Monolithic refractory composition and monolithic refractory
The monolithic refractory composition with refractory aggregate, CaO·Al2O3 alumina cement, and silica sol balances curing strength and explosion resistance, enhancing work efficiency and safety.
Patent Information
- Application Number
- JP2023078197
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing monolithic refractory compositions using silica sol have lower curing strength and are prone to explosions due to rapid temperature rise, posing challenges in maintaining shape and work efficiency, and there is a trade-off between improving curing strength and explosion resistance.
A monolithic refractory composition comprising refractory aggregate, CaO·Al2O3 alumina cement, and silica sol, with specific mass ratios and solid concentrations, to enhance curing strength and explosion resistance.
The composition achieves improved curing strength and explosion resistance, allowing for rapid temperature increase and shortened construction periods.
Abstract
Description
[Technical field]
[0001] The present disclosure relates to castable refractory compositions and castable refractories. [Background technology]
[0002] Unshaped refractories are refractories that are formed through on-site construction, and generally contain alumina cement to promote hardening. However, although alumina cement has high heat resistance among cements, its heat resistance is lower than that of other refractory aggregates. In addition, alumina cement is highly reactive with slag, materials to be treated in the furnace, etc., which reduces the corrosion resistance of the refractory.
[0003] In view of the above problems, low-cement type amorphous refractories are known that reduce the alumina cement content and promote the aggregation of ultrafine powder contained in the amorphous refractory composition through a small amount of alumina cement (see, for example, Patent Documents 1 and 2).
[0004] Specifically, Patent Document 1 discloses a monolithic refractory for dry spraying, which is made by mixing dry powder refractory aggregate, dry powder alumina cement, silica sol, and dry powder hydraulic alumina in a specific ratio. It is said that when this monolithic refractory for dry spraying is used in a dry spraying construction method, the curing strength of the resulting construction can be increased.
[0005] Patent Document 2 discloses a castable refractory that contains silica sol, magnesia fine powder of a specific particle size, and condensed phosphate in a specific ratio. It is said that this castable refractory can ensure an appropriate working time for casting without the addition of alumina cement, and can obtain sufficient hardened strength. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 7174184 [Patent Document 2] Patent No. 6296635 Summary of the Invention [Problem to be solved by the invention]
[0007] Both Patent Documents 1 and 2 are monolithic refractories using silica sol. However, the monolithic refractory composition using silica sol has a lower curing strength than the monolithic refractory composition using cement. If the curing strength is low, the shape of the applied body is not easily maintained when the body is removed from the frame, and workability is reduced. In addition, when the pressure of steam inside the construction body increases and exceeds the strength of the construction body, it will explode, so it is desirable to prevent this explosion. Low-cement type monolithic refractories have a dense structure because they contain ultra-fine powder, and are prone to explosion when heated rapidly. In addition, there is generally a trade-off between improving curing strength and improving explosion resistance, and it is difficult to achieve both at the same time.
[0008] In view of the above situation, the problem that one embodiment of the present disclosure aims to solve is to provide an amorphous refractory composition and an amorphous refractory material that improve the curing strength of the constructed body and have excellent explosion resistance. [Means for solving the problem]
[0009] Specific means for achieving the above object are as follows: <1> Refractory aggregate and CaO·Al as hardener 2 O 3 and a silica sol, The ratio of the CaO·Al to the total mass of the alumina cement 2 O 3 The content of is 55% by mass or more, The content of the alumina cement is 1 to 5 parts by mass relative to 100 parts by mass of the refractory aggregate, The amorphous refractory composition, wherein the silica solid content contained in the silica sol is 1 to 30 parts by mass relative to 100 parts by mass of the refractory aggregate. <2> The silica sol has a silica solid content of 10 to 50 mass%. <1> The amorphous refractory composition according to claim 1. <3> The ratio of the total mass of the solid content of the refractory aggregate, the alumina cement, and the silica sol to the total solid content of the amorphous refractory composition is 99.5 mass% or more; <1> or <2> The amorphous refractory composition according to claim 1. <4> <1> ~ <3> 13. A molded refractory material formed from the molded refractory composition according to claim 12. Effect of the Invention
[0010] According to one embodiment of the present disclosure, it is possible to provide an amorphous refractory composition and an amorphous refractory material that improve the curing strength of a constructed body and have excellent explosion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the embodiments for carrying out the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the components (including element steps, etc.) are not essential unless otherwise specified. The same applies to the numerical values and their ranges, and do not limit the present disclosure.
[0012] In the present disclosure, a numerical range indicated using "~" includes the numerical values before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with the value shown in the synthesis examples. In the present disclosure, each component may contain multiple types of corresponding compounds. When multiple substances corresponding to each component are present in the composition, the content of each component means the total content of the multiple substances present in the composition, unless otherwise specified.
