Polymer
The use of cyclic acrylic monomers in polymers addresses deactivation issues with cyclic ketene acetals, enabling stable storage and versatile polymer production with controlled decomposition.
Patent Information
- Application Number
- JP2023075639
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-01
- Publication Date
- 2024-11-14
AI Technical Summary
Existing polymers using cyclic ketene acetals as monomers face issues with deactivation by hydroxyl groups and limited compatibility with other monomers, necessitating immediate synthesis and restricting polymer variety.
Employing a cyclic acrylic monomer with specific structures represented by general formulas (1) and (2), allowing for stable storage and easy copolymerization with allyl alcohol monomers, enabling a wide range of polymer production through radical ring-opening polymerization.
The new polymers maintain activity over time, facilitating easy polymer manufacturing and offering versatile polymer options without the need for immediate synthesis, with controlled main chain cleavage via transesterification.
Smart Images

Figure 2024160533000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to novel polymers. [Background technology]
[0002] The chemical decomposition of polymer compounds is applied to advanced functional materials such as dismantlable adhesive materials, resist materials, and self-repairing materials, which utilize the changes in physical properties before and after the decomposition, as well as medical materials such as biocompatible materials and drug delivery materials. Furthermore, in recent years, there has been a demand for the use of chemical decomposition of polymer compounds to achieve highly efficient chemical recycling and promote decomposition in nature, and they are expected to become environmentally friendly materials. In light of this background, molecular design is being considered that introduces weak covalent bonds, such as ester bonds and acetal bonds, into the main chains of polymer compounds, which can be broken in response to specific stimuli such as light, heat, acid, and base.
[0003] Therefore, a method of introducing an ester bond into the main chain by radical ring-opening polymerization using a cyclic ketene acetal (hereinafter also referred to as CKA) as a monomer has attracted attention (Non-Patent Document 1). By radical copolymerizing CKA and a vinyl monomer, an ester bond can be introduced into the main chain, and this ester bond can be cleaved by hydrolysis using a strong base. In addition, the present inventors have proposed to generate a nucleophilic group in the side chain of an adjacent unit and induce main chain cleavage by an ester exchange reaction between the main chain and the side chain, rather than directly cleaving the main chain (Non-Patent Document 2). However, CKA is inactivated by hydroxyl groups, and there are problems such as the fact that CKA reacts with water during storage and is inactivated, and that the monomers that copolymerize with CKA are limited (e.g., Fig. 88(b) in Non-Patent Document 1). [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] Antoine Tardy, Julien Nicolas, Didier Gigmes, Catherine Lefay, Yohann Guillaneuf, “Radical Ring-Opening Polymerization: Scope, Limitations, and Application to (Bio)Degradable Materials”, Chem Rev., 2017 Feb 8, 117(3), 1319-1406 [Non-Patent Document 2] Kaho Toyama, Yasuhiro Kosaka, "Synthesis of Easily Degradable Vinyl Polymers via Copolymerization of Allyl Alcohol Derivatives and Cyclic Ketene Acetals," Proceedings of the Society of Polymer Science, Vol. 71, No. 1, 2C10, May 2022 Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention aims to provide a novel polymer using a cyclic acrylic monomer capable of radical ring-opening polymerization as an alternative to cyclic ketene acetals. [Means for solving the problem]
[0006] The means for solving the above problems are as follows. 1. A repeating unit derived from a cyclic acrylic monomer represented by the following general formula (1), A repeating unit derived from an allyl alcohol monomer represented by the following general formula (2), A polymer comprising: [ka] [In the formula, R 1 and R 2 each independently represents a hydrogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a phenyl group, or a substituted phenyl group. X represents a sulfur atom, a sulfonyl group, or a disulfide group. Y is an oxygen atom, a carbon atom, a sulfur atom, or -NR 4- indicates R 4 represents a hydrogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a phenyl group, or a substituted phenyl group. Z is a divalent linking group and forms a 7- to 15-membered ring. [ka] [In the formula, R 3 represents a C1-C6 alkyl group, a C1-C6 haloalkyl group, a phenyl group, or a substituted phenyl group. W represents a hydrogen atom or a trialkylsilyl group. 2. The polymer according to 1, having a structure represented by the following general formula (3): [ka] 3. The polymer according to 1 or 2, wherein X is a sulfur atom and Y is an oxygen atom or a sulfur atom. 4. The polymer according to any one of 1. to 3., wherein W is a hydrogen atom. 5. A method for decomposing the polymer according to 2. in the presence of a base. Effect of the Invention
[0007] The polymer of the present invention is made from a stable cyclic acrylic monomer, and the raw material monomer can be easily stored for a long period of time while maintaining its activity, and there is no need to synthesize the monomer immediately before the production of the polymer, so that the polymer is easy to produce. The cyclic acrylic monomer used as the raw material for the polymer of the present invention is unlikely to undergo reactions other than radical ring-opening polymerization, so other monomers to be copolymerized are not particularly limited, and a variety of polymers can be obtained.
