Resin composition for forming etching mask pattern and method for producing etching mask pattern
A resin composition with a block copolymer and homopolymer combination addresses the challenge of maintaining vertical alignment in thick film etching mask patterns, enabling efficient phase-separated structures for precise etching applications.
Patent Information
- Application Number
- JP2024066934
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-22
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-14
AI Technical Summary
Existing technologies face challenges in forming fine etching mask patterns with vertical alignment and thick film thickness using block copolymers, as increasing film thickness makes it difficult to maintain phase-separated structures with vertical alignment.
A resin composition comprising a block copolymer with specific block structures and a homopolymer having a number average molecular weight of less than 3000, along with a method for applying and phase-separating layers to form an etching mask pattern, ensuring excellent vertical alignment even at high film thicknesses.
The solution enables the formation of etching mask patterns with excellent vertical alignment and phase-separated structures at film thicknesses of 25 nm or more, suitable for use as effective etching masks.
Smart Images

Figure 2024160688000043 
Figure 2024160688000044 
Figure 2024160688000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition for forming an etching mask pattern, and a method for producing an etching mask pattern. [Background technology]
[0002] In recent years, with the further miniaturization of large-scale integrated circuits (LSIs), there is a demand for technology to process more delicate structures. In response to such demands, technology is being developed to form finer patterns by utilizing a phase-separated structure formed by the self-organization of a block copolymer in which mutually incompatible blocks are bonded together (see, for example, Patent Document 1). In order to utilize the phase separation structure of a block copolymer, it is essential to form the self-organized nanostructure formed by microphase separation only in a specific region and to align it in a desired direction. To achieve this position control and orientation control, processes such as graphoepitaxy, which controls the phase separation pattern by a guide pattern, and chemical epitaxy, which controls the phase separation pattern by differences in the chemical state of the substrate, have been proposed (see, for example, Non-Patent Document 1).
[0003] Block copolymers form structures with regular periodic structures through phase separation. The "period of the structure" refers to the period of the phase structure observed when a phase-separated structure is formed, and refers to the sum of the lengths of each phase that is incompatible with each other. When the phase-separated structure forms a cylindrical structure perpendicular to the substrate surface, the period (L0) of the structure is the center-to-center distance (pitch) between two adjacent cylindrical structures.
[0004] It is known that the period of the structure (L0) is determined by the degree of polymerization N and the intrinsic polymerization properties such as the Flory-Huggins interaction parameter χ. In other words, the larger the product of χ and N, χ·N, the greater the mutual repulsion between different blocks in the block copolymer. Therefore, when χ·N>10.5 (hereinafter referred to as the "strength separation limit"), the repulsion between different types of blocks in the block copolymer is large, and phase separation is more likely to occur. At the strength separation limit, the period of the structure is approximately N 2 / 3 χ 1 / 6 Thus, the relationship of the following formula (1) is established. In other words, the period of the structure is proportional to the degree of polymerization N, which correlates with the molecular weight and the molecular weight ratio between different blocks.
[0005] L0 ∝ a N 2 / 3 χ 1 / 6 (1) [In the formula, L0 represents the period of the structure, a represents a parameter indicating the size of the monomer, N represents the degree of polymerization, and χ represents an interaction parameter, and the larger this value is, the higher the phase separation performance is.]
[0006] Therefore, the period (L0) of the structure can be adjusted by adjusting the composition and total molecular weight of the block copolymer. It is known that the periodic structure formed by block copolymers changes from cylinders (columnar), lamellae (plates), to spheres (spherical) depending on the volume ratio of the polymer components, and the period depends on the molecular weight. Therefore, in order to form a structure with a relatively large period (L0) by utilizing the phase-separated structure formed by the self-organization of block copolymers, a method of increasing the molecular weight of the block copolymer can be considered.
[0007] In addition, a method using a block copolymer having a larger interaction parameter (χ) than a block copolymer having a styrene block and a methyl methacrylate block, which is a general-purpose block copolymer, is also considered. For example, Patent Document 2 proposes a block copolymer in which a substituent is introduced into a part of the methyl methacrylate block. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2008-36491 A [Patent Document 2] Patent Publication No. 2022-020519 [Non-patent literature]
[0009] [Non-Patent Document 1] Proceedings of SPIE, Vol. 7637, No. 76370G-1 (2010). Summary of the Invention [Problem to be solved by the invention]
[0010] In order to form a fine pattern using a phase separation structure formed by self-organization of a block copolymer, it is preferable that the phase separation structure formed by the block copolymer has vertical alignment. In addition, in order to use the fine pattern as an etching mask pattern, it is preferable to vertically align the film with a relatively large thickness (for example, a thickness of 25 nm or more). However, the block copolymer described in Patent Document 1 is difficult to form a phase separation structure having vertical alignment when the film thickness is large.
[0011] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a resin composition for forming an etching mask pattern, which has excellent vertical alignment properties even at a thick film thickness, and a method for producing an etching mask pattern using the same. [Means for solving the problem]
[0012] That is, a first aspect of the present invention is a resin composition for forming an etching mask pattern, which contains a block copolymer having a first block and a second block, and a homopolymer having a number average molecular weight of less than 3000, wherein the first block is composed of a polymer composed of a repeating structure of a structural unit represented by the following general formula (b1), the second block is composed of a random copolymer composed of a structure in which a structural unit represented by the following general formula (b2m) and a structural unit represented by the following general formula (b2g) are arranged in a disordered manner, the ratio of the volume of the first block to the total volume of the first block and the second block is 20 to 80 volume%, and the homopolymer is a resin composition for forming an etching mask pattern, which contains a polymer composed of a repeating structure of a structural unit represented by the following general formula (b1).
[0013] [ka] [In formula (b1), R 1 is an alkyl group. b1 is a hydrogen atom or a methyl group. n is an integer of 0 to 5. When n is an integer of 2 or more, multiple R 1 may be the same or different. In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear or branched alkylene group having 1 to 10 carbon atoms which may have a hydroxy group. In formula (b2g) and formula (b2m), R b2is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 may be the same or different. x represents a molar ratio and is greater than 0 and less than 1.
[0014] A second aspect of the present invention is a method for producing an etching mask pattern, comprising the steps of: applying the resin composition for forming an etching mask pattern according to the first aspect onto a support to form a layer containing a block copolymer; and phase-separating the layer containing the block copolymer. Effect of the Invention
[0015] According to the present invention, it is possible to provide a resin composition for forming an etching mask pattern, which has excellent vertical alignment even in a thick film, and a method for producing an etching mask pattern using the same. [Brief description of the drawings]
[0016] [Figure 1] 1A to 1C are schematic process diagrams illustrating an embodiment of a method for producing an etching mask pattern. [Diagram 2] FIG. 13 is a diagram illustrating an embodiment of an optional step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] In this specification and claims, the term "aliphatic" is a relative concept to aromaticity and is defined as meaning a group, compound, etc. that does not have aromaticity. Unless otherwise specified, the term "alkyl group" includes linear, branched and cyclic monovalent saturated hydrocarbon groups. The same applies to the alkyl group in an alkoxy group. Unless otherwise specified, the term "alkylene group" includes linear, branched and cyclic divalent saturated hydrocarbon groups. The term "halogenated alkyl group" refers to an alkyl group in which some or all of the hydrogen atoms have been substituted with halogen atoms, and examples of the halogen atoms include fluorine, chlorine, bromine and iodine atoms. The term "fluorinated alkyl group" or "fluorinated alkylene group" refers to an alkyl group or alkylene group in which some or all of the hydrogen atoms have been substituted with fluorine atoms. The term "structural unit" refers to a monomer unit that constitutes a polymeric compound (resin, polymer, copolymer). The phrase "optionally has a substituent" includes both the case where a hydrogen atom (-H) is replaced with a monovalent group and the case where a methylene group (-CH2-) is replaced with a divalent group. The term "exposure" is intended to include any concept including irradiation with radiation. Unless otherwise specified, the "α-position (carbon atom at the α-position)" refers to the carbon atom to which the side chain of the block copolymer is bonded. The "α-position carbon atom" of a methyl methacrylate unit refers to the carbon atom to which the carbonyl group of methacrylic acid is bonded. The "α-position carbon atom" of a styrene unit refers to the carbon atom to which a benzene ring is bonded. "Number average molecular weight" (Mn) is the number average molecular weight measured by size exclusion chromatography in terms of standard polystyrene unless otherwise specified. "Weight average molecular weight" (Mw) is the weight average molecular weight measured by size exclusion chromatography in terms of standard polystyrene unless otherwise specified. The Mn or Mw value is expressed in units (g mol - ) indicates the molar mass. In the present specification and claims, some structures represented by chemical formulas may have asymmetric carbons and may have enantiomers or diastereomers, in which case a single formula represents all the isomers. These isomers may be used alone or as a mixture.
[0018] (Resin composition for forming etching mask pattern) The resin composition for forming an etching mask pattern of the present embodiment contains a block copolymer having a first block and a second block, and a homopolymer having a number average molecular weight of less than 3000. The first block is composed of a polymer having a repeating structure of a constitutional unit represented by the following general formula (b1). The second block is composed of a random copolymer having a structure in which a constitutional unit represented by the following general formula (b2m) and a constitutional unit represented by the following general formula (b2g) are randomly arranged. The ratio of the volume of the first block to the total volume of the first block and the second block is 20 to 80 volume %. The homopolymer contains a polymer having a repeating structure of a constitutional unit represented by the following general formula (b1).
[0019] [ka] [In formula (b1), R 1 is an alkyl group. b1 is a hydrogen atom or a methyl group. n is an integer of 0 to 5. When n is an integer of 2 or more, multiple R 1 may be the same or different. In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear or branched alkylene group having 1 to 10 carbon atoms which may have a hydroxy group. In formula (b2g) and formula (b2m), R b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 may be the same or different. x represents a molar ratio and is greater than 0 and less than 1.
[0020] <Block copolymer (BCP) component> A block copolymer is a polymer in which multiple types of blocks (partial constituent components in which the same type of constituent units are repeatedly bonded) are bonded together. The blocks constituting a block copolymer may be of two types, or three or more types. The block copolymer in this embodiment (hereinafter also referred to as "(BCP) component") has a first block and a second block.
[0021] <First Block> The first block is composed of a polymer having a repeating structure of a structural unit represented by the following general formula (b1) (hereinafter, also referred to as structural unit (b1)).
[0022] [ka] [In the formula, R 1 is an alkyl group. b1 is a hydrogen atom or a methyl group. n is an integer of 0 to 5. When n is an integer of 2 or more, multiple R 1 may be the same or different.
