Nanocellulose composition, fiber and sheet, and method for producing fiber

A nanocellulose composition with specific fiber length ratios and surface modifications, spun using a coagulating liquid, enhances tensile properties, addressing the weakness of existing nanocellulose materials for industrial use.

JP2024161690APending Publication Date: 2024-11-20HOKKAIDO UNIVERSITY

Patent Information

Application Number
JP2023076584
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-20

AI Technical Summary

Technical Problem

Existing nanocellulose fibers and sheets lack sufficient tensile properties for industrial applications.

Method used

A nanocellulose composition comprising a specific blend of nanocellulose with varying fiber lengths and surface modifications, such as carboxy groups, is spun using a wet spinning method with a coagulating liquid containing cations to enhance tensile properties.

Benefits of technology

The resulting fibers and sheets exhibit improved tensile properties, including higher breaking stress, modulus, and toughness, making them suitable for various industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161690000006
    Figure 2024161690000006
  • Figure 2024161690000007
    Figure 2024161690000007
  • Figure 2024161690000001
    Figure 2024161690000001
Patent Text Reader

Abstract

To provide a nanocellulose composition capable of acquiring sheets or fibers with excellent tensile properties, fibers made by spinning such nanocellulose compositions, a method for producing such fibers, or sheets formed by molding such nanocellulose composition.SOLUTION: There is provided a nanocellulose composition containing nanocellulose with an average fiber length of 10 μm or more, and nanocellulose with an average fiber length of 1 μm or less, wherein a mass ratio of nanocellulose with an average fiber length of 10 μm or more and nanocellulose with an average fiber length of 1 μm or less in the nanocellulose composition is 98:2 to 2:98.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to nanocellulose compositions, fibers and sheets, and methods for making fibers. [Background technology]

[0002] Nanocellulose is a nano-sized material whose main component is cellulose. Nanocellulose has properties such as light weight and high strength, and is therefore expected to have a variety of industrial applications.

[0003] There are various types of nanocellulose, such as cellulose nanofibers that can be obtained by defibrating pulp or the like using mechanical processing, TEMPO oxidation, underwater head-on collision, etc., and bacterially synthesized nanocellulose that can be obtained by fermentation. For example, Patent Document 1 discloses bacterially synthesized nanocellulose that has excellent mechanical strength, etc. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5752332 Summary of the Invention [Problem to be solved by the invention]

[0005] By the way, nanocellulose can be used in combination with other materials, but if it is possible to form fibers or sheets mainly composed of nanocellulose, it may be possible to use it industrially. Therefore, the inventors of the present invention have investigated various nanocelluloses and found that there is room for improvement in terms of strength in fibers and sheets formed from a single type of nanocellulose that has been conventionally known.

[0006] In view of the above circumstances, the present invention aims to provide a nanocellulose composition that can produce a sheet or fiber having excellent tensile properties, a fiber spun from such a nanocellulose composition, and a method for producing such a fiber, or a sheet molded from such a nanocellulose composition. [Means for solving the problem]

[0007] The present disclosure provides nanocellulose compositions described in the following items [1] to [3], fibers described in [4] and [5], a method for producing fibers described in [6], and a sheet described in [7]. [1] A nanocellulose composition containing nanocellulose having an average fiber length of 10 μm or more and nanocellulose having an average fiber length of 1 μm or less, A nanocellulose composition, in which the mass ratio of nanocellulose having an average fiber length of 10 μm or more and nanocellulose having an average fiber length of 1 μm or less in the nanocellulose composition is 98:2 to 2:98. [2] The nanocellulose composition described in [1], wherein the nanocellulose having an average fiber length of 10 μm or more includes bacterial synthetic cellulose. [3] The nanocellulose composition according to [1] or [2], wherein the nanocellulose has an average fiber length of 10 μm or more, and the nanocellulose has an average fiber length of 1 μm or less, and the nanocellulose has a carboxy group on the surface. [4] A fiber obtained by spinning the nanocellulose composition according to any one of [1] to [3]. [5] Cellulose I in wide-angle X-ray diffraction. α (110) face of cellulose I β The fiber according to [4], wherein the degree of orientation in the spinning direction, as determined from the diffraction intensity of the (200) plane of the crystalline structure, is 65% or more. [6] A method for producing the fiber according to [4] or [5], using a wet spinning method in which a coagulation liquid containing a cation having a valence of 2 or more is used. [7] A sheet formed from the nanocellulose composition according to any one of [1] to [3]. Effect of the Invention

[0008] According to the present invention, it is possible to provide a nanocellulose composition capable of producing a sheet or fiber having excellent tensile properties, a fiber obtained by spinning such a nanocellulose composition, and a method for producing such a fiber, or a sheet obtained by molding such a nanocellulose composition. [Brief description of the drawings]

[0009] [Figure 1] 1 shows the distribution curves of fiber length and fiber diameter of various nanocelluloses. [Diagram 2] These are two-dimensional wide-angle X-ray diffraction images of fibers spun from various nanocellulose compositions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiments of the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. When a numerical range is indicated as X to Y, it means X or more and Y or less. For example, "5 to 100 nm" means 5 nm or more and 100 nm or less. Furthermore, the materials, components, or methods exemplified in this specification can be used alone or in combination of two or more types, unless otherwise specified. The average fiber length and the average fiber diameter mean the length-weighted average fiber length and the length-weighted average fiber diameter, respectively, unless otherwise specified.

