Glasses having improved ion exchangeability and thermal expansion
A stoichiometric glass composition combining specific constituent phases addresses the challenge of achieving good chemical strengthening, low brittleness, and favorable thermal expansion, resulting in ultra-thin glasses with enhanced robustness and stability.
Patent Information
- Application Number
- JP2024138470
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2017-02-08
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-13
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing glasses lack a combination of good chemical strengthening properties, low brittleness, and favorable thermal expansion, which are essential for many applications, particularly in ultra-thin glasses, and are often compromised by different thermal histories during shaping processes.
A stoichiometric glass composition is developed by combining specific glass constituent phases, such as albite, reed magnalite, potassium-reed magnalite, grossular, cordierite, and zinc silicate, to achieve the desired balance of chemical strengthening, low brittleness, and thermal expansion properties, with controlled angular degrees of freedom and bond strength.
The solution results in glasses with enhanced chemical strengthening, reduced brittleness, and controlled thermal expansion, enabling reliable use in ultra-thin glass articles with improved robustness and stability across various thermal conditions.
Smart Images

Figure 2024160364000001 
Figure 2024160364000002 
Figure 2024160364000003
Abstract
Description
[Technical field]
[0001] The present invention relates to glasses and glass products which combine good chemical toughening with low fragility and favourable thermal expansion properties, where the low fragility makes the chemical toughening result as virtually independent as possible of the thermal history, which can vary significantly, especially in glasses which are subjected to shaping before toughening.
[0002] In a particular embodiment, the invention relates to ultra-thin glass, which means glass with a thickness of less than 400 μm down to less than 20 μm.
[0003] A method for producing such a glass and its use are also according to the invention.
[0004] The invention relates to glasses having a composition composed of a base glass. These glasses are characterized by a good chemical toughening property combined with an advantageous thermal expansion coefficient. Due to their composition and manufacturing method, glasses are characterized by a greater homogeneity at their surface compared to bulk glasses. Furthermore, these glasses have a low brittleness, which allows them to be processed into very thin glass articles. [Background technology]
[0005] Glasses with good ion exchange, i.e. good chemical strengthening, low so-called brittleness and favorable thermal expansion are required for many applications. Here, the parameter (T GThe significance of fragility, introduced by CA Angell as the derivative of the common logarithm of the viscosity according to the viscosity factor (T / T), is that it is related to the number of configurational degrees of freedom in the glass (see for example R. Boehmer, KL Ngai, CA Angell, DJ Plazek, J. Chem. Phys., 99 (1993) 4201-4209). The greater the fragility, the greater the number of configurational degrees of freedom and the more substantially different the different configurations in which the glass can exist due to different thermal histories. T G means the glass transition temperature, and in the definition of the viscosity curve, that is, when the viscosity is 10 12 is the temperature in pascal seconds.
[0006] These different configurations also affect stress relaxation, an inevitable counter-reaction that occurs during stress generation by ion exchange. This means that glass samples of the same composition but with different thermal histories in the same ion exchange process will develop different stresses. This is particularly important for glasses that are subjected to different shaping processes before tempering, which of course include different thermal histories.
[0007] The method of chemical strengthening can also be called chemical prestressing, chemical annealing, chemical hardening, ion exchange hardening, ion exchange annealing, ion exchange strengthening, or ion exchange prestressing. All these terms refer to methods in which smaller ions in the glass are replaced by larger ions. For example, sodium is replaced by potassium, or lithium is replaced by sodium or potassium, thereby forming a compressive stress layer on the surface of the glass.
[0008] A thermoviscoelastic model describing stress relaxation is described, for example, in George W. Scherer: Relaxation in Glass and Composites. Krieger Publishing Company Malabar (1992), and the relationship between the so-called nonlinearity parameter "x", describing the effect of configuration on the thermal activation of stress relaxation, and fragility is discussed, for example, in Roland Boehmer, Non-linearity and non-exponentiality of primary relaxations, Journal of Non-Crystalline Solids, 172-174 (1994), 628-634.
[0009] Since the glasses according to the invention should also be reliably usable in the non-toughened state, it is all the more important that the low fragility implies a high dimensional stability of the glass at all possible thermal loads below the glass transition temperature, which correlates with the configurational part of the thermal expansion coefficient (see Raphael MCVReis, John C. Mauro, Karen L. Geisingera, Marcel Potuzak, Morten M. Smedskjaer, Xiaoju Guo, Douglas C. Allan, Relationship between viscous dynamics and the configurational thermal expansion coefficient of glass-forming liquids, Journal of Non-Crystalline Solids 358 (2012) 648-651) and, for this configurational part, with the number of configurational parts (see above).
[0010] Ultra-thin glass is affected in a special way by the configuration part of the fragility and the thermal expansion coefficient. As mentioned above, the thickness over a wide range is determined by the mass throughput and the pulling speed. If ultra-thin glass of the same glass type is to be produced with the same pulling equipment, constant mass throughput and uniform width of the pulling ribbon, the pulling speed must first be selected inversely proportional to the thickness, taking into account the constant mass throughput and uniform width of the pulling ribbon. The significant difference in the pulling speed is due to the typical glass thickness range mentioned above. Regardless, after emerging from the nozzle, the glass passes through a substantially identical cooling section, generally formed as a cooling shaft, because it is the same pulling equipment and the initial and final temperatures of the cooling section are equal. The initial temperature is equal to the temperature in the pulling tank and the final temperature is equal to the temperature at which the glass can be freely handled. This means that the cooling speed must also be inversely proportional to the thickness. That is, the glass passes through the cooling shaft with significantly different cooling speeds, where it is difficult to produce a uniform temperature over the width of the ribbon cross section, especially when the cooling speed is high. However, different temperature histories across the width of the glass ribbon lead to distortions, the magnitude of which depends on these differences in temperature histories and also on the above-mentioned configurational part of the thermal expansion coefficient and thus the fragility: low fragility thus ensures a certain robustness of ultra-thin glass against interference effects during the manufacturing process.
