Furniture lined with flame-retardant fabric including flame-shielding cloth
A flame-shielding fabric composed of flame-retardant acrylic and cellulose fibers with magnesium compounds addresses environmental issues and enhances flame shielding in upholstered furniture, ensuring effective flame retardancy and comfort.
Patent Information
- Application Number
- JP2021162014
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-09-30
- Publication Date
- 2024-11-13
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing flame-retardant upholstered furniture using antimony compounds and glass components with low glass transition temperatures face environmental concerns due to elution and discharge, and have insufficient flame shielding performance during combustion, particularly affecting internal structures like urethane foam.
Incorporating a flame-shielding fabric made of flame-retardant acrylic fibers and cellulose fibers, with a specific ratio and magnesium compound content, to achieve reduced environmental impact and enhanced flame shielding properties.
The solution provides upholstered furniture with improved flame retardancy, reduced environmental concerns, and excellent texture by shortening afterflame and residual dust times, while maintaining comfort and preventing flame spread.
Smart Images

Figure 2024160196000001 
Figure 2024160196000002
Abstract
Description
[Technical field]
[0001] FIELD OF THEINVENTION This invention relates to flame retardant upholstered furniture comprising a flame barrier fabric. [Background technology]
[0002] Conventionally, in order to make halogen-containing fibers such as acrylic fibers flame retardant, there is a method of incorporating about 1 to 50 mass% of an antimony compound as a flame retardant (for example, Patent Document 1). Flame retardant acrylic fibers containing such flame retardants are combined with other fibers that are not flame retardant and used as flame-shielding fabrics for flame-retardant upholstered furniture (for example, Patent Document 2).
[0003] Further, glass components having a glass transition temperature of 400° C. or less have been used as compounds other than antimony compounds that impart flame retardancy to halogen-containing fibers (for example, Patent Document 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 61-89339 [Patent Document 2] WO2006008958A1 publication [Patent Document 3] WO2006008900A1 publication Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the case of antimony compounds and glass components with a glass transition temperature of 400°C or less, there was concern about the impact on the environment due to the elution and emission of these compounds, leaving room for improvement. Also, in the case of fire-retardant upholstered furniture, the flame-shielding performance during combustion is insufficient and the internal structural components such as urethane foam may catch fire, so there was a demand for further improvement in flame-shielding performance while maintaining excellent texture, moisture absorption, and feel.
[0006] In order to solve the above-mentioned problems of the conventional art, the present invention provides upholstered furniture that has excellent flame retardancy and texture, and that contains a flame-shielding fabric that has a high flame-shielding property and has a reduced impact on the environment. [Means for solving the problem]
[0007] The present invention relates to flame-retardant upholstered furniture comprising a flame-shielding fabric that includes a flame-retardant acrylic fiber (A) and a cellulosic fiber (B), wherein the flame-retardant upholstered furniture contains a magnesium compound in an amount of 1.5% by mass or more and 13.5% by mass or less based on the total mass of the fabric, and has an afterflame time and afterglow time of 120 seconds or less as measured by a flammability test based on BS5852:2006. Effect of the Invention
[0008] According to the present invention, it is possible to provide flame-retardant upholstered furniture that reduces environmental concerns, has excellent texture, and further has good flame shielding properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The inventors of the present invention have discovered that by covering the internal structure of upholstered furniture with a flame-shielding fabric, it is possible to achieve excellent flame retardancy and flame shielding properties while reducing concerns about the impact on the environment, shortening the afterflame and glow times in combustion tests, and in particular to achieve a high level of flame retardancy while fully preserving the unique texture and comfort of the material, particularly that of urethane foam used in sofas, couches, etc.
[0010] In one or more embodiments of the present invention, the "afterflame time" and the "afterglow time" may each be measured by a flammability test based on BS5852:2006.
[0011] <Flame shielding fabric> The flame-shielding fabric is suitable for use in applications requiring flame-shielding performance. The flame-shielding performance here means that when the flame-shielding fabric is exposed to a flame, the flame-shielding fabric is carbonized to shield the flame and prevent the flame from spreading to the opposite side.
