Method for reusing support, method for manufacturing prepreg, method for manufacturing laminate, method for manufacturing printed wiring board, and method for manufacturing semiconductor package
By ensuring the surface of peeled supports has no convex portions higher than 5 μm, the method addresses the resin repelling issue, enabling cost-effective reuse and improved manufacturing efficiency in prepreg, laminate, and semiconductor package production.
Patent Information
- Application Number
- JP2023075599
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-01
- Publication Date
- 2024-11-14
AI Technical Summary
The challenge of effectively reusing supports peeled from resin films in prepreg production is hindered by the resin film's repelling effect, leading to increased manufacturing costs and inefficiencies in existing methods.
A method for reusing supports by ensuring the surface of peeled supports has no convex portions higher than 5 μm, allowing for the reuse of supports without surface treatment, and using them in prepreg, laminate, printed wiring board, and semiconductor package manufacturing.
Enables the effective reuse of supports, reducing costs and improving manufacturing efficiency in prepreg, laminate, printed wiring board, and semiconductor package production by ensuring resin varnish adherence and uniform thickness accuracy.
Smart Images

Figure 2024160513000002 
Figure 2024160513000003 
Figure 2024160513000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for reusing a support, a method for manufacturing a prepreg, a method for manufacturing a laminate, a method for manufacturing a printed wiring board, and a method for manufacturing a semiconductor package. [Background technology]
[0002] As a method for manufacturing a prepreg for a printed wiring board, there is a method in which a resin film made of a thermosetting resin is prepared in advance, and aggregate and the resin film are heated and pressurized to bond them together to form a prepreg (see, for example, Patent Document 1). The resin film used in this method usually has a support such as polyethylene terephthalate (PET) for easy transportation. Therefore, when preparing a prepreg by this method, it is necessary to peel off this support. On the other hand, as a method for manufacturing a prepreg, there is a method (lay-up method) in which a fiber base material is immersed in a resin varnish and then dried (see, for example, Patent Document 2). The method described in Patent Document 1 requires a support (e.g., PET), which leads to an increase in manufacturing costs compared to the lay-up method described in Patent Document 2. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-132535 A [Patent Document 2] Japanese Patent Application Publication No. 01-272416 Summary of the Invention [Problem to be solved by the invention]
[0004] Furthermore, in recent years, companies are being required to use resources effectively as part of their efforts toward the SDGs (Sustainable Development Goals). Therefore, the present inventors attempted to produce a resin film for prepreg production again using a support peeled off from a resin film in the production of a prepreg using a resin film. However, it was found that the support often repelled the resin varnish, making it difficult to produce a resin film with a support, and it was found that it was not easy to reuse the support.
[0005] Therefore, an object of the present disclosure is to provide a method for reusing a support peeled off from a support-attached resin film. Another object of the present disclosure is to provide a method for manufacturing a prepreg, a method for manufacturing a laminate, a method for manufacturing a printed wiring board, and a method for manufacturing a semiconductor package. [Means for solving the problem]
[0006] As a result of extensive research to solve the above-mentioned problems, the inventors have discovered that the above-mentioned object can be achieved by ensuring that the surface condition of the side of the peeled support that was in contact with the resin film is in a specific state.
[0007] The present disclosure includes the following embodiments [1] to
[12] . [1] A method for reusing a support by attaching a resin film with a support to an aggregate, peeling the support from the resin film with a support, and reusing the peeled support, comprising the steps of: A method for reusing a support in which, when the surface of the peeled support that was in contact with the resin film is observed with a laser microscope within an area of 1,000 μm length x 1,000 μm width at any five points, no protrusions with a height of 5 μm or more are found. [2] The method for reusing a support according to the above [1], wherein the convex portions having a height of 5 μm or more are derived from the resin film. [3] The method for reusing the support according to [1] or [2] above, wherein the width of the protrusions having a height of 5 μm or more is 20 μm or more. [4] The method for reusing a support according to any one of the above [1] to [3], wherein the support has not been surface-treated with a release agent. [5] The method for reusing a support according to any one of the above [1] to [4], wherein the peeled support is reused in the production of a prepreg. [6] A method for producing a prepreg, comprising: attaching a resin film with a support to an aggregate, peeling the support from the resin film with a support, and applying a resin varnish to the peeled support to produce a resin film with a support, A manufacturing method for a prepreg in which, when the surface of the peeled support that was in contact with the resin film is observed with a laser microscope within an area of 1,000 μm length x 1,000 μm width at any five points, no convex parts with a height of 5 μm or more are present. [7] The method for producing a prepreg according to the above [6], wherein the convex portions having a height of 5 μm or more are derived from the resin film. [8] The method for producing a prepreg according to [6] or [7] above, wherein the width of the protrusions having a height of 5 μm or more is 20 μm or more. [9] The method for producing a prepreg according to any one of the above [6] to [8], wherein the support has not been surface-treated with a release agent.
[10] A method for producing a laminate, comprising laminating and molding a prepreg obtained by the production method according to any one of [6] to [9] above.
[11] A method for producing a printed wiring board, comprising forming a circuit on a laminate obtained by the production method according to
[10] above.
[12] A method for manufacturing a semiconductor package by mounting a semiconductor element on a printed wiring board obtained by the manufacturing method described in
[11] above. Effect of the Invention
[0008] According to the present disclosure, it is possible to provide a method for reusing a support peeled off from a support-attached resin film, a method for manufacturing a prepreg, a method for manufacturing a laminate, a method for manufacturing a printed wiring board, and a method for manufacturing a semiconductor package. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic cross-sectional view showing one aspect of the prepreg of the present embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view for explaining one aspect of the prepreg of the present embodiment. [Diagram 3] 1 is a surface observation image converted into black and white mode and used to calculate the abundance ratio of the impregnated region in the prepreg produced in Example 1. [Figure 4] 1 is a surface line roughness measurement image obtained by observing the peeled PET film surface with a laser microscope in Example 1. [Diagram 5] 1 is a surface line roughness measurement image obtained by observing the peeled PET film surface with a laser microscope in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In the numerical ranges described in the present disclosure, the upper or lower limit of the numerical range may be replaced with the values shown in the examples. In addition, the lower and upper limits of a numerical range may be arbitrarily combined with the lower or upper limit of another numerical range. In the expression of a numerical range "AA to BB", the numerical values AA and BB at both ends are included in the numerical range as the lower and upper limits, respectively. In the present disclosure, for example, the expression "10 or more" means 10 and a numerical value exceeding 10, and the same applies when the numerical values are different. Also, for example, the expression "10 or less" means 10 and a numerical value less than 10, and the same applies when the numerical values are different. In the present disclosure, when there are multiple substances corresponding to each component in the resin composition, the content of each component means the total content of the multiple substances present in the resin composition, unless otherwise specified. In this disclosure, the "resin component" does not include inorganic compounds such as inorganic fillers and pigments. Furthermore, the "solid content" refers to the non-volatile content excluding water and the diluent described below contained in the resin composition, and includes liquid, starch syrup, and wax-like substances at room temperature around 25°C. Additionally, any combination of the descriptions in this disclosure is also included in this embodiment.