[0023] In the formula (b1), R 1 R is an alkyl group. The alkyl group preferably has 1 to 5 carbon atoms, more preferably has 1 to 4 carbon atoms, even more preferably has 1 to 3 carbon atoms, and is further preferably an ethyl group or a methyl group. 1 is particularly preferably a methyl group.
[0024] In the formula (b1), R b1 is a hydrogen atom or a methyl group. In the formula (b1), n is preferably an integer of 0 to 3, more preferably an integer of 0 to 2, and further preferably 0 or 1.
[0025] <Second Block> The second block is composed of a random copolymer having a structure in which a structural unit represented by the following general formula (b2m) (hereinafter also referred to as structural unit (b2m)) and a structural unit represented by the following general formula (b2g) (hereinafter also referred to as structural unit (b2g)) are arranged in a disordered manner.
[0026] [ka] [In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear or branched alkylene group having 1 to 10 carbon atoms which may have a hydroxy group. In formula (b2g) and formula (b2m), R b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 may be the same or different. x represents a molar ratio and is greater than 0 and less than 1.
[0027] (B2M) The structural unit (b2m) is a structural unit represented by the above general formula (b2m). In the above formula (b2m), R b2 R is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 The alkyl group having 1 to 5 carbon atoms is preferably a linear or branched alkyl group having 1 to 5 carbon atoms, and specific examples thereof include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, a pentyl group, an isopentyl group, and a neopentyl group. The halogenated alkyl group having 1 to 5 carbon atoms is a group in which some or all of the hydrogen atoms of the alkyl group having 1 to 5 carbon atoms are substituted with halogen atoms. As the halogen atom, a fluorine atom is particularly preferable. R b2is preferably a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a fluorinated alkyl group having 1 to 5 carbon atoms, and from the viewpoint of industrial availability, more preferably a hydrogen atom or a methyl group, and even more preferably a methyl group.
[0028] (B2G) The structural unit (b2g) is a structural unit represented by the above general formula (b2g).
[0029] In the above formula (b2g), R b2 R is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 is R in the above formula (b2m). b2 is the same as:
[0030] In the above formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. The alkyl group may be linear, branched or may include a ring structure. The alkyl group is preferably a linear, branched or cyclic alkyl group, more preferably a linear or cyclic alkyl group. When the alkyl group is linear, the number of carbon atoms may be 1 or more, preferably 2 or more. The upper limit of the number of carbon atoms of the linear alkyl group is not particularly limited, but from the viewpoint of phase separation performance, the number of carbon atoms is preferably 15 or less, more preferably 10 or less, even more preferably 8 or less, and even more preferably 6 or less. When the alkyl group is branched, the number of carbon atoms may be 3 or more. The upper limit of the number of carbon atoms of the branched alkyl group is not particularly limited, but from the viewpoint of phase separation performance, the number of carbon atoms is preferably 15 or less, more preferably 10 or less, even more preferably 8 or less, and even more preferably 6 or less. When the alkyl group contains a ring structure, R 2may be a cycloalkyl group, a straight-chain or branched alkyl group having a cycloalkylene group interposed therein, or a straight-chain or branched alkyl group having a cycloalkyl group bonded to an end thereof. The cycloalkyl group and cycloalkylene group may be a monocyclic group or a polycyclic group, but a monocyclic group is preferred. When the cycloalkyl group or cycloalkylene group is a monocyclic group, a 3- to 8-membered ring is preferred, a 3- to 6-membered ring is more preferred, and a 5- to 6-membered ring is even more preferred. When the alkyl group contains a ring structure, R 2 may have 3 or more carbon atoms. The upper limit of the number of carbon atoms of the alkyl group containing a ring structure is not particularly limited, but from the viewpoint of phase separation performance, the number of carbon atoms is preferably 15 or less, more preferably 10 or less, even more preferably 8 or less, and still more preferably 6 or less. R 2 The alkyl group in the formula (I) preferably has 2 to 15 carbon atoms, more preferably has 2 to 10 carbon atoms, further preferably has 2 to 8 carbon atoms, and further more preferably has 2 to 6 carbon atoms. R 2 The alkyl group is preferably a linear alkyl group or a cycloalkyl group having 2 to 6 carbon atoms.
[0031] R 2 The alkyl group of R may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group, or a phosphoric acid group. 2 When the alkyl group has a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group, or a phosphoric acid group, the fluorine atom, the carboxy group, the amino group, the cyano group, the hydroxy group, or the phosphoric acid group may be a substituent that replaces a hydrogen atom of the alkyl group. The number of hydrogen atoms replaced by the group is not particularly limited, but is preferably 1 to 3. R 2 When the alkyl group has a silicon atom, the silicon atom may be a substituent that replaces a methylene group (-CH2-) in the alkyl group. The number of methylene groups substituted with silicon atoms is not particularly limited, but is preferably 1. R 2is preferably an alkyl group which may be substituted with an alkylsilyl group, a fluoromethyl group, a carboxy group, an amino group, a hydroxy group, a cyano group, or a phosphate group. The alkyl group in the alkylsilyl group preferably has 1 to 3 carbon atoms, more preferably has 1 or 2 carbon atoms. The alkylsilyl group is preferably a trialkylsilyl group, more preferably a triethylsilyl group or a trimethylsilyl group, and even more preferably a trimethylsilyl group. The fluoromethyl group is preferably a trifluoromethyl group.
[0032] R 2 Preferred examples are shown below, but are not limited to these: In the following formula, * represents a bond bonded to the sulfur atom (S) in the above formula (b2g).
[0033] [ka] [In the formula, Y 2 is a single bond or a linear or branched alkylene group having 1 to 15 carbon atoms. p is an integer of 1 to 10.
[0034] In the above formulas (r2-1) to (r2-7), Y 2 is a single bond or a linear or branched alkylene group having 1 to 15 carbon atoms. When the alkylene group is linear, it more preferably has 1 to 10 carbon atoms, even more preferably has 1 to 8 carbon atoms, and particularly preferably has 1 to 5 carbon atoms. When the alkylene group is branched, it more preferably has 2 to 10 carbon atoms, even more preferably has 2 to 8 carbon atoms, and particularly preferably has 2 to 6 carbon atoms. Y 2 The alkylene group is preferably a linear alkylene group having 1 to 5 carbon atoms or a branched alkylene group having 2 to 6 carbon atoms. R 2 is a group represented by any one of the formulas (r2-1) to (r2-8), Y 2 R is preferably a linear or branched alkylene group having 1 to 15 carbon atoms, more preferably a linear alkylene group having 1 to 5 carbon atoms or a branched alkylene group having 2 to 6 carbon atoms.2 is a group represented by the formula (r2-9), Y 2 is preferably a single bond or a linear alkylene group having 1 to 5 carbon atoms, and more preferably a single bond. In the above formula (r2-9), p is preferably an integer of 1 to 6, more preferably an integer of 1 to 4, and even more preferably 3 or 4.
[0035] R 2 Specific examples of are shown below, but are not limited to these. In the following formula, * represents a bond bonded to the sulfur atom (S) in the above formula (b2g).
[0036] [ka] [In the formula, q is an integer of 1 to 15. q' is an integer of 0 to 15. p is an integer of 1 to 10. Each p' is independently an integer of 0 to 10.]
[0037] In the above formula, q is preferably an integer of 1 to 10, more preferably an integer of 1 to 8, further preferably an integer of 1 to 6, and particularly preferably an integer of 1 to 5. In the formulae (r2-18) and (r2-19), q′ is preferably an integer of 0 to 10, more preferably an integer of 0 to 8, even more preferably an integer of 0 to 6, and particularly preferably an integer of 0 to 5. In the above formula (r2-18), p is preferably an integer of 1 to 6, more preferably an integer of 1 to 4, and even more preferably 3 or 4. In the above formula (r2-19), p' is preferably an integer of 1 to 8, more preferably an integer of 1 to 6, even more preferably an integer of 1 to 3, and particularly preferably 1 or 2.
[0038] In the above formula (b2g), R 3is a linear or branched alkylene group having 1 to 10 carbon atoms, which may have a hydroxyl group. When the alkylene group is linear, the number of carbon atoms may be 1 or more, but preferably 3 or more. The upper limit of the number of carbon atoms of the linear alkylene group is preferably 8 or less, more preferably 5 or less, and even more preferably 4 or less, from the viewpoint of phase separation performance. The number of carbon atoms of the linear alkylene group is particularly preferably 3. When the alkylene group is branched, the number of carbon atoms may be 3 or more, but preferably 4 or more. The upper limit of the number of carbon atoms of the branched alkylene group is preferably 8 or less, more preferably 5 or less, from the viewpoint of phase separation performance. The number of carbon atoms of the alkylene group is preferably 3 to 10, more preferably 3 to 8, even more preferably 3 to 5, even more preferably 3 to 4, and especially preferably 3. R 3 The alkylene group is preferably a linear alkylene group having 3 carbon atoms.
[0039] R 3 The alkylene group may have a hydroxy group. The hydroxy group may be a substituent that replaces a hydrogen atom of the alkylene group. The number of hydrogen atoms replaced by the hydroxy group is not particularly limited, but is preferably 1 to 3, more preferably 1 or 2, and even more preferably 1.
[0040] The structural unit (b2g) is preferably a structural unit represented by general formula (b2g-1) shown below.
[0041] [ka] [In the formula, R 4 is a hydrogen atom or a hydroxyl group. k1 and k2 each independently represent an integer of 1 to 5. R b2 and R 2 is R in the above formula (b2g). b2 and R 2 is the same as:
[0042] In the above formula (b2g-1), R b2 and R 2 is R in the above formula (b2g). b2 and R 2 Same as R 2 is preferably one represented by the above formulas (r2-1) to (r2-9), and more preferably one represented by (r2-10) to (r2-19).
[0043] In the above formula (b2g-1), R 4 is a hydrogen atom or a hydroxy group.
[0044] In the formula (b2g-1), k1 and k2 each independently represent an integer of 1 to 5. k1 and k2 each preferably represent an integer of 1 to 3, more preferably 1 or 2, and further preferably 1.
[0045] Specific examples of the structural unit (b2g) are shown below, but are not limited to these. In the following formula, R represents a methyl group or a hydrogen atom, and a methyl group is preferable.
[0046] [ka]
[0047] [ka]
[0048] [ka]
[0049] [ka]
[0050] The second block is composed of a random copolymer having a structure in which the structural units (b2g) and (b2m) are randomly arranged. In the formulas (b2g) and (b2m), x and 1-x represent the molar ratios of the structural units (b2g) and (b2m). x is greater than 0 and less than 1. x can be appropriately determined depending on the type of the desired phase-separated structure. When a phase-separated structure having a lamellar structure is formed, x is preferably 0.01 to 0.3, and more preferably 0.1 to 0.3. When a phase-separated structure having a cylindrical structure is formed, x is preferably 0.01 to 0.1, and more preferably 0.01 or more and less than 0.1.