[0012] In one or more embodiments of the invention, the flame shielding fabric comprises a flame retardant acrylic fiber (A) and a cellulosic fiber (B).
[0013] The ratio of the flame-retardant acrylic fiber (A) to the cellulosic fiber (B) is determined by the durability, strength of the flame-shielding fabric, degree of carbonized film formation, and speed of self-extinguishing, and it is preferable that the ratio of the flame-retardant acrylic fiber (A) is 60 to 90 mass%, and the ratio of the cellulosic fiber (B) is 10 to 40 mass% relative to the total mass of the fabric, and it is more preferable that the ratio of the flame-retardant acrylic fiber (A) is 70 to 80 mass%, and the ratio of the cellulosic fiber (B) is 20 to 30 mass%. If the ratio of the flame-retardant acrylic fiber (A) is less than 60 mass%, the flame retardancy of the flame-shielding fabric becomes insufficient, and if it exceeds 90 mass%, the cellulosic fiber (B) is insufficient, and the ability to form a carbonized film during combustion becomes insufficient, which is not preferable. Furthermore, if the proportion of the cellulosic fiber (B) is less than 10% by mass, the flame-shielding fabric will have insufficient ability to form a charred film upon combustion, whereas if it exceeds 40% by mass, the flame-retardant acrylic fiber (A) will be insufficient, resulting in insufficient flame retardancy of the flame-shielding fabric, which is undesirable.
[0014] The flame-shielding fabric may contain other fibers within a range that does not impair the object and effect of the present invention. Examples of other fibers include natural fibers such as wool fibers, mohair fibers, cashmere fibers, camel fibers, alpaca fibers, angora fibers, and silk fibers. Examples of chemical fibers include polyester fibers, polyamide fibers, aramid fibers, polylactic acid fibers, acrylic fibers, polyolefin fibers, polyvinyl alcohol fibers, polyvinyl chloride fibers, polyvinylidene chloride fibers, polychlar fibers, polyethylene fibers, polyurethane fibers, polyoxymethylene fibers, polytetrafluoroethylene fibers, benzoate fibers, polyphenylene sulfide fibers, polyether ether ketone fibers, polybenzazole fibers, polyimide fibers, and polyamide imide fibers. Flame-retardant polyesters, polyethylene naphthalate fibers, melamine fibers, acrylate fibers, and polybenzoxide fibers may also be used. Other examples include oxidized acrylic fibers, carbon fibers, glass fibers, and activated carbon fibers. Other examples include regenerated collagen fibers, regenerated protein fibers, cellulose acetate fibers, and promix fibers.
[0015] The flame shielding fabric may contain 20% by mass or less, 10% by mass or less, or 8% by mass or less of other fibers based on the total fibers.
[0016] The flame-shielding fabric is preferably a knitted fabric, which may be made of flame-retardant acrylic fiber (A) and cellulosic fiber (B) in the form of, but is not limited to, a blend of cotton, a blend, a core yarn, a cross-knit, or a layered knitted fabric.
[0017] The flame-shielding fabric has a basis weight of 120 g / m 2 More than 220g / m 2 Preferably, 140 g / m or less. 2 More than 200g / m 2 More preferably, the weight of the flame-shielding fabric is 120 g / m 2If the density is less than 220 g / m, the density of the carbonized film formed during combustion will be low, and the performance of preventing ignition of urethane foam used in upholstered furniture such as sofas and couches will be insufficient. 2 When the thickness is more than 100 mm, the flame shielding performance of the carbonized film formed during combustion is good, but this is not preferable from the viewpoint of the texture of upholstered furniture such as sofas and couches. The flame shielding fabric may be used alone or in a combination of two or more layers.
[0018] The flame-shielding fabric may contain an antistatic agent, a heat-coloration inhibitor, a light resistance improver, a whiteness improver, a devitrification inhibitor, etc., as necessary. The flame-shielding fabric of the present invention thus obtained has the desired flame retardancy and excellent texture. Furthermore, upholstered furniture including the flame-shielding fabric of the present invention has the excellent properties of the flame-shielding fabric, i.e., excellent flame-shielding properties and texture.
