharge efficiencies of battery cells fabricated using the obtained Samples 1 to 3 were measured. The results are shown in Figure 27. The charge / discharge efficiency was measured under the conditions of 25°C, charging with CCCV (0.5C, 4.6V, cut-off current 0.05C) and discharging with CC (0.5C, 2.5V), and the charge / discharge was repeated. The C rate was 200mA / g. The charge / discharge efficiency (%) = (discharge capacity / charge capacity) x 100.

[0338] From FIG. 27, it was found that the initial charge-discharge efficiency was less than 100% for Samples 1 to 3. This result suggests that Ni, which was substituted in the Co layer before charging, migrates to other sites by charging. When analyzed together with the above calculation results, it is considered that the phenomenon of "Ni migrates from the Co site to the Li site by charging" occurs. In addition, as the amount of Ni(OH)2 added increases, the initial charge-discharge efficiency tends to decrease. Since it is considered that the discharge capacity decreases due to Ni migrating to the Li site, it is expected that the decrease in charge-discharge efficiency (difference from 100%) is larger for samples with a higher Ni concentration. In other words, it is considered that this tendency reflects the above phenomenon. In addition, the second charge-discharge efficiency of Samples 1 to 3 was approximately 100%. Therefore, it is suggested that the phenomenon is irreversible and occurs only during the first charge.

[0339] From the above calculation results and measurement results, in Fig. 25 alone, the chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) The most stable structure of the compound represented by O2 is one in which Mg is substituted at the Li site and Ni is substituted at the Co site. C The calculation of ΔE and the measurement of the charge-discharge efficiency suggested that the Li site was more stable when Mg and Ni were substituted after charging. Therefore, it was suggested that the compound had a structure in which Mg was substituted at the Li site and Ni was substituted at the Co site when synthesized, but that Ni moved to the Li site and the structure changed when charging. In addition to calculating ΔE, C By calculating ΔE and measuring the charge / discharge efficiency, as described above, it is possible to perform analysis from both calculation and experiment, and therefore it is possible to analyze the structure of the lithium composite oxide more accurately. In addition, by calculating ΔE, it is possible to efficiently C It was found that the calculation cost can be reduced by calculating the above. In addition, the validity of the phenomenon occurring in the compound can be examined by calculation, so that the measurement can be performed efficiently. Therefore, the number of samples and the time required for the measurement can be reduced. [Explanation of symbols]

