In situ protective coating of chamber component for semiconductor processing
In-situ protective coatings deposited using PECVD or ALD at elevated temperatures address contamination issues in semiconductor reaction chambers, ensuring durable and uniform protection against harsh processing conditions.
Patent Information
- Application Number
- JP2024133711
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-10-19
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Semiconductor manufacturing processes face challenges with film impurities and non-uniformities due to contamination from reaction chamber components, leading to device failure and degradation over time, as existing protective coatings are not effective under harsh processing conditions.
In-situ deposition of protective coatings on chamber components using plasma enhanced chemical vapor deposition (PECVD) or atomic layer deposition (ALD) at elevated temperatures, controlling RF signal phases to direct plasma glow discharge for uniform coverage, and etching film materials at higher rates than the coating.
The in-situ coatings provide resistant, high-quality, and durable protection against halogen-based chemicals, reducing particle contamination and chamber degradation, ensuring consistent semiconductor processing quality.
Smart Images

Figure 2024161438000001_ABST
Abstract
Description
[Background technology]
[0001] [Incorporated by reference] PCT applications are being filed contemporaneously herewith as a part of this application. Each application to which this application claims the benefit or priority of a contemporaneously filed PCT application is hereby incorporated by reference in its entirety for all purposes.
[0002] As the semiconductor and other industries advance, device dimensions become smaller and smaller. These innovatively smaller geometries require highly uniform deposition procedures, and the presence of film impurities or other non-uniformities can frequently result in semiconductor device failures.
[0003] The background art described herein is provided to present the contents of the present disclosure to the public, and the presently cited inventors' inventions are not admitted expressly or impliedly as prior art to the present disclosure to the extent that they are described in this background art, as well as in described aspects that are not prior art at the time of filing. Summary of the Invention
[0004] Described herein is a method for depositing a protective coating in a reaction chamber, the method including introducing a first reactant in a vapor phase into the reaction chamber to adsorb onto surfaces of a plurality of chamber components that are part of the reaction chamber, and introducing a second reactant in a vapor phase into the reaction chamber, where the first reactant and the second reactant react to deposit a protective coating on the surfaces of the plurality of chamber components at a temperature greater than about 200° C.
[0005] In some embodiments, the first reactant reacts with the second reactant in a plasma enhanced atomic layer deposition (PEALD) process. In some embodiments, the method further includes controlling a radio frequency (RF) signal supplied to the reaction chamber such that a majority of the plasma glow discharge of the second reactant forms in one or more regions outside the region between the top electrode and the bottom electrode. A phase difference between a first phase of the RF signal supplied to the top electrode and a second phase of the RF signal supplied to the bottom electrode may be about 180 degrees to 0 degrees out of phase. In some embodiments, the first reactant reacts with the second reactant in a thermal ALD process. In some embodiments, the protective coating includes an oxide, a nitride, a carbide, or a combination thereof. The protective coating may include silicon oxide (SiO2), aluminum oxide (Al2O3), zirconium oxide (ZrO2), hafnium oxide (HfO2), tin oxide (SnO2), or silicon nitride (Si3N4). In some embodiments, the method further includes depositing a membrane material on the wafer and the protective coating in the reaction chamber, and etching the membrane material on the wafer and the protective coating, where the membrane material etches at a substantially higher rate than the protective coating. The etchant used to etch the membrane material may include a fluorine-based species, a chlorine-based species, a bromine-based species, an iodine-based species, or a combination thereof. In some embodiments, the method further includes redepositing a protective coating on surfaces of the plurality of chamber components of the reaction chamber after etching the membrane material.
[0006] Another aspect includes a method of depositing a protective coating in a reaction chamber, the method including depositing a protective coating on surfaces of a plurality of chamber components of a reaction chamber, the plurality of chamber components being part of the reaction chamber, the protective coating being deposited by plasma enhanced chemical vapor deposition (PECVD), plasma enhanced atomic layer deposition (PEALD), or thermal atomic layer deposition (thermal ALD) at a temperature greater than about 200° C.
[0007] In some embodiments, the method further comprises depositing a film material on a protective coating on a surface of a plurality of chamber components of the reaction chamber, the film material being etched at a substantially higher rate than the protective coating during exposure to a fluorine-based, chlorine-based, bromine-based, or iodine-based species. In some embodiments, the method further comprises redepositing a protective coating on a surface of a plurality of chamber components of the reaction chamber after exposure to a fluorine-based, chlorine-based, bromine-based, or iodine-based species. In some embodiments, the protective coating is deposited by PECVD or PEALD, and the method further comprises controlling a radio frequency (RF) signal supplied to the reaction chamber such that a majority of the plasma glow discharge forms in one or more regions outside the region between the upper electrode and the lower electrode. A phase difference between a first phase of the RF signal supplied to the upper electrode and a second phase of the RF signal supplied to the lower electrode is about 0 degrees out of phase. In some embodiments, the protective coating comprises silicon oxide (SiO2), aluminum oxide (Al2O3), zirconium oxide (ZrO2), hafnium oxide (HfO2), tin oxide (SnO2), or silicon nitride (Si3N4), and one or more materials of the plurality of chamber components comprises aluminum (Al).
[0008] Another aspect relates to an apparatus that includes a plasma apparatus that includes a reaction chamber that includes a plurality of chamber components, the plasma apparatus further including a controller configured with instructions for performing operations of: introducing a first reactant in a gas phase into the reaction chamber to adsorb onto surfaces of the plurality of chamber components that are part of the reaction chamber; and introducing a second reactant in a gas phase into the reaction chamber, where the first reactant and the second reactant react to deposit a protective coating on the surfaces of the plurality of chamber components at a temperature greater than about 200° C.
[0009] In some embodiments, the first reactant reacts with the second reactant in a plasma enhanced atomic layer deposition (PEALD) process. In some embodiments, the plasma apparatus further comprises an RF power supply coupled to the controller, the controller further configured with instructions to perform an operation of controlling a radio frequency (RF) signal provided to the reaction chamber such that a majority of the plasma glow discharge of the second reactant forms in one or more regions outside the region between the upper electrode and the lower electrode. In some embodiments, a phase difference between a first phase of the RF signal provided to the upper electrode and a second phase of the RF signal provided to the lower electrode is about 180 degrees to 0 degrees out of phase. In some embodiments, the phase difference is 0 degrees out of phase. In some embodiments, the first reactant reacts with the second reactant in a thermal ALD process. In some embodiments, the protective coating comprises an oxide, a nitride, a carbide, or a combination thereof. In some embodiments, the plurality of chamber components comprises at least a chamber wall of the reaction chamber. In some embodiments, the controller is further configured with instructions to perform the operations of depositing a film material on the wafer and the protective coating in the reaction chamber, and etching the film material on the wafer and on the protective coating, wherein the film material is etched at a substantially faster rate than the protective coating.
[0010] Another aspect relates to an apparatus that includes a plasma apparatus comprising a reaction chamber including a plurality of chamber components, the plasma apparatus further comprising a controller configured with instructions to perform an operation of depositing a protective coating on a surface of the plurality of chamber components of the reaction chamber, the plurality of chamber components being part of the reaction chamber, the protective coating being deposited at a temperature greater than about 200° C. by plasma enhanced chemical vapor deposition (PECVD), plasma enhanced atomic layer deposition (PEALD), or thermal atomic layer deposition (thermal ALD).
[0011] In some embodiments, the controller is further configured with instructions to perform an operation of depositing a film material on a protective coating on a surface of a plurality of chamber components of the reaction chamber, the film material being etched at a substantially higher rate than the protective coating during exposure to the fluorine-based, chlorine-based, bromine-based, or iodine-based species. In some embodiments, the controller is further configured with instructions to perform an operation of redepositing a protective coating on a surface of a plurality of chamber components of the reaction chamber after exposure to the fluorine-based, chlorine-based, bromine-based, or iodine-based species. In some embodiments, the protective coating is deposited by PECVD or PEALD, and the controller is further configured with instructions to perform an operation of controlling a radio frequency (RF) signal supplied to the reaction chamber such that a majority of the plasma glow discharge forms in one or more regions outside the region between the upper electrode and the lower electrode.
[0012] These and other aspects are further described below with reference to the drawings. [Brief description of the drawings]
[0013] [Figure 1] 1 is a simplified cross-sectional view of an exemplary apparatus for performing in-situ coating of chamber components of a reaction chamber, according to some embodiments.
