Module, system, and package
By matching the linear expansion coefficients of the substrate and frame materials and using elastic adhesives, the image sensor module minimizes warpage due to temperature changes, ensuring stable operation and assembly accuracy.
Patent Information
- Application Number
- JP2024145745
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional image sensor modules experience warpage due to differences in linear expansion coefficients of materials, leading to transportation and fixation issues during manufacturing and significant deformation under temperature changes.
The image sensor module is designed with a substrate and frame structure where the linear expansion coefficients of the substrate and frame are matched to offset thermal expansion, using adhesives with rubber elasticity to absorb differences, and a light-transmitting member to minimize warpage.
The design significantly reduces warpage of the image sensor module across a wide temperature range, ensuring accurate assembly and operation of the image sensor module.
Smart Images

Figure 2024161135000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an imaging element module, an imaging system, an imaging element package, and a manufacturing method thereof. [Background technology]
[0002] There has been proposed an imaging element module in which electronic components such as a solid-state imaging element are enclosed inside a hollow package. Patent documents 1 and 3 disclose a solid-state imaging element module composed of a substrate, a frame, a solid-state imaging element, and a light-transmitting member. Patent document 2 discloses a solid-state imaging element package composed of a substrate and a resin frame molded on the substrate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-243339 A [Patent Document 2] Patent Application No. 2013-557430 (Patent No. 6176118) [Patent Document 3] JP 2015-185763 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the above-mentioned conventional technology, there is a problem that the difference in the linear expansion coefficient between the materials constituting the image sensor module causes warping of the substrate, which causes problems in the transportation and suction fixation of the image sensor module during the image sensor module manufacturing process. Also, even after the image sensor module is completed, there is a problem that a large warp may occur in the substrate due to a temperature change in the environment in which the image sensor module is used, which may cause a large warp in the light receiving surface of the image sensor.
[0005] An object of the present invention is to provide an image sensor module, an imaging system, an image sensor package, and a method for manufacturing an image sensor module that can suppress deformation due to temperature changes.
Means for Solving the Problems
[0006] According to an embodiment of the present invention, there is provided an image sensor module including a substrate having a first main surface and a second main surface, a solid-state image sensor attached to the first main surface, a frame attached to the first main surface so as to surround the solid-state image sensor, and a light-transmissive member fixed on the frame. The in-plane linear expansion coefficient of the substrate at a temperature equal to or lower than the glass transition temperature Tgp of the substrate is denoted as αPCB1, the in-plane linear expansion coefficient of the substrate at a temperature equal to or higher than the glass transition temperature Tgp is denoted as αPCB2, the linear expansion coefficient of the frame at a temperature equal to or lower than the glass transition temperature Tgf of the frame is denoted as αf1, and the linear expansion coefficient of the frame at a temperature equal to or higher than the glass transition temperature Tgf is denoted as αf2. When the normal temperature is To, an image sensor module is provided that satisfies the relationships of Tgp > Tgf, αf1 < αPCB1, and (Tgp - To) × αPCB1 < (Tgf - To) × αf1 + (Tgp - Tgf) × αf2, or Tgp < Tgf, αPCB1 < αf1, and (Tgf - To) × αf1 < (Tgp - To) × αPCB1 + (Tgf - Tgp) × αPCB2.
[0007] According to another embodiment of the present invention, there is provided an electronic component package including a substrate having a first main surface and a second main surface, and a frame attached to the first main surface, wherein an in-plane linear expansion coefficient of the substrate at a temperature equal to or lower than the glass transition temperature Tgp of the substrate is defined as αPCB1, an in-plane linear expansion coefficient of the substrate at a temperature higher than Tgp is defined as αPCB2, a linear expansion coefficient of the frame at a temperature equal to or lower than the glass transition temperature Tgf of the frame is defined as αf1, a linear expansion coefficient of the frame at a temperature higher than Tgf is defined as αf2, and when the normal temperature is defined as To, Tgp > Tgf, and αf1 < αPCB1, and (Tgp - To) × αPCB1 < (Tgf - To) × αf1 + (Tgp - Tgf) × αf2, or Tgp < Tgf, and αPCB1 < αf1, and (Tgf - To) × αf1 < (Tgp - To) × αPCB1 + (Tgf - Tgp) × αPCB2.
Effect of the Invention
[0008] According to the present invention, it is possible to provide an image sensor module, an imaging system, an image sensor package, and a method for manufacturing the same, which can suppress deformation due to temperature changes.
Brief Description of the Drawings
[0009] [Figure 1] It is a plan view of an image sensor module according to the first embodiment. [Diagram 2] It is a cross-sectional view of an image sensor module according to the first embodiment. [Diagram 3] It is a plan view of an image sensor module according to a modification of the first embodiment. [Figure 4] It is a cross-sectional view of an image sensor module according to a modification of the first embodiment. [Figure 5A] It is a view showing a method for manufacturing an image sensor module according to the first embodiment. [Figure 5B] It is a view showing a method for manufacturing an image sensor module according to the first embodiment. [Figure 6] It is a view showing a method for manufacturing an image sensor module according to a modification of the first embodiment. [Figure 7] FIG. 4 is a diagram illustrating the effect of the first embodiment. [Figure 8] FIG. 4 is a diagram illustrating the effect of the first embodiment. [Figure 9] FIG. 4 is a diagram illustrating the effect of the first embodiment. [Figure 10] FIG. 4 is a diagram illustrating the effect of the first embodiment. [Figure 11] FIG. 4 is a diagram illustrating the effect of the first embodiment. [Figure 12] FIG. 4 is a diagram illustrating the effect of the first embodiment. [Figure 13] FIG. 4 is a diagram illustrating the effect of the first embodiment. [Figure 14A] FIG. 2 is a diagram illustrating an example of the present invention and a comparative example. [Figure 14B] FIG. 2 is a diagram illustrating an example of the present invention and a comparative example. [Figure 15A] FIG. 2 is a diagram illustrating an example of the present invention and a comparative example. [Figure 15B] FIG. 2 is a diagram illustrating an example of the present invention and a comparative example. [Figure 16] FIG. 11 is a block diagram of an imaging system according to a second embodiment. [Figure 17] FIG. 11 is a diagram for explaining an imaging system according to a second embodiment. [Figure 18A] FIG. 11 is a block diagram of an imaging system relating to an in-vehicle camera in a third embodiment. [Figure 18B] FIG. 11 is a block diagram of an imaging system relating to an in-vehicle camera in a third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. [First embodiment] An image sensor module 1 according to a first embodiment of the present invention will be described. FIG. 1 is a plan view of the image sensor module 1 according to this embodiment. Specifically, FIG. 1(a) is a plan view of the front side of the image sensor module 1, FIG. 1(b) is an enlarged view of part A, and FIG. 1(c) is a plan view of the back side of the image sensor module 1. FIG. 2 is a cross-sectional view of the image sensor module 1 according to this embodiment. Specifically, FIG. 2(a) is a cross-sectional view of the image sensor module 1 taken along line II-II' in FIG. 1(a), FIG. 2(b) is an enlarged view of part C in FIG. 2(a), and FIG. 2(c) is an enlarged view of part D in FIG. 2(b). Each figure shows the X, Y, and Z directions. For convenience, the + direction of the Z axis will be described as up, and the - direction as down.
[0011] The imaging element module 1 includes a solid-state imaging element 10 and an imaging element package 50 that houses the solid-state imaging element 10. The imaging element package 50 is mainly configured to include a printed circuit board 20, a light-transmitting member 30, and a resin frame (frame body) 40.
[0012] The resin frame 40 has an opening corresponding to the solid-state imaging element 10. The light-transmitting member 30 can function as an optical member. The solid-state imaging element 10 is fixed to the printed circuit board 20. The light-transmitting member 30 is fixed to the printed circuit board 20 via the resin frame 40, and faces the solid-state imaging element 10 via an internal space 510. The resin frame 40 surrounds the internal space 510 between the light-transmitting member 30 and the solid-state imaging element 10. The above-mentioned internal space 510 is formed within the opening of the resin frame 40.
[0013] The positional relationship of the members constituting the imaging element module 1 can be determined on the XY plane. Here, the direction perpendicular to the XY plane is defined as the Z direction. The front surface 101 of the solid-state imaging element 10 and the back surface 102 of the solid-state imaging element 10 are parallel to the XY plane. As a typical example, the outer surface 301 of the light-transmitting member 30 and the inner surface 302 of the light-transmitting member 30 are parallel to the XY plane. The front surface 101 faces the inner surface 302, and the back surface 102 faces the arrangement region 210 of the printed circuit board 20 and is bonded to the printed circuit board 20.
[0014] A typical solid-state imaging element 10 and imaging element module 1 have a rectangular shape when projected onto the XY plane. The dimension of the solid-state imaging element 10 in the X direction is smaller than the dimensions in the Y and Z directions, and the solid-state imaging element 10 has a generally flat plate shape. Hereinafter, for convenience, the dimension in the Z direction will be referred to as the thickness or height.
[0015] In the X and Y directions, the outer edge of the image sensor module 1 is defined by the outer edge 405 of the resin frame 40 and the outer edge 305 of the light-transmitting member 30, and in this modification, also by the outer edge 205 of the printed circuit board 20. In addition to the outer edge 405, the resin frame 40 has an inner edge 403.
[0016] The area of the shadow of a member projected along the Z direction onto the XY plane is defined as the projection area. Here, when a member different from a member is located within the projection area of a member, it means that the member overlaps with the other member when viewed from the Z direction. Conversely, when a part of the projection area of the other member is located outside the projection area of a member, it can be said that at least a part of the other member is located in an area that does not overlap with the member. The boundary between the inside and outside of the projection area corresponds to the outer edge and inner edge (the inner edge may not exist) that are the contour of the target member. For example, the projection area of the solid-state imaging element 10 includes the projection area of the light-transmitting member 30 facing the solid-state imaging element 10, so the light-transmitting member 30 overlaps the solid-state imaging element 10.
[0017] The solid-state imaging element 10 has a main portion 11 and a sub-portion 12. The main portion 11 is located at the center of the solid-state imaging element 10, and the sub-portion 12 is located at the periphery thereof. The solid-state imaging element 10 is not limited to a CCD (Charged Coupled Device) image sensor, a CMOS (Complementary Metal Oxide Semiconductor) image sensor, or the like. The main portion 11 is an imaging portion and includes a plurality of pixels arranged in a matrix. In the solid-state imaging element 10, a surface 101 that faces the light-transmitting member 30 is a light incidence surface. The light incidence surface can be formed by the outermost layer of a multilayer film provided on a semiconductor substrate having a light-receiving surface. The multilayer film includes layers having optical functions such as a color filter layer, a microlens layer, an anti-reflection layer, and a light-shielding layer, a planarization layer, a passivation layer, and the like.
[0018] The sub-unit 12 includes a drive circuit for driving the main unit 11, and a signal processing circuit for processing signals from or to the main unit 11. When the solid-state imaging element 10 is a CMOS image sensor, it is easy to form these circuits monolithically. The sub-unit 12 is provided with electrodes (electrode pads) 103 for communicating signals between the solid-state imaging element 10 and the outside.
[0019] The solid-state imaging element 10 is disposed in at least a part of the central region of the printed circuit board 20, and the solid-state imaging element 10 is fixed to the printed circuit board 20. Typically, the solid-state imaging element 10 is fixed via an adhesive 502 disposed between the arrangement region 210 of the printed circuit board 20 and the back surface 102 of the solid-state imaging element 10, as shown in Figs. 2 and 3. However, the adhesive 502 may be in contact only with the outer edge 105, which is the side surface of the solid-state imaging element 10, and the inner surface 202 of the printed circuit board 20, and the adhesive 502 may not be disposed between the arrangement region 210 of the printed circuit board 20 and the back surface 102 of the solid-state imaging element 10. The adhesive 502 may be conductive or insulating. In addition, the adhesive 502 preferably has high thermal conductivity, and may contain metal particles.
[0020] Furthermore, when the solid-state imaging element 10 is formed on a silicon wafer substrate, the linear expansion coefficient of the silicon wafer is generally about 3 ppm / ° C., which is significantly different from the linear expansion coefficient in the planar direction of the printed circuit board 20. Therefore, in order to suppress warping of the solid-state imaging element 10, it is preferable to select an adhesive 502 having rubber elasticity. Specifically, silicone resin is preferable, and its elastic modulus is preferably 1 to 100 MPa. In particular, when the planar size of the solid-state imaging element 10 in the XY direction is large, silicone resin is effective in suppressing warping of the solid-state imaging element 10, and is highly effective for solid-state imaging elements of sizes equal to or larger than APSC (Advanced Photo System type C).
[0021] The imaging element package 50 has internal terminals 25 formed on the inner surface (the inner surface 202 of the printed circuit board 20) of the imaging element package 50 (the side of the internal space 510) and external terminals 27 formed on the outer surface (the outer surface 201 of the printed circuit board 20) of the imaging element package 50. A plurality of internal terminals 25 are lined up to form an internal terminal group.
[0022] These internal terminals 25 and external terminals 27 are provided integrally with the printed circuit board 20. In this example, as shown in Fig. 1(a), an internal terminal group consisting of a plurality of internal terminals 25 aligned in rows along the X direction and the Y direction is arranged to surround the solid-state imaging element 10. The arrangement of the internal terminals 25 is not limited to this, and it is also possible to arrange the internal terminal group aligned in rows only along the X direction or only along the Y direction.
[0023] Further, a plurality of external terminals 27 constitute an external terminal group. A plurality of electronic components are connected to some or all of the external terminal group by soldering using a known method. For this reason, the external terminal group is formed in advance in a layout that matches the shapes of these electronic components and the wiring circuit that connects these electronic components. A plating layer suitable for soldering may be formed on the surface of the external terminal group. For example, nickel plating (5 to 10 μm) or gold plating (0.1 to 1 μm) is suitable as the plating layer.
[0024] The electronic components are not limited, and various components may be mounted. Examples include a power supply IC 608, a capacitor 609, a connector 612, and a resistor 611. In addition, oscillator circuit components such as a crystal resonator (not shown) and a PLL (Phase Locked Loop) circuit may be mounted. Components may or may not be mounted on the external terminal 607. Terminals on which no components are mounted may be used as pads to which a probe is contacted when checking the operation of the circuit. In particular, a test pad row 612 can be arranged near the outer edge of the printed circuit board 20 to test electrical characteristics during shipping inspection of the image sensor module 1.