[0008] In the polymer of the present invention having a structure represented by general formula (3), the main chain can be cleaved by a transesterification reaction between the main chain and the side chain. The polymer of the present invention can be used for adhesives, paints, molded articles, etc. In particular, the polymer of the present invention having a structure represented by general formula (3) can be used for dismantling adhesives, degradable paints, resists, etc. because the main chain can be cut and the timing of decomposition can be controlled. [Brief description of the drawings]
[0009] [Figure 1] 1H-NMR spectrum of the binary copolymer obtained in Example 1. [Diagram 2] 2 is a graph showing the change over time in a size exclusion chromatogram when DBU was added to the binary copolymer obtained in Example 1. [Diagram 3] 1H-NMR spectra of the binary copolymer obtained in Example 1 before and after the decomposition reaction with DBU. [Figure 4] 1 is a graph showing the change over time in a size exclusion chromatogram when TBD was added to the binary copolymer obtained in Example 1. [Diagram 5] 1H-NMR spectrum of the binary copolymer obtained in Reference Example 1. [Figure 6] 2 is a graph showing the change over time in a size exclusion chromatogram when DBU was added to the binary copolymer obtained in Reference Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described below. Note that the following description is merely an example of the present invention and does not limit the present invention in any way. The present invention is not limited to the embodiments described below, and may include various modifications, changes, and improvements to each disclosed element (including elements described in the claims, specification, and drawings) within the scope of the present invention and based on the technical ideas of the present invention. Furthermore, various combinations, substitutions, and selections of each disclosed element are possible within the scope of the claims of the present invention. Furthermore, in this specification, the expression "A to B (A and B are numbers)" means a numerical range including both ends, that is, A or more and B or less.
[0011] Cyclic acrylic monomers The cyclic acrylic monomer used in the present invention is represented by the following general formula (1). [ka] [In the formula, R 1 and R 2 each independently represents a hydrogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a phenyl group, or a substituted phenyl group. X represents a sulfur atom, a sulfonyl group, or a disulfide group. Y is an oxygen atom, a carbon atom, a sulfur atom, or -NR 4 - indicates R 4 represents a hydrogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a phenyl group, or a substituted phenyl group. Z is a divalent linking group and forms a 7- to 15-membered ring.
[0012] In this specification, the substituted phenyl group refers to a phenyl group substituted with one or more groups selected from an alkyl group, an alkenyl group, an alkynyl group, an aryl group, a halogen atom, a haloalkyl group, a haloalkenyl group, a haloalkynyl group, a haloaryl group, an alkoxy group, an alkenyloxy group, an aryloxy group, a haloalkoxy group, a haloalkenyloxy group, a haloaryloxy group, an amino group, an alkylamino group, an arylamino group, an acyl group, an aroyl group, an arylacyl group, an acylamino group, an alkylsulfonyloxy group, an arylsulfenyloxy group, a heterocyclyl group, a heterocisyloxy group, a heterocisylamino group, a haloheterocyclyl group, an alkoxycarbonyl group, an alkylthio group, an alkylsulfonyl group, an arylthio group, an arylsulfonyl group, an aminosulfonyl group, a dialkylamino group, and a dialkylsulfonyl group.