[0014] [Figure 2A] 1 is a flow diagram of an exemplary atomic layer deposition (ALD) method for coating multiple chamber components of a reaction chamber, according to some embodiments.
[0015] [Figure 2B] 1 is a flow diagram of an exemplary method for coating multiple chamber components of a reaction chamber, according to some embodiments.
[0016] [Figure 3A] 1 is a simplified cross-sectional view of an exemplary plasma device comprising a reaction chamber in which a plasma glow discharge occurs between an upper electrode and a lower electrode, according to some embodiments.
[0017] [Figure 3B] 3B is a schematic cross-sectional view of an exemplary plasma apparatus comprising the reaction chamber of FIG. 3A in which a plasma glow discharge occurs adjacent to a chamber wall of the reaction chamber, according to some embodiments.
[0018] [Figure 3C] 3C is a schematic cross-sectional view of an exemplary plasma apparatus comprising the reaction chamber of FIG. 3A and FIG. 3B with a protective coating deposited on the chamber walls of the reaction chamber, according to some embodiments.
[0019] [Figure 4A] 2 is a simplified cross-sectional view of an exemplary reaction chamber with film material deposited on a wafer and a protective coating in accordance with some embodiments.
[0020] [Figure 4B] 4B is a simplified cross-sectional view of the exemplary reaction chamber of FIG. 4A with the membrane material etched from the wafer and selectively etched from the protective coating, according to some embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] In this disclosure, the terms "semiconductor wafer," "wafer," "substrate," "wafer substrate," and "semi-finished integrated circuit" are used interchangeably. Those skilled in the art will understand that the term "semi-finished integrated circuit" can refer to a silicon wafer at any of the many stages of integrated circuit manufacturing. Wafers or substrates used in the semiconductor device industry typically have diameters of 200 mm, or 300 mm, or 450 mm. The following detailed description assumes that the disclosure is implemented on a wafer, but the disclosure is not limited thereto. Workpieces may have a variety of shapes, sizes, and materials. In addition to semiconductor wafers, other workpieces that may utilize the present disclosure include various articles such as printed circuit boards. preface
[0022] When manufacturing semiconductor devices, it is advantageous for the manufacturing process to be accurate and repeatable. Unfortunately, as the semiconductor manufacturing equipment processes additional wafers over time, the processing conditions and chemicals within the equipment change. The processing conditions and chemicals can cause contamination and defect problems in the wafers and can lead to degradation of the reaction chambers of the semiconductor manufacturing equipment.
[0023] Semiconductor devices are becoming increasingly susceptible to contamination and failure problems. Particles and film impurities can originate from the inner surfaces of the reaction chamber. For example, particles and film impurities can originate from the inner chamber walls, ceiling, showerhead, substrate support, lift pins, gas lines, nozzles, etc. In a particular example, the reaction chamber and / or chamber components may be made from aluminum, such as aluminum 6061-T6 (which may contain aluminum as well as small amounts of other materials, such as chromium, copper, iron, magnesium, manganese, silicon, titanium, silver, etc.). Often, particles and film impurities are generated when the reaction chamber is exposed to plasma or other harsh processing conditions, and these particles and film impurities can fall onto the wafer surface during processing. For example, chamber components exposed to in situ plasma during deposition can flake off and drop undesirable impurities onto the wafer being processed. This can result in contamination of the wafer and increase the likelihood of device failure.
[0024] The process conditions and chemicals affect not only the wafers being processed in the equipment, but also the inner surfaces of the reaction chamber of the semiconductor manufacturing equipment. As the reaction chamber is used to deposit films on a series of wafers over time, various film by-products are deposited on the inner surfaces of the reaction chamber. The reaction chamber may be subjected to an etching process to remove the deposited films. In some cases, the etching process may include exposing the wafers and the reaction chamber to a halogen-based species, which may include fluorine (F), chlorine (Cl), bromine (Br), or iodine (I). The reaction chamber may be subjected to a cleaning process to remove the film by-products from its inner surfaces. In some cases, the cleaning process includes exposing the reaction chamber to one or more of the halogen-based species. The reaction chamber may be subjected to a deposition process to deposit films on the wafers. In some cases, the deposition process includes exposing the reaction chamber to one or more of the halogen-based species. The reaction chamber, including the chamber components and chamber walls, is often made of a metallic material, such as aluminum. Chamber components and chamber walls made of metallic materials can be attacked by halogen-based species and quickly form volatile salts. For example, aluminum chamber components can be attacked by fluorine radicals and form aluminum fluoride (AlF3), which is volatile under the right conditions. These types of reactions can significantly increase the surface area of the chamber components and change the surface properties of the chamber components, thereby altering the results of deposition or other processing of wafers processed in the reaction chamber over time. Furthermore, these types of reactions can result in corrosion of the chamber components and chamber walls, as well as degradation of the reaction chamber over time.
[0025] One technique to combat particle generation is to coat the reaction chamber surfaces with an undercoat. The undercoat may also be referred to as a conditioning layer or a protective layer. The undercoat is generally a layer of material formed in situ on the interior surfaces of the reaction chamber. The undercoat may function to minimize metal contamination from the exposed interior surfaces. The undercoat is typically deposited when there is no wafer in the reaction chamber. The undercoat is further described in U.S. Patent Application No. 14 / 089,653, filed November 25, 2013, entitled "CHAMBER UNDERCOAT PREPARATION METHOD FOR LOW TEMPERATURE ALD FILMS," which is incorporated by reference in its entirety for all purposes.
[0026] While undercoats help reduce particle generation and associated contamination, they also present certain challenges. First, undercoats often provide incomplete coverage on some of the reaction chamber's inner surfaces. Certain parts of the reaction chamber may not be exposed to the reactants necessary for film formation. Second, undercoats are generally formed as a result of exposure to thermal energy, but are not heated to the appropriate temperature to withstand harsh processing conditions. Such undercoats do not last long and are susceptible to degradation due to thermal and plasma stresses. Third, some undercoats result in a microporous structure that accumulates on the reaction chamber's inner surfaces. The microporous structure may undergo significant reduction when exposed to plasma. Such undercoats that are microporous, provide incomplete coverage, or are not suitable to withstand harsh processing conditions will degrade the reaction chamber. The reaction chamber may degrade over time when exposed to high temperatures and / or plasma, or halogen-based chemicals.
[0027] Another technique to combat particle generation or chamber degradation is to provide a protective coating by ex-situ deposition. Protective coatings are considered to be deposited ex-situ, where the protective coating is deposited on a chamber component in a first reaction chamber, and then the chamber component is removed and installed in a second reaction chamber. In these cases, the chamber component functions as a coated substrate when in the first reaction chamber, and performs its intended function when installed in the second reaction chamber. Ex-situ coatings are further described in U.S. Patent Application Serial No. 15 / 954,454, entitled "EX SITU COATING OF CHAMBER COMPONENTS FOR SEMICONDUCTOR PROCESSING," filed April 16, 2018, which is incorporated by reference in its entirety for all purposes.
[0028] Although ex-situ coatings are effective in limiting particulate contamination, providing more complete coverage of the surfaces of chamber components, and protecting against chamber degradation, they also present certain challenges. First, ex-situ coatings are deposited in a separate reaction chamber, increasing throughput. Not only would the coated chamber components require transport and installation steps to another reaction chamber, but the chamber components would undergo more removal, transport, and reinstallation steps to be periodically recoated. Second, ex-situ coatings are typically deposited using conventional deposition techniques, such as plasma spraying, thermal spraying, or physical vapor deposition (PVD). These deposition techniques are performed at low temperatures, such as below about 200° C. This limits the quality of the protective coating when it is exposed to harsh processing conditions. Thus, such protective coatings are prone to cracking and degradation when exposed to plasma or high temperatures. Once the protective coating is no longer useful, the wafers are susceptible to particulate contamination and drift in processing results, and the reaction chambers are subject to degradation and corrosion. Device
[0029] The methods described herein may be implemented in any suitable apparatus. A suitable apparatus may include hardware for performing process operations and a system controller having instructions for controlling the process operations in accordance with the present embodiments. For example, in some embodiments, the hardware may include one or more processing stations included in a process tool.
