Electric heating type catalyst device

The EHC enhances catalyst activation and purification performance by using a SiC-based base material with strategically positioned Pd and Rh catalyst layers, addressing temperature raising and purification inefficiencies in conventional designs.

JP2024161995AInactive Publication Date: 2024-11-21TOYOTA JIDOSHA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023077111
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-21
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional electrically heated catalyst devices (EHCs) lack sufficient temperature raising properties and exhaust gas purification performance when catalyst temperature is increased by electrical heating, and there is a risk of insufficient purification performance due to inadequate design configurations.

Method used

The EHC includes a base material containing SiC, an inflow side catalyst layer with Pd and CeO2/ZrO2 OSC material, and an outflow side catalyst layer with Rh, both supported on a partition wall structure with specific coating amounts and overlapping regions to enhance catalyst activation and purification performance.

Benefits of technology

The EHC improves exhaust gas purification performance and reduces pressure loss by optimizing catalyst layer distribution and coating amounts, ensuring effective catalyst activation even at low exhaust gas temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161995000001_ABST
    Figure 2024161995000001_ABST
Patent Text Reader

Abstract

To provide an electric heating type catalyst device capable of improving purification performance when the temperature is raised by electric heating.SOLUTION: An electric heating type catalyst device includes a base material, an inflow side catalyst layer, and an outflow side catalyst layer. The base material contains SiC, the inflow side catalyst layer contains Pd, and the outflow side catalyst layer contains Rh. The base material includes a bulkhead defining a plurality of cells extending from an inflow side end surface to an outflow side end surface. The inflow side catalyst layer is provided on the surface of the bulkhead in an inflow side catalyst region extending by a distance exceeding 50% of the entire length in an extension direction of the bulkhead from the inflow side end to the outflow side of the bulkhead. The outflow side catalyst layer is provided on the surface of the bulkhead of a part that is not overlapped with the inflow side catalyst region, and on the surface of the inflow side catalyst layer of a part that is overlapped with the inflow side catalyst region in the outflow side catalyst region extending by a distance exceeding 50% of the entire length in the extension direction of the bulkhead from the outflow side end to the inflow side of the bulkhead. A total coat amount obtained by dividing the total mass of the inflow side catalyst layer and the outflow side catalyst layer by the cubic volume of the base material is 138 g / L or more and 150 g / L or less.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrically heated catalyst device used to purify exhaust gas from an internal combustion engine. [Background technology]

[0002] In recent years, electrically heated catalytic converters (hereinafter sometimes abbreviated as "EHC") have been attracting attention as exhaust gas purification devices that purify exhaust gas from internal combustion engines of vehicles (automobiles) and the like. In order for an exhaust gas purification device to exhibit sufficient purification performance, the temperature of the catalyst used in the exhaust gas purification device must be raised to an activation temperature. In a typical exhaust gas purification device, the catalyst is heated using the heat of the exhaust gas, so high purification performance cannot be obtained when the temperature of the exhaust gas is low, such as immediately after the internal combustion engine starts operating. In contrast, with an EHC, even when the temperature of the exhaust gas is low, such as immediately after the internal combustion engine starts operating, the catalyst temperature can be raised by electrical heating to activate the catalyst. Therefore, even when the temperature of the exhaust gas is low, high purification performance can be obtained, and the purification efficiency of the exhaust gas can be improved.

[0003] A typical configuration of an EHC includes a substrate and a catalyst layer, the substrate containing SiC that functions as a resistive heating element, and the catalyst layer containing a platinum group metal as a catalytic component. For example, an EHC described in Patent Document 1 is known as a conventional EHC. This EHC includes a substrate, a catalyst layer, an intermediate layer disposed between the substrate and the catalyst layer, and an electrode, the substrate containing SiC, the catalyst layer containing a platinum group metal as a catalytic component, the intermediate layer containing substantially no platinum group metal, and the thickness [μm] and specific surface area [m 2 / g] is 1100 or more. With this EHC, the intermediate layer has an appropriate thickness and an appropriate specific surface area, and therefore exhibits a high function as a physical barrier that prevents the migration of platinum group metals. This makes it possible to suppress the migration of platinum group metals from the catalyst layer to the substrate, and improves the high-temperature durability of the EHC. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2021-104484 A Summary of the Invention [Problem to be solved by the invention]

[0005] In various conventional EHC configurations, such as the configuration described in Patent Document 1 that has an intermediate layer disposed between the substrate and catalyst layer, the catalyst does not have sufficient temperature rise capability (warm-up characteristics) due to electrical heating, so there is a risk that the exhaust gas purification performance will be insufficient when the catalyst is heated by electrical heating.

[0006] The present invention has been made in consideration of these points, and its purpose is to provide an electrically heated catalyst device (EHC) that can improve exhaust gas purification performance when the catalyst is heated by electrical heating. [Means for solving the problem]

[0007] In order to solve the above problems, the electrically heated catalytic device of the present invention is an electrically heated catalytic device including a substrate, an inlet-side catalytic layer, and an outlet-side catalytic layer, wherein the substrate contains SiC, the inlet-side catalytic layer contains Pd as a catalytic component, and the outlet-side catalytic layer contains Rh as a catalytic component, the substrate has partition walls defining a plurality of cells extending from an inlet-side end face to an outlet-side end face, the inlet-side catalytic layer has an inlet-side partition wall extending from an inlet-side end of the partition wall to an outlet side along an extension direction for a distance exceeding 50% of the total length in the extension direction of the partition wall. In the catalyst region, the outlet-side catalyst layer is provided on a surface of the partition wall, and is provided on a surface of the partition wall in a portion not overlapping with the inlet-side catalyst region and on a surface of the inlet-side catalyst layer in a portion overlapping with the inlet-side catalyst region, in an outlet-side catalyst region extending from the outlet-side end of the partition wall along the extension direction by a distance exceeding 50% of the entire length of the extension direction of the partition wall, and is characterized in that a total coat amount obtained by dividing the total mass of the inlet-side catalyst layer and the outlet-side catalyst layer by the volume of the base is 138 g / L or more and 150 g / L or less. Effect of the Invention