[0011] Of particular economic importance is the use of such glasses as cover glasses for displays in electronic devices, where measures that result in higher ion exchangeability often result in higher brittleness and vice versa.
[0012] US 2013 / 0165312 A1 discloses cover glasses for semiconductor manufacturing, characterized by a specific thermal expansion, low alpha radiation and a high modulus of elasticity. The glasses described therein contain very high proportions of alkali metal oxides and alkaline earth metal oxides, which allow high thermal expansion. However, they differ from the glasses of the present invention in terms of stoichiometry and therefore cannot be explained in the base glass system of the present invention. Furthermore, the glasses described therein contain very high proportions of Al2O3 and at the same time relatively small amounts of MgO, which allows for a high proportion of albite, which increases the brittleness. Furthermore, in the case of the glasses described therein, the B2O3 content is very low, so that the proportion of leadmargnalite, which is desired according to the present invention and which reduces the brittleness, is lacking. The abovementioned very high proportions of alkali metal oxides and alkaline earth metal oxides result in high values of the thermal expansion coefficient, which in the examples is at least 99.2×10 -7 / K and very large.
[0013] German Utility Model No. 202012012876 (DE202012012876U1) deals with the ion exchange properties of glasses. For the glasses described there, hydrolytic and mechanical stability are of great importance, on the one hand, to avoid breakage and fracture, and on the other hand, to avoid leaching of glass components. Most of the glasses in this document do not contain B2O3. In many of the compositions described in the claims, boron is not present at all. The boron proportion is not quantified in the specification. In the examples, a boron proportion of up to 4.6% occurs. At the same time, however, a measurement rule is established for the boron proportion, according to which the boron proportion in molar percentage must be lower than the difference between the sum of the alkali metal oxide proportions on the one hand and the alumina proportion on the other hand multiplied by 0.3. This measurement rule is used to achieve the highest possible ion mobility. The compositions described in the present invention have nothing in common with this measurement rule. In the present invention, high, but not very high, ion mobility is required to achieve the desired values of fragility and thermal expansion coefficient. Why and how this is mutually exclusive will be described in the present description.
[0014] assignment The prior art lacks glasses that combine good chemical toughening with low brittleness and favorable thermal expansion properties. Furthermore, these glasses must be manufacturable in modern flat glass manufacturing processes.
[0015] This problem is solved by the subject matter of the claims.
[0016] Description of the invention This problem is solved by appropriately combining stoichiometric glasses, i.e. glasses that also exist as crystals with the same stoichiometric ratio and whose properties - as determined in many examples in the literature, for example by NMR measurements - can be considered very similar due to the identical topology of the building blocks of the glass and the crystals. For this purpose, stoichiometric glasses are selected whose mixtures allow the behavior in the sense of solving the problem according to the invention to be achieved. In this application, these stoichiometric glasses are also called "base glasses" or "constituent phases".
[0017] The description of glasses in terms of the constituent phases that belong to them is not a new concept. By specifying the base glass, conclusions can be drawn about the chemical structure of the glass (see Conradt R: "Chemical structure, medium range order, and crystalline reference state of multicomponent oxide liquids and glasses", Journal of Non-Crystalline Solids, Volumes 345-346, 15 October 2004, Pages 16-23).
[0018] According to the invention, glasses are combined with base glasses characterized by the following glass constituent phases:
[0019] [Table 1]
[0020] The glasses of the invention are characterized by their composition and constitution, the composition being chosen within the limits given herein for the constituent phases of the glass.
[0021] Naturally, the glass constituent phases are not crystalline per se in the glass product, but are present amorphously. However, this does not mean that the constituent phases in the amorphous state have completely different constituent units than in the crystalline state. As mentioned above, the topology of the constituent units, i.e., the interatomic distances resulting from, for example, the coordination of the involved cations with the surrounding oxygen atoms or the coordination and strength of the bonds between these cations and the surrounding oxygen atoms, are comparable. Therefore, many properties of the glasses of the invention can be fully explained using the constituent phases (see Conradt R in this regard, cited above), in particular to explain the achievements of the invention and the problems overcome by it. Naturally, the production of glasses can be carried out not only using the corresponding crystals, but also using normal glass raw materials, as long as the formation of the corresponding constituent units of the base glass is possible only in stoichiometric ratios.
[0022] Chemical strengthening by exchange of sodium for potassium in a suitable molten salt, such as potassium nitrate, is achieved in the glasses according to the invention by a substantial proportion of constituent units that contain sodium and have high sodium mobility. One example of a constituent phase that positively influences chemical strengthening is albite. Preferred glasses and glass articles of the invention are chemically strengthened.
[0023] The desired value of the fragility is mapped to the actual oriented parameter, i.e. the number of configurational degrees of freedom, and the corresponding condition of the calculation prescription. According to the work of CA Angell (see, for example, R. Boehmer, KL Ngai, CA Angell, DJ Plazek, J. Chem. Phys., 99 (1993) 4201-4209), the fragility appears as a profile of the viscosity curve according to the Arrhenius law and is approximately equal to the minimum value achieved by uncontaminated, in particular OH-free, quartz glass, and in addition, T G It "melts" at c p There is another contribution that correlates with the number of configurational degrees of freedom that become apparent in dynamic calorimetry as jumps.
[0024] This number can be determined by topological methods and by comparison with calorimetry. Since each configurational change is a dissimilarity mapping and therefore involves a change in the angle of the atoms, the number of configurational degrees of freedom per mole results from the number of angular degrees of freedom (Winkelfreiheitsgrade) per atom. The latter is calculated according to the method described in DE102014119594A1, where for the degree of ionization of the cation-oxygen bond the relationship described in Alberto Garcia, Marvon Cohen, First Principles Ionicity Scales, Phys.Rev.B 1993, 4215-4220 is used. The result of multiplying the gas constant R and T, which is carried out for the example of various commercial glasses such as Borofloat33, Borofloat40, LF5, LLF1, K7, AF45, etc., is calculated according to the method described in DE102014119594A1, where for the degree of ionization of the cation-oxygen bond the relationship described in Alberto Garcia, Marvon Cohen, First Principles Ionicity Scales, Phys.Rev.B 1993, 4215-4220 is used. G in p Comparison with jumps proves the validity of this procedure.