[0011] [Nanocellulose composition] The nanocellulose composition according to this embodiment contains nanocellulose having an average fiber length of 10 μm or more and nanocellulose having an average fiber length of 1 μm or less. The mass ratio of the content of nanocellulose having an average fiber length of 10 μm or more and nanocellulose having an average fiber length of 1 μm or less in the nanocellulose composition according to this embodiment is 2:98 to 98:2.

[0012] Such nanocellulose compositions can produce fibers and / or sheets with excellent tensile properties. The reason for this is not necessarily clear, but the inventors believe that one of the reasons is that nanocellulose with an average fiber length of 1 μm or less fills the gaps in the three-dimensional structure of nanocellulose with an average fiber length of 10 μm or more, forming a dense structure.

[0013] In the nanocellulose composition of this embodiment, the mass ratio of the content of nanocellulose having an average fiber length of 10 μm or more to the content of nanocellulose having an average fiber length of 1 μm or less is preferably 5:95 to 95:5, more preferably 10:90 to 90:10, even more preferably 20:80 to 80:20, and particularly preferably 40:60 to 60:40, from the viewpoint of further improving the tensile properties of the fibers and / or sheets obtained from the nanocellulose composition.

[0014] The nanocellulose composition according to the present embodiment may be composed of nanocellulose having an average fiber length of 10 μm or more, or nanocellulose having an average fiber length of 1 μm or less, and may contain a dispersion medium and other components. When the nanocellulose composition according to the present embodiment contains a dispersion medium, it may be in a gel form.

[0015] The dispersion medium is not particularly limited and may be appropriately determined depending on the application of the nanocellulose composition according to this embodiment. For example, water such as tap water, distilled water, ion-exchanged water, and ultrapure water (including Milli-Q water (ultrapure water obtained by a Milli-Q water production apparatus, Merck)); alcohol-based dispersion medium such as methanol, ethanol, propanol, butanol, 2-methylpropyl alcohol, and 2-methyl-2-propanol; ketone-based dispersion medium such as acetone and methyl ethyl ketone; ester-based dispersion medium such as ethyl acetate; ether-based dispersion medium such as dioxane, diethyl ether, and tetrahydrofuran; amide-based dispersion medium such as N,N-dimethylacetamide, N,N-dimethylformamide, and N-methylpyrrolidone; sulfur-containing dispersion medium such as dimethyl sulfoxide; aliphatic hydrocarbon-based dispersion medium such as butane, pentane, hexane, heptane, octane, and cyclohexane; alicyclic hydrocarbon-based dispersion medium such as cyclohexane, methylcyclohexane, and decahydronaphthalene; aromatic hydrocarbon-based dispersion medium such as toluene and xylene. Among these, water is preferred from the viewpoint of ease of handling, and ultrapure water is more preferred.

[0016] When the nanocellulose composition of this embodiment contains a dispersion medium, the solids content in the nanocellulose composition of this embodiment is not particularly limited and may be determined appropriately depending on the application of the nanocellulose composition of this embodiment, but may be, for example, 0.001 to 20 mass %, or 0.01 to 10 mass %.

[0017] The other components are not particularly limited and may be appropriately determined depending on the application of the nanocellulose composition according to this embodiment, and examples of the other components include nanocellulose other than the above-mentioned nanocellulose; ultraviolet absorbers such as benzophenone compounds, salicylate compounds, benzoate compounds, triazole compounds, and triazine compounds; antioxidants such as phenols, phosphorus compounds, and sulfur compounds; polymerization inhibitors such as 4-tertiary butyl catechol (TBC), hydroquinone, and 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl (4H-TEMPO); stabilizers such as light stabilizers, weather stabilizers, and heat stabilizers; glass fibers. Reinforcing materials such as fiber and carbon fiber; near infrared absorbing agents; flame retardants such as tris(dibromopropyl)phosphate, triallyl phosphate, and antimony oxide; antistatic agents including anionic, cationic, and nonionic surfactants; colorants such as inorganic pigments, organic pigments, and dyes; organic and inorganic fillers; resin modifiers; organic and inorganic fillers; preservatives such as methylparaben, ethylparaben, propylparaben, sodium benzoate, and phenoxyethanol; pH adjusters such as citric acid, phosphoric acid, lactic acid, malic acid, aqueous ammonia, ammonium bicarbonate, ammonium carbonate, potassium hydroxide, and sodium hydroxide. When the nanocellulose composition according to this embodiment contains other components, the content thereof may be, for example, 10% by mass or less, or 5% by mass or less, based on the total solid content.