[0019] The content of magnesium compounds as flame retardants in the flame-shielding fabric can be determined by subjecting the fabric itself to X-ray fluorescence analysis to determine the content of magnesium compounds in the entire fabric. The mass of cellulosic fibers (B) contained in the flame-shielding fabric can be determined by immersing the fabric in an organic solvent such as DMSO, DMF, DMAc, etc., heating the fabric to dissolve the acrylic fibers (A), and extracting the remaining cellulosic fibers (B). The magnesium compounds contained in the acrylic fibers (A) can be determined by weighing the undissolved portion of the organic solvent solution.
[0020] <Magnesium compounds> Since flame-shielding fabrics tend to form a charred layer during combustion, magnesium compounds are used as flame retardants.
[0021] The flame-shielding fabric has a magnesium compound content of 1.5% by mass or more and 13.5% by mass or less, preferably 2.0% by mass or more and 9.0% by mass or less, and most preferably 2.5% by mass or more and 6.0% by mass or less, in the entire fabric. If the flame-retardant content of the entire flame-shielding fabric is less than 1.5% by mass, the flame-shielding performance during combustion is insufficient, and the performance of preventing ignition of urethane foam used in upholstered furniture such as sofas and couches is insufficient. In addition, the magnesium compound content of the entire flame-shielding fabric is preferably high in order to obtain high flame retardancy, but is preferably 13.5% by mass or less from the viewpoint of not impairing the texture, touch, fiber strength, and fabric strength.
[0022] The particle size of the magnesium compound used in the present invention is expressed as a median diameter, and is 0.3 μm or more, preferably 0.3 μm to 2.0 μm, more preferably 0.5 μm to 1.5 μm. If the particle size is less than 0.3 μm, the surface area of the magnesium compound particles increases, and processing becomes difficult due to static electricity generation in the fiber processing step such as spinning. If the particle size exceeds 2.0 μm, it is not preferable in terms of production because it causes clogging of the spinneret in the spinning step. In the present invention, the average particle size of the magnesium compound can be measured, for example, by laser diffraction method in the case of powder, and can be measured by laser diffraction method or dynamic light scattering method in the case of dispersion (dispersion liquid) dispersed in water or organic solvent.
[0023] The amount of the magnesium compound added is preferably 2% by mass or more and 15% by mass or less, more preferably 3% by mass or more and 10% by mass or less, and most preferably 4% by mass or more and 8% by mass or less, relative to 100% by mass of the acrylonitrile copolymer described below. If the amount of the magnesium compound is less than 2% by mass, the flame retardancy becomes insufficient, while if it exceeds 15% by mass, the insulation resistance value increases during processing such as spinning of the fiber, static electricity is easily generated, and problems such as winding during the carding process occur, making processing difficult, which is not preferable.
[0024] Examples of magnesium compounds used in the present invention include magnesium oxide, magnesium peroxide, magnesium hydroxide, magnesium fluoride, magnesium chloride, magnesium bromide, magnesium iodide, magnesium hydride, magnesium diboride, magnesium nitride, magnesium sulfide, magnesium carbonate, calcium magnesium carbonate, magnesium nitrate, magnesium sulfate, magnesium sulfite, magnesium perchlorate, trimagnesium phosphate, magnesium permanganate, and magnesium phosphate. Among these, magnesium oxide and magnesium hydroxide are preferably used from the viewpoint of ease of handling. Furthermore, magnesium hydroxide is preferably used from the viewpoint of Mohs hardness. Two or more magnesium compounds may be used.
[0025] The preferred Mohs hardness of the magnesium compound in the present invention is less than 5. The Mohs hardness here is an index of mineral hardness. For example, Mohs hardness 5 is a degree of hardness that can be scratched with a knife, but not easily, and Mohs hardness 6 is a degree of hardness that is difficult to scratch with a knife and may damage the knife. Magnesium hydroxide compounds and magnesium oxide can ensure flame retardancy equivalent to that of antimony compounds, which are conventional flame retardants. Furthermore, in fibers in which the compounds are dispersed, magnesium hydroxide compounds can be spun more stably than magnesium oxide compounds. Although this is merely speculation, it is presumed that this is because the Mohs hardness of magnesium hydroxide compounds is about 3 and the Mohs hardness of magnesium oxide compounds is about 7, and magnesium hydroxide compounds are softer than magnesium oxide compounds, so that the wear of the cutter blade when cutting the knitted fabric or flame-retardant acrylic fiber of the present invention is reduced, and the wear of the machine used for spinning is reduced.