[0008] According to the electrically heated catalyst device of the present invention, it is possible to improve the exhaust gas purification performance when the temperature of the catalyst is increased by electrical heating. [Brief description of the drawings]

[0009] [Figure 1] 1 is a cross-sectional view that shows a schematic diagram of a catalytic converter equipped with an EHC according to a first embodiment. [Diagram 2] FIG. 2 is a perspective view showing a schematic configuration of an EHC according to the first embodiment. [Diagram 3] 2 is a cross-sectional view that illustrates a schematic view of a main part of a cross section parallel to an extension direction of a partition wall in the EHC according to the first embodiment. FIG. [Figure 4] 1 is a graph showing the change in the amount of NMOG (Non-Methane Organic Gases) emitted versus the total coating amount of the inlet-side catalyst layer and the outlet-side catalyst layer obtained from EHCs of Examples and Comparative Examples. [Diagram 5] 1 is a graph showing the change in maximum oxygen storage amount versus the total coating amount of the inlet-side catalyst layer and the outlet-side catalyst layer obtained from EHCs of Examples and Comparative Examples. [Figure 6] 1 is a graph showing the change in pressure loss versus the total coating amount of the inlet-side catalyst layer and the outlet-side catalyst layer obtained from EHCs of Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the electrically heated catalytic converter (hereinafter sometimes abbreviated as "EHC") of the present invention will be described. In the following description, "inlet side" and "outlet side" refer to the side into which exhaust gas flows and the side from which exhaust gas flows, respectively, in each element. "Upstream side" and "downstream side" refer to the upstream side and downstream side in the direction in which exhaust gas flows, respectively. "Extending direction" refers to the extending direction of the partition wall (the direction in which the partition wall extends), which is approximately the same as the axial direction of the substrate and the extending direction of the cell (the direction in which the cell extends). "Thickness direction" refers to the thickness direction of the partition wall (the direction perpendicular to the surface of the partition wall on the cell side). "Width direction" refers to the width direction of the partition wall (the direction perpendicular to both the extending direction and the thickness direction of the partition wall).

[0011] First, the outline of the EHC according to the embodiment will be described by taking the EHC according to the first embodiment as an example. Fig. 1 is a cross-sectional view that shows a catalytic converter including the EHC according to the first embodiment. Fig. 2 is a perspective view that shows an EHC according to the first embodiment. Fig. 3 is a cross-sectional view that shows a main part of the EHC according to the first embodiment in a cross section parallel to the extension direction of the partition walls.

[0012] The catalytic converter 100 shown in FIG. 1 is installed in an exhaust passage (not shown) of an internal combustion engine (gasoline engine) mounted on a hybrid vehicle (automobile). The catalytic converter 100 is a tandem type catalytic converter including a first exhaust gas purification device 61, which is an EHC 1 according to the first embodiment, and a second exhaust gas purification device 62. The catalytic converter 100 further includes a case 60 having a cylindrical inner pipe 60n, an inlet side connecting pipe 60a, and an outlet side connecting pipe 60b, a mat 64, and an insulator 66. The inner pipe 60n, the inlet side connecting pipe 60a, and the outlet side connecting pipe 60b of the case 60 are made of a metal such as stainless steel. The inlet side connecting pipe 60a is fixed to the inlet side of the inner pipe 60n from the outside, and the diameter of the inlet side becomes smaller. The outlet side connecting pipe 60b is fixed to the outlet side of the inner pipe 60n from the outside, and the diameter of the outlet side becomes smaller. The case 60 constitutes a part of the exhaust passage.

[0013] The first exhaust gas purification device 61 and the second exhaust gas purification device 62 are housed in an inner pipe 60n of the case 60. The first exhaust gas purification device 61 is disposed upstream of the second exhaust gas purification device 62. In the inner pipe 60n of the case 60, a mat 64 is interposed between the first exhaust gas purification device 61 and the second exhaust gas purification device 62 and the inner peripheral surface of the inner pipe 60n of the case 60. The mat 64 is an insulator and is formed, for example, from inorganic fibers mainly composed of alumina. An insulating coating is provided on the inner peripheral surface of the inner pipe 60n of the case 60 by applying an insulating material. For example, a glass coating or the like is used as the insulating coating.

[0014] The inlet connecting pipe 60a of the case 60 connects the inner pipe 60n to the upstream exhaust pipe 51, which has a smaller diameter than the inner pipe 60n of the case 60. The inlet side of the inner pipe 60n of the case 60 has a smaller diameter as it approaches the upstream exhaust pipe 51, and the diameter of the part closest to the upstream exhaust pipe 51 is approximately equal to the diameter of the upstream exhaust pipe 51. The outlet connecting pipe 60b of the case 60 connects the inner pipe 60n to the downstream exhaust pipe 52, which has a smaller diameter than the inner pipe 60n of the case 60. The upstream exhaust pipe 51 and the downstream exhaust pipe 52 each form a part of the exhaust passage.

