Material for forming organic film, patterning process, and organic film compound
The multilayer resist method using a specific organic film-forming material and silicon-containing interlayer film addresses the challenges of pattern collapse and etching resistance in semiconductor manufacturing, enabling precise pattern transfer and planarization on complex substrates.
Patent Information
- Application Number
- JP2023077725
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
AI Technical Summary
The challenge of forming fine patterns in semiconductor manufacturing is exacerbated by the decrease in photoresist film thickness, leading to pattern collapse due to high aspect ratios and inadequate dry etching selectivity, which compromises the transfer of resist patterns to the substrate, while recent resins with high resolution have weaker etching resistance.
A multilayer resist method using an organic film-forming material containing a specific organic film-forming compound with a defined structure, combined with a silicon-containing resist interlayer film, allows for the transfer of patterns through multiple etching steps, ensuring excellent embedding and planarization properties.
This approach enables the formation of fine patterns with high precision on substrates, even those with complex structures, by maintaining etching resistance and planarization, thus overcoming the limitations of single-layer resist methods.
Smart Images

Figure 2024162330000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an organic film-forming material, a pattern forming method, and a compound for an organic film. [Background technology]
[0002] As LSIs become more highly integrated and faster, pattern dimensions are becoming finer. Lithography technology has achieved the formation of finer patterns by shortening the wavelength of light sources and selecting appropriate resist compositions to match them, in line with this trend. The core of this technology is a positive photoresist composition used in a single layer. This single-layer positive photoresist composition has a skeleton in the resist resin that is resistant to dry etching using chlorine- or fluorine-based gas plasma, and also has a switching mechanism that dissolves the exposed areas, forming a pattern by dissolving the exposed areas, and then dry etching the substrate using the remaining resist pattern as an etching mask.
[0003] However, when the thickness of the photoresist film used is made finer, that is, when the pattern width is made smaller, the resolution performance of the photoresist film is reduced, and when an attempt is made to develop the photoresist film into a pattern using a developer, the so-called aspect ratio becomes too large, resulting in problems such as pattern collapse. For this reason, photoresist films have been made thinner as patterns become finer.
[0004] On the other hand, in the processing of a substrate to be processed, a method is usually used in which a photoresist film on which a pattern is formed is used as an etching mask to process the substrate by dry etching, but in reality, there is no dry etching method that can obtain complete etching selectivity between the photoresist film and the substrate to be processed. Therefore, there is a problem that the resist film is also damaged and collapsed during processing of the substrate, and the resist pattern cannot be accurately transferred to the substrate to be processed. Therefore, with the miniaturization of patterns, higher dry etching resistance has been required for resist compositions. However, on the other hand, in order to increase resolution, resins used in photoresist compositions have been required to have low light absorption at the exposure wavelength. Therefore, as the exposure light has become shorter in wavelength from i-line to KrF and ArF, resins have also changed to novolac resins, polyhydroxystyrene, and resins with aliphatic polycyclic skeletons, but in reality, the etching speed under dry etching conditions during substrate processing has become faster, and recent photoresist compositions with high resolution tend to have weaker etching resistance.
[0005] For this reason, the substrate to be processed must be dry etched using a thinner photoresist film with a weaker etching resistance, and it is important to ensure the availability of materials and processes for this processing step.
[0006] One method for solving such problems is the multi-layer resist method, in which a resist underlayer film, which has a different etching selectivity from a photoresist film (i.e., a resist upper layer film), is interposed between the resist upper layer film and a substrate to be processed, a pattern is obtained in the resist upper layer film, and then the pattern is transferred to the resist underlayer film by dry etching using the resist upper layer film pattern as a dry etching mask, and the pattern is further transferred to the substrate to be processed by dry etching using the resist underlayer film as a dry etching mask.
[0007] One of the multilayer resist methods is a three-layer resist method that can be performed using a general resist composition used in a single-layer resist method. In this three-layer resist method, for example, an organic film made of novolac resin or the like is formed on a substrate to be processed as a resist underlayer film, a silicon-containing film is formed on the organic film as a resist intermediate film, and a normal organic photoresist film is formed on the organic film as a resist upper layer film. When dry etching is performed using fluorine-based gas plasma, the organic resist upper layer film has a good etching selectivity to the silicon-containing resist intermediate film, so the resist upper layer film pattern can be transferred to the silicon-containing resist intermediate film by dry etching using fluorine-based gas plasma. According to this method, even if a resist composition that is difficult to form a pattern with a sufficient film thickness for directly processing a substrate to be processed or a resist composition that does not have sufficient dry etching resistance for processing a substrate is used, a pattern can be transferred to the silicon-containing resist intermediate film, and then, by performing pattern transfer by dry etching using oxygen-based or hydrogen-based gas plasma, a pattern of an organic film (resist underlayer film) made of novolac resin or the like that has sufficient dry etching resistance for processing a substrate can be obtained. As the above-mentioned resist underlayer film, many films are already known, for example, the one described in Patent Document 1.
[0008] On the other hand, in recent years, the manufacturing of semiconductor devices having new structures such as a multi-gate structure has been actively studied, and in response to this, there is an increasing demand for resist underlayer films with better planarization and filling properties than before. For example, when the underlying substrate to be processed has a micropattern structure such as a hole, a trench, or a fin, the resist underlayer film needs to have the property of filling the pattern with a film without gaps (gap-filling). In addition, when the underlying substrate to be processed has a step or when a pattern-dense area and a pattern-free area exist on the same wafer, the resist underlayer film needs to planarize the film surface. By planarizing the surface of the resist underlayer film, it is possible to suppress the film thickness fluctuation of the resist intermediate film and resist top layer film formed thereon, and to suppress the focus margin of lithography and the margin reduction in the subsequent processing process of the substrate to be processed.
[0009] In addition, organic film materials with excellent filling / planarization properties are not limited to underlayer films for multilayer resists, but can also be widely used as planarization materials in semiconductor device manufacturing, for example, for substrate planarization prior to patterning by nanoimprinting. Furthermore, while the CMP process is currently commonly used for global planarization in the semiconductor device manufacturing process, CMP is a high-cost process, and these materials are expected to be used as an alternative global planarization method.
[0010] A resist underlayer film material containing a polymer obtained by reacting an aromatic compound with a compound having a carbon-oxygen double bond such as a carbonyl group has been proposed for forming a planarizing film for planarizing uneven semiconductor substrates (Patent Document 2). However, the planarizing performance of the material in a wide trench portion of the substrate is insufficient to meet the requirements of cutting-edge devices, and there is a demand for a resist underlayer film material that has excellent planarization performance on a wider range of substrate structures.
[0011] As mentioned above, the structure of the substrate to be processed is becoming more complex, and new materials with high electron mobility using strained silicon and gallium arsenide, etc., and ultra-thin polysilicon controlled to the angstrom level are being considered for the surface of the substrate to be processed, and it is expected that films will be formed on a wide variety of non-processed substrate surface shapes and materials. Therefore, in order to ensure a process margin, it is important that the film be formed without depending on the material and shape of the substrate to be processed, in addition to having excellent filling and planarization characteristics. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2004-205685 A [Patent Document 2] International Publication No. 2019 / 225615 Summary of the Invention [Problem to be solved by the invention]
[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a compound for an organic film capable of forming an organic film which is excellent not only in heat resistance and in filling and flattening characteristics of a pattern formed on a substrate, but also in film-forming properties and adhesion to the substrate, an organic film-forming material containing the compound, and a pattern formation method using the material. [Means for solving the problem]
[0014] In order to solve the above problems, the present invention provides an organic film-forming material, which contains an organic film compound represented by the following general formula (1) and an organic solvent. [ka] (In the formula, W1 is an n1-valent organic group containing an aromatic ring, and L is a substituent on the aromatic ring, which is L1, L2, or both, represented by the following general formula (2). When the total number of substituents L on the aromatic ring is n1, the number of L1 is x, and the number of L2 is y, the relationships x+y=n1, 2≦n1≦8, 0≦y≦8, and 0≦x≦8 are satisfied.) [ka] (In the formula, n2 represents an integer of 1 to 3, R1 represents any of the following formulas (3), and R2 represents any of the following general formulas (4).) [ka] [ka] (In the formula, R3 is any one of the following formulas (5), n3 represents 0 or 1, and n4 represents 1 or 2.) [ka]
[0015] Such an organic film-forming material not only has excellent heat resistance and flattening properties and ability to fill a pattern formed on a substrate, but also allows the formation of an organic film that has good film-forming properties and adhesion to the substrate.
[0016] In the present invention, L1 and L2 constituting the substituent L on the aromatic ring of the compound for organic film represented by the general formula (1) are preferably represented by the following general formula (6). [ka] (In the formula, R1 and R2 are the same as above.)
[0017] By introducing such a structure, it is possible to achieve both the contradictory properties of thermal fluidity and heat resistance.
[0018] In addition, in the present invention, it is preferable that R1 and R2 in L1 and L2 constituting the substituent L on the aromatic ring of the organic film compound represented by the general formula (1) are any of the combinations shown in the following general formula (7). [ka] (In the formula, R3 and n4 are the same as above.)
[0019] By using such a combination, it is possible to improve the thermosetting property and form an organic film with good heat resistance.
[0020] The total number n1 of the substituents L on the aromatic ring of the compound for an organic film represented by the general formula (1) preferably satisfies 3≦n1≦6.
[0021] By adjusting the number of thermosetting groups as the substituents within such a range, the thermosetting groups do not become excessive, so that rapid thermosetting is not caused, the thermal fluidity is not reduced, the planarization characteristics are not deteriorated, and there is no risk of insufficient solvent resistance or heat resistance due to a shortage of thermosetting groups.
[0022] In the present invention, the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn of the compound for organic film, calculated as polystyrene by gel permeation chromatography, is preferably 1.00≦Mw / Mn≦1.15.
[0023] With such Mw / Mn, an organic film with excellent filling properties and flatness can be formed.
[0024] In the present invention, the organic solvent is preferably a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher.
[0025] If the organic solvent is the above mixture, the addition of a high-boiling point solvent to the organic film compound gives the organic film thermal fluidity, and the organic film forming material also has high filling / planarization properties.
[0026] In the present invention, it is preferable that the organic film-forming material further contains at least one of a surfactant and a plasticizer.
[0027] An organic film-forming material containing such a component will have superior coating properties and filling / flattening properties.
[0028] The present invention also provides a method for forming a pattern on a workpiece, comprising the steps of: forming an organic film on a workpiece using the organic film-forming material described above; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming a resist upper layer film on the silicon-containing resist intermediate film using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask; a pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask; Furthermore, the present invention provides a pattern forming method in which the workpiece is etched using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
[0029] The pattern formation method using the three-layer resist process described above makes it possible to form fine patterns on a workpiece with high precision.
[0030] The present invention also provides a method for forming a pattern on a workpiece, comprising the steps of: forming an organic film on a workpiece using the organic film-forming material described above; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming an organic antireflective coating (BARC) on the silicon-containing resist intermediate film; forming a resist top layer film on the BARC using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; The pattern is transferred to the BARC and the silicon-containing resist intermediate film by etching using the resist top layer film on which the pattern is formed as a mask; a pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask; Furthermore, the present invention provides a pattern forming method in which the workpiece is etched using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
[0031] The pattern formation method using the four-layer resist process described above makes it possible to form fine patterns on a workpiece with even greater precision.
[0032] Further, the present invention provides a method for forming a pattern on a workpiece, comprising the steps of: forming an organic film on a workpiece using the organic film-forming material described above; forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film; forming a resist upper layer film on the inorganic hard mask intermediate film using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the inorganic hard mask intermediate film by etching using the resist upper layer film on which the pattern is formed as a mask; The pattern is transferred to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask; Furthermore, the present invention provides a pattern forming method in which the workpiece is etched using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
[0033] This three-layer resist process pattern formation method makes it possible to form fine patterns on the workpiece with high precision.
[0034] Additionally, the present invention provides a method for forming a pattern on a workpiece, comprising the steps of: forming an organic film on a workpiece using the organic film-forming material described above; forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film; forming an organic antireflective coating (BARC) on the inorganic hard mask intermediate film; forming a resist top layer film on the BARC using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; The pattern is transferred to the BARC and the inorganic hard mask intermediate film by etching using the resist top layer film on which the pattern is formed as a mask; The pattern is transferred to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask; Furthermore, the present invention provides a pattern forming method in which the workpiece is etched using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
[0035] This pattern formation method using a four-layer resist process makes it possible to form fine patterns on the workpiece with greater precision.
[0036] In this case, the inorganic hard mask intermediate film is preferably formed by a CVD method or an ALD method.
[0037] When the inorganic hard mask intermediate film is formed by a CVD method or an ALD method, a fine pattern can be formed on a workpiece with higher accuracy.
[0038] In this case, the method for forming the pattern on the resist upper layer film is preferably a method for forming a pattern by photolithography with a wavelength of 10 nm or more and 300 nm or less, direct drawing with an electron beam, nanoimprinting, or a combination of these.
[0039] When the above-mentioned method is used as a method for forming a circuit pattern on the resist upper layer film, a fine pattern can be formed on the workpiece with higher accuracy.
[0040] In this case, the development method in the pattern forming method is preferably alkaline development or development using an organic solvent.
[0041] When alkaline development or development using an organic solvent is used as the development method, a fine pattern can be formed on the workpiece with higher accuracy.