[0026] The magnesium hydroxide compound is not particularly limited, and may be selected from, for example, powder obtained by crushing natural bruxite, powder obtained by neutralizing an aqueous magnesium salt solution with an alkali, powder obtained by treating magnesium hydroxide particles with a phosphate, a borate, or the like, and a method of gradually producing magnesium hydroxide by hydrating magnesium oxide. Furthermore, the magnesium hydroxide compound may have a coating layer formed by adsorbing an adsorbable substance around the magnesium hydroxide compound particles or by surface treatment. Among them, a coating layer formed by surface treatment with a silane coupling agent is preferable from the viewpoint of static electricity suppression. The reason why static electricity suppression is improved by surface treatment with a silane coupling agent is only a guess, but is thought to be as follows. It is believed that the compatibility between the flame-retardant acrylic fiber (A) and the silane-coupled magnesium hydroxide is improved by silane coupling treatment of the surface of the magnesium hydroxide particles, and as a result, static electricity is suppressed. Furthermore, if a step of attaching an oil agent to the fiber surface is performed for the purpose of improving processability, the effect of the oil agent is sufficiently extended to the surface of the magnesium hydroxide particles, and processability is greatly improved. The type of silane coupling agent is not particularly limited as long as it improves the compatibility with the acrylic resin, and there is no particular limitation as to whether it is a crosslinked type or a non-crosslinked type.
[0027] <Acrylonitrile copolymer> The acrylonitrile copolymer is preferably a copolymer produced from 30-85% by mass of acrylonitrile, 15-65% by mass of one or more halogen-containing monomers selected from the group consisting of halogen-containing vinyl monomers and halogen-containing vinylidene monomers, and 0-3% by mass or less of a sulfonic acid group-containing monomer. More preferably, the copolymer is composed of 40-70% by mass of acrylonitrile, 60-30% by mass of vinyl chloride monomers and / or vinylidene chloride monomers, and 0-3% by mass of a sulfonic acid group-containing vinyl monomer. The acrylonitrile polymer improves the heat resistance and flame retardancy of the acrylic fiber. The other components are not particularly limited as long as they are copolymerizable with acrylonitrile.
[0028] Examples of halogen-containing monomers include halogen-containing vinyl and halogen-containing vinylidene. Examples of halogen-containing vinyl include vinyl chloride and vinyl bromide, and examples of halogen-containing vinylidene include vinylidene chloride and vinylidene bromide. These halogen-containing monomers may be used alone or in combination of two or more. Among vinyl chloride monomers and vinylidene chloride monomers, vinyl chloride monomer is more preferable. When vinyl chloride monomer is used, by selecting a magnesium compound as a flame retardant and blending it in a specific blending amount, a carbonized layer is easily formed during combustion, and high flame retardancy is exhibited. Although the mechanism is not clear, it is speculated that when vinyl chloride is present, the magnesium compound functions as an intumescent flame retardant and is easily formed as a foamed carbonized layer, i.e., an intumescent, during combustion. In addition, when vinylidene chloride monomer is used, if a magnesium compound is selected as a flame retardant, the polymer is colored, and use in bedding and clothing applications is limited, but when vinyl chloride monomer is used, coloring does not progress, which is preferable.
