Wax composition for toner

The wax composition for toner, comprising specific fatty acid esters and a metal salt, addresses the challenges of low-temperature fixability, blocking resistance, and scratch resistance, ensuring performance under high humidity and temperature conditions.

JP2024161990APending Publication Date: 2024-11-21NOF CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023077105
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional toners face challenges in achieving both low-temperature fixability and blocking resistance, have poor scratch resistance, and fail to maintain performance under high temperature and high humidity environments.

Method used

A wax composition for toner containing specific types of fatty acid esters and a fatty acid metal salt, formulated in precise mass ratios, to enhance scratch resistance, low-temperature fixing properties, and color development while preventing blocking in high-temperature, high-humidity conditions.

Benefits of technology

The wax composition improves scratch resistance, low-temperature fixing properties, and color development, while maintaining these properties even under high temperature and high humidity, effectively suppressing deterioration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161990000001
    Figure 2024161990000001
  • Figure 2024161990000002
    Figure 2024161990000002
  • Figure 2024161990000003
    Figure 2024161990000003
Patent Text Reader

Abstract

To provide a wax composition for toner, capable of improving toner scratch resistance, low temperature fixability and coloring development, excellent in blocking resistance and capable of suppressing deterioration in the performance of toner in high temperature and humidity environment.SOLUTION: A wax composition for toner includes specific fatty esters A, B and C. When setting the total of the fatty esters A, B and C to 100 mass%, the content of the fatty ester A is 5-50 mass%, the content of the fatty ester B is 20-90 mass% and the content of the fatty ester C is 1-50 mass%; the mass ratio of the fatty ester A to the total of the fatty esters B and C is 5:95-50:50; the mass ratio of the fatty ester B to the fatty ester C is 95:5-50:50; and the content of a specific fatty acid metal salt D to the total 100 pts.mass of the fatty esters A, B and C is 0-1 pt.mass.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wax composition for toners which is suitably used for toners used in developing electrostatic images recorded by electrophotography, electrostatic recording or the like in image forming apparatuses such as copying machines and laser printers. [Background technology]

[0002] Toners used in image forming devices such as copiers and printers contain a thermoplastic resin (hereinafter simply referred to as "resin") that serves as a binder resin, a colorant (carbon black, magnetic powder, pigment, etc.), a charge control agent, wax, and, if necessary, further contain a fluidity additive, a cleaning aid, a transfer aid, etc. Among these, the wax has the function of preventing the toner from remaining on the fixing roll during fixing (filming), and of promoting the softening of the resin to improve fixing properties.

[0003] In recent years, growing global environmental awareness has led to demands for reduced power consumption and faster printing speeds, and so there has been a focus on lowering the fixing temperature of toners. This has created a demand for waxes that can improve the low-temperature fixing properties of toners. Since the low-temperature fixability of a toner can be improved by lowering the melting temperature of a resin, one method for improving the low-temperature fixability of a toner is to lower the melting point of the wax. On the other hand, a lower melting point of the wax causes the wax to dissolve onto the toner surface during storage of the toner, resulting in a problem of blocking between toner particles. In response to this, Patent Document 1 discloses a toner wax composition in which an ester of a linear saturated fatty acid and a linear saturated alcohol, and an ester of a linear saturated fatty acid and a neopentyl polyol are mixed in a specific mass ratio as a wax that achieves both low-temperature fixability and blocking resistance of a toner.

[0004] Furthermore, as printing speeds increase, printed matter comes into contact with each other more frequently, and printed images are scraped off due to friction and load, so a toner with excellent abrasion resistance is also desired. Patent Document 2 discloses a toner that contains a mixture of a specific polyhydric alcohol ester compound and a small amount of a specific polyhydric alcohol partial ester compound as a release agent (wax), as a toner with excellent low-temperature fixing ability and abrasion resistance of printed images.

[0005] Furthermore, with the spread of print-on-demand digital printing in the commercial printing field, printed matter with high graphic output and unconventional metallic printed matter have appeared, and as the demand for toners with good color development increases, materials that can contribute to high color development are also required. In response to this, Patent Document 3 discloses an ester compound containing a pentaerythritol-derived component, a C14-24 linear saturated fatty acid-derived component, and an adipic acid-derived component in specific ratios as a toner wax that can impart low-temperature fixing properties and blocking resistance to toners and improve color development.

[0006] In recent years, copiers, printers, and the like have been rapidly spreading in emerging countries. Countries classified as emerging countries often have environments with much higher temperatures and humidity than developed countries, and toner in a cartridge is more likely to absorb moisture, raising concerns about poor toner performance. For this reason, a toner that can maintain its performance even in a high-temperature, high-humidity environment is in demand. Patent Document 4 discloses a toner that contains a crystalline polyester resin component and a specific non-crystalline polyester resin component as a binder resin, thereby having excellent low-temperature fixing ability even after being exposed to a high-temperature, high-humidity environment. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2010-122425 A [Patent Document 2] JP 2005-157039 A [Patent Document 3] Patent Publication No. 2021-196608 [Patent Document 4] JP 2022-43977 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, with conventional toners, it has been difficult to achieve both low-temperature fixability and blocking resistance, excellent abrasion resistance and color development, and maintain toner performance in a high-temperature and high-humidity environment. The toner containing the wax disclosed in Patent Document 1 has not been examined for abrasion resistance, and may not have sufficient abrasion resistance. The toners containing the wax disclosed in Patent Documents 2 and 3 have not been examined under high temperature and high humidity conditions, and may not have sufficient performance after being exposed to a high temperature and high humidity environment. The toner disclosed in Patent Document 4 can maintain low-temperature fixability even after exposure to a high-temperature, high-humidity environment, but no consideration has been given to its abrasion resistance and color development, and it is possible that the toner may not have sufficient performance after exposure to a high-temperature, high-humidity environment.

