Electronic component processing film and electronic component processing method
The electronic component processing film with specific modulus and tensile strength properties, combined with an acrylic adhesive and polyvinyl chloride base layer, addresses tearing issues during stretching, enabling high stretching ratios and cost-effective manufacturing.
Patent Information
- Application Number
- JP2023077471
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing electronic component processing films tear easily during stretching due to insufficient tensile strength and modulus, limiting their ability to achieve the required stretching ratio for spacing chips.
An electronic component processing film with a 50% modulus of 9 MPa or less and a tensile strength of 22 MPa or more, composed of an adhesive layer with acrylic adhesive and a base layer containing polyvinyl chloride, allowing for a stretching ratio of 150% or more.
The film effectively suppresses tearing during stretching, ensuring high stretching ratios without equipment heating, reducing manufacturing costs and improving workability and productivity.
Smart Images

Figure 2024162171000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a film for processing electronic components and a method for processing electronic components. [Background technology]
[0002] Manufacturing methods for electronic components such as semiconductor chips and ceramic capacitors include a process in which a wafer placed on a stretchable film is diced into individual pieces of a desired size, and then the film is stretched to increase the distance between the chips and pick up the chips.
[0003] In recent years, the diversification of electronic component processing techniques has progressed, and a technique for processing individual chips as electronic components on a stretched film has been considered. For this reason, a film capable of widening the gap between chips compared to when the purpose is to pick up the chips has been developed. For example, Patent Document 1 proposes a method for manufacturing a semiconductor device that includes a step of widening the gap between individual chips on a film from a distance of 100 μm or less to a distance of 300 μm or more, and a film used in this method. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2018 / 216621 Summary of the Invention [Problem to be solved by the invention]
[0005] When a film having individualized electronic components arranged thereon is stretched, the film may not be stretched to the required dimension and may tear. Considering the workability and productivity of electronic component processing, it is desirable that the film is not easily torn during the stretching process.
[0006] One embodiment of the present disclosure provides an electronic component processing film in which film breakage during stretching is suppressed, and an electronic component processing method using the electronic component processing film. [Means for solving the problem]
[0007] Means for solving the above problems include the following embodiments. <1> A film for processing electronic components, comprising an adhesive layer and a base layer, and satisfying the following requirements (1) and (2). (1) 50% modulus is 9 MPa or less (2) Tensile strength is 22 MPa or more <2> The stretching ratio when stretched at 23°C is 150% or more. <1> 2. The electronic component processing film according to claim 1 . <3> The adhesive layer comprises an acrylic adhesive. <1> 2. The electronic component processing film according to claim 1 . <4> The substrate layer comprises polyvinyl chloride. <1> 2. The electronic component processing film according to claim 1 . <5> <1> ~ <4> 13. An electronic component processing method comprising the step of stretching the electronic component processing film with individualized electronic components placed on the adhesive layer of the electronic component processing film described in any one of claims 1 to 12. <6> The method includes a step of processing electronic components on the electronic component processing film after the step of stretching the electronic component processing film. <5> The electronic component processing method according to claim 1 . Effect of the Invention
[0008] According to one embodiment of the present disclosure, there is provided an electronic component processing film in which film breakage during stretching is suppressed, and an electronic component processing method using the electronic component processing film. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of the configuration of an electronic component processing film. [Diagram 2] FIG. 2 is a plan view showing the shape of a test piece used in a tensile test of an electronic component processing film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, several embodiments of the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the components (including element steps, etc.) are not essential unless otherwise specified. The same applies to the numerical values and their ranges, and do not limit the present disclosure. In the present disclosure, the term "step" includes not only a step that is independent of other steps, but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved. In the present disclosure, a numerical range indicated using "~" includes the numerical values before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present disclosure, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit of the numerical range may be replaced with a value shown in the examples. In the present disclosure, each component may contain multiple types of the corresponding substance. When multiple substances corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, "(meth)acrylic" means at least one of acrylic and methacrylic.
[0011] <Electronic component processing film> The film for processing electronic components of the present disclosure is a film for processing electronic components that includes an adhesive layer and a base layer and satisfies the following requirements (1) and (2). (1) 50% modulus is 9 MPa or less (2) Tensile strength is 22 MPa or more
[0012] As a result of the investigations conducted by the present inventors, it was found that the above-mentioned film for processing electronic parts is prevented from breaking during stretching and can ensure a sufficient stretch ratio. The reasons for this are considered to be, for example, as follows.