[0051] In the (BCP) component, the volume ratio of the first block to the total volume of the first block and the second block is 20 to 80% by volume. The volume ratio of the first block can be appropriately determined depending on the type of the desired phase-separated structure. When a phase-separated structure having a lamellar structure is formed, the volume ratio of the first block is preferably 35 to 65% by volume. When a phase-separated structure having a cylindrical structure is formed, the volume ratio of the first block is preferably 20 to 35% by volume or 65 to 80% by volume.
[0052] The ratio of the volume of the first block to the total volume of the first block and the second block in the (BCP) component can be calculated as follows. 1 From the results of H NMR analysis, the mole percentages of the first block and the second block in the (BCP) component are calculated, and furthermore, the mass percentage of each block is calculated from the molecular weight of each block. The mass percentage of each block is divided by the density of each block to calculate the volume ratio of each block, and the volume percentage of the first block in the (BCP) component is calculated from the volume ratio. The density of each block can be estimated by the atomic group contribution method (Fedors, RF Polym. Eng. Sci. 1974, 14, 147-154.). When the first block is a polystyrene block (PS), the density of PS is 1.05 gm -3When the second block is a polystyrene block (PS), the density of PS is 1.05 gm -3 When the second block has a structural unit derived from methyl methacrylate, the density of the structure composed of the structural units is 1.18 gcm -3 When the second block has a structural unit derived from 2-hydroxy-3-(2,2,2-trifluoroethylsulfanyl)propyl methacrylate, the density of the structure composed of the structural units is 1.43 gcm -3 The density of each block can be determined by using the density described in the literature (Polymer Handbook, 4th ed.; Wiley: New York, 2004).
[0053] The (BCP) component may have other blocks in addition to the first block and the second block. In a preferred embodiment, the (BCP) component is a block copolymer composed of a first block and a second block.
[0054] The number average molecular weight (Mn) of the (BCP) component (based on polystyrene conversion by size exclusion chromatography) is not particularly limited, but is preferably 5,000 to 100,000, more preferably 6,000 to 7,000, further preferably 8,000 to 40,000, and particularly preferably 10,000 to 40,000. The molecular weight dispersity (Mw / Mn) of each block constituting the (BCP) component is preferably from 1.0 to 1.5, more preferably from 1.0 to 1.4, and even more preferably from 1.0 to 1.3.
[0055] <Production method of block copolymer (BCP) component> The (BCP) component can be produced, for example, by a production method having the steps shown below. Step (p1): A step of obtaining a block copolymer having a first block and a precursor of a second block (hereinafter, also referred to as a "BCP precursor"). Step (p2): Adding R to the precursor of the second block in the BCP precursor 2 Compounds represented by -SH (R 2 is R in the above formula (b2g). 2 ) to obtain a block copolymer (component (BCP)) containing a first block and a second block.
[0056] Process (p1): The precursor of the second block is a random copolymer having a structure in which the structural unit (b2gp), which is a precursor of the structural unit (b2g), and the structural unit (b2m) are randomly arranged. The structural unit (b2gp) is a structural unit containing an epoxy group or a vinyl group, and examples of the structural unit represented by the following general formula (b2gp) are:
[0057] [ka] [In the formula, Rp 2 represents an epoxy group or a vinyl group. 2 R represents a linear or branched alkylene group having 1 to 8 carbon atoms. b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms.]
[0058] The BCP precursor can be obtained, for example, by carrying out a polymerization reaction of a monomer (e.g., styrene or a derivative thereof, hereinafter also referred to as monomer (b1)) that derives the structural unit (b1), and then adding a monomer (e.g., glycidyl methacrylate, allyl methacrylate, etc., hereinafter also referred to as monomer (b2gp)) that derives the structural unit (b2m) to the polymerization reaction liquid and further carrying out a polymerization reaction. Alternatively, the BCP precursor can be obtained by carrying out a polymerization reaction using a mixture of monomer (b2gp) and monomer (b2m), and then adding monomer (b1) to the polymerization reaction liquid and further carrying out a polymerization reaction. The polymerization reaction is preferably living polymerization because it is narrowly dispersed and easy to synthesize. Preferred living polymerization methods include living anionic polymerization and living radical polymerization, and living anionic polymerization is particularly preferred because it can achieve a more narrow dispersion.
[0059] Process (p2): R 2 A compound represented by the formula (hereinafter referred to as "compound (R 2 The compound (b2gp) reacts with the epoxy group or vinyl group of the structural unit (b2gp) to convert the structural unit (b2gp) into the structural unit (b2g). When the building block (b2gp) contains an epoxy group, the BCP precursor and the compound (R 2 The reaction of R2gp with the compound (R-SH) can be carried out in an organic solvent such as tetrahydrofuran in the presence of a catalyst such as lithium hydroxide. The reaction temperature can be set, for example, at 20 to 60°C, preferably 30 to 50°C, and more preferably 35 to 45°C. The reaction time can be appropriately set depending on the amount of BCP precursor used, and may be a time sufficient for all of the structural units (b2gp) in the precursor of the second block to be converted to structural units (b2g). The reaction time can be set, for example, for 1 to 10 hours. When the structural unit (b2gp) contains a vinyl group, the reaction of the BCP precursor with the compound (R2gp with 2The reaction of -SH) can be carried out by a thiol-ene reaction. The thiol-ene reaction can be carried out in an organic solvent such as tetrahydrofuran in the presence of a catalyst such as azobisisobutyronitrile (AIBN). The reaction temperature can be, for example, 60 to 90°C, preferably 70 to 90°C, and more preferably 75 to 85°C. The reaction time can be appropriately set depending on the amount of the BCP precursor used, and may be a time sufficient for all of the structural units (b2gp) in the precursor of the second block to be converted to structural units (b2g). The reaction time can be, for example, 1 to 10 hours.
[0060] [ka] [In the formula, R 1 , R b1 and n is R in the formula (b1). 1 , R b1 and n, respectively. 2 and R 3 is R in the above formula (b2g). 2 and R 3 is the same as R b2 and x represents R in the formula (b2g) and the formula (b2m). b2 and x. Yp 2 Rp represents a linear or branched alkyl group having 1 to 8 carbon atoms. 2 represents an epoxy group or a vinyl group.
[0061] <Homopolymer: (H) component> The homopolymer is a homopolymer (hereinafter also referred to as "component (H)") having a number average molecular weight of less than 3000. The component (H) includes a polymer consisting of a repeating structure of the structural unit (b1) represented by the general formula (b1) above.
[0062] (Polymer consisting of repeating units of structural unit (b1): component (H1)) The component (H) contains a polymer (hereinafter also referred to as "component (H1)") consisting of a repeating structure of the structural unit (b1). The explanation of the structural unit (b1) contained in the component (H1) is the same as the explanation of the structural unit (b1) contained in the first block of the component (BCP) above. The structural unit (b1) in the (H1) component may be the same as or different from the structural unit (b1) in the first block of the (BCP) component, but is preferably the same. For example, when the first block of the (BCP) component is a polystyrene block, the (H1) component is preferably polystyrene.
[0063] The number average molecular weight (Mn) of the (H1) component (based on polystyrene conversion by size exclusion chromatography) may be less than 3,000. When the (H1) component has an Mn of less than 3,000, the (H1) component is easily dispersed uniformly in the layer containing the block copolymer, and the vertical alignment property is improved at a high film thickness (for example, a film thickness of 25 nm or more). The upper limit of the (H1) component's Mn is, for example, 2,900 or less, 2,800 or less, 2,700 or less, 2,600 or less, 2,500 or less, 2,400 or less, 2,300 or less, 2,200 or less, 2,100 or less, or 2,000 or less. The lower limit of the (H1) component's Mn is, for example, 1,000 or more, or 1,200 or more. The Mn of the component (H1) is, for example, in the range of 1,000 to 2,900, preferably 1,000 to 2,500, and more preferably 1,200 to 2,000. When the Mn content of the component (H1) is within the above preferred range, a phase-separated structure with excellent vertical alignment properties is easily formed.
[0064] The content of the (H1) component in the resin composition for forming an etching mask pattern of this embodiment is 1 part by mass or more, preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, relative to 100 parts by mass of the (BCP) component. The upper limit of the content of the (H1) component is 100 parts by mass or less, preferably 70 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 30 parts by mass or less, relative to 100 parts by mass of the (BCP) component. The content of the (H1) component is in the range of 1 to 100 parts by mass, preferably 10 to 70 parts by mass, more preferably 15 to 50 parts by mass, and even more preferably 15 to 30 parts by mass, relative to 100 parts by mass of the (BCP) component. When the content of the component (H1) is within the above preferred range, a phase-separated structure that is excellent in vertical alignment property is easily formed.
[0065] The component (H1) may be used alone or in combination of two or more types. When the component (H) contains two or more types of the component (H1), the content of the component (H1) means the total content of the two or more types of the component (H1).
[0066] (other homopolymers) In addition to the component (H1), the component (H) may contain another homopolymer. Examples of the other homopolymer include a polymer having a repeating structure of the structural unit (b2m) represented by the general formula (b2m) (hereinafter, also referred to as "component (H2)").
[0067] <Polymer consisting of repeating structural units (b2m): component (H2)> The explanation for the structural unit (b2m) contained in the (H2) component is the same as the explanation for the structural unit (b2m) contained in the second block of the (BCP) component above. The structural unit (b2m) of the component (H2) may be the same as or different from the structural unit (b2m) of the second block of the component (BCP), but is preferably the same. For example, when the second block of the component (BCP) is a polymethyl methacrylate block, the component (H1) is preferably polymethyl methacrylate.
[0068] The number average molecular weight (Mn) of the (H2) component (based on polystyrene conversion by size exclusion chromatography) may be less than 3,000. When the (H2) component has an Mn of less than 3,000, the (H2) component is easily dispersed uniformly in the layer containing the block copolymer, and the vertical alignment property is improved at a high film thickness (for example, a film thickness of 25 nm or more). The upper limit of the Mn of the (H2) component is, for example, 2,900 or less, 2,800 or less, 2,700 or less, 2,600 or less, 2,500 or less, 2,400 or less, 2,300 or less, 2,200 or less, 2,100 or less, or 2,000 or less. The lower limit of the Mn of the (H2) component is, for example, 1,000 or more, or 1,200 or more. The Mn of the component (H2) is, for example, in the range of 1,000 to 2,900, preferably 1,000 to 2,500, and more preferably 1,200 to 2,000. When the Mn content of the component (H2) is within the above preferred range, a phase-separated structure with excellent vertical alignment is easily formed.