[0009] The present invention has been made in consideration of the above problems, and has an object to provide a wax composition for a toner that can improve the abrasion resistance, low-temperature fixing property and color development of a toner, improve the blocking resistance of the toner, and suppress deterioration of the abrasion resistance, low-temperature fixing property and color development of the toner in a high-temperature and high-humidity environment. [Means for solving the problem]

[0010] As a result of intensive research conducted by the present inventors to solve the above problems, they discovered that a wax composition containing three specific types of fatty acid esters and having a controlled content of specific fatty acid metal salts improves the abrasion resistance, low-temperature fixing property and color development of a toner, suppresses blocking between toner particles in a high-temperature and high-humidity environment, and maintains the abrasion resistance, low-temperature fixing property and color development performance of the toner, thereby completing the present invention.

[0011] That is, the toner wax composition of the present invention contains fatty acid ester A, fatty acid ester B, and fatty acid ester C, The fatty acid ester A is a diester compound of a divalent linear saturated fatty acid having 10 to 30 carbon atoms and a monovalent linear saturated alcohol having 12 to 24 carbon atoms, The fatty acid ester B is a monoester compound of a monovalent linear saturated fatty acid having an even carbon number of 10 to 30 and a monovalent linear saturated alcohol having a carbon number of 12 to 24, The fatty acid ester C is a monoester compound of a monovalent linear saturated fatty acid having an odd carbon number of 11 to 29 and a monovalent linear saturated alcohol having a carbon number of 12 to 24, When the total amount of the fatty acid ester A, the fatty acid ester B, and the fatty acid ester C is taken as 100% by mass, the content of the fatty acid ester A is 5 to 50% by mass, the content of the fatty acid ester B is 20 to 90% by mass, and the content of the fatty acid ester C is 1 to 50% by mass, a mass ratio of the fatty acid ester A to the total of the fatty acid ester B and the fatty acid ester C (fatty acid ester A: the total of fatty acid ester B and fatty acid ester C) is 5:95 to 50:50; a mass ratio of the fatty acid ester B to the fatty acid ester C (fatty acid ester B:fatty acid ester C) is 95:5 to 50:50; The toner wax composition includes a fatty acid metal salt D having a content of 0 to 1 part by mass relative to a total of 100 parts by mass of the fatty acid ester A, the fatty acid ester B, and the fatty acid ester C, and the fatty acid metal salt D is a salt of a monovalent linear saturated fatty acid having 10 to 30 carbon atoms and at least one metal selected from the group consisting of sodium, potassium, and calcium. Effect of the Invention

[0012] The wax composition for toner of the present invention can improve the abrasion resistance, low-temperature fixing property and color development of the toner, suppress blocking between toner particles in a high-temperature and high-humidity environment, and maintain the abrasion resistance, low-temperature fixing property and color development performance of the toner. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described. In this specification, a numerical range defined using the symbol "~" is intended to include both the upper and lower limits of the symbol "~". For example, "2~10" represents a range of 2 or more and 10 or less.

[0014] The toner wax composition of the present invention contains at least fatty acid ester A, fatty acid ester B, and fatty acid ester C, and fatty acid metal salt D is an optional component. Each component will be described below.

[0015] [Fatty acid ester A] The fatty acid ester A used in the present invention is a diester compound of a divalent linear saturated fatty acid having 10 to 30 carbon atoms and a monovalent linear saturated alcohol having 12 to 24 carbon atoms.

[0016] The divalent linear saturated fatty acid used in the fatty acid ester A has a carbon number of 10 to 30, preferably 12 to 30, more preferably 20 to 30, and further preferably 24 to 30. In addition, the carbon number of the divalent linear saturated fatty acid used in the fatty acid ester A is preferably an even number. Examples of the divalent linear saturated fatty acid used in the fatty acid ester A include decanedioic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane dioic acid, docosane dioic acid, tetracosane dioic acid, hexacosane dioic acid, octacosane dioic acid, and triacontanedioic acid.

[0017] The monohydric linear saturated alcohol used in the fatty acid ester A has a carbon number of 12 to 24, preferably 14 to 24, more preferably 16 to 24, and further preferably 18 to 24. The carbon number of the monohydric linear saturated alcohol used in the fatty acid ester A is preferably an even number. Examples of the monovalent linear saturated alcohol used in the fatty acid ester A include lauryl alcohol, myristyl alcohol, palmityl alcohol, stearyl alcohol, arachidyl alcohol, behenyl alcohol, lignoceryl alcohol, etc. Among them, monovalent linear saturated alcohols having 18 to 22 carbon atoms such as stearyl alcohol (octadecyl alcohol), arachidyl alcohol (icosanol), and behenyl alcohol (docosanol) are preferred.

[0018] The number of carbon atoms in the diester compound used as the fatty acid ester A is not particularly limited, but is preferably 40-76, more preferably 48-72, and further preferably 56-64.

[0019] [Fatty acid ester B] The fatty acid ester B used in the present invention is a monoester compound of a monovalent linear saturated fatty acid having an even number of carbon atoms of 10 to 30 and a monovalent linear saturated alcohol having 12 to 24 carbon atoms.

[0020] The carbon number of the monovalent linear saturated fatty acid used in fatty acid ester B is 10 to 30 and an even number, preferably 12 to 30 and an even number, more preferably 20 to 30 and an even number, and further preferably 24 to 30 and an even number. Examples of the monovalent linear saturated fatty acid used in the fatty acid ester B include decanoic acid, dodecanoic acid, tetradecanoic acid, hexadecanoic acid, octadecanoic acid, eicosanoic acid, docosanoic acid, tetracosanoic acid, hexacosanoic acid, octacosanoic acid, and triacontanoic acid. The explanation of the monohydric linear saturated alcohol used in the fatty acid ester B is the same as the explanation of the monohydric linear saturated alcohol used in the fatty acid ester A described above.