[0025] In this embodiment, the electrodes 103 of the solid-state imaging element 10 constituting the imaging element module 1 and the internal terminals 25 of the imaging element package 50 are electrically connected via connecting conductors 104. The connecting conductors 104 are metal wires, and may be mainly gold wires, aluminum wires, copper wires, etc. The connecting conductors 104 are connected to the internal terminals 25 by ultrasonic thermocompression bonding using a wire bonder.
[0026] Furthermore, the electrodes 103 and the internal terminals 25 may be connected by flip-chip connection. In this case, the electrodes 103 are provided on the back surface 102 of the solid-state imaging element 10, and the internal terminals 25 and the connecting conductors 104 are located in the arrangement region 210.
[0027] The printed circuit board 20 is a so-called multi-layer build-up board. As shown in the enlarged view of Fig. 2(c), the multi-layer build-up board includes a double-sided board in which conductor layers 211a, 211b are provided on both sides of an insulating layer 220 made of prepreg, which serves as a core. The conductor layers 211a, 211b are patterned into a desired pattern by lithography, and then necessary locations are connected by internal wiring 260 provided in drill vias.
[0028] Furthermore, an insulating layer 221a and a conductor layer 212a are formed in this order on the upper surface of the double-sided substrate, and an insulating layer 221b and a conductor layer 212b are formed in this order on the lower surface of the double-sided substrate. The conductor layers 212a and 212b are also patterned into a desired pattern by lithography, similar to the conductor layers 211a and 211b. At that time, the necessary parts are connected to the conductor layers 211a and 211b by internal wiring 261a and 261b provided in the laser vias. Thereafter, an insulating layer 222a and a conductor layer 213a, an insulating layer 222b and a conductor layer 213b are formed in the same manner. Also, an insulating layer 223a and a conductor layer 214a, and an insulating layer 223b and a conductor layer 214b are formed. The conductor layers 211a to 214a are connected by the internal wiring 261a, and the conductor layers 211b to 214b are connected by the internal wiring 261b. The insulating layers 221a to 223a and 221b to 223b are also made of prepreg.
[0029] The thickness of the insulating layer 220 is about 0.05 to 1.5 mm, and the thicknesses of the insulating layers 221a to 223a and 221b to 223b are about 0.05 to 0.3 mm. In the present embodiment, the printed circuit board 20 is a build-up board, but the present invention is not limited to this. For example, the thickness of the insulating layer 220 may be the same as that of the other insulating layers 221a to 223a and 221b to 223b, or may be a board that does not use drill vias (any-layer board).
[0030] Prepreg is a material in which fibers are woven or knitted into a cloth and impregnated with resin. Resins that are widely used are those that are mainly composed of epoxy or phenol. In addition, resins often contain insulating fillers such as paper and glass. Furthermore, the fibers are generally glass fibers, but are not limited to this as long as they are insulating.
[0031] An internal terminal 25 is formed on the conductor layer 214a on the inner surface (first main surface) 202 side of the printed circuit board 20, and an external terminal 27 is formed on the conductor layer 214b on the outer surface (second main surface) 201 side, each of which is patterned by lithography. In this way, the internal terminal 25 and the external terminal 27 are electrically continuous via the internal wiring 26 consisting of the internal wirings 260, 261a, and 261b of the printed circuit board 20. Copper is generally suitable for the conductor layers 211a to 214a and 211b to 214b. Other metals may be used as necessary.
[0032] In FIG. 2(c), a capacitor 609 is connected to the external terminal 27 via a solder 601. The length of the connection conductor 104 is approximately the thickness of the solid-state imaging element 10, for example, 0.1 to 1 mm. The thickness of the printed circuit board 20 is 0.1 to 1 mm, and when the internal wirings 261a, 261b, and 260 are arranged in a straight line, the length is approximately 0.1 to 1 mm. In other words, the distance from the electrode 103 of the solid-state imaging element 10 to the terminal of the capacitor 609 can be approximately 0.2 to 2 mm, and the inductance of this wiring can be suppressed to approximately 0.2 to 2 nH. This value is sufficiently smaller than the wiring inductance when the printed circuit board on which the solid-state imaging element is mounted and the board on which the electronic components are mounted are different, as in Patent Document 1 and Patent Document 3.
[0033] In this embodiment, it is preferable to arrange the electronic components so that they do not overlap the projected area of the internal terminal 25 onto the outer surface 201 and the projected area of the electrode 103 onto the outer surface 201. This is because it is necessary to perform wire bonding with a part of a heated metal stage in contact with the projected area of the internal terminal 25 onto the outer surface 201 and the projected area of the electrode 103 onto the outer surface 201 in order to reliably perform ultrasonic thermocompression bonding at a stable temperature.
[0034] The printed circuit board 20 may have a central region that is recessed from the peripheral region surrounding the central region, i.e., a concave shape. Also, as shown in Fig. 2(c), a solder resist layer 230 is formed on the surface, and it is preferable that the solder resist layer 230 has openings formed by patterning as necessary.
[0035] In FIG. 2, the resin frame 40 completely covers the outer edge 205 of the printed circuit board 20. When the outer edge 205 is formed by a general router process using an end mill, foreign matter consisting of glass fibers, fillers, and resins in the prepreg constituting the printed circuit board adheres to the surface of the outer edge 205. It is difficult to completely remove the foreign matter by cleaning. If these foreign matters scatter and adhere to the main part 11 of the solid-state imaging element 10 during the manufacturing process of the imaging element module 1, the possibility of failure in the electrical characteristic test increases, and undesirable results may occur. Therefore, it is effective to completely cover the outer edge 205 of the printed circuit board 20 with the resin frame 40 in order to increase the yield. Such a resin frame 40 can be made by insert molding the printed circuit board 20 into a mold in which a predetermined shape of the resin frame 40 is engraved, as described in Patent Document 3. In this case, it is preferable to engrave a relief portion for the electronic components on the surface of the mold that abuts against the outer surface 201 so that the electronic components do not hit the mold and are crushed.
[0036] The material of the resin frame 40 preferably has the strength and shape stability required for the imaging element module. In addition, the resin frame 40 preferably does not contain halogens that adversely affect the solid-state imaging element under the usage environment of the imaging element module, or substances that dissolve in moisture over a long period of time and migrate to the inner surface 302 of the light-transmitting member 30 and precipitate. For example, thermoplastic resins such as polyethylene resin, polypropylene resin, ethylene-vinyl acetate resin, polystyrene, AS resin, ABS resin, acrylic resin, polyvinyl chloride, cellulose-based resin, polyacetal, polyamide, polyethylene terephthalate, polybutylene terephthalate, polycarbonate, modified polyphenylene ether, polyphenylene sulfide, polyether ether ketone, liquid crystal polymer, polysulfone, polyether sulfone, polyarylate, polyamide imide, polyether imide, and polymethylpentene can also be used. Note that thermosetting resins are preferable in order to stably maintain strength and shape over a wide temperature range from -400°C to 130°C. As the thermosetting resin, phenol resin, urea resin, melamine resin, diallyl phthalate resin, unsaturated polyester resin, polyimide resin, urethane resin, etc. can also be used, but those mainly composed of epoxy resin are preferable. In particular, those based on bisphenol A or novolac glycidyl ether type resin, mixed with aromatic amine hardener, phenol resin hardener or acid anhydride hardener, and filler are preferable.
[0037] Fillers containing silica powder, talc, etc. at about 70 to 85% by weight are preferred because they cause little dimensional change after molding. It is also preferred to add a release agent or flame retardant to improve releasability from the mold.
[0038] FIG. 3 is a plan view of an image sensor module 1 as a modification of the present embodiment. In detail, FIG. 3(a) is a plan view of the front side of the image sensor module 1, FIG. 3(b) is an enlarged view of part A, and FIG. 3(c) is a plan view of the back side of the image sensor module 1. FIG. 4 is a cross-sectional view of the image sensor module 1 as a modification of the present embodiment. In detail, FIG. 4(a) is a cross-sectional view of the image sensor module 1 taken along line IV-IV' in FIG. 3(a), FIG. 4(b) is an enlarged view of part C in FIG. 4(a), and FIG. 4(c) is an enlarged view of part D in FIG. 4(b). Each figure shows the X direction, the Y direction, and the Z direction. Hereinafter, the image sensor module 1 as a modification will be described with reference to each drawing, with the same or similar configurations being given common reference symbols.
[0039] 4, the resin frame 40 does not cover the outer edge 205 of the printed circuit board 20. Therefore, if the outer edge 205 of the printed circuit board is processed by the above-mentioned router processing, a decrease in yield due to adhesion of foreign matter to the main part 11 of the solid-state imaging element 10 becomes an issue. However, by processing the outer edge 205 by wet dicing, it is possible to avoid the decrease in yield to some extent.
[0040] In the modified example, the same materials as those described above in the present embodiment can be used. The resin frame can be formed by transfer molding as in the first example, but in this example, injection molding or compression molding may also be used. In this example, the resin frame 40 is molded as a single body and fixed on the inner surface 202 of the printed circuit board 20 via an adhesive 501. The resin used for this adhesive fixation preferably has the strength and shape stability required for the image sensor module, similar to the resin frame 40. In addition, it is preferable that the resin frame 40 does not contain halogens that adversely affect the solid-state image sensor in the usage environment of the image sensor module, or substances that dissolve in moisture over a long period of time and migrate to the inner surface 302 of the light-transmitting member 30 and precipitate. For example, a thermosetting epoxy resin is suitable, and may contain a filler, a coupling agent, and a flame retardant in an appropriate amount.
[0041] 2 and 4, the resin frame 40 may surround only the solid-state imaging element 10 without surrounding the internal space 510 by reducing the distance between the solid-state imaging element 10 and the light-transmitting member 30 or by providing a frame portion on the light-transmitting member 30. In other words, it is sufficient that the resin frame 40 surrounds at least one of the internal space 510 and the solid-state imaging element 10.
[0042] The light-transmitting member 30 faces the solid-state imaging element 10 and has a function of protecting the solid-state imaging element 10. The light-transmitting member 30 is required to be transparent to light (typically visible light) having a wavelength to which the solid-state imaging element 10 is sensitive. Preferred materials for such a light-transmitting member 30 include plastic, glass, quartz, and the like. Note that, as described below, when the light-transmitting member 30 is attached to the resin frame 40, quartz can efficiently suppress warping of the solid-state imaging element 10. For this reason, it is preferable to use quartz as the light-transmitting member 30. An anti-reflection coating and an infrared cut coating may be formed on the surface of the light-transmitting member 30.
[0043] The light-transmitting member 30 is bonded to the resin frame 40 via an adhesive 503. The solid-state imaging element 10 and an internal space 510 are located between the central region of the printed circuit board 20 and the central region of the light-transmitting member 30. In this embodiment, the light-transmitting member 30 is located farther from the solid-state imaging element 10 and the printed circuit board 20 in the Z direction than the resin frame 40, and the adhesive 503 is provided on an inner surface 302 of the light-transmitting member 30 that faces the solid-state imaging element 10. However, as shown in FIG. 3 of JP-A-2003-101042, a part of the resin frame 40 may be disposed farther from the solid-state imaging element 10 and the printed circuit board 20 in the Z direction than the light-transmitting member 30, and the adhesive 503 may be provided on an outer surface 301 of the light-transmitting member 30.
[0044] The thickness of the adhesives 501, 502, and 503 may be, for example, 1 to 1000 μm, typically 10 to 100 μm. In the first example, the resin frame 40 and the printed circuit board 20 are directly joined, and in the modified example, the resin frame 40 and the printed circuit board 20 are bonded using the adhesive 501. The solid-state imaging element 10 and the printed circuit board 20 are bonded using the adhesive 502, and the light-transmitting member 30 and the resin frame 40 are bonded using the adhesive 503. The order of these bonding processes is not particularly limited, but it is preferable that the resin frame 40 and the printed circuit board 20 are bonded prior to the bonding of the light-transmitting member 30 and the resin frame 40. It is also preferable that the resin frame 40 and the printed circuit board 20 are bonded prior to the bonding of the solid-state imaging element 10 and the printed circuit board 20. That is, the resin frame 40 and the printed circuit board 20 are bonded together first, and the imaging element package 50 is formed. After the solid-state imaging element 10 is fixed to the imaging element package 50 , the light-transmitting member 30 is adhered to the imaging element package 50 .
[0045] The printed circuit board 20 and the resin frame 40 are preferably bonded together at the entire circumference of the bonding surfaces of the printed circuit board 20 and the resin frame 40 directly or by an adhesive 501. The light-transmitting member 30 and the resin frame 40 are also preferably bonded together at the entire circumference of the bonding surfaces by an adhesive 503. In this way, by making the entire circumference of the peripheral regions of the printed circuit board 20 and the light-transmitting member 30 into the bonding region, the internal space 510 around the solid-state imaging element 10 can be made airtight against the outside air. As a result, it is possible to suppress the intrusion of foreign matter into the internal space 510 and improve reliability. It is preferable to use a sufficient amount of adhesive to ensure airtightness.
[0046] The above-mentioned adhesives 501, 502, and 503 are each formed by applying and solidifying the adhesive. The types of adhesives include a dry-curing type that is cured by evaporation of a solvent, a chemical reaction type that is cured by polymerization of molecules by light or heat, and a hot melt type that is cured by solidifying a molten adhesive. Typical adhesives include a photocurable resin that is cured by ultraviolet light or visible light, and a thermosetting resin that is cured by heat. Thermosetting resins can be suitably used for the adhesives 501 and 502, and a photocurable resin can be suitably used for the adhesive 503. The color of the adhesive can be white, black, transparent, or the like, without any particular limitation, in the case of a thermosetting resin. Photocurable resins are transparent to visible light and ultraviolet light. The adhesive may contain an appropriate amount of inorganic or organic filler. The moisture resistance can be improved by including a filler. The elastic modulus of the adhesive after curing is not limited, but in the case of bonding different materials, a range of 1 MPa to 100 GPa is suitable. However, the elastic modulus is not limited to this value. As described later, when a large-sized solid-state imaging element 10 such as an APSC size or a FULL size is used, the difference in linear expansion with the printed circuit board 20 can be absorbed by using an adhesive having rubber elasticity. In this case, the elastic modulus is preferably 1 to 100 MPa.
[0047] The resin frame 40 has a joint surface 401 facing the printed circuit board 20 and directly bonded to the printed circuit board 20 or bonded to an adhesive 501, and a joint surface 402 facing the light-transmitting member 30 and bonded to an adhesive 503. The resin frame 40 is provided so as to surround an internal space 510 between the solid-state imaging element 10 and the light-transmitting member 30. In the resin frame 40, a surface that faces the internal space 510 and surrounds the internal space 510 is an inner edge 403. An outer edge 405 of the resin frame 40 is exposed to the external space. The resin frame 40 in FIG. 1 and FIG. 3 has an extension portion 404 that extends from between the printed circuit board 20 and the light-transmitting member 30 toward the external space in the Y direction. In the modified example in FIG. 3, the extension portion 404 is provided with a through hole 406, and the through hole 406 can be used as a screw hole for fixing to a housing of an electronic device or the like, or as a positioning hole. The electronic devices include imaging devices such as still cameras and video cameras, and information terminals with imaging functions.