[0011] [How to reuse the support] One aspect of this embodiment is the following method for reusing a support. A method for reusing a support by attaching a resin film with a support to an aggregate, peeling the support from the resin film with a support, and reusing the peeled support, comprising the steps of: A method for reusing a support in which, when the surface of the peeled support that was in contact with the resin film is observed with a laser microscope within an area of 1,000 μm length x 1,000 μm width at any five points, no protrusions with a height of 5 μm or more are found.
[0012] When the surface of the support peeled off from the resin film with the support is observed by a laser microscope in an area of 1,000 μm long x 1,000 μm wide at any five points, the absence of convex parts with a height of 5 μm or more enables reuse of the peeled off support, and the presence of convex parts with a height of 5 μm or more makes reuse of the peeled off support difficult. When a convex part with a height of 5 μm or more exists on the peeled off support, the convex part is usually a convex part derived from the resin film. When a convex part with a height of 5 μm or more (convex part derived from the resin film) exists on the peeled off support, the resin varnish is repelled, making it difficult to manufacture a prepreg using the peeled off support, and it is presumed that the absence of a convex part with a height of 5 μm or more (convex part derived from the resin film) enables the manufacture of a prepreg using the support peeled off from the resin film with the support. According to this embodiment, the support can be reused even if the support is not surface-treated with a release agent. Furthermore, according to this embodiment, it is possible to reuse the support peeled off from the support-attached resin film in the production of prepregs and the like. Here, "reuse" in the present disclosure means reusing the support without melting it, and does not include so-called recycling, in which the support is melted, molded, and used for other purposes. In addition, "attaching" includes not only a state in which the resin component of the resin film with a support is in contact with the aggregate, but also a state in which the resin component in the resin film penetrates into the voids in the aggregate, with the latter state being particularly preferred.
[0013] Whether or not the peeled support has a protrusion having a height of 5 μm or more (protrusion derived from the resin film) is determined by observing an arbitrary 5 positions in an area of 1,000 μm length × 1,000 μm width with a laser microscope. As the laser microscope, for example, a laser microscope "VK-X series" manufactured by Keyence Corporation may be used. Specific examples of the "VK-X series" include the shape measurement laser microscope VK-X100. There are no particular limitations on the means for preventing the peeled-off support from having protrusions with a height of 5 μm or more (protrusions derived from the resin film), but examples of the means include including a siloxane compound in the raw material components of the resin film, and controlling the temperature, pressure, and vacuum time when attaching (impregnating) the resin film with the support to the aggregate, as described below.
[0014] The height of the protrusions may be 7 μm or more, 10 μm or more, 20 μm or more, 50 μm or more, 80 μm or more, or 100 μm or more. The greater the height of the protrusions, the easier they are to repel resin varnish, and the more difficult it tends to be to manufacture a prepreg using a support peeled off from the support-attached resin film. There is no particular upper limit to the height of the convex portions, and the height may be 400 μm or less, 300 μm or less, 200 μm or less, 150 μm or less, or 120 μm or less. In view of the above, the height of the convex portion may be 5 to 400 μm.
[0015] The width of the convex portion having a height of 5 μm or more may be 20 μm or more, 50 μm or more, 70 μm or more, 80 μm or more, 90 μm or more, or 100 μm or more. The larger the width of the convex portion, the easier it is to repel resin varnish, and the more difficult it tends to be to manufacture a prepreg using the support peeled off from the support-attached resin film. There is no particular upper limit to the width of the convex portion having a height of 5 μm or more, and it may be 500 μm or less, 300 μm or less, 150 μm or less, or 120 μm or less. In view of the above, the width of the protrusions having a height of 5 μm or more may be 20 to 500 μm.
[0016] In the method for reusing a support of this embodiment, the operation of attaching the resin film with the support to an aggregate relates to the production of a prepreg. That is, the method for reusing a support of this embodiment relates to a method for reusing a support that is peeled off from the resin film during the production of a prepreg and is usually unnecessary. The purpose of reusing the support is not particularly limited, and it can be used for the production of a film with a resin for embedding a circuit, in addition to the production of a prepreg.
[0017] [Prepreg manufacturing method] One aspect of this embodiment is the following method for producing a prepreg. A method for producing a prepreg, comprising: attaching a resin film with a support to an aggregate, peeling the support from the resin film with a support, and applying a resin varnish to the peeled support to produce a resin film with a support, A manufacturing method for a prepreg in which, when the surface of the peeled support that was in contact with the resin film is observed with a laser microscope within an area of 1,000 μm length x 1,000 μm width at any five points, no convex parts with a height of 5 μm or more are present.
[0018] In the manufacturing method of the prepreg of this embodiment, each wording is as explained in the method of reusing the support body.
[0019] Hereinafter, one embodiment of the method for producing a prepreg will be described. A preferred aspect of this embodiment is a method in which the resin film with a support is attached to an aggregate, the support is peeled off, a resin film with a support is produced using the peeled support, and the resin film with the support is heated and pressurized under reduced pressure or normal pressure to be attached to the aggregate. This production method is a method for producing a prepreg by reusing the support. The manufacturing method of the prepreg before and after the reuse of the support is not particularly limited, but from the viewpoint of increasing the thickness accuracy, the following manufacturing method is preferred. That is, a manufacturing method of the prepreg is preferred in which an aggregate is impregnated with a resin film with a support prepared using a peeled support by lamination, the resin film of the resin film with the support being formed from a thermosetting resin composition, the aggregate is provided with an impregnated region and an unimpregnated region with the thermosetting resin composition, and the unimpregnated region is made to exist intermittently. It is more preferred that the unimpregnated region exists intermittently in the in-plane direction.