[0025] Since the glass according to the invention represents a combination of the above-mentioned constituent phases, it is sufficient to indicate the number of angular degrees of freedom per atom for each constituent phase in numerical terms in order to establish the calculation rules.
[0026] [Table 2]
[0027] Therefore, the calculation rule for measuring the angular freedom f per atom in the finished glass is:
number
[0028] The position of the thermal expansion coefficient in the targeted range is likewise guaranteed by calculation rules. This results from the average bond strength. It is known from the literature that the thermal expansion coefficient is inversely proportional to this (or to the "depth of the interatomic potential well"). In a simple image of an oxide glass, the cations are each placed in a potential well formed by the surrounding oxygen atoms, and the depth is determined by the sum of the bond strengths of the various single bonds to the surrounding oxygen atoms, i.e. the total interaction energy of the central cation with the surrounding oxygen atoms in the potential well. The reverse case therefore no longer needs to be considered. The analysis is more difficult since an oxygen atom can be between several different types of cations, which does not happen in pure oxide glasses on the other hand. These values are tabulated, for example, in DE102014119594A1.
[0029] [Table 3]
[0030] The values of Sr, Ba, Zn and Ti are not taken from DE102014119594A1 but are exactly the same as the sources cited therein and are calculated according to the methods described therein.
[0031] From the composition of the glass from the constituent phases listed above, the number of different cations in each phase, and the potential well depth per cation tabulated above, the average potential well depth can be calculated:
number
[0032] This average bond strength, as found by comparison with various commercial glasses such as Borofloat 33, Borofloat 40, AF5, AF32, etc., is related to the coefficient of thermal expansion according to the following formula:
number
[0033] The constituent phases are selected because their combination exhibits the desired ion exchange behavior and the desired values of brittleness and expansion coefficient. The role of the individual constituent phases is explained in more detail again below.
[0034] Albit The base glass represented as a constituent phase in the glass of the present invention is albite glass. Albite (NaAlSiO8) is known to have a high sodium diffusivity due to its structure consisting of a framework of SiO4- and AlO4 tetrahedrons with mobile sodium ions in the framework (see Geochimica et Cosmochimica Acta, 1963, Vol. 27, 107-120). The proportion of albite glass therefore contributes to a high sodium mobility that is beneficial for influencing the ion exchange and thus the chemical strengthening properties of the glass. Albite has the advantage of a significantly lower melting point (1100-1120°C) compared to nepheline (a potassium-free artificial variant: NaAlSiO4) which has an even higher sodium diffusivity, which improves the meltability of the glass.
[0035] The calculated proportion of albite in the glass according to the invention is at least 10 mol% and at most 40 mol%. If the amount of albite is too low, the ion exchangeability or chemical strengthening properties are impaired with respect to the exchange of sodium by potassium. Advantageously, the glass contains a proportion of albite of at least 15 mol%, more preferably at least 18 mol%, particularly preferably at least 20 mol%. Pure albite glass has probably optimal chemical strengthening properties, but is not effective with respect to the required brittleness. For albite, the number of angular degrees of freedom per atom is 0.318898019 and is thus higher than in the glass according to the invention. Thus, albite is advantageously used in a proportion of not more than 35 mol%, in particular not more than 32 mol%, more preferably not more than 30 mol%, particularly preferably not more than 25 mol%. According to the invention, 1 mole of albite means 1 mole of (Na2O·Al2O3·6SiO2) / 8.
[0036] Reedmergnerit The boron analogue leadmargunalite has a considerably lower number of angular degrees of freedom per atom than albite, i.e. 0.235470229. The glass according to the invention therefore contains leadmargunalite glass as an additional base glass, in particular the glass contains more leadmargunalite than albite. This base glass is constructed similarly to albite glass from SiO4- and BO4 tetrahedra, but has a more compact structure, due to the greater bond strength of the BO bonds compared to the Al-O bonds. Furthermore, the BO bonds are more covalent than the Al-O bonds. Firstly, both contribute less to the fragility, but the mobile sodium atoms in the framework according to the method of Anderson and Stuart (Journal of the American Ceramic Society, Vol. 37, No. 12, 573-580) have a higher thermal activation enthalpy than in albite glass, and therefore contribute less to the sodium ion mobility at the same temperature in leadmargunalite glass than in albite glass. According to the invention, the glasses described herein advantageously contain at least 10 mol% leadmargunalite, more preferably at least 15 mol% or at least 18 mol%, in particular at least 20.5 mol% or at least 25 mol%, particularly preferably at least 30 mol% leadmargunalite. However, in order to ensure sufficient temperability, the amount of leadmargunalite is limited to a maximum of 65 mol%, preferably a maximum of 60 mol%, more preferably a maximum of 45 mol%, more preferably a maximum of 40 mol%, particularly preferably 35 mol%. According to the invention, 1 mol of leadmargunalite means 1 mol of (Na2O·B2O3·6SiO2) / 8.
[0037] Kalium-Reedmergnerit To increase the devitrification stability, the glass can be further doped with potassium analogues of leadmargunalite. The finished glass, when such additions are made as alkali metals, contains potassium as well as sodium and is therefore more stable against devitrification. It behaves the same as leadmargunalite in terms of the number of angular degrees of freedom per atom. This number is 0.238787725. This base glass is henceforth called "potassium-leadmargunalite", since it can be understood as a potassium-analog of leadmargunalite with the danburite structure.
[0038] The glasses according to the invention may contain potassium leadmargunalite in a proportion of 0 to 32 mol % or up to 30 mol %. From the standpoint of devitrification stability, preferred embodiments contain at least 1 mol % potassium leadmargunalite, in particular at least 5 mol % or at least 8 mol % potassium leadmargunalite. In order not to impair the chemical toughening properties, the amount of potassium leadmargunalite in the glasses according to the invention is advantageously limited to a maximum of 25 mol %, more preferably a maximum of 20 mol %, particularly preferably a maximum of 15 mol %. 1 mol of potassium leadmargunalite means 1 mol of (K2O·B2O3·6SiO2) / 8.