[0069] When the (H) component contains the (H2) component, the content of (H2) in the composition for forming an etching mask pattern of this embodiment may be 90 parts by mass or less, preferably 70 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 30 parts by mass or less, relative to 100 parts by mass of the (BCP) component. When the (H) component contains the (H2) component, the content of the (H2) component may be 1 part by mass or more, 5 parts by mass or more, 10 parts by mass or more, or 15 parts by mass or more, relative to 100 parts by mass of the (BCP) component. The content of the (H2) component may be in the range of 0 to 90 parts by mass, preferably 0 to 70 parts by mass, more preferably 0 to 50 parts by mass, even more preferably 0 to 30 parts by mass, and even more preferably 0 to 25 parts by mass, relative to 100 parts by mass of the (BCP) component. When the content of the component (H2) is within the above preferred range, a phase-separated structure with excellent vertical alignment properties is easily formed.
[0070] The component (H2) may be used alone or in combination of two or more types. When the (H) component contains two or more types of (H2) components, the content of the (H2) component means the total content of the two or more types of (H2) components.
[0071] When the (H) component contains the (H2) component, the content of the (H2) component is preferably 100 parts by mass or less per 100 parts by mass of the (H1) component. The content of the (H2) component may be 90 parts by mass or less, 80 parts by mass or less, 70 parts by mass or less, 60 parts by mass or less, 50 parts by mass or less, or 40 parts by mass or less per 100 parts by mass of the (H1) component.
[0072] The content of the (H) component in the resin composition for forming an etching mask pattern of this embodiment is preferably 100 parts by mass or less relative to 100 parts by mass of the (BCP) component. When the (H) component contains two or more homopolymers, the content of the (H) component means the total content of the two or more homopolymers. The content of the (H) component is 5 parts by mass or more relative to 100 parts by mass of the (BCP) component, preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 30 parts by mass or more. The upper limit of the content of the (H) component is 100 parts by mass or less relative to 100 parts by mass of the (BCP) component, preferably 70 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less. The content of the (H) component is in the range of 5 to 100 parts by mass relative to 100 parts by mass of the (BCP) component, preferably 10 to 70 parts by mass, more preferably 20 to 60 parts by mass, and even more preferably 30 to 50 parts by mass. When the content of the component (H) is within the above preferred range, a phase-separated structure with excellent vertical alignment properties is easily formed.
[0073] The resin composition for forming an etching mask pattern of this embodiment may or may not contain a homopolymer having an Mn of 3,000 or more, but preferably does not contain one. By not containing a homopolymer having an Mn of 3,000 or more, the resin composition for forming an etching mask pattern of this embodiment is more likely to form a phase-separated structure with excellent vertical alignment.
[0074] <Organic solvent components> The resin composition for forming an etching mask pattern of the present embodiment can be prepared by dissolving the above-mentioned components (BCP) and (H) in an organic solvent component. The organic solvent component may be any solvent capable of dissolving each component used to form a homogeneous solution, and any solvent known in the art as a solvent for film compositions mainly composed of resins may be used.
[0075] Examples of the organic solvent component include lactones such as γ-butyrolactone; ketones such as acetone, methyl ethyl ketone, cyclohexanone, methyl-n-pentyl ketone, methyl isopentyl ketone, and 2-heptanone; polyhydric alcohols such as ethylene glycol, diethylene glycol, propylene glycol, and dipropylene glycol; compounds having an ester bond such as ethylene glycol monoacetate, diethylene glycol monoacetate, propylene glycol monoacetate, and dipropylene glycol monoacetate; and ether bonds such as monoalkyl ethers, monomethyl ether, monoethyl ether, monopropyl ether, and monobutyl ether of the polyhydric alcohols or the compounds having an ester bond, or monophenyl ether. derivatives of polyhydric alcohols such as compounds having a bond [among which, propylene glycol monomethyl ether acetate (PGMEA) and propylene glycol monomethyl ether (PGME) are preferred]; cyclic ethers such as dioxane, esters such as methyl lactate, ethyl lactate (EL), methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, and ethyl ethoxypropionate; and aromatic organic solvents such as anisole, ethyl benzyl ether, cresyl methyl ether, diphenyl ether, dibenzyl ether, phenetole, butyl phenyl ether, ethylbenzene, diethylbenzene, pentylbenzene, isopropylbenzene, toluene, xylene, cymene, and mesitylene. The organic solvent component may be used alone or in a mixture of two or more kinds. Among them, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), cyclohexanone, and EL are preferred.
[0076] A mixed solvent obtained by mixing PGMEA and a polar solvent is also preferred. The mixing ratio (mass ratio) may be appropriately determined in consideration of the compatibility between PGMEA and the polar solvent, and is preferably within a range of 1:9 to 9:1, and more preferably 2:8 to 8:2. For example, when EL is blended as the polar solvent, the mass ratio of PGMEA:EL is preferably 1:9 to 9:1, more preferably 2:8 to 8:2. When PGME is blended as the polar solvent, the mass ratio of PGMEA:PGME is preferably 1:9 to 9:1, more preferably 2:8 to 8:2, and even more preferably 3:7 to 7:3. When PGME and cyclohexanone are blended as the polar solvent, the mass ratio of PGMEA:(PGME+cyclohexanone) is preferably 1:9 to 9:1, more preferably 2:8 to 8:2, and even more preferably 3:7 to 7:3.
[0077] As the organic solvent component in the resin composition for forming an etching mask pattern, a mixed solvent of PGMEA or EL, or a mixed solvent of the PGMEA and a polar solvent, and γ-butyrolactone is also preferred. In this case, the mass ratio of the former to the latter is preferably 70:30 to 95:5. The organic solvent component contained in the resin composition for forming an etching mask pattern is not particularly limited, and is appropriately set at a coatable concentration according to the coating film thickness, and is generally used so that the solid content concentration is within the range of 0.2 to 70 mass %, preferably 0.2 to 50 mass %.
[0078] <Optional ingredients> In addition to the above-mentioned component (BCP), component (H) and organic solvent component, the resin composition for forming an etching mask pattern may further contain, as desired, compatible additives such as additional resins for improving the performance of the layer, surfactants for improving coatability, dissolution inhibitors, plasticizers, stabilizers, colorants, antihalation agents, dyes, sensitizers, base amplifiers, basic compounds and the like.
[0079] According to the resin composition for forming an etching mask pattern of the present embodiment described above, by containing the component (H) in addition to the component (BCP), a phase-separated structure with good vertical alignment can be formed even with a high film thickness (for example, a film thickness of 25 nm or more). Therefore, a vertically aligned phase-separated structure can be formed with a high film thickness (for example, a film thickness of 25 nm or more, preferably 30 nm or more), and the phase-separated structure can be used as an etching mask pattern.
[0080] The (BCP) component can increase the value of χ compared to a block copolymer (PS-b-PMMA) having a styrene block and a methyl methacrylate block, because the second block has the structural unit (b2g). This allows a fine phase-separated structure with a shorter period to be formed using a block copolymer with a lower degree of polymerization (N). However, when the value of χ is high, the vertical alignment tends to decrease. In particular, at a film thickness applicable to an etching mask pattern (for example, a film thickness of 25 nm or more, preferably 30 nm or more), the (BCP) component is less likely to form a vertically aligned phase-separated structure. The resin composition for forming an etching mask pattern of the present embodiment contains the component (H) in addition to the component (BCP), thereby improving the vertical alignment property and enabling the formation of a vertically oriented phase-separated structure with a film thickness applicable to an etching mask pattern.
[0081] (Method of manufacturing an etching mask pattern) The method for producing an etching mask pattern of the present embodiment includes a step of applying the resin composition for forming an etching mask pattern of the above-described embodiment onto a support to form a layer containing a block copolymer (hereinafter referred to as "step (i)"), and a step of phase-separating the layer containing the block copolymer (hereinafter referred to as "step (ii)"). Hereinafter, such a method for producing an etching mask pattern will be specifically described with reference to Fig. 1. However, the present invention is not limited to this.
[0082] FIG. 1 shows an embodiment of a method for producing an etching mask pattern. In the embodiment shown in FIG. 1, first, a primer is applied onto a support 1 to form a primer layer 2 (FIG. 1(I)). Next, the resin composition for forming an etching mask pattern of the above-mentioned embodiment is applied onto the undercoat agent layer 2 to form a layer containing a block copolymer (BCP layer) 3 (FIG. 1(II); this is step (i)). Next, an annealing treatment is performed by heating, so that the BCP layer 3 is separated into a phase 3a and a phase 3b (FIG. 1(III); step (ii)). As a result, a structure 3' containing a phase-separated structure is produced on the support 1 on which the undercoat agent layer 2 has been formed. The structure 3' containing a phase-separated structure can be used to produce an etching mask pattern.
[0083] [Step (i)] In the step (i), a resin composition for forming an etching mask pattern is applied onto a support 1 to form a BCP layer 3 . In the embodiment shown in FIG. 1, first, a base agent is applied onto a support 1 to form a base agent layer 2 . By providing the undercoat agent layer 2 on the support 1, a balance of hydrophilicity and hydrophobicity between the surface of the support 1 and the layer (BCP layer) 3 containing a block copolymer can be achieved. That is, when the primer layer 2 contains a resin component having the structural unit (b1) constituting the first block, the adhesion between the phase of the BCP layer 3 consisting of the first block and the support 1 is enhanced. When the primer layer 2 contains a resin component having the structural unit (b2) constituting the second block, the adhesion between the phase of the BCP layer 3 consisting of the second block and the support 1 is enhanced. Accordingly, due to phase separation of the BCP layer 3, a phase-separated structure oriented in a direction perpendicular to the surface of the support 1 is easily formed.
[0084] Primer: As the undercoat agent, a resin composition can be used. The resin composition for the undercoat agent can be appropriately selected from among conventionally known resin compositions used for thin film formation, depending on the type of block constituting the (BCP) component. The resin composition for the undercoat agent may be, for example, a thermally polymerizable resin composition, or may be a photosensitive resin composition such as a positive resist composition or a negative resist composition. In addition, a compound may be used as a surface treatment agent, and a non-polymerizable film formed by applying the compound may be used as the undercoat agent layer. For example, a siloxane-based organic monomolecular film formed using phenethyltrichlorosilane, octadecyltrichlorosilane, hexamethyldisilazane, or the like as a surface treatment agent may also be suitably used as the undercoat agent layer.