[0030] The deposition techniques for providing in situ protective coatings on chamber components described herein may be performed in any plasma enhanced chemical vapor deposition (PECVD) or atomic layer deposition (ALD) apparatus. The apparatus may take many forms and may be part of a process tool that includes one or more chambers or reactors (sometimes referred to as processing stations). For certain operations, exemplary apparatus such as the VECTOR™ family of products or the Striker™ family of products (each available from Lam Research Corporation, Fremont, Calif.) may be suitable apparatus.
[0031] FIG. 1 illustrates a schematic cross-section of an exemplary apparatus for performing in-situ coating of chamber components of a reaction chamber, according to some embodiments. The apparatus 100 may include a reaction chamber 102 and may deposit a protective coating on multiple chamber components of the reaction chamber 102 as described herein. It will be appreciated that the apparatus 100 may be used to deposit a film, etch a film, and / or clean a film by-product in the reaction chamber 102 for semiconductor processing. In some embodiments, the apparatus 100 may deposit a film on a wafer using an ALD technique or a PECVD technique, and the apparatus 100 may deposit a protective coating on chamber components of the reaction chamber 102 using an ALD technique or a PECVD technique. For simplicity, the apparatus 100 is depicted as a single reactor having the reaction chamber 102 for maintaining a low pressure environment. However, it will be appreciated that multiple apparatuses 100 may be included in a typical process tool environment. It will be further appreciated that in some embodiments, one or more hardware parameters of device 100, including those described in detail below, may be programmatically adjusted by one or more system controllers.
[0032] The reaction chamber 102 is in fluid communication with a reactant supply system 101 for supplying process gases to a distribution showerhead 106. The reactant supply system 101 comprises a mixing vessel for mixing and / or conditioning process gases for supply to the showerhead 106. One or more mixing vessel inlet valves 120 may control the introduction of process gases to the mixing vessel 104. Similarly, a showerhead inlet valve 105 may control the introduction of process gases to the showerhead 106.
[0033] Some reactants may be stored in liquid form until evaporation following delivery to the reaction chamber 102. For example, the embodiment of FIG. 1 includes an evaporation point 103 that evaporates the liquid reactants delivered to the mixing vessel 104. The evaporation point 103 may be omitted if the reactants are all gases. In some embodiments, the evaporation point 103 may be a heated evaporator. The reactant vapor generated from such an evaporator may condense in downstream supply piping. Exposure of incompatible gases to the condensed reactants may generate small particles. These small particles may clog piping, interfere with valve operation, contaminate wafers, etc. Some approaches to addressing these issues include cleaning and / or pumping vacuum on the supply piping to remove residual reactants. However, cleaning the supply piping may increase the cycle time of the reaction chamber and reduce the throughput of the reaction chamber. Thus, in some embodiments, the supply piping downstream of the evaporation point 103 may be heat traced. In some examples, the mixing vessel 104 may also be heat traced. In one non-limiting example, the piping downstream of the evaporation point 103 has a temperature profile that increases from about 100° C. to about 150° C. at the mixing vessel 104 .
[0034] In some embodiments, the liquid reactant may be vaporized in the liquid injector. For example, the liquid injector may inject a pulse of the liquid reactant into the carrier gas stream upstream of the mixing vessel 104. In one embodiment, the liquid injector may vaporize the reactant by rapidly switching the liquid from high pressure to low pressure. In another embodiment, the liquid injector may atomize the liquid into dispersed droplets that are then vaporized in the heated delivery tubing. It will be appreciated that smaller droplets may evaporate faster than larger droplets, reducing the delay between liquid injection and complete evaporation. Faster evaporation can reduce the length of tubing downstream from the evaporation point 103. In one scenario, the liquid injector may be attached directly to the mixing vessel 104. In another scenario, the liquid injector may be attached directly to the showerhead 106.
[0035] In some embodiments, a liquid flow controller (LFC) may be provided upstream of the evaporation point 103 to control the mass flow rate of liquid for evaporation and delivery to the reaction chamber 102. For example, the LFC may include a thermal mass flow meter (MFM) located downstream thereof. In response to a feedback control signal provided by a proportional integral derivative (PID) controller in electrical communication with the MFM, the plunger valve of the LFC may then be adjusted. However, it may take more than a second to stabilize the liquid flow rate using feedback control. This may extend the time to dose the liquid reactant. Thus, in some embodiments, the LFC may be dynamically switched between a feedback control mode and a direct control mode. In some embodiments, the LFC may be dynamically switched from the feedback control mode to the direct control mode by shutting down the sense tube and the PID controller of the LFC.
[0036] The reaction chamber 102 includes chamber walls 109 that enclose the reaction chamber 102 from the outside environment. The chamber walls 109 include chamber sidewalls, ceiling, floor, etc. The reaction chamber 102 further includes a showerhead 106 for distributing process gases. It will be appreciated that the showerhead 106 may have any suitable shape and may have any number and arrangement of ports for distributing process gases to the reaction chamber 102. The reaction chamber 102 further includes a chuck or pedestal 108 for supporting a wafer 112. In the embodiment illustrated in FIG. 1, the pedestal 108 and wafer 112 are shown positioned below the showerhead 106, with the wafer 112 resting on lift pins 130 of the pedestal 108. It will be appreciated that deposition of a protective coating on chamber components of the reaction chamber 102 may occur when the wafer 112 is not present in the reaction chamber 102, as described herein. However, it will be appreciated that, as described herein, deposition of a protective coating on chamber components of the reaction chamber 102 may occur while the wafer 112 is present in the reaction chamber 102. Chamber components on which the protective coating may be deposited include, but are not limited to, the chamber walls 109 (including sidewalls, ceiling, floor, etc.), the pedestal 108, the showerhead 106, and the lift pins 130.
[0037] In some embodiments, the area 107 is located between the showerhead 106 and the pedestal 108. In some embodiments, the position of the showerhead 106 or the position of the pedestal 108 may be adjusted to change the size of the area 107 between the showerhead 106 and the pedestal 108. It will be appreciated that the vertical position of the showerhead 106 and / or the pedestal 108 may be changed by any suitable mechanism. Examples of the size of the area 107 include, but are not limited to, a volume of about 0.1 liters to about 2 liters. Large areas may be required to accommodate relatively large chamber components. In some embodiments, a plasma glow discharge may be generated between the showerhead 106 and the pedestal 108 in the area 107 to deposit a protective coating on the chamber components. In some embodiments, a plasma glow discharge may be generated in an area adjacent to the chamber wall 109 outside the area 107 to deposit a protective coating on the chamber components.
[0038] As shown in FIG. 1, the showerhead 106 and the pedestal 108 may be in electrical communication with an RF power source 114 and a matching network 116 to power the plasma. In some embodiments, the plasma energy may be controlled by controlling one or more of the process station pressure, the gas concentration, the RF power source, the RF source frequency, the phase difference of the RF signal, and the timing of the plasma power pulse. For example, the RF power source 114 and the matching network 116 may operate at any suitable power to generate a plasma having a desired composition of radical species. Similarly, the RF power source 114 may provide RF power at any suitable frequency. In some embodiments, the RF power source 114 may be configured to control high frequency RF power and low frequency RF power sources independent of each other. Examples of low frequency RF frequencies may include, but are not limited to, frequencies from 50 kHz to 700 kHz. Examples of high frequency RF frequencies may include, but are not limited to, frequencies from 1.8 MHz to 2.45 GHz. The RF power source 114 may also control the phase difference of the RF signals provided to both the lower electrode and the upper electrode. For example, the phase difference can be anywhere between about 180 degrees and 0 degrees out of phase. It will be appreciated that any suitable parameters may be adjusted non-continuously or continuously to provide plasma energy for surface reactions. In one non-limiting example, the plasma power may be pulsed intermittently.
[0039] In some embodiments, the plasma may be monitored in situ with one or more plasma monitors. In one scenario, the plasma power may be monitored with one or more voltage power sensors (e.g., VI probes). In another scenario, the plasma density and / or process gas concentration may be measured with one or more optical emission spectroscopy (OES) sensors. In yet another scenario, the plasma position may be monitored and measured with one or more phase sensors. In some embodiments, one or more plasma parameters may be programmatically adjusted based on measurements from such in situ plasma monitors. Other plasma monitors may include, but are not limited to, infrared (IR) monitors, acoustic monitors, and pressure transducers.