[0029] The sulfonic acid group-containing monomer is not particularly limited, but for example, unsaturated carboxylic acids and their salts represented by acrylic acid and methacrylic acid, methacrylic acid esters represented by methyl methacrylate, esters of unsaturated carboxylic acids represented by glycidyl methacrylate, vinyl esters represented by vinyl acetate and vinyl butyrate, sulfonic acid-containing monomers, etc. can be used. The sulfonic acid-containing monomer is not particularly limited, but allyl sulfonic acid, methallyl sulfonic acid, styrene sulfonic acid, isoprene sulfonic acid, 2-acrylamido-2-methylpropane sulfonic acid, and metal salts and amine salts thereof such as sodium salts can be used. These other copolymerizable vinyl monomers may be used alone or in combination of two or more. A monomer containing a sulfonic acid group is used as needed, but if the content of the monomer containing a sulfonic acid group in the acrylic polymer is 3 mass% or less, the production stability of the spinning process is excellent.
[0030] The acrylonitrile copolymer can be obtained by known polymerization methods such as bulk polymerization, suspension polymerization, emulsion polymerization, solution polymerization, etc. Among these, from an industrial viewpoint, suspension polymerization, emulsion polymerization, and solution polymerization are preferred.
[0031] <Flame-retardant acrylic fiber (A)> The flame-retardant acrylic fiber (A) is made of the above-mentioned acrylonitrile polymer and is used to improve the flame retardancy of the flame-shielding fabric. It is carbonized during combustion, which creates an oxygen-deficient state inside the flame-shielding fabric and helps prevent the penetration of flames on the surface.
[0032] The flame-retardant acrylic fiber (A) uses a magnesium compound, which reduces the generation of carbon monoxide, a harmful gas, during combustion compared to when an antimony compound is used. This acrylic fiber has excellent spinnability, little coloring (high brightness), and high flame retardancy while reducing its impact on the environment.
[0033] From the viewpoint of durability, the flame-retardant acrylic fiber (A) preferably has a single fiber strength of 1.0 to 4.0 cN / dtex, more preferably 1.5 to 3.5 cN / dtex. From the viewpoint of practicality, the flame-retardant acrylic fiber (A) preferably has an elongation of 20 to 40%, more preferably 20 to 30%. The single fiber strength and elongation can be measured in accordance with JIS L 1015.
[0034] The flame-retardant acrylic fiber (A) may be short or long, and can be appropriately selected depending on the method of use. The single fiber fineness is appropriately selected depending on the application of the fiber composite to be used, and is preferably 1 to 50 dtex, more preferably 1.5 to 30 dtex, and even more preferably 1.7 to 15 dtex. The cut length is appropriately selected depending on the application of the fiber composite. For example, short-cut fibers (fiber length 0.1 mm to 5 mm), short fibers (fiber length 38 mm to 128 mm), or long fibers (filaments) that are not cut at all can be mentioned.
[0035] The flame-retardant acrylic fiber (A) may contain other flame retardants other than the magnesium compound, which are unlikely to have an adverse effect on the environment due to elution or emission. In addition, other additives such as antistatic agents (also called antistatic agents), thermal coloring inhibitors, light resistance improvers, whiteness improvers, devitrification inhibitors, colorants, etc. may be contained as necessary. The application method is not particularly limited, and may be spray application or application after cutting.
[0036] The flame-retardant acrylic fiber (A) is not particularly limited, but can be produced by spinning a composition containing an acrylic copolymer containing at least acrylonitrile and a halogen-containing monomer, and a magnesium compound, followed by heat treatment. Specific production methods include known methods such as wet spinning, dry spinning, and semi-dry and semi-wet methods. For example, in the case of wet spinning, the acrylic copolymer is dissolved in an organic solvent, and then a magnesium compound is added to obtain a spinning stock solution. In the case of wet spinning, the spinning stock solution is extruded through a nozzle into a coagulation bath to be coagulated, and then stretched, washed with water, dried, heat-treated, and if necessary, crimped and cut, to produce the fiber. Examples of the organic solvent include dimethylformamide, dimethylacetamide, acetone, and dimethylsulfoxide, but inorganic solvents such as an aqueous rhodanide solution and an aqueous nitric acid solution may also be used.