[0020] 1 and 2, when impregnating an aggregate such as glass cloth with a resin film, by intentionally providing an area in the aggregate that is not impregnated with the thermosetting resin composition, a layer of the thermosetting resin composition near the surface (hereinafter, abbreviated as a resin layer) exists without following the undulations of the aggregate such as glass cloth. As a result, the thickness of the metal-clad laminate is prevented from becoming uneven, and high thickness precision can be achieved in the metal-clad laminate. Furthermore, the non-impregnated regions are not continuous from one end of the prepreg to the other end but are present discontinuously, which tends to improve insulation reliability. Although the exact reason is unclear, it is speculated that this is because the thermosetting resin composition is sufficiently impregnated in the vicinity of the area with high aggregate density when the metal-clad laminate is produced.
[0021] In this embodiment, the ratio of the impregnated region of the thermosetting resin composition in the aggregate is defined as that obtained by the following calculation method. From the viewpoint of the thickness accuracy of the metal-clad laminate, the ratio of the impregnated region obtained based on the "calculation method" described later is not particularly limited, but may be 30 to 98%, 30 to 95%, 35 to 95%, 40 to 95%, 45 to 90%, 50 to 90%, 55 to 90%, or 60 to 85%. When the ratio is 98% or less, the effect of improving the thickness accuracy of the metal-clad laminate tends to be large, and when it is 95% or less, this tendency becomes even greater. In addition, when the ratio is 30% or more, the powder falling off of the thermosetting resin composition from the prepreg is suppressed, so that the secondary effect of good handleability tends to be obtained. If the ratio of the impregnated regions is 30% or more, non-impregnated regions are likely to exist intermittently, and from this viewpoint, the ratio of the impregnated regions is preferably 50% or more. In this embodiment, from the viewpoint of satisfying the condition that "when an area of 1,000 μm long × 1,000 μm wide at any five points on the surface of the peeled support on the side where the resin film was in contact is observed with a laser microscope, no convex parts with a height of 5 μm or more are present," the ratio of the impregnated regions is preferably 30 to 95%, more preferably 30 to 90%, and may be 35 to 90%. In particular, when the thermosetting resin composition contains a siloxane compound, the ratio of the impregnated regions is preferably in the above range, and when the thermosetting resin composition does not contain a siloxane compound, the ratio of the impregnated regions is preferably 35 to 95%, more preferably 40 to 90%, and even more preferably 45 to 90%.
[0022] -Calculation method- A surface observation image is obtained by observing the surface of the prepreg using an optical microscope at a magnification of 50. The observation conditions are those described in detail in the Examples from the viewpoint of photographing in an appropriate brightness. The obtained surface observation image is converted to black and white mode by image editing software, and then saved in BMP (Microsoft Windows Bitmap Image) format. Next, the black and white mode surface observation image saved in BMP format is converted to RGB (Red, Green, Blue) values for each pixel by image conversion software, and then saved in CSV (comma-separated values) format. The RGB data saved in CSV format is pasted into Microsoft Excel (Microsoft Corporation), and the areas of the black parts (RGB value = 255) and the white parts (RGB value = 0) are calculated. From these values, the area ratio of the black parts to the total of the black parts and the white parts is calculated. The area ratio of the black parts thus obtained is regarded as the abundance ratio of the impregnated region. As the image editing software, for example, "Microsoft Paint" (manufactured by Microsoft Corporation) can be used. Furthermore, as the image conversion software, for example, free software "bmp2csv" can be used. In the above observation, when the surface observation image taken at a moderate brightness is converted to a black and white mode, the surface where the unimpregnated region of the thermosetting resin composition exists below the observation surface is a void portion that easily reflects light, and is therefore represented as "white", and the other surfaces are represented as "black". Here, when taking a surface observation image, it is preferable to adjust the exposure time during surface photography within a range of 60 to 100 ms, so that the image can be taken at a moderate brightness that can fully reflect the impregnated region and the unimpregnated region. In the surface observation image of the prepreg, the areas in order of color intensity are "areas in the resin layer where no aggregate exists", "areas in which the aggregate is sufficiently impregnated with the thermosetting resin composition", and "areas in which the aggregate is insufficiently impregnated with the thermosetting resin composition". In this embodiment, the "areas in the resin layer where no aggregate exists" are also included in the impregnated region. If the surface observation image is too bright, not only the part where the resin is not sufficiently impregnated into the aggregate but also the part where the resin is sufficiently impregnated into the aggregate will tend to be shown in white in the surface observation image in the black and white mode, and if the image is even brighter, the surface observation image in the black and white mode will tend to be white overall. On the other hand, if the surface observation image is too dark, the surface observation image in the black and white mode will tend to be black overall, making it difficult to reflect the presence of unimpregnated areas. Therefore, it is preferable to take a photograph at a moderate brightness. As an example of converting a surface observation image taken at a moderate brightness into a black and white mode, the surface observation image converted into the black and white mode obtained in Example 1 is shown in FIG. 3. In FIG. 3, it can be observed that impregnated areas and unimpregnated areas alternate in the in-plane direction. In addition, the area ratio of the white areas to the total area of the white and black areas can be easily calculated by using the COUNTIF function in Microsoft Excel (Microsoft Corporation).
[0023] The resin film with a support can be produced by forming a layer of a thermosetting resin composition (resin layer) on one side of the support. The resin layer can be formed, for example, by applying the resin varnish to one side of the support and then drying it. The method of applying the resin varnish is not particularly limited, and can be carried out using a known coating device such as a comma coater, a bar coater, a kiss coater, a roll coater, a gravure coater, a die coater, etc. It is preferable to appropriately select these coating devices depending on the film thickness of the resin layer. The drying temperature and drying time will vary depending on the amount of organic solvent used, the boiling point of the organic solvent, etc., but for example, in the case of a resin varnish containing 30 to 70 mass % of an organic solvent, a resin film can be suitably formed by drying at 50 to 160°C for 1 to 8 minutes.