[0013] If the 50% modulus of the electronic component processing film is 9 MPa or less, the electronic component processing film is easily stretched when stretched. As a result, the load on the electronic component processing film is reduced, and it is believed that the film is less likely to break when stretched. Similarly, if the tensile strength of the electronic component processing film is 22 MPa or more, it is believed that the electronic component processing film is less likely to break when stretched.
[0014] In the present disclosure, a film for processing electronic components is deemed to satisfy requirement (1) when the 50% modulus in both the MD and TD directions is 9 MPa or less. In the present disclosure, a film for processing electronic components is deemed to satisfy requirement (2) when the tensile strength in both the MD and TD directions is 22 MPa or more. In the present disclosure, the MD direction and TD direction of the electronic component processed film refer to the MD direction (machine direction) and TD direction (direction perpendicular to the MD direction) of the base material used in the electronic component processed film during production.
[0015] In the present disclosure, the 50% modulus of the electronic component processing film may be 9 MPa or less, and may be 8.8 MPa or less. The lower limit of the 50% modulus of the electronic component processing film is not particularly limited, but may be 4 MPa or more or 6 MPa or more from the viewpoint of ease of stretching the electronic component processing film during stretching.
[0016] In the present disclosure, the tensile strength of the electronic component processing film may be 22 MPa or more, and may be 24 MPa or more or 25 MPa or more. The upper limit of the tensile strength of the electronic component processing film is not particularly limited, but may be 30 MPa or less or 29 MPa or less from the viewpoint of suppressing film breakage during stretching.
[0017] In the present disclosure, the 50% modulus and tensile strength of the electronic component processing film are measured according to a method conforming to JIS K 7127. Specifically, a Tensilon tensile tester "RTA-100 type" manufactured by Orientec Co., Ltd. or a similar tester having a jig for holding both ends of the test piece is used.
[0018] For the measurement, a test piece with the shape shown in Figure 2 is prepared, and both ends of the test piece are gripped by the jig of the testing machine to perform a tensile test. The distance between the gripping positions of the jig is 40 mm. The test is performed in an environment of 23±5°C, with a tensile speed of 500 mm / min.
[0019] The 50% modulus of the test piece is calculated from the thickness (mm) and width (10 mm in this test) of the test piece before the test, and the maximum load (N) when the test piece is stretched to 50% (from 40 mm to 60 mm in this test) using the following formula.
[0020]
number
[0021] The tensile strength of the test piece is calculated from the thickness (mm) and width (10 mm in this test) of the test piece before the test and the maximum load (N) until the test piece breaks, using the following formula.
[0022]
number
[0023] The 50% modulus and tensile strength of the electronic component processed film can be adjusted, for example, by changing the thickness of the base layer or adhesive layer contained in the electronic component processed film, the type and amount of components contained in the base layer (thermoplastic resin, plasticizer, etc.), the type and amount of components contained in the adhesive layer (polymer material, polyisocyanate, plasticizer, etc.), the manufacturing conditions of the base layer (stretching ratio, etc.), etc.
[0024] Fig. 1 is a cross-sectional view showing an example of the structure of an electronic component processing film. The electronic component processing film 40 shown in Fig. 1 includes a base layer 10, an adhesive layer 30 provided on the main surface of the base layer 10, and a separator 20 covering the surface of the adhesive layer 20 opposite to the base layer 10. The shape of the electronic component processing film in plan view is not particularly limited, and may be, for example, circular like a film generally used in a process for dividing electronic components.
[0025] The stretching ratio of the electronic component processing film is not particularly limited and can be selected according to the application of the electronic component processing film, etc. From the viewpoint of ensuring sufficient spacing between electronic components during processing of the electronic components, the higher the stretching ratio of the electronic component processing film, the more preferable. The stretch ratio of the film for processing electronic components may be, for example, 110% or more, 130% or more, or 150% or more.
[0026] In this disclosure, the stretch rate of the electronic component processing film is based on the dimensional change rate of the central part of the electronic component processing film. When the electronic component processing film is stretched, the central part tends to be less stretched than the peripheral part. For this reason, in this disclosure, the stretch rate of the electronic component processing film is measured in the central part.