[0039] In a preferred embodiment, the proportion of leadmargunalite in the glass is greater than the proportion of potassium-leadmargunalite, in particular at least two times greater.
[0040] The proportion of albite, leadmargunalite and potassium-leadmargunalite in the glass of the present invention in the above-mentioned base glass is advantageously at least 50 mol %, in particular at least 60 mol % in total. However, the proportion is advantageously limited to a maximum of 90 mol %, in particular to a maximum of 80 mol %. What the three constituent phases presented above (albite, leadmargunalite and potassium-leadmargunalite) have in common is that they contain a significant amount of alkali metals, which result in a high thermal expansion. Therefore, instead of alkali metals, further constituent phases are introduced, in which alkaline earth metals or zinc, i.e. cations that result in the average expansion coefficient, are present.
[0041] Grossular, Cordierit and Willemite Three additional optional constituent phases, grossular (CaAlSiO 12 ), cordierite (Mg2Al4Si5O 18 ) and willemite (Zn2SiO4) have high proportions of alkaline earth metals or zinc, respectively, and therefore a significant influence on the expansion coefficient. Conversely, the respective numbers of angular terms per atom are very high (grossular: 0.666147023, cordierite: 0.427525473, willemite: 0.725827911).
[0042] The glasses according to the invention can therefore contain grossular in a proportion of 0-10 mol %, in particular up to 9 mol % or up to 8.5 mol %. In preferred embodiments, at least 1 mol %, in particular at least 3 mol %, preferably at least 5 mol % of grossular is used. In a particular embodiment of the glasses according to the invention, no grossular is present. 1 mol of grossular means 1 mol of (3CaO·Al2O3·3SiO2) / 7.
[0043] The glass according to the invention may contain cordierite in a proportion of 0-10 mol %, in particular up to 8.5 mol % or up to 5 mol %. In preferred embodiments, at least 1 mol %, in particular at least 3 mol %, preferably at least 4 mol % of cordierite is used. In a particular embodiment of the glass according to the invention, no cordierite is present. 1 mol of cordierite means 1 mol of (2MgO·2Al2O3·5SiO2) / 9.
[0044] The glass according to the invention can therefore contain willemite in a proportion of 0-15 mol %, in particular up to 10 mol %, preferably up to 8.5 mol % or up to 7.5 mol %. In a preferred embodiment, at least 0.5 mol %, in particular at least 3 mol %, preferably at least 5 mol % of willemite is used. 1 mol of willemite means 1 mol of (2ZnO·SiO2) / 3.
[0045] In a preferred embodiment, the total proportion of grossular, cordierite and willemite in the glass according to the invention is at least 3 mol %, in particular at least 4 mol % or at least 5 mol %, in order to influence the thermal expansion coefficient as desired. However, it has proven advantageous to use these base glasses in a total amount of up to 25 mol %, in particular up to 20 mol %, 15 mol % or 10 mol %.
[0046] In the present specification, when a glass does not contain a component or a constituent phase or does not contain a specific component or a constituent phase, it is intended that this component or constituent phase may possibly be present in the glass as an impurity. That is, it means that it is not added in an essential amount. An essential amount is, according to the present invention, an amount less than 300 ppm (mol), preferably less than 100 ppm (mol), particularly preferably less than 50 ppm (mol), most preferably less than 10 ppm (mol). The glass of the present invention is in particular free of lithium, lead, arsenic, antimony, bismuth and / or cadmium.
[0047] Silicon dioxide and boron trioxide Finally, in order to adjust the brittleness to a low level, it is also possible to include a proportion of base glass consisting of pure SiO2. The glass according to the invention can have a proportion of SiO2 as base glass of at least 0 mol%, at most 50 mol%, at most 40 mol%, at most 30 mol%, at most 25 mol%, or at most 20 mol%. However, its content is limited to at most 18 mol%, more preferably at most 16 mol%, even more preferably at most 14 mol% or at most 12 mol%. Since a too high proportion of silicon dioxide impairs the melting property, in a particularly preferred embodiment, this component is included in an amount of less than 10 mol%. It has been found to be advantageous to use SiO2 in an amount of at least 1 mol%, in particular at least 3 mol% or at least 5 mol%.
[0048] The proportion of silicon dioxide is advantageously lower than the respective proportions of reedmargnalite and / or albite. In particular, the molar ratio of the proportion of silicon dioxide to reedmargnalite and / or albite is at most 1:2, at most 1:3, in particular at most 1:4. The limitation of the proportion of silicon dioxide is considered in particular to accentuate the properties of reedmargnalite and albite, which are essential base glasses in the glass of the invention.
[0049] The proportion of diboron trioxide, although less than silicon dioxide, also reduces the brittleness without affecting the melting property. It is therefore possible to provide a proportion of diboron trioxide of 0 mol% to 15 mol%, to 12 mol% or to 10 mol%. In a preferred embodiment, the proportion of diboron trioxide is at least 1 mol%, in particular up to 5 mol%, or up to 3 mol%.
[0050] The total proportion of silicon dioxide and diboron trioxide is preferably, according to the invention, at most 50 mol%, at most 40 mol%, at most 35 mol%, or at most 30 mol%, in particular at most 20 mol%, more preferably at most 15 mol%, particularly preferably at most 12.5 mol%.
[0051] Refractive index increasing component In order to substitute window glass as an optical cover glass, the refractive index needs to be adjusted to 1.5 to 1.6, for example 1.523 (typical refractive index of window glass at sodium D line, see M. Rubin, Optical properties of soda lime silica glasses, Solar Energy Materials 12 (1985), 275-288). Therefore, according to the present invention, heavy ions that increase the refractive index, namely up to three components, titanium-wadeit (containing titanium), strontium-feldspar (containing strontium), and ferrite feldspar (containing barium), are provided.