[0037] <Cellulosic fiber (B)> The cellulose fiber (B) is used to maintain the strength of the flame-shielding fabric, and has the effect of maintaining the strength of the carbonized film during combustion. Specific examples of the cellulose fiber (B) include natural cellulose fibers such as cotton fiber, kapok fiber, flax fiber, hemp fiber, ramie fiber, jute fiber, Manila hemp fiber, and kenaf fiber, and regenerated cellulose fibers such as rayon, polynosic, cupra, and lyocell, and these may be used in combination. These cellulose fibers may be flame-retardant. Furthermore, regenerated cellulose fibers may contain components that impart functionality to the extent that they do not cause problems in fiber processing, such as silicic acid-containing cellulose fibers.
[0038] The cellulosic fiber (B) may be short or long, and can be appropriately selected depending on the method of use. The single fiber fineness is appropriately selected depending on the application of the fiber composite to be used, and is preferably 1 to 50 dtex, more preferably 1.5 to 30 dtex, and even more preferably 1.7 to 15 dtex. The cut length is appropriately selected depending on the application of the fiber composite. For example, short cut fiber (fiber length 0.1 mm to 5 mm), short fiber (fiber length 38 mm to 128 mm), or long fiber (filament) that is not cut at all can be mentioned.
[0039] <Flame-retardant upholstered furniture> Flame retardant upholstered furniture includes a flame barrier fabric that covers the interior structure of the upholstered furniture, providing excellent flame retardancy.
[0040] Examples of upholstered furniture include sofas and couches that are made up of springs, urethane, a wooden frame, and fabric.
[0041] The flame-shielding properties of the flame-shielding fabric reduce the spread of fire to the internal structure of upholstered furniture, so that upholstered furniture of any structure can be obtained that is flame-retardant as well as has an excellent texture and feel.
[0042] In one or more embodiments of the use of the flame-shielding fabric of the present invention for upholstered furniture, an internal structure, such as urethane foam or wadding, is wrapped in the flame-shielding fabric. When a flame-shielding barrier nonwoven fabric is sandwiched between a surface fabric and an internal structure, the flame-shielding fabric of the present invention is always placed on the outside of the internal structure as an interliner at least in the area where the surface fabric and the internal structure contact, and the surface fabric is stretched on top of it. The surface fabric is not particularly limited as long as it does not impair the texture and feel required for upholstered furniture. In addition, from the viewpoint of further improving the flame retardancy, a flame retardant may be coated on the back side of the surface fabric, for example, to the extent that the texture is not impaired.
[0043] Flame-retardant upholstered furniture has excellent flame resistance, and after-flame and after-glow times after exposure to flame are less than 2 minutes in a flammability test based on BS5852:2006. From the viewpoint of further improving flame resistance, it is preferable for flame-retardant upholstered furniture to have after-flame and after-glow extinguished within 60 seconds after exposure to flame as measured in a flammability test based on BS5852:2006. EXAMPLES
[0044] The present invention will be described in more detail below with reference to examples. Note that the present invention is not limited to the following examples. In the following, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.
[0045] (Production of a model for evaluating flame retardancy) Flame retardancy of upholstered furniture was evaluated by assembling a model according to the method described in BS5852;2006, and using the flame-shielding fabric described below as an interliner to construct a flame retardancy evaluation model.
[0046] (Flame retardancy evaluation) The evaluation was carried out according to BS5852:2006, the British standard for flame retardancy testing of upholstered furniture. As a standard for flame retardancy testing of household chairs, the seat and back of a urethane foam covered with a surface fabric were placed at right angles, and the flame was applied to the flame-contacting part for 20 seconds with a burner (Ignition Source 1) supplying 45 ml / min of butane gas, and the flame retardancy and afterglow time were measured. When using knit fabric, the flaming knit fabric was sandwiched between the surface fabric and the urethane foam, and the seat and back of the urethane foam covered with the knit fabric and surface fabric were placed at right angles, and the flame retardancy was evaluated in the same manner as above. Afterglow time and afterglow time of 1 minute or less were rated as ◎, those within 2 minutes were rated as 〇, and those over 2 minutes were rated as ×.
[0047] (Texture) The softness of the flame shielding fabric was subjected to a sensory evaluation by a specialist sensory evaluator, and the fabric was judged as pass or fail (◯, ×).
[0048] (judgement) The pass / fail judgment of the flame shielding fabric was made based on the flame retardancy evaluation and the texture.