[0021] The number of carbon atoms in the monoester compound used as fatty acid ester B is not particularly limited, but is preferably 26-56, more preferably 28-50, and further preferably 30-46.

[0022] [Fatty acid ester C] The fatty acid ester C used in the present invention is a monoester compound of a monovalent linear saturated fatty acid having an odd carbon number of 11 to 29 and a monovalent linear saturated alcohol having 12 to 24 carbon atoms.

[0023] The carbon number of the monovalent linear saturated fatty acid used in the fatty acid ester C is 11 to 29 and an odd number, preferably 13 to 29 and an odd number, more preferably 21 to 29 and an odd number, and further preferably 25 to 29 and an odd number. Examples of the monovalent linear saturated fatty acid used in the fatty acid ester C include undecanoic acid, tridecanoic acid, pentadecanoic acid, heptadecanoic acid, nonadecanoic acid, henicosanoic acid, tricosanoic acid, pentacosanoic acid, heptacosanoic acid, and nonacosanoic acid. The explanation of the monohydric linear saturated alcohol used in the fatty acid ester C is the same as the explanation of the monohydric linear saturated alcohol used in the fatty acid ester A described above.

[0024] The number of carbon atoms in the monoester compound used as the fatty acid ester C is not particularly limited, but is preferably 27-55, more preferably 29-51, and further preferably 31-47.

[0025] Examples of the methods for producing the above-mentioned fatty acid ester A, fatty acid ester B, and fatty acid ester C include a synthesis method by oxidation reaction, synthesis from a fatty acid or its derivative, a method using a dehydration condensation reaction between an alcohol and a fatty acid, a method using a reaction between an acid halide and an alcohol, and a method using an ester exchange reaction. A catalyst may be used during the reaction. Examples of the catalyst include general acidic or alkaline catalysts used in esterification reactions, such as zinc acetate and titanium compounds. The above-mentioned fatty acid ester A, fatty acid ester B, and fatty acid ester C are obtained, for example, by an esterification reaction using the above-mentioned alcohol or its derivative and the above-mentioned fatty acid or its derivative as raw materials, and are typically obtained by a dehydration condensation reaction between the above-mentioned alcohol and fatty acid. When obtaining the above-mentioned fatty acid esters A, B and C, it is preferable to react the raw material alcohol with the raw material fatty acid so that the molar ratio of the hydroxyl group (-OH) of the raw material alcohol to the carboxyl group (-COOH) of the raw material fatty acid is 1:1, or so that there is a slight excess of either the hydroxyl group or the carboxyl group. After the esterification reaction, a deacidification step using an alkaline aqueous solution may be appropriately carried out, and the product may be further purified by a recrystallization method, a distillation method, a solvent extraction method or the like.

[0026] [Fatty acid metal salt D] The fatty acid metal salt D used in the present invention is a salt of a monovalent linear saturated fatty acid having 10 to 30 carbon atoms and at least one metal selected from the group consisting of sodium, potassium and calcium. Of these, sodium is preferred as the metal. The wax composition of the present invention improves the abrasion resistance, low-temperature fixability and color development of the toner, and inhibits blocking between toner particles even in a high-temperature, high-humidity environment while maintaining the abrasion resistance, low-temperature fixability and color development of the toner. This effect is further enhanced when the wax composition of the present invention contains fatty acid metal salt D in the amount described below.

[0027] The monovalent linear saturated fatty acid used in fatty acid metal salt D has a carbon number of 10 to 30, preferably 12 to 30, more preferably 20 to 30, and even more preferably 24 to 30. In addition, the carbon number of the monovalent linear saturated fatty acid used in fatty acid metal salt D is preferably an even number. Examples of the monovalent linear saturated fatty acid used in the fatty acid metal salt D include decanoic acid, dodecanoic acid, tetradecanoic acid, hexadecanoic acid, octadecanoic acid, eicosanoic acid, docosanoic acid, tetracosanoic acid, hexacosanoic acid, octacosanoic acid, and triacontanoic acid.

[0028] The fatty acid metal salt D can be obtained by various methods according to conventional methods. For example, it can be produced by any of the methods of fat and oil saponification, fatty acid neutralization, and methyl ester saponification. The apparatus may be either continuous or batch type. When preparing the fatty acid metal salt, it is common to add a basic metal hydroxide after dissolving the fatty acid, but the fatty acid may be added later, or the amount of metal hydroxide added may be adjusted to allow free fatty acid to remain.

[0029] [Wax Composition for Toner] The toner wax composition of the present invention contains the above-mentioned fatty acid ester A, fatty acid ester B, and fatty acid ester C in the following mass ratio. The toner wax composition of the present invention may further contain the above-mentioned fatty acid metal salt D in the following mass ratio. As disclosed in Patent Documents 1 to 4, fatty acid esters have been used conventionally as toner waxes. The toner wax composition of the present invention is a mixture containing the above-mentioned three fatty acid esters A, B, and C in a specific mass ratio and having the above-mentioned fatty acid metal salt D content of a specific amount or less, and thus can improve the abrasion resistance, low-temperature fixability, and color development of the toner compared to conventional toner waxes, improve the blocking resistance of the toner, and suppress deterioration of the abrasion resistance, low-temperature fixability, and color development of the toner in a high-temperature and high-humidity environment. Furthermore, by further containing the fatty acid metal salt D described above, the toner wax composition of the present invention exhibits the above-mentioned effects even more excellently compared to a toner wax consisting only of a fatty acid ester.