[0018] The nanocellulose according to the present embodiment is a fibrous nano-sized material mainly composed of cellulose. Here, the fibrous nano-sized material refers to a material having an average fiber diameter of 1 to 100 nm and an average aspect ratio of 5 or more. In the nanocellulose, microfibrils in which a plurality of cellulose molecular chains are bundled may be formed. The nanocellulose is not particularly limited, and examples thereof include cellulose nanofibers, cellulose nanocrystals (including cellulose nanowhiskers), and bacterial synthetic cellulose. The average aspect ratio is a value represented by the ratio of the average fiber diameter to the average fiber length (average fiber length / average fiber diameter). The average fiber length and the average fiber diameter may be determined using an atomic force microscope.

[0019] Cellulose nanofibers can be obtained by defibrating a cellulose source such as pulp. Pulp is not particularly limited, but examples thereof include coniferous wood pulp, broadleaf wood pulp, esparto pulp, Manila hemp pulp, sisal hemp pulp, cotton pulp, recycled waste paper pulp, etc. In addition, the method of defibrating is not particularly limited, but examples thereof include chemical treatment methods such as TEMPO (2,2,6,6-tetramethylpiperidine-1-oxyl) oxidation method and chemical modification method (phosphorylation method, sulfation method, carboxymethylation method, etc.); and physical treatment methods such as grinder method, underwater counter collision (ACC) method, high-pressure homogenizer method, disk mill method, bead mill method, ball mill method, etc.

[0020] Cellulose nanocrystals can be obtained by hydrolyzing a cellulose source such as pulp. The pulp is not particularly limited, but for example, the pulp exemplified in the above-mentioned cellulose nanofiber can be used. In addition, examples of the hydrolysis method include acid-enzyme hydrolysis.

[0021] Bacterial synthetic cellulose can be obtained by a fermentation method. The fermentation method includes culturing a cellulose-producing bacterium. The cellulose-producing bacterium is not particularly limited, but examples thereof include Gluconacetobacter, Agrobacterium, Rhizobium, Sarcina, Pseudomonas, Achromobacter, Alcaligenes, Aerobacter, and Azotobacter. In order to improve the mixability of bacterial synthetic cellulose with other materials, a polysaccharide may be added to the medium to obtain bacterial synthetic cellulose having a polysaccharide adsorbed on the surface. Examples of polysaccharides include carboxymethylcellulose, hydroxypropylmethylcellulose, and hydroxyethylcellulose. The content (adsorption amount) of carboxymethylcellulose in the bacterial synthetic cellulose having carboxymethylcellulose adsorbed thereon is not particularly limited, but may be, for example, 10 to 20% by mass. The content (adsorption amount) of hydroxypropylmethylcellulose in the bacterial synthetic cellulose having hydroxypropylmethylcellulose adsorbed thereon is not particularly limited, but may be, for example, 20 to 40% by mass.

[0022] Nanocellulose preferably has a carboxy group on the surface. When nanocellulose having a carboxy group on the surface is used, when the nanocellulose is spun by a wet spinning method using a coagulation liquid containing a cation having a valence of 2 or more, the valence of the nanocellulose can be crosslinked by a cation having a valence of 2 or more, and the tensile properties of the obtained fiber can be further improved. Nanocellulose having a carboxy group on the surface can be obtained, for example, by the TEMPO oxidation method, the carboxymethylation method, the fermentation method using a medium containing carboxymethylcellulose, or the like.

[0023] The nanocellulose composition according to this embodiment may be used as is, but it is preferable to process it into a shape such as a sheet (including a film), fiber, molded body, or encapsulated body.

[0024] (Nanocellulose with an average fiber length of 10 μm or more) The nanocellulose having an average fiber length of 10 μm or more according to this embodiment has an average fiber length of preferably 10 μm to 100 μm, more preferably 10 μm to 50 μm, even more preferably 10 μm to 30 μm, and particularly preferably 15 μm to 20 μm. The nanocellulose having an average fiber length of 10 μm or more according to this embodiment may have an average fiber diameter of 1 to 30 nm, or 5 to 15 nm, and an average aspect ratio of 100 or more, 500 or more, or 1000 or more. The average aspect ratio is a value expressed as the ratio of the average fiber diameter to the average fiber length (average fiber length / average fiber diameter). The average fiber length and the average fiber diameter may be determined using an atomic force microscope.