[0085] Examples of such resin compositions include a resin composition containing a resin having both the structural unit (b1) constituting the first block and the structural unit (b2m) constituting the second block, and a resin composition containing a resin having both structural units that have high affinity with each of the blocks constituting the (BCP) component. As the resin composition for the primer, it is preferable to use, for example, a composition containing a resin having both styrene and methyl methacrylate as constituent units, or a compound or composition containing both a moiety having high affinity for styrene, such as an aromatic ring, and a moiety having high affinity for methyl methacrylate (such as a highly polar functional group). Examples of resins having both styrene and methyl methacrylate as structural units include random copolymers of styrene and methyl methacrylate, alternating polymers of styrene and methyl methacrylate (monomers copolymerized alternately), random copolymers of styrene, methyl methacrylate, and (hydroxyethyl) methacrylate, etc. From the viewpoint of forming a vertically oriented phase separation structure in the BCP layer, the proportion of styrene structural units in the resin is preferably 20 to 90 mol%, more preferably 30 to 85 mol%, relative to the total (100 mol%) of all structural units constituting the resin. In addition, as a composition containing both a site having a high affinity for styrene and a site having a high affinity for methyl methacrylate, for example, a composition containing a resin obtained by polymerizing at least a monomer having an aromatic ring and a monomer having a highly polar functional group as a monomer can be mentioned. Examples of monomers having an aromatic ring include monomers having aryl groups in which one hydrogen atom has been removed from an aromatic hydrocarbon ring, such as a phenyl group, a biphenyl group, a fluorenyl group, a naphthyl group, an anthryl group, or a phenanthryl group, or monomers having heteroaryl groups in which a part of the carbon atoms constituting the ring of these groups is substituted with a heteroatom such as an oxygen atom, a sulfur atom, or a nitrogen atom. In addition, examples of monomers having a highly polar functional group can include monomers having a trimethoxysilyl group, a trichlorosilyl group, an epoxy group, a glycidyl group, a carboxy group, a hydroxyl group, a cyano group, or a hydroxyalkyl group in which a part of the hydrogen atoms of an alkyl group is substituted with a hydroxyl group. From the viewpoint of forming a vertically oriented phase separation structure in the BCP layer, the proportion of structural units derived from a monomer having an aromatic ring in the resin is preferably 20 to 90 mol %, and more preferably 30 to 85 mol %, relative to the total (100 mol %) of all structural units constituting the resin. Other examples of compounds that contain both a moiety with high affinity for styrene and a moiety with high affinity for methyl methacrylate include compounds that contain both an aryl group and a highly polar functional group, such as phenethyltrichlorosilane, and compounds that contain both an alkyl group and a highly polar functional group, such as alkylsilane compounds.
[0086] The resin composition for the base can be produced by dissolving the above-mentioned resin in a solvent. Such a solvent may be any solvent capable of dissolving each component used to form a homogeneous solution, and examples thereof include the same organic solvent components as those exemplified in the description of the resin composition for forming an etching mask pattern of the above embodiment.
[0087] The type of the support 1 is not particularly limited as long as the resin composition can be applied to the surface thereof. For example, substrates made of inorganic substances such as metals (silicon, copper, chromium, iron, aluminum, etc.), glass, titanium oxide, silica, and mica; substrates made of oxides such as SiO2; substrates made of nitrides such as SiN; substrates made of oxynitrides such as SiON; and substrates made of organic substances such as acrylic, polystyrene, cellulose, cellulose acetate, and phenolic resin. Among these, metal substrates are preferred, and for example, a cylinder structure is easily formed on a silicon substrate (Si substrate) or a copper substrate (Cu substrate). Among these, a Si substrate is particularly preferred. The size and shape of the support 1 are not particularly limited. The support 1 does not necessarily have to have a smooth surface, and substrates of various shapes can be appropriately selected. For example, substrates having a curved surface, flat plates with an uneven surface, and substrates having a flaky shape can be mentioned.
[0088] The surface of the support 1 may be provided with an inorganic and / or organic film. Examples of inorganic films include inorganic anti-reflective coatings (inorganic BARCs). Examples of organic films include organic anti-reflective coatings (organic BARCs). The inorganic film can be formed, for example, by applying an inorganic anti-reflective coating composition, such as a silicon-based material, onto a support and baking the composition. The organic film can be formed, for example, by applying an organic film-forming material, which is a resin component that constitutes the film, dissolved in an organic solvent, onto a substrate using a spinner or the like, and baking the material at a temperature of preferably 200 to 300° C., preferably for 30 to 300 seconds, more preferably for 60 to 180 seconds. This organic film-forming material does not necessarily need to be sensitive to light or electron beams, as in the case of a resist film, and may or may not be sensitive. Specifically, resists and resins that are commonly used in the manufacture of semiconductor elements and liquid crystal display elements can be used. In addition, the organic film forming material is preferably a material capable of forming an organic film that can be etched, particularly dry etched, so that the organic film pattern can be formed by etching the organic film using a pattern made of block copolymer formed by processing the BCP layer 3. Among them, it is preferable that the material be a material capable of forming an organic film that can be etched by oxygen plasma etching or the like. Such an organic film forming material may be a material that has been used to form an organic film such as organic BARC. For example, the ARC series manufactured by Nissan Chemical Industries, Ltd., the AR series manufactured by Rohm and Haas, and the SWK series manufactured by Tokyo Ohka Kogyo Co., Ltd. can be mentioned.
[0089] The method for applying the primer onto the support 1 to form the primer layer 2 is not particularly limited, and may be any of the conventionally known methods. For example, the undercoat layer 2 can be formed by applying the undercoat agent onto the support 1 by a conventionally known method such as spin coating or using a spinner to form a coating film, and then drying the coating film. The coating film can be dried by any method capable of volatilizing the solvent contained in the undercoat agent, such as baking. In this case, the baking temperature is preferably 80 to 300° C., more preferably 180 to 270° C., and further preferably 220 to 250° C. The baking time is preferably 30 to 500 seconds, and more preferably 60 to 400 seconds. The thickness of the undercoat agent layer 2 after the coating film has dried is preferably about 10 to 100 nm, and more preferably about 40 to 90 nm.
[0090] The surface of the support 1 may be washed before forming the primer layer 2 on the support 1. Washing the surface of the support 1 improves the coatability of the primer. The cleaning treatment may be carried out by any of the conventional methods known in the art, including, for example, oxygen plasma treatment, ozone oxidation treatment, acid-alkali treatment, and chemical modification treatment.
[0091] After forming the primer layer 2, the primer layer 2 may be rinsed with a rinsing liquid such as a solvent, if necessary. The rinsing removes uncrosslinked portions and the like in the primer layer 2, improving the affinity with at least one block constituting the block copolymer, and facilitating the formation of a phase-separated structure consisting of cylindrical structures oriented perpendicular to the surface of the support 1. The rinse liquid may be any liquid capable of dissolving the uncrosslinked portions, and examples of such liquid include solvents such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), ethyl lactate (EL), and mixtures of two or more of these solvents, as well as commercially available thinners. After the cleaning, post-baking may be performed to volatilize the rinsing liquid. The temperature conditions for this post-baking are preferably 80 to 300°C, more preferably 90 to 270°C, and even more preferably 100 to 250°C. The baking time is preferably 30 to 500 seconds, and more preferably 60 to 240 seconds. The thickness of the undercoat agent layer 2 after such post-baking is preferably about 1 to 10 nm, and more preferably about 2 to 7 nm.
[0092] Next, on the undercoat agent layer 2, a layer (BCP layer) 3 containing a (BCP) component is formed. The method for forming the BCP layer 3 on the undercoat layer 2 is not particularly limited, and examples thereof include a method in which the resin composition for forming an etching mask pattern of the above-mentioned embodiment is applied onto the undercoat layer 2 by a conventionally known method such as using spin coating or a spinner to form a coating film, and then drying.
[0093] The thickness of the BCP layer 3 may be sufficient to form an etching mask pattern, and is preferably 25 nm or more, more preferably 30 nm or more, and even more preferably 36 nm or more. The upper limit of the thickness of the BCP layer 3 is, for example, 100 nm or less, preferably 90 nm or less, more preferably 80 nm or less, even more preferably 70 nm or less, and particularly preferably 60 nm or less. For example, when the support 1 is a Si substrate, the thickness of the BCP layer 3 is preferably adjusted to 25 to 100 nm, more preferably 30 to 90 nm, even more preferably 30 to 80 nm, and particularly preferably 30 to 60 nm.
[0094] [Step (ii)] In step (ii), the BCP layer 3 formed on the support 1 is subjected to phase separation. By heating the support 1 after step (i) to perform an annealing treatment, the block copolymer is selectively removed to form a phase-separated structure that exposes at least a part of the surface of the support 1. That is, a structure 3' including a phase-separated structure separated into phases 3a and 3b is produced on the support 1. The temperature condition of the annealing treatment is preferably equal to or higher than the glass transition temperature of the (BCP) component used and lower than the thermal decomposition temperature, and for example, when the block copolymer is a polystyrene-polymethyl methacrylate (PS-PMMA) block copolymer (mass average molecular weight 5000 to 100000), the temperature is preferably 180 to 270° C. The heating time is preferably 30 to 3600 seconds. Moreover, the annealing process is preferably carried out in a gas with low reactivity, such as nitrogen.
[0095] According to the method for producing an etching mask pattern of the embodiment described above, since the resin composition for forming an etching mask pattern of the embodiment described above is used, it is possible to obtain a structure containing a vertically oriented phase separation structure with a film thickness sufficient for forming an etching mask pattern (for example, a film thickness of 25 nm or more, preferably a film thickness of 30 nm or more). Therefore, an etching mask pattern can be produced using the structure containing the phase separation structure.
[0096] [Optional process] The method for producing a structure containing a phase-separated structure is not limited to the above-described embodiment, and may include steps (optional steps) other than steps (i) and (ii).
[0097] Such optional steps include a step of selectively removing a phase of at least one type of block of the first block and the second block constituting the (BCP) component from the BCP layer 3 (hereinafter referred to as "step (iii)"), a guide pattern formation step, and the like.
[0098] Regarding step (iii) In the step (iii), a phase consisting of at least one of the first and second blocks constituting the (BCP) component is selectively removed from the BCP layer formed on the undercoat agent layer 2. This forms an etching mask pattern.
[0099] As a method for selectively removing a phase consisting of any one of the blocks, a method for subjecting the BCP layer to an oxygen plasma treatment, a method for subjecting the BCP layer to a hydrogen plasma treatment, or the like can be mentioned. For example, after phase separation of a BCP layer containing the (BCP) component, the BCP layer is subjected to oxygen plasma treatment, hydrogen plasma treatment, or the like, whereby the phase consisting of the first block is not selectively removed, but the phase consisting of the second block is selectively removed.
[0100] FIG. 2 shows an example embodiment of step (iii). In the embodiment shown in Figure 2, the structure 3' produced on the support 1 in step (ii) is subjected to an oxygen plasma treatment to selectively remove the phase 3a and form an etching mask pattern consisting of spaced apart phases 3b, where phase 3b is the phase consisting of the first block and phase 3a is the phase consisting of the second block.