[0048] In order to increase the airtightness of the internal space 510, it is preferable that the resin frame 40 surrounds the internal space 510 without any gaps. In addition, in order to ensure the rigidity of the resin frame 40 and therefore the rigidity of the imaging element module 1, it is preferable that the resin frame 40 is a closed loop without any breaks. In addition, as described later, in order to ensure thermal conductivity, it is preferable that the resin frame 40 is a closed loop that is continuous in the circumferential direction. However, due to manufacturing constraints, the resin frame 40 may be formed by dividing each side into a plurality of parts. In addition, slits may be provided in the resin frame 40 to communicate the internal space 510 with the external space. In the case where a break is present in the resin frame 40 in this way, it is preferable that the discontinuous parts (slits) generated in the resin frame 40 are as few as possible, and specifically, it is preferable that the break is less than 10% of the circumferential length surrounding the internal space 510 and the solid-state imaging element 10. That is, when the resin frame 40 exists along the circumference surrounding the internal space 510 and the solid-state imaging element 10, over 90% or more of the circumferential length, the resin frame 40 can be considered to surround the internal space 510 and the solid-state imaging element 10. For example, when the inner edge 403 is a rectangle of 20 mm in length and 20 mm in width, and the circumferential length of the inner edge 403 is 80 mm, if the width of the slits provided in the resin frame 40 is less than 8 mm in total, the resin frame 40 can be considered to surround the internal space 510. Even in this case, it is preferable that the width of each slit is small. For example, it is more preferable to provide two slits of 4 mm in width than to provide one slit of 8 mm in width.
[0049] In this embodiment, the resin frame 40 and the printed circuit board 20 are bonded together using an adhesive, and therefore this embodiment is suitable for cases in which the material of the resin frame 40 is different from the material of the printed circuit board 20. This embodiment is also suitable for cases in which the material of the resin frame 40 is different from the material of the light-transmitting member 30.
[0050] The resin frame 40 has a function of defining the distance between the solid-state imaging element 10 and the light-transmitting member 30, and supporting the light-transmitting member 30. The resin frame 40 may also have holes for screwing or positioning as described above.
[0051] Next, a method for manufacturing the imaging element package 50 and the imaging element module 1 according to the first embodiment will be described. Figures 5A and 5B are diagrams showing the method for manufacturing the imaging element package 50 and the imaging element module 1 according to the first embodiment, and show a cross section taken along line II-II' in Figure 1(a).
[0052] 5A(a), first, a printed circuit board 20 is prepared. Internal terminals 25, internal wiring 26, and external terminals 27 are formed on the printed circuit board 20. The internal terminals 25 are provided on an inner surface 202 of the printed circuit board 20, and the external terminals 27 are provided on an outer surface 201 of the printed circuit board 20. Such a printed circuit board 20 is formed, for example, as follows.
[0053] The printed circuit board 20 has a cross-sectional structure shown in the enlarged view of part D in FIG. 2, and is formed by a so-called multi-layer build-up board construction method. In the multi-layer build-up board construction method, first, conductor layers 211a, 211b are formed on both sides of an insulating layer 220 made of prepreg, which serves as a core, to prepare a double-sided board. Next, vias are formed at predetermined positions using a drill, and internal wiring 260 is formed by metal plating. Next, the conductor layers 211a, 211b are patterned into a desired pattern by lithography. This completes the double-sided board.
[0054] Furthermore, an insulating layer 221a and a conductor layer 212a are formed in order on the upper surface of the double-sided substrate, and an insulating layer 221b and a conductor layer 212b are formed in order on the lower surface of the double-sided substrate. Next, vias are formed again at predetermined positions using a laser. Furthermore, internal wiring 261a and 261b are formed in the laser vias by plating, and necessary locations are connected to the conductor layers 211a and 211b. The conductor layers 212a and 212b are also patterned into a desired pattern by lithography, similar to the conductor layers 211a and 211b. Thereafter, insulating layers 222a and 222b, conductor layers 213a and 213b are formed in the same manner, and insulating layers 223a, 223b, and conductor layers 214a and 214b are formed. Finally, a solder resist layer 230 is formed, and desired openings are formed by lithography.
[0055] FIG. 5A(b) shows a process of mounting electronic components 600 on the outer surface 201 of the printed circuit board 20. The electronic components 600 are soldered to the outer surface 201 of the printed circuit board 20 by a surface mounting method. First, a printing mask having openings that match the arrangement of the external terminals 27 provided on the outer surface 201 of the printed circuit board 20 is prepared. Next, the printing mask is abutted on the outer surface 201 so that the openings and the external terminals 28 match. In this state, solder paste is placed on the mask, and the solder paste is printed on the outer surface 201 using a squeegee. Next, the desired electronic components 600 are mounted on the outer surface 201 using a mounter so that the external terminals 27 match the terminals of each electronic component 600. The electronic components 600 may include a power supply IC 608, a capacitor 609, and the like, as described above. The printed circuit board 20 on which the electronic components 600 are mounted passes through a reflow furnace to complete the soldering between the external terminals 27 and the terminals of each electronic component 600. If the flux contained in the solder paste comes off the printed circuit board 20 in a later process and adheres to the solid-state imaging element 10, it may cause a decrease in yield. Therefore, it is desirable to wash away the flux using a cleaning machine and cleaning solution.
[0056] FIG. 5A(c) shows a process of inserting the printed circuit board 20 into a mold to mold the resin frame 40. The upper mold 4001 abuts against a part of the inner surface 202, and the lower mold 4002 abuts against the vicinity of the outer edge 205 of the outer surface 201, thereby forming closed spaces 4003, 4004, and 4005. The closed space 4003 is connected to a gate, a runner, a cull, and a pod (not shown). The mold is preheated to a temperature equal to or higher than the glass transition temperature Tgf of the resin frame 40. The resin forming the resin frame 40 is prepared in advance as a tablet in which desired materials such as a main component, a hardener, a mold release agent, a coupling agent, and a flame retardant are mixed in a powder state and solidified into a cylindrical shape. The tablet is put into the aforementioned pod, and is pressed into only the closed space 4003 of the mold by applying pressure through the cull, runner, and gate. After a curing time determined by the properties of the resin has elapsed, the mold is opened, and the image pickup device package 50 shown in Fig. 5A(d) is taken out. The closed space 4004 is provided so that the lower mold 4002 does not come into contact with the electronic component 600 and damage the electronic component 600. The closed space 4005 is also provided so as not to damage the internal terminals 25 of the printed circuit board 20. This example is an example of so-called transfer molding, but the molding method may be injection molding, compression molding, or the like.
[0057] FIG. 5B(e) shows a process of fixing the solid-state imaging element 10 on the inner surface 202 of the printed circuit board 20. An adhesive 502 is applied to at least one of the inner surface 202 of the printed circuit board 20 and the back surface 102 of the solid-state imaging element 10, or typically only to the inner surface 202 of the printed circuit board 20. Then, the solid-state imaging element 10 is placed on the adhesive 502. After this, the adhesive 502 is cured to bond the solid-state imaging element 10 and the printed circuit board 20. It is desirable that the adhesive 502 maintains sufficient adhesive strength in the usage environment of the imaging element module 1. In addition, an adhesive that contains a solvent component that exhibits high wettability, and the solvent component bleeds out and contaminates the surface of the internal terminal 25 on the inner surface 202 of the printed circuit board 20 is not preferable as an adhesive. Furthermore, an adhesive that contains halogen and is corrosive to semiconductor wiring, or a cured product that contains a volatile component and dissolves in condensation water generated on the inner surface 302 of the light-transmitting member 30, thereby contaminating the inner surface 302, is also not preferable. Generally, epoxy, which is hard and has high strength, is used as the adhesive. In this embodiment, it is preferable to use an adhesive having rubber elasticity in order to absorb the difference in linear expansion between the large solid-state imaging element 10 of APSC size or FULL size and the printed circuit board 20. A particularly suitable elastic modulus is 1 to 100 MPa. The adhesive 502 may be bonded to the entire surface or a part of the back surface 102 of the solid-state imaging element 10. The adhesive 502 may also be bonded to a part of the outer edge 105 of the solid-state imaging element 10.
[0058] 5B(f) shows a process for electrically connecting the solid-state imaging element 10 and the printed circuit board 20. In this example, wire bonding connection is used. One end of the metal wire supplied from the tip of the capillary 345 is connected to the electrode 103, and then the other end of the metal wire is connected to the internal terminal 25. In this manner, the connection conductor 104 is formed by the metal wire. When flip-chip connection is employed, the bump can serve as both the adhesive 502 and the connection conductor 104.
[0059] Fig. 5B(g) shows a step of bonding the light-transmitting member 30 to the resin frame 40. Fig. 5B(g) shows the image sensor module 1 after all of the internal terminals 25 and all of the electrodes 103 have been connected by the connection conductors 104.
[0060] An adhesive 503 is applied to at least one of the joint surface 402 of the resin frame 40 and the inner surface 302, which is the joint surface of the light-transmitting member 30. As described above, the typical adhesive 503 is a photocurable resin. The adhesive 503 can be applied by a printing method, a dispensing method, or the like. Next, the light-transmitting member 30 is placed on the resin frame 40. At this point, the adhesive 503 is liquid. Therefore, the light-transmitting member 30 is pressed against the resin frame 40 by its own weight or pressure, and excess adhesive 503 may overflow from between the resin frame 40 and the light-transmitting member 30. After that, the applied adhesive 503 is solidified by an appropriate method. As a result, the liquid adhesive 503 becomes a solid adhesive 503, and the resin frame 40 and the light-transmitting member 30 are bonded via the adhesive 503.
[0061] In the case where the adhesive 503 is formed on the entire circumference of the joint surface, if a thermosetting adhesive is used as the adhesive 503, the internal space 510 may thermally expand when heated, and the adhesive 503 in a liquid state may be pushed out due to internal pressure. In this embodiment, by using a photocurable resin as the adhesive 503, such leaching of the adhesive 503 can be prevented. Note that after the photocurable adhesive is semi-cured by photocuring, thermal curing can be used as an auxiliary post-curing. In order to suitably use the photocurable adhesive 503, it is preferable that the light-transmitting member 30 has sufficient light transmittance for wavelengths to which the adhesive 503 reacts, such as ultraviolet light.
[0062] In this manner, the imaging element package 50 and the imaging element module 1 according to the present embodiment can be manufactured.
[0063] Next, a method for manufacturing the imaging element package 50 and the imaging element module 1 according to a modified example of this embodiment will be described. FIG. 6 shows a method for manufacturing the imaging element package 50 according to the modified example. FIG. 6(a) shows a process corresponding to FIG. 5A(c), and FIG. 6(b) shows a process corresponding to FIG. 5A(d). The imaging element package 50 in this embodiment is obtained by adhering a resin frame 40, which is separately manufactured, to the inner surface 202 of the printed circuit board 20. FIG. 6(a) shows a process for applying an adhesive 501 onto the inner surface 202 of the printed circuit board 20. Here, a resin frame 40 molded in advance is prepared.
[0064] It is preferable that unevenness is formed on the surface of the resin frame 40 by sandblasting. An adhesive 501 is applied to at least one of the inner surface 202 of the printed circuit board 20 and the joining surface 401 of the resin frame 40. The adhesive 501 is typically a thermosetting resin. The adhesive 501 can be applied by a printing method, a dispensing method, or the like.
[0065] Next, the resin frame 40 is placed on the inner surface 202 of the printed circuit board 20. At this point, the adhesive 501 is liquid. When the resin frame 40 is pressed against the printed circuit board 20 by its own weight or pressure, excess adhesive 501 may overflow from between the resin frame 40 and the printed circuit board 20. However, it is desirable that the outer edge 405 of the resin frame 40 shown in FIG. 6(b) is larger than the outer edge 205 of the printed circuit board 20 so that the overflowing adhesive 501 does not hang down.
[0066] Next, the adhesive 501 is solidified by an appropriate method. A suitable adhesive 501 is a thermosetting resin, which is thermally cured by heating at about 80 to 200°C. As a result, the liquid adhesive 501 becomes solid, and the resin frame 40 and the printed circuit board 20 are bonded via the adhesive 501. Furthermore, after thermal curing, the resin frame 40 and the printed circuit board 20 are cooled to a predetermined temperature (for example, room temperature). The cooling method is not particularly limited, and may be natural cooling or forced cooling using air cooling or the like. In this manner, the imaging element package 50 including the resin frame 40 and the printed circuit board 20 can be manufactured. From the imaging element package 50 in this embodiment, it is possible to manufacture the imaging element module 1 of the modified example shown in FIG. 3 by a method similar to the manufacturing method of FIG. 5A and FIG. 5B.
[0067] Next, the linear expansion coefficient αc of the solid-state imaging element 10, the linear expansion coefficient αPCB of the printed circuit board 20, the linear expansion coefficient αf of the resin frame 40, and the linear expansion coefficient αL of the light-transmitting member 30 in this embodiment will be described.
[0068] The solid-state imaging device 10 is mainly made of a silicon wafer. Therefore, the rate of thermal expansion and contraction during heating or cooling can be regarded as the linear expansion coefficient of crystalline silicon. Since crystalline silicon has anisotropy, strictly speaking, it shows different linear expansion coefficients depending on the direction of the crystal axis, but in this embodiment, the anisotropy can be ignored. Therefore, the linear expansion coefficient αc of the solid-state imaging device 10 can be 3 to 4 ppm / °C.
[0069] As shown in the enlarged view of part D in FIG. 2 and FIG. 4, the printed circuit board 20 includes at least a plurality of conductor layers and an insulating layer between the conductor layers. Generally, copper is used for the conductor layers. The printed circuit board 20 of this embodiment uses a prepreg. The prepreg is a cloth formed by weaving or knitting fibers and impregnated with resin. The fibers are glass fibers. Epoxy is mainly used as the resin. The resin may contain organic or inorganic fillers, hardeners, coupling agents, flame retardants, pigments, etc. The printed circuit board 20 may also have a solder resist layer 230. As shown in FIG. 2 and FIG. 4, the printed circuit board 20 has a multilayer structure consisting of a plurality of layers parallel to the XY plane.