[0025] The nanocellulose having an average fiber length of 10 μm or more according to this embodiment preferably contains bacterial synthetic cellulose. In addition, when the nanocellulose composition according to this embodiment is spun by a wet spinning method using a coagulation liquid containing a cation with a valence of 2 or more, the nanocellulose having an average fiber length of 10 μm or more according to this embodiment preferably contains nanocellulose having a carboxy group on the surface, and more preferably contains bacterial synthetic cellulose with carboxymethyl cellulose adsorbed on the surface, from the viewpoint of further improving the tensile properties of the obtained fiber.

[0026] In terms of improving the mixability with other materials, the nanocellulose having an average fiber length of 10 μm or more according to this embodiment has a light transmittance of 35% or more, more preferably 50% or more, and even more preferably 70% or more at a wavelength of 500 nm when the nanocellulose having an average fiber length of 10 μm or more is dispersed in water at 0.1% by mass. The light transmittance may be measured by an absorptiometer.

[0027] (Nanocellulose with an average fiber length of 1 μm or less) The nanocellulose having an average fiber length of 1 μm or less according to this embodiment has an average fiber length of preferably 0.05 μm to 1 μm, more preferably 0.1 μm to 0.8 μm, and even more preferably 0.3 μm to 0.7 μm. The nanocellulose having an average fiber length of 1 μm or less according to this embodiment may have an average fiber diameter of 0.5 nm to 20 nm, or 1 nm to 10 nm, and an average aspect ratio of 10 or more, or 100 or more. The average aspect ratio is a value expressed as the ratio of the average fiber diameter to the average fiber length (average fiber length / average fiber diameter). The average fiber length and the average fiber diameter may be determined using an atomic force microscope.

[0028] The nanocellulose having an average fiber length of 1 μm or less according to this embodiment preferably contains cellulose nanofibers. In addition, when the nanocellulose composition is spun by a wet spinning method using a coagulation liquid containing a cation with a valence of 2 or more, the nanocellulose having an average fiber length of 1 μm or less according to this embodiment preferably contains nanocellulose having a carboxy group on the surface from the viewpoint of further improving the tensile properties of the obtained fiber, more preferably contains cellulose nanofibers obtained by the TEMPO oxidation method or the carboxymethylation method, and even more preferably contains cellulose nanofibers obtained by the TEMPO oxidation method (i.e., TEMPO oxidized cellulose nanofibers).

[0029] [Fibers spun from nanocellulose composition] The fiber according to the present embodiment is not particularly limited, but may be, for example, a fiber obtained by spinning the nanocellulose composition according to one aspect of the present embodiment. The fiber diameter of the fiber according to the present embodiment is not particularly limited, but may be, for example, 0.1 mm to 10 mm, or 1 mm to 5 mm.

[0030] The degree of orientation of the fibers according to the present embodiment is preferably 65% ​​or more, and more preferably 70% or more, from the viewpoint of further improving the tensile properties of the fibers. The degree of orientation of the fibers is measured by the cellulose I diffraction method using a wide-angle X-ray diffraction method.α (110) face of cellulose I β It can be determined from the diffraction intensity of the (200) plane of the cellulose I type crystal. α (110) face of cellulose I β The diffraction pattern originating from the (200) plane of the cellulose I crystal is observed at the same position. α The crystal type is triclinic, and cellulose I β The cellulose I crystal is monoclinic. α (110) face of cellulose I β The diffraction of the (200) plane of the crystal can be determined in accordance with Moon, Robert J., et al. "Cellulose nanomaterials review: structure, properties and nanocomposites" Chemical Society Reviews 40.7(2011): 3941-3994.

[0031] More specifically, the method for determining the degree of orientation of the fibers according to this embodiment is as follows. First, the degree of orientation of cellulose I is determined from a two-dimensional wide-angle X-ray diffraction image obtained by irradiating X-rays perpendicular to the spinning direction. α (110) face of cellulose I β The distribution curve of the diffraction intensity of the (200) plane of the type crystal with respect to the azimuth angle is obtained. Next, the distribution curve of cellulose I α (110) face of cellulose I β After performing Gaussian distribution fitting on the peak derived from the diffraction of the (200) plane of the crystal, the half-width (Wh) is obtained, and the degree of orientation is calculated from the following formula. Orientation degree (%)={(180-Wh) / 180}×100

[0032] The fiber according to the present embodiment is not particularly limited, and is preferably used, for example, as twisted yarn, fabric, knitted fabric, strand, rope, paper, nonwoven fabric, felt, fiber-reinforced resin material, adhesive, chopped strand, resin composition filler, flowability adjusting material, and the like. Fabric and knitted fabric may be obtained by weaving twisted yarn. Strands may be obtained by twisting twisted yarn, and ropes may be obtained by twisting strands, etc. In addition, fiber-reinforced resin material and adhesive may be obtained by compounding the fiber according to the present embodiment with a resin. Chopped strands and resin composition filler may be obtained by cutting twisted yarn, etc.

[0033] (Method for producing fibers by spinning nanocellulose composition) The method for spinning the nanocellulose composition according to one aspect of this embodiment is not particularly limited, and examples thereof include wet spinning, dry spinning, dry jet wet spinning, melt spinning, etc., and wet spinning is preferred.