[0040] In some embodiments, the plasma may be controlled by input / output control (IOC) array instructions. In one example, instructions for setting plasma conditions for a plasma process stage may be included in a corresponding plasma excitation recipe stage of a deposition process recipe. In some cases, the process recipe stages may be arranged in sequence such that all instructions for a deposition process stage are executed simultaneously with that process stage. In some embodiments, instructions for setting one or more plasma parameters may be included in a recipe stage prior to the plasma process stage. For example, a first recipe stage may include instructions for setting flow rates of inert and / or reactive gases, instructions for setting a plasma generator to a power set point, and time delay instructions for the first recipe stage. A subsequent second recipe stage may include instructions for starting the plasma generator and time delay instructions for the second recipe stage. A third recipe stage may include instructions for stopping the plasma generator and time delay instructions for the third recipe stage. It will be appreciated that these recipe steps may be further subdivided and / or repeated in any suitable manner within the scope of this disclosure.
[0041] In some embodiments, the RF power source 114 and matching network 116 may be omitted if the protective coating is formed by a thermally driven reaction rather than a plasma driven reaction. For example, the protective coating may be formed by thermal ALD. The RF power source 114 and matching network 116 may still be effective for non-deposition related processes, such as cleaning and treatment operations.
[0042] In some embodiments, the pedestal 108 may be temperature controlled by a heater 110. Additionally, in some embodiments, pressure control of the reaction chamber 102 may be provided by an exhaust valve 118. As shown in FIG. 1, the exhaust valve 118 regulates the vacuum provided by a downstream vacuum pumping system (not shown). The vacuum pumping system may include a roughing pump and / or a turbomolecular pump. However, in some embodiments, pressure control of the reaction chamber 102 may be adjusted by modifying the flow rate of one or more gases introduced into the reaction chamber 102.
[0043] In some embodiments, the controller 150 is part of a system that may be part of the apparatus 100. Such systems may include processing tools, chambers, processing platforms, and / or semiconductor processing equipment with specific processing components (wafer pedestals, gas flow systems, etc.). These systems may be integrated with electronics for controlling pre-, during, and post-processing operations of the semiconductor wafer or substrate. This electronics may be referred to as a "controller" and may control various components or sub-components of the system. The controller may be programmed to control any of the processes disclosed herein, including supply of process gases, temperature settings, pressure settings, vacuum settings, power settings, RF generator settings, RF matching circuit settings, phase difference settings, frequency settings, flow rate settings, fluid supply settings, position operation settings, wafer loading and unloading from tools and other transport tools, and / or wafer loading and unloading from load locks connected or coupled to the specific system, depending on the processing conditions and / or type of system.
[0044] The controller 150 may be in operational communication with the apparatus 100. In some embodiments, the controller 150 comprises a processor system (e.g., a microprocessor) configured to execute instructions held in a data system (e.g., a memory). In some embodiments, the controller 150 may be in communication with a plasma generator controller to control plasma parameters and / or plasma conditions. In some embodiments, the controller 150 may be in communication with the pedestal 108 to control the pedestal lift and temperature. The controller 150 may include instructions for controlling process conditions of operation of the apparatus 100. The controller 150 will typically include one or more memory devices and one or more processors. The processor may include a CPU or calculator, analog and / or digital input / output connections, stepper motor controller boards, etc. Instructions for performing appropriate control operations are executed by the processor. These instructions may be stored in a memory device associated with the controller 150 or provided over a network.
[0045] In some embodiments, the controller 150 may control all or most of the operation of the apparatus 100. For example, the controller 150 may execute system control software including a set of instructions for controlling plasma generation, plasma position, and parameters (e.g., gas flow composition and temperature) during deposition of a protective coating in the reaction chamber 102. In some embodiments, the controller 150 may execute control software including a set of instructions for controlling chamber pressure, gas flow rates, phase difference of RF signals, and other parameters (including coating of chamber components with a protective coating). In some embodiments, other computer programs, scripts, or routines stored in a memory device associated with the controller 150 may be used.
[0046] In some embodiments, the controller 150 may be configured with instructions to perform an operation of depositing a protective coating on a surface of a plurality of chamber components of the reaction chamber 102, the plurality of chamber components being part of the reaction chamber 102, the protective coating being deposited by plasma enhanced chemical vapor deposition (PECVD), plasma enhanced atomic layer deposition (PEALD), or thermal atomic layer deposition (thermal ALD) at a temperature above about 200° C. In some embodiments, the controller 150 may be further configured with instructions to perform an operation of depositing a film material on a surface of the plurality of chamber components of the reaction chamber 102 in the protective coating, the film material being etched at a substantially higher rate than the protective coating during exposure to a fluorine-based etch, a chlorine-based etch, a bromine-based etch, or an iodine-based etch. In some embodiments, the controller 150 may be further configured with instructions to perform an operation of controlling an RF signal provided to the reaction chamber such that a majority of the plasma glow discharge forms in one or more regions outside of a region adjacent to the pedestal 108.
[0047] In general, the controller 150 may be defined as electronic equipment having various integrated circuits, logic, memory, and / or software that receive instructions, issue instructions, control operations, enable cleaning operations, enable endpoint measurements, etc. The integrated circuits may include chips in firmware format that store program instructions, digital signal processors (DSPs), chips defined as application specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute the program instructions (e.g., software). The program instructions may be instructions communicated to the controller in the form of various personalizations (or program files) that define operational parameters for performing a particular process on or for a semiconductor wafer or for a system. In some embodiments, the operational parameters may be part of a recipe defined by a process engineer to accomplish one or more layers, materials, surfaces, circuits, and / or one or more processing steps during the manufacture of a wafer die.
[0048] In some embodiments, the controller 150 may be part of or coupled to a computer that is integrated or coupled with the system, or otherwise networked or combined with the system. For example, the controller 150 may be in the "cloud" or may be all or part of a fab host computer system, allowing remote access of wafer processing. The computer may allow remote access to the system to monitor the progress of a manufacturing operation, examine the history of past manufacturing operations, and examine trends or performance criteria from multiple manufacturing operations to modify parameters of a current process, set up a processing step following a current process, or start a new process. In some examples, a remote computer (e.g., a server) may provide a process recipe to the system over a network, which may include a local network or the Internet. The remote computer may include a user interface that allows entry or programming of parameters and / or settings that are then communicated from the remote computer to the system. In some examples, the controller 150 receives instructions in the form of data that specify parameters for each processing step to be performed during one or more operations. It should be understood that the parameters may be specific to the type of process being performed and the type of tool that the controller 150 is configured to connect to or control. Thus, as described above, the controller 150 may be distributed, for example by including one or more individual controllers networked together and cooperating toward a common purpose, such as the process and control described herein. An example of a controller distributed for such a purpose would be one or more integrated circuits of a chamber that are located remotely (e.g., at the platform level or as part of a remote computer) and that cooperate to control a process in the chamber.
[0049] As noted above, depending on the process steps being performed by the tool, the controller 150 may be in communication with one or more of other tool circuits or tool modules, other tool components, cluster tools, other tool interfaces, adjacent tools, nearby tools, tools installed throughout the factory, a main computer, another controller, or tools used to transport materials to and from tool locations and / or load ports in a semiconductor manufacturing factory.
[0050] The above-mentioned apparatus / processes may be used in conjunction with lithographic patterning tools or processes, for example, for the fabrication or manufacture of semiconductor devices, displays, LEDs, solar panels, etc. Such tools / processes will usually (but not necessarily) be used or performed together in a common fabrication facility. Lithographic patterning of a film typically includes some or all of the following operations: (1) applying photoresist to a workpiece (i.e., substrate) using a spin-on or spray-on tool; (2) curing the photoresist using a hotplate, furnace, or UV curing tool; (3) exposing the photoresist to visible, UV, or X-ray light using a tool such as a wafer stepper; (4) developing and thereby patterning the photoresist to selectively remove the resist using a tool such as a wet bench; (5) transferring the resist pattern to an underlying film or workpiece using a dry etching tool or a plasma-assisted etching tool; and (6) removing the resist using a tool such as an RF or microwave plasma resist stripper, each of which may be performed in several possible tools. In-situ protective coating
[0051] The present disclosure relates to in-situ deposition of protective coatings on chamber components in a reaction chamber. The in-situ protective coatings may be deposited on chamber walls and other exposed internal surfaces of chamber components in a reaction chamber. The in-situ protective coatings are deposited in a high temperature and / or plasma environment to withstand subsequent plasma processing, high temperature processing, and other harsh processing conditions. For example, the in-situ protective coatings may be deposited in a reaction chamber at a temperature above about 200° C., or from about 250° C. to about 650° C. The material of the in-situ protective coating may be highly resistant to one or more halogen-based chemicals. A layer subsequently deposited on the in-situ protective coating may have a different etch selectivity than the in-situ protective coating. In some embodiments, the in-situ protective coating is deposited prior to use in wafer processing in the reaction chamber. In some embodiments, the in-situ protective coating is deposited or redeposited after one or more wafers are processed in the reaction chamber. The reaction chamber may be part of a processing apparatus, such as the apparatus 100 of FIG. 1.