[0042] In this case, it is preferable to use, as the workpiece, a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.
[0043] In the present invention, the above-mentioned materials can be used as the workpiece.
[0044] In this case, the metal is preferably silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, cobalt, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, manganese, molybdenum, ruthenium, or an alloy thereof.
[0045] The above metals can be used.
[0046] The present invention also provides a compound for organic films, which is represented by the following general formula (1): [ka] (In the formula, W1 is an n1-valent organic group containing an aromatic ring, and L is a substituent on the aromatic ring, which is L1, L2, or both, represented by the following general formula (2). When the total number of substituents L on the aromatic ring is n1, the number of L1 is x, and the number of L2 is y, the relationships x+y=n1, 2≦n1≦8, 0≦y≦8, and 0≦x≦8 are satisfied.) [ka] (In the formula, n2 represents an integer of 1 to 3, R1 represents any of the following formulas (3), and R2 represents any of the following general formulas (4).) [ka] [ka] (In the formula, R3 is any one of the following formulas (5), n3 represents 0 or 1, and n4 represents 1 or 2.) [ka]
[0047] Such a compound for an organic film not only has excellent heat resistance and filling and flattening properties for a pattern formed on a substrate, but can also be used as an organic film-forming material capable of forming an organic film having good film-forming properties and adhesion to a substrate. Effect of the Invention
[0048] As described above, the organic film-forming material of the present invention has various properties such as heat resistance and filling / flattening properties, and is useful for forming an organic film that can be formed without depending on the substrate to be processed.Therefore, it is extremely useful as an organic film-forming material in a multi-layer resist process such as a two-layer resist process, a three-layer resist process using a silicon-containing resist underlayer film, or a four-layer resist process using a silicon-containing resist intermediate film and an organic anti-reflective film, or as a flattening material for manufacturing a semiconductor device.In addition, the pattern forming method of the present invention can form a fine pattern on a substrate to be processed with high accuracy in a multi-layer resist process.
[0049] The compound for organic film of the present invention represented by the above general formula (1) has excellent heat resistance and thermosetting properties, and therefore the compound alone can be used as an organic film material. Since the compound has excellent thermal fluidity, when the organic film is used as a resist underlayer film, it also has excellent filling / planarization properties for a pattern substrate. In addition, since the molecule contains an amide structure, it is possible to improve not only heat resistance, but also adhesion to the substrate and film-forming properties. Also, by introducing an alkylene group between the amide structure and the aromatic ring, crystallinity is reduced, improving not only thermal fluidity but also film-forming properties. Furthermore, by appropriately selecting the main skeleton represented by W1, it is possible to adjust various physical properties, such as optical properties and etching resistance, according to the required performance when using an organic film as a resist underlayer film. [Brief description of the drawings]
[0050] [Figure 1] FIG. 2 is an explanatory diagram of an example of a pattern forming method using a three-layer resist process of the present invention. [Diagram 2] FIG. 2 is an explanatory diagram of a method for evaluating embedding characteristics in an embodiment. [Diagram 3] FIG. 4 is an explanatory diagram of a method for evaluating flattening characteristics in an embodiment. [Figure 4] FIG. 2 is an explanatory diagram of a method for measuring adhesion in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0051] As described above, in the fine patterning process using a multilayer resist method in the manufacturing process of semiconductor device, there has been a demand for an organic film-forming material capable of forming an organic film with excellent film-forming properties and flatness even on a substrate to be processed having a portion that is particularly difficult to flatten, such as a wide trench structure, a pattern formation method using the same, and a compound for an organic film.
[0052] The present inventors have discovered that an organic film-forming material using a compound having a specific substituent on an aromatic ring according to the present invention is useful for forming an organic film having excellent filling / planarization properties, and have thus completed the present invention.
[0053] That is, the present invention relates to an organic film-forming material, which contains a compound for an organic film represented by the following general formula (1) and an organic solvent. [ka] (In the formula, W1 is an n1-valent organic group containing an aromatic ring, and L is a substituent on the aromatic ring, which is L1, L2, or both, represented by the following general formula (2). When the total number of substituents L on the aromatic ring is n1, the number of L1 is x, and the number of L2 is y, the relationships x+y=n1, 2≦n1≦8, 0≦y≦8, and 0≦x≦8 are satisfied.) [ka] (In the formula, n2 represents an integer of 1 to 3, R1 represents any of the following formulas (3), and R2 represents any of the following general formulas (4).) [ka] [ka] (In the formula, R3 is any one of the following formulas (5), n3 represents 0 or 1, and n4 represents 1 or 2.) [ka]
[0054] The present invention will be described in detail below, but the present invention is not limited thereto.
[0055] <Organic film forming material> The organic film-forming material of the present invention contains an organic film compound represented by the following general formula (1) and an organic solvent. Each component contained in the organic film-forming material of the present invention will be described in detail below.
[0056] <Compounds for organic films> The compound for organic films of the present invention is represented by the following general formula (1). [ka] (In the formula, W1 is an n1-valent organic group containing an aromatic ring, and L is a substituent on the aromatic ring, which is L1, L2, or both, represented by the following general formula (2). When the total number of substituents L on the aromatic ring is n1, the number of L1 is x, and the number of L2 is y, the relationships x+y=n1, 2≦n1≦8, 0≦y≦8, and 0≦x≦8 are satisfied.) [ka] (In the formula, n2 represents an integer of 1 to 3, R1 represents any of the following formulas (3), and R2 represents any of the following general formulas (4).) [ka] [ka] (In the formula, R3 is any one of the following formulas (5), n3 represents 0 or 1, and n4 represents 1 or 2.) [ka]
[0057] W1 in the above general formula (1) is an n1-valent organic group containing an aromatic ring, and specific examples thereof include the structures shown below. These aromatic rings may have a substituent other than L, and examples thereof include an alkyl group having 1 to 10 carbon atoms, an alkynyl or alkenyl group having 3 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, a nitro group, a halogen group, a nitrile group, a sulfonyl group, an alkoxycarbonyl group having 2 to 10 carbon atoms, and an alkanoyloxy group having 2 to 10 carbon atoms.
[0058] [ka]
[0059] [ka]
[0060] [ka]
[0061] [ka]
[0062] [ka]
[0063] [ka]
[0064] [ka]
[0065] [ka]
[0066] [ka]
[0067] [ka]
[0068] The total number n1 of the substituents L on the aromatic ring of the compound for an organic film represented by the general formula (1) preferably satisfies 3≦n1≦6.
[0069] Furthermore, the structural formula of the above general formula (1) represented by W1 and L is preferably a structural formula represented by the following general formula (8), that is, the substituent L on the aromatic ring is a substituent of the aromatic ring bonded to W2 via an ether bond as shown below. W2 is an n6-valent organic group, n5 represents 1 or 2, and n6 represents an integer of 1 to 3. In this case, n1, which is the number of substituents of the substituent L on the aromatic ring in the above general formula (1), is the product of n5 and n6, and satisfies the relationship of 3≦n5×n6≦6. In this way, by making the linking group with W2 a substituent on the aromatic ring via an ether bond, it is possible to impart thermal fluidity without impairing heat resistance. [ka]
[0070] W2 in the above general formula (8) is preferably as follows: Such a structure is preferred from the viewpoint of easy availability of raw materials. [ka] (In the formula, the dashed lines represent bonds.)
[0071] The substituent L on the aromatic ring shown in the above general formula (2), L1 or L2, is composed of a substituent containing R1 and R2 via an oxygen atom or a nitrogen atom, and the structure of the substituent after the oxygen atom of L1 is the same as that after the nitrogen atom of L2. If the terminal group structure having this same structure is conveniently designated as R4, L1 and L2 can be shown as shown in the following general formula (9). [ka] (In the formula, R1, R2, and n2 are the same as above.)
[0072] Examples of R4 in L1 and L2 in the above general formula (9) include the following structures. The alkylene chain linked between the bond in R4 and the amide bond is a linking group that contributes to fluidity and film-forming properties, and is combined with the curing properties of the crosslinking group having an unsaturated bond at the end to provide flatness and fluidity. By introducing an alkylene group, even if the skeleton represented by W1 is made into a rigid structure, it is possible to alleviate crystallinity and provide thermal fluidity and film-forming properties. Among these, those having n2=1 and a propargyl group or an ethynyl group are preferred from the viewpoint of heat resistance, and those having a tertiary amide structure in which R1 is not a hydrogen atom, that is, R1 and R2 have a substituent other than a hydrogen atom, are even more preferred from the viewpoint of thermal fluidity and complete solubility in solvents (in the following formula, n2 is the same as above, and the dashed lines indicate bonds to oxygen and nitrogen atoms).
[0073] [ka]
[0074] [ka]
[0075] [ka]
[0076] It is preferable that L1 and L2 constituting the substituent L on the aromatic ring of the compound for organic thin film represented by the general formula (1) are represented by the following general formula (6). From the viewpoint of the synthesis of the compound and the heat resistance of the obtained compound, it is preferable that it is as follows. [ka] (In the formula, R1 and R2 are the same as above.)
[0077] It is preferable that R1 and R2 in L1 and L2 constituting the substituent L on the aromatic ring of the organic film compound represented by the general formula (1) are any of the combinations represented by the following general formula (7). By using such a combination, an organic film having excellent heat resistance and a good balance of thermosetting property and thermal fluidity can be formed. [ka] (In the formula, R3 and n4 are the same as above.)
[0078] Furthermore, the substituents R1 and R2 on L1 and L2 constituting the aromatic ring group substituent L can be used in combination with a plurality of structures. Specifically, as shown in the production method, it is possible to adjust the ratio of the substituents R1 and R2 on L1 and L2 at any ratio by using a combination of reagents that introduce a plurality of terminal groups.
[0079] In addition, the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn in terms of polystyrene as measured by gel permeation chromatography of the organic film compound represented by the above general formula (1) is preferably 1.00≦Mw / Mn≦1.15, and more preferably 1.00≦Mw / Mn≦1.10. By definition, if it is a monomolecular compound, Mw / Mn is 1.00, but due to the separation property of the gel permeation chromatography method, the measured value may exceed 1.00. Generally, it is extremely difficult for a polymer having a repeating unit to approach Mw / Mn=1.00 unless a special polymerization method is used, and the polymer has a distribution of Mw and the Mw / Mn value exceeds 1. In the present invention, 1.00≦Mw / Mn≦1.15 is defined as an index indicating monomolecularity in order to distinguish between monomolecular compounds and polymers. In addition, when a compound having a plurality of terminal group structures is used as described above, the above range of Mw / Mn is set because the compound has a distribution of Mw / Mn unlike a single compound. Even in this case, the Mw / Mn distribution does not become large, unlike polymers.
[0080] By controlling the Mw / Mn of the compound for the organic film within such a range, an organic film having excellent filling properties and flatness can be formed.
[0081] Depending on the combination of substituents introduced into the compound for organic films of the present invention, it is possible to impart thermosetting properties, thermal fluidity, and adhesion, and therefore, by using the compound for organic films of the present invention, it is possible to form organic films that are excellent in heat resistance, filling / planarization properties, film-forming properties, and the like.
[0082] [Method of manufacturing organic film compounds] As an example of a method for producing the organic film compound represented by the general formula (1) of the present invention, a method of obtaining the compound by a substitution reaction using a base catalyst between a compound (modifying agent) having R1 and R2 as substituents having a leaving group X shown below and a compound having a hydroxyl group on an aromatic ring, so-called phenols, or a compound having an amino group as a substituent on an aromatic ring, so-called anilines, etc., can be exemplified. In the reaction used in STEP 1 and STEP 2, it is possible to use one or more raw materials, which can be appropriately selected and combined according to the required properties. In the following formula, R1, R2, W1, n1, and n2 are the same as above, and X represents a halogen atom, a tosylate group, or a mesylate group.
[0083] [Phenols (STEP 1)] [ka]
[0084] [Anilines (STEP 2)] [ka]
[0085] Furthermore, when both hydroxyl groups and amino groups are present on the aromatic ring, the number of substituents in the raw material can be adjusted so that the relationship x+y=n1, 2≦n1≦8, 0≦x≦8, 0≦y≦8 is satisfied, where x is the number of hydroxyl groups and y is the number of amino groups (Pattern 1). In addition, the hydroxyl or amino groups on the aromatic ring can be reacted with multiple modifying agents in any ratio, allowing the introduction rate of the substituents on the hydroxyl or amino groups to be controlled in any ratio. As an example, 1aand R 2a , R 1b and R 2b If the substituents have different combinations, R 1a , R 2a The ratio of the substituents having a is a%, R 1b , R 2b When the introduction rate of the substituent having the formula (I) is b%, the introduction rate can be controlled at any rate so that a+b=100% (Pattern 2, Pattern 3). This allows the introduction rate to be controlled even when the hydroxyl group and amino group are simultaneously present as in Pattern 1, and furthermore, even when three or more types of modifying agents are used, the introduction rate can be controlled at any rate so that the introduction rate of the substituent is 100%. In the following formula, W1, R1, and R2 are the same as above, and x and y are integers that satisfy x+y=n1. R 1a and R 2a , R 1b and R 2b is either R1 or R2, but R 1a ≠R 1b , R 2a ≠R 2b The relationship is satisfied. R included in n1 1a , R 2a The proportion of substituents is a%, R 1b , R 2b If the proportion of substituents is b%, then a+b=100% is satisfied, and n 1a is n1×a÷100, n 1b represents n1 × b ÷ 100, where n 1a +n 1b =n1 relationship is satisfied.