[0034] The wet spinning method is not particularly limited, but may be, for example, a method in which a spinning solution containing a nanocellulose composition is prepared, the spinning solution is extruded through a nozzle into a coagulation solution in a coagulation bath, and solidified.

[0035] The spinning solution is not particularly limited, but for example, the nanocellulose composition of this embodiment in which the dispersion medium is water can be used, and if necessary, water can be added so that the total solid content in the nanocellulose composition of this embodiment is 0.1 to 5 mass%.

[0036] The spinning solution may be degassed. The degassing method is not particularly limited, but for example, the solution may be degassed for 1 to 10 minutes under reduced pressure of 2500 Pa to 4000 Pa while being heated to 70°C to 90°C or after being heated to 70°C to 90°C. During degassing, the spinning solution may be stirred as necessary. After degassing, the solution may be allowed to cool to room temperature (for example, 25°C).

[0037] When the spinning solution is extruded through a nozzle into the coagulation liquid in the coagulation bath, in order to further improve the tensile properties of the fiber, it is preferable that the nanocellulose composition is extruded vertically downward from the nozzle into the coagulation liquid and that the distance from the extrusion part of the nozzle to the bottom of the coagulation bath is 0.5 m or more, or 1 m or more.

[0038] The diameter of the nozzle and the injection speed from the nozzle are not particularly limited, but for example, when the inner diameter of the nozzle is 1 mm to 3 mm, the injection speed from the nozzle is preferably 0.5 mL / min to 2.5 mL / min.

[0039] The coagulation liquid preferably contains cations with a valence of 2 or more, and more preferably is a saturated solution of cations with a valence of 2 or more. When the coagulation liquid contains cations with a valence of 2 or more, if the nanocellulose composition contains nanocellulose having a carboxyl group on the surface, the tensile properties of the fiber obtained by crosslinking these can be further improved. The cations with a valence of 2 or more are not particularly limited, but include, for example, metal ions and polycations. Examples of metal ions include alkaline earth metal ions such as magnesium ions, calcium ions, and barium ions; divalent cations derived from transition metals such as iron (II) ions, copper (II) ions, and tetraammine copper (II) ions; trivalent cations derived from transition metals such as aluminum ions and iron (III) ions; and cations with a valence of 4 or more derived from transition metals such as titanium (IV) ions. Examples of polycations include linear, branched, or cyclic aliphatic or aromatic hydrocarbon polyamine salts such as ethylenediamine salts, hexamethylenediamine salts, ethylhexyldiamine salts, diethylenetriamine salts, triethylenetetramine salts, tetraethylenepentamine salts, pentamethyldiethylenetriamine salts, cyclohexanediamine salts, isophoronediamine salts, norbornenediamine salts, bisaminomethylcyclohexane salts, xylylenediamine salts, phenylenediamine salts, and biphenyldiamine salts; (co)polymerized polyamine salts obtained by (co)polymerizing nitrogen-containing monomers such as (meth)acrylamide and diallyldimethylammonium; salts of peptides consisting of amino acids having multiple amino groups in one molecule such as asparagine, glutamine, arginine, histidine, and lysine; and salts of aminopolysaccharides such as chitosan. The solvent of the coagulation liquid is not particularly limited and may be one that can be desolvated, and examples thereof include lower alcohols having 1 to 5 carbon atoms such as methanol, ethanol, and 2-propanol; and acetone. As the coagulation liquid, when the nanocellulose composition contains nanocellulose having carboxy groups on the surface, a saturated ethanol solution of calcium chloride, a saturated ethanol solution of aluminum sulfate, etc. are preferred from the viewpoint of further improving the tensile properties of the obtained fiber.

[0040] The solidified fibers may be washed and dried. In washing, for example, Milli-Q water (ultrapure water obtained by a Milli-Q water production apparatus, Merck) may be used, and the fibers may be stirred for 30 minutes to 2 hours. In drying, the fibers may be left to stand on a Teflon (registered trademark) sheet at 60 to 80°C for 6 to 18 hours.

[0041] [Sheet formed by molding nanocellulose composition] The sheet formed from the nanocellulose composition according to one aspect of this embodiment is not particularly limited, and may be, for example, a nonwoven fabric. The thickness of the sheet according to this embodiment may be, for example, 5 μm to 250 μm, or 20 μm to 100 μm. The thickness of the sheet according to this embodiment may be, for example, 250 μm to 5 mm, or 500 μm to 2 mm.

[0042] The sheet according to the present embodiment can be used, for example, as a papermaking material, a recording medium material, a clothing material, a heat insulating material, a sound absorbing material, a filtering material, an adsorbent material, a protective material, a bonding material, an adhesive material, a strength imparting material, a shock absorbing material, an anti-friction material, an anti-wear material, an anti-slip material, and the like, without any particular limitation.