[0030] In the toner wax composition of the present invention, when the total of fatty acid ester A, fatty acid ester B and fatty acid ester C is taken as 100% by mass, the content of fatty acid ester A is 5 to 50% by mass, the content of fatty acid ester B is 20 to 90% by mass, and the content of fatty acid ester C is 1 to 50% by mass. Although not particularly limited, the content of fatty acid ester A is preferably 10 to 50% by mass, the content of fatty acid ester B is preferably 25 to 85% by mass, and the content of fatty acid ester C is preferably 5 to 25% by mass. In addition, when the total amount of the toner wax composition of the present invention is taken as 100% by mass, the total content of fatty acid ester A, fatty acid ester B, and fatty acid ester C is preferably 99% by mass or more. In other words, the content of other components different from fatty acid ester A, fatty acid ester B, or fatty acid ester C is preferably 1% by mass or less. The other components contained in the toner wax composition of the present invention are typically fatty acid metal salts D.

[0031] In the toner wax composition of the present invention, the mass ratio of fatty acid ester A to the total of fatty acid ester B and fatty acid ester C (fatty acid ester A: total of fatty acid ester B and fatty acid ester C) is 5:95 to 50:50, preferably 10:90 to 30:70. When the mass ratio of fatty acid ester A to the total of fatty acid ester B and fatty acid ester C is within the above range, the effect of improving the abrasion resistance, low-temperature fixability and color development of the toner, the effect of suppressing the decrease in blocking resistance of the toner, and the effect of suppressing the deterioration of the abrasion resistance, low-temperature fixability and color development of the toner in a high-temperature and high-humidity environment are excellent. In addition, when the toner wax composition of the present invention further contains fatty acid metal salt D, when the mass ratio of fatty acid ester A to the total of fatty acid ester B and fatty acid ester C is within the above range, the effect of fatty acid metal salt D in the wax composition is easily obtained.

[0032] In the toner wax composition of the present invention, the mass ratio of fatty acid ester B to fatty acid ester C (fatty acid ester B: fatty acid ester C) is 95:5 to 50:50, preferably 90:10 to 60:40. When the mass ratio of fatty acid ester B to fatty acid ester C is within the above range, the effect of improving the abrasion resistance, low-temperature fixability, and color development of the toner, the effect of suppressing the decrease in blocking resistance of the toner, and the effect of suppressing the deterioration of the abrasion resistance, low-temperature fixability, and color development of the toner in a high-temperature and high-humidity environment are excellent. In addition, when the toner wax composition of the present invention further contains fatty acid metal salt D, when the mass ratio of fatty acid ester B to fatty acid ester C is within the above range, the effect of fatty acid metal salt D in the wax composition is easily obtained.

[0033] In the toner wax composition of the present invention, the content of fatty acid metal salt D is 0 to 1 part by mass relative to 100 parts by mass in total of fatty acid ester A, fatty acid ester B, and fatty acid ester C. When the toner wax composition of the present invention contains fatty acid metal salt D, the content of fatty acid metal salt D is preferably 0.001 to 1 part by mass, more preferably 0.002 to 0.5 parts by mass, and even more preferably 0.003 to 0.1 part by mass relative to 100 parts by mass in total of fatty acid ester A, fatty acid ester B, and fatty acid ester C. When the content of fatty acid metal salt D is within the above range, the effect of the toner wax composition of the present invention becomes even more excellent.

[0034] In the toner wax composition of the present invention, in order to further enhance the above-mentioned effects, the difference between the maximum carbon number and the minimum carbon number among the carbon numbers of the divalent linear saturated fatty acid used in the fatty acid ester A, the carbon number of the monovalent linear saturated fatty acid used in the fatty acid ester B, and the carbon number of the monovalent linear saturated fatty acid used in the fatty acid ester C is preferably 6 or less, more preferably 3 or less, and even more preferably 1 or less. In the case where the toner wax composition of the present invention further contains fatty acid metal salt D, the difference between the maximum carbon number and the minimum carbon number among the carbon number of the divalent linear saturated fatty acid used in fatty acid ester A, the carbon number of the monovalent linear saturated fatty acid used in fatty acid ester B, the carbon number of the monovalent linear saturated fatty acid used in fatty acid ester C, and the carbon number of the monovalent linear saturated fatty acid used in fatty acid metal salt D is preferably 6 or less, more preferably 3 or less, and even more preferably 1 or less. In the toner wax composition of the present invention, the difference between the maximum carbon number and the minimum carbon number among the carbon numbers of the monovalent linear saturated alcohol used in the fatty acid ester A, the carbon number of the monovalent linear saturated alcohol used in the fatty acid ester B, and the carbon number of the monovalent linear saturated alcohol used in the fatty acid ester C is preferably 6 or less, more preferably 4 or less, and even more preferably 2 or less.

[0035] To obtain the toner wax composition of the present invention, the above-mentioned fatty acid ester A, fatty acid ester B, and fatty acid ester C, and other components such as fatty acid metal salt D as necessary, may be synthesized separately and then mixed, or may be synthesized all at once if possible in terms of reaction. When mixing, it is preferable to produce the toner wax composition of the present invention by heating and melting the components at a temperature equal to or higher than the melting point thereof, mixing uniformly, cooling and solidifying, and pulverizing or granulating the components.

[0036] The toner wax composition of the present invention is contained in a toner together with a binder resin, a colorant, a charge control agent, etc. The toner containing the toner wax composition of the present invention is produced by a conventional production method. The content of the toner wax composition of the present invention contained in the toner is preferably 0.1 to 15 parts by mass with respect to 100 parts by mass of the binder resin. The toner wax composition of the present invention may be contained in the toner either alone or in combination of two or more.

[0037] The binder resin is not particularly limited, and any of those conventionally used as binder resins for toners, such as styrene resin, acrylic ester resin, styrene-acrylic ester copolymer resin, polyester resin, polyvinyl chloride resin, polyvinyl acetate resin, phenol resin, and epoxy resin, can be used. The colorant is not particularly limited, and any of those conventionally used as toner colorants, such as carbon black, magnetic powder, and pigments of various colors, can be used. EXAMPLES

[0038] The present invention will now be described more specifically with reference to examples and comparative examples.