[0013] R 1 and R 2each independently represents a hydrogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a phenyl group, or a substituted phenyl group. Among these, from the viewpoints of polymerizability and prevention of chain transfer reaction to the resulting polymer, a phenyl group, a methyl group, or a hydrogen atom is preferred, from the viewpoint of polymerizability, a methyl group and a hydrogen atom are more preferred, and a hydrogen atom is particularly preferred. X represents a sulfur atom, a sulfonyl group, or a disulfide group. Among these, the sulfur atom and the sulfonyl group are preferred because of ease of synthesis, and the sulfur atom is more preferred. Y is an oxygen atom, a carbon atom, a sulfur atom, or -NR 4 - indicates R 4 represents a hydrogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a phenyl group, or a substituted phenyl group. Among these, an oxygen atom, a sulfur atom, or -NR 4 - is preferred, and an oxygen atom or a sulfur atom is more preferred.
[0014] Z is a divalent linking group. In this specification, the divalent linking group is -CH-, -CHR 5 R is one or a combination of two or more selected from -, -C(=O)-O-, -OC(=O)-, -O-, and -S-. 5 represents a hydrogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a phenyl group, or a substituted phenyl group. Examples of divalent linking groups (represented as X on the left and Y on the right) include -(CH2)2-, -CH2-CH(CH3)-, -(CH2)3-, -(CH2)2-O-(CH2)2, -(CH2)6-, -(CH2)2-C(=O)-O-(CH2)4-(CH2)2-C(=O)-O-(CH2)6-, -(CH2)2-C(=O)-O-(CH2)2-SS-(CH2)2-, and the like.
[0015] The cyclic acrylic monomer used in the present invention has a 7- to 15-membered ring. Among these, in order to ensure ring-opening polymerizability, a 7- to 13-membered ring is preferred, and a 7- to 11-membered ring is more preferred.
[0016] Specifically, the compounds represented by the following general formulas (1)-1 to (1)-11 can be suitably used as the cyclic acrylic monomer. [ka]
[0017] [ka]
[0018] [ka]
[0019] Allyl alcohol monomers The allyl alcohol monomer used in the present invention is represented by the following general formula (2). [ka] [In the formula, R 3 represents a C1-C6 alkyl group, a C1-C6 haloalkyl group, a phenyl group, or a substituted phenyl group. W represents a hydrogen atom or a trialkylsilyl group.
[0020] R 3 represents a C1-C6 alkyl group, a C1-C6 haloalkyl group, a C1-C6 hydroxyalkyl group, a phenyl group, or a substituted phenyl group. Among these, from the viewpoint of ease of monomer synthesis, a C1-C6 alkyl group is preferred, and an ethyl group or a methyl group is more preferred. W represents a hydrogen atom or a trialkylsilyl group. The alkyl group of the trialkylsilyl group includes a C1-C6 alkyl group, such as a trimethylsilyl group, a triethylsilyl group, and a dimethyl-tert-butylsilyl group. Among these, a hydrogen atom or a trimethylsilyl group is preferred, and a hydrogen atom is more preferred.
[0021] "polymer" The polymer of the present invention has a repeating unit derived from a cyclic acrylic monomer represented by general formula (1) and a repeating unit derived from an allyl alcohol monomer represented by general formula (2). The polymer of the present invention may also contain other comonomers in addition to the cyclic acrylic monomer and allyl alcohol monomer described above. The other comonomers are not particularly limited as long as they are radically copolymerizable with the cyclic acrylic monomer and allyl alcohol monomer, and examples thereof include (meth)acrylic acid, (meth)acrylic acid esters, (meth)acrylamide, styrene, vinyl acetate, etc.
[0022] The polymer of the present invention preferably has a structure represented by the following general formula (3). [ka]
[0023] Decomposition of polymers The polymer of the present invention having a structure represented by general formula (3) can cleave the main chain by undergoing an ester exchange reaction between the main chain and the side chain by making the side chain derived from the allyl alcohol monomer an alkoxide group. The reaction formula is shown below. Since a stable six-membered ring is formed by this ester exchange reaction, the reaction is irreversible and proceeds efficiently.
[0024] [ka]
[0025] To start the decomposition, the side chain derived from the allyl alcohol monomer may be made into an alkoxide group, and for example, a basic compound or a fluoride ion may be used as a decomposition initiator. As the decomposition initiator, TBD (1,5,7-triazabicyclo[4.4.0]dec-5-ene), DBU (1,8-diazabicyclo[5.4.0]undec-7-ene), DBN (1,5-diazabicyclo[4.3.0]nonene-5), tetrabutylammonium fluoride, etc. may be used. Among these, TBD, which is also a catalyst for the transesterification reaction, can particularly rapidly promote the decomposition.
