Fluorine-containing amorphous carbon film, and manufacturing method for the same

A single-layer fluorine-containing amorphous carbon film addresses the complexity and cost issues of multiple film layers in display devices by integrating hard coat, antireflection, and antifouling properties, achieved through a plasma-enhanced chemical vapor deposition method with controlled gas mixtures.

JP2024161697APending Publication Date: 2024-11-20KEIO UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023076611
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-20

AI Technical Summary

Technical Problem

Conventional display devices require multiple thin films with different functions, such as antireflection and antifouling layers, leading to a complex and expensive production process.

Method used

A single-layer fluorine-containing amorphous carbon film composed of carbon, fluorine, and oxygen, with specific atomic content ranges, is produced using a plasma-enhanced chemical vapor deposition method, utilizing a mixture of fluorocarbon and inert gases to achieve hard coat, antireflection, and antifouling properties in a single layer.

Benefits of technology

The film provides hard coat, antireflection, and antifouling properties with high light transmittance, low refractive index, and excellent water repellency, simplifying the production process and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161697000001_ABST
    Figure 2024161697000001_ABST
Patent Text Reader

Abstract

To provide a fluorine-containing amorphous carbon film and a manufacturing method for the same having properties of hard coat, antireflection and anti-fouling at the same time.SOLUTION: A fluorine-containing amorphous carbon film is a monolayer film comprising carbon, fluorine, and oxygen, and an average fluorine-containing rate in a film thickness direction is between 30 atom % to 40 atom %, an average oxygen containing rate in the film thickness direction is between 5 atom % and 20 atom %, and the rest is carbon atoms. The fluorine-containing amorphous carbon film installs a substrate in a chamber, introduces into the chamber raw material gas whose chemical formula is expressed by carbon and fluorine only and inactive gas diluting the raw material gas, forms the fluorine-containing amorphous carbon film on the substrate under plasma generation, and sets a mixture ratio of the inactive gas with respect to the raw material gas larger than 1 / 4 and smaller than 11 / 1 by flow ratio into the chamber.SELECTED DRAWING: Figure 11
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fluorine-containing amorphous carbon film and a method for producing the same, and more particularly to a fluorine-containing amorphous carbon film that realizes a hard coating having a low refractive index and excellent water repellency, and a method for producing the same. [Background technology]

[0002] In mobile display devices such as smartphones and tablet terminals, many functional layers are laminated on the surface of a glass substrate that serves as the base material of the display. For example, a hard coat layer for preventing scratches and damage, an anti-reflection layer for reducing light reflection, and an anti-soiling layer for preventing dirt and fingerprints from adhering are provided. A coating liquid using a fluorine-containing alkoxysilane has been proposed to form an anti-reflection film with a low refractive index (see, for example, Patent Document 1). In addition, an anti-reflection film having scratch resistance and anti-soiling properties, which is formed by laminating a hard coating layer and a low refractive index layer containing hollow inorganic nanoparticles, has been proposed (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-224302 A [Patent Document 2] Patent Publication No. 2021-76849 Summary of the Invention [Problem to be solved by the invention]

[0004] Conventional display devices are coated with multiple thin films with different functions, such as anti-reflection layers and anti-fouling layers, making the production process complicated and expensive. When using the low refractive index anti-reflection film proposed in Patent Document 1, a separate hard coating layer and anti-fouling layer are required. The anti-reflection film proposed in Patent Document 2 is a composite film of a hard coating layer and a low refractive index layer, and the production method is complicated and expensive.

[0005] In view of the above problems, an object of the present invention is to provide a fluorine-containing amorphous carbon film having hard coat, anti-reflection and anti-soiling properties in combination, and a method for producing the same. [Means for solving the problem]

[0006] In one aspect of the present invention, the fluorine-containing amorphous carbon film is a single layer film composed of carbon, fluorine, and oxygen, in which the average fluorine content in the thickness direction is 30 atomic % or more and 40 atomic % or less, the average oxygen content in the thickness direction is 5 atomic % or more and 20 atomic % or less, and the remainder is carbon atoms.

[0007] In another aspect of the present invention, a method for producing a fluorine-containing amorphous carbon film includes the steps of: A substrate is placed in the chamber; A source gas whose chemical formula is represented only by carbon and fluorine and an inert gas for diluting the source gas are introduced into the chamber, and a fluorine-containing amorphous carbon film is formed on the surface of the substrate under plasma generation; The mixture ratio of the inert gas to the source gas is set to a flow rate ratio into the chamber that is greater than 1 / 4 and smaller than 11 / 1. Effect of the Invention

[0008] A fluorine-containing amorphous carbon film having hard coat, anti-reflection and anti-soiling properties and a method for producing the same are realized. [Brief description of the drawings]