[0039] [Production Example A1: Preparation of fatty acid ester A1] Into a 2 L four-neck flask equipped with a nitrogen inlet tube, a stirring blade, and a cooling tube, 534 g (1.17 mol) of octacosane diacid and 665 g (2.46 mol) of octadecyl alcohol were added, and the mixture was reacted at 220°C for 10 hours under a nitrogen stream while distilling off the generated water, thereby obtaining a crude product. The crude product was recrystallized twice using 1 L of hexane per 100 g of the crude product to obtain a purified product, which was then dried under reduced pressure to obtain 720 g of dioctadecyl octacosanedioate (fatty acid ester A1).

[0040] [Production Example A2: Preparation of fatty acid ester A2] Dioctadecyl eicosanedioate (fatty acid ester A2) was obtained in the same manner as in Production Example A1, except that the raw material fatty acid was changed to the same molar amount of eicosanedioic acid.

[0041] [Production Example A3: Preparation of fatty acid ester A3] Dodecanedioic acid didocosyl (fatty acid ester A3) was obtained in the same manner as in Production Example A1, except that the raw material fatty acid was changed to the same molar amount of dodecanedioic acid and the raw material alcohol was changed to the same molar amount of docosanol.

[0042] [Production Example A4: Preparation of fatty acid ester A4] Didecyl eicosanedioate (fatty acid ester A4) was obtained in the same manner as in Production Example A1, except that the raw material fatty acid was changed to the same molar amount of eicosanedioic acid and the raw material alcohol was changed to the same molar amount of decyl alcohol.

[0043] [Table 1]

[0044] [Production Example B1: Preparation of fatty acid ester B1] In a 2 L four-neck flask equipped with a nitrogen inlet tube, a stirring blade, and a cooling tube, 900 g (2.12 mol) of octacosanoic acid and 546 g (2.02 mol) of octadecyl alcohol were added, and the mixture was reacted at 220°C for 10 hours under a nitrogen stream while distilling off the generated water, thereby obtaining a crude product. The crude product was recrystallized twice using 1 L of hexane per 100 g of the crude product to obtain a purified product, which was then dried under reduced pressure to obtain 710 g of octadecyl octacosanoate (fatty acid ester B1).

[0045] [Production Example B2: Preparation of fatty acid ester B2] Octadecyl eicosanoate (fatty acid ester B2) was obtained in the same manner as in Production Example B1, except that the raw material fatty acid was changed to the same molar amount of eicosanoic acid.

[0046] [Production Example B3: Preparation of fatty acid ester B3] Octadecyl dodecanoate (fatty acid ester B3) was obtained in the same manner as in Production Example B1, except that the raw material fatty acid was changed to the same molar amount of dodecanoic acid.

[0047] [Production Example B4: Preparation of fatty acid ester B4] Octadecyl octanoate (fatty acid ester B4) was obtained in the same manner as in Production Example B1, except that the raw material fatty acid was changed to the same molar amount of octanoic acid.

[0048] [Table 2]

[0049] [Production Example C1: Preparation of fatty acid ester C1] Into a 2 L four-neck flask equipped with a nitrogen inlet tube, a stirring blade, and a cooling tube, 930 g (2.12 mol) of nonacosanoic acid and 546 g (2.02 mol) of octadecyl alcohol were added, and the mixture was reacted at 220°C for 10 hours under a nitrogen stream while distilling off the generated water, thereby obtaining a crude product. The crude product was recrystallized twice using 1 L of hexane per 100 g of the crude product to obtain a purified product, which was then dried under reduced pressure to obtain 650 g of octadecyl nonacosanoate (fatty acid ester C1).

[0050] [Production Example C2: Preparation of fatty acid ester C2] Octadecyl henicosanoate (fatty acid ester C2) was obtained in the same manner as in Production Example C1, except that the raw fatty acid was changed to the same molar amount of henicosanoic acid.

[0051] [Production Example C3: Preparation of fatty acid ester C3] Octadecyl tridecanoate (fatty acid ester C3) was obtained in the same manner as in Production Example C1, except that the raw material fatty acid was changed to the same molar amount of tridecanoic acid.

[0052] [Production Example C4: Preparation of fatty acid ester C4] Octadecyl nonanoate (fatty acid ester C4) was obtained in the same manner as in Production Example C1, except that the raw material fatty acid was changed to the same molar amount of nonanoic acid.

[0053] [Table 3]

[0054] [Production Example D1: Preparation of fatty acid metal salt D1] 1000 g of octacosanoic acid was placed in a benchtop kneader (manufactured by Irie Shokai Co., Ltd., model: PNV-5H) as a fatty acid, and heated to the temperature at which the fatty acid melts (95°C) to completely melt it. Next, 313 g of 30% aqueous sodium hydroxide solution was added to the melted fatty acid, and the mixture was stirred for 30 minutes to neutralize the fatty acid, thereby obtaining a crude product. The obtained crude product was dried and dehydrated to obtain 1030 g of sodium octacosanoate (fatty acid metal salt D1).

[0055] [Production Example D2: Preparation of fatty acid metal salt D2] Sodium eicosanoate (fatty acid metal salt D2) was obtained in the same manner as in Production Example D1, except that the raw material fatty acid was changed to the same molar amount of eicosanoic acid.

[0056] [Production Example D3: Preparation of fatty acid metal salt D3] Sodium dodecanoate (fatty acid metal salt D3) was obtained in the same manner as in Production Example D1, except that the raw material fatty acid was changed to the same molar amount of dodecanoic acid.

[0057] [Production Example D4: Preparation of fatty acid metal salt D4] Sodium hexanoate (fatty acid metal salt D4) was obtained in the same manner as in Production Example D1, except that the raw material fatty acid was changed to the same molar amount of hexanoic acid.