[0052] The proportion of titanium-wadeite in the glasses of the invention may be between 0 mol% and 24 mol%. Advantageously, the content is at most 20 mol%, more preferably at most 18 mol%. In some embodiments of the glasses of the invention, titanium-wadeite is absent. However, in preferred embodiments, the content of this component is at least 1 mol%, at least 5 mol%, at least 10 mol%, or even at least 13 mol%. One mole of titanium-wadeite means one mole of (K2O·TiO2·3SiO2) / 5. The TiO2 present in the glass increases the solarization resistance, which is important in particular for applications where a long service life is advantageous.
[0053] The proportion of strontium-feldspar in the glasses of the invention may be between 0 mol% and 20 mol%. Advantageously, the content is at most 10 mol%, more preferably at most 5 mol%. In some embodiments of the glasses of the invention, no strontium-feldspar is present. However, in preferred embodiments, the content of this component is at least 0.5 mol%, at least 1 mol%, at least 2 mol%, or even at least 3 mol%. One mole of strontium-feldspar means one mole of (SrO·Al2O3·2SiO2) / 4.
[0054] The proportion of ferrite in the glasses of the invention may be between 0 mol% and 20 mol%. Advantageously, the content is at most 10 mol%, more preferably at most 5 mol%. In some embodiments of the glasses of the invention, no ferrite is present. However, in preferred embodiments, the content of this component is at least 0.5 mol%, at least 1 mol%, at least 2 mol% or even at least 3 mol%. 1 mol of ferrite means 1 mol of (BaO·Al2O3·2SiO2) / 4.
[0055] As a measurement rule for selecting a refractive index in the range of 1.45 to 1.6, the Appen rules are used, which are explained in detail in H. Bach, N. Neuroth, Properties of Optical Glass, second corrected printing, Schott-Series on Glass, Springer-Verlag Berlin Heidelberg New York (1998), 73-76, including a detailed description of the calculation method and the necessary parameters. This mentioned publication of the Schott publication series is fully incorporated in the disclosure content of this application. This publication of the Schott publication series cites the original document of Appen.
[0056] Further ingredients In addition to the components already mentioned, the glass can contain further components, referred to herein as "residue". The proportion of the residue in the glass according to the invention is advantageously at most 5 mol %, in order not to disturb the glass properties, which are adjusted by the careful selection of the appropriate base glass. In particularly preferred embodiments, the proportion of the residue in the glass is at most 4 mol % or at most 3 mol %, more preferably at most 2 mol % or at most 1 mol %. The residue contains in particular oxides that are not contained in the base glass described herein. The residue therefore does not in particular comprise SiO2, TiO2, B2O3, Al2O3, ZnO, MgO, CaO, BaO, SrO, Na2O or K2O. According to the invention, further simple oxide additions are used as the residue, so-called "intermediates", i.e. oxides located between network formers such as SiO2 and network converters such as Na2O (see KH Sun, Journal of The American Ceramic Society Vol. 30, Nr. 9 (1947), 277-281). These oxides do not form glasses by themselves, but can be incorporated into the network within the abovementioned percentage ranges. The remainder can therefore contain oxides such as ZrO2 in particular. According to the theory of A. Dietzel, Die Kationenfeldstaerken und ihre Beziehungen zu Entglasungsvorgaengen, zur Verbindungsbildung und zu den Schmelzpunkten von Silicaten, Berichte der Bunsengesellschaft für physikalische Chemie Vol. 48 Nr. 1 (1942), 9-23, the "intermediates" also include Nb2O5 and Ta2O5, as can be calculated using the ionic radii according to R. Shannon, Revised Effective Ionic Radii and Systematic Studies of Interatomic Distances in Halides and Chalcogenides, Acta Cryst. (1976) A32, 751-767.
[0057] Advantageous Embodiments In preferred embodiments, the glasses according to the invention are characterized by the following preferred and particularly preferred proportions of constituent phases in the base glass composition. The preferred proportion ranges and further features described above and below for the glasses according to the invention also apply to the preferred and particularly preferred embodiments outlined below: [Table 5]
[0058] In preferred embodiments, the glasses according to the invention are characterized by the following preferred and particularly preferred proportions of constituent phases in the base glass composition. The preferred proportion ranges and further features described above and below for the glasses according to the invention also apply to the preferred and particularly preferred embodiments outlined below: [Table 6]
[0059] Other glass properties The glass of the present invention is advantageously present as a glass product, in particular as a glass ribbon or glass plate having a thickness of at most 2 mm, in particular at most 1 mm, particularly preferably at most 500 μm, at most 250 μm, at most 150 μm or at most 100 μm.The glass of the present invention can be processed into thin or ultra-thin glass.In particular thin glass can be difficult to chemically strengthen, so the high hardness that the glass according to the present invention has when not strengthened is particularly advantageous in the case of thin glass.
[0060] The glasses of the invention exhibit a thermal expansion (also CTE) of up to 8 ppm / K, in particular up to 7.5 ppm / K, which is advantageous for many applications, based on the combination of the glass constituent phases. The aforementioned thermal expansion coefficient is in a preferred embodiment at least 4 ppm / K or at least 5 ppm / K. The thermal expansion can be calculated as described above in equation (3).
[0061] The glass is based on a substantial proportion of albite glass and advantageously has a thickness of at least 15 μm at a temperature of 450° C. in KNO3. 2 / h or at least 20 μm 2 The glass has a chemical toughening property characterized by a diffusion capacity limit value of 1000 / h. The diffusion capacity limit value is a measure of the rate at which potassium ions are incorporated into the glass during chemical toughening. The limit value is calculated from the depth of the compressive stress layer (DoL) and time (t) as explained in German Utility Model No. DE202012012876U1.