[0009] [Figure 1]1 is a schematic diagram of an embodiment of a fluorine-containing amorphous carbon film formed on a substrate. [Diagram 2] FIG. 1 is a schematic diagram of a film forming apparatus used to form a fluorine-containing amorphous carbon film. [Diagram 3] FIG. 4 is a diagram showing the relationship between the gas flow rate ratio and the light transmittance in Example 1. [Figure 4] FIG. 4 is a diagram showing the relationship between the gas flow rate ratio and the extinction coefficient in Example 1. [Diagram 5] FIG. 4 is a diagram showing the relationship between the gas flow rate ratio and the refractive index in the first embodiment. [Figure 6] FIG. 4 is a diagram showing the relationship between the gas flow rate ratio and the water droplet contact angle in Example 1. [Figure 7] FIG. 11 is a diagram showing the relationship between film formation pressure and light transmittance in Example 2. [Figure 8] FIG. 13 is a diagram showing the elemental contents of films formed at different pressures in Example 2. [Figure 9] FIG. 11 is a diagram showing the relationship between the film formation pressure and the refractive index in Example 2. [Figure 10] FIG. 11 is a diagram showing the relationship between the film formation pressure and the water droplet contact angle in Example 2. [Figure 11] FIG. 11 is a diagram showing element contents when the gas flow rate ratio is changed in Example 3. [Figure 12] FIG. 11 is a diagram showing the relationship between the gas flow rate ratio and the refractive index in Example 3. [Figure 13] FIG. 11 is a diagram showing the relationship between the gas flow rate ratio and the light transmittance in Example 3. [Figure 14] FIG. 11 is a graph showing the relationship between the gas flow rate ratio and the water droplet contact angle in Example 3. [Figure 15] FIG. 11 is a diagram showing the relationship between the gas flow rate ratio and the film formation rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The fluorine-containing amorphous carbon film and its manufacturing method of the present invention will be described in detail below with reference to the drawings. The following embodiments are examples for embodying the technical ideas of the invention, and the present invention is not limited to the described configurations and numerical values. In the drawings, components having the same functions may be given the same reference numerals, and duplicate descriptions may be omitted. Partial substitution or combination between different embodiments and configuration examples is possible. The size, positional relationship, etc. of each member shown in each drawing may be exaggerated to make the invention easier to understand.

[0011] <Composition of fluorine-containing amorphous carbon film> FIG. 1 is a schematic diagram of a fluorine-containing amorphous carbon film 10 according to an embodiment formed on the surface of a substrate 11 as a base material. The fluorine-containing amorphous carbon film 10 is a single-layer thin film formed in a single film formation process. The thickness of the fluorine-containing amorphous carbon film 10 can be appropriately designed depending on the member to which the fluorine-containing amorphous carbon film 10 is applied, and is, for example, 25 nm to 500 nm, preferably 50 nm to 250 nm. The fluorine-containing amorphous carbon film 10 has a different fluorine content between the surface region and a region 12 deeper on the substrate 11 side. The vicinity of the surface of the fluorine-containing amorphous carbon film 10, specifically a region shallower than 10 nm from the surface, is a high-fluorine-containing region 13 having a higher fluorine content than the region 12 deeper than 10 nm.

[0012] The fluorine-containing amorphous carbon film 10 is a single layer film made of carbon, fluorine, and oxygen. In the embodiments and claims, when the fluorine-containing amorphous carbon film 10 is expressed as a film "made of carbon, fluorine, and oxygen" or a film "composed of carbon, fluorine, and oxygen," this is intended to mean that trace amounts of impurities that are inevitably or unintentionally mixed in are not considered as constituent elements.

[0013] The average fluorine content in the thickness direction of the fluorine-containing amorphous carbon film 10 is 30 atomic % or more and 40 atomic % or less, the average oxygen content in the thickness direction is 5 atomic % or more and 20 atomic % or less, and the remainder is carbon atoms. In the high-concentration fluorine-containing region 13 on the surface, the fluorine content is 50 atomic % or more and 75 atomic % or less, the oxygen content is 5 atomic % or more and 20 atomic % or less, and the remainder is carbon atoms. In the composition in the region 12 at a depth of 10 nm or more from the surface, the fluorine content is 30 atomic % or more and 40 atomic % or less, the oxygen content is 5 atomic % or more and 20 atomic % or less, and the remainder is carbon atoms. The average content of each element in the thickness direction is dominated by the composition in the region 12 at a depth of 10 nm or more from the surface.

[0014] The fluorine-containing amorphous carbon film 10 is a highly hard film with a low refractive index and excellent water repellency, and has the functions of hard coat, anti-reflection, and anti-fouling in a single layer. The fluorine-containing amorphous carbon film 10 is applied to the surface of a glass substrate such as a display or a transparent panel. The hard coat property is a property that suppresses the occurrence of scratches and cracks in the glass substrate when an impact is applied from the outside, and includes abrasion resistance and scratch resistance. In order to be called a hard coat, not only is it possible to prevent scratches and cracks, but the film itself is required to have high hardness to protect the substrate. The substrate is formed of a glass material such as quartz glass, soda-lime glass, sapphire glass, or optical glass. In order to protect the substrate, the fluorine-containing amorphous carbon film 10 preferably has a hardness of 0.65 GPa or more as measured by the nanoindentation method. When applied to a display terminal or a transparent panel, high light transmittance is also required. As described later, the light transmittance of the fluorine-containing amorphous carbon film 10 of the embodiment is 90%, preferably 95% or more, and more preferably 98% or more.