[0052] As used herein, the protective coating is considered to be deposited "in situ" on a chamber component that is part of a reaction chamber. That is, deposition of the protective coating is performed on a chamber component that serves its intended purpose (as a showerhead, lift pin, etc.) when the chamber component is installed in the reaction chamber. Thus, the chamber component is coated in the same reaction chamber in which the chamber component is involved in the fabrication process. The chamber component does not necessarily have to be coated in another chamber of which it is a part. As used herein, the in situ protective coating of the present disclosure may be referred to as a protective coating, a surface coating, an in situ coating, an undercoat, a conditioning layer, a protective layer, a surface layer, an in situ layer, etc.
[0053] As discussed above, the protective coating of the present disclosure may be deposited using PECVD or ALD techniques. In some embodiments, the protective coating may be deposited by thermal ALD or plasma-enhanced ALD (PEALD). The deposition process may supply reactive gases to the wafer surface to induce reactions in a plasma or thermal environment to form a film of material. PECVD uses plasma to enhance the film deposition mechanism and can provide high growth rates and high throughput of materials. ALD uses two or more process gases introduced in alternating sequence. ALD uses surface self-limiting reactions to deposit films layer by layer. PECVD uses active gas phase reactions for deposition, while ALD uses surface-mediated deposition reactions for layer by layer deposition. A typical ALD cycle includes (i) a dose of precursor material delivered and adsorbed on the substrate surface; (ii) purging excess precursor material from the chamber and leaving a self-limiting monolayer on the substrate surface, (iii) providing a reactant material that reacts with the adsorbed precursor material, and (iv) purging unreacted reactants or reaction by-products from the chamber. The deposition reaction of the ALD cycle may be thermally or plasma induced. ALD may be used to form highly conformal films.
[0054] A protective coating or undercoat may be deposited on surfaces of chamber components of a reaction chamber. The protective coating may be deposited in situ to reduce particle contamination and defect issues in wafer processing. The protective coating may be formed under high temperature and / or plasma conditions in the reaction chamber to provide a high quality coating.
[0055] 2A shows a flow diagram of an exemplary ALD method for coating multiple chamber components of a reaction chamber, according to some embodiments. The operations of process 200a of FIG. 2A may include additional operations, fewer operations, or different operations. The ALD method may include thermal ALD or PEALD.
[0056] In block 210 of process 200a, a first reactant is introduced into the reaction chamber in a vapor phase and adsorbs onto the surfaces of multiple chamber components that are part of the reaction chamber. The first reactant adsorbs onto the exposed surfaces of the chamber components in a self-limiting manner. The first reactant is provided to the reaction chamber in a dose phase of an ALD cycle, and an exemplary dose time for the first reactant can be from about 1 second to about 30 seconds. In some embodiments, the dose phase in block 210 can be followed by a purge phase, which can purge any excess first reactant from the reaction chamber. In some embodiments, the first reactant can include a metal-containing precursor and / or a silicon-containing precursor.
[0057] In block 220 of process 200a, a second reactant is introduced in a gas phase into the reaction chamber. There, the first reactant and the second reactant react to deposit a layer of a protective coating on the surfaces of a number of chamber components at a temperature above about 200° C. In some cases, the reaction is thermally driven, and in some cases, the reaction is plasma driven. In some embodiments, the deposition reaction occurs in a high temperature environment. The high temperature environment includes a temperature above about 200° C., about 225° C. to about 700° C., about 250° C. to about 650° C., or about 300° C. to about 600° C. It will be appreciated that in the deposition of some protective coatings, the high temperature environment is not necessarily for depositing a high quality film. The high temperature environment may be sustained throughout the reaction by ensuring that the reaction chamber reaches and maintains a high temperature, or at least by ensuring that chamber components, such as the substrate support (e.g., pedestal), reach and maintain a high temperature.
[0058] The second reactant adsorbs on the exposed surfaces of the chamber components and forms an adsorption-controlled amount of a protective coating. The second reactant is provided to the reaction chamber in a reaction stage of an ALD cycle. The reaction stage of the ALD cycle may expose the surfaces of multiple chamber components to plasma and / or high temperature, and such exposure may last for a period of time from about 0.5 seconds to about 20 minutes. In some embodiments, the reaction at block 220 may be followed by a purge stage, which may purge any excess second reactant and by-products from the reaction chamber. In some embodiments, the second reactant may include an oxygen-containing gas (e.g., O2), a nitrogen-containing gas (e.g., N2 or NH3), or a carbon-containing gas. The plasma-activated species of the second reactant may include radicals and / or ions of the second reactant.
[0059] The protective coating may be deposited on the surfaces of multiple chamber components without a wafer in the reaction chamber. Thus, the ALD cycles to deposit the protective coating occur without a wafer in the reaction chamber. However, it will be appreciated that in some cases, the protective coating may be deposited on the surfaces of multiple chamber components with a wafer in the reaction chamber. In some embodiments, blocks 210 and 220 are repeated such that multiple ALD cycles are performed to form a protective coating of a desired thickness. In some embodiments, the thickness of the protective coating is about 0.1 μm to about 4 μm, or about 0.5 μm to about 3 μm, or about 0.5 μm to about 2 μm.
[0060] The protective coating may be resistant to at least some halogen-based chemicals, which may include fluorine-based species (e.g., F2, HF3, ClF3), chlorine-based species (e.g., Cl2, ClF3, BCl3), bromine-based species (e.g., HBr), iodine-based species (e.g., I2), or combinations thereof. Exposure to the halogen-based chemicals may occur during deposition, etching, and / or cleaning processes. The halogen-based chemicals may include halogen-containing etchants, halogen-containing precursors, and halogen-containing by-products. The protective coating may be deposited on surfaces of multiple chamber components to protect them from impingement. In some embodiments, the resistance of the protective coating to a particular halogen-based chemical may be measured or determined by its etch rate. In some embodiments, the protective coating has an etch rate of less than about 10 Å / min, less than about 5 Å / min, less than about 3 Å / min, less than about 1 Å / min, or between about 0.01 Å / min and about 1 Å / min when exposed to one or more halogen-based chemicals. The etch rate may vary depending on the type of halogen-based chemical. For example, the protective coating may be resistant to fluorine-based species but not chlorine-based species. In some embodiments, removal of the protective coating may occur using another chemistry that does not damage the underlying material (e.g., aluminum) of the chamber component.
[0061] In some embodiments, the protective coating comprises an oxide, a nitride, a carbide, or a combination thereof. For example, the protective coating may comprise silicon oxide (SiO2), aluminum oxide (Al2O3), zirconium oxide (ZrO2), hafnium oxide (HfO2), tin oxide (SnO2), or silicon nitride (Si3N4). It will be appreciated that the protective coating may include other types of materials that are resistant to halogen-based chemicals, but are not limited to binary metal oxides, nitrides, or carbides. The etch rate of the protective coating depends on its composition and the chemicals to which it is exposed. For example, Al2O3 may be highly resistant to chlorine-based species, ZrO2 may be highly resistant to fluorine-based and bromine-based species, HfO2 may be highly resistant to chlorine-based species, SnO2 may not be resistant to chlorine-based species, and SiO2 may not be resistant to fluorine-based species. Thus, a deposited layer of SiO2 may be removed at a high etch rate when exposed to a chlorine-based species, while a protective coating of Al2O3 may be removed at a much slower etch rate when exposed to the same chlorine-based species. Table 1 lists protective coatings and their relative etch rates when exposed to specific halogen-based chemicals. [Table 1] A protective coating having a low etch rate to a particular halogen-based chemical is promising as a protective coating if the etched film has a high etch rate when etched by the particular halogen-based chemical.