[0058] [Table 4]

[0059] Wax compositions 1 to 12 will be specifically described below. [Example 1] 20 g of fatty acid ester A1, 56 g of fatty acid ester B1, 24 g of fatty acid ester C1, and 0.005 g of fatty acid metal salt D1 were taken, heated to 90°C to melt and mix uniformly, cooled, solidified, and then pulverized to obtain wax composition 1.

[0060] [Examples 2 to 12] Wax compositions 2 to 12 were obtained in the same manner as wax composition 1, except that fatty acid ester A, fatty acid ester B, fatty acid ester C, and fatty acid metal salt D were changed to the combinations and contents shown in Table 5. The content of fatty acid metal salt D shown in Table 5 is the mass of fatty acid metal salt D when the total amount of fatty acid esters A, B, and C is taken as 100 parts by mass.

[0061] [Table 5]

[0062] [evaluation] Wax compositions 1 to 12 obtained in each of the Examples and Comparative Examples were evaluated as follows. The following evaluations were made simply to evaluate the performance of the toner containing the wax composition. The evaluation results are shown in Table 6.

[0063] (1) Scratch resistance (1)-1. Preparation of resin composition A mixture of 77.6 parts by mass of polyester resin (product name: Diaclone FC-1565, manufactured by Mitsubishi Chemical Corporation) and 2.4 parts by mass of the wax composition was melt-kneaded using a twin-screw kneader (product name: Labo Plastomill (registered trademark), model: 4C150-01, manufactured by Toyo Seiki Seisakusho Co., Ltd.) at a temperature of 130°C, a rotation speed of 80 rpm, and a kneading time of 5 minutes to produce a resin composition (kneaded product).

[0064] (1)-2. Preparation of resin powder The obtained resin composition (kneaded product) was pulverized in a mixer and then passed through a sieve with 100 μm openings to obtain a resin powder.

[0065] (1)-3. Preparation of resin pellets for evaluation 3 g of the obtained resin powder was molded using a tablet molding machine under conditions of a load of 10 t and a molding time of 60 seconds to prepare resin pellets for evaluation having a diameter of 25 mm and a thickness of 5 mm.

[0066] (1)-4. Evaluation of abrasion resistance The resin pellets for evaluation prepared above were heated for 5 seconds on a hot plate heated to 160° C. under a load of 500 g, and then cooled to room temperature. A friction test was performed on the heated surface using a Bowden tester under the following test conditions. (Test conditions) Steel ball: diameter 3mm, load: 500g, speed: 10mm / s, measurement distance: 10mm, number of times: 1000 times After the friction test, the abrasion depth of the pellet surface was measured using a contact type film thickness meter, and the abrasion resistance was evaluated based on the abrasion depth. The evaluation criteria were as follows: (Evaluation Criteria) ◎: Wear depth is less than 15μm ○: Wear depth is 15 μm or more and less than 50 μm △: Wear depth is 50μm or more and less than 150μm ×: Wear depth is 150 μm or more

[0067] (2) Low-temperature fixability (2)-1. Preparation of resin pellets for evaluation Resin pellets for evaluation were prepared by the same procedures as those described above in "(1)-1. Preparation of resin composition," "(1)-2. Preparation of resin powder," and "(1)-3. Preparation of resin pellets for evaluation."

[0068] (2)-2. Evaluation of low-temperature fixability The tack strength of the resin pellets for evaluation was measured using a tack tester under the following test conditions. Specifically, the tack strength was determined as the force applied when a probe was pressed against the resin pellets with the following load, held for a predetermined time, and then peeled off. (Test conditions) Probe: Metal probe with Teflon (registered trademark) sticker attached to the contact surface, Probe temperature: 130°C, Press time: 0.05 seconds, Load: 20N The smaller the tackiness of the resin pellets at 130° C., the more excellent the low-temperature fixability. The evaluation criteria are as follows. (Evaluation Criteria) ◎: Tack strength less than 250gf ○: Tack strength is 250gf or more and less than 350gf △: Tack strength is 350gf or more and less than 500gf ×: Tack strength is 500gf or more

[0069] (3) Color development (3)-1. Preparation of colorant-containing resin composition A mixture of 96 parts by mass of polyester resin (product name: Diaclone FC-1565, manufactured by Mitsubishi Chemical Corporation), 3 parts by mass of the wax composition, and 1 part by mass of a colorant (product name: PV-FAST BLUE BG, manufactured by Clariant) was melt-kneaded using a twin-screw kneader (product name: Labo Plastomill (registered trademark), manufactured by Toyo Seiki Seisakusho Co., Ltd.) at a temperature of 130°C, a rotation speed of 80 rpm, and a kneading time of 5 minutes to obtain a colorant-containing resin composition (kneaded product). (3)-2. Preparation of evaluation samples The obtained colorant-containing resin composition (kneaded product) was molded into a smooth plate (100 mm×100 mm) by a heat press machine to prepare an evaluation sample.

[0070] (3)-3. Preparation of blank samples A colorant-containing resin composition was prepared in the same manner as in the above "(3)-1. Preparation of colorant-containing resin composition" except that the amount of polyester resin was 99 parts by mass, the amount of colorant was 1 part by mass, and no wax composition was added. Using the obtained colorant-containing resin composition, a smooth plate-shaped molded body was prepared as a blank sample in the same manner as the above "(3)-2. Preparation of evaluation sample".