[0024] (Thickness of resin film) The thickness of the resin film may be appropriately determined depending on the thickness of the prepreg. For example, when the thickness of the aggregate is in the range of 40 to 120 μm, the thickness of the resin film is preferably 10 to 100 μm, more preferably 10 to 70 μm, further preferably 10 to 50 μm, and may be 15 to 50 μm or 20 to 45 μm. Here, the thickness of the resin film is a value measured as follows. First, the total thickness of the resin-attached film after coating is measured using a Digimatic indicator at any five points. The resin layer at the measurement points is peeled off with an adhesive tape, and the thickness of the support is measured using a Digimatic indicator, and the average value of the values obtained by subtracting the thickness of the support from the total thickness is obtained. When the thickness of the resin film is equal to or greater than the lower limit, it tends to be possible to secure a sufficient amount of resin for impregnating an aggregate such as a thick glass cloth having a thickness of 40 μm or more. When the thickness of the resin film is equal to or less than the upper limit, it tends to be easy to manufacture the resin film.
[0025] (Support) Examples of the support include organic films such as polyethylene terephthalate (PET), biaxially oriented polypropylene (OPP), polyethylene, polyvinyl fluorate, and polyimide; metal or alloy films such as copper and aluminum. These supports may or may not be surface-treated with a release agent. The thickness of the support is not limited, and from the viewpoints of ease of handling when applying the thermosetting resin composition and economic efficiency, it is preferably 10 to 200 μm, more preferably 20 to 100 μm, and even more preferably 30 to 70 μm. The support does not have to be made of a single component, but may be formed of multiple layers (two or more layers) of different materials. As the support, a commercially available product can be used.
[0026] (Method of impregnating aggregate with resin film) Next, a method for impregnating the aggregate with the resin film by lamination will be described. First, the resin film with a support is placed on at least one surface of the aggregate so that the resin film is in contact with the aggregate. Then, the resin film with the support and the aggregate are heated and pressurized, so that the aggregate is impregnated with the resin film. At this time, the aggregate is provided with discontinuous regions that are not impregnated with the thermosetting resin composition. In this way, the prepreg of this embodiment with a support is obtained. The heating and pressure application here is preferably carried out by lamination, which can be performed by (a) roll lamination under normal pressure, or (b) lamination under reduced pressure by vacuum lamination or the like.
[0027] (a) The conditions for roll lamination under normal pressure are not particularly limited, but the heating temperature is preferably 80 to 180° C., and the pressing pressure is preferably 0.05 to 1.0 MPa / m. (b) The conditions for the method of laminating under reduced pressure are not particularly limited, but the heating temperature is preferably 50 to 170°C, more preferably 110 to 160°C, the pressurizing time is preferably 10 to 120 seconds, more preferably 20 to 80 seconds, and the compression pressure is preferably 0.05 to 1.0 MPa, more preferably 0.1 to 0.6 MPa.
[0028] (Method of providing intermittent non-impregnated areas) The method for providing the aggregate with the non-impregnated regions with the thermosetting resin composition intermittently is not particularly limited, and examples thereof include a method of adjusting the conditions for heating and pressurizing the support-attached resin film and the aggregate, specifically, a method of adjusting the lamination conditions. Specific methods for adjusting the heating and pressurizing conditions are not particularly limited, but include, for example, the following methods. First, a prepreg is prepared under a predetermined heating and pressing condition, and then the ratio of the impregnated region of the thermosetting resin composition in the aggregate is calculated based on the calculation method. As a result, if the impregnated region is 100%, that is, if there is no unimpregnated region, the heating temperature or the bonding pressure is lowered, or both the heating temperature and the bonding pressure are lowered, the prepreg is reprepared, and the ratio of the impregnated region is calculated again. By repeating this process as necessary, the conditions for producing a prepreg having discontinuous unimpregnated regions (preferably discontinuous in the in-plane direction) can be easily grasped. When it is desired to adjust the proportion of unimpregnated regions to a lower value, the heating temperature or the bonding pressure may be increased, or both the heating temperature and the bonding pressure may be increased, and the prepreg may be produced again.
[0029] The heating temperature is preferably 120° C. or higher, more preferably 120 to 170° C., and even more preferably 130 to 160° C., from the viewpoint of providing discontinuous regions in the aggregate that are not impregnated with the thermosetting resin composition. The compression pressure is preferably 0.2 MPa or more, more preferably 0.2 to 1.0 MPa, even more preferably 0.3 to 0.8 MPa, and particularly preferably 0.3 to 0.6 MPa, from the viewpoint of providing discontinuous regions in the aggregate that are not impregnated with the thermosetting resin composition. When lamination is performed under reduced pressure, it is also possible to adjust the proportion of unimpregnated regions by adjusting the degree of vacuum and the time of vacuum application. Furthermore, in the manufacturing method of the prepreg "before" the support is reused, from the viewpoint of satisfying the condition that "when an area of 1,000 μm length × 1,000 μm width at any five locations on the surface of the peeled support on the side where the resin film was in contact is observed with a laser microscope, no convex parts with a height of 5 μm or more are present", the heating temperature is preferably 120 to 160°C, more preferably 125 to 155°C, and even more preferably 130 to 150°C, the compression bonding pressure is preferably 0.30 to 0.70 MPa, more preferably 0.35 to 0.65 MPa, and even more preferably 0.40 to 0.60 MPa, and when laminating under reduced pressure, the vacuum time is preferably 10 to 55 seconds, more preferably 15 to 50 seconds, even more preferably 20 to 45 seconds, and particularly preferably 20 to 40 seconds.
[0030] It is preferable to laminate the resin film by disposing one or more sheets on each side of the aggregate. The number of resin films per side of the aggregate is preferably one or two, and more preferably one.
[0031] (Thermosetting resin composition) Next, the thermosetting resin composition that is the raw material of the resin film used in this embodiment will be described. Examples of the thermosetting resin contained in the thermosetting resin composition include epoxy resins, maleimide compounds, phenolic resins, polyimide resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins, melamine resins, etc. These may be used alone or in combination of two or more.