[0070] Since the printed circuit board 20 has a multi-layer structure, there are many parameters that affect the in-plane linear expansion coefficient of the printed circuit board 20. However, the main influential parameters are the thickness of the conductor layer, the residual rate of the conductor layer after patterning (ratio of projected area onto the XY plane before and after patterning), the number of conductor layers, the linear expansion coefficient of the conductor, the elastic modulus of the conductor, the thickness and number of layers of the prepreg, the linear expansion coefficient of the prepreg in the in-plane direction, and the bending elastic modulus of the prepreg in the Z-axis direction. By adjusting these, the linear expansion coefficient αPCB of the printed circuit board 20 in the in-plane direction is determined.
[0071] When the conductor layer is made of copper, the coefficient of linear expansion of the conductor layer is about 17 ppm / ° C., and the modulus of elasticity is 100 to 120 GPa.
[0072] The linear expansion coefficient of the prepreg is anisotropic depending on the direction of the fibers of the cloth contained therein. When the prepreg includes a cloth woven with X-direction fibers and Y-direction fibers, the linear expansion coefficient is small in the X and Y directions. On the other hand, in the Z-axis direction perpendicular to the fibers, the linear expansion coefficient is relatively large. When the number density of the cloth is different in the X and Y directions, the linear expansion coefficient is different in the X and Y directions. The linear expansion coefficient changes depending on the type of resin impregnated into the cloth, the type of filler, and the amount of filler added. When the prepreg is glass epoxy, the linear expansion coefficient in the in-plane direction of the XY plane is 0.5 to 30 ppm / °C. On the other hand, the linear expansion coefficient in the Z direction is 1 to 300 ppm / °C. The bending elastic modulus of the prepreg in the Z-axis direction is 3 to 100 GPa.
[0073] The solder resist layer 230 has a linear expansion coefficient of 1 to 300 ppm / °C. Also, the elastic modulus is 100 MPa to 10 GPa. The solder resist layer 230 generally has a thickness of 4 to 30 μm, which is thin compared to the total thickness of the printed circuit board. Therefore, the contribution of the solder resist layer 230 to the αPCB is small.
[0074] The prepreg has a glass transition temperature Tgp, which is approximately the glass transition temperature of the resin to be impregnated. The linear expansion coefficient of the prepreg in the in-plane direction differs at temperatures higher than the glass transition temperature Tgp and at temperatures lower than the glass transition temperature Tgp. At temperatures higher than the glass transition temperature Tgp, the linear expansion coefficient is a large value. Therefore, the linear expansion coefficient αPCB in the in-plane direction of the printed circuit board 20, which is a multilayer body including the prepreg, also shows different values at temperatures higher than the glass transition temperature Tgp and at temperatures lower than the glass transition temperature Tgp. The linear expansion coefficient at temperatures lower than the glass transition temperature Tgp is denoted as αPCB1, and the linear expansion coefficient at temperatures higher than the glass transition temperature Tgp is denoted as αPCB2.
[0075] The resin frame 40 is a mixture of resin and filler as described above. Therefore, the linear expansion coefficient of the resin frame 40 is determined by the linear expansion coefficient of the resin, the elastic modulus of the resin, the linear expansion coefficient of the filler, the size of the filler, the filling rate of the filler, and the elastic modulus of the filler. The resin frame 40 also has a glass transition temperature Tgf. The glass transition temperature Tgf of the resin frame 40 is approximately the glass transition temperature of the resin contained in the resin frame 40. However, when the filler contains an organic filler, the glass transition temperature of the filler affects the glass transition temperature of the resin frame 40. The linear expansion coefficient of the resin frame 40 differs at temperatures higher and lower than the glass transition temperature Tgf. At temperatures higher than the glass transition temperature Tgf, the linear expansion coefficient is a large value. The linear expansion coefficient at a temperature lower than the glass transition temperature Tgf is αf1, and the linear expansion coefficient at a temperature higher than the glass transition temperature Tgf is αf2.
[0076] As described above, resin, glass, sapphire, quartz, etc. can be used as the light-transmitting member 30. Examples of resin include acrylic resin and polycarbonate resin. The linear expansion coefficient of these materials is 50 to 100 ppm / °C. The linear expansion coefficient of glass and sapphire is 1 to 10 ppm / °C. As glass, borosilicate glass and quartz glass are suitable. Crystalline members such as sapphire and quartz have different values of linear expansion coefficient in the direction of the crystal axis and in the direction perpendicular to the crystal axis. The linear expansion coefficient of sapphire in the crystal axis direction is 7.7 ppm / °C, and the linear expansion coefficient in the direction perpendicular to the crystal axis is 7 ppm / °C, and the difference between the two values is small. However, the linear expansion coefficient of quartz in the crystal axis direction is 8 ppm / °C, while the linear expansion coefficient in the direction perpendicular to the crystal axis is 13.4 ppm / °C, which is a relatively large difference. In the case of quartz, it is possible to attach it to the resin frame 40 as a component of a so-called optical low-pass filter. In this case, the crystal axis of the quartz crystal needs to be tilted 45 degrees from the Z direction. In this case, the linear expansion coefficient αL of the light-transmitting member 30 in the in-plane direction is 10 to 13.4 ppm / °C.
[0077] The linear expansion coefficients can be measured by thermal mechanical analysis (TMA). The linear expansion coefficients of multilayer materials such as the printed circuit board 20 or anisotropic members can also be measured using a dilatometer in accordance with ASTM D696. Furthermore, the dimensional change of the sample can be measured directly using a camera. The linear expansion coefficient can be measured by holding the sample in a constant temperature chamber and using a camera to measure the linear expansion coefficient by digital image correlation (DIC).
[0078] Fig. 7 shows the relationship between the linear expansion coefficients of the members in the first embodiment. In Fig. 7, the horizontal axis represents the temperature of the members, and the vertical axis represents the elongation per unit length of each member when the elongation of the member at room temperature To is set to zero. That is, Fig. 7 shows a graph in which the elongation per unit length of each member is plotted at each temperature. The slope of the graph represents the linear expansion coefficient of the member, and the temperature at the point where the graph bends represents the glass transition point of the member.
[0079] For example, the graph for the resin frame bends at temperature Tgf, so the glass transition temperature of the resin frame is Tgf. The slope of the graph below the glass transition temperature Tgf indicates the linear expansion coefficient αf1 of the resin frame below the glass transition temperature Tgf. The slope of the graph above the glass transition temperature Tgf indicates the linear expansion coefficient αf2 of the resin frame above the glass transition temperature Tgf.
[0080] In FIG. 7, the graph of the printed circuit board 20 in the first embodiment is labeled as printed circuit board A and is bent at the glass transition temperature Tgp. Therefore, the glass transition temperature of the printed circuit board 20 is the temperature Tgp. The slope of the graph below the glass transition temperature Tgp indicates the linear expansion coefficient αPCB1 in the in-plane direction of the printed circuit board 20 below the glass transition temperature Tgp. The slope of the graph above the glass transition temperature Tgp indicates the linear expansion coefficient αPCB2 in the in-plane direction of the printed circuit board 20 above the glass transition temperature Tgp. Note that the room temperature To means a normal room temperature, which is 20 to 30° C., and is 25° C. on average. In the first embodiment, it is desirable that the glass transition temperatures Tgp, Tgf, To, the linear expansion coefficients αf1, αf2, αPCB1, and αPCB2 satisfy the following formulas. Tgp>Tgf, and αf1<αPCB1, and (Tgp-To)×αPCB1<(Tgf-To)×αf1+(Tgp-Tgf)×αf2
[0081] By satisfying the above formula, as shown in FIG. 7, the graph of the printed circuit board 20 (printed circuit board A) and the graph of the resin frame 40 have an intersection point. The temperature at the intersection point is Tc. FIG. 10(a) shows a state in which the resin frame 40 and the printed circuit board 20 are fixed at temperature Tm. When the printed circuit board 20 is inserted into the above-mentioned mold for molding, FIG. 10(a) shows a state in which the integrated printed circuit board 20 and resin frame 40 are removed from the mold at temperature Tm. In this state, the printed circuit board 20 and the resin frame 40 are flat.
[0082] Fig. 10(b) shows a state in which the printed circuit board 20 has been cooled from temperature Tm to temperature Tc. According to the graph in Fig. 7, the linear expansion coefficient of the resin frame 40 is higher than that of the printed circuit board 20 between temperature Tm and temperature Tc. Therefore, in the process of cooling from temperature Tm to temperature Tc, the resin frame 40 shrinks more than the printed circuit board 20. Therefore, as shown in Fig. 10(b), at temperature Tc, the printed circuit board 20 and the resin frame 40 are warped in a concave shape.
[0083] Furthermore, FIG. 10(c) shows a state in which the printed circuit board 20 is cooled from temperature Tc to temperature (room temperature) To. Similarly, according to the graph in FIG. 7, when comparing the linear expansion coefficient of the resin frame 40 and the linear expansion coefficient of the printed circuit board 20 between temperature Tc and room temperature To, the printed circuit board 20 is higher. Therefore, in the process of cooling from temperature Tc to room temperature To, the printed circuit board 20 shrinks more than the resin frame 40. Therefore, as shown in FIG. 10(c), at room temperature To, the printed circuit board 20 and the resin frame 40 return to flat again. At this time, in order to return to a flatter state, it is preferable that the area of the region i between the graph of the printed circuit board 20 (printed circuit board A) and the graph of the resin frame 40 between temperature Tc and temperature Tm in the graph in FIG. 7 is equal to the area of the region ii between the graph of the printed circuit board 20 (printed circuit board A) and the graph of the resin frame 40 between room temperature To and temperature Tc. The value obtained by integrating the graph of the linear expansion coefficient of a material within a given temperature range indicates the amount of shrinkage of the material within that temperature range. Therefore, if the area of region i is equal to the area of region ii, the amount of shrinkage of printed circuit board 20 and the amount of shrinkage of resin frame 40 between temperature Tm and room temperature To will be equal. This makes it possible to suppress deformation of printed circuit board 20 and resin frame 40 due to temperature changes.
[0084] If the linear expansion coefficient in the in-plane direction of the printed circuit board 20 is the value of the graph shown for the printed circuit board B in FIG. 7, the linear expansion coefficient of the printed circuit board B is always lower than the linear expansion coefficient of the resin frame during the period from temperature Tm to room temperature To. Therefore, in the process of cooling from temperature Tm to room temperature To, the resin frame 40 shrinks more than the printed circuit board 20. As a result, at room temperature To, the printed circuit board 20 and the resin frame 40 are significantly deformed into a concave shape, and when assembling a solid-state imaging element module, the workpiece is not sufficiently adsorbed and fixed to the workpiece stage in the assembly device, resulting in a problem of reduced assembly accuracy. Furthermore, problems such as a decrease in the operation rate of the device and a decrease in yield rate occur.
[0085] In addition, when the linear expansion coefficient in the in-plane direction of the printed circuit board 20 is the value of the graph shown for the printed circuit board C in FIG. 7, the linear expansion coefficient of the printed circuit board B always exceeds the linear expansion coefficient of the resin frame 40 during the period from the temperature Tm to the room temperature To. Therefore, in the process of cooling from the temperature Tm to the room temperature To, the printed circuit board 20 shrinks more than the resin frame 40. As a result, at the room temperature To, the printed circuit board 20 and the resin frame 40 are significantly deformed in a convex shape. Therefore, when assembling the image sensor module, the workpiece is not sufficiently adsorbed and fixed to the workpiece stage in the assembly device, causing a problem of reduced assembly accuracy. In addition, problems such as a decrease in the operation rate of the device and a decrease in yield rate occur.
[0086] Figure 8 shows the relationship between the linear expansion coefficients of each component in another example. In Figure 8, like Figure 7, the horizontal axis represents the temperature of the component, and the vertical axis represents the amount of elongation per unit length of each component when the elongation of the component at room temperature To is set to zero. In other words, Figure 8 is a graph plotting the amount per unit length of each component. The slope of the graph is the linear expansion coefficient of that component. The temperature at the point where the graph bends is the glass transition point of that component.
[0087] The graph for the printed circuit board 20 is bent at the temperature Tgp. Therefore, the glass transition temperature of the printed circuit board 20 is the temperature Tgp. The slope of the graph below the temperature Tgp indicates the linear expansion coefficient αPCB1 of the printed circuit board 20 at temperatures below the temperature Tgp. Moreover, the slope of the graph above the temperature Tgp indicates the linear expansion coefficient αPCB2 of the printed circuit board 20 at temperatures above the temperature Tgp.
[0088] In Fig. 8, the graph for the resin frame 40 is shown as resin frame A and is bent at temperature Tgf. Therefore, the glass transition temperature of the resin frame 40 is temperature Tgf. The slope of the graph below temperature Tgf indicates the linear expansion coefficient αf1 of the resin frame 40 below temperature Tgf. Moreover, the slope of the graph above temperature Tgf indicates the linear expansion coefficient αf2 of the resin frame 40 above temperature Tgf. Room temperature To represents normal room temperature, as in Fig. 7.
[0089] In FIG. 8, it is desirable that the temperatures Tgp, Tgf, To, and the linear expansion coefficients αf1, αf2, αPCB1, and αPCB2 satisfy the following formulas. Tgp <Tgf、かつ αPCB1<αf1, and (Tgf-To)×αf1<(Tgp-To)×αPCB1+(Tgf-Tgp)×αPCB2
[0090] By satisfying the above formula, as shown in FIG. 8, the graph of the printed circuit board 20 and the graph of the resin frame 40 (resin frame A) have an intersection point. The temperature at the intersection point is defined as Tc. FIG. 11(a) shows a state in which the resin frame 40 and the printed circuit board 20 are fixed at temperature Ta. In the case where the above-mentioned resin frame 40 is bonded to the printed circuit board 20 via adhesive 501, FIG. 11(a) shows a state in which the integrated printed circuit board 20 and resin frame 40 are taken out from an oven at temperature Ta. In this state, the printed circuit board 20 and resin frame 40 are flat.
[0091] Fig. 11(b) shows a state in which the printed circuit board 20 has been cooled from temperature Ta to temperature Tc. According to the graph in Fig. 8, the linear expansion coefficient of the printed circuit board 20 is higher than that of the resin frame 40 between temperatures Ta and Tc. Therefore, in the process of cooling from temperature Ta to temperature Tc, the printed circuit board 20 shrinks more than the resin frame 40. Therefore, as shown in Fig. 11(b), at temperature Tc, the printed circuit board 20 and the resin frame 40 are warped in a convex shape.