[0015] The first exhaust gas purification device 61 is a straight-flow type three-way catalyst, which is the EHC 1 according to the first embodiment. As shown in Figures 1 to 3, the EHC 1 according to the first embodiment is a straight-flow type three-way catalyst, and includes a substrate 10, an inlet side catalyst layer 20, an outlet side catalyst layer 30, a positive electrode 40a, and a negative electrode 40b.

[0016] The substrate 10 is a member that supports the inlet-side catalyst layer 20 and the outlet-side catalyst layer 30. The substrate 10 contains a Si-SiC composite material. The substrate 10 is a substrate in which a frame portion 11 and a partition wall 14 that divides the space inside the frame portion 11 are integrally formed. The outer shape of the frame portion 11 is cylindrical. The partition wall 14 is a porous body that defines a plurality of cells 12 extending from the inlet-side end face 10Sa to the outlet-side end face 10Sb of the substrate 10. The shape of the partition wall 14 includes a plurality of wall portions 14A that are arranged parallel to each other and spaced apart from each other, and a plurality of wall portions 14B that are perpendicular to the plurality of wall portions 14A and arranged parallel to each other and spaced apart from each other, so that the cross-sectional shape perpendicular to the extension direction of the plurality of cells 12 is rectangular, and the cross section perpendicular to the extension direction is lattice-shaped. The plurality of cells 12 are adjacent to each other across the partition wall 14, and both the inlet-side end 12a and the outlet-side end 12b are open.

[0017] The inlet-side catalyst layer 20 contains a catalyst component Pd (palladium), a carrier containing an OSC material, which is a composite oxide mainly composed of CeO2 and ZrO2, and an oxide other than the OSC material, and a Ba compound (e.g., BaSO4). The catalyst component and the Ba compound are supported on a carrier containing an OSC material and an oxide other than the OSC material. The inlet-side catalyst layer 20 is provided on a cell-side surface 14s of the partition wall 14 in an inlet-side catalyst region 14X that extends from an inlet-side end 14a of the partition wall 14 along the extension direction to a position 14c away from the inlet-side end 14a of the partition wall 14 on the outlet side at a distance exceeding 50% of the entire length of the partition wall 14 in the extension direction.

[0018] The outflow side catalyst layer 30 contains a catalyst component Rh (rhodium) and a carrier containing an OSC material and an oxide other than the OSC material. The catalyst component is supported on a carrier containing an OSC material and an oxide other than the OSC material. The outflow side catalyst layer 30 is provided on the cell side surface 14s of the partition wall 14 in a portion that does not overlap with the inflow side catalyst region 14X, and on the surface 20s of the inflow side catalyst layer 20 in a portion that overlaps with the inflow side catalyst region 14X, in the outflow side catalyst region 14Y that extends from the outflow side end 14b of the partition wall 14 along the extension direction to a position 14d away from the inflow side by a distance exceeding 50% of the total length in the extension direction of the partition wall 14.

[0019] A part 30p of the inlet side of the outlet side catalyst layer 30 overlaps with the inlet side catalyst layer 20. The total coating amount obtained by dividing the total mass of the inlet side catalyst layer 20 and the outlet side catalyst layer 30 by the volume of the substrate 10 (hereinafter, sometimes abbreviated as "the total coating amount of the inlet side catalyst layer 20 and the outlet side catalyst layer 30") is 138 g / L or more and 150 g / L or less.

[0020] The positive electrode 40a and the negative electrode 40b are attached to the outer peripheral surface 11s of the frame 11 of the substrate 10. The positive electrode 40a has a positive electrode layer 42a provided on the outer peripheral surface 11s of the frame 11 and a positive electrode terminal 44a connected to the positive electrode layer 42a. The negative electrode 40b has a negative electrode layer 42b provided on the outer peripheral surface 11s of the frame 11 of the substrate 10 and a negative electrode terminal 44b connected to the negative electrode layer 42b. The positive electrode layer 42a and the negative electrode layer 42b extend in the circumferential and axial directions along the outer peripheral surface 11s of the frame 11 so that a current can flow uniformly throughout the substrate 10. The positive electrode terminal 44a and the negative electrode terminal 44b each penetrate the wall of the inner tube 60n of the case 60. Insulators 66 are fitted between the positive electrode terminal 44a and the negative electrode terminal 44b and the wall of the inner tube 60n of the case 60. The insulators 66 are made of an insulating material such as alumina. This electrically insulates the EHC 1 from the case 60. In the EHC 1, a voltage is applied between the positive electrode 40a and the negative electrode 40b to pass a current through the substrate 10, causing the substrate 10 to generate heat through electrical resistance.

[0021] As shown in FIG. 1, the second exhaust gas purification device 62 is a straight-flow type three-way catalyst, and includes a substrate 70 and a catalyst layer (not shown). The substrate 70 is a member that supports the catalyst layer. The substrate 70 contains cordierite. The substrate 70 is a substrate in which a frame (not shown) and a partition wall (not shown) that separates the space inside the frame are integrally formed. The outer shape of the frame is cylindrical. The partition wall is a porous body that defines a plurality of cells (not shown) that extend from the inlet side end face to the outlet side end face of the substrate 70. The plurality of cells are adjacent to each other with the partition wall sandwiched therebetween, and both the inlet side end and the outlet side end are open. The catalyst layer is provided on the cell side surface of the partition wall. The catalyst layer contains catalytic components Pd and Rh, a carrier containing an OSC material and an oxide other than the OSC material, and a Ba compound (for example, BaSO4). The catalyst component and the Ba compound are supported on a carrier containing an OSC material and an oxide other than the OSC material.