[0062] Deposition of a protective coating under certain processing conditions improves the quality of the coating. In some embodiments, the quality of the coating may be at least correlated with its density. Thus, a protective coating deposited in situ under processing conditions described herein (e.g., high temperature) may have a higher density than a coating deposited ex situ and / or under different processing conditions (e.g., low temperature). This may be true even if the coatings share the same composition. Due to the improved density, the protective coating may be substantially pinhole-free. In some embodiments, processing conditions for depositing high quality coatings include a high temperature range (e.g., greater than about 200° C.). In some embodiments, processing conditions for depositing high quality coatings include a low chamber pressure (e.g., less than about 10 Torr). In some embodiments, high quality coatings last longer and can sustain thermal and plasma stresses compared to coatings deposited ex situ and / or under different processing conditions.
[0063] Deposition of protective coatings by ALD typically provides high conformality. In some embodiments, conformality may be calculated by comparing the average thickness of the deposited film on the bottom, sidewall, or top surface of the feature to the average thickness of the deposited film on the bottom, sidewall, or top surface of the feature. For example, conformality may be calculated by dividing the average thickness of the deposited film on the sidewall by the average thickness of the deposited film on the top surface of the feature and multiplying by 100 to get a percentage. In some embodiments, the conformality of the protective coating is about 50% to about 100%, about 80% to about 100%, or about 85% to about 100%.
[0064] In some embodiments, the surfaces of the chamber components include exposed inner surfaces of the chamber components of the reaction chamber. Conditions of the ALD process performed in blocks 210 and 220 can be adjusted to promote conformal deposition of a high quality in situ protective coating on the exposed inner surfaces of the chamber components. In some embodiments, the chamber components include chamber walls, which can include sidewalls, floor, and ceiling of the reaction chamber. In some embodiments, a plasma glow discharge can be generated in an area adjacent to the chamber walls of the reaction chamber to direct the plasma to the chamber walls. In some cases, the plasma glow discharge can be generated in an area outside the area between the showerhead and the pedestal of the reaction chamber. Directing the plasma to the chamber walls can promote a more uniform, more complete, and more conformal deposition of the protective coating on the exposed inner surfaces of the chamber components.
[0065] In some embodiments, the plasma may be directed toward the chamber walls by controlling the phase between the RF signals provided to each of the showerhead and pedestal of the reaction chamber, or more generally, between the RF signals provided to each of the upper and lower electrodes of the reaction chamber. Controlling the phase difference between the RF signals provided to the upper and lower electrodes helps to control the location of the plasma glow discharge generated in the reaction chamber. The phase difference between a first phase of the RF signal provided to the upper electrode and a second phase of the RF signal provided to the lower electrode may be approximately 180 degrees to 0 degrees out of phase. For example, the phase difference between the upper and lower electrodes may be substantially 0 degrees out of phase such that the plasma glow discharge is centered near the chamber walls.
[0066] In some embodiments of the process 200a, a film material is deposited on the surfaces of multiple chamber components of the reaction chamber and is etched at a substantially higher rate than the protective coating during exposure to a fluorine-based etch, a chlorine-based etch, a bromine-based etch, or an iodine-based etch. The film material may be removed from the reaction chamber without removing the protective coating. In some embodiments, the film material is deposited on the wafer and anywhere in the reaction chamber in the reaction. In some embodiments, the film material is deposited on the protective coating as an additional protective layer. Depending on the deposition / etch / clean chemistry expected to be provided by the reaction chamber, multiple protective coatings may be selected to be deposited on the surfaces of the chamber components. A first protective coating may be resistant to a first etchant, and a second protective coating may be resistant to a second etchant. For example, the second protective coating may include Al2O3 to resist a chlorine-based etchant, and the first protective coating may include ZrO2 to resist a fluorine-based etchant. It will be appreciated that additional protective coatings may be deposited on the surfaces of multiple chamber components depending on the etching / cleaning operations expected to be performed in the reaction chamber, each protective coating being selected for resistance to a particular etching / cleaning chemistry.
[0067] In block 240 of the process 200a, a film material is deposited on the wafer and the protective coating in the reaction chamber as needed. After the protective coating is deposited on the surfaces of the plurality of chamber components, the wafer may be introduced into the reaction chamber for processing. The film material may be formed of a material different from that of the protective coating. For example, the film material may include metals, metal oxides, dielectric materials, semiconductive materials, etc. When depositing the film material on the wafer, deposition of the film material may occur on the surfaces of the plurality of chamber components. The thickness of the film material on the wafer may be greater than the thickness of the film material on the surfaces of the plurality of chamber components.
[0068] In block 250 of process 200a, the film material on the protective coating is optionally etched, the film material being etched at a substantially faster rate than the protective coating. Substantially faster herein may be an etch rate that is greater than 5 times, greater than 10 times, or greater than 100 times. In some embodiments, the film material may be etched from the wafer in addition to being etched from the surfaces of the chamber components. The film material may be etched using a halogen-based etchant, the halogen-based etchant including a fluorine-based species, a chlorine-based species, a bromine-based species, an iodine-based species, or combinations thereof. The halogen-based etchant may be used as part of a cleaning process to remove the film material from the reaction chamber. The film material has a different etch selectivity than the underlying protective coating. The etchant may be selective for the film material relative to the protective coating. In some embodiments, the etch selectivity of the film material relative to the protective coating is greater than about 10:1 when exposed to a halogen-based etchant. In this manner, the protective coating may be protected when cleaning the film from the reaction chamber. In some embodiments, the endpoint etch may be used to determine when the halogen-based etchant has completed etching the membrane material so that the protective coating is not etched. In some embodiments, the composition of the protective coating may be selected depending on the resistance properties required when the chamber component surface is exposed to a particular type of deposition or cleaning chemical.
[0069] In block 260 of process 200a, a protective coating is redeposited on the surfaces of the chamber components of the reaction chamber as needed. After processing one or more wafers in the reaction chamber, the protective coating initially deposited in blocks 210 and 220 may degrade or corrode over time. It will be appreciated that the protective coating may be deposited at the beginning of use of the reaction chamber, or may be deposited / redeposited on the surfaces of the chamber components after use of the reaction chamber. In some embodiments, the protective coating is redeposited using the same processing conditions as described in blocks 210 and 220. This allows for "healing" of the protective coating after use of the reaction chamber. In some embodiments, the protective coating is redeposited on the surfaces of the chamber components after processing hundreds of thousands of wafers. In some embodiments, the redeposition of the protective coating may occur periodically and automatically.
[0070] 2B shows a flow diagram of an example method for coating multiple chamber components of a reaction chamber according to some embodiments. The operations of process 200b of FIG. 2B may include additional operations, fewer operations, or different operations.
[0071] In block 230 of the process 200b, a protective coating is deposited on the surfaces of a plurality of chamber components that are part of the reaction chamber. The protective coating is deposited by plasma enhanced chemical vapor deposition (PECVD), plasma enhanced atomic layer deposition (PEALD), or thermal atomic layer deposition (thermal ALD) at a temperature above about 200° C. The protective coating may be deposited on the surfaces of the plurality of chamber components with or without a wafer in the reaction chamber. In some embodiments, the thickness of the protective coating is about 0.1 μm to about 4 μm, or about 0.5 μm to about 3 μm, or about 0.5 μm to about 2 μm.
[0072] Aspects of depositing a protective coating on surfaces of multiple chamber components by PEALD and thermal ALD are described in blocks 210 and 220 of Figure 2A. In embodiments in which PECVD is used, a protective coating may be deposited on surfaces of multiple chamber components with a higher throughput than ALD methods, but may not achieve a higher conformality than ALD methods.
[0073] In some embodiments, the protective coating may be deposited at an elevated temperature greater than about 200° C., from about 225° C. to about 700° C., from about 250° C. to about 650° C., or from about 300° C. to about 600° C. The high temperature environment may be sustained during the reaction by ensuring that the reaction chamber reaches and maintains the elevated temperature, or at least by ensuring that chamber components, such as the substrate support, reach and maintain the elevated temperature.