[0092] Furthermore, FIG. 11(c) shows a state in which the printed circuit board 20 is cooled from temperature Tc to room temperature To. Similarly, according to the graph in FIG. 8, the linear expansion coefficient of the resin frame 40 is higher than that of the printed circuit board 20 between temperature Tc and room temperature To. Therefore, in the process of cooling from temperature Tc to room temperature To, the resin frame 40 shrinks more than the printed circuit board 20. Therefore, as shown in FIG. 11(c), the printed circuit board 20 and the resin frame 40 return to flat again at room temperature To. At this time, in order to return the printed circuit board 20 and the resin frame 40 to a flatter state, it is preferable that the area of the region i between the graph of the printed circuit board 20 and the graph of the resin frame 40 (resin frame A) between temperature Tc and temperature Ta in the graph in FIG. 8 is equal to the area of the region ii between the graph of the printed circuit board 20 (printed circuit board A) and the graph of the resin frame 40 between room temperature To and temperature Tc. As in the first embodiment, when the area of region i is equal to the area of region ii, the amount by which the printed circuit board 20 shrinks and the amount by which the resin frame 40 shrinks between temperature Ta and room temperature To are equal. This makes it possible to suppress deformation of the printed circuit board 20 and the resin frame 40 due to temperature changes.
[0093] If the linear expansion coefficient of the resin frame 40 is the value shown in the graph for the resin frame B in FIG. 8, the linear expansion coefficient of the resin frame B is always lower than the linear expansion coefficient of the resin frame during the period from temperature Ta to room temperature To. Therefore, in the process of cooling from temperature Ta to room temperature To, the printed circuit board 20 shrinks more than the resin frame 40. As a result, at room temperature To, the printed circuit board 20 and the resin frame 40 are significantly warped in a convex shape, and when assembling the solid-state imaging element module, the workpiece is not sufficiently adsorbed and fixed to the workpiece stage in the assembly device, resulting in a problem of reduced assembly accuracy. Furthermore, problems such as a decrease in the operation rate of the device and a decrease in yield rate occur.
[0094] Furthermore, when the linear expansion coefficient in the in-plane direction of the resin frame 40 is the value shown in the graph for the resin frame C in FIG. 8, the linear expansion coefficient of the resin frame B always exceeds the linear expansion coefficient of the printed circuit board during the period from temperature Ta to room temperature To. Therefore, in the process of cooling from temperature Ta to room temperature To, the resin frame 40 shrinks more than the printed circuit board 20. As a result, at room temperature To, the printed circuit board 20 and the resin frame 40 are significantly warped in a concave shape, and when assembling the solid-state imaging element module, the workpiece is not sufficiently adsorbed and fixed to the workpiece stage in the assembly device, causing a problem of reduced assembly accuracy. In addition, problems such as a decrease in the operation rate of the device and a decrease in yield may occur.
[0095] In this embodiment, in addition to the room temperatures To, Tgo, Tgf, and the linear expansion coefficients αf1, αf2, αPCB1, and αPCB2 satisfying the above-mentioned conditions, it is preferable that the linear expansion coefficients αPCB1 and αf1 are smaller than the linear expansion coefficient αL of the translucent member 30 in the in-plane direction and larger than the linear expansion coefficient αc of the solid-state imaging element 10 in the in-plane direction.
[0096] The reason will be explained with reference to FIG. 9. Under the above conditions, the linear expansion coefficients αPCB1 and αf1 are not the same but are relatively close to each other. FIG. 9 particularly shows a case where the linear expansion coefficients αPCB1 and αf1 are equal. In FIG. 9, the horizontal axis represents the linear expansion coefficient α, and the vertical axis represents the amount of warping of the light incident surface of the solid-state imaging element 10. Graph 9a represents the amount of warping of the light incident surface when the temperature of the imaging element module is low temperature T1. Graph 9b represents the amount of deformation when the temperature of the imaging element module is high temperature T2.
[0097] In FIG. 9, when the linear expansion coefficient α is the median value of the linear expansion coefficient αc of the solid-state imaging element 10 and the linear expansion coefficient αL of the light-transmitting member 30, it can be confirmed that the amount of surface warping of the solid-state imaging element 10 is constant even if the temperature of the solid-state imaging element module changes from low temperature T1 to high temperature T2. That is, in this case, it is possible to suppress the surface warping of the solid-state imaging element 10 in a wide temperature range. In this embodiment, the linear expansion coefficients αPCB1 and αf1 do not necessarily match, but they are almost close to each other, so it can be seen that the same characteristics as those in FIG. 9 are shown. Therefore, it is preferable that the linear expansion coefficients of each member satisfy the formula αc<αPCB≒αf1<αL. More preferably, it is preferable that αPCB≒αf1≒(αc+αL) / 2 is satisfied.
[0098] The reason for this will be explained with reference to FIG. 12. FIG. 12(a) shows a cross-sectional view of an image sensor module in which the solid-state image sensor 10 is not virtually provided at low temperature T1. In this case, the linear expansion coefficients of the members are αf1≒αPCB1<αL, so the image sensor module is subject to an effect of deforming the cross section in a concave shape. On the other hand, FIG. 12(b) shows a cross-sectional view of an image sensor module in which the light-transmitting member 30 is not virtually provided at low temperature T1. The linear expansion coefficients of the members are Ac<αf1≒αPCB1, so the printed circuit board 20 and the resin frame 40 are subject to an effect of deforming in a convex shape. As shown in FIG. 12(c), in the actual image sensor module as a whole, the effects of FIG. 12(a) and (b) are offset, so no deformation occurs and the cross-sectional shape is kept flat.
[0099] Similarly, FIG. 13(a) shows a cross-sectional view of an image sensor module in which the solid-state image sensor 10 is not provided at a high temperature T2. In this case, the linear expansion coefficients of each member are αf1 ≒ αPCB1 < αL, so the image sensor module is deformed in a convex shape. On the other hand, FIG. 13(b) shows a cross-sectional view of an image sensor module in which the light-transmitting member 30 is not provided at a high temperature T2. The linear expansion coefficients of each member are Ac < αf1 ≒ αPCB1, so the printed circuit board 20 and the resin frame 40 are deformed in a concave shape. As shown in FIG. 13(c), in the actual solid-state image sensor module as a whole, the effects of FIG. 13(a) and (b) are offset, no deformation occurs, and the cross-sectional shape is kept flat.
[0100] As described above, according to this embodiment, an imaging element module that is less likely to deform over a wide temperature range can be obtained.
[0101] It is preferable that the adhesive 502 for bonding the solid-state imaging element 10 to the printed circuit board 20 has rubber elasticity. This is because the effect of the linear expansion coefficient Ac<<αf1≒αPCB1 is mitigated by the stretching of the adhesive 502. Therefore, in this case, it is preferable that αf1≒αPCB1≒<αL.
[0102] According to this embodiment, by configuring the printed circuit board and the resin frame so that their respective deformation amounts due to temperature are offset, it is possible to provide an imaging element module with extremely little warping.
[0103] As described above, in large-sized image sensor modules such as APSC size and FULL size, image sensor packages having solder terminals of LGA (Land Grid Array) type and LCC (Leadless Chip Carrier) type are adopted. Since the wiring interval is once widened to the pitch (0.8 to 1.5 mm) between the solder terminals of the printed circuit board, the wiring length of the wiring from the terminal of the solid-state image sensor to the bypass capacitor, the ground loop, and the power supply loop may become relatively long. In this way, when the inductance of the wiring cannot be ignored, it is necessary to suppress high-frequency noise. In particular, when the ground loop or power supply loop becomes long and the loop area becomes large, the magnetic noise caused by the change in the magnetic field passing through the loop cannot be ignored. The number of pixels of the solid-state image sensor and the number of images taken per unit time are increasing, and the digitalization of the output is progressing, so there is an increasing need to increase the transmission speed of the output signal of the solid-state image sensor. For this reason, high-speed serial transmission such as LVDS (Low Voltage Differential Signalling) and SLVS (Scalable Low Voltage Signalling) is used. In high-speed serial transmission, the signals handled are smaller in amplitude and higher in frequency, so the inductance and loop area of the wiring cannot be ignored. Furthermore, because high-speed transmission signals are transmitted with small amplitudes, it is preferable for the transmission wiring to be impedance-matched and with little power loss, and there is an increasing need to use copper wiring.
[0104] The above-mentioned Patent Document 2 discloses a configuration in which a solid-state imaging element is mounted directly on the front surface of a substrate on which electronic components such as a bypass capacitor, a power supply IC, and a connector are mounted on the back surface, thereby shortening the wiring length from the power input PAD of the serial transmission circuit of the solid-state imaging element to the bypass capacitor, and reducing the inductance of the wiring. Furthermore, with this configuration, since the wiring length can be shortened, the loop area of the power loop and the ground loop can also be kept small. However, in Patent Document 2, when a printed circuit board including copper wiring with less power loss is used by using prepreg for the substrate, the rigidity of the substrate is low, so that the substrate may warp due to the difference in linear expansion coefficient between the materials constituting the imaging element module. In the imaging element module manufacturing process, there may be cases where the transportation and suction fixation of the imaging element module are hindered. In addition, even after the imaging element module is completed, a large warp may occur in the substrate due to a temperature change in the environment in which the imaging element module is used, and further a large warp may occur in the light receiving surface of the solid-state imaging element. In particular, when an APSC-sized or full-sized solid-state imaging element is incorporated into a camera such as a DSLR (Digital Single Lens Reflex) camera, it is necessary to suppress the warpage of the surface of the solid-state imaging element to an extremely small range. For example, it is preferable to suppress the warpage to within 50 μm, and preferably within 25 μm.
[0105] According to the above-described embodiment, by configuring the printed circuit board and the resin frame so that their respective deformation amounts due to temperature are offset, it is possible to provide an image sensor module with extremely little warping, thereby solving the above-described problem. In particular, when a solid-state image sensor is mounted on a printed circuit board made of prepreg, it is possible to suppress to an extremely small range the warping of the light receiving surface of the solid-state image sensor that may occur due to temperature changes in the manufacturing process and the usage environment of the image sensor module.
[0106] [Example 1] An embodiment of the present invention will be described below. The imaging element module 1 shown in FIG. 1, FIG. 2, FIG. 5A, and FIG. 5B was fabricated. First, a printed circuit board 20 was fabricated. The glass transition temperature Tgp of the prepreg used was 220° C. The subtractive method was used. A so-called 2-4-2 8-layer board consisting of two stacked layers of laser vias and four core layers of drill vias was fabricated. The conductors were made of 20 μm thick copper, which was patterned by lithography. The thickness of the insulating layer between the conductors was 250 μm for the core and 50 μm for the others. The internal terminals 25 were patterned on the conductor layer of the inner surface 202, and the solder terminals for mounting electronic components, alignment marks for mounting electronic components, and pad rows 612 for contacting test probes were patterned on the conductor layer of the outer surface 201, and both the outer surface 201 and the inner surface 202 were covered with a solder resist layer 203 with a thickness of 20 μm. The patterning of the conductor layer was adjusted so that the area before patterning was 100 and the area of the portion remaining after patterning was 70. Adjusting the area after patterning of each layer in this manner is preferable for adjusting the linear expansion coefficient α PCB in the in-plane direction of the printed circuit board 20 to a desired value.
[0107] Finally, the internal terminals 25, solder terminals, pads, and other necessary locations were opened by patterning, and then the surface was nickel-plated to 4-100 μm and gold-plated to 0.1-0.8 μm. The total thickness was 720 μm. The produced printed circuit board was an assembly containing four printed circuit boards on one sheet, and the outer shape of each printed circuit board was processed by router processing. For each printed circuit board, several locations were left unprocessed by the router, and the production of the printed circuit board was completed with the four boards remaining in an integrated sheet form.
[0108] After the printed circuit board was produced, the linear expansion coefficient αPCB in the in-plane direction was measured. A known digital image correlation method was used for the measurement. As a result of the measurement, the glass transition temperature Tgp of the printed circuit board was 220°C. In addition, the linear expansion coefficient αPCB1 below the glass transition temperature Tgp was 10 ppm / °C, and the linear expansion coefficient αPCB2 above the glass transition temperature Tgp was 20 ppm / °C.
[0109] Next, solder paste was printed on the solder terminals using a printer, and electronic components were mounted on top of the solder paste using a mounter. The solder paste contains flux, but halogen-free flux was used. The mounted electronic components were a total of 137 items, including ceramic capacitors, tantalum capacitors, chip resistors, power supply ICs, B-to-B connectors, crystal oscillators, PLLs, EPROMs, temperature measurement ICs, and transistors. After mounting each electronic component, the board was passed through a known reflow oven to complete the solder joints.
[0110] Next, a serial number and a data matrix code were printed on the solder resist layer on the outer surface 201 of the printed circuit board 20 using a laser marker. The laser used was YV04 (yttrium vanadium tetroxide). Furthermore, the flux contained in the solder paste was removed using a cleaning machine, a dryer, and a flux cleaning solution.
[0111] Next, a general press machine and a punching die were used to cut the portion of the outer shape of the printed circuit board 20 that had not been router-processed, and the sheet-like printed circuit board was separated into individual pieces of the printed circuit board 20. Next, a resin frame 40 was molded on the printed circuit board 20. First, as shown in FIG. 5A(c), the printed circuit board 20 on which electronic components were mounted was sandwiched and fixed between upper and lower dies. The dies were preheated to 150°C. The dies were provided with a closed space 4003 in which the outer edge 205 of the printed circuit board 20 and the outer periphery of the inner surface 202 were exposed. The closed space 4003 was connected to a gate, a runner, a cull, and a pod, and a tablet containing epoxy as the main component, a hardener, a silica filler, a coupling agent, a flame retardant, and a mold release agent was placed in the pod, and the tablet was pressed with a plunger to fill the closed space 4003 with resin. After filling, the resin was held for 3 minutes to harden the resin. After hardening, the mold was opened, the integrated printed circuit board 20 and resin frame were removed, and unnecessary gates, runners, and subsequent resin were cut off to remove the imaging element package 50. The removed imaging element package 50 was placed in an oven at 150° C. for three hours for post-curing, and the resin frame 40 was finally hardened.
[0112] The glass transition temperature and linear expansion coefficient were measured by a TMA (Thermal Mechanical Analysis) measuring device using a molded product of the resin used. According to the measurement results, the glass transition temperature Tgf was 140°C, the linear expansion coefficient αf1 below the glass transition temperature Tgf was 9 ppm / °C, and the linear expansion coefficient αf2 above the glass transition temperature Tgf was 30 ppm / °C.