[0101] The etching mask pattern obtained as described above can be used as is for etching a support, but by further heating it, the shape of the etching mask pattern on the support 1 can also be changed. The heating temperature is preferably equal to or higher than the glass transition temperature of the block copolymer used and lower than its thermal decomposition temperature, and is preferably carried out in a gas with low reactivity such as nitrogen.
[0102] Guide pattern formation process The method for producing a structure containing a phase-separated structure may include a step of providing a guide pattern on the undercoat agent layer (guide pattern forming step) prior to the above-mentioned steps (i) and (ii), which allows control of the arrangement of the phase-separated structure. For example, even in the case of a block copolymer that forms a random fingerprint-like phase separation structure when no guide pattern is provided, by providing a groove structure of the resist film on the surface of the undercoat layer, a phase separation structure oriented along the groove can be obtained. Based on this principle, a guide pattern may be provided on the undercoat layer 2. In addition, if the surface of the guide pattern has affinity with any of the blocks constituting the (BCP) component, a phase separation structure oriented perpendicular to the support surface is easily formed.
[0103] The guide pattern can be formed using, for example, a resist composition. The resist composition for forming the guide pattern can be appropriately selected from resist compositions generally used for forming resist patterns and their modifications, and can be used by selecting one having affinity with any of the blocks constituting the (BCP) component. The resist composition may be either a positive resist composition for forming a positive pattern in which the exposed portion of the resist film is dissolved and removed, or a negative resist composition for forming a negative pattern in which the unexposed portion of the resist film is dissolved and removed, but is preferably a negative resist composition. As the negative resist composition, for example, a resist composition containing an acid generator and a base component whose solubility in a developer containing an organic solvent is reduced by the action of an acid, and the base component contains a resin component having a structural unit that is decomposed by the action of an acid to increase polarity, is preferable. After the resin composition for forming an etching pattern is poured onto the undercoat layer on which the guide pattern is formed, an annealing treatment is performed to cause phase separation. Therefore, it is preferable that the resist composition for forming the guide pattern is one capable of forming a resist film having excellent solvent resistance and heat resistance. EXAMPLES
[0104] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0105] (Synthesis of BCP precursor: BCP precursor (1)) All anionic polymerizations were carried out under an argon atmosphere. 30 mL of tetrahydrofuran (THF) and lithium chloride (LiCl) (21.2 mg, 0.500 mmol) were transferred to a 50 mL Schlenk tube and cooled to -78 °C in a cool-nic bath. Sec-butyl lithium (Sec-BuLi) (1.05 M in hexane / cyclohexane) was added to the Schlenk tube until the color of the solution turned yellow. The Schlenk tube was removed from the cool-nic bath and warmed at room temperature until the solution became colorless. The Schlenk tube was again cooled to -78 °C in a cool-nic bath and sec-BuLi (0.095 mL, 0.100 mmol) was added as initiator. Styrene (1.03 mL, 9.04 mmol) was added and stirred for 30 min. This resulted in a bright orange solution. 1,1-diphenylethylene (DPE) (0.088 mL, 0.50 mmol) was added, and the color of the solution changed to deep red. After stirring for 30 min, a monomer mixture of methyl methacrylate (MMA) (0.80 mL, 7.50 mmol) and glycidyl methacrylate (GMA) (0.325 mL, 2.50 mmol) was added and stirred for 30 min. The color of the solution changed from red to transparent. The polymerization was terminated by adding 3 mL of degassed methanol (MeOH) to the Schlenk flask as a terminator. The Schlenk flask was removed from the coolnics bath, and the solution was poured into MeOH for reprecipitation. The precipitated solid was filtered and then dried under reduced pressure at 40 °C to obtain a white powder of BCP precursor (1) (1.76 g, 88% yield).
[0106] (Synthesis of block copolymer: BCP(1)) A 10 mL glass tube was charged with 0.2 g of BCP precursor (1) and THF (20 wt% solution) and immersed in an ice-water bath. 1 wt% lithium hydroxide (LiOH) aqueous solution (LiOH 0.05 molar equivalents / GMA unit) and 2,2,2-trifluoroethanethiol (2 molar equivalents / GMA unit) were added to the glass tube. After stirring at room temperature for 20 min, the reactor was set to 40 °C and stirred for 3 h to synthesize BCP (1). Depending on the Mn and PHFMA fraction of the synthesized BCP (1), it was repeatedly precipitated several times with methanol or methanol / hexane to remove residual reagents. The product was dried under reduced pressure at room temperature overnight to obtain a white powder of BCP (1). The Mn and polydispersity (PDI = Mw / Mn) of BCP (1) measured by size exclusion chromatography (SEC) were 23,000 g mol -1 and 1.05. 1 H NMR(400MHz,Acetone-d6,δ,ppm):0.84(s,α-CH3,PMMA),0.87(s,α-CH3,PMMA),1.00(s,α-CH3,PMMA),1.03(s,α-CH3,PHF MA),1.23-1.73(br,backbone,-CH2-CH-,PS),1.75-2.23(br,backbone,-CH2-CH-,PS,br,backbone,-CH2-C(CH3)-,PHFMA and PMMA),2.78-3.00(d,CH(OH)-CH2-S-,PHFMA),3.40-3.77(s,-S-CH2-CF3,PHFMA),3.54-3.75(s,-OCH3,PMMA),3.92-4.07(d,-(C=O)O-CH2-,P HFMA),4.07-4.18(m,-CH(OH)-,PHFMA)4.50-4.72(br,-CH(OH)-,PHFMA),6.36-6.84(m,o-aromatic,PS),6.85-7.35(m,m-,p-aromatic,PS).
[0107] (Synthesis of block copolymer: BCP(2)) BCP precursor (2) was synthesized in the same manner as BCP precursor (1) above, except that the amount of styrene used was 2.71 mL (23.8 mmol), the amount of MMA used was 0.91 mL (8.5 mmol), and the amount of GMA used was 0.065 mL (0.5 mmol). Next, BCP (2) was synthesized in the same manner as BCP (1) above, except that BCP precursor (2) was used instead of BCP precursor (1). The Mn and polydispersity (PDI = Mw / Mn) of BCP (2) measured by size exclusion chromatography (SEC) were 33,000 g mol -1 and 1.05.
[0108] [ka]
[0109] (Measurement of the volume of each block) The mole percentage of each block in the block copolymer is 1 The mass percentage of each block was calculated from the results of H NMR analysis, and the mass percentage of each block was further calculated. The mass percentage of each block was then divided by the density of each block to calculate the volume ratio of each block. From the volume ratio, the proportion of the volume of the polystyrene block in the total volume of the block copolymer was calculated. The density of each block was estimated by the atomic group contribution method (Fedors, RF Polym. Eng. Sci. 1974, 14, 147-154.). The density of the polystyrene block was 1.05 gm -3 The density of the structure composed of structural units derived from methyl methacrylate was 1.18 gcm -3 The density of the structure composed of building blocks derived from 2-hydroxy-3-(2,2,2-trifluoroethylsulfanyl)propyl methacrylate was 1.43 gcm -3 was used.
[0110] Table 1 shows the number average molecular weight (Mn), polydispersity (PDI=Mw / Mn), volume ratio (vol%) of the polystyrene block (PS) to the total volume of the block copolymer, and the value of x in the above reaction formula.
[0111] [Table 1]
[0112] (Preparation of primer) The components shown in Table 2 were mixed and dissolved to prepare each of the base agents NL-1 to NL-3 (solid content concentration: 1% by mass).
[0113] [Table 2]
[0114] In Table 2, the abbreviations have the following meanings. The numbers in brackets [ ] are the amounts used (parts by mass). The number average molecular weight (Mn) of each polymer was determined by size exclusion chromatography (SEC). The copolymer composition ratio of each polymer (the ratio (molar ratio) of each structural unit in the structural formula) is 3 The carbon-carbon valence was determined by C-NMR. (P)-1: A polymer represented by the following chemical formula (P-1). Mn=24000. l / m / n=39 / 56 / 5. (P)-2: Polymer represented by the following chemical formula (P-1). Mn=28000. l / m / n=49 / 46 / 5. (P)-3: Polymer represented by the following chemical formula (P-1). Mn=30000. l / m / n=61 / 34 / 5. (S)-1: Propylene glycol monomethyl ether acetate (PGMEA).
[0115] [ka]
[0116] In Table 2, "Water contact angle (°)" was measured as follows. A primer layer was formed in the same manner as described later in "Formation of primer layer". Water (2 μL) was dropped onto the surface of the primer layer, and the contact angle (static contact angle) was measured using DROP MASTER-700 (product name, manufactured by Kyowa Interface Science Co., Ltd.).
[0117] (Examples 1 to 3, Comparative Example 1) <Preparation of Resin Composition for Forming Etching Mask Pattern> The components shown in Table 3 were mixed and dissolved to prepare respective examples of resin compositions for forming etching mask patterns (solid content concentration: 1.25% by mass).
[0118] [Table 3]
[0119] In Table 3, the abbreviations have the following meanings. The numbers in brackets [ ] indicate the blend amount (parts by mass). BCP-1: BCP(1). PS-2k: Polystyrene. Number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 2000. PMMA-2k: Polymethylmethacrylate. The number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 2000. (S)-1: PGMEA.
[0120] <Production of Etching Mask Pattern (1)> After forming a base layer on a wafer using the above base agent NL-1, an etching mask pattern was obtained using the resin composition for forming an etching mask pattern of each of the above examples by a manufacturing method having the steps (i) to (iii) shown below.
[0121] Applying the primer layer: The above-mentioned primer NL-1 was spin-coated on a silicon substrate, and then heated at 250°C for 5 minutes in an air atmosphere. The substrate was then rinsed with a mixed solvent of propylene glycol monomethyl ether (PGME) / propylene glycol monomethyl ether acetate (PGMEA) (PGME / MGMEA = 7 / 3 (mass ratio)). The substrate was then heated at 100°C for 1 minute. As a result, a 5 nm thick primer layer made of the primer NL-1 was formed on the substrate surface.
[0122] Process (i): Onto the above undercoat agent layer, the resin composition for forming an etching mask pattern of each example was spin-coated to a film thickness of 36 nm to form a resin composition layer (a layer containing a block copolymer).
[0123] Step (ii): The resin composition layer formed on the undercoat layer was prebaked at 90° C. for 60 seconds in a nitrogen atmosphere, and then annealed at 240° C. for 5 minutes in a nitrogen atmosphere to form a phase-separated structure.
[0124] Step (iii): The substrate on which the phase-separated structure was formed was subjected to oxygen plasma treatment (200 mL / min, 40 Pa, 40°C, 200 W, 10 seconds) using TCA-3822 (Tokyo Ohka Kogyo Co., Ltd.) to selectively remove the PMMA phase.