[0027] As shown in the results of the examples described later, the electronic parts processing film of the present disclosure effectively prevents film breakage even when stretched at room temperature. Therefore, equipment for heating the electronic parts processing film during stretching can be omitted, and production costs can be reduced. The film for processing electronic components according to the present disclosure may have a stretch ratio of 110% or more, 130% or more, or 150% or more when stretched at room temperature (eg, 23° C.).
[0028] (base material layer) The material of the base layer of the electronic component processing film is not particularly limited. From the viewpoint of obtaining good stretchability, the base layer preferably contains a resin, more preferably a thermoplastic resin. Examples of the thermoplastic resin include polyvinyl chloride, polyester, polyolefin, polyamide, polyimide, polyurethane, and thermoplastic elastomer. From the viewpoint of stretchability, polyvinyl chloride is preferred.
[0029] In order to impart flexibility to the base layer, the base layer may contain a plasticizer. The type of plasticizer is not particularly limited, and may be selected from the plasticizers contained in the adhesive layer. In terms of the stretchability of the base and the migration to the adhesive layer, polyester plasticizers are preferred.
[0030] The content of the plasticizer contained in the base layer may be, for example, 10 parts by mass to 55 parts by mass, 20 parts by mass to 50 parts by mass, or 25 parts by mass to 45 parts by mass, relative to 100 parts by mass of the resin contained in the base layer. By setting the content of the plasticizer within the above numerical range, the stretchability of the electronic component processing film can be improved.
[0031] From the viewpoint of improving visibility during processing, the base layer may contain a colorant. Examples of the colorant include dyes and pigments, and from the viewpoint of durability, pigments are preferred. The color of the colorant is preferably a color other than black, and more preferably blue. Specific examples of the colorant include alkali blue, disazo yellow, phthalocyanine blue, Prussian blue, ultramarine blue, and cobalt blue.
[0032] When the colorant is particulate, the maximum particle diameter is preferably smaller than the thickness of the base layer when stretched. If the maximum diameter of the colorant contained in the base layer is smaller than the thickness of the base layer when stretched, the colorant is prevented from falling off the base layer when the base layer is stretched, which is advantageous in terms of maintenance of the electronic component processing device. For example, the maximum particle diameter of the colorant is preferably 25 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less. In the present disclosure, the maximum particle diameter of a colorant is defined as the maximum value of the maximum diameter of each particle (the length when the diameter of the projected image is the longest) obtained from the projected image of colorant particles (preferably 100 or more particles).
[0033] The content of the colorant in the base layer is, for example, preferably 0.1 mass % to 2.0 mass % of the total solid content of the base layer, more preferably 0.2 mass % to 1.5 mass %, and even more preferably 0.3 mass % to 1.0 mass %.
[0034] The thickness of the base layer is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 50 μm or more from the viewpoint of ensuring sufficient strength, and is preferably 500 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less from the viewpoint of ensuring sufficient stretchability.
[0035] If necessary, the surface of the base layer opposite to the surface onto which the adhesive layer is applied may be subjected to a matte finish, an antistatic finish, or the like.
[0036] (Adhesive layer) The adhesive layer contains, for example, a polymer material such as a resin. From the viewpoint of the properties such as the stretchability of the electronic component processing film, it is preferable that the polymer material contained in the adhesive layer contains one or more types selected from the group consisting of (meth)acrylic resin, urethane resin, natural rubber, synthetic rubber and thermoplastic elastomer.
[0037] Examples of the thermoplastic elastomer include styrene-based thermoplastic elastomers such as styrene-isoprene block copolymer (SIS), and hydrogenated styrene-based thermoplastic elastomers such as styrene-ethylene-butylene-styrene block copolymer (SEBS).
[0038] The (meth)acrylic resin and the urethane resin may be crosslinked with a crosslinking agent. The natural rubber and the synthetic rubber may be vulcanized with a peroxide, sulfur, or the like.
[0039] Among the above, from the viewpoint of the stretchability of the electronic component processing film and preventing the electronic components from falling off in a stretched state, it is preferable that the adhesive layer contains a (meth)acrylic resin, and it is more preferable that the adhesive layer contains a (meth)acrylic resin that is crosslinked with a polyisocyanate.