[0113] Next, the upper surface 402 of the resin frame 40 of the completed imaging element package 50 was roughened. The roughening was performed by a known method, and the arithmetic mean roughness Ra was 7 to 10 μm. The surface was washed with a pure water washer and dried to complete the imaging element package. The warpage of the die attach surface (the surface to which the solid-state imaging element 10 is fixed) of the completed imaging element package was measured, and found to be about -10 μm. The warpage of the back surface of the imaging element package was also small, being about +10 μm. Here, minus indicates that the cross section is deformed concavely, and plus indicates that the cross section is deformed convexly.
[0114] Next, an imaging element module was assembled. First, in a CMOS wafer process and a color filter process, a plurality of solid-state imaging elements 10 were formed on the surface of a silicon wafer having a diameter of 12 inches and a thickness of 775 μm, and the solid-state imaging elements 10 were diced into individual pieces. Next, the surfaces of the individualized solid-state imaging elements were cleaned to obtain solid-state imaging elements 10 of APSC size. The linear expansion coefficient αc of the solid-state imaging element 10 was 3 ppm / °C. The imaging element package 50 described above was fixed by suction on the suction stage 670 of the die bonder. The part indicated by the arrow in FIG. 5B(e) was sucked with a pump. The central part was not sucked because it was leaking to the atmosphere. The suction vacuum degree during suction was -60 kPa. In this state, a silicone resin having rubber elasticity was applied with a dispenser to the inner surface 202 of the printed circuit board 20 included in the imaging element package 50 and to the central part of the printed circuit board 20. The silicone resin was applied in a linear shape, and three lines of silicone resin were applied in a linear shape long in the X direction of FIG. 5B(e) while being offset in the Y direction. The solid-state imaging element 10 was mounted on the applied silicone resin, and the entire imaging element package was placed in an oven at 120°C. The entire imaging element package 50 was heated in the oven for 50 minutes to harden the silicone resin, and the imaging element package 50 and the solid-state imaging element 10 were fixed to each other. The positional deviation of the fixed solid-state imaging element 10 in the X and Y directions was within 100 μm, and sufficient accuracy was obtained. In addition, the amount of warping of the light incident surface of the solid-state imaging element 10 was measured and found to be +10 μm. As described above, a minus sign indicates a concave deformation, and a plus sign indicates a convex deformation.
[0115] Next, the electrode 103 of the solid-state imaging element 10 was connected to the internal terminal 25 of the printed circuit board 20 using a wire bonder. A gold wire with a diameter of 23 μm was used as the wire. The same suction stage 670 as that of the die bonder was used. Stable processing was performed at a suction vacuum of -67 kPa. Finally, the translucent member 30 was bonded and fixed to the joint surface 402 of the resin frame 40 with an adhesive 503. Here, quartz was used as the translucent member 30. The crystal axis of the quartz was set in a direction tilted 45 degrees in the XZ plane with respect to the Z axis. At this time, the linear expansion coefficient of the quartz in the X direction was 13 ppm / °C, and the linear expansion coefficient in the Y direction was 10 ppm / °C. The quartz used had a thickness of 500 μm, and was chamfered at four corners and eight edges.
[0116] The device was a mounter, and the same stage as that of a die bonder was used as the suction stage. The suction vacuum degree here was also -63 kPa, and stable processing was performed. The adhesive 503 was applied to the joint surface 402 of the resin frame 40 using a known dispenser. A gap was provided during application to allow air to escape. An ultraviolet-curing resin containing epoxy as the main component was used as the adhesive 503. In order to allow the adhesive 503 to absorb the stress generated in proportion to the difference in linear expansion coefficient between the light-transmitting member 30 and the resin frame 40 by distortion, a resin spacer with a diameter of 30 μm was added to the adhesive, and the thickness of the adhesive was adjusted to 30 to 50 μm. Finally, the adhesive 503 was cured by irradiating it with ultraviolet light of 4000 mJ. The elastic modulus of the adhesive 503 used when cured was 5 GPa.
[0117] In this manner, the imaging element module of Example 1 was completed. In the completed imaging element module, the warpage of the solid-state imaging element 10 was measured between -40°C and 60°C, which is the usage environment of the camera. After the light-transmitting member 30 was attached to the resin frame 40, the warpage of the surface of the solid-state imaging element 10 at room temperature was +10 μm, the warpage at -40°C was +20 μm, and the warpage at 60°C was 0 μm, meaning that the warpage could be made sufficiently small. As a result, good results were obtained.
[0118] [Example 2] The following mainly describes the differences from Example 1. In Example 2, the type of prepreg used in the printed circuit board 20 is different from that in Example 1. The completed printed circuit board 20 had a glass transition temperature Tgp of 190°C, a linear expansion coefficient αPCB1 below the glass transition temperature Tgp of 12 ppm / °C, and a linear expansion coefficient αPCB2 above the temperature Tgp of 28 ppm / °C.
[0119] At this time, the warp of the die-attach surface after the resin frame 40 was attached was as small as 0 μm, and a stable suction force was obtained in the die bonder, wire bonder, and light-transmitting member mounter. After the solid-state imaging element 10 was bonded to the imaging element package 50, the warp of the solid-state imaging element 10 was +20 μm. Furthermore, after the light-transmitting member 30 was attached to the resin frame 40, the warp of the solid-state imaging element 10 was +20 μm, which was sufficiently small. Furthermore, the warp of the solid-state imaging element 10 when the imaging element module was kept at -40° C. was +30 μm, and the warp of the solid-state imaging element 10 when kept at 60° C. was +10 μm, so the warp could be made sufficiently small.
[0120] [Example 3] Next, the third embodiment will be described with a focus on differences from the first embodiment. In the third embodiment, borosilicate glass was used as the light-transmitting member 30 instead of quartz. The linear expansion coefficient αL of the borosilicate glass was 7 ppm / °C. At this time, the warp of the die-attach surface after the resin frame 40 was attached was small at -10 μm, and a stable suction force was obtained in the die bonder, wire bonder, and light-transmitting member mounter. The warp of the solid-state imaging element 10 after the solid-state imaging element 10 was bonded to the imaging element package 50 was +10 μm, and the warp of the surface of the solid-state imaging element 10 after the light-transmitting member 30 was attached to the resin frame 40 was +10 μm, which were sufficiently small. In addition, the warp of the surface of the solid-state imaging element 10 when the imaging element module was set at -40°C was +30 μm, and the warp of the surface of the solid-state imaging element 10 when the imaging element module was set at 60°C was -10 μm, both of which were small. However, the amount of change in the warp increased.
[0121] [Example 4] Next, the fourth embodiment will be described with a focus on differences from the second embodiment. In the fourth embodiment, borosilicate glass was used instead of quartz crystal as the light-transmitting member 30. The linear expansion coefficient αL of the borosilicate glass was 7 ppm / °C. At this time, the warp of the die-attach surface after the resin frame 40 was attached was 0 μm, which was small, and a stable suction force was obtained in the die bonder, wire bonder, and light-transmitting member mounter. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was attached to the imaging element package 50 was +20 μm, and the warp of the surface of the solid-state imaging element 10 after the light-transmitting member 30 was attached to the resin frame 40 was +20 μm, which was sufficiently small. In addition, the warp of the surface of the solid-state imaging element 10 when the imaging element module was set at -40°C was +40 μm, and the warp of the surface of the solid-state imaging element 10 when the imaging element module was set at 60°C was 0 μm, both of which were small. However, the amount of change in the warp increased.
[0122] [Example 5] Next, the fifth embodiment will be described with a focus on differences from the first embodiment. In the fifth embodiment, the adhesive 502 for fixing the solid-state imaging element 10 to the printed circuit board 20 was changed from silicone resin to non-rubber-elastic epoxy resin. At this time, the warp of the die-attach surface after the resin frame 40 was attached was small at -10 μm, and a stable suction force was obtained in the die bonder, wire bonder, and translucent member mounter. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was attached to the imaging element package 50 was +20 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was +20 μm, which were sufficiently small. In addition, the warp of the surface of the solid-state imaging element 10 when the imaging element module 50 was set at -40°C was +30 μm, and the warp of the surface of the solid-state imaging element 10 when the imaging element module 50 was set at 60°C was +10 μm, both of which were small. However, the maximum value of the warp increased.
[0123] [Example 6] Next, the sixth embodiment will be described with a focus on differences from the second embodiment. In the sixth embodiment, the adhesive 502 for fixing the solid-state imaging element 10 to the printed circuit board 20 was changed from silicone resin to epoxy resin, as in the fifth embodiment. At this time, the warp of the die-attach surface after the resin frame 40 was attached was 0 μm, which was small, and a stable suction force was obtained in the die bonder, wire bonder, and translucent member mounter. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was attached to the imaging element package 50 was +30 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was +30 μm, which was sufficiently small. In addition, the warp of the surface of the solid-state imaging element 10 when the imaging element module was set at −40° C. was +40 μm, and the warp of the surface of the solid-state imaging element 10 when the imaging element module was set at 60° C. was +20 μm, both of which were small. However, the maximum value of the warp increased.
[0124] [Comparative Example 1] The comparative example 1 will be described with a focus on differences from the example 1. In the comparative example 1, the type of prepreg used in the printed circuit board 20 is different from that in the example 1. The glass transition temperature Tgp of the completed printed circuit board 20 was 250°C, the linear expansion coefficient αPCB1 below the glass transition temperature Tgp was 5 ppm / °C, and the linear expansion coefficient αPCB2 above the temperature Tgp was 10 ppm / °C. At this time, the warp of the die attach surface after the resin frame 40 was attached was large at -100 μm, and the suction force of the die bonder, wire bonder, and translucent member mounter was insufficient, and the yield reduction and the reduction in the device operating rate due to the occurrence of positional accuracy defects were remarkable. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was bonded to the imaging element package 50 was -90 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was large at -90 μm, and did not meet the accuracy required for the camera. Furthermore, when the image sensor module was kept at -40°C, the warp of the surface of the solid-state image sensor 10 was -150 μm, and when kept at 60°C, the warp was -30 μm, again failing to ensure the stability required for a camera.
[0125] [Comparative Example 2] Comparative Example 2 will be described, focusing on the differences from Example 1. In Comparative Example 2, the type of prepreg used in the printed circuit board 20 was changed. The glass transition temperature Tgp of the completed printed circuit board 20 was 160°C, the linear expansion coefficient αPCB1 below the glass transition temperature Tgp was 16 ppm / °C, and the linear expansion coefficient αPCB2 above the temperature Tgp was 36 ppm / °C. At this time, the warp of the die attach surface after the resin frame 40 was attached was large at +110 μm, and the suction power of the die bonder, wire bonder, and translucent material mounter was insufficient, resulting in a significant decrease in yield due to poor positional accuracy and a significant decrease in the device operating rate.
[0126] The warpage of the surface of the solid-state imaging element 10 after bonding the solid-state imaging element 10 to the imaging element package 50 was +115 μm, and the warpage of the surface of the solid-state imaging element 10 after attaching the light-transmitting member 30 to the resin frame 40 was +115 μm, which was large and did not satisfy the accuracy required for a camera. In addition, when the imaging element module 50 was kept at -40° C., the warpage of the surface of the solid-state imaging element 10 was +130 μm, and when kept at 60° C., the warpage was +80 μm, and the stability required for a camera could not be ensured.
[0127] [Comparative Example 3] The comparative example 3 will be described with a focus on differences from the comparative example 1. In the comparative example 3, the light-transmitting member 30 was changed from quartz to borosilicate glass. The linear expansion coefficient αL of the borosilicate glass was 7 ppm / °C. At this time, the warp of the die-attach surface after the resin frame 40 was attached was large at -100 μm, and the suction force of the die bonder, wire bonder, and light-transmitting member mounter was insufficient, and the yield reduction and the decrease in the device operation rate due to the occurrence of positional accuracy defects were remarkable. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was bonded to the imaging element package 50 was -90 μm, and the warp of the surface of the solid-state imaging element 10 after the light-transmitting member 30 was attached to the resin frame 40 was -90 μm, which was large and did not satisfy the accuracy required for a camera. In addition, the warp of the surface of the solid-state imaging element 10 when the imaging element module was set at -40°C was -140 μm, and the warp when the imaging element module was set at 60°C was -40 μm, and the stability required for a camera could not be ensured.
[0128] [Comparative Example 4] The following describes Comparative Example 4, focusing on differences from Comparative Example 2. In Comparative Example 4, the translucent member 30 was changed from quartz to borosilicate glass. The linear expansion coefficient αL of borosilicate glass was 7 ppm / °C. At this time, the warp of the die-attach surface after the resin frame 40 was attached was large at +110 μm, and the suction power of the die bonder, wire bonder, and translucent member mounter was insufficient, resulting in a significant decrease in yield and a decrease in device operation rate due to poor positional accuracy. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was attached to the imaging element package 50 was +115 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was +115 μm, which was large and did not meet the accuracy required for a camera. Furthermore, when the solid-state imaging element module 50 was heated to −40° C., the warp of the surface of the solid-state imaging element 10 was +140 μm, and when heated to 60° C., the warp was +70 μm, so the stability required for a camera could not be ensured.
[0129] [Comparative Example 5] The following describes Comparative Example 5, focusing on differences from Comparative Example 1. In Comparative Example 5, the adhesive 502 for fixing the solid-state imaging element 10 to the imaging element module was changed from silicone resin to epoxy resin. At this time, the warp of the die-attach surface after the resin frame 40 was attached was large at -100 μm, and the suction power of the die bonder, wire bonder, and translucent member mounter was insufficient, resulting in a significant decrease in yield and a significant decrease in the device operating rate due to poor positioning accuracy. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was attached to the imaging element package 50 was -80 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin 40 frame was -80 μm, which was large and did not satisfy the accuracy required for a camera. In addition, the warp of the surface of the solid-state imaging element 10 when the imaging element module 50 was kept at -40°C was -140 μm, and the warp of the surface of the solid-state imaging element 10 when kept at 60°C was -20 μm, and the stability required for a camera could not be ensured.
[0130] [Comparative Example 6] The following describes Comparative Example 6, focusing on differences from Comparative Example 2. In Comparative Example 6, the adhesive 502 for fixing the solid-state imaging element 10 to the imaging element module 50 was changed from silicone resin to epoxy resin. At this time, the warp of the die-attach surface after the resin frame 40 was attached was large at +110 μm, and the suction power of the die bonder, wire bonder, and translucent member mounter was insufficient, resulting in a significant decrease in yield and a decrease in the device operation rate due to poor positioning accuracy. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was attached to the imaging element package 50 was +125 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was +125 μm, which was large and did not satisfy the accuracy required for a camera. In addition, the warp of the surface of the solid-state imaging element 10 when the solid-state imaging element module 50 was set at -40° C. was +140 μm, and the warp of the surface of the solid-state imaging element 10 when the solid-state imaging element module 50 was set at 60° C. was +90 μm, and the stability required for a camera could not be ensured.