[0032] From the viewpoint of low warpage, the content of the thermosetting resin in the thermosetting resin composition is preferably 1 to 90 parts by mass, more preferably 10 to 80 parts by mass, even more preferably 40 to 80 parts by mass, and particularly preferably 60 to 80 parts by mass, relative to 100 parts by mass of the resin component in the thermosetting resin composition.
[0033] The thermosetting resin composition, even if it does not contain a siloxane compound, can satisfy the condition that "when the surface of the peeled support on the side where the resin film was in contact is observed with a laser microscope within an area of 1,000 μm length × 1,000 μm width at any five locations, no convex parts with a height of 5 μm or more are present." In the method for producing a prepreg "before" the support is reused, it is preferable that the thermosetting resin composition contains a siloxane compound, since this tends to expand the lamination conditions that make it easier to satisfy the above condition. The siloxane compound is not particularly limited as long as it is a compound containing a siloxane skeleton, and one type may be used alone, or two or more types may be used in combination. In the manufacturing method of the prepreg "before" the support is reused, the siloxane compound is preferably a siloxane compound having a functional group, from the viewpoint of satisfying the condition that "when an area of 1,000 μm length × 1,000 μm width at any five points on the surface of the peeled support on the side where the resin film was in contact is observed with a laser microscope, there are no convex parts with a height of 5 μm or more." Examples of the functional group include an amino group, a hydroxyl group, and an epoxy group. The siloxane compound is more preferably a siloxane diamine.
[0034] As the siloxane compound, commercially available products can be used. For example, examples of "siloxane compounds having two primary amino groups in one molecule" having a methyl group on the side chain include "KF-8010" (amino functional group equivalent: 430 g / mol), "X-22-161A" (amino functional group equivalent: 800 g / mol), "X-22-161B" (amino functional group equivalent: 1,500 g / mol), "KF-8012" (amino functional group equivalent: 2,200 g / mol), "KF-8008" (amino functional group equivalent: 5,700 g / mol), and "X-22-9409" (amino functional group equivalent: 700 g / mol) (all manufactured by Shin-Etsu Chemical Co., Ltd.). Examples of "siloxane compounds having two primary amino groups per molecule" with phenyl groups on the side chains include "X-22-1660B-3" (amino functional group equivalent: 2,200 g / mol) (manufactured by Shin-Etsu Chemical Co., Ltd.), "BY-16-853U" (amino functional group equivalent: 460 g / mol), "BY-16-853" (amino functional group equivalent: 650 g / mol), and "BY-16-853B" (amino functional group equivalent: 2,200 g / mol) (all manufactured by Dow Corning Toray Co., Ltd.). Examples of siloxane compounds modified with epoxy groups at both ends include "X-22-163" (epoxy group functional group equivalent: 200 g / mol), "X-22-163A" (epoxy group functional group equivalent: 1,000 g / mol), "X-22-163B" (epoxy group functional group equivalent: 1,800 g / mol), and "KF-105" (epoxy group functional group equivalent: 490 g / mol). Examples of side chain carbinol modified siloxane compounds include "X-22-4015" (hydroxyl value 30 mg KOH / g) and "X-22-4039" (hydroxyl value 58 mg KOH / g). These may be used alone or in combination of two or more.
[0035] When the siloxane compound has a functional group at its terminal, the functional group equivalent is preferably 300 to 3,000 g / mol, more preferably 400 to 2,500 g / mol, further preferably 600 to 1,500 g / mol, and may be 600 to 1,100 g / mol. In the case of a siloxane compound having a hydroxyl group in the side chain, the hydroxyl value is preferably from 20 to 100 mgKOH / g, and more preferably from 25 to 70 mgKOH / g.
[0036] In the manufacturing method for a prepreg "before" the support is reused, the content of the siloxane compound in the thermosetting resin composition is preferably 2 to 30 parts by mass, more preferably 2 to 25 parts by mass, and even more preferably 3 to 20 parts by mass, relative to 100 parts by mass of the resin component in the thermosetting resin composition, from the viewpoint of satisfying the condition that "when an arbitrary five area of 1,000 μm length × 1,000 μm width on the surface of the peeled support on the side that was in contact with the resin film is observed with a laser microscope, there are no convex parts with a height of 5 μm or more."
[0037] The thermosetting resin composition may further contain inorganic fillers, organic fillers, curing accelerators, flame retardants, ultraviolet absorbers, antioxidants, photopolymerization initiators, fluorescent brightening agents, adhesion improvers, and the like. The thermosetting resin composition may contain an acrylic resin. However, from the viewpoint of satisfying the condition that "when an area of 1,000 μm long × 1,000 μm wide at any five locations on the surface of the peeled support on the side where the resin film was in contact is observed with a laser microscope, no convex parts with a height of 5 μm or more are present," it is preferable that the content of the acrylic resin is small. For example, the content of the acrylic resin is preferably 30 parts by mass or less, more preferably 15 parts by mass or less, even more preferably 5 parts by mass or less, particularly preferably 1 part by mass or less, and most preferably 0 part by mass, relative to 100 parts by mass of the resin component in the thermosetting resin composition.
[0038] When producing a resin film, the thermosetting resin composition is preferably in the form of a varnish in which each component is dissolved or dispersed in an organic solvent. Examples of the organic solvent include alcohol-based solvents such as methanol, ethanol, propanol, butanol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as butyl acetate and propylene glycol monomethyl ether acetate; ether-based solvents such as tetrahydrofuran; aromatic solvents such as toluene, xylene, and mesitylene; nitrogen-containing solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; and sulfur-containing solvents such as dimethylsulfoxide. These may be used alone or in combination of two or more.