[0043] (Method for producing a sheet formed by molding a nanocellulose composition) The method for forming the nanocellulose composition according to this embodiment into a sheet is not particularly limited, and examples thereof include wet methods (including papermaking methods) and dry methods.

[0044] The wet method is not particularly limited, but may be, for example, a nanocellulose composition according to the present embodiment in which the dispersion medium is water, filtered to reduce the moisture from the nanocellulose composition, followed by dehydration pressing at 8 to 12 MPa and room temperature (e.g., 25°C), and heating pressing at 8 to 12 MPa and 100 to 120°C. For example, when forming a sheet having a thickness of 5 μm to 250 μm, Milli-Q water (ultrapure water obtained by a Milli-Q water production device, Merck) may be added to the nanocellulose composition so that the total solid content in the nanocellulose composition is 0.05 to 0.5 mass%, and the mixture may be stirred for 15 minutes to 1 hour, followed by vacuum filtration, dehydration pressing for 3 to 10 minutes 2 to 3 times, and then heating pressing for 5 to 15 minutes 1 to 2 times. Furthermore, when forming a sheet having a thickness of 250 μm to 5 mm, water may be added to the nanocellulose composition as necessary so that the total solid content in the nanocellulose composition is 0.5 to 5 mass%, after which pressure filtration is performed, and dehydration pressing is performed 3 to 5 times for 5 to 15 minutes, followed by 5 to 7 hot pressings for 5 to 15 minutes. EXAMPLES

[0045] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass". Furthermore, unless otherwise specified, the thickness and bulk density of the sheet in the table, as well as the tensile properties of the sheet and fiber, are given in the form of "average value ± standard deviation".

[0046] In the examples, evaluation of nanocellulose, etc., and production and evaluation of sheets and fibers were performed by the methods shown below.

[0047] <Analysis of nanocellulose fiber length and diameter> The fiber length and fiber diameter distribution curves, as well as the average fiber length, average fiber diameter, and average aspect ratio of nanocellulose were determined using an atomic force microscope (NanoNaviII L-trace, Hitachi High-Tech Science Corporation). More specifically, 50 μL of aqueous dispersion of nanocellulose (1 mass ppm) was dropped onto a mica substrate, and after natural drying, the sample was observed under a microscope in dynamic force mode with a measurement range of 90 × 90 μm. The obtained observation image was analyzed using the analysis software "FiberApp" to determine the fiber length and fiber diameter distribution curves, as well as the average fiber length and average fiber diameter. The average aspect ratio was calculated by calculating (average fiber length / average fiber diameter). The fiber length distribution curve and average fiber length were determined by randomly extracting 200 nanocellulose fibers, and the fiber diameter distribution curve and average fiber diameter were determined by randomly extracting 600 nanocellulose fibers from the observation image.

[0048] <Quantitative determination of the amount of polysaccharides adsorbed on bacterially synthesized cellulose> After freeze-drying the bacterial synthetic cellulose with adsorbed carboxymethyl cellulose or hydroxypropyl cellulose, 30 mg was weighed into a vial and dried at 105°C for 5 hours to obtain an absolute dry state. After cooling to room temperature in a desiccator, 3 mL of tetrabutylphosphonium hydride (60% by mass aqueous solution) was added and stirred overnight at 30°C to completely dissolve the bacterial synthetic cellulose. The solution was added to 100 mL of Milli-Q water (ultrapure water obtained by a Milli-Q water production device, Merck) and stirred for 30 minutes to re-precipitate the cellulose. The residue was then collected by vacuum filtration and dried at 105°C for 2 hours, after which the mass W of the residue was calculated. cel The amount of carboxymethyl cellulose or hydroxypropyl cellulose adsorbed onto the bacterially synthesized cellulose was calculated using the following formula: Adsorption amount (%) = {(30-W cel ) / 30}×100

[0049] <Transmittance measurement of nanocellulose> An aqueous dispersion containing 0.1% by mass of nanocellulose was prepared, and transmittance was measured at a constant wavelength of 500 nm using an absorption spectrophotometer (U-2001, Hitachi, Ltd.). A polystyrene disposable cuvette (semi-microcell, optical path length 10 mm, optical path width 4 mm) was used as the cell.