[0086] [Pattern 1] [ka]
[0087] [Pattern 2] [ka]
[0088] [Pattern 3] [ka]
[0089] Examples of the base catalyst for the substitution reaction shown above include inorganic base compounds such as sodium hydrogen carbonate, sodium carbonate, potassium carbonate, calcium carbonate, cesium carbonate, sodium hydroxide, potassium hydroxide, sodium hydride, and potassium phosphate, and organic amine compounds such as triethylamine, pyridine, and N-methylmorpholine, which may be used alone or in combination of two or more. The amount of the catalyst used is in the range of 0.1 to 20 mol, preferably 0.2 to 10 mol, relative to the hydroxyl or amino group which is the substituent of the raw material.
[0090] The solvent used in this case is not particularly limited as long as it is inert to the above reaction, but for example, ether solvents such as diethyl ether, tetrahydrofuran, dioxane, etc., aromatic solvents such as benzene, toluene, xylene, etc., acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, N-methylpyrrolidone, water, etc., can be used alone or in combination. These solvents can be used in the range of 0 to 2,000 parts by mass per 100 parts by mass of the reaction raw materials, and the reaction temperature is preferably from -50°C to the boiling point of the solvent, more preferably from room temperature to 150°C. The reaction time is appropriately selected from 0.1 to 100 hours.
[0091] The reaction method includes a method of charging phenols or anilines and a modifying agent in a solvent all at once, a method of dropping phenols or anilines and a modifying agent separately or mixed and dispersed or dissolved, and a method of dropping one of phenols or anilines and a modifying agent dispersed or dissolved in a solvent and charging it. In addition, when multiple types of phenols or anilines and a modifying agent are charged, they can be mixed and reacted in advance, or reacted individually and sequentially. In the case of using a catalyst, the phenols or anilines and the modifying agent can be charged all at once, or the catalyst can be dispersed or dissolved in advance and then dropped. After the reaction is completed, the unreacted raw materials and catalysts present in the system can be removed by diluting with an organic solvent, and then crystallizing with a separation wash or poor solvent to obtain a powder. In addition, after diluting with an organic solvent, the solvent can be replaced with a desired organic solvent and recovered as a solution. Furthermore, after recovery as a powder by crystallization or the like, it can also be dissolved in a desired organic solvent and recovered as a solution.
[0092] The organic solvent used for the liquid separation washing is not particularly limited as long as it can dissolve the target substance and separate into two layers even when mixed with water, but examples thereof include hydrocarbons such as hexane, heptane, benzene, toluene, and xylene, esters such as ethyl acetate, n-butyl acetate, and propylene glycol methyl ether acetate, ketones such as methyl ethyl ketone, methyl amyl ketone, cyclohexanone, and methyl isobutyl ketone, ethers such as diethyl ether, diisopropyl ether, methyl-t-butyl ether, and ethylcyclopentyl methyl ether, chlorine-based solvents such as methylene chloride, chloroform, dichloroethane, and trichloroethylene, and mixtures thereof. The washing water used in this case is usually what is called deionized water or ultrapure water. The number of washings may be one or more times, but since washing 10 or more times does not necessarily provide the effect of washing, it is preferably about 1 to 5 times.
[0093] In order to remove acidic components in the system during separation washing, washing may be performed with a basic aqueous solution. Specific examples of the base include alkali metal hydroxides, alkali metal carbonates, alkaline earth metal hydroxides, alkaline earth metal carbonates, ammonia, and organic ammonium.
[0094] Furthermore, in order to remove metal impurities or base components in the system during separation washing, washing with an acidic aqueous solution may be performed. Specific examples of the acid include inorganic acids such as hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, phosphoric acid, and heteropolyacids, and organic acids such as oxalic acid, fumaric acid, maleic acid, trifluoroacetic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and trifluoromethanesulfonic acid.
[0095] The above-mentioned separation washing with a basic aqueous solution and an acidic aqueous solution may be performed either alone or in combination. From the viewpoint of removing metal impurities, the separation washing is preferably performed in the order of a basic aqueous solution and an acidic aqueous solution.
[0096] After the above-mentioned separation washing with the basic aqueous solution or acidic aqueous solution, washing with neutral water may be performed successively. The number of washings may be one or more times, but is preferably about 1 to 5 times. As the neutral water, the above-mentioned deionized water or ultrapure water may be used. The number of washings may be one or more times, but if the number of washings is too few, the basic components and acidic components may not be removed. Even if washing is performed 10 times or more, the effect of washing alone may not be obtained, so it is preferably about 1 to 5 times.
[0097] Furthermore, the reaction product after the liquid separation operation can be recovered as a powder by concentrating the solvent to dryness or crystallizing it under reduced pressure or normal pressure, but it can also be left in a solution state of a moderate concentration in order to improve operability when preparing an organic film-forming material. The concentration at this time is preferably 0.1 to 50 mass%, more preferably 0.5 to 30 mass%. At such a concentration, the viscosity is unlikely to increase, so operability is not impaired, and the amount of solvent is not excessive, so it is economical.
[0098] The solvent used in this case is not particularly limited as long as it can dissolve the organic film compound, and specific examples include ketones such as cyclohexanone and methyl-2-amyl ketone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol; ethers such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, and diethylene glycol dimethyl ether; and esters such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, and propylene glycol mono-tert-butyl ether acetate. These can be used alone or in combination of two or more.
[0099] In preparing the organic film compound used in the organic film-forming material obtained by this method, various modifying agents can be used alone or in combination according to the required performance, as described above. For example, those having a side chain structure that contributes to improving planarization characteristics, and an aromatic ring structure that contributes to etching resistance and heat resistance, etc., can be combined in any ratio. Therefore, organic film-forming materials using these organic film compounds can achieve a high level of compatibility not only with filling / planarization characteristics and film-forming properties, but also with etching resistance and optical properties.
[0100] As described above, the compound for organic film of the present invention provides an organic film-forming material capable of exhibiting excellent filling / planarization characteristics and film-forming properties.
[0101] The compounds for organic films according to the present invention may be used singly or in combination of two or more.
[0102] [Organic solvents] The organic solvent usable in the organic film-forming material of the present invention is not particularly limited as long as it dissolves the organic film compound of the present invention, as well as optional components such as surfactants, plasticizers, acid generators, crosslinking agents, and other additives. Specifically, organic solvents with a boiling point of less than 180° C., such as those described in paragraphs
[0091] to
[0092] of JP-A-2007-199653, can be used. Among them, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, 2-heptanone, cyclopentanone, cyclohexanone, and mixtures of two or more of these are preferably used.
[0103] Such an organic film-forming material can be applied by spin coating, and since it contains the compound for an organic film of the present invention as described above, it is an organic film-forming material that has both heat resistance and high-level filling / planarization properties.
[0104] Furthermore, in the organic film forming material of the present invention, it is possible to add a high boiling point solvent having a boiling point of 180° C. or more to the organic solvent having a boiling point of less than 180° C. (a mixture of an organic solvent having a boiling point of less than 180° C. and an organic solvent having a boiling point of 180° C. or more). The high boiling point organic solvent is not particularly limited as long as it can dissolve the organic film compound and optional components such as surfactant, plasticizer, acid generator, crosslinking agent, and other additives, and ...3-Hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerin, n-nonyl acetate, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, diethylene glycol monoethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol monoisobutyl ether, diethylene glycol monohexyl ether, diethylene glycol monophenyl ether, diethylene glycol monobenzyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, triethylene glycol monomethyl ether, triethylene glycol-n-butyl ether, triethylene glycol butyl methyl ether, triethylene Glycol diacetate, tetraethylene glycol dimethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, tripropylene glycol mono-n-propyl ether, tripropylene glycol mono-n-butyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, triacetin, propylene glycol diacetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol methyl-n-propyl ether, dipropylene glycol methyl ether acetate, 1,4-butanediol diacetate, 1,3-butylene glycol diacetate, 1,Examples of the monomer include 6-hexanediol diacetate, triethylene glycol diacetate, γ-butyrolactone, dihexyl malonate, diethyl succinate, dipropyl succinate, dibutyl succinate, dihexyl succinate, dimethyl adipate, diethyl adipate, and dibutyl adipate, and these may be used alone or in combination.
[0105] The boiling point of the high boiling point solvent may be appropriately selected according to the temperature at which the organic film-forming material is heat-treated, and the boiling point of the high boiling point solvent to be added is preferably 180°C to 300°C, and more preferably 200°C to 300°C. If the boiling point is too low, there is no risk of the solvent volatilizing too quickly during baking (heat treatment), and sufficient thermal fluidity can be obtained. In addition, if the boiling point is too high, there is no risk of the solvent remaining in the film after baking without volatilizing, and therefore there is no risk of adversely affecting the film properties such as etching resistance.
[0106] Furthermore, when the high boiling point solvent is used, the blending amount of the high boiling point solvent is preferably 1 to 30 parts by mass per 100 parts by mass of the organic solvent having a boiling point of less than 180° C. If the blending amount is such, there is no risk that the blending amount is too small to impart sufficient thermal fluidity during baking, or that the blending amount is too large to remain in the film, leading to deterioration of film properties such as etching resistance.
[0107] In the case of such an organic film-forming material, by imparting thermal fluidity to the above-mentioned organic film compound by adding a high boiling point solvent, the organic film-forming material becomes one having both high-level filling and planarizing properties.
[0108] In the present invention, it is preferable that the organic film-forming material further contains at least one of a surfactant and a plasticizer.
[0109] [Surfactants] A surfactant can be added to the organic film-forming material of the present invention in order to improve the coating property in spin coating. For example, the surfactants described in paragraphs
[0142] to
[0147] of JP 2009-269953 A can be used.
[0110] The surfactants may be used alone or in combination of two or more. The amount of the surfactant added is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the compound for organic film.
[0111] [Plasticizer] In addition, a plasticizer can be added to the organic film-forming material of the present invention in order to further improve the flattening / filling properties. The plasticizer is not particularly limited, and various known plasticizers can be widely used. Examples include low molecular weight compounds such as phthalates, adipic esters, phosphates, trimellitates, and citrates, polyethers, polyesters, and polymers such as polyacetal polymers described in JP-A-2013-253227. When a plasticizer is added, the amount of the plasticizer is preferably 1 to 100 parts by mass, more preferably 5 to 30 parts by mass, based on 100 parts by mass of the organic film compound.
[0112] In addition, in the organic film-forming material of the present invention, as an additive for imparting filling / flattening properties in the same manner as a plasticizer, for example, a liquid additive having a polyethylene glycol or polypropylene glycol structure, or a thermally decomposable polymer having a weight loss rate of 40% by mass or more between 30°C and 250°C and a weight average molecular weight of 300 to 200,000 is preferably used. This thermally decomposable polymer preferably contains a repeating unit having an acetal structure represented by the following general formula (DP1) or (DP1a). When these thermally decomposable polymers are added, the amount of addition is preferably 1 to 100 parts by mass, more preferably 5 to 30 parts by mass, relative to 100 parts by mass of the compound for organic film.
[0113] [ka] (In the formula, R a is a hydrogen atom or an optionally substituted saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms. L is a saturated or unsaturated divalent organic group having 2 to 30 carbon atoms.
[0114] [ka] (In the formula, R b is an alkyl group having 1 to 4 carbon atoms. Z is a saturated or unsaturated divalent hydrocarbon group having 4 to 10 carbon atoms, which may have an ether bond. t represents the average number of repeating units and is 3 to 500.
[0115] Furthermore, the following flowability promoters can be used as additives for improving the filling / flattening properties as described above. As the flowability promoter, one or more compounds selected from the following general formulas (i) to (iii) can be used. When these flowability promoters are added, the amount added is preferably 1 to 100 parts by mass, more preferably 5 to 30 parts by mass, based on 100 parts by mass of the compound for organic film.
[0116] [ka] (In the formula, R c are each independently a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms which may be substituted. a W is a phenylene group or a divalent group represented by the following general formula (i-1). b , W c is a single bond or a divalent group represented by the following formula (i-2): a is an integer from 1 to 10, and n a is an integer between 0 and 5.) [ka] (In the formula, * indicates a bond position, and R d , R e , Rf , R g is a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms. d , W e Each of m is independently a single bond or a carbonyl group. b , m c is an integer from 0 to 10, and m b +m c ≧1.) [ka] (In the formula, * indicates the bond position.)
[0117] [ka] (In the formula, R h are each independently a hydrogen atom or an optionally substituted organic group having 1 to 10 carbon atoms. f W is a divalent group represented by the following general formula (ii-1). g is a single bond or a divalent group represented by the following formula (ii-2): d is an integer from 2 to 10, and n b is an integer between 0 and 5.) [ka] (In the formula, * indicates a bond position, and R i , R j , R k , R l is a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms. e , m f is an integer from 0 to 10, and m e +m f ≧1.) [ka] (In the formula, * indicates the bond position.)
[0118] [ka] (In the formula, R m, R n R is a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms which may be substituted, and may be bonded to each other to form a cyclic structure. o , R p is an organic group having 1 to 10 carbon atoms, R o is a group containing either an aromatic ring or a divalent group represented by the following general formula (iii-1): g , W h is a single bond or a divalent group represented by the following formula (iii-2), and at least one of them is a divalent group represented by the following formula (iii-2). [ka] (In the formula, * indicates a bond position, and W i is an organic group having 1 to 4 carbon atoms. [ka] (In the formula, * indicates the bond position.)