[0039] (aggregate) Examples of aggregates that can be used in this embodiment include inorganic fiber substrates such as glass and carbon; organic fiber substrates such as aramid and cellulose; and metal fiber substrates made of iron, copper, aluminum, alloys of these metals, etc. These may be used alone or in combination of two or more. In particular, from the viewpoint of dielectric properties, inorganic fibers are preferred, and glass is more preferred. The aggregate may be in the form of, for example, a woven fabric, a nonwoven fabric, a roving, a chopped strand mat, a surfacing mat, etc. Among these, the woven fabric is preferred. The thickness of the aggregate is, for example, 5 μm to 0.5 mm, and from the viewpoint of enabling low warpage and high density wiring, it is preferably 5 μm to 100 μm, more preferably 8 μm to 60 μm, and even more preferably 10 to 30 μm. From the viewpoints of heat resistance, moisture resistance, processability, etc., these aggregates may be surface-treated with a silane coupling agent or the like, or may be mechanically opened.
[0040] The solid content of the thermosetting resin composition in the prepreg is preferably 20 to 90 mass %.
[0041] [Method of manufacturing laminate and method of manufacturing printed wiring board] In this embodiment, a method for producing a laminate is also provided by laminating and molding the prepreg obtained by the above-mentioned production method (however, the prepreg is produced by reusing the peeled support). More specifically, a laminate (also called a laminated plate) can be produced by preparing one sheet or a stack of 2 to 20 sheets of the prepreg obtained in this embodiment, and laminating and molding a metal foil such as copper or aluminum on one or both sides of the prepreg as necessary. The metal foil is not particularly limited as long as it is used for electrical insulating material applications, but copper foil is preferred. When the metal foil is copper foil, the resulting laminate (laminate) is generally called a copper-clad laminate. The molding conditions for producing the laminate can be, for example, those for laminates and multilayer boards for electrical insulating materials. Specifically, the laminate can be produced using a multi-stage press, a multi-stage vacuum press, a continuous molding machine, an autoclave molding machine, etc., under conditions of a temperature of 100 to 250°C, a pressure of 0.2 to 10 MPa, and a heating time of 0.1 to 5 hours. The laminate can also be produced by combining the FPR precursor and an inner layer wiring board and laminating and molding them. Furthermore, a printed wiring board can be manufactured by forming a circuit in the laminate, specifically, by processing the metal foil into a circuit.
[0042] [Semiconductor package] The present embodiment also provides a method for manufacturing a semiconductor package by mounting a semiconductor element on the printed wiring board obtained by the above manufacturing method. The semiconductor package can be manufactured by mounting a semiconductor element such as a semiconductor chip or memory at a predetermined position on the printed wiring board and sealing the semiconductor element with a sealing resin or the like. EXAMPLES
[0043] The present embodiment will now be described in more detail with reference to the following examples, but these examples are not intended to limit the present embodiment. The prepregs obtained in the following examples and the PET films after peeling were evaluated by the following methods.
[0044] [1. Ratio of impregnated areas] The ratio (%) of the area impregnated with the thermosetting resin composition in the aggregate was calculated based on the following calculation method. -Calculation method- The surface of the prepreg was observed under the following conditions using an optical microscope (manufactured by Olympus Corporation, product name: MX61L-F) to obtain a surface observation image. <Observation conditions> ·Magnification: 50x Observation mode: dark field Sensitivity: ISO400 Exposure time for surface photography: 60-100ms - Brightness of the observation environment: Two 35W fluorescent lamps were installed 2m above the observation stage. The obtained surface observation image was converted to black and white mode using image editing software, and then saved in BMP (Microsoft Windows Bitmap Image) format. Next, the black and white mode surface observation image saved in BMP format was converted to RGB (Red, Green, Blue) values for each pixel using image conversion software, and then saved in CSV (comma-separated values) format. The RGB data saved in CSV format was pasted into Microsoft Excel (Microsoft Corporation), and the areas of the black parts (RGB value = 255) and white parts (RGB value = 0) were calculated. From these values, the area ratio of the black parts to the total of the black and white parts was calculated. The area ratio of the black parts thus obtained was taken as the presence ratio (%) of the impregnated region. Here, when photographing the surface observation image, the image was photographed at an appropriate brightness by adjusting the exposure time during surface photographing between 60 and 100 ms as described above so as to adequately reflect the impregnated and non-impregnated areas. The image editing software used was "Microsoft Paint" (manufactured by Microsoft Corporation), and the image conversion software used was "bmp2csv," which is free software.
[0045] [2. PET film surface] (2-1. Visual Evaluation) The surface condition of the PET film peeled off in each example was visually observed and rated according to the following evaluation criteria. Note that an A rating means that the resin has been sufficiently transferred to the aggregate, the peelability from the support is good, and the product passes the test. Both B and C ratings are failures as products. A: There is no resin on the support at all. B: A thin layer of resin is attached to the support. C: A large amount of resin is attached to the support. (2-2. Evaluation using a laser microscope) As an evaluation method stricter than visual inspection, evaluation was performed using a laser microscope. Specifically, the PET film peeled off in each example was evaluated using a laser microscope "Shape Measuring Laser Microscope VK-X100" manufactured by Keyence Corporation. The evaluation method consisted of observing an area of 1,000 μm length × 1,000 μm width at any five points on the PET film with the laser microscope, and evaluating according to the following evaluation criteria. A: No protrusions having a height of 5 μm or more were observed. B: One to four or more protrusions having a height of 5 μm or more were observed. C: Five or more protrusions having a height of 5 μm or more were observed.
[0046] [3. Reusability of PET film] The PET film peeled off in each example was recoated with the resin varnish prepared in each example, and the appearance of the recoated film was evaluated according to the following evaluation criteria. A: The resin varnish was not repelled by the PET and could be applied successfully. C: The resin varnish was repelled by the PET and could not be applied.
[0047] Manufacturing Example 1 (Preparation of Resin Varnish A) (1-1. Preparation of modified maleimide resin) 595.8 g of bis(4-maleimidophenyl)methane, 54.2 g of 4,4'-diaminodiphenylmethane, and 350.0 g of propylene glycol monomethyl ether were placed in a 2 L reaction vessel equipped with a thermometer, a stirrer, and a moisture meter with a reflux condenser, and the mixture was allowed to react for 5 hours under reflux to obtain a solution of a modified maleimide resin. (1-2. Preparation of resin varnish A) 107 parts by mass of the modified maleimide resin solution, 30 parts by mass of tetrafunctional naphthalene-type epoxy resin "EXA-4710" (manufactured by DIC Corporation), 18 parts by mass of aluminum hydroxide (average particle size: 4.0 μm), 130 parts by mass of spherical fused silica (average particle size: 0.5 μm), 0.3 parts by mass of isocyanate masked imidazole, and a mixture of methyl isobutyl ketone and cyclohexanone as solvents were mixed to prepare resin varnish A with a solids concentration of 65% by mass.