[0015] Anti-reflection properties refer to the function of reducing light reflection by utilizing optical interference. When the fluorine-containing amorphous carbon film 10 is applied to a display, it reduces light reflection on the display surface to improve visibility. To achieve this, it is required that the film has a low refractive index relative to the underlying substrate. Even in the highest case, the fluorine-containing amorphous carbon film 10 has a refractive index of 1.40±0.02, which is lower than the refractive index of quartz glass (1.50). When the film is formed under favorable conditions, the refractive index can be reduced to 1.32, and the film has a high anti-reflection function.

[0016] Antifouling properties refer to the property of being resistant to dirt. When applied to a display, the outermost surface of the display is required to have a small surface free energy or a large contact angle with water (high water repellency) in order to prevent dirt and fingerprints from adhering thereto. The fluorine-containing amorphous carbon film 10 has a large water droplet contact angle of 95° or more and is highly water repellent. The basis for this will be described later.

[0017] <Method for producing fluorine-containing amorphous carbon film> 2 is a schematic diagram of a film forming apparatus 100 used to produce the fluorine-containing amorphous carbon film 10. The fluorine-containing amorphous carbon film 10 is formed using a source gas whose chemical formula is represented only by carbon (C) and fluorine (F) and an inert gas. That is, a mixed gas of a fluorocarbon gas that does not contain water or hydrogen and an inert gas is used.

[0018] The film forming apparatus 100 is a CVD (Chemical Vapor Deposition) film forming apparatus. CVD has a high film forming speed, a large processing area, and can form a high density film compared to vacuum deposition. In this example, the film forming apparatus 100 is a capacitively coupled high frequency plasma CVD apparatus, and has a pair of parallel plate type electrodes 101 and 102 in a chamber 104. The chamber 104 is configured so that a substrate 11 can be placed between the electrodes 101 and 102, and for example, the substrate 11 can be placed on the lower electrode 101.

[0019] During film formation, the chamber 104 is maintained at a medium or high vacuum of 24 Pa or less. One electrode 101 is connected to a high-frequency power supply 103, and the other electrode 102 is grounded. High-frequency power is applied between the electrodes 101 and 102 to generate plasma. Frequencies used for excitation of low-temperature plasma include the HF band (3 to 30 MHz), the VHF band (30 to 300 MHz), and the UHF band (300 to 3000 MHz), but in this embodiment, a power frequency of 13.56 MHz, which is common in plasma excitation processes, is used. A raw material gas and an inert gas for diluting the raw material gas are introduced into the chamber 104 from a gas inlet Pin. The raw material gas molecules are decomposed by the plasma generated in the chamber 104, and chemical species generated by the decomposition are deposited on the substrate 11. Unnecessary gas is exhausted from an exhaust port Pout.

[0020] As the raw material gas, at least one gas selected from tetrafluoromethane (CF4), hexafluoroethane (C2F6), octafluoropropane (C3F8), and octafluorocyclobutane (C4F8) can be used. The inert gas for dilution is argon (Ar), nitrogen (N), krypton (Kr), xenon (Xe), etc. By using a fluorocarbon gas that does not contain hydrogen as the raw material gas, it is possible to eliminate C-H bonds that tend to increase the refractive index due to polarization.

[0021] The method for producing a fluorine-containing amorphous carbon film includes the steps of: a) A substrate 11 is placed in a chamber 104 of a film forming apparatus 100; b) A source gas whose chemical formula is represented only by carbon and fluorine and an inert gas for diluting the source gas are introduced into the chamber 104, and a fluorine-containing amorphous carbon film is formed on the surface of the substrate 11 under plasma generation; c) setting the mixture ratio of the inert gas to the source gas in terms of the flow rate into the chamber 104 to be greater than 1 / 4 and smaller than 11 / 1; More preferably, the flow rate ratio of the inert gas to the source gas into the chamber 104 is set to 1 / 2 or more and 7 / 2 or less. The reason for the preferable range of the mixture ratio of the inert gas to the source gas will be described later.

[0022] <Characteristics evaluation> In the following, a number of types of samples are produced by changing the film formation conditions of the fluorine-containing amorphous carbon film 10, and the characteristics are evaluated.