[0026] The temperature at which the decomposition is carried out is not particularly limited, but from the viewpoint of ease of handling, it is preferably 20 to 100°C, more preferably 20 to 50°C, and particularly preferably 20 to 25°C. The solvent for carrying out the decomposition is not particularly limited, and it is not necessary to use a solvent. However, from the viewpoint of smoothly generating an alkoxide, a solvent in which the polymer of the present invention is soluble is preferred, and acetone, chloroform, toluene, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, N-methylpyrrolidone, methanol, tetrahydrofuran, acetonitrile, and 2-butanone are preferred, with tetrahydrofuran being more preferred. The pH for carrying out the decomposition is not particularly limited, but when the solvent is water, methanol, or the like that can decompose the ester bond in the main chain of the polymer of the present invention, the pH is preferably 5 to 9 in order to suppress the hydrolysis.
[0027] Polymer manufacturing method The polymer of the present invention can be produced by a conventionally known radical polymerization reaction. The cyclic acrylic monomer represented by the general formula (1) is not deactivated by a hydroxyl group, unlike cyclic ketene acetal (CKA), so the monomer can be stored for a long period of time while maintaining its activity, and there is no need to synthesize the monomer immediately before the production of the polymer. As described above, the polymer of the present invention having the structure represented by general formula (3) can cleave the main chain at the position represented by general formula (3) where the cyclic acrylic monomer and the allyl alcohol monomer are bonded in a specific order. Therefore, the decomposition property can be adjusted by the molar ratio of the cyclic acrylic monomer and the allyl alcohol monomer. Specifically, the closer the composition ratio of the repeating unit derived from the cyclic acrylic monomer and the repeating unit derived from the allyl alcohol monomer is to equimolar, the more the structure represented by the above general formula (3) is formed. Therefore, the decomposition property of the obtained polymer can be controlled by the monomer charging ratio.
[0028] The polymer of the present invention can be used for adhesives, paints, molded articles, etc. The polymer having the structure represented by the general formula (3) can be used for dismantling adhesives, degradable paints, resists, etc. because the main chain of the polymer can be cut by a basic compound or the like and the timing of decomposition can be controlled. EXAMPLES
[0029] <Analytical equipment> (NMR spectrum) Measurements were performed using a nuclear magnetic resonance (NMR) spectrometer "AVANCE NEO" (Bruker) at 25° C. Deuterated chloroform was used as the measurement solvent, and tetramethylsilane was used as the internal standard. (molecular weight) Two size exclusion columns "Shodex HK-404L" (Showa Denko) were connected in series to an EXTREMA chromatograph (JASCO) and heated to 40°C. N,N-dimethylformamide (for GPC, Wako Pure Chemical Industries) was used as the eluent at 0.8 mL / min, and the column was detected with an ultraviolet absorption spectrometer "UV-4070" (detection at 280 nm, JASCO) and a differential refractometer (RI-4035, JASCO). The molecular weight was measured using standard polymethyl methacrylate (TSK Gel Oligomer Kit, Tosoh, MW: 6.48 × 10 5 , 2.52×10 5 , 1.42×10 5 , 2.91×10 4 , 8.59×10 3, 4.25×10 3 ) was used for calibration.
[0030] <Example 1: Synthesis of a binary copolymer of ethyl 2-(hydroxymethyl)acrylate and 3-methylene-1-oxa-5-thiacycloundecan-2-one> 2-(hydroxymethyl)ethyl acrylate (0.776g, 5.96mmol) and 3-methylene-1-oxa-5-thiacycloundecan-2-one (0.273g, 1.18mmol) were dissolved in 1,4-dioxane (2.35mL), 2,2'-azobisisobutyronitrile (22mg, 0.13mmol) was added, and the mixture was freeze-degassed three times, and then heated at 70°C for 5 hours. After cooling to room temperature, the mixture was added dropwise to diethyl ether (50mL) cooled with liquid nitrogen. The precipitate collected by decantation was dissolved in chloroform (1.5mL) and added dropwise to diethyl ether (30mL) cooled with liquid nitrogen. The precipitate was collected by decantation, dissolved again in chloroform (1.0mL), and added dropwise to diethyl ether (30mL) cooled with liquid nitrogen. The precipitate was collected by decantation and dried in vacuum to give the copolymer as a transparent glassy solid (0.292 g, 29.2% yield).