[0062] Embodiment 1: 6.5 ppm / K <CTE<8ppm / K In one embodiment, the glass according to the invention has a CTE between 6.5 ppm / K and 8 ppm / K. The glass of this embodiment is achieved by satisfying the aforementioned inequality and applying formula (3) above. In this embodiment, the glass is particularly, but not exclusively, intended for combination with an alumina ceramic. An exemplary such structure is described in US Pat. No. 6,109,994, in which the glass cover plate ends in a field emission display structure that includes a column structure of alumina. Although a high CTE cannot be reconciled with a very low fragility, the number of angular degrees of freedom per atom calculated according to formula (1) above must be <0.30, preferably <0.29, particularly preferably <0.28, even more preferably <0.27, even more preferably <0.26, even more preferably <0.25. In particular, the number of angular degrees of freedom per atom is at least 0.1.
[0063] Embodiment 2: 4.5 ppm / K <CTE<6.5ppm / K In one embodiment, the glass according to the invention has a CTE between 4.5 ppm / K and 6.5 ppm / K. The glass of this embodiment satisfies the aforementioned inequality and is achieved by applying formula (3) above. In this embodiment, the glass is specifically, but not exclusively, intended for combination with aluminum nitride (see, e.g., CK Lee, S. Cochran, A. Abrar, KJ Kirk, F. Placido, Thick aluminum nitride films deposited by room-temperature sputtering for ultrasonic applications, Ultrasonics 42 (2004) 485-490). The number of angular degrees of freedom per atom calculated according to formula (1) above should be <0.30, preferably <0.29, particularly preferably <0.28, even more preferably <0.27, even more preferably <0.26, even more preferably <0.25, even more preferably <0.24, even more preferably <0.23, even more preferably <0.22, even more preferably <0.21, even more preferably <0.20. In particular, the number of angular degrees of freedom per atom is at least 0.1.
[0064] Embodiment 3: 3.5 ppm / K <CTE<4.5ppm / K In one embodiment, the glass according to the present invention has a CTE between 3.5 ppm / K and 4.5 ppm / K. The glass of this embodiment is achieved by satisfying the aforementioned inequality and applying formula (3) above. In this embodiment, the glass is specifically, but not exclusively, intended for combination with silicon or silicon-based components. Glasses with thermal expansion in this range are broadly combined with silicon or silicon-based components (see, e.g., F. Saharil, RV Wright, P. Rantakari, PB Kirby, T. Vaha-Heikkila, F. Niklaus, G. Stemme, J. Oberhammer, Low-temperature CMOS-compatible 3D-integration of monocrystalline-silicon based PZT RF MEMS switch actuators on rf substrates“, 2010 IEEE 23rd International Conference on Micro Electro Mechanical Systems (MEMS), 2010, 47-50). The number of angular degrees of freedom per atom calculated according to the above formula (1) should be <0.30, preferably <0.29, particularly preferably <0.28, even more preferably <0.27, even more preferably <0.26, even more preferably <0.25, even more preferably <0.24, even more preferably <0.23, even more preferably <0.22, even more preferably <0.21, even more preferably <0.20, even more preferably <0.19, even more preferably <0.18, even more preferably <0.17, even more preferably <0.16, even more preferably <0.15. In particular, the number of angular degrees of freedom per atom is at least 0.1.
[0065] In particular, it applies to the glass of the present invention that the number of angular degrees of freedom per atom in the bulk is less than 0.30, preferably less than 0.29, particularly preferably less than 0.28, even more preferably less than 0.27, even more preferably less than 0.26, even more preferably less than 0.25, even more preferably less than 0.24, even more preferably less than 0.23, even more preferably less than 0.22, even more preferably less than 0.21, even more preferably less than 0.20, even more preferably less than 0.19, even more preferably less than 0.18, even more preferably less than 0.17, even more preferably less than 0.16, even more preferably less than 0.15. If it is ensured that the number of angular degrees of freedom per atom does not exceed this value, the fragility remains in the desired range. In particular, this value is advantageous in order to allow the manufacture of ultra-thin glass articles as well. In particular, the number of angular degrees of freedom per atom is at least 0.1.
[0066] Manufacturing method The process is as follows: - melting glass raw materials; - forming glass articles, in particular glass ribbons or glass plates, from molten glass; - The process of cooling the glass The present invention also relates to a method for producing the glass of the present invention,
[0067] Cooling may be active cooling using a coolant, for example a cooling fluid, or may be accomplished by passive cooling.
[0068] In one embodiment, the forming of the glass article is carried out by the downdraw method, the overflow fusion method or the redraw method. In the flat glass method, the glass having the desired very low thickness can be produced. Furthermore, these methods have the advantage that they can achieve a high cooling rate.
[0069] The choice of raw materials is not limited to any particular raw materials. In particular, it is not necessary to use the above-mentioned base glasses as raw materials for these glasses, even if this is possible in principle. Rather, it is important to use raw materials with the appropriate stoichiometry so that the base glass is stoichiometrically contained in the glass.
[0070] surface quality The glasses of the present invention are advantageously characterized by a property gradient between the bulk glass and the surface of the glass article made of the glass. Likewise, glass articles made of the glasses described herein are also part of the present invention.
[0071] By "surface" is meant, according to the invention, the part of the glass close to the glass / air interface. The glass forming the surface is referred to herein as "surface glass", the rest of the glass further inside as "bulk glass". It is difficult to draw an exact line between surface and bulk, and therefore, in the present invention, the surface glass is defined to exist at a depth of about 6 nm. The properties of the surface glass at a depth of about 6 nm are therefore investigated. The properties of the bulk glass are investigated by calculation, since the glass composition does not change deeper than that by the manufacturing. In any case, the bulk glass exists at a depth of 500 nm. The surface can be influenced advantageously by certain measures during the glass manufacturing. The properties of the surface glass are very important for certain properties of the glass measured at the surface. These include in particular the alkali resistance and the hydrolysis resistance. The composition of the surface glass at a depth of about 6 nm can be measured by Cs-TOF-SIMS at 1000 eV.
[0072] It has been found that the loss of surface material occurring within the scope of the production of the glass according to the invention is mostly related to sodium and boron. Sodium is assigned to leadmargunalite and albite in the glass according to the invention. Boron is assigned to either leadmargunalite or potassium-leadmargunalite in the glass according to the invention or is present as the inherent constituent phase B2O3. Furthermore, it has been found that instead of the loss of sodium, boron and other elements, silicon is relatively enriched at the surface. However, this is only desirable within limit values.