[0119] [Acid generator] In the organic film-forming material of the present invention, an acid generator can be added to further promote the curing reaction. The acid generator may be one that generates an acid by thermal decomposition or one that generates an acid by light irradiation, and either one can be added. Specifically, the materials described in paragraphs
[0061] to
[0085] of JP-A-2007-199653 can be added, but are not limited thereto.
[0120] The acid generators can be used alone or in combination of two or more. The amount of the acid generator added is preferably 0.05 to 50 parts by mass, more preferably 0.1 to 10 parts by mass, based on 100 parts by mass of the compound for organic film.
[0121] [Crosslinking agent] In addition, a crosslinking agent can be added to the organic film-forming material of the present invention in order to enhance the curing property and further suppress intermixing with the resist upper layer film. The crosslinking agent is not particularly limited, and various known crosslinking agents can be widely used. Examples include melamine-based crosslinking agents, glycoluril-based crosslinking agents, benzoguanamine-based crosslinking agents, urea-based crosslinking agents, β-hydroxyalkylamide-based crosslinking agents, isocyanurate-based crosslinking agents, aziridine-based crosslinking agents, oxazoline-based crosslinking agents, epoxy-based crosslinking agents, and polynuclear phenol-based crosslinking agents.
[0122] Specific examples of the melamine-based crosslinking agent include hexamethoxymethylated melamine, hexabutoxymethylated melamine, alkoxy- and / or hydroxy-substituted products thereof, and partial self-condensates thereof. Specific examples of glycoluril crosslinking agents include tetramethoxymethylated glycoluril, tetrabutoxymethylated glycoluril, alkoxy and / or hydroxy substituted products thereof, and partial self-condensates thereof. Specific examples of benzoguanamine-based crosslinking agents include tetramethoxymethylated benzoguanamine, tetrabutoxymethylated benzoguanamine, alkoxy- and / or hydroxy-substituted products thereof, and partial self-condensates thereof. Specific examples of the urea-based crosslinking agent include dimethoxymethylated dimethoxyethyleneurea, its alkoxy and / or hydroxyl substituted derivatives, and partial self-condensates thereof. A specific example of the β-hydroxyalkylamide crosslinking agent is N,N,N',N'-tetra(2-hydroxyethyl)adipamide. Specific examples of the isocyanurate crosslinking agent include triglycidyl isocyanurate and triallyl isocyanurate. Specific examples of the aziridine crosslinking agent include 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane and 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate]. Specific examples of the oxazoline-based crosslinking agent include 2,2'-isopropylidenebis(4-benzyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-methylenebis4,5-diphenyl-2-oxazoline, 2,2'-methylenebis-4-phenyl-2-oxazoline, 2,2'-methylenebis-4-tertbutyl-2-oxazoline, 2,2'-bis(2-oxazoline), 1,3-phenylenebis(2-oxazoline), 1,4-phenylenebis(2-oxazoline), and 2-isopropenyloxazoline copolymer. Specific examples of epoxy crosslinking agents include diglycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, poly(glycidyl methacrylate), trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol tetraglycidyl ether.
[0123] Specific examples of polynuclear phenol-based crosslinking agents include compounds represented by the following general formula (1A). [ka] (In the formula, Q is a single bond or a hydrocarbon group having 1 to 20 carbon atoms and a valence of s. 10 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. s is an integer of 1 to 5.
[0124] Q is a single bond or a hydrocarbon group having 1 to 20 carbon atoms and a valence of s. s is an integer of 1 to 5, and is more preferably 2 or 3. Specific examples of Q include groups in which q hydrogen atoms have been removed from methane, ethane, propane, butane, isobutane, pentane, cyclopentane, hexane, cyclohexane, methylpentane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, benzene, toluene, xylene, ethylbenzene, ethylisopropylbenzene, diisopropylbenzene, methylnaphthalene, ethylnaphthalene, and eicosane. R10 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Specific examples of the alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a pentyl group, an isopentyl group, a hexyl group, an octyl group, an ethylhexyl group, a decyl group, and an eicosanyl group, and a hydrogen atom or a methyl group is preferable.
[0125] Specific examples of the compound represented by the above general formula (1A) include the following compounds. Among these, from the viewpoint of improving the curability and thickness uniformity of the organic film, hexamethoxymethylated products of triphenolmethane, triphenolethane, 1,1,1-tris(4-hydroxyphenyl)ethane, and tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene are preferred. In the formula, R 10 is the same as above. [ka]
[0126] [ka]
[0127] The crosslinking agent may be used alone or in combination of two or more. The amount of the crosslinking agent added is preferably 1 to 100 parts by mass, more preferably 5 to 50 parts by mass, based on 100 parts by mass of the compound for organic film.
[0128] [Other ingredients] The organic film-forming material of the present invention can also be blended with other compounds or polymers. The blending compounds or blending polymers are mixed with the organic film-forming material of the present invention to improve the film-forming properties of spin coating and the filling properties of substrates having steps.
[0129] Such materials include phenol, o-cresol, m-cresol, p-cresol, 2,3-dimethylphenol, 2,5-dimethylphenol, 3,4-dimethylphenol, 3,5-dimethylphenol, 2,4-dimethylphenol, 2,6-dimethylphenol, 2,3,5-trimethylphenol, 3,4,5-trimethylphenol, 2-tert-butylphenol, 3-tert-butylphenol, 4-tert-butylphenol, 2-phenylphenol, 3-phenylphenol, 4-phenylphenol, 3,5-diphenylphenol, Phenylphenol, 2-naphthylphenol, 3-naphthylphenol, 4-naphthylphenol, 4-tritylphenol, resorcinol, 2-methylresorcinol, 4-methylresorcinol, 5-methylresorcinol, catechol, 4-tert-butylcatechol, 2-methoxyphenol, 3-methoxyphenol, 2-propylphenol, 3-propylphenol, 4-propylphenol, 2-isopropylphenol, 3-isopropylphenol, 4-isopropylphenol, 2-methoxy-5-methylphenol, 2-t ert-Butyl-5-methylphenol, pyrogallol, thymol, isothymol, 4,4'-(9H-fluoren-9-ylidene)bisphenol, 2,2'-dimethyl-4,4'-(9H-fluoren-9-ylidene)bisphenol, 2,2'-diallyl-4,4'-(9H-fluoren-9-ylidene)bisphenol, 2,2'-difluoro-4,4'-(9H-fluoren-9-ylidene)bisphenol, 2,2'-diphenyl-4,4'-(9H-fluoren-9-ylidene)bisphenol, 2,2'-dimethoxy-4,4'-(9H -fluoren-9-ylidene)bisphenol, 2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 3,3,3',3'-tetramethyl-2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 3,3,3',3',4,4'-hexamethyl-2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 2,3,2',3'-tetrahydro-(1,1')-spirobiindene-5,5'-diol, 5,5'-dimethyl-3,3,3',3'-tetramethyl-2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 1-naphthol, 2-naphthol, 2-methyl-1-naphthol, 4-methoxy-1-naphthol, 7-methoxy-2-naphthol, dihydroxynaphthalenes such as 1,5-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, and 2,6-dihydroxynaphthalene, 3-hydroxynaphthalene-2-methyl carboxylate, indene, hydroxyindene, benzofuran, hydroxyanthracene, acenaphthylene, and biphenyl. Examples of the novolak resins include bisphenol, trisphenol, dicyclopentadiene, tetrahydroindene, 4-vinylcyclohexene, norbornadiene, 5-vinylnorborn-2-ene, α-pinene, β-pinene, and limonene; polyhydroxystyrene, polystyrene, polyvinylnaphthalene, polyvinylanthracene, polyvinylcarbazole, polyindene, polyacenaphthylene, polynorbornene, polycyclodecene, polytetracyclododecene, polynortricyclene, poly(meth)acrylate, and copolymers thereof. In addition, naphthol dicyclopentadiene copolymers described in JP-A-2004-205685, fluorene bisphenol novolac resins described in JP-A-2005-128509, acenaphthylene copolymers described in JP-A-2005-250434, fullerenes having phenol groups described in JP-A-2006-227391, bisphenol compounds and novolac resins described in JP-A-2006-293298, adamantanephenol compounds and novolac resins described in JP-A-2006-285095, bisnaphthol compounds and novolac resins described in JP-A-2010-122656, and fullerene resin compounds described in JP-A-2008-158002 can also be blended.
[0130] The blending amount of the above-mentioned blending compound or blending polymer is preferably 0 to 1,000 parts by mass, and more preferably 0 to 500 parts by mass, based on 100 parts by mass of the above-mentioned organic film compound.
[0131] The organic film-forming material can be used as an organic film material or a planarizing material for manufacturing semiconductor devices.
[0132] In addition, the organic film-forming material of the present invention is extremely useful as an organic film material for multilayer resist processes, such as a two-layer resist process, a three-layer resist process using a silicon-containing resist intermediate film, and a four-layer resist process using a silicon-containing inorganic hard mask intermediate film and an organic antireflective film.
[0133] <Organic film formation method> Furthermore, the organic film forming material described above can be used to form an organic film that functions as an organic film for a multi-layer resist film used in lithography or a planarizing film for semiconductor manufacturing.
[0134] In the organic film forming method using the organic film forming material of the present invention, the organic film forming material can be coated on a substrate (workpiece) to be processed by spin coating or the like. By using spin coating or the like, good embedding properties can be obtained. After spin coating, the organic solvent is evaporated, and baking (heat treatment) is performed to promote a crosslinking reaction in order to prevent mixing with the resist upper layer film or the resist intermediate film. The baking is preferably performed at 100°C or higher and 600°C or lower for 10 to 600 seconds, more preferably at 200°C or higher and 500°C or lower for 10 to 300 seconds. Considering the influence on device damage and wafer deformation, the upper limit of the heating temperature in the wafer process of lithography is preferably 600°C or lower, more preferably 500°C or lower.
[0135] In addition, in a method for forming an organic film using the organic film forming material of the present invention, the organic film forming material of the present invention can be coated on a substrate to be processed by a spin coating method or the like as described above, and the organic film forming material can be baked and hardened in an atmosphere having an oxygen concentration of 0.1% or more and 21% or less to form an organic film.
[0136] By baking the organic film-forming material of the present invention in such an oxygen atmosphere, a sufficiently hardened organic film can be obtained. Although the atmosphere during baking may be air, it is preferable to seal in an inert gas such as N2, Ar, or He to reduce oxygen in order to prevent oxidation of the organic film. In order to prevent oxidation, it is necessary to control the oxygen concentration, which is preferably 1,000 ppm or less, and more preferably 100 ppm or less. Preventing oxidation of the organic film during baking is preferable because it prevents the absorption from increasing and the etching resistance from decreasing.
[0137] Such an organic film forming method using the organic film forming material of the present invention can obtain a flat cured film regardless of the unevenness of the substrate to be processed due to its excellent filling / planarizing properties, and is therefore extremely useful when forming a flat organic film on a substrate to be processed having structures or steps with a height of 30 nm or more.
[0138] The thickness of this organic film or the organic film such as a planarizing film for manufacturing a semiconductor device may be appropriately selected, but is preferably 30 to 20,000 nm, and more preferably 50 to 15,000 nm.
[0139] <Pattern formation method> In the present invention, a method for forming a pattern by a three-layer resist process using such an organic film-forming material is a method for forming a pattern on a substrate to be processed, which includes at least the following steps: forming an organic film on a workpiece using the organic film-forming material described above; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming a resist upper layer film on the silicon-containing resist intermediate film using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask; a pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask; Furthermore, the present invention provides a pattern forming method in which the workpiece is etched using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
[0140] Since the silicon-containing resist intermediate film in the above three-layer resist process exhibits resistance to etching by oxygen gas or hydrogen gas, it is preferable that the dry etching of the organic film in the above three-layer resist process is performed using the silicon-containing resist intermediate film as a mask, using an etching gas mainly composed of oxygen gas or hydrogen gas.
[0141] As the silicon-containing resist intermediate film in the above three-layer resist process, a polysiloxane-based intermediate film is also preferably used. By imparting an anti-reflection effect to the silicon-containing resist intermediate film, reflection can be suppressed. In particular, for 193 nm exposure, if a material containing many aromatic groups and having high etching selectivity with the substrate is used as the organic film, the k value becomes high and the substrate reflection becomes high, but by imparting absorption to the silicon-containing resist intermediate film to obtain an appropriate k value, it becomes possible to suppress reflection, and the substrate reflection can be reduced to 0.5% or less. As the silicon-containing resist intermediate film having an anti-reflection effect, anthracene is preferably used for 248 nm and 157 nm exposure, and polysiloxane with a pendant light-absorbing group having a phenyl group or a silicon-silicon bond and crosslinked by acid or heat is preferably used for 193 nm exposure.