[0049] (Surface fabric) The surface fabric used in the flame retardancy evaluation was a commercially available 100% polyethylene terephthalate fabric with a basis weight of approximately 250 g / m 2 Plain weave fabric was used.
[0050] (Back-coated surface fabric) The surface fabric used in the flame retardancy evaluation was a surface fabric with a coating on the back side. It was made of 100% polyethylene terephthalate available on the market, with a basis weight of approximately 250 g / m2. 2 The plain weave fabric was coated with a processing liquid according to Comparative Example 3 of Patent Document No. 5961684. Specifically, 30 parts by mass of a mixture of 60% by mass of zinc borate and 40% by mass of aluminum hydroxide and 5 parts by mass of a carboxymethyl cellulose thickener (70% by mass aqueous solution) were added to 100 parts by mass of a polyurethane resin emulsion with a solid content of 50% by mass while stirring to prepare a processing liquid, which was then coated onto the plain weave fabric using a doctor knife method. The solid content of the processing liquid was 100 g / m 2 The pre-drying was performed at 80°C for 5 minutes, and the curing was performed at 150°C for 1 minute.
[0051] (Production Example 1) As the flame-retardant acrylic fiber (A), an acrylic copolymer consisting of 50% by mass of acrylonitrile, 49.5% by mass of vinyl chloride, and 0.5% by mass of sodium p-styrenesulfonate obtained by emulsion polymerization of acrylonitrile, vinyl chloride, and sodium p-styrenesulfonate was dissolved in dimethylformamide so that the resin concentration was 30% by mass. 5 parts by mass of silane-coupled magnesium hydroxide (manufactured by Kyowa Chemical Industry Co., Ltd., product name "Kisuma 5P") was added to the obtained resin solution per 100 parts by mass of resin to prepare a spinning dope. The magnesium hydroxide was added in advance to 30% by mass per 100% by mass of dimethylformamide, and used as a dispersion prepared by uniformly dispersing it. The obtained spinning dope was extruded into a 50% by mass aqueous solution of dimethylformamide using a nozzle with a nozzle hole diameter of 0.08 mm and 300 holes to coagulate, then washed with water and dried at 120°C, stretched to 3 times its original size after drying, and further heat-treated at 145°C for 5 minutes to obtain a flame-retardant acrylic fiber. The obtained flame-retardant acrylic fiber had a single fiber fineness of 1.72 dtex, a strength of 2.7 cN / dtex, an elongation of 28%, and a cut length of 51 mm.
[0052] (Production Example 2) A flame-retardant acrylic fiber was obtained in the same manner as in Production Example 1, except that the acrylic copolymer of Production Example 1 was used as the flame-retardant acrylic fiber (A) and 2 parts by mass of silane coupling-treated magnesium hydroxide (manufactured by Kyowa Chemical Industry Co., Ltd., product name "Kisuma 5P") was added to the acrylic copolymer solution per 100 parts by mass of the acrylic copolymer. The obtained flame-retardant acrylic fiber had a single fiber fineness of 1.7 dtex, a strength of 3.2 cN / dtex, an elongation of 30%, and a cut length of 51 mm.
[0053] (Production Example 3) As the flame-retardant acrylic fiber (A) containing no flame retardant, acrylic fiber SB manufactured by Kaneka Corporation with a staple fiber fineness of 1.7 dtex and a cut length of 51 mm was used.
[0054] (Examples 1 to 4) The flame-retardant acrylic fiber (A) produced in Production Example 1 or 2 and natural cotton fiber with a cut length of 31 mm or less as the cellulosic fiber (B) were mixed in the ratios shown in Table 1 below to produce a spun yarn. The spun yarn was spun using a Shima Seiki Seisakusho Co., Ltd. flat knitting machine SG122FC to produce a yarn with a basis weight of about 150 g / m 2 The single knit fabrics were prepared. These knit fabrics were used as flame-shielding fabrics and were tested in the above-mentioned flame retardancy evaluation. The surface fabric used was a surface fabric that was not back-coated.