[0050] <Seat manufacturing> 270 g of MilliQ water (ultrapure water obtained by Milli-Q water production apparatus, Merck) was added to 30 g of the nanocellulose composition described below and stirred for 30 minutes, and then vacuum filtration was performed using a vacuum filtration apparatus (VT-500, ADVANTEC). After that, a sheet was produced by applying a dehydration press (room temperature, 10 MPa, 5 minutes x 2 times) and a heat press (105 ° C, 10 MPa, 10 minutes). In the dehydration press, three sheets of filter paper (No. 101, diameter 125 mm, ADVANTEC), one Teflon sheet (Nitoflon 900UL, Nitto Denko), a nanocellulose composition, one membrane filter (A045A090C, ADVANTEC), and nine sheets of filter paper were stacked and pressed from the bottom. In addition, in the heat press, five sheets of filter paper (No. 101, diameter 125 mm, ADVANTEC Co., Ltd.), one sheet of Kimtowel (Nippon Paper Crecia), one sheet of mesh sheet (PF020, ADVANTEC Co., Ltd.), the nanocellulose composition, one sheet of mesh sheet (PF020, ADVANTEC Co., Ltd.), one sheet of Kimtowel (Nippon Paper Crecia), and five sheets of filter paper (No. 101, diameter 125 mm, ADVANTEC Co., Ltd.) were stacked and pressed from the bottom.

[0051] <Sheet tensile test> The tensile properties of the sheet were evaluated by a tensile test using a universal testing machine (34SC-1 (500N), INSTRON). More specifically, the sheet was punched into strips (40 x 6 mm) using a test piece punching machine (SDL-100, DUMBBELL), dried at 105°C for 2 days, fixed so that the distance between the grippers was 1 cm, and a tensile test (cross-head speed: 10 mm / min) was performed using a universal testing machine to determine the tensile properties of breaking stress, breaking elongation, Young's modulus, and toughness. Each tensile test was performed five times, and the average value was calculated.

[0052] <Sheet thickness and bulk density measurement> The thickness of the sheet was measured with a micrometer. The bulk density was calculated as the bulk volume (cm3) calculated from the area and thickness of the sheet. 3 The thickness and bulk density were calculated by dividing the mass (g) of the sheet by the mass (g). The thickness and bulk density were calculated by averaging five sheets.

[0053] <Production of fibers by wet spinning method> The nanocellulose composition described below was added to a separable round-bottom flask, and heated and stirred at 200 rpm using a small stirrer (SPZ-2000, Tokyo Rika Kikai) in a bead bath (BBH-1, AS ONE) at 80 ° C. After that, it was degassed under reduced pressure (3333 Pa) for 5 minutes, and then the nanocellulose composition was added to a syringe (20 mL, Terumo Syringe, TERUMO) and allowed to cool to room temperature. Next, the nanocellulose composition was injected from the syringe into an injection needle (inner diameter: 2.40 mm) using a syringe pump (YSP-101, YMC) at an injection rate of 1 mL / min, and injected into an acrylic cylinder (diameter: 1 m, inner diameter: 2 cm, Kokugo) containing CaCl2 / EtOH saturated solution installed vertically through a lablan silicone tube (30 cm, 2 × 4, AS ONE). The fibers were then washed with Milli-Q water (ultrapure water obtained using a Milli-Q water production device, Merck) for 1 hour, placed on a Teflon sheet (TOMBO 9000, Nichias) and dried in an oven at 70°C for 12 hours to produce fibers.

[0054] <Wide-angle X-ray diffraction method> The orientation of the fibers was investigated using a wide-angle X-ray scattering device (BL-6A, Photon Factory). More specifically, the fibers were cut into 1 cm pieces, bundled into 10 pieces, and fixed with instant adhesive. X-rays were irradiated perpendicular to the spinning direction of the fiber bundle to obtain a two-dimensional wide-angle X-ray diffraction image. The X-ray wavelength was 1.5 Å, the exposure time was 60 seconds, and the detector was a PILATUS3 1M (Dectris Ltd., Switzerland, 981 × 1043 pixels, 172 × 172 μm pixel size). The sample-detector distance (SDD = 250.58265 mm) was calibrated using the diffraction pattern of silver behenate. From the obtained two-dimensional wide-angle X-ray diffraction images, cellulose I was observed at azimuth angles of 90° to 270°. α (110) face of cellulose I β The distribution curve of the diffraction intensity of the (200) plane of the cellulose I crystal was obtained. α (110) face of cellulose I β The peak derived from the diffraction of the (200) plane of the type crystal was fitted with a Gaussian distribution in the azimuth angle range of 90° to 270°, and the half-width (Wh) was obtained, and the degree of orientation was calculated from the following formula. Orientation degree (%)={(180-Wh) / 180}×100

[0055] <Tensile test of fibers> The tensile properties of the fibers were evaluated by tensile tests using a universal testing machine (AG-100kNXplus, Shimadzu Corporation). More specifically, the fibers were cut to 3 cm, fixed so that the distance between the grips was 1 cm, and tensile tests (test speed 5 mm / min) were performed to determine the tensile properties, namely, Young's modulus, breaking stress, and breaking strain. Each tensile test was performed five times, and the average values ​​were calculated.