[0142] The present invention is also suitable as a four-layer resist process using an organic anti-reflective film, in which case, at least, a method for forming a pattern on a workpiece, comprising the steps of: forming an organic film on a workpiece using the organic film-forming material described above; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming an organic antireflective coating (BARC) on the silicon-containing resist intermediate film; forming a resist top layer film on the BARC using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; The pattern is transferred to the BARC and the silicon-containing resist intermediate film by etching using the resist top layer film on which the pattern is formed as a mask; a pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask; Furthermore, the present invention provides a pattern forming method in which the workpiece is etched using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
[0143] In addition, an inorganic hard mask intermediate film may be formed instead of the silicon-containing resist intermediate film. In this case, the method for forming a pattern on a workpiece includes at least the following steps: forming an organic film on a workpiece using the organic film-forming material described above; forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film; forming a resist upper layer film on the inorganic hard mask intermediate film using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the inorganic hard mask intermediate film by etching using the resist upper layer film on which the pattern is formed as a mask; The pattern is transferred to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask; Furthermore, the present invention provides a pattern forming method in which the workpiece is etched using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
[0144] As described above, when forming an inorganic hard mask intermediate film on an organic film, a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film (SiON film) can be formed by a CVD method, an ALD method, or the like. For example, methods for forming a silicon nitride film are described in JP-A-2002-334869 and WO-A-2004 / 066377. The thickness of the inorganic hard mask intermediate film is preferably 5 to 200 nm, more preferably 10 to 100 nm. In addition, a SiON film, which has a high effect as an anti-reflection film, is most preferably used as the inorganic hard mask intermediate film. Since the substrate temperature when forming the SiON film is 300 to 500°C, the organic film needs to withstand a temperature of 300 to 500°C. The organic film forming material used in the present invention has high heat resistance and can withstand high temperatures of 300 to 500°C, so it is possible to combine an inorganic hard mask intermediate film formed by a CVD method or an ALD method with an organic film formed by a spin coating method.
[0145] The present invention is also suitable as a four-layer resist process using an organic anti-reflective film, in which case, at least, a method for forming a pattern on a workpiece, comprising the steps of: forming an organic film on a workpiece using the organic film-forming material described above; forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film; forming an organic antireflective coating (BARC) on the inorganic hard mask intermediate film; forming a resist top layer film on the BARC using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; The pattern is transferred to the BARC and the inorganic hard mask intermediate film by etching using the resist top layer film on which the pattern is formed as a mask; The pattern is transferred to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask; Furthermore, the present invention provides a pattern forming method in which the workpiece is etched using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
[0146] As described above, a photoresist film may be formed on the inorganic hard mask intermediate film as a resist top layer, but an organic anti-reflective coating (BARC) may be formed on the inorganic hard mask intermediate film by spin coating, and a photoresist film may be formed on top of that. In particular, when a SiON film is used as the inorganic hard mask intermediate film, the two-layer anti-reflective coating of the SiON film and the BARC makes it possible to suppress reflection even in immersion exposure with a high NA exceeding 1.0. Another advantage of forming the BARC is that it has the effect of reducing the tailing of the photoresist pattern directly above the SiON film.
[0147] The resist top layer film in the above three-layer resist process may be either positive or negative, and may be the same as a commonly used photoresist composition. After spin-coating the photoresist composition, pre-baking is performed, preferably at 60 to 180°C for 10 to 300 seconds. Thereafter, exposure is performed according to a conventional method, followed by post-exposure baking (PEB) and development to obtain a resist pattern. The thickness of the resist top layer film is not particularly limited, but is preferably 30 to 500 nm, and more preferably 50 to 400 nm.
[0148] Examples of the exposure light include high energy rays with a wavelength of 300 nm or less, specifically, excimer lasers with wavelengths of 248 nm, 193 nm, and 157 nm, soft X-rays with wavelengths of 3 to 20 nm, electron beams, and X-rays.
[0149] The method for forming a pattern on the resist upper layer film is preferably a method for forming a pattern by photolithography with a wavelength of 10 nm or more and 300 nm or less, direct writing with an electron beam, nanoimprinting, or a combination of these.
[0150] In the pattern forming method, the development method is preferably alkaline development or development using an organic solvent.
[0151] Next, etching is performed using the obtained resist upper layer film pattern as a mask. In the three-layer resist process, etching of the silicon-containing resist intermediate film or the inorganic hard mask intermediate film is performed using a fluorocarbon gas as a mask. This forms a silicon-containing resist intermediate film pattern or an inorganic hard mask intermediate film pattern.
[0152] Next, the organic film is etched using the obtained silicon-containing resist intermediate film pattern or inorganic hard mask intermediate film pattern as a mask.
[0153] The next step, etching of the substrate (workpiece) can also be done by standard methods; for example, if the substrate is a SiO2, SiN, or silica-based low dielectric constant insulating film, etching is done mainly with fluorocarbon gases, while for p-Si, Al, or W, etching is done mainly with chlorine- or bromine-based gases. When etching the substrate with fluorocarbon gases, the silicon-containing resist intermediate film pattern in the three-layer resist process is stripped at the same time as the substrate is processed. When etching the substrate with chlorine- or bromine-based gases, the silicon-containing resist intermediate film pattern must be stripped by separate dry etching with fluorocarbon gases after substrate processing.
[0154] The organic film obtained by using the organic film-forming material of the present invention is characterized by excellent etching resistance when etching the substrate to be processed.
[0155] As the workpiece, it is preferable to use a semiconductor device substrate, or the semiconductor device substrate on which any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film is formed. More specifically, although not limited to, a substrate such as Si, α-Si, p-Si, SiO2, SiN, SiON, W, TiN, Al, or the like, or the substrate on which the above-mentioned metal film or the like is formed as a workpiece layer, may be used.
[0156] As the processed layer, various low-k films such as Si, SiO2, SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, Al-Si, and their stopper films are used, and can be formed to a thickness of usually 50 to 10,000 nm, particularly 100 to 5,000 nm. When forming the processed layer, the substrate and the processed layer are made of different materials.
[0157] As the metal, it is preferable to use silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, cobalt, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, manganese, molybdenum, ruthenium, or an alloy thereof.
[0158] In addition, it is preferable to use a substrate having a structure or steps with a height of 30 nm or more as the substrate to be processed.
[0159] An example of a three-layer resist process is specifically shown below with reference to Figure 1. In the case of the three-layer resist process, as shown in Figure 1(A), an organic film 3 is formed on a processable layer 2 laminated on a substrate 1 using the organic film-forming material of the present invention, and then a silicon-containing resist intermediate film 4 is formed thereon, and a resist upper layer film 5 is formed thereon.
[0160] Next, as shown in FIG. 1(B), a desired portion 6 of the resist top layer film 5 is exposed, and PEB and development are performed to form a resist top layer film pattern 5a as shown in FIG. 1(C). Using the obtained resist top layer film pattern 5a as a mask, the silicon-containing resist intermediate film 4 is etched using a CF-based gas to form a silicon-containing resist intermediate film pattern 4a as shown in FIG. 1(D). After removing the resist top layer film pattern 5a, the organic film 3 is oxygen plasma etched using the obtained silicon-containing resist intermediate film pattern 4a as a mask to form an organic film pattern 3a as shown in FIG. 1(E). Furthermore, after removing the silicon-containing resist intermediate film pattern 4a, the processed layer 2 is etched using the organic film pattern 3a as a mask to form a pattern 2a as shown in FIG. 1(F).
[0161] When an inorganic hard mask intermediate film is used, the silicon-containing resist intermediate film 4 is the inorganic hard mask intermediate film, and when a BARC is laid down, the BARC is provided between the silicon-containing resist intermediate film 4 and the resist top layer film 5. The etching of the BARC may be performed consecutively prior to the etching of the silicon-containing resist intermediate film 4, or the etching of the silicon-containing resist intermediate film 4 may be performed by changing the etching device after etching only the BARC.
[0162] As described above, the pattern forming method of the present invention makes it possible to form a fine pattern on a substrate to be processed with high precision in a multi-layer resist process. EXAMPLES
[0163] The present invention will be described in more detail below with reference to Synthesis Examples, Examples, and Comparative Examples, but the present invention is not limited thereto. Note that, as for the molecular weight and dispersity, the weight average molecular weight (Mw) and number average molecular weight (Mn) in terms of polystyrene were determined by gel permeation chromatography (GPC) using tetrahydrofuran as an eluent, and the dispersity (Mw / Mn) was determined.
[0164] Synthesis Examples Synthesis of organic film compounds (A1) to (A25) and comparative compounds (R1) to (R3)
[0165] The compounds (A1) to (A25) for organic films were synthesized using the compounds (B1) to (B12) having amino groups and hydroxyl groups, and the modifying agents (C1) to (C8) shown below. The compound (R3) for comparison was synthesized using the raw material compound (D1) for comparison.
[0166] Compounds with amino and hydroxyl groups: [ka]
[0167] Modifiers: [ka]
[0168] Compound raw materials for comparative examples: [ka]
[0169] (Synthesis Example 1) Synthesis of organic membrane compound (A1) [ka] In a nitrogen atmosphere, 10.0 g of compound (B1), 38.5 g of potassium carbonate, and 140 g of DMF (dimethylformamide) were added to prepare a homogeneous dispersion at an internal temperature of 50°C. A solution of 45.8 g of modifying agent (C1) and 180 g of DMF mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 500 g of MIBK (methyl isobutyl ketone) and 500 g of pure water were added to prepare a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 200 g of 3.0% aqueous nitric acid solution and five times with 200 g of pure water, and the organic layer was dried under reduced pressure. 110 g of THF was added to the residue to prepare a homogeneous solution, and then dropped into 700 g of hexane to crystallize. The crystallized crystals were separated by filtration, washed twice with 200 g of hexane, and collected. The collected crystals were dried in a vacuum at 70°C to obtain organic membrane compound (A1). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A1): Mw = 840, Mw / Mn = 1.02
[0170] (Synthesis Example 2) Synthesis of organic membrane compound (A2) [ka] In a nitrogen atmosphere, 10.0 g of compound (B1), 38.5 g of potassium carbonate, and 140 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 67.5 g of modifying agent (C5) and 270 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 500 g of MIBK and 500 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 200 g of 3.0% aqueous nitric acid solution and five times with 200 g of pure water, and the organic layer was dried under reduced pressure. 170 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 1000 g of methanol to crystallize. The crystals that were crystallized were separated by filtration, washed twice with 300 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A2). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A2): Mw = 1,200, Mw / Mn = 1.01
[0171] (Synthesis Example 3) Synthesis of organic membrane compound (A3) [ka] In a nitrogen atmosphere, 10.0 g of compound (B2), 14.2 g of potassium carbonate, and 75 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 22.3 g of modifying agent (C2) and 70 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 300 g of MIBK and 300 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 100 g of 3.0% aqueous nitric acid solution and five times with 100 g of pure water, and the organic layer was dried under reduced pressure. 70 g of THF was added to the residue to obtain a homogeneous solution, and then dropped into 400 g of hexane to crystallize. The crystallized crystals were separated by filtration, washed twice with 100 g of hexane, and collected. The collected crystals were dried in a vacuum at 70°C to obtain an organic membrane compound (A3). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A3): Mw=710, Mw / Mn=1.01
[0172] (Synthesis Example 4) Synthesis of organic membrane compound (A4) [ka] In a nitrogen atmosphere, 10.0 g of compound (B2), 14.2 g of potassium carbonate, and 75 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 24.8 g of modifying agent (C5) and 75 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 300 g of MIBK and 300 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 100 g of 3.0% aqueous nitric acid solution and five times with 100 g of pure water, and the organic layer was dried under reduced pressure. 80 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 500 g of methanol to crystallize. The crystallized crystals were separated by filtration, washed twice with 100 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A4). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A4): Mw=780, Mw / Mn=1.02
[0173] (Synthesis Example 5) Synthesis of organic membrane compound (A5) [ka] In a nitrogen atmosphere, 10.0 g of compound (B3), 20.8 g of potassium carbonate, and 120 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 31.9 g of modifying agent (C3) and 100 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 300 g of MIBK and 300 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 100 g of 3.0% aqueous nitric acid solution and five times with 100 g of pure water, and the organic layer was dried under reduced pressure. 90 g of THF was added to the residue to obtain a homogeneous solution, and then dropped into 550 g of hexane to crystallize. The crystallized crystals were separated by filtration, washed twice with 100 g of hexane, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A5). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A5): Mw = 1,260, Mw / Mn = 1.02
[0174] (Synthesis Example 6) Synthesis of organic membrane compound (A6) [ka] In a nitrogen atmosphere, 10.0 g of compound (B3), 20.8 g of potassium carbonate, and 120 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 42.0 g of modifying agent (C6) and 130 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 400 g of MIBK and 400 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 120 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 600 g of methanol to crystallize. The crystallized crystals were separated by filtration, washed twice with 150 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A6). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A6): Mw=1,630, Mw / Mn=1.01
[0175] (Synthesis Example 7) Synthesis of organic membrane compound (A7) [ka] In a nitrogen atmosphere, 10.0 g of compound (B4), 16.2 g of potassium carbonate, and 80 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 24.9 g of modifying agent (C3) and 75 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 200 g of MIBK and 200 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 100 g of 3.0% aqueous nitric acid solution and five times with 100 g of pure water, and the organic layer was dried under reduced pressure. 75 g of THF was added to the residue to obtain a homogeneous solution, and then dropped into 400 g of hexane to crystallize. The crystallized crystals were separated by filtration, washed twice with 100 g of hexane, and collected. The collected crystals were dried in a vacuum at 70°C to obtain an organic membrane compound (A7). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A7): Mw=890, Mw / Mn=1.01