[0023] <Example 1> A SiO2 substrate is used as the substrate 11. The SiO2 substrate is placed on the electrode 101, and a high-frequency power of 13.56 MHz and 200 W is applied to the film forming apparatus 100 to excite low-temperature plasma. The pressure in the chamber 104 before plasma ignition is set to 24 Pa, and Ar gas and C4F8 gas are introduced into the chamber 104. The ratio of the flow rate of the Ar gas to the C4F8 gas (Ar / C4F8) is changed to 1 / 4, 1 / 2, and 1 / 1. High-frequency power is applied to generate plasma, and three types of samples are prepared by forming films with final film thicknesses of 50 nm, 100 nm, and 150 nm at each flow rate ratio. The film thickness, element content, light transmittance, extinction coefficient, refractive index, water droplet contact angle, and hardness are measured using the prepared samples. The film thickness is obtained by fitting the measurement data after creating a structural model of the thin film in the spectroscopic ellipsometry method used to measure the extinction coefficient and refractive index described later.

[0024] (1) Element content The elemental content is measured using a sample with a film thickness of 150 nm, which was prepared by setting the Ar / C4F8 flow rate ratio to 1 / 4 and 1 / 1, respectively. The elemental ratios on the sample surface and inside the film, which was etched with Ar at an acceleration energy of 700 kV, are measured by X-ray photoelectron spectroscopy (XPS). The measurement depths inside the film are 10 nm and 30 nm from the surface. The XPS device used is a JPS-9010TR manufactured by JEOL Ltd. The depth resolution for measurements of the film surface and inside the film is approximately 5 nm. The elemental ratios inside the film were the same at depths of 10 nm and 30 nm, so they were collectively referred to as the elemental ratios inside the film.

[0025] Specifically, for a sample with an Ar / C4F8 flow rate of 1 / 4, -Element ratio of film surface: F content 50 atomic %, C content 38 atomic %, O content 12 atomic %, -Element ratio inside the film: F content 32 atomic %, C content 58 atomic %, O content 10 atomic %, It is.

[0026] On the other hand, in the sample with an Ar / C4F8 flow ratio of 1 / 1, -Element ratio of film surface: F content 73 atomic %, C content 23 atomic %, O content 4 atomic %, -Element ratio inside the film: F content 38 atomic %, C content 54 atomic %, O content 8 atomic %, By setting the Ar / C4F8 flow rate ratio at 1 / 1, the F content at the film surface was improved to 73 atomic %. The F content also increased inside the film, although not as much as at the film surface. It can be seen that the Ar / C4F8 flow rate ratio affects the element profile in the film thickness direction of the fluorine-containing amorphous carbon film 10.

[0027] (2) Light transmittance Figure 3 shows the light transmittance characteristics of samples fabricated with different film thicknesses and gas flow ratios. The light transmittance of samples fabricated with film thicknesses set to 50 nm, 100 nm, and 150 nm for each of the three gas flow ratios mentioned above is measured using an ultraviolet-visible spectrometer (Shimadzu UV-Vis3600Plus). The gray circles indicate the light transmittance of samples with an Ar / C4F8 flow ratio of 1 / 1, the clay squares indicate the light transmittance of samples with an Ar / C4F8 flow ratio of 1 / 2, and the white triangles indicate the light transmittance of samples with an Ar / C4F8 flow ratio of 1 / 4. The slight variation in film thickness among samples is due to process variation. Regardless of the gas flow ratio, high light transmittance is achieved for all samples. Even at a film thickness of 150 nm, a light transmittance of over 90% is obtained, making the film highly practical as a protective film for displays. When the film thickness is 100 nm or less, the light transmittance is 94% or more, and when the film thickness is 50 nm, the light transmittance is 97% or more. Even when the Ar / C4F8 flow rate ratio is 1 / 4, the film has a high light transmittance that is applicable to displays.

[0028] (3) Extinction coefficient Figure 4 shows the light absorption characteristics of samples made with different gas flow ratios. The horizontal axis is the wavelength, and the vertical axis is the extinction coefficient. The extinction coefficient, together with the refractive index (described later), was measured by spectroscopic ellipsometry using an Accurion EP4 Imaging Ellipsometer. The extinction coefficient indicates the degree of light absorption. All samples had a small extinction coefficient of 0.025 or less at a wavelength of 350 nm, meaning that there was almost no light absorption of visible light. In particular, when the Ar / C4F8 flow ratio was 1 / 2, the extinction coefficient was 0.010 or less. Even when the Ar / C4F8 flow ratio was 1 / 4, the extinction characteristics were sufficient for use in displays.

[0029] (4) Refractive index Figure 5 shows the refractive index at a wavelength of 550 nm for samples fabricated with different gas flow ratios. The refractive index of the sample with an Ar / C4F8 flow ratio of 1 / 2 is 1.40, and the refractive index of the sample with an Ar / C4F8 flow ratio of 1 / 1 is 1.39. In contrast, the refractive index of the sample with an Ar / C4F8 flow ratio of 1 / 4 is 1.46. The sample with an Ar / C4F8 flow ratio of 1 / 4 has good light transmittance and extinction coefficient, but the refractive index cannot be sufficiently lowered, making it difficult to apply in situations where anti-reflection function is a priority.