[0131] [Example 7] The seventh embodiment will be described with a focus on differences from the first embodiment. In the seventh embodiment, the type of prepreg used for the printed circuit board 20 is different. The completed printed circuit board 20 had a glass transition temperature Tgp of 190°C, a linear expansion coefficient αPCB1 below the glass transition temperature Tgp of 12 ppm / °C, and a linear expansion coefficient αPCB2 above the temperature Tgp of 28 ppm / °C. The resin frame 40 was produced by molding alone. The produced resin frame 40 was bonded to the printed circuit board 20 via an adhesive 501. A resin containing epoxy as a main component was selected for the resin frame 40, and molding was performed by injection molding. The glass transition temperature Tgf was 220°C, the linear expansion coefficient αf1 of the resin frame 40 below the glass transition temperature Tgf was 13 ppm / °C, and the linear expansion coefficient αf2 of the resin frame 40 above the glass transition temperature Tgf was 26 ppm / °C.
[0132] The process of bonding the resin frame 40 to the printed circuit board 20 is as shown in FIG. 6. The printed circuit board 20 was fixed on a mounter, and adhesive 501 was applied to the periphery of the inner surface 202 of the printed circuit board 20 with a dispenser. The adhesive 501 used was a thermosetting epoxy resin. Then, the resin frame 40 was mounted on the adhesive 501 with the mounter. At this time, the amount of resin applied was adjusted so that a part of the adhesive 501 wetted up the inner edge 403 of the resin frame 40 and wetted down the outer edge 205 of the printed circuit board 20. Next, the adhesive 501 was hardened by placing it in an oven at 200°C. At this time, the warp of the die attachment surface after the resin frame 40 was attached was small at -15 μm, and sufficient suction force was obtained in the die bonder, wire bonder, and translucent material mounter. The warpage of the surface of the solid-state imaging element 10 after bonding the solid-state imaging element 10 to the imaging element package 50 was +15 μm, and the warpage of the surface of the solid-state imaging element 10 after the light-transmitting member 30 was attached to the resin frame 40 was +5 μm, which were sufficiently small. Furthermore, the warpage of the surface of the solid-state imaging element 10 of the imaging element module 50 at -40°C was +15 μm, and the warpage at 60°C was -5 μm, both of which were small.
[0133] [Example 8] The eighth embodiment will be described with a focus on differences from the seventh embodiment. In the eighth embodiment, the type of prepreg used in the printed circuit board 20 is different. The glass transition temperature Tgp of the completed printed circuit board 20 was 160°C, the linear expansion coefficient αPCB1 below the glass transition temperature Tgp was 16 ppm / °C, and the linear expansion coefficient αPCB2 above the glass transition temperature Tgp was 36 ppm / °C. In addition, the resin of the resin frame 40 and the adhesive 501 were changed. The glass transition temperature Tgf of the resin frame 40 after the change was 200°C, the linear expansion coefficient αf1 below the glass transition temperature Tgf was 18 ppm / °C, the linear expansion coefficient αf2 above the glass transition temperature Tgf was 39 ppm / °C, and the curing temperature of the adhesive 501 was 170°C. At this time, the warp of the die attachment surface after the resin frame 40 was attached was small at -5 μm, and sufficient suction force was obtained in the die bonder, wire bonder, and translucent member mounter. The warpage of the surface of the solid-state imaging element 10 after bonding the solid-state imaging element 10 to the imaging element package 50 was +15 μm, which was sufficiently small, and the warpage of the surface of the solid-state imaging element 10 after the light-transmitting member was attached to the resin frame 40 was +15 μm. Moreover, the warpage of the surface of the solid-state imaging element 10 of the imaging element module 50 at -40° C. was +35 μm, and the warpage at 60° C. was +5 μm, both of which were small.
[0134] [Example 9] The following describes Example 9, focusing on differences from Example 7. In Example 9, the light-transmitting member 30 was changed from quartz to borosilicate glass. The linear expansion coefficient αL of borosilicate glass was 7 ppm / °C. At this time, the warp of the die-attach surface after the resin frame 30 was attached was small at 15 μm, and sufficient suction force was obtained in the die bonder, wire bonder, and light-transmitting member mounter. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was bonded to the imaging element package 50 was +5 μm, and the warp of the surface of the solid-state imaging element 10 after the light-transmitting member 30 was attached to the resin frame 40 was +5 μm, which was sufficiently small. In addition, the warp of the surface of the solid-state imaging element 10 of the imaging element module 50 at -40°C was +35 μm, and the warp at 60°C was -15 μm, both of which were small. However, the amount of change in warp increased.
[0135] [Example 10] The tenth embodiment will be described with a focus on differences from the eighth embodiment. In the tenth embodiment, the translucent member 30 was changed from quartz to borosilicate glass. The linear expansion coefficient αL of the borosilicate glass was 7 ppm / °C. At this time, the warp of the die-attach surface after the resin frame 40 was attached was small at -5 μm, and sufficient suction force was obtained in the die bonder, wire bonder, and translucent member mounter. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was bonded to the imaging element package 50 was +15 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was +15 μm, which was sufficiently small. In addition, the warp of the solid-state imaging element surface of the imaging element module 50 at -40°C was +45 μm, and the warp at 60°C was -5 μm, both of which were small. However, the amount of change in warp increased.
[0136] [Example 11] The eleventh embodiment will be described with a focus on differences from the seventh embodiment. In the eleventh embodiment, the adhesive 502 for fixing the solid-state imaging element 10 to the imaging element module 50 was changed from silicone resin to epoxy resin. In this case, the warp of the die-attach surface after the resin frame 40 was attached was small at -15 μm, and sufficient suction force was obtained in the die bonder, wire bonder, and translucent member mounter. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was attached to the imaging element package 50 was +15 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was +15 μm, which was sufficiently small. In addition, the warp of the surface of the solid-state imaging element 10 of the imaging element module 50 at -40°C was +25 μm, and the warp at 60°C was -5 μm, both of which were small. However, the maximum value of the warp increased.
[0137] [Example 12] The twelfth embodiment will be described with a focus on differences from the eighth embodiment. In the twelfth embodiment, the adhesive 502 for fixing the solid-state imaging element 10 to the imaging element module 50 was changed from silicone resin to epoxy resin. In this case, the warp of the die-attach surface after the resin frame 40 was attached was small at -5 μm, and sufficient suction force was obtained in the die bonder, wire bonder, and translucent member mounter. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was attached to the imaging element package was +25 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was +25 μm, which was sufficiently small. In addition, the warp of the surface of the solid-state imaging element 10 of the imaging element module 50 at -40°C was +45 μm, and the warp at 60°C was +15 μm, both of which were small. However, the maximum value of the warp increased.
[0138] [Comparative Example 7] The comparative example 7 will be described with a focus on the differences from the example 7. In the comparative example 7, the type of resin used for the resin frame 40 is different. The glass transition temperature Tgf of the completed resin frame 40 was 250°C, the linear expansion coefficient αf1 below the glass transition temperature Tgf was 9 ppm / °C, and the linear expansion coefficient αf2 above the glass transition temperature Tgf was 30 ppm / °C. At this time, the warp of the die attachment surface after the resin frame 40 was attached was +105 μm, and the warp of the back surface was -105 μm, which was large, and sufficient suction force could not be obtained in the die bonder, wire bonder, and translucent member mounter, and the yield reduction due to the occurrence of positional accuracy failure and the decrease in the device operating rate were remarkable. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was bonded to the imaging element package 50 was +115 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was +115 μm, which was large, and did not meet the accuracy required for the camera. Furthermore, the warp of the surface of the solid-state imaging element 10 of the imaging element module 50 at −40° C. was +160 μm, and the warp at 60° C. was +40 μm, so the stability required for a camera could not be ensured.
[0139] [Comparative Example 8] The comparative example 8 will be described with a focus on the differences from the example 8. In the comparative example 8, the type of resin used for the resin frame 40 is different. The glass transition temperature Tgf of the completed resin frame 40 was 180°C, the linear expansion coefficient αf1 below the glass transition temperature Tgf was 20 ppm / °C, and the linear expansion coefficient αf2 above the temperature Tgf was 40 ppm / °C. At this time, the warp of the die attach surface after the resin frame 40 was attached was large at -120 μm, and sufficient suction force was not obtained in the die bonder, wire bonder, and translucent member mounter, and the yield reduction and the reduction in the device operation rate due to the occurrence of positional accuracy failure were remarkable. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was bonded to the imaging element package 50 was -105 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was large at -105 μm, and did not meet the accuracy required for the camera. Moreover, the warp of the surface of the solid-state imaging element 10 of the imaging element module 50 at -40°C was -170 µm, and the warp at 60°C was -95 µm, so the stability required for a camera could not be ensured.
[0140] [Comparative Example 9] The following describes Comparative Example 9, focusing on differences from Comparative Example 7. In Comparative Example 9, the translucent member 30 was changed from quartz to borosilicate glass. The linear expansion coefficient αL of borosilicate glass was 7 ppm / °C. At this time, the warp of the die attach surface after the resin frame 30 was attached was large at +105 μm, and sufficient suction force was not obtained in the die bonder, wire bonder, and translucent member mounter, and the yield reduction and the device operation rate reduction due to the occurrence of positional accuracy failure were significant. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was attached to the imaging element package 50 was +115 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was +115 μm, which was large and did not satisfy the accuracy required for a camera. In addition, the warp of the surface of the solid-state imaging element 10 of the solid-state imaging element module at -40°C was +170 μm, and the warp at 60°C was +30 μm, and the stability required for a camera could not be ensured.
[0141] [Comparative Example 10] The following describes Comparative Example 10, focusing on differences from Comparative Example 8. In Comparative Example 10, the translucent member 30 was changed from quartz to borosilicate glass. The linear expansion coefficient αL of borosilicate glass was 7 ppm / °C. At this time, the warp of the die attach surface after the resin frame 40 was attached was large at -1200 μm, and sufficient suction force could not be obtained in the die bonder, wire bonder, and translucent member mounter, and the yield reduction and the device operation rate reduction due to poor positioning accuracy were significant. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was attached to the imaging element package 50 was -105 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was large at -105 μm, and did not meet the accuracy required for a camera. Moreover, the warp of the surface of the solid-state imaging element 10 of the imaging element module 50 at -40°C was -190 µm, and the warp at 60°C was -105 µm, and the stability required for a camera could not be ensured.
[0142] [Comparative Example 11] The following describes Comparative Example 11, focusing on differences from Comparative Example 7. In Comparative Example 11, the adhesive 502 for fixing the solid-state imaging element 10 to the imaging element module 50 was changed from silicone resin to epoxy resin. At this time, the warp of the die-attach surface after the resin frame 40 was attached was large at +105 μm, and sufficient suction force was not obtained in the die bonder, wire bonder, and translucent member mounter, resulting in a significant decrease in yield and device operation rate due to poor positioning accuracy. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was attached to the imaging element package 50 was +125 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was +125 μm, which was large and did not satisfy the accuracy required for a camera. In addition, the warp of the surface of the solid-state imaging element 10 of the imaging element module 50 at -40°C was +170 μm, and the warp at 60°C was +50 μm, and the stability required for a camera could not be ensured.
[0143] [Comparative Example 12] The comparative example 12 will be described with a focus on differences from the comparative example 8. In the comparative example 12, the adhesive 502 for fixing the solid-state imaging element 10 to the imaging element module was changed from silicone resin to epoxy resin. At this time, the warp of the die attach surface after the resin frame 40 was attached was large at -120 μm, and sufficient suction force was not obtained in the die bonder, wire bonder, and translucent member mounter, and the yield reduction and the device operation rate reduction due to the occurrence of positional accuracy failure were remarkable. The warp of the surface of the solid-state imaging element 10 after the solid-state imaging element 10 was attached to the imaging element package 50 was -95 μm, and the warp of the surface of the solid-state imaging element 10 after the translucent member 30 was attached to the resin frame 40 was -95 μm, which was large and did not satisfy the accuracy required for a camera. In addition, the warp of the surface of the solid-state imaging element 10 of the imaging element module at -40°C was -160 μm, and the warp at 60°C was -85 μm, and the stability required for a camera could not be ensured.
[0144] Figures 14A, 14B, 15A, and 15B show the measurement results and the judgment results of the examples and the comparative examples. Figure 14A shows the relationship between the linear expansion coefficient and the glass transition temperature in Examples 1 to 6 and Comparative Examples 1 to 6, and Figure 14B shows the amount of warping, the suction transport judgment results, the warping judgment results, etc. in the same examples and the same comparative examples. Similarly, Figure 15A shows the relationship between the linear expansion coefficient and the glass transition temperature in Examples 7 to 12 and Comparative Examples 7 to 12, and Figure 15B shows the amount of warping, the suction transport judgment results, the warping judgment results, etc. in the same examples and the same comparative examples.
[0145] 14 and 15 show the relationship between temperatures Tgp and Tgf, the relationship between linear expansion coefficients αPCB1 and αf1, the relationship between ((Tgp-To)×αPCB1) and ((Tgf-To)×αf1+(Tgp-Tgf)×αf2), the results of suction transport judgment, and the results of warping judgment on the image sensor surface. In light of these, the effects of Examples 1 to 12 of the present invention are clear.
[0146] [Second embodiment] The image sensor module in the above-described embodiment can be applied to various imaging systems. Examples of imaging systems include digital still cameras, digital camcorders, camera heads, copiers, fax machines, mobile phones, vehicle-mounted cameras, observation satellites, and surveillance cameras. Fig. 16 shows a block diagram of a digital still camera as an example of an imaging system.
[0147] The imaging system shown in FIG. 16 includes a barrier 1001, a lens 1002, an aperture 1003, an imaging device 1004, a signal processing device 1007, a timing generating unit 1008, an overall control and calculation unit 1009, a memory unit 1010, a recording medium control I / F unit 1011, a recording medium 1012, an external I / F unit 1013, an angular velocity sensor (detection unit) 1015, and an actuator 1016. The barrier 1001 protects the lens 1002, which forms an optical image of a subject on the imaging device 1004. The aperture 1003 varies the amount of light that passes through the lens 1002. The imaging device 1004 is composed of the above-mentioned image sensor module 1, and converts the optical image formed by the lens 1002 into image data. The signal processing device 1007 performs various corrections and data compression on the image data output from the imaging device 1004. A timing generating unit 1008 outputs various timing signals to the imaging device 1004 and the signal processing device 1007. An overall control / calculation unit 1009 controls the entire digital still camera, and a memory unit 1010 temporarily stores image data. A recording medium control I / F unit 1011 is an interface for recording or reading image data to a recording medium 1012, and the recording medium 1012 is a removable recording medium such as a semiconductor memory for recording or reading imaging data. An external I / F unit 1013 is an interface for communicating with an external computer or the like. Timing signals and the like may be input from outside the imaging system, and the imaging system only needs to have at least the imaging device 1004 and a signal processing device 1007 for processing image signals output from the imaging device 1004.