[0176] (Synthesis Example 8) Synthesis of organic membrane compound (A8) [ka] In a nitrogen atmosphere, 10.0 g of compound (B4), 16.2 g of potassium carbonate, and 80 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 29.0 g of modifying agent (C4) and 90 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 200 g of MIBK and 200 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 100 g of 3.0% aqueous nitric acid solution and five times with 100 g of pure water, and the organic layer was dried under reduced pressure. 90 g of THF was added to the residue to obtain a homogeneous solution, and then dropped into 450 g of hexane to crystallize. The crystallized crystals were separated by filtration, washed twice with 100 g of hexane, and collected. The collected crystals were dried in a vacuum at 70°C to obtain an organic membrane compound (A8). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A8): Mw=980, Mw / Mn=1.02
[0177] (Synthesis Example 9) Synthesis of organic membrane compound (A9) [ka] In a nitrogen atmosphere, 10.0 g of compound (B5), 11.5 g of potassium carbonate, and 60 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 18.0 g of modifying agent (C2) and 75 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 200 g of MIBK and 200 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 100 g of 3.0% aqueous nitric acid solution and five times with 100 g of pure water, and the organic layer was dried under reduced pressure. 65 g of THF was added to the residue to obtain a homogeneous solution, and then dropped into 400 g of hexane to crystallize. The crystallized crystals were separated by filtration, washed twice with 100 g of hexane, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A9). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A9): Mw = 1,080, Mw / Mn = 1.02
[0178] (Synthesis Example 10) Synthesis of organic membrane compound (A10) [ka] In a nitrogen atmosphere, 10.0 g of compound (B5), 11.5 g of potassium carbonate, and 60 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 29.2 g of modifying agent (C7) and 90 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 300 g of MIBK and 200 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 100 g of 3.0% aqueous nitric acid solution and five times with 100 g of pure water, and the organic layer was dried under reduced pressure. 90 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 400 g of methanol to crystallize. The crystals that were crystallized were separated by filtration, washed twice with 100 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A10). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A10): Mw = 1,540, Mw / Mn = 1.03
[0179] (Synthesis Example 11) Synthesis of organic membrane compound (A11) [ka] In a nitrogen atmosphere, 10.0 g of compound (B6), 21.8 g of potassium carbonate, and 100 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 33.4 g of modifying agent (C3) and 130 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 400 g of MIBK and 300 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to obtain a homogeneous solution, and then dropped into 400 g of hexane to crystallize. The crystallized crystals were separated by filtration, washed twice with 100 g of hexane, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A11). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A11): Mw = 1,220, Mw / Mn = 1.03
[0180] (Synthesis Example 12) Synthesis of organic membrane compound (A12) [ka] In a nitrogen atmosphere, 10.0 g of compound (B6), 21.8 g of potassium carbonate, and 100 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 54.0 g of modifying agent (C8) and 160 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 400 g of MIBK and 300 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 140 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 500 g of methanol to crystallize. The crystals that were crystallized were separated by filtration, washed twice with 200 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A12). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A12): Mw = 1,920, Mw / Mn = 1.03
[0181] (Synthesis Example 13) Synthesis of organic membrane compound (A13) [ka] In a nitrogen atmosphere, 10.0 g of compound (B7), 27.8 g of potassium carbonate, and 120 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 43.6 g of modifying agent (C2) and 130 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 400 g of MIBK and 400 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 110 g of THF was added to the residue to obtain a homogeneous solution, and then dropped into 500 g of hexane to crystallize. The crystallized crystals were separated by filtration, washed twice with 150 g of hexane, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A13). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A13): Mw = 1,550, Mw / Mn = 1.01
[0182] (Synthesis Example 14) Synthesis of organic membrane compound (A14) [ka] In a nitrogen atmosphere, 10.0 g of compound (B7), 27.8 g of potassium carbonate, and 120 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 56.1 g of modifying agent (C6) and 170 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 500 g of MIBK and 400 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 140 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 600 g of methanol to crystallize. The crystallized crystals were separated by filtration, washed twice with 150 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A14). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A14): Mw = 1,900, Mw / Mn = 1.02
[0183] (Synthesis Example 15) Synthesis of organic membrane compound (A15) [ka] In a nitrogen atmosphere, 10.0 g of compound (B8), 26.7 g of potassium carbonate, and 130 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 68.0 g of modifying agent (C7) and 200 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 500 g of MIBK and 400 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 170 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 1000 g of methanol to crystallize. The crystallized crystals were separated by filtration, washed twice with 300 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A15). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A15): Mw = 2,450, Mw / Mn = 1.02
[0184] (Synthesis Example 16) Synthesis of organic membrane compound (A16) [ka] In a nitrogen atmosphere, 10.0 g of compound (B8), 26.7 g of potassium carbonate, and 130 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 66.0 g of modifying agent (C8) and 200 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 500 g of MIBK and 400 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 170 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 1000 g of methanol to crystallize. The crystals that were crystallized were separated by filtration, washed twice with 300 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A16). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A16): Mw = 2,380, Mw / Mn = 1.03
[0185] (Synthesis Example 17) Synthesis of organic membrane compound (A17) [ka] In a nitrogen atmosphere, 10.0 g of compound (B9), 19.7 g of potassium carbonate, and 90 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 30.9 g of modifying agent (C2) and 90 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 200 g of MIBK and 200 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 100 g of 3.0% aqueous nitric acid solution and five times with 100 g of pure water, and the organic layer was dried under reduced pressure. 90 g of THF was added to the residue to obtain a homogeneous solution, and then dropped into 400 g of hexane to crystallize. The crystallized crystals were separated by filtration, washed twice with 100 g of hexane, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A17). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A17): Mw = 1,730, Mw / Mn = 1.01
[0186] (Synthesis Example 18) Synthesis of organic membrane compound (A18) [ka] In a nitrogen atmosphere, 10.0 g of compound (B9), 19.7 g of potassium carbonate, and 90 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 34.4 g of modifying agent (C5) and 100 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 200 g of MIBK and 200 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 100 g of 3.0% aqueous nitric acid solution and five times with 100 g of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 400 g of methanol to crystallize. The crystallized crystals were separated by filtration, washed twice with 100 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A18). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A18): Mw = 1,880, Mw / Mn = 1.02
[0187] (Synthesis Example 19) Synthesis of organic membrane compound (A19) [ka] In a nitrogen atmosphere, 10.0 g of compound (B10), 37.3 g of potassium carbonate, and 150 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 57.2 g of modifying agent (C3) and 170 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 400 g of MIBK and 400 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 140 g of THF was added to the residue to obtain a homogeneous solution, and then dropped into 600 g of hexane to crystallize. The crystallized crystals were separated by filtration, washed twice with 200 g of hexane, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A19). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A19): Mw = 2,050, Mw / Mn = 1.03
[0188] (Synthesis Example 20) Synthesis of organic membrane compound (A20) [ka] In a nitrogen atmosphere, 10.0 g of compound (B10), 37.3 g of potassium carbonate, and 150 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 65.3 g of modifying agent (C5) and 200 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 500 g of MIBK (methyl isobutyl ketone) and 500 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 160 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 1,000 g of methanol to crystallize. The crystallized crystals were separated by filtration, washed twice with 300 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A20). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A20): Mw = 2,460, Mw / Mn = 1.02
[0189] (Synthesis Example 21) Synthesis of organic membrane compound (A21) [ka] In a nitrogen atmosphere, 10.0 g of compound (B11), 27.2 g of potassium carbonate, and 110 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 42.7 g of modifying agent (C2) and 130 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 400 g of MIBK and 400 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 110 g of THF was added to the residue to obtain a homogeneous solution, and then dropped into 500 g of hexane to crystallize. The crystallized crystals were separated by filtration, washed twice with 200 g of hexane, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A21). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A21): Mw = 2,310, Mw / Mn = 1.03
[0190] (Synthesis Example 22) Synthesis of organic membrane compound (A22) [ka] In a nitrogen atmosphere, 10.0 g of compound (B11), 27.2 g of potassium carbonate, and 110 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 54.9 g of modifying agent (C6) and 160 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 500 g of MIBK and 500 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 140 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 600 g of methanol to crystallize. The crystals that were crystallized were separated by filtration, washed twice with 200 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A22). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A22): Mw = 2,940, Mw / Mn = 1.02
[0191] (Synthesis Example 23) Synthesis of organic membrane compound (A23) [ka] In a nitrogen atmosphere, 10.0 g of compound (B12), 22.3 g of potassium carbonate, and 100 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 34.3 g of modifying agent (C3) and 110 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 400 g of MIBK and 300 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to obtain a homogeneous solution, and then dropped into 500 g of hexane to crystallize. The crystallized crystals were separated by filtration, washed twice with 200 g of hexane, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A23). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A23): Mw = 2,360, Mw / Mn = 1.03
[0192] (Synthesis Example 24) Synthesis of organic membrane compound (A24) [ka] In a nitrogen atmosphere, 10.0 g of compound (B12), 22.3 g of potassium carbonate, and 100 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 39.1 g of modifying agent (C5) and 120 g of DMF were mixed and homogenized in advance was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 400 g of MIBK and 300 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 110 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 500 g of methanol to crystallize. The crystallized crystals were separated by filtration, washed twice with 200 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain a compound for organic membranes (A24). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A24): Mw = 2,840, Mw / Mn = 1.04
[0193] (Synthesis Example 25) Synthesis of organic membrane compound (A25) [ka] In a nitrogen atmosphere, 10.0 g of compound (B11), 27.2 g of potassium carbonate, and 110 g of DMF were added to obtain a homogeneous dispersion at an internal temperature of 50°C. A solution in which 16.7 g of modifying agent (C3) and 50 g of DMF were mixed and homogenized in advance was slowly dropped, and the mixture was reacted at an internal temperature of 50°C for 8 hours. A solution in which 23.8 g of decorating agent (C5) and 75 g of DMF were mixed and homogenized in advance was slowly dropped, and the mixture was reacted for another 16 hours. After cooling to room temperature, 500 g of MIBK (methyl isobutyl ketone) and 500 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 150 g of 3.0% aqueous nitric acid solution and five times with 150 g of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to obtain a homogeneous solution, and then the solution was dropped into 500 g of hexane to crystallize. The crystals were separated by filtration, washed twice with 200 g of hexane, and collected. The collected crystals were dried in vacuum at 70° C. to obtain a compound for organic membranes (A25). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A25): Mw = 1,830, Mw / Mn = 1.09
[0194] (Comparative Synthesis Example 1) Synthesis of Comparative Compound (R1) [ka] Under a nitrogen atmosphere, 13.7 g of m-ethynylaniline, 13.3 g of triethylamine, and 150 g of THF were stirred at room temperature to obtain a homogeneous solution. 10 g of THF and 10.0 g of cyanuric acid chloride were mixed in advance to obtain a homogeneous solution, which was slowly added dropwise, and the reaction was carried out under reflux for 5 hours. After cooling to room temperature, 150 g of methyl isobutyl ketone and 100 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 50 g of 3.0% aqueous nitric acid solution and five times with 50 g of pure water, and the organic layer was dried under reduced pressure. 60 g of THF was added to the residue to obtain a homogeneous solution, and then crystals were crystallized with 200 g of hexane. The crystallized crystals were separated by filtration, washed twice with 100 g, and collected. The collected crystals were dried in a vacuum at 70 ° C to obtain a comparative compound (R1). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (R1): Mw=430, Mw / Mn=1.01
[0195] (Comparative Synthesis Example 2) Synthesis of Comparative Compound (R2) [ka] Under a nitrogen atmosphere, 13.7 g of m-ethynylaniline, 13.3 g of triethylamine, and 150 g of THF were stirred in an ice bath to obtain a homogeneous solution. 10 g of THF and 10.0 g of trimesic acid chloride were mixed in advance to obtain a homogeneous solution, which was slowly dropped and reacted in an ice bath for 1 hour and at room temperature for 3 hours. After cooling to room temperature, 150 g of methyl isobutyl ketone and 100 g of pure water were added to obtain a homogeneous solution, and the water layer was removed. The organic layer was further washed twice with 50 g of 3.0% aqueous nitric acid solution and five times with 50 g of pure water, and the organic layer was dried under reduced pressure. 60 g of THF was added to the residue to obtain a homogeneous solution, and then crystals were crystallized with 200 g of methanol. The crystallized crystals were separated by filtration, washed twice with 100 g of methanol, and collected. The collected crystals were dried in a vacuum at 70 ° C to obtain a comparative compound (R2). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (R2): Mw=520, Mw / Mn=1.01
[0196] (Comparison synthesis 3) Synthesis of Comparative Compound (R3) [ka] Under a nitrogen atmosphere, 10.00 g of the raw material compound for comparison (D1), 4.76 g of potassium carbonate, and 50 g of DMF were made into a uniform dispersion at an internal temperature of 50 ° C. under a nitrogen atmosphere. 3.72 g of propargyl bromide was slowly dropped, and the reaction was carried out at an internal temperature of 50 ° C. for 16 hours. After cooling to room temperature, 100 g of methyl isobutyl ketone and 50 g of pure water were added to make a uniform solution, and then the water layer was removed. The organic layer was further washed twice with 30 g of 3.0% aqueous nitric acid solution and five times with 30 g of pure water, and the organic layer was dried under reduced pressure. 30 g of THF was added to the residue, and crystals were crystallized with 100 g of methanol. The crystallized crystals were separated by filtration, washed twice with 60 g of methanol, and collected. The collected crystals were dried in a vacuum at 70 ° C. to obtain a compound for comparison (R3). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (R3): Mw=960, Mw / Mn=1.07
[0197] Tables 1 to 4 show the results of Mw and Mw / Mn of the organic film compounds (A1) to (A25) and the comparative compounds (R1) to (R3) used in the examples.