[0022] When exhaust gas passes through the catalytic converter 100 during operation of the internal combustion engine, the exhaust gas first flows into the cells 12 of the EHC1 (first exhaust gas purification device 61) according to the first embodiment from the inlet end 12a and flows out of the cells 12 from the outlet end 12b. The exhaust gas then flows into the cells of the second exhaust gas purification device 62 from the inlet end and flows out of the cells from the outlet end. In the catalytic converter 100, before the internal combustion engine starts to operate, a voltage is applied between the positive electrode 40a and the negative electrode 40b of the EHC1 to pass a current through the substrate 10, thereby allowing the substrate 10 to generate heat through electrical resistance. This allows the catalyst temperature of the EHC1 to be increased and the catalyst to be activated, even if the temperature of the exhaust gas is low immediately after the internal combustion engine starts to operate. Furthermore, the heat of the exhaust gas heated by passing through the EHC1 can also be used to increase the temperature of the catalyst of the second exhaust gas purification device 62 and activate the catalyst.

[0023] According to the EHC1 of the first embodiment, a portion 30p of the inlet side of the outlet catalytic layer 30 overlaps with the inlet catalytic layer 20, so that the barrier effect of the inlet catalytic layer 20 prevents Si in the substrate 10 from diffusing to the outlet catalytic layer 30 containing Rh, a catalytic component that contributes greatly to purification performance. This makes it possible to suppress deterioration of the outlet catalytic layer 30 and improve purification performance. In addition, since the total coating amount of the inlet catalytic layer 20 and the outlet catalytic layer 30 is 138 g / L or more, the OSC characteristics are improved, and purification performance can be effectively improved.

[0024] Furthermore, according to EHC1, the total coating amount of the inlet-side catalyst layer 20 and the outlet-side catalyst layer 30 is 150 g / L or less, which improves the temperature rise (warm-up characteristics) of the catalyst by electric heating, thereby improving the exhaust gas purification performance when the catalyst is heated by electric heating. Also, the total coating amount of the inlet-side catalyst layer 20 and the outlet-side catalyst layer 30 is 150 g / L or less, which makes these layers thinner, thereby reducing pressure loss. In addition, since the substrate 10 contains a Si-SiC composite material, the partition walls are thicker and the air holes of the partition walls are narrower than, for example, a normal substrate containing cordierite. Therefore, the pressure loss is greatly reduced.

[0025] Therefore, according to the EHC according to the embodiment, for example, like the EHC1 according to the first embodiment, it is possible to improve the exhaust gas purification performance when the temperature of the catalyst is raised by electrical heating. Furthermore, it is possible to reduce the pressure loss. Next, the details of each component of the EHC according to the embodiment will be described.

[0026] 1. Base material The substrate contains silicon carbide (SiC) and has partition walls that define a plurality of cells extending from an inlet end face to an outlet end face.

[0027] By containing SiC, the substrate is less susceptible to cracking due to thermal cycles and can function as a resistance heating element. Therefore, by containing SiC in the substrate, the EHC according to the embodiment can be used as an electrically heated catalytic device. The substrate may be, for example, a substrate containing SiC as a pure substance, or a substrate containing a Si-SiC (silicon-silicon carbide) composite material in which Si is bonded to SiC, but a substrate containing a Si-SiC composite material is preferred. This is because excellent electrical conductivity can be obtained.

[0028] The substrate is usually a substrate in which a frame and a partition wall that divides the space inside the frame are integrally formed. The outer shape of the substrate (outer shape of the frame) is not particularly limited, and may be, for example, cylindrical. When the outer shape of the substrate is cylindrical, the outer diameter of the substrate (outer diameter of the frame) is not particularly limited and may be the same as that of a known EHC, but is preferably, for example, 75 mm or more and 95 mm or less. When the outer diameter is equal to or more than the lower limit, an increase in pressure loss can be avoided, and when the outer diameter is equal to or less than the upper limit, a radial temperature distribution difference during electrical heating can be suppressed. The axial length of the substrate is not particularly limited and may be the same as that of a known EHC, but when the EHC is used in a tandem-type catalytic converter as in the first embodiment, the axial length of the substrate is preferably 45 mm or more and 70 mm or less. When the length is equal to or more than the lower limit, purification characteristics can be ensured, and when the length is equal to or less than the upper limit, pressure loss can be reduced.

[0029] The shape of the partition wall is not particularly limited and may be the same as that of a known EHC, but usually includes a plurality of wall parts arranged parallel to each other and spaced apart from each other, and a plurality of wall parts intersecting the plurality of wall parts and arranged parallel to each other and spaced apart from each other, so that the cross-sectional shape perpendicular to the extension direction of the plurality of cells is a desired shape. The length of the partition wall in the extension direction is not particularly limited, but is usually approximately the same as the axial length of the substrate. The thickness of the partition wall is not particularly limited and may be the same as that of a known EHC, but is preferably, for example, 85 μm or more and 210 μm or less. When the thickness is the lower limit or more, the effect of reducing pressure loss due to the coat width of the inlet side catalyst layer and the outlet side catalyst layer being 60% or more is remarkable, and structural reliability can be ensured, and when the thickness is the upper limit or less, unnecessary increase in pressure loss can be avoided.