[0148] The imaging device 1004 and the AD conversion unit may be provided on the same semiconductor substrate, or the imaging device 1004 and the AD conversion unit may be formed on different semiconductor substrates. The imaging device 1004 and the signal processing device 1007 may be formed on the same semiconductor substrate. Each pixel may include a first photoelectric conversion unit and a second photoelectric conversion unit. The signal processing device 1007 may be configured to process a pixel signal generated by the first photoelectric conversion unit and a pixel signal generated by the second photoelectric conversion unit, and acquire distance information from the imaging device 1004 to a subject.
[0149] The angular velocity sensor 1015 is fixed to the housing of the imaging system or the like, and detects camera shake of the imaging system. Camera shake is detected as the amount of displacement in the X-axis direction and the Y-axis direction on the light receiving surface of the imaging device. The actuator 1016 is composed of an electromagnetic driving mechanism or a piezoelectric driving mechanism, and displaces the position of the imaging device 1004. The actuator 1016 is controlled by the overall control / calculation unit 1009, and drives the imaging device 1004 in a direction that cancels the amount of displacement detected by the angular velocity sensor 1015.
[0150] Fig. 17 is a diagram for explaining an imaging device 1004 in this embodiment. Fig. 17(A) is a plan view of the imaging device 1004, and Fig. 17(B) is a side view of the imaging device 1004. The imaging device 1004 is attached to the upper surface of a substrate 1017, and an actuator 1016 is provided on the lower surface of the substrate 1017. The actuator 1016 can move the imaging device 1004 in the X direction and the Y direction.
[0151] The imaging device 1004 in this embodiment is configured by the imaging element module 1 in the first embodiment. In the imaging element module 1, electronic devices such as the solid-state imaging element 10 are directly attached to the printed circuit board 20 without using a ceramic package. This allows the imaging device 1004 to be lightweight, and a sensor-shift type image stabilization mechanism that controls the displacement of the imaging device 1004 can be adopted.
[0152] [Third embodiment] 18A and 18B are block diagrams of an imaging system related to a vehicle-mounted camera in this embodiment. The imaging system 2000 has the imaging device 1004 of the above-mentioned embodiment. The imaging system 2000 has an image processing unit 2030 that performs image processing on a plurality of image data acquired by the imaging device 1004, and a parallax calculation unit 2040 that calculates parallax (phase difference of parallax images) from a plurality of image data acquired by the imaging system 2000. The imaging system 2000 also has a distance measurement unit 2050 that calculates a distance to an object based on the calculated parallax, and a collision determination unit 2060 that determines whether or not there is a possibility of a collision based on the calculated distance. Here, the parallax calculation unit 2040 and the distance measurement unit 2050 are examples of distance information acquisition means that acquire distance information to an object. That is, the distance information is information related to the parallax, the defocus amount, the distance to the object, and the like. The collision determination unit 2060 may determine the possibility of a collision using any of these distance information. The distance information acquisition means may be realized by dedicated hardware, a software module, a field programmable gate array (FPGA), an application specific integrated circuit (ASIC), or a combination of these.
[0153] The imaging system 2000 is connected to a vehicle information acquisition device 2310, and can acquire vehicle information such as vehicle speed, yaw rate, and steering angle. The imaging system 2000 is also connected to a control ECU 2410, which is a control device that outputs a control signal to generate a braking force for the vehicle based on the judgment result of the collision judgment unit 2060. The imaging system 2000 is also connected to an alarm device 2420 that issues an alarm to the driver based on the judgment result of the collision judgment unit 2060. For example, when the judgment result of the collision judgment unit 2060 indicates that there is a high possibility of a collision, the control ECU 2410 performs vehicle control to avoid a collision and reduce damage by applying the brakes, releasing the accelerator, suppressing engine output, etc. The alarm device 2420 warns the user by sounding an alarm, displaying alarm information on a screen of a car navigation system, etc., or vibrating a seat belt or steering wheel. The imaging system 2000 functions as a control means that controls the operation of controlling the vehicle as described above.
[0154] In this embodiment, the surroundings of the vehicle, for example, the front or rear, are imaged by the imaging system 2000. Fig. 18B shows an imaging system for imaging the area in front of the vehicle (imaging range 2510). A vehicle information acquisition device 2310 serving as an imaging control means sends an instruction to the imaging system 2000 or the imaging device 1004 to perform the operations described in the first to fifth embodiments. With this configuration, the accuracy of distance measurement can be further improved.
[0155] Although the above describes an example of control to prevent collision with other vehicles, the present invention can also be applied to control of automatic driving by following other vehicles, control of automatic driving to prevent deviation from lanes, etc. Furthermore, the imaging system is not limited to vehicles such as the vehicle itself, but can be applied to moving bodies (moving devices) such as ships, aircraft, and industrial robots. In addition, the imaging system can be applied not only to moving bodies, but also to a wide range of devices that use object recognition, such as intelligent transport systems (ITS).
[0156] [Other embodiments] The present invention is not limited to the above-described embodiments, and various modifications are possible. For example, an example in which a part of the configuration of any of the embodiments is added to another embodiment, or an example in which a part of the configuration of another embodiment is replaced with another embodiment is also an embodiment of the present invention. In addition, the present invention can be applied to electronic devices other than solid-state imaging devices.
[0157] It should be noted that the above-mentioned embodiments are merely examples of the implementation of the present invention, and the technical scope of the present invention should not be interpreted as being limited by these embodiments. In other words, the present invention can be implemented in various forms without departing from its technical concept or main features. [Explanation of symbols]
[0158] 1. Image sensor module 10 Solid-state imaging element 20 Printed circuit board 201 Outer surface (second main surface) of printed circuit board 202 Inner surface (first main surface) of printed circuit board 205 Outer edge of printed circuit board 30 Translucent material 40 Resin Frame 50 Image sensor package 510 Interior Space 600 parts
Claims
1. a substrate having a first main surface, a second main surface, and an outer edge continuous with the first main surface and the second main surface, the substrate including a plurality of conductor layers and a plurality of insulating layers; A solid-state imaging element attached to the first main surface; a frame attached to the first main surface so as to surround the periphery of the solid-state imaging element; an imaging element module including a light-transmitting member fixed onto the frame body, When the linear expansion coefficient of the substrate in the in-plane direction at or below the glass transition temperature Tgp of the substrate is denoted as αPCB1, the linear expansion coefficient of the substrate in the in-plane direction at or above the glass transition temperature Tgp is denoted as αPCB2, the linear expansion coefficient of the frame at or below the glass transition temperature Tgf of the frame is denoted as αf1, the linear expansion coefficient of the frame at or above the glass transition temperature Tgf is denoted as αf2, and room temperature is denoted as To, Tgp<Tgf, and αPCB1 < αf1, and (Tgf-To)×αf1<(Tgp-To)×αPCB1+(Tgf-Tgp)×αPCB2, An imaging element module, characterized in that the following relationship is satisfied.
2. a substrate having a first main surface, a second main surface, and an outer edge continuous with the first main surface and the second main surface, the substrate including a plurality of conductor layers and a plurality of insulating layers; A solid-state imaging element attached to the first main surface; a frame attached to the first main surface so as to surround the periphery of the solid-state imaging element; an imaging element module including a light-transmitting member fixed onto the frame body, an internal terminal provided on a first main surface of the substrate and an electrode of the solid-state imaging element are electrically connected; on the second main surface of the substrate, no electronic components are provided in projection areas of the internal terminals and the electrodes, and the electronic components are provided outside the projection areas; When the linear expansion coefficient of the substrate in the in-plane direction at or below the glass transition temperature Tgp of the substrate is denoted as αPCB1, the linear expansion coefficient of the substrate in the in-plane direction at or above the glass transition temperature Tgp is denoted as αPCB2, the linear expansion coefficient of the frame at or below the glass transition temperature Tgf of the frame is denoted as αf1, the linear expansion coefficient of the frame at or above the glass transition temperature Tgf is denoted as αf2, and room temperature is denoted as To, Tgp>Tgf, and αf1<αPCB1, and (Tgp-To)×αPCB1<(Tgf-To)×αf1+(Tgp-Tgf)×αf2 or Tgp<Tgf, and αPCB1 < αf1, and (Tgf-To)×αf1<(Tgp-To)×αPCB1+(Tgf-Tgp)×αPCB2, An imaging element module, characterized in that the following relationship is satisfied.
3. 3. The image sensor module according to claim 2, wherein the glass transition temperature Tgp is higher than the glass transition temperature Tgf, and the frame is molded on the substrate.
4. An imaging element module as described in any one of claims 1 to 3, characterized in that the linear expansion coefficient αPCB1 and the linear expansion coefficient αf1 are smaller than the linear expansion coefficient αL of the translucent member in the in-plane direction and larger than the linear expansion coefficient αc of the solid-state imaging element in the in-plane direction.
5. 5. The image sensor module according to claim 1, wherein the substrate is a printed circuit board including a prepreg.
6. 6. The imaging element module according to claim 1, wherein the frame includes a resin.
7. 7. The image sensor module according to claim 1, wherein the solid-state image sensor is attached to the first main surface by an adhesive.
8. 8. The imaging element module according to claim 7, wherein the adhesive is a resin having rubber elasticity.
9. 9. The imaging element module according to claim 1, wherein the frame covers the outer edge of the substrate.
10. 9. The imaging element module according to claim 1, wherein the frame does not cover the outer edge of the substrate.
11. 11. An imaging system comprising: a signal processing device that processes pixel signals output from the solid-state imaging device according to claim 1.
12. A detection unit that detects a motion of the imaging system; 12. The imaging system according to claim 11, further comprising an actuator that displaces the imaging element module based on a signal from the detection unit.
13. The solid-state imaging device includes a plurality of pixels, The pixel includes a plurality of photoelectric conversion units, 13. The imaging system according to claim 11, wherein the signal processing device processes the pixel signals generated by the plurality of photoelectric conversion units, respectively, and acquires information based on a distance from the solid-state imaging element to a subject.
14. a substrate having a first main surface, a second main surface, and an outer edge continuous with the first main surface and the second main surface, the substrate including a plurality of conductor layers and a plurality of insulating layers; a frame body attached to the first main surface, When the linear expansion coefficient of the substrate in the in-plane direction at or below the glass transition temperature Tgp of the substrate is denoted as αPCB1, the linear expansion coefficient of the substrate in the in-plane direction at or above Tgp is denoted as αPCB2, the linear expansion coefficient of the frame at or below the glass transition temperature Tgf of the frame is denoted as αf1, the linear expansion coefficient of the frame at or above Tgf is denoted as αf2, and room temperature is denoted as To, Tgp<Tgf, and αPCB1 < αf1, and (Tgf-To)×αf1<(Tgp-To)×αPCB1+(Tgf-Tgp)×αPCB2, An imaging element package characterized in that the above relationship is satisfied.
15. providing a substrate having a first main surface, a second main surface, and an outer edge continuous with the first main surface and the second main surface, the substrate including a plurality of conductor layers and a plurality of insulating layers; attaching a solid-state imaging element to the first main surface; attaching a frame to the first main surface so as to surround the periphery of the solid-state imaging element; a manufacturing method for an imaging element module, comprising the step of attaching a light-transmitting member onto the frame body. And, When the linear expansion coefficient of the substrate in the in-plane direction at or below the glass transition temperature Tgp of the substrate is denoted as αPCB1, the linear expansion coefficient of the substrate in the in-plane direction at or above the glass transition temperature Tgp is denoted as αPCB2, the linear expansion coefficient of the frame at or below the glass transition temperature Tgf of the frame is denoted as αf1, the linear expansion coefficient of the frame at or above the glass transition temperature Tgf is denoted as αf2, and room temperature is denoted as To, Tgp<Tgf, and αPCB1 < αf1, and (Tgf-To)×αf1<(Tgp-To)×αPCB1+(Tgf-Tgp)×αPCB2, Fulfilling the relationship, 4. The method for manufacturing an image sensor module, wherein the step of attaching the frame to the substrate is performed at a temperature between the glass transition temperature Tgp and the glass transition temperature Tgf.
16. providing a substrate having a first main surface, a second main surface, and an outer edge continuous with the first main surface and the second main surface, the substrate including a plurality of conductor layers and a plurality of insulating layers, and the substrate having an electronic component on the second main surface; attaching a solid-state imaging element to the first main surface; a step of electrically connecting an internal terminal provided on a first main surface of the substrate to an electrode of the solid-state imaging element; attaching a frame to the first main surface so as to surround the periphery of the solid-state imaging element; a manufacturing method for an imaging element module, comprising the step of attaching a light-transmitting member onto the frame body. And, on the second main surface of the substrate, no electronic components are provided in projection areas of the internal terminals and the electrodes, and the electronic components are provided outside the projection areas; When the linear expansion coefficient of the substrate in the in-plane direction at or below the glass transition temperature Tgp of the substrate is denoted as αPCB1, the linear expansion coefficient of the substrate in the in-plane direction at or above the glass transition temperature Tgp is denoted as αPCB2, the linear expansion coefficient of the frame at or below the glass transition temperature Tgf of the frame is denoted as αf1, the linear expansion coefficient of the frame at or above the glass transition temperature Tgf is denoted as αf2, and room temperature is denoted as To, Tgp>Tgf, and αf1<αPCB1, and (Tgp-To)×αPCB1<(Tgf-To)×αf1+(Tgp-Tgf)×αf2 or Tgp<Tgf, and αPCB1 < αf1, and (Tgf-To)×αf1<(Tgp-To)×αPCB1+(Tgf-Tgp)×αPCB2, Fulfilling the relationship, a step of attaching the frame to the substrate at a temperature between the glass transition temperature Tgp and the glass transition temperature Tgf;
17. 17. The method for manufacturing a solid-state imaging element module according to claim 16, wherein the glass transition temperature Tgp is higher than the glass transition temperature Tgf, and the frame is molded onto the substrate at a temperature between the glass transition temperature Tgp and the glass transition temperature Tgf.
Citation Information
Patent Citations
Camera device
JP1991269418A
Image sensor module
JP2010252095A
Electronic component, electronic module, and manufacturing method of these
JP2013243339A
Imaging unit and imaging device
JP2015146380A
Hollow package for mounting semiconductor element
JP2015185763A