[0198] [Table 1]
[0199] [Table 2]
[0200] [Table 3]
[0201] [Table 4]
[0202] Preparation of organic film-forming materials (UDL-1 to 29, comparative UDL-1 to 3) The above organic film compounds (A1) to (A25), comparative compounds (R1) to (R3), and high boiling point solvents (S1) 1,6-diacetoxyhexane: boiling point 260°C, (S2) tripropylene glycol monomethyl ether: boiling point 242°C were used, and propylene glycol monomethyl ether acetate (PGMEA) containing 0.1 mass% of PF-6320 (manufactured by Omnova) was used to dissolve them in the proportions shown in Table 5, and filtered through a 0.1 μm fluororesin filter to prepare organic film-forming materials (UDL-1 to 29, comparative UDL-1 to 3).
[0203] [Table 5]
[0204] Example 1 Solvent Resistance Measurement (Examples 1-1 to 1-29, Comparative Examples 1-1 to 1-3) The UDL-1 to 29 and comparative UDL-1 to 3 prepared above were applied onto a silicon substrate and baked in air at the temperature shown in Table 6 for 60 seconds, after which the film thickness was measured, PGMEA solvent was dispensed onto the substrate, left for 30 seconds, spin-dried, and baked at 100°C for 60 seconds to evaporate the PGMEA, and the film thickness was measured before and after the PGMEA treatment. The remaining film ratio was calculated using the film thickness a after film formation and the film thickness b after the PGMEA treatment. The results are shown in Table 6. [Table 6]
[0205] As shown in Table 6, the organic films using the organic film compound of the present invention (Examples 1-1 to 1-29) had a residual film rate of 99.5% or more after PGMEA treatment, and it is understood that a crosslinking reaction occurs by heat treatment, thereby exhibiting sufficient solvent resistance.
[0206] Example 2 Evaluation of heat resistance characteristics (Examples 2-1 to 2-29, Comparative Examples 2-1 to 2-3) The above organic film-forming materials (UDL-1 to 29, Comparative UDL-1 to 3) were each coated on a silicon substrate and baked in air at the temperature shown in Table 7 for 60 seconds to form a 200 nm coating film, and the film thickness a was measured. This substrate was further baked at 400°C for an additional 20 minutes in a nitrogen stream with an oxygen concentration controlled to 0.2% or less, and the film thickness b was measured. The remaining film ratio was calculated using the film thickness a after baking and the film thickness b after baking. These results are shown in Table 7. [Table 7]
[0207] As shown in Table 7, the organic films (Examples 2-1 to 2-29) using the organic film compound of the present invention showed less than 5% film thickness loss even after long-term baking at 400°C, demonstrating that the organic film-forming material of the present invention has excellent heat resistance. In particular, the compound having the structure represented by the general formula (2) where n2=1 and a propargyl group or an ethynyl group is introduced retains a film remaining rate of 98% or more, demonstrating particularly excellent heat resistance.
[0208] Example 3: Evaluation of filling characteristics (Examples 3-1 to 3-29, Comparative Examples 3-1 to 3-3) The organic film-forming materials (UDL-1 to 29, Comparative UDL-1 to 3) prepared above were each applied onto a SiO2 wafer substrate having a dense hole pattern (hole diameter 0.16 μm, hole depth 0.50 μm, distance between the centers of two adjacent holes 0.32 μm) and baked in air at the temperature shown in Table 8 for 60 seconds to form an organic film. The substrate used was a base substrate 7 (SiO2 wafer substrate) having a dense hole pattern as shown in Figure 2 (G) (overhead view) and (H) (cross-sectional view). The film-forming properties and filling properties of each of the obtained wafer substrates were evaluated.
[0209] The film-forming properties were evaluated as good when no dewetting was observed for each wafer obtained, and as poor when dewetting was observed. The filling properties were evaluated by observing the cross-sectional shape using a scanning electron microscope (SEM) to confirm whether the holes were filled with organic film 8 without any voids (air gaps) inside the holes. The results are shown in Table 8. In this evaluation, when an organic film material with good filling properties was used, the organic film was filled without voids inside the holes as shown in Figure 2 (I), and the evaluation was good. When an organic film material with poor filling properties was used, voids occurred inside the holes, and the evaluation was poor.
[0210] [Table 8]
[0211] As shown in Examples 3-1 to 3-29 in Table 8, when the organic film compound of the present invention was used, it was found that all of the organic film forming materials could be formed on a SiO2 wafer substrate having the above-mentioned dense hole pattern, and could fill the hole pattern without voids, and had excellent filling properties. In addition, Comparative Example 3-3 could also be formed on the above-mentioned substrate, and could fill the hole pattern without voids. On the other hand, Comparative Example 3-1 did not have an amide structure, and Comparative Example 3-2 had a structure having no alkylene group between the amide structure and the aromatic ring, so the film forming properties were poor, and film formation failure (dewetting) occurred on the substrate. It is considered that the structures of the compounds used in these organic film forming materials both have high thermal fluidity, but because they do not have an amide structure, the adhesion to the substrate is weak, or because they do not have an alkylene group between the amide structure and the aromatic ring, the crystallinity is high, and the cohesion is strong, causing the above-mentioned film formation failure.
[0212] Example 4: Evaluation of planarization characteristics (Examples 4-1 to 4-29, Comparative Examples 4-1 to 4-3) The organic film forming materials (UDL-1 to 29, comparative UDL-1 to 3) prepared above were each applied onto a base substrate 9 (SiO2 wafer substrate) having a giant isolated trench pattern (trench width 50 μm, trench depth 0.115 μm) shown in FIG. 3(J), baked in air at the temperature shown in Table 9 for 60 seconds, and the step (delta 10) of the organic film 10 between the trench portion and the non-trench portion shown in FIG. 3(K) was observed using KLA-TENCOR Alpha-Step D-600 (contact profiler). The results are shown in Table 9. In this evaluation, the step was evaluated as S when it was less than 60 nm, A when it was 60 nm or more and less than 80 nm, B when it was 80 nm or more and less than 100 nm, C when it was 100 nm or more and less than 115 nm, and D when it was 115 nm or more. In this evaluation, it can be said that the smaller the step, the better the flattening characteristics. In this evaluation, a trench pattern with a depth of 0.115 μm was planarized using an organic film forming material with a normal film thickness of about 0.2 μm, which is a strict evaluation condition for evaluating the superiority or inferiority of the planarization characteristics.
[0213] [Table 9]
[0214] As shown in Examples 4-1 to 4-29 in Table 9, when the organic film compound of the present invention is used, all organic film forming materials have excellent film forming properties compared to Comparative Examples 4-1 to 4-2, and the step between the organic film of the trench part and the non-trench part is small compared to Comparative Example 4-3, and it can be seen that the planarization characteristics are excellent. In particular, the compound having an ether bond as shown in the general formula (8) and the compound having a tertiary amide structure have excellent thermal fluidity, and therefore the planarization characteristics of the organic film material containing the compound having both of these characteristics were the best. In addition, the organic film forming material containing a high boiling point solvent was given thermal fluidity, and therefore had better planarization characteristics than the organic film material not containing a high boiling point solvent (Examples 4-26 to 4-29). On the other hand, in Comparative Examples 4-1 and 4-2, film formation failure (dewetting) occurred on the giant isolated trench pattern substrate, which is considered to be the same reason as the film formation failure occurred on the SiO2 wafer substrate having the dense hole pattern. Moreover, the compound of Comparative Example 4-3 had poor thermal fluidity and thus had poor planarization characteristics.
[0215] Example 5 Adhesion Test (Examples 5-1 to 5-29, Comparative Examples 5-1 to 5-3) The organic film-forming materials (UDL-1 to 29, Comparative UDL-1 to 3) were applied onto a SiO2 wafer substrate and baked for 60 seconds in air at the temperatures listed in Table 10 using a hot plate to form an organic film with a thickness of 200 nm. The wafer with the organic film was cut into a 1 x 1 cm square, and aluminum pins with epoxy adhesive were attached to the cut wafers using a special tool. The aluminum pins were then attached to the substrate by heating at 150°C for 1 hour in an oven. After cooling to room temperature, the initial adhesion was evaluated by resistance using a thin film adhesion strength measuring device (Sebastian Five-A).
[0216] An explanatory diagram of the adhesion measurement method is shown in Figure 4. In Figure 4, 11 is the silicon wafer (substrate), 12 is the cured film, 13 is an aluminum pin with adhesive, 14 is the support base, 15 is the grip, and 16 indicates the tensile direction. The adhesion strength is the average value of 12 measurements, and the higher the value, the higher the adhesion of the organic film to the substrate. The adhesion was evaluated by comparing the obtained values. The results are shown in Table 10.
[0217] [Table 10]
[0218] As shown in Examples 5-1 to 5-29 in Table 10, the organic film-forming material using the organic film compound having an amide structure of the present invention showed higher adhesion than Comparative Examples 5-1 and 5-3. In addition, the compound used in Comparative ULD-2, which caused film formation failure in Comparative Examples 3-2 and 4-2, had an amide structure, so that the adhesion was equivalent to that of the organic film compound of the present invention as shown in Comparative Example 5-2. From these results, it is considered that the organic film-forming material of the present invention has excellent thermal fluidity, and at the same time, it shows excellent film-forming properties due to the high adhesion due to the amide structure and the relaxation effect of crystallinity due to the presence of an alkylene group between the amide structure and the aromatic ring.
[0219] Example 6 Pattern formation test (Examples 6-1 to 6-29, Comparative Example 6-1) The organic film forming materials (UDL-1 to 29, comparative UDL-3) were applied onto a base substrate 9 (SiO2 wafer substrate) having a giant isolated trench pattern (trench width 50 μm, trench depth 0.115 μm) shown in FIG. 3(J), and baked in air on a bare Si substrate under the conditions shown in Table 14 to form an organic film (resist underlayer film). A silicon-containing resist intermediate film material (SOG-1) was applied thereon and baked at 220° C. for 60 seconds to form a resist intermediate film with a thickness of 35 nm, and a resist upper layer film material (SL resist for ArF) was applied and baked at 105° C. for 60 seconds to form a resist upper layer film with a thickness of 100 nm. An immersion protective film (TC-1) was applied to the resist upper layer film and baked at 90° C. for 60 seconds to form a protective film with a thickness of 50 nm. It should be noted that the pattern formation test could not be carried out for Comparative UDL-1 and 2 in which film formation defects occurred in Comparative Examples 4-1 and 4-2.
[0220] The resist top layer film material (SL resist for ArF) was prepared by dissolving a polymer (RP1), an acid generator (PAG1), and a basic compound (Amine1) in a solvent containing 0.1 mass% FC-430 (manufactured by Sumitomo 3M Limited) in the ratios shown in Table 11, and filtering the solution through a 0.1 μm fluororesin filter.
[0221] [Table 11]
[0222] The structural formulae of the polymer (RP1), acid generator (PAG1), and basic compound (Amine1) used are shown below. [ka]
[0223] The immersion protective film material (TC-1) was prepared by dissolving the protective film polymer (PP1) in an organic solvent in the ratio shown in Table 12 and filtering through a 0.1 μm fluorine resin filter.
[0224] [Table 12]
[0225] The structural formula of the protective film polymer (PP1) used is shown below. [ka]
[0226] The silicon-containing resist intermediate film material (SOG-1) was prepared by dissolving the polymer represented by ArF silicon-containing intermediate film polymer (SiP1) and the thermal crosslinking catalyst (CAT1) in an organic solvent containing 0.1 mass% of FC-4430 (manufactured by Sumitomo 3M) in the ratios shown in Table 13, and filtering the solution through a fluorine resin filter having a pore size of 0.1 μm.
[0227] [Table 13]
[0228] The structural formulae of the ArF silicon-containing intermediate film polymer (SiP1) and crosslinking catalyst (CAT1) used are shown below. [ka]
[0229] Next, the resist was exposed to light using an ArF immersion exposure apparatus (Nikon Corporation; NSR-S610C, NA 1.30, σ 0.98 / 0.65, 35 degree dipole s-polarized illumination, 6% halftone phase shift mask) while changing the exposure dose, baked at 100°C for 60 seconds (PEB), and developed in a 2.38 mass% aqueous solution of tetramethylammonium hydroxide (TMAH) for 30 seconds to obtain a positive line-and-space pattern (resist upper layer film pattern) with a pitch of 100 nm and resist line widths ranging from 50 nm to 30 nm.
[0230] Next, using a Tokyo Electron etching device Telius, the resist top layer film pattern was used as a mask by dry etching to process the silicon-containing intermediate film (SOG-1 film), the organic film was used as a mask to process the SOG-1 film, and the SiO2 wafer substrate was used as a mask to process the organic film.