[0030] The partition walls are porous. The porosity of the partition walls is not particularly limited and may be the same as that of known EHC, but is preferably, for example, 35% to 45%. When the porosity is the lower limit or more, unnecessary increase in pressure loss can be avoided, and when the porosity is the upper limit or less, the effect of reducing pressure loss due to the inlet-side catalyst layer and the outlet-side catalyst layer having a coat width of 60% or more is remarkable. The average pore diameter of the partition walls is not particularly limited and may be the same as that of known EHC, but is preferably, for example, 4 μm to 11 μm. When the average pore diameter is the lower limit or more, unnecessary increase in pressure loss can be avoided, and when the average pore diameter is the upper limit or less, the effect of reducing pressure loss due to the inlet-side catalyst layer and the outlet-side catalyst layer having a coat width of 60% or more is remarkable. The "average pore diameter of the partition walls" refers to, for example, that measured by mercury intrusion porosimetry.

[0031] The cross-sectional shape perpendicular to the stretching direction of the multiple cells is not particularly limited and may be the same as that of known EHCs, for example, a polygon such as a rectangle, a circle, etc. The cell density is not particularly limited and may be the same as that of known EHCs, for example, 350 to 700 cells per square inch is preferable. When the cell density is equal to or higher than the lower limit, contact with the exhaust gas is increased and purification properties can be ensured, and when the cell density is equal to or lower than the upper limit, an increase in pressure loss can be avoided. The length of the multiple cells in the stretching direction is not particularly limited, but is usually approximately the same as the axial length of the substrate.

[0032] 2.Inlet side catalyst layer The inlet-side catalyst layer contains Pd as a catalyst component. Pd has excellent exhaust gas purification performance for CO and HC. The inlet-side catalyst layer is provided on the surface of the partition wall in an inlet-side catalyst region extending from the inlet-side end of the partition wall along the extension direction to the outlet side by a distance exceeding 50% of the total length of the partition wall in the extension direction. The inlet-side catalyst region is not particularly limited as long as it is a region extending from the inlet-side end of the partition wall to the outlet side by a distance exceeding 50% and not exceeding 100% of the total length of the partition wall in the extension direction, but among them, a region extending from the inlet-side end of the partition wall to the outlet side by a distance of 60% to 90% of the total length of the partition wall in the extension direction is preferred. This is because the purification performance can be further improved.

[0033] Pd is preferably in the form of fine particles in order to increase the contact area with exhaust gas. The average particle size of the fine particle Pd is preferably, for example, 1 nm or more and 15 nm or less. The average particle size of Pd can be obtained by acquiring an electron microscope image (e.g., a TEM image, etc.) of Pd and calculating the average particle size of any 20 or more particles in the image.

[0034] The inlet side catalyst layer usually contains an OSC material (oxygen storage material). The OSC material is not particularly limited as long as it has oxygen storage capacity, and examples thereof include CeO2 and composite oxides containing CeO2. Examples of composite oxides containing CeO2 include ceria-zirconia composite oxides containing CeO2 and ZrO2. Among them, ceria-zirconia composite oxides are preferable as the OSC material. This is because ZrO2 can suppress the thermal deterioration of CeO2. The ceria-zirconia composite oxide may be a ceria-zirconia composite oxide made of CeO2 and ZrO2, or may contain metal elements other than Ce and Zr. Among the metal elements other than Ce and Zr, rare earth elements (e.g., Sc, Y, La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, etc.) are preferable. This is because it can improve heat resistance and oxygen absorption / release properties. The CeO2 content in the composite oxide containing CeO2 is preferably, for example, 15 mass% or more and 55 mass% or less. When the content is equal to or more than the lower limit, the composite oxide can fully exhibit the oxygen storage capacity. When the content is equal to or less than the upper limit, the basicity of the OSC material can be suppressed.

[0035] The OSC material may function as a carrier for supporting Pd. The inlet-side catalyst layer may further contain a carrier other than the OSC material as a carrier for supporting Pd. Examples of the carrier other than the OSC material include a carrier containing an oxide other than the OSC material. Examples of the oxide include Al2O3, TiO2, ZrO2, SiO2, and alumina-zirconia composite oxides containing Al2O3 and ZrO2. The carrier containing an oxide other than the OSC material may further contain an oxide of a rare earth element. This is because the heat resistance and the like can be improved. Examples of the oxide of a rare earth element include Pr2O3, Nd2O3, La2O3, and Y2O3. The content of the oxide of a rare earth element in the carrier containing an oxide other than the OSC material may be, for example, 1 mass% or more and 10 mass% or less.

[0036] The Pd content in the inlet side catalyst layer is not particularly limited, but is preferably, for example, 0.01 mass % to 8 mass % based on the total mass of the OSC material and the carrier other than the OSC material contained in the inlet side catalyst layer.

[0037] The inlet side catalyst layer may further contain at least one Ba component selected from the group consisting of Ba (barium) and Ba compounds. This is because it can suppress the poisoning of Pd by HC and suppress the sintering of Pd. Examples of Ba compounds include BaSO4, (CH3COO)2Ba, Ba(NO3)2, BaCO3, etc., among which BaSO4, (CH3COO)2Ba, etc. are preferred, and BaSO4 is particularly preferred.