[0040] From the viewpoint of ensuring adhesion to electronic components, the (meth)acrylic resin is preferably a copolymer (acrylic copolymer) containing a monomer having a low glass transition temperature (for example, -20°C or lower) as a copolymerization component. Examples of monomers having a glass transition temperature of -20°C or lower include n-butyl acrylate (-54°C), ethyl acrylate (-22°C), and 2-ethylhexyl acrylate (-70°C). The glass transition temperature of the monomer is a value measured by differential scanning calorimetry (DSC) of a homopolymer obtained using the monomer. The (meth)acrylic resin preferably contains monomers having a glass transition temperature of -20°C or lower in an amount of 50% by mass or more of the total monomers. The (meth)acrylic resin may be a copolymer containing, as copolymerization components, a monomer having a glass transition temperature of −20° C. or lower and acrylonitrile.
[0041] The crosslinking agent for the (meth)acrylic resin means a compound having two or more functional groups capable of reacting with the (meth)acrylic resin in one molecule, and specific examples thereof include polyisocyanate, epoxy-based crosslinking agents, metal chelate-based crosslinking agents, and aziridine-based crosslinking agents. From the viewpoints of ease of ensuring anchoring to the base layer and ease of controlling the properties by the amount used, polyisocyanate is preferred as the crosslinking agent.
[0042] In the present disclosure, polyisocyanate means a compound having two or more isocyanate groups in one molecule, and includes aliphatic polyisocyanates, alicyclic polyisocyanates, and aromatic polyisocyanates.
[0043] The polyisocyanate is preferably a polyfunctional isocyanate compound (a compound having three or more isocyanate groups in one molecule). Examples of the polyfunctional isocyanate compound include a trimer of a bifunctional isocyanate compound and a polymer compound having a trimer of a bifunctional isocyanate compound in the molecule.
[0044] Examples of the trimer of a difunctional isocyanate compound include an isocyanurate of a difunctional isocyanate compound, an adduct of a difunctional isocyanate compound, and a biuret of a difunctional isocyanate compound. Examples of the bifunctional isocyanate compound include aliphatic diisocyanate compounds such as hexamethylene diisocyanate, pentamethylene diisocyanate, tetramethylene diisocyanate, trimethylhexamethylene diisocyanate, and lysine diisocyanate; alicyclic diisocyanate compounds such as isophorone diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated 4,4'-diphenylmethane diisocyanate; and aromatic diisocyanate compounds such as tolylene diisocyanate, xylylene diisocyanate, and 4,4'-diphenylmethane diisocyanate. Among the polyisocyanates, adducts of aliphatic diisocyanate compounds are preferred, and adducts of hexamethylene diisocyanate are more preferred.
[0045] When the adhesive layer contains a (meth)acrylic resin crosslinked with a polyisocyanate, the amount of polyisocyanate per 100 parts by mass of the (meth)acrylic resin is preferably 0.5 parts by mass or more, more preferably 1.0 part by mass or more, and even more preferably 2.0 parts by mass or more. By setting the content of polyisocyanate within the above range, the stretch ratio of the film for processing electronic parts can be improved. The upper limit of the polyisocyanate content is not particularly limited, but can be, for example, 4.0 parts by mass or less per 100 parts by mass of the (meth)acrylic resin.
[0046] The adhesive layer may contain a plasticizer. The type of plasticizer is not particularly limited and can be selected according to the type of adhesive, etc. Specific examples include polyester plasticizers such as polyester adipate, phthalates such as bis(2-ethylhexyl) phthalate, terephthalates such as bis(2-ethylhexyl) terephthalate, adipic acids such as bis(2-ethylhexyl) adipate, trimellitic acid esters, phosphoric acid esters, citrate esters, and epoxidized vegetable oils.
[0047] Among the above plasticizers, polyester plasticizers, terephthalic acid esters, and phthalic acid esters are preferred, and from the viewpoint of affinity with living bodies and the environment, polyester plasticizers and terephthalic acid esters are more preferred. The plasticizer contained in the adhesive layer may be one type or two or more types.
[0048] When the adhesive layer contains a plasticizer, the content of the plasticizer per 100 parts by mass of the polymer material is preferably 0.1 part by mass or more, more preferably 1.0 part by mass or more, and even more preferably 2.5 parts by mass or more. The content of the plasticizer may be 50 parts by mass or less, 40 parts by mass or less, 30 parts by mass or less, or 20 parts by mass or less, relative to 100 parts by mass of the polymer material.