[0340] 100: positive electrode active material, 100A-1: positive electrode active material, 100C: positive electrode active material, 200: active material layer, 201: graphene compound, 211a: positive electrode, 211b: negative electrode, 212a: lead, 212b: lead, 214: separator, 215a: joint, 215b: joint, 217: fixing member, 250: battery, 251: exterior body, 261: folded portion, 262: seal portion, 263: seal portion, 271: ridge line, 272: valley line, 273: space, 300: secondary battery, 301: positive electrode can, 302: negative electrode can, 303: gasket, 304: positive electrode, 305: positive electrode current collector, 306: positive electrode Active material layer, 307: negative electrode, 308: negative electrode current collector, 309: negative electrode active material layer, 310: separator, 500: secondary battery, 501: positive electrode current collector, 502: positive electrode active material layer, 503: positive electrode, 504: negative electrode current collector, 505: negative electrode active material layer, 506: negative electrode, 507: separator, 508: electrolyte, 509: exterior body, 510: positive electrode lead electrode, 511: negative electrode lead electrode, 600: secondary battery, 601: positive electrode cap, 602: battery can, 603: positive electrode terminal, 604: positive electrode, 605: separator, 606: negative electrode, 607: negative electrode terminal, 608: insulating plate, 609: insulating plate, 611: P TC element, 612: safety valve mechanism, 613: conductive plate, 614: conductive plate, 615: module, 616: lead, 617: temperature control device, 900: circuit board, 902: mixture, 903: mixture, 904: mixture, 905: mixture, 910: label, 911: terminal, 912: circuit, 913: secondary battery, 914: antenna, 915: antenna, 916: layer, 917: layer, 918: antenna, 919: terminal, 920: display device, 921: sensor, 922: terminal, 930: housing, 930a: housing, 930b: housing, 931: negative electrode, 932: positive electrode, 933: separator, 9 50: winding body, 951: terminal, 952: terminal, 980: secondary battery, 981: film, 982: film, 993: winding body, 994: negative electrode, 995: positive electrode, 996: separator, 997: lead electrode, 998: lead electrode, 7100: portable display device, 7101: housing, 7102: display unit, 7103: operation button, 7104: secondary battery, 7200: portable information terminal, 7201: housing, 7202: display unit, 7203: band, 7204: buckle, 7205: operation button, 7206: input / output terminal, 7207: icon, 7300: display device, 7304: display unit,7400: mobile phone, 7401: housing, 7402: display unit, 7403: operation button, 7404: external connection port, 7405: speaker, 7406: microphone, 7407: secondary battery, 7408: lead electrode, 7409: current collector, 8000: display device, 8001: housing, 8002: display unit, 8003: speaker unit, 8004: secondary battery, 8021: Charging device, 8022: cable, 8024: secondary battery, 8100: lighting device, 8101: housing, 8102: light source, 8103: secondary battery, 8104: ceiling, 8105: side wall, 8106: floor, 8107: window, 8200: indoor unit, 8201: housing, 8202: air outlet, 8203: secondary battery, 8204: outdoor unit, 8300: electric refrigerator-freezer, 8301: Housing, 8302: refrigerator door, 8303: freezer door, 8304: secondary battery, 8400: automobile, 8401: headlight, 8406: electric motor, 8500: automobile, 8600: scooter, 8601: side mirror, 8602: secondary battery, 8603: turn signal light, 8604: under-seat storage, 9600: tablet terminal, 9625: switch, 9626: display mode change switch, 9627: power switch, 9628: operation switch, 9629: fastener, 9630: housing, 9630a: housing, 9630b: housing, 9631: display unit, 9633: solar cell, 9634: charge / discharge control circuit, 9635: power storage unit, 9636: DCDC converter, 9637: converter, 9640: moving part,

Claims

1. LiCoO 2 A compound with Ni and Mg atoms added as replacement elements of the chemical formula Li (1-x-y) Co (1-a-b) Ni (x+a) Mg (y+b) O 2 In the compound represented by the formula (0<x+a≦0.015 and 0<y+b≦0.06), a first step of calculating first stabilization energies of the compound represented by the chemical formula for a substitution position where a Li atom in the same Li layer is substituted with the Ni atom and the Mg atom, a substitution position where a Li atom in a different Li layer is substituted with the Ni atom and the Mg atom, a substitution position where a Co atom in the same Co layer is substituted with the Ni atom and the Mg atom, a substitution position where a Co atom in a different Co layer is substituted with the Ni atom and the Mg atom, a substitution position where a Li atom in the Li layer is substituted with the Mg atom and a Co atom in the Co layer is substituted with the Ni atom, and a substitution position where a Li atom in the Li layer is substituted with the Ni atom and a Co atom in the Co layer is substituted with the Mg atom; A second step of calculating a second stabilization energy of the compound represented by the chemical formula when the cation occupancy rate of the Li site is changed for the substitution position having the lowest first stabilization energy and the substitution position having the second lowest first stabilization energy, A method for analyzing a lithium composite oxide, which predicts the structure of the compound after charging.

2. In claim 1, The method for analyzing a lithium composite oxide, wherein the Ni atom and the Mg atom in the first step have a combination of first adjacent to third adjacent atoms.

3. In claim 1 or 2, The method for analyzing a lithium composite oxide includes changing the cation occupancy rate in a range of at least 80% to 100% and carrying out the calculation.

Citation Information

Patent Citations

  • Electrolyte and lithium ion secondary battery

    JP2013020702A

  • Positive electrode active material, method for manufacturing positive electrode active material, and secondary battery

    JP2018206747A

  • Surface-stabilized cathode materials for lithium-ion batteries and methods for synthesizing same

    JP2019530630A

  • Method of designing and modifying lithium ion battery cathode materials

    US20170293707A1

  • Power storage device

    JP2012018914A