[0030] (5) Water droplet contact angle FIG. 6 shows the water droplet contact angle of samples prepared with different gas flow ratios. The water droplet contact angle of each sample is measured by the sessile drop method using DM-500 manufactured by Kyowa Interface Science Co., Ltd. The water droplet contact angle of the sample with an Ar / C4F8 flow ratio of 1 / 2 is 95°, and the water droplet contact angle of the sample with an Ar / C4F8 flow ratio of 1 / 4 is 92.5°. Both have sufficient water droplet contact angles and have high antifouling effects. For reference, the water droplet contact angle of the sample prepared by further increasing the Ar ratio to 2 / 1 is 101.7° and has high water repellency. From the viewpoint of antifouling, the Ar / C4F8 flow ratio is 1 / 4 or more, preferably 1 / 2 or more.

[0031] (6)Hardness The hardness of each sample is measured by nanoindentation. When measuring by nanoindentation, the film thickness is preferably 250 nm or more, so the hardness is measured using a sample with a film thickness of 250 nm. The measurement is performed using a Nano Indenter G200 manufactured by Toyo Corporation. The hardness of the sample with an Ar / C4F8 flow rate ratio of 1 / 2 is 0.76 GPa, and the hardness of the sample with an Ar / C4F8 flow rate ratio of 1 / 1 is 0.65 GPa. The hardness of the sample with an Ar / C4F8 flow rate ratio of 1 / 4 is 0.48 GPa, which is slightly less hard than the other samples.

[0032] In Example 1, according to the above characteristic evaluation, in order to satisfy all the requirements for hard coat, anti-reflection, and anti-soiling, the flow rate ratio of the raw material gas (fluorocarbon gas) to the inert gas is preferably greater than 1 / 4, and more preferably greater than 1 / 2.

[0033] <Example 2> In Example 2, the Ar / C4F8 flow rate ratio is fixed, and the deposition pressure is changed to prepare a plurality of types of samples. The same high-frequency plasma CVD deposition apparatus 100 as in Example 1 is used. The inert gas is Ar, the raw material gas is C4F8, and a high-frequency power of 13.56 MHz and 200 W is applied to the electrode 101 under reduced pressure, and plasma is excited between the electrode 102 facing the electrode 101 to deposit a fluorine-containing amorphous carbon film 10 on a quartz glass substrate 11 placed on the electrode 101. The Ar / C4F8 flow rate ratio is set to 1 / 2, and the deposition pressure is changed to 12 Pa, 24 Pa, and 48 Pa. For the samples prepared at each deposition pressure, the film thickness, light transmittance, element content inside the film, refractive index, and water droplet contact angle are measured.

[0034] 7 shows the relationship between the film formation pressure and the light transmittance. The film formation pressure is shown as the composite pressure of the gas pressures in the chamber 104 during film formation. When the film formation pressure is 12 Pa and 24 Pa, the light transmittance is 90% or more, but when the film formation pressure is 36 Pa, the light transmittance drops to less than 85%. For this reason, it is preferable to set the film formation pressure to less than 36 Pa, for example, 35 Pa or less, preferably 30 Pa or less, and more preferably 24 Pa or less.

[0035] FIG. 8 shows the elemental content of films formed at different pressures. The elemental content is measured at a depth of 20 nm from the film surface by etching and XPS. There is no significant difference in the carbon (C) content, but the fluorine (F) content is 45 atomic % at film formation pressures of 12 Pa and 24 Pa, while it is 40 atomic % at film formation pressure of 36 Pa, and the oxygen (O) content increases accordingly. In order to increase the fluorine ratio and lower the refractive index while ensuring hardness and transparency, it is desirable for the film formation pressure to be less than 36 Pa, for example, 35 Pa or less, preferably 30 Pa or less, and more preferably 24 Pa or less.

[0036] Figure 9 shows the relationship between the film formation pressure and the refractive index. When the film formation pressure is 24 Pa, a refractive index of 1.38 is obtained, and when the film formation pressure is 12 Pa, a refractive index lower than 1.36 is realized. When the film formation pressure is 36 Pa, the refractive index becomes 1.40. Although a film with a refractive index of 1.40 can be used as an anti-reflective film, taking into consideration hardness and transparency, it is found that the film formation pressure is preferably less than 36 Pa, for example, 35 Pa or less, preferably 30 Pa or less, and more preferably 24 Pa or less.

[0037] Figure 10 shows the relationship between the film formation pressure and the water droplet contact angle. A contact angle of nearly 95° was obtained at film formation pressures of 24 Pa and 36 Pa, and a contact angle of over 100° was obtained at 12 Pa. Even at a pressure of 36 Pa, a fluorine-containing amorphous carbon film with antifouling properties was obtained.