[0231] The etching conditions are as follows. Transfer conditions of the resist top layer film pattern onto the SOG-1 film. Chamber pressure 10.0Pa RF power: 1,500W CF4 gas flow rate: 15sccm O2 gas flow rate: 75sccm Time 15sec
[0232] Conditions for transferring SOG-1 film onto organic film. Chamber pressure 2.0Pa RF power 500W Ar gas flow rate: 75sccm O2 gas flow rate: 45sccm Time 120sec
[0233] Transfer conditions of organic film onto SiO2 wafer substrate. Chamber pressure 2.0Pa RF power: 2,200W C5F 12 Gas flow rate: 20sccm C2F6 gas flow rate: 10sccm Ar gas flow rate: 300sccm O2 gas flow rate: 60sccm Time 90sec
[0234] The cross sections of the patterns were observed using an electron microscope (S-4700) manufactured by Hitachi, Ltd., and the shapes were compared. The results are summarized in Table 14.
[0235] [Table 14]
[0236] As shown in Table 14, in the organic film-forming material of the present invention, as in the results of Examples 6-1 to 6-29, the resist upper layer film pattern was finally transferred well to the substrate in all cases, and it was confirmed that the organic film-forming material of the present invention is suitably used for microfabrication by the multilayer resist method. On the other hand, in Comparative Example 6-1, as in the results of Comparative Example 4-3, the step on the pattern substrate was large, and there were parts where the focus was shifted during exposure, so that the patterning shape of the resist upper layer film was defective, and the pattern collapsed in part during pattern processing.
[0237] From the above, it has become clear that the compound for organic films of the present invention and the organic film-forming material of the present invention containing the same have good film-forming properties and adhesion, and are excellent in filling / planarization characteristics, and are therefore extremely useful as an organic film (resist underlayer film) used in a multi-layer resist method, and that the pattern formation method of the present invention using the compound can form a fine pattern with high precision even if the workpiece is a substrate having steps.
[0238] The present specification includes the following aspects. [1]: An organic film-forming material, comprising a compound for an organic film represented by the following general formula (1) and an organic solvent: [ka] (In the formula, W1 is an n1-valent organic group containing an aromatic ring, and L is a substituent on the aromatic ring, which is L1, L2, or both, represented by the following general formula (2). When the total number of substituents L on the aromatic ring is n1, the number of L1 is x, and the number of L2 is y, the relationships x+y=n1, 2≦n1≦8, 0≦y≦8, and 0≦x≦8 are satisfied.) [ka] (In the formula, n2 represents an integer of 1 to 3, R1 represents any of the following formulas (3), and R2 represents any of the following general formulas (4).) [ka] [ka] (In the formula, R3 is any one of the following formulas (5), n3 represents 0 or 1, and n4 represents 1 or 2.) [ka] [2]: The organic film-forming material according to the above [1], characterized in that L1 and L2 constituting the substituent L on the aromatic ring of the organic film compound represented by the above general formula (1) are represented by the following general formula (6): [ka] (In the formula, R1 and R2 are the same as above.) [3]: The organic film-forming material according to the above [1] or [2], characterized in that R1 and R2 in L1 and L2 constituting the substituent L on the aromatic ring of the organic film compound represented by the above general formula (1) are any of the combinations represented by the following general formula (7). [ka] (In the formula, R3 and n4 are the same as above.) [4]: The organic film forming material according to any one of [1] to [3] above, characterized in that the total number n1 of the substituents L on the aromatic ring of the organic film compound represented by the general formula (1) satisfies 3≦n1≦6. [5]: The organic film forming material according to any one of [1] to [4] above, characterized in that the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn of the organic film compound in terms of polystyrene as determined by a gel permeation chromatography method is 1.00≦Mw / Mn≦1.15. [6]: The organic film-forming material according to any one of [1] to [5] above, characterized in that the organic solvent is a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher. [7]: The organic film-forming material according to any one of [1] to [6] above, further comprising at least one of a surfactant and a plasticizer. [8]: A method for forming a pattern on a workpiece, comprising: forming an organic film on a workpiece using any one of the organic film forming materials [1] to [7] above; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming a resist upper layer film on the silicon-containing resist intermediate film using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask; a pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask; The pattern forming method further comprises etching the workpiece using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece. [9]: A method for forming a pattern on a workpiece, comprising: forming an organic film on a workpiece using any one of the organic film forming materials [1] to [7] above; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming an organic antireflective coating (BARC) on the silicon-containing resist intermediate film; forming a resist top layer film on the BARC using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; The pattern is transferred to the BARC and the silicon-containing resist intermediate film by etching using the resist top layer film on which the pattern is formed as a mask; a pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask; The pattern forming method further comprises etching the workpiece using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
[10] : A method for forming a pattern on a workpiece, comprising: forming an organic film on a workpiece using any one of the organic film forming materials [1] to [7] above; forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film; forming a resist upper layer film on the inorganic hard mask intermediate film using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the inorganic hard mask intermediate film by etching using the resist upper layer film on which the pattern is formed as a mask; The pattern is transferred to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask; The pattern forming method further comprises etching the workpiece using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
[11] : A method for forming a pattern on a workpiece, comprising: forming an organic film on a workpiece using any one of the organic film forming materials [1] to [7] above; forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film; forming an organic antireflective coating (BARC) on the inorganic hard mask intermediate film; forming a resist top layer film on the BARC using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; The pattern is transferred to the BARC and the inorganic hard mask intermediate film by etching using the resist top layer film on which the pattern is formed as a mask; The pattern is transferred to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask; The pattern forming method further comprises etching the workpiece using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
[12] : The pattern forming method according to
[10] or
[11] above, wherein the inorganic hard mask intermediate film is formed by a CVD method or an ALD method.
[13] : The pattern formation method according to any one of [8] to
[12] above, characterized in that the pattern formation method for the resist upper layer film is a pattern formation method using photolithography, direct writing using an electron beam, nanoimprinting, or a combination thereof, with a wavelength of 10 nm or more and 300 nm or less.
[14] : The method for forming a pattern according to any one of the above [8] to
[13] , characterized in that the development method in the method for forming a pattern is alkaline development or development with an organic solvent.
[15] : The pattern formation method according to any one of [8] to
[14] above, characterized in that the workpiece is a semiconductor device substrate, or the semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.
[16] : The pattern formation method according to
[15] above, characterized in that the metal used is silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, cobalt, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, manganese, molybdenum, ruthenium, or an alloy thereof.
[17] : A compound for organic films, characterized by being represented by the following general formula (1): [ka] (In the formula, W1 is an n1-valent organic group containing an aromatic ring, and L is a substituent on the aromatic ring, which is L1, L2, or both, represented by the following general formula (2). When the total number of substituents L on the aromatic ring is n1, the number of L1 is x, and the number of L2 is y, the relationships x+y=n1, 2≦n1≦8, 0≦y≦8, and 0≦x≦8 are satisfied.) [ka] (In the formula, n2 represents an integer of 1 to 3, R1 represents any of the following formulas (3), and R2 represents any of the following general formulas (4).) [ka] [ka] (In the formula, R3 is any one of the following formulas (5), n3 represents 0 or 1, and n4 represents 1 or 2.) [ka]
[0239] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]
[0240] 1...substrate; 2...processed layer; 2a...pattern formed on the processed layer; 3...organic film, 3a...organic film pattern, 4...silicon-containing resist intermediate film, 4a...silicon-containing resist intermediate film pattern, 5...resist upper layer film, 5a...resist upper layer film pattern, 6...desired portion, 7 ... base substrate having a dense hole pattern, 8 ... organic film, 9...Base substrate having a giant isolated trench pattern; 10...Organic film; delta 10: difference in thickness between the organic film in the trench portion and the non-trench portion, 11...silicon wafer; 12...hardened film; 13...aluminum pin with adhesive; 14...support base, 15...grasp, 16...pulling direction.
Claims
1. An organic film-forming material, comprising a compound for an organic film represented by the following general formula (1) and an organic solvent: [Formula 1] (In the formula, W 1 n includes an aromatic ring 1 L is a substituent on an aromatic ring and is represented by the following general formula (2): 1 , L 2 The total number of substituents L on the aromatic ring is n 1 , L 1 Let the number of x and L be 2 When the number of is y, x + y = n 1 , 2≦n 1 ≦8, 0≦y≦8, 0≦x≦8.) [Case 2] (In the formula, n 2 represents an integer of 1 to 3; R 1 is any one of the following formulas (3), and R 2 is any one of the following general formulas (4). [C3] [C4] (In the formula, R 3 is any one of the following formulas (5), 3 represents 0 or 1, n 4 represents 1 or 2.) [C5]
2. L constituting the substituent L on the aromatic ring of the organic film compound represented by the general formula (1) 1 , L 2 The organic film-forming material according to claim 1, characterized in that is represented by the following general formula (6): [C6] (In the formula, R 1 and R 2 is the same as above.)
3. L constituting the substituent L on the aromatic ring of the organic film compound represented by the general formula (1) 1 , L 2 Inside R 1 , R 2 is any of the combinations represented by the following general formula (7): [C7] (In the formula, R 3 , n 4 is the same as above.)
4. The total number of substituents L on the aromatic ring of the organic film compound represented by the general formula (1), n 1 Where 3≦n 1 2. The organic film-forming material according to claim 1, which satisfies the condition of ≦6.
5. The organic film forming material according to claim 1, characterized in that the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn of the organic film compound in terms of polystyrene as determined by gel permeation chromatography method is 1.00≦Mw / Mn≦1.
15.
6. 2. The organic film-forming material according to claim 1, wherein the organic solvent is a mixture of one or more organic solvents having a boiling point of less than 180° C. and one or more organic solvents having a boiling point of 180° C. or higher.
7. 2. The organic film-forming material according to claim 1, further comprising at least one of a surfactant and a plasticizer.
8. A method for forming a pattern on a workpiece, comprising the steps of: forming an organic film on a workpiece by using the organic film-forming material according to any one of claims 1 to 7; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming a resist upper layer film on the silicon-containing resist intermediate film using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask; a pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask; The pattern forming method further comprises etching the workpiece using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
9. A method for forming a pattern on a workpiece, comprising the steps of: forming an organic film on a workpiece by using the organic film-forming material according to any one of claims 1 to 7; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming an organic antireflective coating (BARC) on the silicon-containing resist intermediate film; forming a resist top layer film on the BARC using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; The pattern is transferred to the BARC and the silicon-containing resist intermediate film by etching using the resist top layer film on which the pattern is formed as a mask; a pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask; The pattern forming method further comprises etching the workpiece using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
10. A method for forming a pattern on a workpiece, comprising the steps of: forming an organic film on a workpiece by using the organic film-forming material according to any one of claims 1 to 7; forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film; forming a resist upper layer film on the inorganic hard mask intermediate film using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the inorganic hard mask intermediate film by etching using the resist upper layer film on which the pattern is formed as a mask; the pattern is transferred to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask; The pattern forming method further comprises etching the workpiece using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
11. A method for forming a pattern on a workpiece, comprising the steps of: forming an organic film on a workpiece by using the organic film-forming material according to any one of claims 1 to 7; forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the organic film; forming an organic antireflective coating (BARC) on the inorganic hard mask intermediate film; forming a resist top layer film on the BARC using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; The pattern is transferred to the BARC and the inorganic hard mask intermediate film by etching using the resist top layer film on which the pattern is formed as a mask; the pattern is transferred to the organic film by etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask; The pattern forming method further comprises etching the workpiece using the organic film to which the pattern has been transferred as a mask to form a pattern on the workpiece.
12. 11. The pattern formation method according to claim 10, wherein the inorganic hard mask intermediate film is formed by a CVD method or an ALD method.
13. 9. The method for forming a pattern according to claim 8, wherein the method for forming a pattern on the resist upper layer film is a method for forming a pattern by photolithography having a wavelength of 10 nm or more and 300 nm or less, direct writing using an electron beam, nanoimprinting, or a combination thereof.
14. 9. The method for forming a pattern according to claim 8, wherein the developing method in the method for forming a pattern is alkaline development or development with an organic solvent.
15. 9. The pattern forming method according to claim 8, wherein the workpiece is a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.
16. 16. The pattern formation method according to claim 15, wherein the metal is silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, cobalt, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, manganese, molybdenum, ruthenium, or an alloy thereof.
17. A compound for organic films, characterized by being represented by the following general formula (1): [C8] (In the formula, W 1 n includes an aromatic ring 1 L is a substituent on an aromatic ring and is represented by the following general formula (2): 1 , L 2 The total number of substituents L on the aromatic ring is n 1 , L 1 Let the number of x and L be 2 When the number of is y, x + y = n 1 , 2≦n 1 ≦8, 0≦y≦8, 0≦x≦8.) [C9] (In the formula, n 2 represents an integer of 1 to 3; R 1 is any one of the following formulas (3), and R 2 is any one of the following general formulas (4). [C10] [C11] (In the formula, R 3 is any one of the following formulas (5), 3 represents 0 or 1, n 4 represents 1 or 2.) [C12]
Citation Information
Patent Citations
Crosslinkable polyphenyl ether resin, its compositions and its preparing method
CN1364821A
Calixarene derivative for sensitive material, calixarene-based composite material and sensor element and sensor using them
JP2011084487A
Organic colorant having silver gloss and coloring composition
JP2017165834A
Anthraquinone compounds used in the color filter of LCD
JP2017522407A
Material for forming organic film, substrate for manufacturing semiconductor device, method for forming organic film, patterning method, and compound for forming organic film