[0071] (3)-4. Evaluation of color development The surfaces of the evaluation samples were measured in reflection mode using a color difference meter (ZE6000, manufactured by Nippon Denshoku Industries Co., Ltd.) to obtain the a* and b* values ​​for each hue in the CIE1976 (L*, a*, b*) color space (known as CIELAB). The chroma C of the evaluation sample was calculated using the obtained measurements using the following formula. C={(a*) 2 +(b*) 2} 1 / 2 The blank sample was also measured in the same manner using a color difference meter, and the chroma C of the blank sample was blank asked for. The color development improvement rate Kc is calculated by dividing the chroma C of the evaluation sample by the chroma C of the blank sample. blank The color development improvement rate Kc was calculated by the following formula: The larger the value of the color development improvement rate Kc calculated in this way, the more excellent the color development improvement effect. Kc=C / C blank

[0072] (4) Blocking resistance after exposure to high temperature and humidity (4)-1. Preparation of resin powder for evaluation A resin powder was prepared by the same procedures as those described in "(1)-1. Preparation of resin composition" and "(1)-2. Preparation of resin powder" above, and used as the resin powder for evaluation.

[0073] (4)-2. Evaluation of blocking resistance 10 g of the resin powder for evaluation was placed in a glass vial and left for 72 hours under high temperature and high humidity conditions of 40°C and 90% RH. The vial was turned upside down and the resin powder for evaluation was taken out without applying force. The mass X of the resin powder for evaluation that flowed out without being deposited in the vial and had a particle size of 100 μm or less was measured. The blocking resistance was calculated from the mass X using the following formula to evaluate the blocking resistance. The evaluation criteria are as follows. Blocking resistance rate (%) = {X(g) / 10(g)} x 100 (Evaluation Criteria) ◎: Blocking resistance rate is 95% or more ○: Blocking resistance rate is 80% or more and less than 95% △: Blocking resistance rate is over 70% and less than 80% ×: Blocking resistance rate is 70% or less

[0074] (5) Scratch resistance after being left at high temperature and high humidity (5)-1. Preparation of resin pellets for evaluation after exposure to high temperature and humidity A resin powder was obtained by the same procedures as those in "(1)-1. Preparation of resin composition" and "(1)-2. Preparation of resin powder" above, and the obtained resin powder was left for 72 hours under high temperature and high humidity conditions of 40°C and 90% RH. Using the resin powder after the leaving, resin pellets were prepared by the same procedures as those in "(1)-3. Preparation of resin pellets for evaluation" above, and these were used as resin pellets for evaluation after leaving at high temperature and high humidity.

[0075] (5)-2. Evaluation of abrasion resistance after exposure to high temperature and humidity The wear depth of the resin pellets for evaluation after exposure to high temperature and high humidity was measured in the same manner as in "(1)-4. Evaluation of abrasion resistance" above. The wear depth D1 (μm) measured in "(1)-4. Evaluation of abrasion resistance" above before exposure to high temperature and high humidity conditions and the wear depth D2 (μm) measured for the resin pellets for evaluation after exposure to high temperature and high humidity conditions were used to calculate the rate of change in wear depth according to the following formula. Rate of change (%) = (|D1-D2| / D1) x 100 The abrasion resistance after exposure to high temperature and high humidity was evaluated based on the rate of change in abrasion depth. The evaluation criteria were as follows: (Evaluation Criteria) ◎: Change in wear depth is less than 2.0% ○: The rate of change in wear depth is 2.0% or more and less than 5.0% △: Change in wear depth is 5.0% or more and less than 15.0% ×: Change in wear depth is 15.0% or more

[0076] (6) Low-temperature fixability after exposure to high temperature and humidity (6)-1. Preparation of resin pellets for evaluation after exposure to high temperature and humidity Resin pellets for evaluation after exposure to high temperature and high humidity were prepared in the same manner as in "(5)-1. Preparation of resin pellets for evaluation after exposure to high temperature and high humidity" above.

[0077] (6)-2. Evaluation of low-temperature fixability after exposure to high temperature and humidity The tack strength of the resin pellets for evaluation after storage at high temperature and high humidity was measured in the same manner as in "(2)-2. Evaluation of low temperature fixing property" above. The rate of change in tack strength was calculated from the following formula using the tack strength T1 (gf) measured in "(2)-2. Evaluation of low temperature fixing property" above before storage under high temperature and high humidity conditions and the tack strength T2 (gf) measured for the resin pellets for evaluation after storage at high temperature and high humidity. Rate of change (%) = (|T1-T2| / T1) x 100 The low-temperature fixability after being left at high temperature and high humidity was evaluated based on the rate of change in tack strength. The evaluation criteria were as follows. (Evaluation Criteria) ◎: Change in tack strength is less than 2.0% ○: The rate of change in tack strength is 2.0% or more and less than 5.0% △: The rate of change in tack strength is 5.0% or more and less than 15.0% ×: The rate of change in tack strength is 15.0% or more

[0078] (7) Color development after exposure to high temperature and humidity (7)-1. Preparation of evaluation samples after exposure to high temperature and humidity A colorant-containing resin composition (kneaded product) was obtained by the same procedure as in "(3)-1. Preparation of colorant-containing resin composition" above, and the obtained colorant-containing resin composition (kneaded product) was left for 72 hours under high temperature and high humidity conditions of 40°C and 90% RH. The colorant-containing resin composition (kneaded product) after the leaving was molded into a smooth plate (100 mm x 100 mm) by the same procedure as in "(3)-2. Preparation of evaluation sample" above, and used as an evaluation sample after leaving at high temperature and high humidity.