[0048] Manufacturing Example 2 (Preparation of Resin Varnish B) Resin varnish B with a solids concentration of 65% by mass was prepared by mixing 60 parts by mass of phenol novolac epoxy resin "EPICLON (registered trademark) N-770" (manufactured by DIC Corporation, epoxy equivalent: 188 g / eq), 40 parts by mass of biphenyl aralkyl phenol resin (manufactured by UBE Corporation, product name: MEH-7700), 18 parts by mass of aluminum hydroxide (average particle size: 4.0 μm), 86 parts by mass of spherical fused silica (average particle size: 0.5 μm), 0.5 parts by mass of isocyanate masked imidazole, and a mixture of methyl isobutyl ketone and cyclohexanone as solvents.
[0049] Production Example 3 (Preparation of Resin Varnish C; Containing Siloxane Compound) 10 parts by mass of siloxane modified with amines at both ends (manufactured by Shin-Etsu Chemical Co., Ltd., product name: X-22-161A, functional group equivalent of amino group: 800 g / mol), 40 parts by mass of α-naphthol / cresol novolac type epoxy resin (manufactured by Nippon Kayaku Co., Ltd., product name: NC-7000L, epoxy equivalent: 223 to 238 g / eq), 40 parts by mass of 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, 9 parts by mass of 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 200 parts by mass of spherical fused silica (average particle size: 0.5 μm), 0.2 parts by mass of tetraphenylphosphonium tetra-p-tolylborate, and methyl ethyl ketone as a solvent were added and mixed to prepare resin varnish C with a solid content concentration of 65% by mass.
[0050] Manufacturing Example 4 (Preparation of Resin Varnish D) Acrylic resin (manufactured by Negami Chemical Industries, Ltd., product name: HAN5-M90S, acrylic resin containing nitrile groups, weight average molecular weight: 90 × 10 4 ), 45 parts by mass of tetrabromobisphenol A type epoxy resin (manufactured by DIC Corporation, product name: EPICLON 153), 10 parts by mass of cresol novolac type resin (manufactured by DIC Corporation, product name: KA-1165), 25 parts by mass of aluminum hydroxide (average particle size: 4.0 μm), 25 parts by mass of spherical fused silica (average particle size: 0.5 μm), 0.1 parts by mass of 2-phenylimidazole, and methyl ethyl ketone as a solvent were added and mixed to prepare resin varnish D with a solids concentration of 40 mass%.
[0051] Example 1 (1. Preparation of resin film) The resin varnish A obtained in Production Example 1 was applied onto a PET film (manufactured by Toray Industries, Inc., thickness: 50 μm, film with no release treatment and surface roughness (Ra) of 0.04 μm, product name: Lumirror (registered trademark) S10) using a comma coater. At this time, the amount of application was adjusted so that the thickness after drying would be 30 μm. Thereafter, a resin film with a PET film was produced by heating and drying at 130° C. for 2 minutes. (2. Preparation of prepreg) Next, glass cloth "IPC#2116" (manufactured by Nitto Boseki Co., Ltd., basis weight: 104 g / m 2 The resin layer surface of the resin film with the PET film was placed on both sides of a glass cloth (substrate width: 530 mm, thickness: 91 μm) so that the resin layer surface of the resin film with the PET film was in contact with the glass cloth. This laminate of "PET film / resin film / glass cloth / resin film / PET film" was heated and pressed under vacuum using a vacuum laminating device. In this way, a prepreg with a PET film was obtained in which the glass cloth was impregnated with the thermosetting resin composition of the resin film. The conditions for the vacuum lamination were a hot plate temperature of 130°C, a pressure of 0.5 MPa, a degree of vacuum of 100 kPa or less, and a vacuum time of 30 seconds. The PET film was peeled off from the obtained prepreg with the PET film using a peeling device having a mechanism for peeling with a blade, to obtain prepreg 1. The peeled PET film was taken up on a roll. Next, the peeled PET film was evaluated according to the above-mentioned method. (3. Reusing peeled PET film; making prepregs) The same operations were carried out in the above "1. Preparation of resin film", except that the PET film peeled off in "2. Preparation of prepreg" was used instead of the PET film "Lumirror (registered trademark) S10". Subsequently, the same operations as in "2. Preparation of prepreg" were carried out again to obtain a prepreg. The results are shown in Table 1. Figure 4 shows one of the surface line roughness measurement images obtained by observation with a laser microscope.
[0052] Example 2 In Example 1, the resin varnish A used in "1. Preparation of resin film" was changed to the resin varnish B obtained in Production Example 2, and the conditions for vacuum lamination in "2. Preparation of prepreg" were changed to 140°C. Except for this, the same operations and evaluations were performed. The results are shown in Table 1.
[0053] Example 3 In Example 1, the PET film used in "1. Preparation of resin film" was changed to a PET film (manufactured by Toray Industries, Inc., thickness: 50 μm, matte type film with no release treatment and surface roughness (Ra) of 0.27 μm, product name: Lumirror (registered trademark) #50-X44), the amount of resin varnish applied was adjusted so that the thickness after drying would be 35 μm, and the conditions for vacuum lamination in "2. Preparation of prepreg" were changed from 130° C. to 140° C., except for these, the same operations and evaluations were performed. The results are shown in Table 1.
[0054] Example 4 The same operations and evaluations were carried out as in Example 1, except that the conditions for vacuum lamination in "2. Preparation of prepreg" were changed to 150°C, 0.6 MPa, and 40 seconds, respectively, for the hot plate temperature, compression pressure, and vacuum time. The results are shown in Table 1.
[0055] Example 5 The same operations and evaluations were performed as in Example 1, except that the vacuum laminator in "2. Preparation of prepreg" was changed to a roll laminator under normal pressure, the hot plate temperature and compression pressure were changed to 150°C and 0.4 MPa, and the conveying speed was changed to 2.0 m / min. The results are shown in Table 1.