[0073] According to DE102014101756B4, it is particularly favorable for hydrolytic stability if sodium ions are reduced at the surface. However, this reduction simultaneously affects the fragility or the number of angular degrees of freedom and the thermal expansion coefficient. The latter can be achieved by applying the above formula (2) for the average potential well depth to the standardized proportion of the individual cations d j / Σd j This becomes especially clear when the equation is transformed so that its relationship to:
number
[0074] When the average potential well depth is calculated when the proportion of cations with low potential well depths listed in Table 3 is decreased, the value in the surface region is clearly higher, which means that the thermal expansion coefficient at the surface is smaller, and therefore the expansion coefficients at the interior and surface are different.
[0075] Advantageously, the thermoforming applied to the glass of the invention results in a change in the glass composition at the surface. This change results in a deviation in the thermal expansion of the surface glass compared to the bulk glass. Based on the composition and in combination with the preferred embodiment of the manufacturing method, the glass according to the invention can have a coefficient of thermal expansion (CTE) in the bulk glass at a depth of about 6 nm at the surface, calculated from the composition measured by Cs-TOF-SIMS according to formula (4), of at least 50%, preferably at least 60%, at least 70% or at least 80%, which is particularly preferred according to the invention. In view of hydrolytic stability, the coefficient of thermal expansion calculated according to formula (4) is at most 99%, in particular at most 98% or at most 95%, at a depth of about 6 nm at the surface compared to that of the bulk glass. This value can in particular be measured immediately after the manufacture of the glass.
[0076] The loss of certain glass components at the glass surface, and therefore the thermal expansion, not only depends on the glass composition but also on the manufacturing method. In particular, the loss of free B2O3 can be adjusted by adjusting the water vapor partial pressure when forming the glass article. The higher the water vapor partial pressure, the more diboron trioxide will evaporate in the form of metaboric acid. Similarly, the thermal expansion coefficient at the surface glass can be influenced by increasing the pulling speed and decreasing the water vapor partial pressure. Thus, the skilled person can adjust the desired properties.
[0077] The glass of the invention may be in the form of a glass product, in particular a glass sheet or glass plate, and may have at least one, in particular two, fire-polished surfaces. A "fire-polished surface" is a surface characterized by a particularly low roughness. By the manufacturing method according to the invention, glass products with special surface quality can be manufactured. The glass product has at least one, in particular two, fire-polished surfaces, depending on the manufacturing method by which it is obtained. In contrast to mechanical polishing, during fire polishing the surface is not scraped off, but the polished material is heated to a high temperature so that it flows smoothly. Therefore, the cost of producing a smooth surface by fire polishing is substantially lower than the cost of producing a mechanically polished surface. The roughness of a fire-polished surface is lower than the roughness of a mechanically polished surface. By "surface" is meant the upper and / or lower surface in relation to the molded glass article, i.e. these two surfaces are the largest compared to the other surfaces.
[0078] The fire-polished surface of the glass according to the invention advantageously has a root-mean-square roughness (Rq or RMS) of at most 5 nm, preferably at most 3 nm, particularly preferably at most 1 nm. The surface roughness Rt of the glass is advantageously at most 6 nm, more preferably at most 4 nm, particularly preferably at most 2 nm. The roughness depth is determined according to DIN EN ISO 4287. The roughness Ra according to the invention is preferably less than 1 nm.
[0079] In the case of mechanically polished surfaces, the roughness values are worse. Moreover, in the case of mechanically polished surfaces, polishing tracks can be seen under an atomic force microscope (AFM). Furthermore, residues of mechanical polishing agents such as diamond powder, iron oxide and / or CeO2 can be seen under the AFM as well. Since mechanically polished surfaces must always be cleaned after polishing, leaching of certain ions occurs at the surface of the glass. This depletion of certain ions can be detected by secondary ion mass spectrometry (ToF-SIMS). Such ions are, for example, Ca, Zn, Ba and alkali metals.
[0080] use The use of the glasses according to the invention as cover glasses or display glasses, in particular as substrate glasses for metal lines or as electrically insulating dielectric interlayers, in particular as interposers, for example in electronic or optoelectronic devices or as plastic substitutes in surface shaping, is also in accordance with the invention.
[0081] Working Example The compositions shown in the base glasses can be easily converted to compositions in mole percent using a matrix. The compositions in the base glasses are shown in the following standardized form as above: [Table 7]
[0082] Conversion of these compositions to the following simple oxide compositions in mole percent is accomplished using the following matrix:
[0083] [Table 8] Here, the composition notation in mole percent for the base glass is multiplied into the matrix from the right as a column vector.
[0084] [Table 9]
[0085] The result of multiplying the column vector by the matrix is the composition of the glass in mole percent.
[0086] Conversely, compositions in mole percent can be easily converted to base glass compositions via the respective inverse matrices, where it should be understood that only those base glass compositions that do not result in a negative value for the base glass upon conversion are considered to be in accordance with the present invention.
[0087] Glass according to the invention As a first example, consider a glass having the following composition: Example 1 [Table 10]
[0088] This glass has the following properties: The number of angular degrees of freedom per atom calculated according to 1.(1) is therefore 0.291. 2. The average potential well depth calculated according to (2) is 1499 kJ / mol, which also results in a thermal expansion of 7.4 ppm / K according to (3).
[0089] The second example glass is obtained by replacing 8% potassium-leadmargnalite with albite, the purpose of which is to improve chemical toughening. Example 2 [Table 11]
[0090] This glass has the following properties: The number of angular degrees of freedom per atom calculated according to 1.(1) is therefore 0.298. 2. The average potential well depth calculated according to (2) is 1499 kJ / mol, as in Example 1, which also results in a thermal expansion of 7.4 ppm / K according to (3).
[0091] Example 1 and Example 2 were prepared as experimental melts. It was investigated how glass could be chemically strengthened. The samples were strengthened in KNO3 once at 440°C and once at 450°C for 9 hours.