[0079] (7)-2. Evaluation of color development after exposure to high temperature and humidity After storing the sample in a high-temperature, high-humidity environment, the chroma C of the sample was measured using the method described in "(3)-4. Evaluation of color development" above. HH The chroma C of the evaluation sample after exposure to high temperature and high humidity was calculated. HH , and the chroma C of the blank sample measured in "(3)-4. Evaluation of color development" above blank Using the value of , the color development improvement rate Kc after exposure to high temperature and high humidity HH was calculated using the following formula. KcHH =C HH / C blank The color development improvement rate Kc before leaving the sample under high temperature and high humidity conditions obtained in "(3)-4. Evaluation of color development" above and the color development improvement rate Kc after leaving the sample under high temperature and high humidity conditions HH Using these values, the rate of change in the color development improvement rate was calculated according to the following formula. Rate of change (%) = (|Kc - Kc HH | / Kc)×100 The color development after standing at high temperature and high humidity was evaluated based on the rate of change in the color development improvement rate. The evaluation criteria are as follows. (Evaluation Criteria) ◎: The change in color development improvement rate is less than 2.0% ○: The change rate of the color development improvement rate is 2.0% or more and less than 5.0% △: The change rate of the color development improvement rate is 5.0% or more and less than 15.0% ×: The change in color development improvement rate is 15.0% or more

[0080] [Table 6]

[0081] In Table 6, the values ​​in parentheses are the measured or calculated values ​​obtained in the above evaluations (1) to (7). Wax compositions 1 to 7 in Examples 1 to 7 contained the above-mentioned fatty acid ester A, fatty acid ester B, and fatty acid ester C, and when the total of fatty acid esters A, B, and C was taken as 100 mass%, the content of fatty acid ester A was 5 to 50 mass%, the content of fatty acid ester B was 20 to 90 mass%, and the content of fatty acid ester C was 1 to 50 mass%, the mass ratio of fatty acid ester A to the total of fatty acid ester B and fatty acid ester C was 5:95 to 50:50, the mass ratio of fatty acid ester B to fatty acid ester C was 95:5 to 50:50, and the content of the above-mentioned fatty acid metal salt D was 0 to 1 part by mass relative to 100 parts by mass of the total of fatty acid esters A, B, and C, i.e., they were toner wax compositions of the present invention. According to the results of the above evaluation, when wax compositions 1 to 7 of Examples 1 to 7 were used, the abrasion resistance, low-temperature fixability, and color development were excellent, and the blocking resistance when stored under high temperature and high humidity conditions was excellent. Even after exposure to high temperature and high humidity conditions, the deterioration of the abrasion resistance, low temperature fixability, and color development was suppressed. On the other hand, the wax composition 8 of Comparative Example 1 did not contain the fatty acid ester C. When the wax composition 8 of Comparative Example 1 was used, the abrasion resistance and color development were poor, and after exposure to high temperature and high humidity conditions, the abrasion resistance, low temperature fixability, and color development were deteriorated. In the wax composition 9 of Comparative Example 2, the content of fatty acid metal salt D exceeded 1 part by mass per 100 parts by mass of the total of fatty acid ester A, fatty acid ester B, and fatty acid ester C. When the wax composition 9 of Comparative Example 2 was used, the abrasion resistance, low-temperature fixability, and color development were poor, and the abrasion resistance, low-temperature fixability, and color development were deteriorated after exposure to high-temperature and high-humidity conditions. In the wax composition 10 of Comparative Example 3, the carbon number of the alcohol used in the fatty acid ester A was less than 12, and the carbon number of the fatty acid used in the fatty acid ester B and the fatty acid used in the fatty acid ester C were all less than 12. In the wax composition 11 of Comparative Example 4, the mass ratio of the fatty acid ester A to the total of the fatty acid ester B and the fatty acid ester C was 60:40, the content of the fatty acid ester A was high at 60 mass%, and the mass ratio of the fatty acid ester B to the fatty acid ester C was 40:60, and the content of the fatty acid ester B was low at 16 mass%. In the wax composition 12 of Comparative Example 5, the fatty acid ester A was not included, the mass ratio of the fatty acid ester B to the fatty acid ester C was 40:60, and the content of the fatty acid ester C was high at 60 mass%. When wax composition 10 of Comparative Example 3, wax composition 11 of Comparative Example 4, or wax composition 12 of Comparative Example 5 was used, the abrasion resistance, low-temperature fixability, and color development were poor, and the blocking resistance when stored under high-temperature and high-humidity conditions was also poor. After exposure to high-temperature and high-humidity conditions, the abrasion resistance, low-temperature fixability, and color development were deteriorated.

Claims

[Claim 1] comprising fatty acid ester A, fatty acid ester B, and fatty acid ester C; The fatty acid ester A is a diester compound of a divalent linear saturated fatty acid having 10 to 30 carbon atoms and a monovalent linear saturated alcohol having 12 to 24 carbon atoms, The fatty acid ester B is a monoester compound of a monovalent linear saturated fatty acid having an even number of carbon atoms of 10 to 30 and a monovalent linear saturated alcohol having a carbon number of 12 to 24, the fatty acid ester C is a monoester compound of a monovalent linear saturated fatty acid having an odd carbon number of 11 to 29 and a monovalent linear saturated alcohol having a carbon number of 12 to 24, When the total amount of the fatty acid ester A, the fatty acid ester B, and the fatty acid ester C is taken as 100% by mass, the content of the fatty acid ester A is 5 to 50% by mass, the content of the fatty acid ester B is 20 to 90% by mass, and the content of the fatty acid ester C is 1 to 50% by mass, a mass ratio of the fatty acid ester A to the total of the fatty acid ester B and the fatty acid ester C (fatty acid ester A:total of fatty acid ester B and fatty acid ester C) is 5:95 to 50:50; a mass ratio of the fatty acid ester B to the fatty acid ester C (fatty acid ester B:fatty acid ester C) is 95:5 to 50:50; a content of fatty acid metal salt D is 0 to 1 part by mass relative to a total of 100 parts by mass of fatty acid ester A, fatty acid ester B, and fatty acid ester C, and fatty acid metal salt D is a salt of a monovalent linear saturated fatty acid having 10 to 30 carbon atoms and at least one metal selected from the group consisting of sodium, potassium, and calcium.

Citation Information

Patent Citations

  • Electrostatic charge image developing toner and image forming method

    JP2005157039A

  • Toner wax composition for polyester resin

    JP2010122425A

  • Wax for toner

    JP2021196608A

  • Toner, toner cartridge, and image forming apparatus

    JP2022043977A