[0125] [Resolution evaluation] The surface (phase-separated state) of the obtained substrate was observed with a length-measuring SEM (scanning electron microscope, product name: CG6300, manufactured by Hitachi High-Technologies Corporation), and the formation of a microphase-separated structure (lamellar structure) was confirmed. As a result of such observation, the resolution was evaluated based on the following evaluation criteria. The results are shown in Table 4 as "resolution". (Evaluation Criteria) A: A microphase-separated structure without discontinuities was observed over the entire surface. B: Disconnection was observed in part of the microphase-separated structure. C: No microphase-separated structure was observed.
[0126] [Evaluation of vertical alignment] The surface (phase-separated state) of the obtained substrate was observed with a length-measuring SEM (scanning electron microscope, product name: CG6300, manufactured by Hitachi High-Technologies Corporation). As a result of such observation, the vertical alignment of the etching pattern was evaluated based on the following evaluation criteria. The results are shown in Table 3 as "vertical alignment". (Evaluation Criteria) A: A vertical lamellar pattern is formed over the entire surface. B: Vertical lamellar pattern partially formed. C: No terrace structure or pattern.
[0127] [Table 4]
[0128] From the results shown in Table 4, etching mask patterns with good resolution and vertical alignment were formed in Examples 1 to 3. On the other hand, in Comparative Example 1, a vertical lamellar pattern could not be formed, and an etching mask pattern could not be formed.
[0129] (Examples 4 to 8, Comparative Examples 2 to 4) <Preparation of Resin Composition for Forming Etching Mask Pattern> The components shown in Table 5 were mixed and dissolved to prepare respective examples of resin compositions for forming etching mask patterns (solid content concentration: 1.25% by mass).
[0130] [Table 5]
[0131] In Table 5, the abbreviations have the following meanings. The numbers in brackets [ ] indicate the blend amount (parts by mass). BCP-1: BCP(1). PS-2k: Polystyrene. Number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 2000. PS-1.5k: Polystyrene. The number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 1500. PS-3k: Polystyrene. Number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 3000. PS-5k: Polystyrene. Number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 5000. PMMA-2k: Polymethylmethacrylate. The number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 2000. PMMA-1.5k: Polymethylmethacrylate. The number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 1500. PMMA-3k: Polymethylmethacrylate. The number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 3000. PMMA-5k: Polymethylmethacrylate. The number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 5000. (S)-1: PGMEA.
[0132] <Production of Etching Mask Pattern (2)> An etching mask pattern was formed in the same manner as in <Production of Etching Mask Pattern (1)> above, except that the above-mentioned undercoat agent NL-1 or NL-2 was used as the undercoat agent.
[0133] [Resolution evaluation] The resolution of the etching pattern formed using each of the resin compositions for forming an etching mask pattern was evaluated in the same manner as above. The results are shown in Table 6 as "resolution".
[0134] [Evaluation of vertical alignment] The vertical alignment property of the etching pattern formed using each of the resin compositions for forming an etching mask pattern was evaluated in the same manner as above. The results are shown in Table 6 as "vertical alignment property".
[0135] [Table 6]
[0136] From the results shown in Table 6, an etching mask pattern with good resolution and vertical alignment could be formed regardless of which base agent was used in Examples 4 to 8. On the other hand, in Comparative Example 1, regardless of which base agent was used, a vertical lamellar pattern could not be formed, and an etching mask pattern could not be formed.
[0137] (Examples 9 to 10, Comparative Examples 5 to 7) <Preparation of Resin Composition for Forming Etching Mask Pattern> The components shown in Table 7 were mixed and dissolved to prepare respective examples of resin compositions for forming etching mask patterns (solid content concentration: 1.25% by mass).
[0138] [Table 7]
[0139] In Table 7, the abbreviations have the following meanings. The numbers in brackets [ ] indicate the blend amount (parts by mass). BCP-2: BCP(2). BCP-3: Block copolymer BCP(3) (PS-b-PMMA) shown below. The number average molecular weight (Mn), polydispersity (PDI=Mw / Mn), and volume ratio (vol %) of the polystyrene block (PS) to the total volume of the block copolymer are summarized in Table 8.
[0140] [ka]
[0141] [Table 8]
[0142] PS-2k: Polystyrene. Number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 2000. PMMA-2k: Polymethylmethacrylate. The number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 2000. (S)-1: PGMEA.
[0143] <Production of Etching Mask Pattern (3)> An etching mask pattern was formed in the same manner as in <Production of Etching Mask Pattern (1)> above, except that the undercoat agent NL-3 was used as the undercoat agent and the annealing temperature was set to 220°C.
[0144] [Resolution evaluation] The surface (phase-separated state) of the obtained substrate was observed with a length measuring SEM (scanning electron microscope, product name: CG6300, manufactured by Hitachi High-Technologies Corporation), and the formation of a microphase-separated structure (cylinder structure) was confirmed. As a result of such observation, the resolution was evaluated based on the following evaluation criteria. The results are shown in Table 4 as "resolution". (Evaluation Criteria) A: A microphase-separated structure without discontinuities was observed over the entire surface. B: Disconnection was observed in part of the microphase-separated structure. C: No microphase-separated structure was observed.
[0145] [Evaluation of vertical alignment] The surface (phase-separated state) of the obtained substrate was observed with a length-measuring SEM (scanning electron microscope, product name: CG6300, manufactured by Hitachi High-Technologies Corporation). As a result of such observation, the vertical alignment of the etching pattern was evaluated based on the following evaluation criteria. The results are shown in Table 9 as "vertical alignment". (Evaluation Criteria) A: A vertical cylinder pattern is formed over the entire surface. B: Vertical cylinder pattern is partially formed. C: No terrace structure or pattern.
[0146] [Table 9]
[0147] From the results shown in Table 9, etching mask patterns with good resolution and vertical alignment were formed in Examples 9 to 10. On the other hand, in Comparative Examples 5 to 7, a vertical cylinder pattern could not be formed, and an etching mask pattern could not be formed.
[0148] (Synthesis of block copolymer: BCP(4)) BCP(4) was synthesized in the same manner as above (Synthesis of block copolymer: BCP(1)), except that ethanethiol was used instead of 2,2,2-trifluoroethanethiol. The Mn and polydispersity (PDI = Mw / Mn) of BCP(4) measured by size exclusion chromatography (SEC) were 23,000 g mol -1 and 1.05. 1 H NMR(400MHz,CDCl3,δ,ppm):0.85-1.02(α-CH3,PMMA,PGEMA,-S-CH2-CH3,PGEMA,),1.23-1.69(-CH2-CH-,PS backbone),1.74-2.02(-CH2-CH-,PS backbone,-CH2-C(CH3)-,PGEMA and PMMA),2.63(-CH(OH)-CH2-S-CH2-CH3,PGEMA),3.60(-O-CH3,PMMA),3.99(-(C=O)O-CH2-CH(OH),PGEMA),6.39-6.85(o-aromatic,PS),6.91-7.42(p-,m-aromatic,PS).
[0149] (Synthesis of block copolymer: BCP(5)) BCP(5) was synthesized in the same manner as described above (Synthesis of block copolymer: BCP(2)), except that ethanethiol was used instead of 2,2,2-trifluoroethanethiol. The Mn and polydispersity (PDI = Mw / Mn) of BCP(5) measured by size exclusion chromatography (SEC) were 33,000 g mol -1 and 1.05.
[0150] [ka]
[0151] (Synthesis of block copolymer: BCP(6)) BCP(6) was synthesized in the same manner as described above (Synthesis of block copolymer: BCP(1)), except that 1-propanethiol was used instead of 2,2,2-trifluoroethanethiol. The Mn and polydispersity (PDI = Mw / Mn) of BCP(6) measured by size exclusion chromatography (SEC) were 23,000 g mol -1 and 1.05. 1 H NMR(400MHz,CDCl3,δ,ppm):0.85-1.02(α-CH3,PMMA,PGPMA,-S-CH2-CH2-CH3,PGPMA,),1.23-1.69(-S-CH2-CH2-CH3,PGPMA,-CH2-CH-,PS backbone),1.74-2.02(-CH2-CH-,PS backbone,-CH2-C(CH3)-,PGPMA and PMMA),2.63(-CH(OH)-CH2-S-CH2-CH2-,PGPMA),3.60(-O-CH3,PMMA),3.99(-(C=O)O-CH2-CH(OH),PGPMA),6.39-6.85(o-aromatic,PS),6.91-7.42(p-,m-aromatic,PS).
[0152] (Synthesis of block copolymer: BCP(7)) BCP(7) was synthesized in the same manner as described above (Synthesis of block copolymer: BCP(2)), except that 1-propanethiol was used instead of 2,2,2-trifluoroethanethiol. The Mn and polydispersity (PDI = Mw / Mn) of BCP(7) measured by size exclusion chromatography (SEC) were 33,000 g mol -1 and 1.05.
[0153] [ka]
[0154] (Synthesis of block copolymer: BCP(8)) BCP(8) was synthesized in the same manner as described above (Synthesis of block copolymer: BCP(1)), except that 1-hexanethiol was used instead of 2,2,2-trifluoroethanethiol. The Mn and polydispersity (PDI = Mw / Mn) of BCP(8) measured by size exclusion chromatography (SEC) were 23,000 g mol -1 and 1.05. 1 H NMR(400MHz,CDCl3,δ,ppm):0.85-1.02(α-CH3,PMMA, PGHMA,-CH2-CH2-CH3,PGHMA,),1.23-1.69(-S-CH2-CH2-CH2-CH2-CH2-,PGHMA,-CH2-CH-,PS backbone),1.74-2.02(-CH2-CH-,PS backbone,-CH2-C(CH3)-,PGHMA and PMMA),2.63(-CH(OH)-CH2-S-CH2-CH2-,PGHMA),3.60(-O-CH3,PMMA),3.99(-(C=O)O-CH2-CH(OH),PGHMA),6.39-6.85(o-aromatic,PS),6.91-7.42(p-,m-aromatic,PS).
[0155] (Synthesis of block copolymer: BCP(9)) BCP(9) was synthesized in the same manner as described above (Synthesis of block copolymer: BCP(2)), except that 1-hexanethiol was used instead of 2,2,2-trifluoroethanethiol. The Mn and polydispersity (PDI = Mw / Mn) of BCP(9) measured by size exclusion chromatography (SEC) were 33,000 g mol -1 and 1.05.