[0038] From the results of Example 2, it was confirmed that in order to provide all the functions of hard coating, anti-reflection, and anti-soiling, the film formation pressure is less than 36 Pa, for example, 35 Pa or less, preferably 30 Pa or less, and more preferably 24 Pa or less. On the other hand, since the film formation speed also decreases as the film formation pressure decreases (1 nm / s at a film formation pressure of 24 Pa, and 0.5 nm / s at 12 Pa), in order to realize a film formation speed suitable for practical use at an industrial level, the film formation pressure is preferably 6 Pa or more.

[0039] <Example 3> In Example 3, the film formation pressure is fixed, and the ratio of the inert gas to the raw material gas is changed in the direction of increasing, and the composition and characteristics are evaluated. A quartz glass substrate 11 is placed in the same film formation apparatus 100 as in Examples 1 and 2, and the film formation pressure is fixed at 24 Pa. The inert gas is Ar gas, and the raw material gas is C4F8 gas. The Ar / C4F8 flow rate ratio is changed to 1 / 2, 3 / 2, 5 / 2, and 7 / 2, and a sample with a film thickness of 250 nm is prepared, and the element content, refractive index, light transmittance, and water droplet contact angle are measured. The measurement method is the same as in Examples 1 and 2.

[0040] (1) Element content FIG. 11 shows the elemental content in the film when the gas flow ratio is changed in Example 3. Etching is performed by accelerating Ar ions at 700 kV, and the elemental content in the thin film is measured by XPS using JPS-9010TR manufactured by JEOL Ltd. The surface layer is from the surface to a depth of 5 nm, the intermediate layer is at a depth of 80-160 nm, and the substrate vicinity is at a depth of 240 nm, and XPS measurements are performed at each depth. In the surface layer to a depth of 5 nm, the fluorine (F) content increases as the Ar / C4F8 flow ratio increases, and is 61 atomic % or more in all cases. In the intermediate layer, the F content is stable at 40 atomic % when the Ar / C4F8 flow ratio is 1 / 2, 3 / 2, or 5 / 2, but when the flow ratio is increased to 7 / , the F content increases to 43 atomic %. Even near the substrate, the F content is stable at nearly 40 atomic % except for the flow ratio of 3 / 2, and even at the flow ratio of 3 / 2, the F content is 30 atomic % or more. This result is consistent with the result of Example 1. On the other hand, the C element content is higher in the intermediate layer and in the vicinity of the substrate than in the surface layer. The O element content does not change significantly in the thickness direction, and is not significantly affected by changes in the Ar / C4F8 flow rate ratio.

[0041] (2) Refractive index FIG. 12 shows the relationship between the Ar / C4F8 flow ratio and the refractive index. The refractive index at a wavelength of 500 nm is measured for each sample prepared in Example 3 by spectroscopic ellipsometry. The higher the Ar / C4F8 flow ratio, the lower the refractive index. At a flow ratio of 7 / 2, the refractive index values ​​are distributed in the range of 1.32 to 1.36, with a median value of 1.34. It is expected that a stable refractive index of 1.32 can be obtained by reducing the deposition pressure and increasing the gas flow ratio. The fluorine-containing amorphous carbon film is effectively used as an anti-reflective film.

[0042] (3) Light transmittance FIG. 13 shows the relationship between the Ar / C4F8 flow ratio and the light transmittance. Each sample prepared in Example 3 is measured using ultraviolet-visible spectroscopy. For reference, light with a wavelength of 400 nm to 800 nm is transmitted through a sample of a quartz glass substrate 11 with no film formed on its surface, and the transmittance is measured. D "without film" is the transmission spectrum of a quartz glass substrate 11 with no film formed on its surface. E, F, G, and H are expressed in terms of the Ar:C4F8 flow ratio, and correspond to flow ratios of 1 / 2, 3 / 2, 5 / 2, and 7 / 2, respectively. All samples have a transmittance of 90% or more in the visible light region, showing high light transmittance.

[0043] (4) Water droplet contact angle FIG. 14 shows the relationship between the Ar / C4F8 flow rate ratio and the water droplet contact angle. The water droplet contact angle is measured by the sessile drop method for each sample prepared in Example 3. For reference, the water droplet contact angle is measured for a quartz glass substrate with no film formed on its surface. In all samples, the water droplet contact angle is 90° or more. The water droplet contact angle increases when the ratio of Ar gas is increased. The water droplet contact angle is 94.6° when the flow rate ratio is 1 / 2, and the water droplet contact angle is 100.3° when the flow rate ratio is 7 / 2. For the quartz glass with no film formed on its surface, the water droplet contact angle does not even reach 60°, and it is found that the fluorine-containing amorphous carbon film of Example 3 has a high antifouling effect.

[0044] Based on the measurements and evaluations of Examples 1 to 3, the fluorine-containing amorphous carbon film 10 of the embodiment is characterized in that the fluorine content in a region shallower than 10 nm from the surface is higher than that in a region 12 at a depth of 10 nm or more. If there are many C-F bonds in the surface layer, polarization is suppressed, and interactions such as reverse polarization induced by light or electromagnetic waves are small, making it easy to transmit light and resulting in low refraction. The fluorine content inside the film is also 40 atomic % on average, and polarization inside the film is also suppressed, resulting in an extremely low refractive index. Thus, the fluorine-containing amorphous carbon film 10 of the embodiment has an amorphous carbon fluoride film with a high fluorine content formed near the surface, and also has a high fluorine content inside and does not contain hydrogen, so that it has extremely excellent optical properties.