[0049] If necessary, the adhesive layer may contain a surfactant, a tackifier, a filler, and the like.
[0050] From the viewpoint of ensuring sufficient adhesive strength to electronic components, the thickness of the adhesive layer is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. From the viewpoint of economic efficiency, the thickness of the adhesive layer is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less.
[0051] (Separator) If necessary, a separator may be provided on the outer surface of the adhesive layer (the surface opposite to the side facing the base layer).
[0052] The material of the separator is not particularly limited, but from the viewpoint of the coatability of the adhesive layer and the smoothness of the adhesive layer to be formed, it is preferable that the separator is a film having a release treatment applied to the surface of the resin film. Examples of the release treatment include applying a release material to the surface of the resin film to form a release layer.
[0053] The resin film may be a stretched film or a non-stretched film, but is preferably a stretched film from the viewpoint of winding and processability of the film for processing electronic parts.
[0054] Examples of resin materials that may be used to form the resin film include polyethylene terephthalate (PET), triacetyl cellulose (TAC), polyethylene naphthalate (PEN), polymethyl methacrylate (PMMA), polycarbonate (PC), polyimide (PI), polyethylene (PE), polypropylene (PP), polyvinyl alcohol (PVA), polyvinyl chloride (PVC), cycloolefin copolymer (COC), cycloolefin polymer (COP), norbornene resin, polyethersulfone, cellophane, and aromatic polyamide.
[0055] The thickness of the separator is not particularly limited, but can be, for example, 10 μm to 300 μm.
[0056] <Electronic component processing method> The electronic component processing method of the present disclosure includes a step of stretching the electronic component processing film described above in a state in which individual electronic components are arranged on the electronic component processing film (stretching step).
[0057] In the above method, the electronic components placed on the electronic component processing film may be individualized on the electronic component processing film, or may be individualized before being placed on the electronic component processing film.
[0058] If the electronic components are singulated before being placed on the electronic component processing film, the singulated electronic components can be placed on the electronic component processing film, for example, by singulating the electronic components on another film, and then attaching the adhesive layer of the electronic component processing film to the singulated electronic components, thereby transferring the electronic components to the electronic component processing film.
[0059] The stretching ratio of the film for electronic parts processing in the stretching step is not particularly limited and can be selected according to the type of processing to be performed after stretching, etc. For example, the film for electronic parts processing may be stretched so that the stretching ratio is 110% or more, 130% or more, or 150% or more.
[0060] The distance between adjacent electronic components after the stretching step (if the distance is not constant, the minimum distance) is not particularly limited and can be selected depending on the type of processing to be performed after stretching, etc. For example, the distance between the electronic components may be 100 μm or more, 200 μm or more, or 300 μm or more.
[0061] From the viewpoint of workability during processing of electronic components, it is preferable that the variation in the distance between electronic components after the stretching step is small. For example, the value obtained by multiplying the ratio of the maximum distance between electronic components after the stretching step to the minimum distance (maximum value / minimum value) by 100 is preferably 300 or less, more preferably 200 or less, and even more preferably 150 or less.
[0062] If necessary, after the stretching step, processing of electronic parts (sealing treatment, heat treatment, etc.) may be performed on the film for processing electronic parts.
[0063] After the stretching step and the processing of the electronic parts, which is performed as necessary, are performed, the electronic parts are picked up from the film for processing electronic parts. The method for picking up the electronic parts is not particularly limited, and can be a known method. Before picking up, a treatment (such as ultraviolet irradiation or heat treatment) may be carried out to reduce the adhesive strength of the adhesive layer.
[0064] The type of electronic component used in the above method is not particularly limited, and examples thereof include various semiconductor chips and ceramic capacitors. EXAMPLES
[0065] Hereinafter, one embodiment of the present disclosure will be described in more detail with reference to examples, although the present disclosure is not limited to these examples.