[0156] [ka]
[0157] (Synthesis of block copolymer: BCP(10)) BCP(10) was synthesized in the same manner as above (Synthesis of block copolymer: BCP(1)), except that cyclohexanethiol was used instead of 2,2,2-trifluoroethanethiol. The Mn and polydispersity (PDI = Mw / Mn) of BCP(10) measured by size exclusion chromatography (SEC) were 23,000 g mol -1 and 1.05. 1 H NMR(400MHz,CDCl3,δ,ppm):0.85-1.02(α-CH3,PMMA,PGCMA),1.23-1.69(-S-CH(CH2-CH2)-CH2-CH2-CH2-,PGCMA,-CH2-CH-,PS backbone),1.74-2.02(-S-CH(CH2-CH2)-CH2-CH2-CH2-,PGCMA,-CH2-CH-,PS backbone,-CH2-C(CH3)-,PGCMA and PMMA),2.63(-CH(OH)-CH2-S-CH(CH2-CH2)-CH2-CH2-CH2-,PGCMA),3.60(-O-CH3,PMMA),3.99 (-(C=O)O-CH2-CH(OH),PGCMA),6.39-6.85(o-aromatic,PS),6.91-7.42(p-,m-aromatic,PS).
[0158] (Synthesis of block copolymer: BCP(11)) BCP(11) was synthesized in the same manner as described above (Synthesis of block copolymer: BCP(2)), except that cyclohexanethiol was used instead of 2,2,2-trifluoroethanethiol. The Mn and polydispersity (PDI = Mw / Mn) of BCP(11) measured by size exclusion chromatography (SEC) were 33,000 g mol -1 and 1.05.
[0159] [ka]
[0160] (Measurement of the volume of each block) The volume ratio of each block was calculated in the same manner as above. From the volume ratio, the proportion of the volume of the polystyrene block in the total volume of the block copolymer was calculated in the same manner as above. In the block copolymers (4) to (11), the density of the structure composed of the structural unit corresponding to the structural unit (b2g) (structural unit having a sulfide group) was 1.18 g cm -3 was used.
[0161] Table 10 shows the number average molecular weight (Mn), polydispersity (PDI=Mw / Mn), volume ratio (vol%) of the polystyrene block (PS) to the total volume of the block copolymer, and the value of x in the above reaction formula for the block copolymers (4) to (11) synthesized above.
[0162] [Table 10]
[0163] (Examples 11 to 30, Comparative Examples 8 to 15) <Preparation of Resin Composition for Forming Etching Mask Pattern> The components shown in Tables 11 and 12 were mixed and dissolved to prepare respective examples of resin compositions for forming etching mask patterns (solid content concentration: 1.25% by mass).
[0164] [Table 11]
[0165] [Table 12]
[0166] In Tables 11 and 12, the abbreviations have the following meanings: The numbers in brackets [ ] are the blend amounts (parts by mass). BCP-4~BCP-11: The above BCP(4)~BCP(11). PS-2k: Polystyrene. Number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 2000. PMMA-2k: Polymethylmethacrylate. The number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 2000. (S)-1: PGMEA.
[0167] <Manufacture of Etching Mask Pattern> An etching mask pattern was formed in the same manner as in <Production of Etching Mask Pattern (1)> above.
[0168] [Resolution evaluation] The resolution of the etching pattern formed using the resin composition for forming an etching mask pattern of each example was evaluated by the same method as described above (Examples 1 to 3, Comparative Example 1). The results are shown in Tables 13 to 14 as "resolution".
[0169] [Evaluation of vertical alignment] The surface (phase-separated state) of the obtained substrate was observed with a length-measuring SEM (scanning electron microscope, product name: CG6300, manufactured by Hitachi High-Technologies Corporation). As a result of such observation, the vertical alignment of the etching pattern was evaluated based on the following evaluation criteria. The results are shown in Tables 13 to 14 as "vertical alignment". (Evaluation Criteria) A: A vertical lamellar pattern is formed over the entire surface. B: Vertical lamellar pattern partially formed. C: No terrace structure or pattern.
[0170] [Table 13]
[0171] [Table 14]
[0172] From the results shown in Tables 13 and 14, etching mask patterns with good resolution and vertical alignment were formed in Examples 11 to 30. On the other hand, in Comparative Examples 8 to 15, a vertical lamellar pattern could not be formed, and an etching mask pattern could not be formed.
[0173] (Synthesis of block copolymer: BCP(12)) BCP(12) was synthesized in the same manner as described above (Synthesis of block copolymer: BCP(1)), except that 3-mercapto-1-hexanol was used instead of 2,2,2-trifluoroethanethiol. The Mn and polydispersity (PDI = Mw / Mn) of BCP(12) measured by size exclusion chromatography (SEC) were 23,000 g mol -1 and 1.05. 1H NMR(400MHz,CDCl3,δ,ppm):0.71-1.05(α-CH3,PMMA and PGOMA,-S-CH-CH2-CH2-CH3,PGOMA),1.43-2.02(-S-CH-CH2-CH2-CH3,PGOMA,-S-CH-CH2-CH2-OH,PGOMA,-CH2-CH-,PS backbone,-CH2-C(CH3)-,PGOMA and PMMA),2.68-2.88(-CH(OH)-CH2-S-CH(-,PGOMA),3.60(-O-CH3,PMMA),3.73(-S-CH-CH2-CH2-OH,PGOM A),4.08(-(C=O)O-CH2-CH(OH),PGOMA),6.39-6.85(o-aromatic,PS),6.91-7.42(p-,m-aromatic,PS).
[0174] (Synthesis of block copolymer: BCP(13)) BCP(13) was synthesized in the same manner as described above (Synthesis of block copolymer: BCP(2)), except that 3-mercapto-1-hexanol was used instead of 2,2,2-trifluoroethanethiol. The Mn and polydispersity (PDI = Mw / Mn) of BCP(13) measured by size exclusion chromatography (SEC) were 33,000 g mol -1 and 1.05.
[0175] [ka]
[0176] (Measurement of the volume of each block) The volume ratio of each block was calculated in the same manner as above. From the volume ratio, the proportion of the volume of the polystyrene block in the total volume of the block copolymer was calculated in the same manner as above. In the block copolymers (12) to (13), the density of the structure composed of the structural unit corresponding to the structural unit (b2g) (structural unit having a sulfide group) was 1.18 g cm -3 was used.
[0177] Table 15 shows the number average molecular weight (Mn), polydispersity (PDI=Mw / Mn), volume ratio (vol%) of the polystyrene block (PS) to the total volume of the block copolymer, and the value of x in the above reaction formula for the block copolymers (12) and (13) synthesized above.
[0178] [Table 15]
[0179] (Examples 31 to 35, Comparative Examples 16 and 17) <Preparation of Resin Composition for Forming Etching Mask Pattern> The components shown in Tables 16 and 17 were mixed and dissolved to prepare resin compositions for forming etching mask patterns (solid content concentration: 1.25% by mass).
[0180] [Table 16]
[0181] [Table 17]
[0182] In Tables 16 and 17, the abbreviations have the following meanings. The numbers in brackets [ ] are the amounts blended (parts by mass). BCP-12~BCP-13: The above BCP(12)~BCP(13). PS-2k: Polystyrene. Number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 2000. PMMA-2k: Polymethylmethacrylate. The number average molecular weight (Mn) measured by size exclusion chromatography (SEC) is 2000. (S)-1: PGMEA.
[0183] <Manufacture of Etching Mask Pattern> In Comparative Example 16 and Examples 31 to 33, etching mask patterns were formed in the same manner as in <Production of Etching Mask Pattern (1)> above.
[0184] In Comparative Example 17 and Examples 34 to 35, etching mask patterns were formed in the same manner as in <Production of Etching Mask Pattern (3)> above.
[0185] [Resolution evaluation] The resolution of the etching pattern formed using the resin composition for forming an etching mask pattern of each example was evaluated by the same method as described above (Examples 1 to 3, Comparative Example 1). The results are shown in Tables 18 and 19 as "resolution".
[0186] [Evaluation of vertical alignment] The surface (phase-separated state) of the obtained substrate was observed with a length-measuring SEM (scanning electron microscope, product name: CG6300, manufactured by Hitachi High-Technologies Corporation). As a result of such observation, the vertical alignment of the etching pattern was evaluated based on the following evaluation criteria. The results are shown in Tables 18 and 19 as "vertical alignment". (Evaluation Criteria) A: A vertical lamellar pattern is formed over the entire surface. B: Vertical lamellar pattern partially formed. C: No terrace structure or pattern.
[0187] [Table 18]
[0188] [Table 19]
[0189] From the results shown in Tables 18 and 19, etching mask patterns with good resolution and vertical alignment were formed in Examples 31 to 35. On the other hand, in Comparative Examples 16 and 17, a vertical lamellar pattern could not be formed, and an etching mask pattern could not be formed. [Explanation of symbols]
[0190] 1... Support, 2... Base layer, 3... BCP layer, 3'... Structure, 3a... Phase, 3b... Phase.
Claims
1. A resin composition for forming an etching mask pattern, comprising a block copolymer having a first block and a second block, and a homopolymer having a number average molecular weight of less than 3,000, The first block is composed of a polymer having a repeating structure of a structural unit represented by the following general formula (b1): The second block is composed of a random copolymer having a structure in which a constitutional unit represented by the following general formula (b2m) and a constitutional unit represented by the following general formula (b2g) are randomly arranged, a ratio of a volume of the first block to a total volume of the first block and the second block is 20 to 80 volume %, The homopolymer includes a polymer having a repeating structure of a structural unit represented by the following general formula (b1): A resin composition for forming an etching mask pattern. 【Chemistry 1】 [In formula (b1), R 1 is an alkyl group. b1 is a hydrogen atom or a methyl group. n is an integer of 0 to 5. When n is an integer of 2 or more, a plurality of R 1 may be the same or different. In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear or branched alkylene group having 1 to 10 carbon atoms which may have a hydroxyl group. In formula (b2g) and formula (b2m), R b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 may be the same or different. x represents a molar ratio and is greater than 0 and less than 1.
2. 2. The resin composition for forming an etching mask pattern according to claim 1, wherein the homopolymer further contains a polymer having a repeating structure of a structural unit represented by general formula (b2m).
3. 3. The resin composition for forming an etching mask pattern according to claim 1, wherein the homopolymer has a number average molecular weight of 1,000 or more.
4. 3. The resin composition for forming an etching mask pattern according to claim 1, wherein the content of the homopolymer is 10 to 50 parts by mass based on 100 parts by mass of the block copolymer.
5. A step of applying the resin composition for forming an etching mask pattern according to claim 1 or 2 onto a support to form a layer containing a block copolymer; allowing the layer containing the block copolymer to phase separate; The method for producing an etching mask pattern includes the steps of:
6. The method for producing an etching mask pattern according to claim 5 , wherein the layer containing the block copolymer is formed to a thickness of 25 nm or more.
Citation Information
Patent Citations
Pattern formation method and mold
JP2008036491A
Resin composition for forming phase separation structure, method for producing structure body including phase separation structure, and block copolymer
JP2022020519A