[0074] The protective coating may be resistant to at least some halogen-based chemicals, which may include fluorine-based species (e.g., F2, NF3, ClF3), chlorine-based species (e.g., Cl2, ClF3), bromine-based species (e.g., HBr), iodine-based species (e.g., I2), or combinations thereof. Exposure to halogen-based chemicals may occur during deposition, etching, and / or cleaning processes. The halogen-based chemicals may include halogen-containing etchants, halogen-containing precursors, and halogen-containing by-products. In some embodiments, the etch rate of the protective coating is less than about 10 Å / min, less than about 5 Å / min, less than about 3 Å / min, less than about 1 Å / min, or from about 0.01 Å / min to about 1 Å / min when exposed to one or more halogen-based chemicals. The etch rate may vary depending on the type of halogen-based chemical.
[0075] In some embodiments, the protective coating comprises an oxide, a nitride, a carbide, or a combination thereof. For example, the protective coating may comprise SiO2, Al2O3, ZrO2, HfO2, SnO2, or Si3N4. It will be appreciated that the protective coating is not limited to binary metal oxides, nitrides, or carbides, but may include other types of materials that are resistant to halogen-based chemistries. The etch rate of the protective coating depends on its composition and the chemicals to which it is exposed.
[0076] Protective coatings deposited in situ and under the process conditions described herein may have a higher density and therefore higher quality than coatings deposited ex situ and / or under different process conditions, even when they share the same composition. Due to the increased density, the protective coating may be substantially pinhole-free. The protective coating may last longer and sustain thermal and plasma stresses compared to coatings deposited ex situ and / or under different process conditions.
[0077] In some embodiments, the surfaces of the chamber components include exposed inner surfaces of the chamber components of the reaction chamber. In some embodiments, the chamber components include chamber walls, which may include sidewalls, a floor, and a ceiling of the reaction chamber. In some embodiments, the plasma glow discharge may be generated in an area adjacent to the chamber wall of the reaction chamber to direct the plasma to the chamber wall. The plasma glow discharge may be generated in an area outside the area between the showerhead and the pedestal of the reaction chamber.
[0078] In some embodiments, the plasma may be directed toward the chamber walls by controlling the phase between the RF signals provided to each of the showerhead and pedestal of the reaction chamber, or more generally, between the RF signals provided to each of the upper and lower electrodes of the reaction chamber. Controlling the phase difference between the RF signals provided to the upper and lower electrodes helps to control the location of the plasma glow discharge generated in the reaction chamber. The phase difference between a first phase of the RF signal provided to the upper electrode and a second phase of the RF signal provided to the lower electrode may be approximately 180 degrees to 0 degrees out of phase. For example, the phase difference between the upper and lower electrodes may be substantially 0 degrees out of phase such that the plasma glow discharge is centered near the chamber walls.
[0079] In some embodiments of process 200b, a film material is deposited on the surfaces of multiple chamber components of the reaction chamber and etches at a substantially higher rate than the protective coating during exposure to a fluorine-based etch, a chlorine-based etch, a bromine-based etch, or an iodine-based etch. Multiple protective coatings may be selected to be deposited on the surfaces of the chamber components depending on the deposition / etch / clean chemistries that the reaction chamber is expected to provide. One protective coating may be resistant to a first etchant, and another protective coating may be resistant to a second etchant. For example, the second protective coating may include Al2O3 to resist a chlorine-based etchant, and the protective coating deposited in block 230 may include ZrO2 to resist a fluorine-based etchant. It will be appreciated that additional protective coatings may be deposited on the surfaces of multiple chamber components depending on the deposition / etch / clean operations that are expected to be performed in the reaction chamber. Each protective coating may be selected for resistance to a particular chemical.
[0080] As shown in process 200b of FIG. 2B, blocks 240, 250, and 260 may be performed after block 230, if necessary. Embodiments of blocks 240, 250, and 260 are described in process 200a of FIG. 2A. A film material may be deposited on the wafer and a protective coating in the reaction chamber in block 240. The film material on the protective coating may be etched at a substantially higher rate than the protective coating in block 250. The protective coating may be redeposited on surfaces of multiple chamber components of the reaction chamber in block 260.
[0081] Incomplete coverage of the in situ protective coatings described in the present disclosure may be avoided or otherwise mitigated by advancing the deposition to the surfaces of the chamber components of the reaction chamber. More complete coverage may provide a more uniformly deposited protective coating that is less porous than a typical undercoat. In some embodiments, more complete coverage may be achieved using an apparatus configured to control the position of the plasma glow discharge such that the plasma is more directed toward the surfaces of the chamber components of the reaction chamber. In some embodiments where thermal ALD is provided, more complete coverage may be achieved using an apparatus configured to heat the surfaces of the chamber components of the reaction chamber to high temperatures.
[0082] 3A-3C show an exemplary plasma apparatus comprising a reaction chamber configured to direct a plasma such that a protective coating is deposited on at least the chamber walls of the reaction chamber. Aspects of such a plasma apparatus are described in more detail in U.S. patent application Ser. No. 15 / 786,497, filed Oct. 17, 2017, entitled "METHODS AND SYSTEMS FOR CONTROLLING PLASMA GLOW DISCHARGE IN A PLASMA CHAMBER," the entire contents of which are incorporated by reference for all purposes.
[0083] FIG. 3A illustrates a schematic cross-section of an exemplary plasma apparatus including a reaction chamber in which a plasma glow discharge is generated between an upper electrode and a lower electrode, according to some embodiments. The reaction chamber 300 includes a chamber wall 302. The chamber wall 302 may be grounded by an electrical ground 310. The upper electrode 304 may function as a showerhead for distributing process gases to the reaction chamber 300, and the lower electrode 306 may function as a pedestal for supporting a wafer in the reaction chamber 300. In some embodiments, an RF power source 320 is coupled to one of the electrodes 304 and 306 and a ground 308, and is coupled together to both the upper electrode 304 and the lower electrode 306. The RF power source 320 may be connected to a controller 322, which may include a phase change control. The controller 322 may be configured to modulate a phase of an RF signal output from the RF power source 320. In some embodiments, the controller 322 may be configured to modulate a phase difference between a first phase supplied to the upper electrode 304 and a second phase supplied to the lower electrode 306. The position of the plasma glow discharge 330 can be affected by the phase difference, which can be anywhere from about 0 degrees to 180 degrees out of phase.
[0084] 3A, the reaction chamber 300 may provide a plasma glow discharge 330 that is centered between the upper electrode 304 and the lower electrode 306. In some embodiments, the phase difference between the RF signals provided to the upper electrode 304 and the lower electrode 306 may be substantially 180 degrees out of phase. By controlling the phase difference to be out of phase, more of the plasma glow discharge 330 may be contained between the upper electrode 304 and the lower electrode 306. However, by controlling the phase difference to be less than 180 degrees out of phase and closer to 0 degrees out of phase, the plasma glow discharge 330 may move toward the chamber wall 302.
[0085] FIG. 3B illustrates a schematic cross-section of an exemplary plasma apparatus comprising the reaction chamber of FIG. 3A, in which a plasma glow discharge is generated adjacent to a chamber wall of the reaction chamber, according to some embodiments. In the reaction chamber 300, the plasma glow discharge 340 is pushed or moved toward the chamber wall 302, which provides a path to electrical ground 310. The plasma is not ignited, or is substantially not ignited, between the upper electrode 304 and the lower electrode 306, and is directed toward the electrical ground 310 of the chamber wall 302. In other words, the plasma glow discharge 340 is located in an area outside the area adjacent to the lower electrode 306. In some embodiments, the phase difference between the RF signals provided to the upper electrode 304 and the lower electrode 306 may be substantially 0 degrees out of phase. That is, the RF signals are provided to the upper electrode 304 and the lower electrode 306 substantially in phase. By controlling the phase difference to be in phase, the plasma glow discharge 340 can be adjacent to the chamber wall 302, including the sidewall, floor, and ceiling of the reaction chamber 300.