[0045] In the above embodiment, C4F8 is used as the raw material gas, but fluorocarbon gas such as CF4, C2F6, C3F8, etc. may be used, or a mixture gas of two or more gases selected from CF4, C2F6, C3F8, and C4F8 may be used. The plasma excitation of Ar gas promotes the decomposition of fluorocarbon molecules, and promotes the radicalization and ionization of C, F, and CF groups. In particular, when the flow rate of Ar gas is 50% or more of the flow rate of the fluorocarbon raw material gas, the decomposition and activation of the fluorocarbon gas is promoted, and the fluorine content in the film is increased.

[0046] The fluorocarbon gas is dissociated by the Ar plasma to generate an amorphous CF film, but Ar ions also have an etching effect, and when the Ar gas flow rate is four times or more that of the fluorocarbon raw material gas, the etching effect becomes large and the film formation rate decreases. Figure 15 shows the relationship between each flow rate ratio and the film formation rate at a film formation pressure of 24 Pa. The higher the Ar ratio, the lower the film formation rate becomes, but when the bar graph in Figure 15 is extrapolated, it is possible to increase the Ar gas flow rate ratio until the film formation rate drops to 0.1 nm / s, which is considered to be unsuitable for practical use at an industrial level, and further improvement in optical properties can be expected. In this case, the Ar gas flow rate ratio to the raw material gas can be increased to 11 / 1. From the above, it is preferable that the flow rate ratio of Ar gas to the raw material gas is greater than 1 / 4 and less than or equal to 11 / 1.

[0047] On the other hand, the moment the plasma excitation stops, the etching effect of the Ar ions decreases, and activated CF radicals and CF ions accumulate near the surface to a thickness of several nm, forming an amorphous CF film with a high fluorine content. The higher the fluorine content of the surface, the lower the surface reflectance due to the weak polarization of the F atoms, and the better the optical properties are, such as increased light transmittance and a lower refractive index. In addition, the surface free energy decreases, increasing water repellency and improving antifouling properties.

[0048] In conclusion, the fluorine-containing amorphous carbon film 10 of the embodiment is a single layer film made of carbon, fluorine, and oxygen, and has an average fluorine content of 30 atomic % to 40 atomic % in the thickness direction, an average oxygen content of 5 atomic % to 20 atomic % in the thickness direction, and the remainder is carbon atoms. Meanwhile, a region shallower than 10 nm deep from the surface becomes a high-concentration fluorine-containing region 13, and has a fluorine content of 50 atomic % to 75 atomic % and an oxygen content of 5 atomic % to 20 atomic % in the thickness direction, and the remainder is carbon atoms.

[0049] The fluorine-containing amorphous carbon film 10 of the embodiment is a thin film with excellent optical properties (low reflectance, high light transmittance, low refractive index) and excellent antifouling properties, and is highly hard, making it suitable as a protective coating for mobile displays such as smartphones. In addition, the film can be formed at low cost in a short time using plasma CVD at low pressure. The fluorine-containing amorphous carbon film 10 can be formed at low cost through a single film formation process, and is advantageous in terms of cost. A thin film with excellent optical properties and antifouling properties can be produced at low cost using a raw material gas whose chemical formula is represented only by carbon and fluorine, making it suitable for mass production of protective films for displays and transparent panels.