[0038] In general, in order to highly diffuse the Ba component in the inlet-side catalyst layer, the smaller the average particle size of the Ba component, the better. In particular, when the average particle size is several nm, the Ba component has excellent diffusibility. However, the average particle size of the Ba component is 100 nm or more and 350 nm or less. By making the average particle size of the Ba component significantly larger than several nm, the contact between the Ba element contained in the inlet-side catalyst layer and the Si contained in the base material can be reduced, and further, by making the average particle size of the Ba component 100 nm or more and 350 nm or less, the Ba element can be dispersed and present in the inlet-side catalyst layer together with Pd. Therefore, by making the average particle size of the Ba component 100 nm or more and 350 nm or less, the diffusion of Si from the base material to the inlet-side catalyst layer by the Ba element can be suppressed. This can suppress the deterioration of the OSC material, and therefore the high-temperature durability of the OSC material can be improved. The average particle size of the Ba component is preferably 150 nm or more and 200 nm or less. This is because the high-temperature durability of the OSC material can be significantly improved. Moreover, by making the average particle size of the Ba component 100 nm or more, damage to the base material can be suppressed, and the NOx purification performance can be improved.

[0039] The average particle size of the Ba component can be determined, for example, by the following method. First, a part of the inlet side catalyst layer is taken from the EHC as a sample. Next, an image of the sample is taken using, for example, an electron microscope such as SEM or TEM. Next, 20 or more particles that are entirely visible are selected from the particles of the Ba component in the taken image, and the area of ​​each selected particle is measured. Next, the diameter of a circle having an area equal to the area of ​​each selected particle is calculated. Next, the arithmetic mean of the diameters calculated for each selected particle is calculated as the average particle size of the Ba component.

[0040] The Ba component is present at least on the surface of the OSC material, and is usually supported on the OSC material. The Ba component may be supported on both the OSC material and a carrier other than the OSC material. The ratio of the Ba component supported on the OSC material is, for example, 10 mass% or more. The dispersion form of the Ba component is not particularly limited, but the inlet-side catalyst layer is usually formed by coating the surface of the partition wall with a slurry in which a catalyst component source, a Ba component source, and an OSC material are mixed, so that the Ba component is uniformly dispersed in the inlet-side catalyst layer. The content of the Ba component in the inlet-side catalyst layer is not particularly limited, but for example, the ratio of the mass of the Ba component converted into sulfate to the mass of Pd contained in the inlet-side catalyst layer is 1 / 80 or more and 20 or less.

[0041] The inlet side catalyst layer may further contain, for example, a binder, an additive, etc., in addition to Pd, Ba components, OSC material, and a carrier other than the OSC material. Examples of the binder include alumina sol and silica sol. Examples of the additive include NO x Examples of the additives include adsorbents and stabilizers.

[0042] The thickness of the inlet-side catalyst layer is not particularly limited, and may be appropriately determined depending on the size of the cells of the substrate and the flow rate of the exhaust gas supplied to the EHC. The thickness of the inlet-side catalyst layer is not particularly limited, but is preferably, for example, 1 μm or more and 500 μm or less. The coating amount obtained by dividing the mass of the inlet-side catalyst layer by the volume of the substrate is not particularly limited, but is preferably, for example, 50 g / L or more and 150 g / L or less. This is because the purification performance can be effectively improved by the coating amount being equal to or more than the lower limit. This is because the pressure loss can be effectively suppressed by the coating amount being equal to or less than the upper limit.

[0043] 3. Outlet catalyst layer The outflow side catalyst layer contains Rh as a catalyst component. Rh has excellent NOx purification performance. The outflow side catalyst layer is provided on the surface of the partition wall in a portion that does not overlap with the inflow side catalyst region and on the surface of the inflow side catalyst layer in a portion that overlaps with the inflow side catalyst region in an outflow side catalyst region that extends from the outflow side end of the partition wall along the extension direction to the inflow side by a distance exceeding 50% of the entire length in the extension direction of the partition wall. The outflow side catalyst region is not particularly limited as long as it is a region that extends from the outflow side end of the partition wall to the inflow side by a distance exceeding 50% and not exceeding 100% of the entire length in the extension direction of the partition wall, but among them, a region that extends from the outflow side end of the partition wall to the inflow side by a distance of 60% to 90% of the entire length in the extension direction of the partition wall is preferable. This is because the purification performance can be further improved.

[0044] Rh is preferably in the form of fine particles from the viewpoint of increasing the contact area with exhaust gas. The average particle size of the fine particle Rh is preferably, for example, 1 nm or more and 15 nm or less. The average particle size of Rh can be obtained by acquiring an electron microscope image (e.g., a TEM image, etc.) of Rh and calculating the average particle size of any 20 or more particles in the image.

[0045] The outflow side catalyst layer usually contains an OSC material. The OSC material is the same as the OSC material described in the above section "2. Inflow side catalyst layer". The OSC material may function as a carrier that supports Rh. The outflow side catalyst layer may further contain a carrier other than the OSC material as a carrier that supports Rh. The carrier other than the OSC material is the same as the carrier other than the OSC material described in the above section "2. Inflow side catalyst layer".

[0046] The content of Rh in the outlet side catalyst layer is not particularly limited, but is preferably, for example, 0.01 mass % to 8 mass % based on the total mass of the OSC material and the carrier other than the OSC material contained in the outlet side catalyst layer.

[0047] The outflow side catalyst layer may further contain, for example, a binder, an additive, etc. in addition to Rh, an OSC material, a carrier other than an OSC material, etc. The binder and the additive are the same as those described in the above section "2. Inflow side catalyst layer".

[0048] The thickness of the outflow side catalyst layer is not particularly limited, and may be appropriately determined depending on the size of the cells of the substrate and the flow rate of the exhaust gas supplied to the EHC. The thickness of the outflow side catalyst layer is not particularly limited, but is preferably, for example, 1 μm or more and 500 μm or less. The coating amount obtained by dividing the mass of the outflow side catalyst layer by the volume of the substrate is not particularly limited, but is preferably, for example, 30 g / L or more and 100 g / L or less. This is because the purification performance can be effectively improved by the coating amount being equal to or more than the lower limit. This is because the pressure loss can be effectively suppressed by the coating amount being equal to or less than the upper limit.