[0056] <Nanocellulose> The nanocelluloses used were TEMPO-oxidized cellulose nanofibers (TOCN, Nippon Paper Industries Co., Ltd.), bacterial synthetic cellulose with carboxymethyl cellulose adsorbed on the surface (CM-NFBC, Kusano Sakuko Co., Ltd.), and bacterial synthetic cellulose with hydroxypropyl cellulose adsorbed on the surface (HP-NFBC, Kusano Sakuko Co., Ltd.). The distribution curves of the fiber length and fiber diameter of these nanocelluloses, measured according to the above-mentioned nanocellulose fiber length and fiber diameter analysis method, are shown in Figure 1, and the average fiber length, average fiber diameter, and average aspect ratio are shown in Table 1.

[0057] [Table 1]

[0058] Table 2 shows the amount of carboxymethyl cellulose adsorbed in CM-NFBC and the amount of hydroxypropyl cellulose adsorbed in HP-NFBC, which were quantified according to the above-mentioned method for quantifying the amount of polysaccharides adsorbed in bacterial synthetic cellulose, as well as the light transmittance at a wavelength of 500 nm of an aqueous dispersion containing 0.1 mass% CM-NFBC or HP-NFBC, which was measured according to the above-mentioned method for measuring the transmittance of nanocellulose.

[0059] [Table 2]

[0060] <Nanocellulose composition> The nanocellulose compositions of Examples 1 to 5 and Comparative Examples 1 and 2 were prepared by mixing 1.0 mass% aqueous dispersions of each nanocellulose shown in Table 1 in the ratios shown in Table 3.

[0061] [Table 3]

[0062] <Sheet> According to the above-mentioned sheet manufacturing method, sheets of Examples 1a to 5a and Comparative Examples 1a to 2a were manufactured from the nanocellulose compositions of Examples 1 to 5 and Comparative Examples 1 to 2, respectively. The tensile properties of the sheets measured according to the above-mentioned sheet tensile test method, and the thickness and bulk density of the sheets measured according to the above-mentioned sheet thickness and bulk density measurement method are shown in Table 4. As is clear from Table 4, the sheets of Examples 1a to 5a had higher breaking stress and Young's modulus and were excellent in tensile properties compared to the sheets of Comparative Examples 1a to 2a. Among them, the sheets of Examples 2a to 4a had higher breaking stress and more excellent tensile properties. Moreover, the sheet of Example 3a had even higher breaking stress, Young's modulus, and toughness, and was even more excellent in tensile properties.

[0063] [Table 4]

[0064] <Textile> According to the method for producing fibers by the wet spinning method described above, fibers of Example 3b and Comparative Example 2b were produced from the nanocellulose compositions of Example 3 and Comparative Example 2, respectively. The two-dimensional wide-angle X-ray diffraction images of the fibers obtained according to the wide-angle X-ray diffraction method of the fibers are shown in FIG. 2. As shown in FIG. 2, in Example 3b and Comparative Example 2b, cellulose I α (110) face of cellulose I β Diffraction of the (200) plane of the type crystal was confirmed. In addition, the degree of orientation obtained according to the wide-angle X-ray diffraction measurement method of the above fiber is shown in Table 5. As is clear from Table 5, the degree of orientation of Example 3b was higher than that of Comparative Example 2b.

[0065] [Table 5]

[0066] The tensile properties of the fibers obtained according to the above fiber tensile test method are shown in Table 5. As is clear from Table 5, the fiber of Example 3b had larger Young's modulus, breaking stress and breaking strain than the fiber of Comparative Example 2b, and was superior in tensile properties.

Claims

1. A nanocellulose composition containing nanocellulose having an average fiber length of 10 μm or more and nanocellulose having an average fiber length of 1 μm or less, A nanocellulose composition, wherein the mass ratio of nanocellulose having an average fiber length of 10 μm or more and nanocellulose having an average fiber length of 1 μm or less in the nanocellulose composition is 98:2 to 2:

98.

2. 2. The nanocellulose composition of claim 1, wherein the nanocellulose having an average fiber length of 10 μm or more comprises bacterially synthesized cellulose.

3. The nanocellulose composition of claim 1, wherein the nanocellulose having an average fiber length of 10 μm or more and the nanocellulose having an average fiber length of 1 μm or less have carboxy groups on the surface.

4. A fiber spun from the nanocellulose composition according to any one of claims 1 to 3.

5. Cellulose I in wide-angle X-ray diffraction α The (110) face of cellulose I β 5. The fiber according to claim 4, wherein the degree of orientation in the spinning direction, as determined from the diffraction intensity of the (200) plane of the crystal, is 65% or more.

6. The method for producing the fiber according to claim 4, which is a wet spinning method using a coagulation liquid containing a cation having a valence of divalent or higher.

7. A sheet formed from the nanocellulose composition according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Power line conveying and controlling system

    JP1982052332A

Cited By

  • Method for producing an aqueous dispersion of holocellulose nanofibers, method for producing freeze-dried holocellulose nanofibers, and method for producing a redispersed aqueous solution of holocellulose nanofibers.