[0050] The above disclosure includes the following aspects. (Section 1) A fluorine-containing amorphous carbon film, It is composed of a single layer of carbon, fluorine, and oxygen, the average fluorine content in the film thickness direction is 30 atomic % or more and 40 atomic % or less, the average oxygen content in the film thickness direction is 5 atomic % or more and 20 atomic % or less, and the remainder is carbon atom; Fluorine-containing amorphous carbon film. (Section 2) a high-concentration fluorine-containing region having a higher fluorine content in a region shallower than 10 nm deep from the surface compared to a region having a depth of 10 nm or more; The fluorine content in the high-concentration fluorine-containing region is 50 atomic % or more and 75 atomic % or less, the oxygen content is 5 atomic % or more and 20 atomic % or less, and the remainder is carbon atoms. Item 1. A fluorine-containing amorphous carbon film according to item 1. (Section 3) The refractive index of the monolayer film is 1.32 or more and less than 1.40. Item 3. A fluorine-containing amorphous carbon film according to item 1 or 2. (Section 4) The light transmittance of the monolayer film is 90% or more. Item 4. The fluorine-containing amorphous carbon film according to any one of items 1 to 3. (Section 5) The water droplet contact angle of the monolayer film is 90° or more. Item 5. A fluorine-containing amorphous carbon film according to any one of items 1 to 4. (Section 6) The hardness of the monolayer film is 0.65 GPa or more as measured by a nanoindentation method. Item 6. The fluorine-containing amorphous carbon film according to any one of items 1 to 5. (Section 7) The thickness of the monolayer film is 25 nm or more and 500 nm or less. Item 7. A fluorine-containing amorphous carbon film according to any one of items 1 to 6. (Section 8) The thickness of the monolayer film is 50 nm to 250 nm; Item 8. A fluorine-containing amorphous carbon film according to item 7. (Section 9) A substrate is placed in the chamber; A source gas whose chemical formula is represented only by carbon and fluorine and an inert gas for diluting the source gas are introduced into the chamber, and a fluorine-containing amorphous carbon film is formed on the surface of the substrate under plasma generation; A mixing ratio of the inert gas to the source gas is set to be greater than 1 / 4 and less than 11 / 1 in terms of a flow rate ratio into the chamber; A method for producing a fluorine-containing amorphous carbon film. (Section 10) A mixing ratio of the inert gas to the source gas is set to 1 / 2 or more and 7 / 2 or less in terms of a flow rate ratio into the chamber. Item 10. A method for producing a fluorine-containing amorphous carbon film according to item 9. (Section 11) Set the pressure in the chamber to 24 Pa or less. Item 11. A method for producing a fluorine-containing amorphous carbon film according to item 9 or 10. (Section 12) The raw material gas is CF4, C2F6, C3F8, C4F8, or a mixed gas of two or more gases selected therefrom; Item 11. A method for producing a fluorine-containing amorphous carbon film according to any one of items 9 to 10. (Section 13) The inert gas is Ar gas. Item 13. A method for producing a fluorine-containing amorphous carbon film according to any one of items 9 to 12. [Explanation of symbols]

[0051] 10 Fluorine-containing amorphous carbon film 11 Substrate 12 areas 13 High concentration fluorine-containing area 100 Film deposition equipment 104 Chamber

Claims

1. A fluorine-containing amorphous carbon film, It is composed of a single layer of carbon, fluorine, and oxygen, an average fluorine content in the film thickness direction is 30 atomic % or more and 40 atomic % or less, an average oxygen content in the film thickness direction is 5 atomic % or more and 20 atomic % or less, and the remainder is carbon atom; Fluorine-containing amorphous carbon film.

2. a high-concentration fluorine-containing region having a higher fluorine content in a region shallower than 10 nm in depth from the surface than in a region having a depth of 10 nm or more; the high-concentration fluorine-containing region has a fluorine content of 50 atomic % or more and 75 atomic % or less, an oxygen content of 5 atomic % or more and 20 atomic % or less, and the remainder being carbon atoms; The fluorine-containing amorphous carbon film according to claim 1 .

3. The refractive index of the monolayer film is 1.32 or more and less than 1.

40. The fluorine-containing amorphous carbon film according to claim 1 .

4. The light transmittance of the monolayer film is 90% or more. The fluorine-containing amorphous carbon film according to claim 1 .

5. The water droplet contact angle of the monolayer film is 90° or more. The fluorine-containing amorphous carbon film according to claim 1 .

6. The hardness of the monolayer film is 0.65 GPa or more as measured by a nanoindentation method. The fluorine-containing amorphous carbon film according to claim 1 .

7. The thickness of the monolayer film is 25 nm or more and 500 nm or less. The fluorine-containing amorphous carbon film according to claim 1 .

8. The thickness of the monolayer film is 50 nm to 250 nm. The fluorine-containing amorphous carbon film according to claim 7.

9. A substrate is placed in the chamber; A source gas whose chemical formula is represented only by carbon and fluorine and an inert gas for diluting the source gas are introduced into the chamber, and a fluorine-containing amorphous carbon film is formed on the surface of the substrate under plasma generation; A mixing ratio of the inert gas to the source gas is set to be greater than 1 / 4 and smaller than 11 / 1 in terms of a flow rate ratio into the chamber; A method for producing a fluorine-containing amorphous carbon film.

10. a mixing ratio of the inert gas to the source gas is set to 1 / 2 or more and 7 / 2 or less in terms of a flow rate ratio into the chamber; The method for producing a fluorine-containing amorphous carbon film according to claim 9 .

11. Set the pressure in the chamber to 24 Pa or less. The method for producing a fluorine-containing amorphous carbon film according to claim 9 .

12. The source gas is CF 4 , C 2 F 6 , C 3 F 8 , C 4 F 8 or a mixture gas of two or more gases selected from these; The method for producing a fluorine-containing amorphous carbon film according to claim 9 .

13. The inert gas is Ar gas. The method for producing a fluorine-containing amorphous carbon film according to any one of claims 9 to 12.

Citation Information

Patent Citations

  • Coating liquid for formation of low-refractive-index film, low-refractive-index film, production method of low-refractive-index film and application article

    JP2015224302A

  • Antireflection film and manufacturing method thereof

    JP2021076849A