[0031] The binary copolymer shown in Figure 1 1 In the H-NMR spectrum, all signals were assigned to units derived from ethyl 2-(hydroxymethyl)acrylate and 3-methylene-1-oxa-5-thiacycloundecane-2-one. From the integral intensity ratio of the signal of the methyl group contained in the unit derived from ethyl 2-(hydroxymethyl)acrylate observed at around 1.3 ppm and the signal of the O-methylene group observed at 3.4 to 4.4 ppm, the copolymer composition was determined to be [ethyl 2-(hydroxymethyl)acrylate]:[3-methylene-1-oxa-5-thiacycloundecane-2-one]=74:26. The number average molecular weight (Mn) calculated in terms of poly(methyl methacrylate) obtained from the size exclusion chromatogram was 10,400, and the molecular weight dispersity (Mw / Mn) was 1.65.
[0032] <Example 2: Solution decomposition of a binary copolymer using 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU)> The binary copolymer (30 mg) synthesized in Example 1 was dissolved in tetrahydrofuran (0.30 mL), and 1,8-diazabicyclo[5.4.0]undec-7-ene (25 μL, 167 μmol) was added while stirring in an oil bath at 25°C. After 5 minutes, 25 μL of the sample was taken for size exclusion chromatography measurement. 2 μL of acetic acid was added to the taken sample to stop the reaction, and then it was diluted with 0.5 mL of chloroform. This was washed with 0.5 mL of distilled water, and the organic layer was recovered and concentrated to measure the size exclusion chromatogram. Furthermore, 1 hour after the start of the reaction, 100 μL was taken from the reaction mixture, and 9 μL of acetic acid was added to stop the reaction, and the same operation was performed to obtain the size exclusion chromatogram and the size exclusion chromatogram. 1 H-NMR spectrum was measured. 24 hours after the start of the reaction, the remaining sample was analyzed using size exclusion chromatogram and 1 H-NMR spectrum was measured.
[0033] The change in size exclusion chromatogram with the reaction time is shown in Figure 2. The peak top molecular weight (Mp) before the reaction was 15,400, but decreased to 5,300 5 minutes after the start of the reaction and to 800 after 24 hours. The decrease in molecular weight confirmed main chain scission, and it was also confirmed that the binary copolymer obtained in Example 1 had a structure represented by general formula (3). Before and 24 hours after the start of the reaction 1A comparison of H-NMR spectra is shown in Figure 3. The signal originating from the O-methylene group adjacent to the OH group of the side chain, which was around 3.6 ppm, changed to a sharp shape, and the signal originating from the O-methylene group adjacent to the ester bond, which was around 4.2 ppm, decreased. In addition, a sharp signal originating from the lactone ring formed by the transesterification reaction between the main chain and the side chain appeared around 4.4 to 4.6 ppm. These changes are due to the fact that in a hetero chain consisting of consecutive units derived from 2-(hydroxymethyl)ethyl acrylate and units derived from 3-methylene-1-oxa-5-thiacycloundecane-2-one, a five-membered ring lactone was formed by the transesterification reaction between the main chain and the side chain, and an alcohol terminal was generated due to the cleavage of the main chain.
[0034] Example 3: Solution decomposition of a binary copolymer using 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD) The binary copolymer (11 mg) synthesized in Example 1 was dissolved in tetrahydrofuran (0.20 mL) and 1,5,7-triazabicyclo[4.4.0]dec-5-ene (8 mg, 57 μmol) was added while stirring at room temperature. After 5 minutes, 0.10 mL of the sample was taken for size exclusion chromatography measurement and diluted with N,N-dimethylformamide to measure the size exclusion chromatogram. Size exclusion chromatograms before and after 5 minutes of reaction are shown in Figure 4. The peak top molecular weight (Mp) before the reaction was 15,400, but after 5 minutes the molecular weight had decreased to a range below the minimum value of the calibration curve. Mp estimated by extrapolating the calibration curve was 170.