[0056] Example 6 In Example 1, the resin varnish A used in "1. Preparation of resin film" was changed to the resin varnish C obtained in Production Example 3, and the conditions of the vacuum lamination in "2. Preparation of prepreg" were changed to the hot plate temperature, compression pressure, and vacuum time of 120°C, 0.3 MPa, and 20 seconds, respectively, except for these, the same operation and evaluation were performed. The results are shown in Table 1.
[0057] Example 7 In Example 1, the glass cloth used in "2. Preparation of prepreg" was "IPC#1078" (manufactured by Nitto Boseki Co., Ltd., basis weight: 47 g / m 2The same operations and evaluations were carried out except that the substrate was changed to a thickness of 44 μm (substrate width: 530 mm, thickness: 44 μm). The results are shown in Table 1.
[0058] Example 8 In Example 2, the amount of resin varnish applied was adjusted so that the thickness after drying in "1. Preparation of resin film" was 16 μm, and the glass cloth used in "2. Preparation of prepreg" was "IPC#1037" (manufactured by Nitto Boseki Co., Ltd., basis weight: 24 g / m 2 The same operations and evaluations were performed except that the conditions for vacuum lamination were changed to a hot plate temperature of 130°C and a vacuum time of 20 seconds. The results are shown in Table 1.
[0059] Example 9 In Example 1, the amount of resin varnish applied was adjusted so that the thickness after drying in "1. Preparation of resin film" was 14 μm, and the glass cloth used in "2. Preparation of prepreg" was "IPC#1027" (manufactured by Nitto Boseki Co., Ltd., basis weight: 20 g / m 2 The same operations and evaluations were carried out except that the substrate was changed to a plate having a width of 530 mm and a thickness of 21 μm. The results are shown in Table 1.
[0060] Comparative Example 1 The same operations and evaluations were carried out as in Example 1, except that the resin varnish A used in "1. Preparation of resin film" was changed to the resin varnish D obtained in Production Example 4. The results are shown in Table 1. Figure 5 shows one of the surface line roughness measurement images obtained by observation with a laser microscope.
[0061] Comparative Example 2 The same operations and evaluations were performed as in Example 6, except that the vacuum laminator in “2. Preparation of prepreg” was changed to a roll laminator under normal pressure, the hot plate temperature and bonding pressure were changed to 100° C. and 0.2 MPa, respectively, and the conveying speed was changed to 2.0 m / min. The results are shown in Table 1.
[0062] Comparative Example 3 The same operations and evaluations were carried out as in Example 1, except that the conditions for vacuum lamination in "2. Preparation of prepreg" were changed to the hot plate temperature, compression pressure, and vacuum time of 110°C, 0.2 MPa, and 20 seconds. The results are shown in Table 1.
[0063] Comparative Example 4 The same operations and evaluations were carried out as in Example 1, except that the conditions for vacuum lamination in "2. Preparation of prepreg" were changed to the hot plate temperature and vacuum time of 150°C and 60 seconds. The results are shown in Table 1.
[0064] [Table 1]
[0065] As can be seen from Table 1, when the PET film peeled off from the supported resin film used in the production of the prepreg was observed with a laser microscope in an area of 1,000 μm length × 1,000 μm width at any five points, if no protrusions with a height of 5 μm or more were present (Examples 1 to 9), the peeled PET film could be reused in the production of the prepreg. On the other hand, in Comparative Examples 1 to 4, where convex parts of 5 μm or more in height were present when observed with a laser microscope in an arbitrary five locations of 1,000 μm in length × 1,000 μm in width, the peeled PET film could not be reused for the production of prepregs. In particular, in Comparative Examples 2 and 3, although no resin adhesion was confirmed on the peeled PET film surface by visual inspection, the presence of convex parts of 5 μm or more in height when observed with a laser microscope meant that the peeled PET film could not be reused for the production of prepregs, which is an important result.
Claims
1. A method for reusing a support by attaching a resin film with a support to an aggregate, peeling the support from the resin film with a support, and reusing the peeled support, comprising the steps of: A method for reusing a support, in which when an area of 1,000 μm length x 1,000 μm width at any five points on the surface of the peeled support on the side where the resin film was in contact is observed with a laser microscope, no protrusions with a height of 5 μm or more are present.
2. The method for reusing a support according to claim 1 , wherein the convex portions having a height of 5 μm or more are derived from the resin film.
3. 2. The method for reusing a support according to claim 1, wherein the width of the protrusions having a height of 5 μm or more is 20 μm or more.
4. 2. The method for reusing a support according to claim 1, wherein the support is one that has not been surface-treated with a release agent.
5. The method for reusing a support according to claim 1, wherein the peeled support is reused for the production of a prepreg.
6. A method for producing a prepreg, comprising: attaching a resin film with a support to an aggregate, peeling the support from the resin film with a support, and applying a resin varnish to the peeled support to produce a resin film with a support, A method for producing a prepreg, in which when the surface of the peeled support on the side that was in contact with the resin film is observed with a laser microscope within an area of 1,000 μm in length and 1,000 μm in width at any five locations, no convex parts with a height of 5 μm or more are present.
7. The method for producing a prepreg according to claim 6, wherein the convex portions having a height of 5 μm or more are derived from the resin film.
8. The method for producing a prepreg according to claim 6, wherein the width of the convex portion having a height of 5 μm or more is 20 μm or more.
9. The method for producing a prepreg according to claim 6, wherein the support is not surface-treated with a release agent.
10. A method for producing a laminate by laminating and molding a prepreg obtained by the method according to any one of claims 6 to 9.
11. A method for producing a printed wiring board, comprising forming a circuit on a laminate obtained by the method according to claim 10.
12. A method for manufacturing a semiconductor package, comprising mounting a semiconductor element on a printed wiring board obtained by the manufacturing method according to claim 11.
Citation Information
Patent Citations
Manufacture of prepreg
JP1989272416A
Manufacturing process for prepreg with carrier, prepreg with carrier, manufacturing process for thin double-sided plate, thin double-sided plate and manufacturing process for multilayer-printed circuit board
JP2011132535A