[0086] FIG. 3C illustrates a schematic cross-section of an exemplary plasma apparatus including the reaction chamber of FIGS. 3A and 3B with a protective coating deposited on the chamber walls of the reaction chamber, according to some embodiments. By controlling the position of the plasma glow discharge 340 adjacent to the chamber walls 302, the plasma may be preferentially directed to the exposed inner surfaces of multiple chamber components, including the chamber walls 302. Such surfaces may include sidewalls, floors, ceilings, portions of the showerhead, portions of the substrate support, portions of lift pins, portions of gas lines, and / or portions of nozzles that would otherwise be difficult to expose to the plasma. In some embodiments, the plasma may be preferentially directed anywhere throughout the reaction chamber 300. Directing the plasma in such a manner allows the protective coating to be deposited on the exposed inner surfaces of multiple chamber components that would otherwise be difficult to cover. This allows for more complete coverage of the protective coating 350 throughout the reaction chamber 300. As shown in FIG. 3C, the protective coating 350 is formed on the chamber walls 302, the surface of the upper electrode 304, and the surface of the lower electrode 306. It will be appreciated that the thickness of the protective coating 350 on the surfaces of the top electrode 304 and bottom electrode 306 may be less than the thickness of the protective coating 350 on the chamber walls 302. The protective coating 350 is deposited in a high temperature environment, which may be greater than about 200° C. The protective coating 350 is selective to various halogen-based chemistries. The protective coating 350 is a high quality in-situ protective coating as described in this disclosure.
[0087] FIG. 4A depicts a schematic cross-section of an exemplary reaction chamber with a film material deposited on a wafer and a protective coating, according to some embodiments. The reaction chamber 400 comprises a chamber wall 402 with a protective coating 444 deposited thereon. The protective coating 444 may be selected in terms of etch selectivity to a film that will subsequently be deposited in the reaction chamber 400 and in terms of the deposition / etch / clean chemistries to which the reaction chamber 400 will be exposed. In FIG. 4A, a film material 442a is deposited on a wafer 436 supported on a pedestal 406. A film material 442b is also deposited on the chamber wall 402 and has the same composition as the film material 442a deposited on the wafer 436. In some embodiments, the film materials 442a and 442b include a metal, a metal oxide, a dielectric material, or a semiconducting material. The film material 442b deposited on the chamber wall 402 is deposited on the protective coating 444.
[0088] FIG. 4B illustrates a schematic cross-section of the exemplary reaction chamber of FIG. 4A where the membrane material is etched from the wafer and selectively etched from the protective coating, according to some embodiments. The membrane material 442a is etched from the wafer 436, and the membrane material 442b on the chamber walls 402 is selectively etched such that the protective coating 444 is maintained on the chamber walls 402. In some embodiments, a halogen-based etchant is used to perform the etching process, and the protective coating 444 is resistant to the halogen-based etchant chemistry. Thus, the membrane material 442b is etched at a substantially higher rate than the protective coating 444 during the etching process. The halogen-based etchant may be selected as part of an etching / cleaning operation to remove the membrane materials 442a and 442b from the reaction chamber 400, and the protective coating 444 may be selected to be resistant to the halogen-based etchant. conclusion
[0089] In the foregoing description, numerous specific details are set forth in order to provide a thorough understanding of the present embodiments. The disclosed embodiments may be practiced without some or all of these specific details. In other instances, well-known process operations have not been described in detail so as not to unnecessarily obscure the disclosed embodiments. While the disclosed embodiments are described in conjunction with specific embodiments, it will be understood that they are not intended to limit the disclosed embodiments.
[0090] Although the above embodiments have been described in some detail for clarity of understanding, it will be apparent that certain changes and modifications may be implemented within the scope of the appended claims. It should be noted that there are many alternative ways of implementing the processes, systems, and apparatus of the present embodiments. Thus, the present embodiments should be considered as illustrative rather than restrictive, and should not be limited to the details described herein.
Claims
1. 1. A method comprising: introducing a gas phase first reactant into a reaction chamber such that the first reactant adsorbs onto surfaces of a plurality of chamber components, the plurality of chamber components being a part of the reaction chamber; introducing a second reactant in a gas phase into the reaction chamber, wherein the first reactant and the second reactant react to deposit a protective coating on the surfaces of the plurality of chamber components at a temperature greater than about 200° C.; A method comprising:
2. 2. The method of claim 1 , The method, wherein the first reactant reacts with the second reactant in a plasma-enhanced atomic layer deposition (PEALD) process.
3. The method of claim 2 further comprising: controlling a radio frequency (RF) signal supplied to the reaction chamber such that a majority of a plasma glow discharge of the second reactant forms in one or more regions outside a region between an upper electrode and a lower electrode.
4. 4. The method of claim 3, A method wherein a phase difference between a first phase of the RF signal supplied to the upper electrode and a second phase of the RF signal supplied to the lower electrode is about 180 degrees to 0 degrees out of phase.
5. 5. The method of claim 4, The phase difference is about 0 degrees out of phase.
6. 2. The method of claim 1 , The method, wherein the first reactant reacts with the second reactant in a thermal ALD process.
7. The method according to any one of claims 1 to 6, The method, wherein the protective coating comprises an oxide, a nitride, a carbide, or a combination thereof.
8. 8. The method of claim 7, The protective coating is made of silicon oxide (SiO 2 ), aluminum oxide (Al 2 O 3 ), zirconium oxide (ZrO 2 ), hafnium oxide (HfO 2 ), tin oxide (SnO 2 ), or silicon nitride (Si 3 N 4 ).
9. The method according to any one of claims 1 to 6, The method, wherein a material of one or more of the chamber components comprises aluminum (Al).
10. The method according to any one of claims 1 to 6, The method, wherein the plurality of chamber components includes at least a chamber wall of the reaction chamber.
11. The method according to any one of claims 1 to 6, further comprising: depositing a film material onto the wafer and onto the protective coating in the reaction chamber; Etching the film material on the wafer and on the protective coating, the film material being etched at a substantially faster rate than the protective coating; A method comprising:
12. 12. The method of claim 11, The method, wherein the etchant used to etch the membrane material comprises a fluorine-based species, a chlorine-based species, a bromine-based species, an iodine-based species, or a combination thereof.
13. 12. The method of claim 11 further comprising: the method including redepositing the protective coating on the surfaces of the plurality of chamber components of the reaction chamber after etching the membrane material.
14. The method according to any one of claims 1 to 6, The method, wherein the first reactant reacts with the second reactant to deposit the protective coating on the surfaces of the plurality of chamber components at a temperature of about 250° C. to about 650° C.
15. 1. A method comprising:
1. A method comprising: depositing a protective coating on surfaces of a plurality of chamber components of a reaction chamber, the plurality of chamber components being part of the reaction chamber, and the protective coating being deposited at a temperature greater than about 200° C. by plasma-enhanced chemical vapor deposition (PECVD), plasma-enhanced atomic layer deposition (PEALD), or thermal atomic layer deposition (thermal ALD).
16. 16. The method of claim 15 further comprising:
11. The method of claim 10, further comprising: depositing a film material on the protective coating on the surfaces of the plurality of chamber components of the reaction chamber, the film material being etched at a substantially higher rate than the protective coating during exposure to a fluorine-based species, a chlorine-based species, a bromine-based species, or an iodine-based species.
17. 17. The method of claim 16 further comprising: redepositing the protective coating on the surfaces of the plurality of chamber components of the reaction chamber after exposure to the fluorine-based species, the chlorine-based species, the bromine-based species, or the iodine-based species.
18. 17. The method of claim 16, The protective coating is deposited by PECVD or PEALD, and the method further comprises: A method comprising controlling a radio frequency (RF) signal supplied to the reaction chamber such that a majority of a plasma glow discharge forms in one or more regions outside a region between an upper electrode and a lower electrode.
19. 20. The method of claim 18, A method wherein a phase difference between a first phase of the RF signal supplied to the upper electrode and a second phase of the RF signal supplied to the lower electrode is approximately 0 degrees out of phase.
20. The method according to any one of claims 15 to 19, The protective coating is made of silicon oxide (SiO 2 ), aluminum oxide (Al 2 O 3 ), zirconium oxide (ZrO 2 ), hafnium oxide (HfO 2 ), tin oxide (SnO 2 ), or silicon nitride (Si 3 N 4 ) and wherein a material of one or more of the plurality of chamber components comprises aluminum (Al).
Citation Information
Patent Citations
Method of tuning an in-situ process chamber for a plasma ion implantation system
JP2007538413A
Improvement of plasma process uniformity of entire wafer through distribution of power of a plurality of VHF sources
JP2008187179A
Substrate processing apparatus and semiconductor device manufacturing method
JP2012216696A
Method of manufacturing semiconductor integrated circuit device
JP2013191875A
Chamber undercoat preparation method for low temperature ald films
JP2015122486A