[0035] <Reference Example 1: Decomposition of a binary copolymer of methyl methacrylate and 3-methylene-1-oxa-5-thiacycloundecan-2-one> (Synthesis of binary copolymers) Methyl methacrylate (0.253g, 2.53mmol) and 3-methylene-1-oxa-5-thiacycloundecan-2-one (0.101g, 0.504mmol) were dissolved in 1,4-dioxane (1.0mL), 2,2'-azobisisobutyronitrile (11mg, 67mmol) was added, and the mixture was freeze-degassed three times and then heated at 70°C for 15 hours. After cooling to room temperature, the mixture was dropped into methanol (20mL) cooled with dry ice. The precipitate collected by decantation was dissolved in dichloromethane (1.0mL) and dropped into methanol (20mL) cooled with dry ice. The precipitate was collected by centrifugation and decantation, and dried in vacuum to obtain a binary copolymer as a transparent glassy solid (97mg, yield: 27.4%).
[0036] Figure 5 shows the structure of the resulting binary copolymer. 1 The H-NMR spectrum shows that all signals were assigned to units derived from methyl methacrylate and 3-methylene-1-oxa-5-thiacycloundecane-2-one. From the integral intensity ratio of the methyl group signal in the unit derived from methyl methacrylate observed at around 0.8-1.3 ppm and the O-methylene group signal observed at 4.0-4.4 ppm, the copolymer composition was determined to be [methyl methacrylate]:[3-methylene-1-oxa-5-thiacycloundecane-2-one]=79:21. The number average molecular weight (Mn) calculated as poly(methyl methacrylate) was 11,800, and the molecular weight dispersity (Mw / Mn) was 1.59, as determined by size exclusion chromatogram.
[0037] (Decomposition of binary copolymers using 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU)) The same procedure as in Example 2 was repeated except that the binary copolymer (10 mg) of methyl methacrylate and 3-methylene-1-oxa-5-thiacycloundecane-2-one obtained in Reference Example 1 was used, and 0.1 mL of tetrahydrofuran and 7.8 μL (52.3 μmol) of 1,8-diazabicyclo[5.4.0]undec-7-ene were used. Size exclusion chromatograms before and 24 hours after the start of the reaction are shown in FIG. 6. The peak top molecular weight (Mp) before the reaction was 15,300, whereas it was 12,800 24 hours after the start of the reaction, and the waveform on the high molecular weight side of the peak did not change before and after the reaction. That is, no significant decrease in molecular weight was observed as observed in Example 2. Therefore, it was confirmed that even in the presence of 1,8-diazabicyclo[5.4.0]undec-7-ene, main chain cleavage cannot be effectively induced unless an alcohol capable of bond exchange with the ester bond in the main chain is present in the side chain.
Claims
1. A repeating unit derived from a cyclic acrylic monomer represented by the following general formula (1), A repeating unit derived from an allyl alcohol monomer represented by the following general formula (2), A polymer comprising: 【Chemistry 1】 [In the formula, R 1 and R 2 Each independently represents a hydrogen atom, C 1 -C 6 Alkyl group, C 1 -C 6 It represents a haloalkyl group, a phenyl group, or a substituted phenyl group. X represents a sulfur atom, a sulfonyl group, or a disulfide group. Y is an oxygen atom, a carbon atom, a sulfur atom, or -NR 4 - indicates R 4 is a hydrogen atom, C 1 -C 6 Alkyl group, C 1 -C 6 It represents a haloalkyl group, a phenyl group, or a substituted phenyl group. Z is a divalent linking group that forms a 7- to 15-membered ring. 【Chemistry 2】 [In the formula, R 3 is C 1 -C 6 Alkyl group, C 1 -C 6 It represents a haloalkyl group, a phenyl group, or a substituted phenyl group. W represents a hydrogen atom or a trialkylsilyl group.
2. The polymer according to claim 1, characterized in that it has a structure represented by the following general formula (3): 【Chemistry 3】
3. 3. The polymer according to claim 1, wherein X is a sulfur atom and Y is an oxygen atom or a sulfur atom.
4. 3. The polymer according to claim 1, wherein W is a hydrogen atom.