[0049] 4. EHC The EHC includes a substrate, an inlet-side catalytic layer, and an outlet-side catalytic layer. In the EHC, the total coating amount obtained by dividing the total mass of the inlet-side catalytic layer and the outlet-side catalytic layer by the volume of the substrate is 138 g / L or more and 150 g / L or less. The EHC may further include a positive electrode and a negative electrode as in the first embodiment. The positive electrode and the negative electrode are not particularly limited and may be the same as known EHCs, for example, metal electrodes, carbon electrodes, etc. The type of EHC is not particularly limited and may be a straight-flow type or wall-flow type three-way catalyst. The EHC is disposed in the exhaust passage of an internal combustion engine of a vehicle (automobile) or the like and used to purify exhaust gas from the internal combustion engine. The EHC is not particularly limited, but is preferably used in a tandem-type catalytic converter as in the first embodiment. EXAMPLES

[0050] The EHC according to the embodiment will be described in more detail below with reference to examples and comparative examples.

[0051] [Example 1] An example of the EHC according to the first embodiment (a straight-flow type three-way catalyst) was produced. First, a substrate having a cylindrical frame and a partition wall integrally formed therewith was prepared. The substrate had the following structure.

[0052] (base material) Substrate material: Si-SiC composite Base material size: Outer diameter x axial length = 80 mm x 65 mm Partition thickness: 190μm Partition wall porosity: 40% Average pore size of partition wall: 7.5μm Cell Density: 600 cells per square inch

[0053] Next, a Pd nitrate solution, a ceria-zirconia composite oxide powder, an Al2O3 powder, BaSO4 with an average particle size of 100 nm, a binder, and ion-exchanged water were mixed together to prepare a slurry for the inlet side catalyst layer (Pd-containing slurry).

[0054] Next, the slurry for the inlet-side catalyst layer was poured into the cells of the substrate from the inlet-side end, and was supplied to coat the surface of the cell side of the partition wall in the inlet-side catalyst region extending from the inlet-side end of the partition wall along the extension direction to the outlet side for a distance of 75% of the total length of the partition wall in the extension direction. At this time, the supply amount of the slurry was adjusted so that the coating amount obtained by dividing the mass of the inlet-side catalyst layer by the volume of the substrate (hereinafter, abbreviated as "coating amount of the inlet-side catalyst layer") was 96 g / L. Next, the substrate coated with the slurry was dried by heating at 120°C for 2 hours in a dryer, and then fired at 500°C for 2 hours in an electric furnace. In this way, the inlet-side catalyst layer was formed.

[0055] Next, a Rh nitrate solution, a ceria-zirconia composite oxide powder, an alumina-zirconia composite oxide powder, an Al2O3 powder, a binder, and ion-exchanged water were mixed together to prepare a slurry for the outlet side catalyst layer (Rh-containing slurry).

[0056] Next, the slurry for the outflow side catalyst layer was poured into the cells of the substrate from the outflow side end, and was supplied to coat the cell side surface of the partition wall in the part that does not overlap with the inflow side catalyst region and the surface of the inflow side catalyst layer in the part that overlaps with the inflow side catalyst region in the outflow side catalyst region extending from the outflow side end of the partition wall along the extension direction to the inflow side for a distance of 75% of the total length in the extension direction of the partition wall. At this time, the supply amount of the slurry was adjusted so that the coating amount obtained by dividing the mass of the outflow side catalyst layer by the volume of the substrate (hereinafter, abbreviated as "coating amount of the outflow side catalyst layer") was 54 g / L. Next, the substrate coated with the slurry was dried by heating at 120 ° C. for 2 hours in a dryer, and then fired at 500 ° C. for 2 hours in an electric furnace. In this way, the outflow side catalyst layer was formed.

[0057] Next, a positive electrode and a negative electrode were attached to the outer peripheral surface of the frame of the substrate. As a result, an EHC was produced so that the total coating amount (the total mass of the inlet-side catalyst layer and the outlet-side catalyst layer divided by the volume of the substrate) was 150 g / L.

[0058] [Example 2] An EHC was prepared in the same manner as in Example 1, except that the amount of slurry supplied was adjusted so that the coating amount of the inlet-side catalyst layer was 88.5 g / L, and the amount of slurry supplied was adjusted so that the coating amount of the outlet-side catalyst layer was 49.5 g / L, so that the total coating amount of the inlet-side catalyst layer and the outlet-side catalyst layer was 138 g / L.

[0059] [Comparative Example] An EHC was produced in the same manner as in Example 1, except that the supply amount of the slurry was adjusted so that the coating amount of the inlet-side catalyst layer was 128 g / L, and the supply amount of the slurry was adjusted so that the coating amount of the outlet-side catalyst layer was 72 g / L, so that the total coating amount of the inlet-side catalyst layer and the outlet-side catalyst layer was 200 g / L.

[0060] [evaluation] The EHCs produced in the examples and comparative examples were evaluated for exhaust gas purification performance, OSC characteristics, and pressure drop characteristics when the catalyst temperature was increased by electrical heating.