[0092] Glass sheets (30 mm x 30 mm x 1 mm) were produced from the experimental melts. To homogenize the surface, the samples were precleaned in an ultrasonic bath at 37 kHz in 1% 12PA (weak alkaline cleaner) for 3 min. The samples were treated in KNO3 at 440 °C and 450 °C for 9 h, respectively. After ion exchange, the potassium nitrate salts must be removed from the samples. For this, the samples were cleaned at 130 kHz in 1% 12PA for 5 min and subsequently rinsed with deionized water.
[0093] The compressive stress (CS) and the depth of penetration (DoL) on the sheets were measured. The measurements of the compressive stress and the depth of penetration were carried out with a surface stress meter.
[0094] For each sample, CS and DoL were measured three times in the middle of each face. The table shows the average value and standard deviation of the measured laboratory melts (VSM).
[0095] [Table 12]
[0096] This embodiment is carried out as an ingot. For production by the pulling technique, the water vapor partial pressure is adjusted so that the total boron content at the surface is at least 80% of the boron content in the interior of the glass.
[0097] Example 3 [Table 13]
[0098] This glass has the following properties: The number of angular degrees of freedom per atom calculated according to 1.(1) is therefore 0.25. 2. The thermal expansion calculated according to (2) and (3) is 6.62 ppm / K.
[0099] Example 4 [Table 14]
[0100] This glass has the following properties: The number of angular degrees of freedom per atom calculated according to 1.(1) is therefore 0.196. 2. The thermal expansion calculated according to (2) and (3) is 4.96 ppm / K.
[0101] Example 5 [Table 15]
[0102] This glass has the following properties: The number of angular degrees of freedom per atom calculated according to 1.(1) is therefore 0.193. 2. The thermal expansion calculated according to (2) and (3) is 4.67 ppm / K.
[0103] Example 6 [Table 16]
[0104] This glass has the following properties: The number of angular degrees of freedom per atom calculated according to 1.(1) is therefore 0.274. 2. The thermal expansion calculated according to (2) and (3) is 7.01 ppm / K.
Claims
1. The following glass constituent phases: [Table 1] A glass having a composition characterized by:
2. 2. The glass according to claim 1, having an average thickness of at most 2 mm, in particular at most 1 mm or at most 0.5 mm.
3. The following glass constituent phases: [Table 2] 3. The glass of claim 1, having a composition characterized by:
4. The following glass constituent phases: [Table 3] 3. The glass of claim 1, having a composition characterized by:
5. The glass of any one of claims 1 to 4, wherein the sum of the proportions of leadmargunalite and potassium-leadmargunalite in the glass is greater than the proportion of albite.
6. 6. The glass according to claim 1, wherein the proportion of leadmarginalite and / or albite is greater than the proportion of silicon dioxide, in particular at least two times greater.
7. In addition to the constituent phases, the remainder may contain further components in a proportion not exceeding 5 mol %, in particular the following oxides: SiO 2 , TiO 2 , B 2 O 3 , Al 2 O 3 , ZnO, MgO, CaO, BaO, SrO, Na 2 O and / or K 2 The glass of claim 1 , which is free of O.
8. 8. The glass according to claim 7, wherein the residue has a proportion in the glass of at most 2 mol %, in particular at most 1 mol %.
9. 9. The glass according to claim 1, wherein the proportion of willemite is at least 0.5 mol-% and at most 7.5 mol-%.
10. 10. The glass according to claim 1, wherein the proportion of leadmargunalite is greater than the proportion of potassium-leadmargunalite, in particular the proportion of leadmargunalite is at least two times greater than the proportion of potassium-leadmargunalite.
11. 11. The glass according to claim 1, characterized in that it has a thermal expansion coefficient, calculated according to equations (2) and (3), between 6.5 ppm / K and 8 ppm / K, and that the number of angular degrees of freedom per atom, calculated according to equation (1), is at most 0.
30.
12. 11. The glass according to claim 1, characterized in that it has a thermal expansion coefficient, calculated according to equations (2) and (3), between 4.5 ppm / K and 6.5 ppm / K and that the number of angular degrees of freedom per atom, calculated according to equation (1), is at most 0.
30.
13. 11. The glass according to claim 1, characterized in that the thermal expansion coefficient, calculated according to equations (2) and (3), is between 3.5 ppm / K and 4.5 ppm / K and that the number of angular degrees of freedom per atom, calculated according to equation (1), is at most 0.
30.
14. 14. The glass according to claim 1, wherein the thermal expansion coefficient of the surface glass, calculated according to formulas (2) and (3), corresponds to at least 50% of the thermal expansion coefficient of the bulk glass, calculated according to formulas (2) and (3).
15. 15. The glass according to claim 1 , wherein the thermal expansion coefficient of the surface glass, calculated according to the formulas (2) and (3), corresponds to at most 99%, preferably 98%, particularly preferably 95% of the thermal expansion coefficient of the bulk glass, calculated according to the formulas (2) and (3).
16. The following steps: - melting suitable glass frits to produce a glass according to any one of claims 1 to 15, forming flat glass articles, in particular glass ribbons or glass plates, from the molten glass; - Cooling the glass The method of producing glass comprising the steps of:
17. 17. The method of claim 16, wherein forming the glass article is performed by a downdraw process, an overflow fusion process, or a redraw process.
18. 16. Use of the glass according to any one of claims 1 to 15 as a cover glass or display glass, substrate glass or an electrically insulating dielectric interlayer, in particular an interposer, in particular in electronic or optoelectronic devices or as a plastic substitute in surface shaping.
Citation Information
Patent Citations
Method for manufacturing tempered glass substrate and tempered glass substrate
JP2008195602A
Glass plate and method for producing glass plate
JP2011148683A
Titanium oxide-containing borosilicate glass free from arsenic and antimony and method for manufacturing the same
JP2013056817A
Flexible ultra-thin chemically strengthened glass
JP2016508954A
Glass base plate for display cover glass, and process for production thereof
WO2011065293A1