[0055] Comparative Example 1 A fabric was produced in the same manner as in Example 1, except that the flame-retardant acrylic fiber (A) produced in Production Example 3 was used. The surface fabric used was a surface fabric that was not back-coated.
[0056] (Comparative Examples 2 and 3) A fabric was produced in the same manner as in Example 1, except that the ratio of the flame-retardant acrylic fiber (A) produced in Production Example 2 to the cellulosic fiber (B) was changed. A surface fabric that was not back-coated was used.
[0057] Comparative Example 4 The same procedure as in Comparative Example 3 was followed except that a back-coated surface fabric was used as the surface fabric.
[0058] [Table 1]
[0059] From the results in Table 1, it is clear that the knit fabrics of Examples 1 and 2 have excellent flame shielding properties, and fabric-upholstered furniture with excellent flame retardancy was obtained. On the other hand, it is clear that in Comparative Example 1, sufficient flame shielding properties were not obtained because the amount of flame retardant in the knit fabric was insufficient.
[0060] [Table 2]
[0061] From the results in Table 2, it is clear that the knitted fabrics of Examples 1, 3, and 4 have excellent flame shielding properties, and upholstered furniture with excellent flame retardancy was obtained. On the other hand, in Comparative Example 2, the proportion of cellulosic fiber (B) in the knitted fabric was too low, and it was not possible to obtain sufficient flame shielding performance. In Comparative Example 3, the proportion of cellulosic fiber (B) in the knitted fabric was too high, and it was not possible to obtain sufficient fire extinguishing performance.
[0062] In all of Examples 1 to 4 and Comparative Examples 1 and 2, no coating was applied to the surface fabric, and the texture was evaluated as ◯. On the other hand, in Comparative Example 4, in which a back coating was applied to the surface fabric, the flame retardancy passed, but the fabric itself became very hard, and the texture was evaluated as x.
Claims
1. A flame-retardant upholstered furniture comprising a flame-shielding fabric comprising a flame-retardant acrylic fiber (A) and a cellulosic fiber (B), The magnesium compound contained in the flame shielding fabric is 1.5% by mass or more and 13.5% by mass or less based on the total mass of the fabric, Flame retardant upholstered furniture having an afterflame time and afterglow time of 120 seconds or less as measured by flammability test in accordance with BS5852:2006.
2. The flame-shielding fabric contains 60 to 90 mass% of the flame-retardant acrylic fiber (A) and 10 to 40 mass% of the cellulosic fiber (B) relative to the total mass of the fabric, and has a basis weight of 120 g / m 2 220g / m or more 2 2. The flame retardant upholstered furniture of claim 1, wherein:
3. 3. The flame-retardant upholstered furniture according to claim 1 or 2, wherein the flame-retardant acrylic fiber (A) is composed of an acrylonitrile copolymer produced from 30 to 85% by mass of acrylonitrile, 15 to 65% by mass of one or more halogen-containing monomers selected from the group consisting of halogen-containing vinyl monomers and halogen-containing vinylidene monomers, and 0 to 3% by mass of a sulfonic acid group-containing monomer.
4. 4. The flame-retardant upholstered furniture according to claim 1, wherein the flame-retardant acrylic fiber (A) contains 2 to 15 mass % of a magnesium compound throughout the entire interior of the fiber.
5. 5. The flame-retardant upholstered furniture of claim 4, wherein the magnesium compound has an average particle size of 0.3 μm or more.
6. 6. The flame retardant upholstered furniture of claim 4 or 5, wherein the magnesium compound is magnesium oxide and / or magnesium hydroxide.
7. 7. The flame-retardant upholstered furniture according to claim 1, wherein the cellulosic fiber (B) is at least one selected from the group consisting of natural cellulose fibers and regenerated cellulose fibers.
8. The flame-retardant upholstered furniture according to any one of claims 1 to 7, wherein the flame-blocking fabric is a knitted fabric.
Citation Information
Patent Citations
Composite fire retardant fiber
JP1986089339A
Flame retardant knit fabric
WO2006008900A1
Flame-retardant synthetic fiber, flame-retardant fiber composite, and upholstered furniture product made with flame-retardant fiber composite