[0061] (Exhaust gas purification performance) For the EHCs of Examples 1 and 2 and Comparative Example, the amount of NMOG (Non-Methane Organic Gases) emitted [mg / mile] was measured as an index of exhaust gas purification performance when the catalyst was heated by electrical heating. At this time, first, the EHC of each example was endured for 80 hours at an inlet gas temperature of 950°C in an engine with a displacement of 4L. Next, the EHC of each example was mounted on an actual vehicle having an engine with a displacement of 2.4L, and the vehicle was driven with the driving mode set to LA#4 mode to measure the amount of NMOG emitted from the catalyst. At this time, the bed temperature of the catalyst was raised to 500°C in 60 seconds by applying a voltage between the positive and negative electrodes of the EHC from the start of the vehicle's driving. The results are shown in Table 1 below.

[0062] (OSC characteristics) The maximum oxygen storage capacity was determined for the EHCs of Example 1 and Comparative Example as an index showing the OSC characteristics. First, as a durability test of the EHCs of each example, a deterioration acceleration test was performed for 80 hours at a catalyst bed temperature of 950°C using a 1UR-FE engine manufactured by Toyota Motor Corporation. In the test, the exhaust gas composition was adjusted by adjusting the throttle opening and engine load, and rich-stoichiometric-lean was repeated in a constant cycle to accelerate deterioration. Next, the EHCs of each example after the durability test were mounted on a 2AR-FE engine manufactured by Toyota Motor Corporation, the inlet gas temperature was set to 600°C, and the A / F of the inlet gas atmosphere was feedback-controlled to periodically oscillate between 14.1 and 15.1, and the excess or deficiency of oxygen was calculated from the difference between the stoichiometric point and the A / F sensor output using the formula: OSC(g)=0.23×ΔA / F×injected fuel amount, and the maximum oxygen storage capacity was determined. The results are shown in Table 1 below.

[0063] (Pressure loss characteristics) For the EHC of Example 1 and the Comparative Example, 7 m of air was blown into the EHC of each example. 3 The pressure loss [kPa] was measured when the mixture was passed through the pipe at 20° C. / min. The results are shown in Table 1 below.

[0064] [Table 1]

[0065] Fig. 4 is a graph showing the change in NMOG emission amount versus the total coating amount of the inlet-side catalyst layer and the outlet-side catalyst layer obtained from the EHC of the example and the comparative example. Fig. 5 is a graph showing the change in maximum oxygen storage amount versus the total coating amount of the inlet-side catalyst layer and the outlet-side catalyst layer obtained from the EHC of the example and the comparative example. Fig. 6 is a graph showing the change in pressure loss versus the total coating amount of the inlet-side catalyst layer and the outlet-side catalyst layer obtained from the EHC of the example and the comparative example.

[0066] As shown in Table 1 and Figure 4, the NMOG emissions decreased as the total coating amount of the inlet-side catalyst layer and the outlet-side catalyst layer decreased from 200 g / L to 138 g / L. As the total coating amount decreased, the temperature rise property (warm-up characteristic) of the catalyst by electric heating improved, and it is considered that the exhaust gas purification performance when the catalyst is heated by electric heating improved. In addition, as shown in Table 1 and Figure 5, the maximum oxygen storage amount increased as the total coating amount increased. It is considered that the OSC characteristic improved as the total coating amount increased. Furthermore, as shown in Table 1 and Figure 6, the pressure loss decreased as the total coating amount decreased. It is considered that the pressure loss decreased because the inlet-side catalyst layer and the outlet-side catalyst layer became thinner as the total coating amount decreased.

[0067] The above describes in detail an embodiment of the electrically heated catalytic converter (EHC) of the present invention, but the present invention is not limited to the above embodiment, and various design modifications can be made without departing from the spirit of the present invention described in the claims. [Explanation of symbols]

[0068] 1: electrically heated catalyst device (EHC), 10: substrate, 10Sa: inlet end face, 10Sb: outlet end face, 11: frame, 12: cell, 12a: inlet end, 12b: outlet end, 14: partition wall, 14a: inlet end, 14b: outlet end, 14X: inlet catalyst region, 14Y: outlet catalyst region, 20: inlet catalyst layer, 30: outlet catalyst layer

Claims

[Claim 1] An electrically heated catalytic device comprising a substrate, an inlet-side catalytic layer, and an outlet-side catalytic layer, The substrate contains SiC, The inlet-side catalytic layer contains Pd as a catalytic component, The outlet-side catalytic layer contains Rh as a catalytic component, The substrate has partition walls that define a plurality of cells extending from an inlet end surface to an outlet end surface, the inlet-side catalyst layer is provided on a surface of the partition wall in an inlet-side catalyst region extending from the inlet-side end of the partition wall to the outlet side along the extension direction by a distance exceeding 50% of the entire length of the partition wall in the extension direction, the outflow-side catalyst layer is provided on a surface of the partition wall in a portion that does not overlap with the inflow-side catalyst region and on a surface of the inflow-side catalyst layer in a portion that overlaps with the inflow-side catalyst region, in an outflow-side catalyst region extending from the outflow-side end of the partition wall along the extension direction to the inflow side by a distance that exceeds 50% of the entire length in the extension direction of the partition wall, an electrically heated catalyst device, characterized in that a total coating amount obtained by dividing the total mass of the inlet side catalyst layer and the outlet side catalyst layer by the volume of the base material is 138 g / L or more and 150 g / L or less.

Citation Information

Patent Citations

  • A two -layer TWC catalyst in novel three districts for petrol waste gas is used

    CN208057201U

  • Diesel oxidation catalytic converter WITH NOx ADSORPTION ACTIVITY

    DE102017120303A1

  • Catalytic converter

    JP2016175053A

  • Exhaust gas purification catalyst

    JP2022030628A

  • Novel TWC catalysts for gasoline exhaust gas applications

    US20200102868A1