[0066] (Preparation of Adhesive Layer Composition) The components shown below (parts by mass, calculated as solid content) were mixed to prepare a composition for adhesive layer. Polymer component: Acrylic adhesive (Tohpe Corporation, XE-2644, copolymer of 80% to 90% by mass of n-butyl acrylate and 10% to 20% by mass of acrylonitrile): 100 parts by mass Plasticizer: Polyester adipic acid (ADEKA Corporation, Adeka Cizer P-200): 20 parts by weight Polyisocyanate: Hexamethylene diisocyanate adduct (Asahi Kasei Corporation, Duranate E405-80T): 2 parts by mass
[0067] (Preparation of the substrate) A polyvinyl chloride film having a thickness of 120 μm and having the physical properties shown in Table 1 below was prepared as a substrate. The 50% modulus and tensile strength of the substrate were measured in the same manner as the 50% modulus and tensile strength of the film for processing electronic components.
[0068] [Table 1]
[0069] (Production of electronic component processing film) The adhesive layer composition was applied to the release-treated surface of a PET film having a thickness of 38 μm, one side of which was treated for release, so that the thickness after drying was 20 μm, and then dried to form an adhesive layer. Next, the adhesive layer side of the PET film was attached to one side of a substrate at room temperature (25° C.), and the adhesive layer was transferred onto the substrate by pressing with a rubber roll. After that, the PET film was peeled off to produce an electronic component processing film having a substrate layer and an adhesive layer.
[0070] (Evaluation of stretchability) The electronic component processed film was cut into a circle with a diameter of 400 mm to prepare a test piece, and the test piece was stretched using a push-up type stretching device. Specifically, the test piece was placed on a circular stage (diameter 216 mm) of a stretching device "OEX-1200" manufactured by Omiya Kogyo Co., Ltd. or a similar push-up type stretching device so that the center of the stage and the center of the test piece were aligned. Next, in an environment of 23°C, the stage was pushed up to a height of 130 mm at an upward speed of 10 mm / s. The dimensional change rate (%) of the center of the test piece before and after the push-up was calculated using the following formula, and the calculated value was taken as the elongation rate (%).
[0071] The dimensional change rate at the center of the test piece means the dimensional change rate of a region corresponding to a circle having a diameter D (216 mm) centered at the center of the test piece. The dimensional change rate at the center of the test piece is the average value of the measured values obtained in the MD and TD directions of the test piece.
[0072] Elongation rate (%) = Dimensional change rate (%) at center part = (D1 / D2) x 100 D1: Dimension of diameter D after stretching D2: Diameter D before stretching
[0073] The above-mentioned stretching was carried out on a total of 10 test pieces, and the average stretching ratio of the test pieces in which no film breakage occurred during stretching was calculated. The results are shown in Table 2. Table 2 also shows the number of test pieces in which film breakage occurred during stretching.
[0074] [Table 2]
[0075] In Table 1, "ND" indicates that the stretching ratio could not be measured for all test pieces because the film broke during stretching. As shown in Table 1, the films for electronic parts processing produced in the examples that satisfied (1) and (2) were prevented from breaking during stretching. The films for electronic parts processing produced in Comparative Examples 1 and 2 that satisfied (2) but did not satisfy (1) broke in 10 out of 10 test pieces during stretching. The films for electronic parts processing produced in Comparative Example 3 that satisfied (1) but did not satisfy (2) broke in 5 out of 10 test pieces during stretching. [Explanation of symbols]
[0076] 40...electronic component processing film, 10...base material layer, 30...adhesive layer, 20...separator
Claims
1. A film for processing electronic components, comprising an adhesive layer and a base layer, and satisfying the following requirements (1) and (2): (1) The 50% modulus is 9 MPa or less. (2) Tensile strength is 22 MPa or more.
2. 2. The film for processing electronic parts according to claim 1, which has a stretch ratio of 150% or more when stretched at 23°C.
3. The film for processing electronic components according to claim 1 , wherein the adhesive layer comprises an acrylic adhesive.
4. The electronic component processing film according to claim 1 , wherein the base layer comprises polyvinyl chloride.
5. An electronic component processing method comprising a step of stretching the electronic component processing film with an individualized electronic component placed on the adhesive layer of the electronic component processing film according to any one of claims 1 to 4.
6. 6. The method for processing electronic parts according to claim 5, further comprising the step of processing electronic parts on said electronic part processing film after said step of stretching said electronic part processing film.
Citation Information
Patent Citations
Semiconductor device manufacturing method and expand tape
WO2018216621A1