[0013] (Amorphous refractory composition) The monolithic refractory composition of the present disclosure comprises a refractory aggregate and CaO·Al as a hardener. 2 O 3 and a silica sol, wherein the amount of the CaO·Al relative to the total mass of the alumina cement is 2 O 3 The content of the alumina cement is 1 to 5 parts by mass relative to 100 parts by mass of the refractory aggregate, and the silica solid content contained in the silica sol is 1 to 30 parts by mass relative to 100 parts by mass of the refractory aggregate.
[0014] The monolithic fireproof composition of the present disclosure has improved curing strength of the applied body and excellent resistance to explosion. The reason for the above effects is not clear, but is presumed to be as follows. The monolithic refractory composition of the present disclosure is CaO·Al 2 O 3 This includes alumina cement with a CaO·Al content of 55 mass% or more. 2 O 3 Since silica sol has excellent compressive strength, it is presumed that the curing strength of the applied body is improved. Also, compared to monolithic refractories hardened with alumina cement, monolithic refractories hardened with silica sol are more likely to allow water vapor to escape outside the monolithic refractory, and therefore are presumed to have improved explosion resistance. Furthermore, when the silica solid content in the silica sol is 1 to 30 parts by mass per 100 parts by mass of refractory aggregate, and the content of alumina cement is 1 to 5 parts by mass per 100 parts by mass of refractory aggregate, CaO·Al 2 O 3 It is presumed that the advantages of using the alumina cement containing the silica sol and the advantages of using the silica sol are not impaired. By achieving a balance in this way, the monolithic refractory composition of the present disclosure is prevented from causing explosion. This allows the monolithic refractory composition of the present disclosure to be heated rapidly, thereby shortening the construction period.
[0015] <Refractory aggregate> The refractory aggregate is not particularly limited as long as it can be used to manufacture unshaped refractory materials. For example, alumina (Al 2 O3 ), zirconia (ZrO 2 ), zircon (ZrO 2 SiO 2 The fire-resistant aggregate may be used alone or in combination of two or more kinds.
[0016] Alumina includes chamotte (Al 2 O 3 Content: 40~50% by mass), mullite (Al 2 O 3 Content: about 60% by mass), bauxite (Al 2 O 3 Content: 80~89% by mass), high purity alumina (Al 2 O 3 Content: 90% by mass or more). In this disclosure, the "content of refractory aggregate" means the content of chamotte, mullite, bauxite, high-purity alumina, etc.
[0017] The particle size of the refractory aggregate is not particularly limited, but from the viewpoint of improving workability and the like, it is preferably 45 μm to 5 mm. In the present disclosure, the particle size of the refractory aggregate can be measured by a sieving test in accordance with JIS Z 8815:1994, and is the particle size at which the cumulative volume is 50%.
[0018] <Alumina cement> In order to increase the curing strength of the applied structure, the ratio of CaO·Al to the total mass of alumina cement is 2 O 3 The content is 55% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, particularly preferably 90% by mass or more, most preferably 95% by mass or more, and may be 100% by mass.
[0019] Alumina cement is made up of CaO·Al 2 O 3 It may contain other components other than 12CaO 7Al 2 O 3 , CaO 2Al2 O 3 , CaO·Al 2 OCaSO 4 , CaO·Al 2 O 3 Fe 2 O 3 , CaO·Al 2 O 3 ·CaF 2 , CaO·Na 2 O. Al 2 O 3 etc.
[0020] From the viewpoint of increasing the curing strength of the applied body, the content of other components relative to the total mass of the alumina cement is preferably 20 mass% or less, more preferably 10 mass% or less, even more preferably 5 mass% or less, and particularly preferably zero.
[0021] In addition, from the viewpoint of increasing the curing strength of the construction and improving the explosion resistance, the content of alumina cement is 1 to 5 parts by mass, preferably 1 to 4 parts by mass, and more preferably 1 to 3 parts by mass, per 100 parts by mass of the fire-resistant aggregate.
[0022] <Silica sol> The silica sol preferably has a silica solid content concentration of 10 to 50% by mass. When the silica solid content concentration is 10% by mass or more, the hardening property of the silica sol and the refractory aggregate tends to be sufficient. When the silica solid content concentration is 50% by mass or less, the viscosity of the silica sol does not become too high, and the mixability of the silica sol and the refractory aggregate is excellent. The silica sol may be a commercially available product.
[0023] From the viewpoint of achieving a balance between improving the curing strength of the construction and improving the explosion resistance, the silica solid content in the silica sol is 1 to 30 parts by mass, preferably 1 to 20 parts by mass, more preferably 1 to 15 parts by mass, and even more preferably 1 to 10 parts by mass, per 100 parts by mass of the fire-resistant aggregate.
[0024] <Additives> The moldable refractory composition of the present disclosure may contain additives other than the above-mentioned components. Additives include refractory particles (silica, titania, diaspore, aluminium shale, pyrophyllite, sillimanite, andalusite, silica, chromite, spinel, magnesia, zirconia, zircon, chromia, silicon nitride, aluminum nitride, alumina, silicon carbide, boron carbide, titanium boride, zirconium boride, etc.), dispersants (phosphate-based dispersants, carboxylate-based dispersants, sulfonate-based dispersants, etc.), bentonite, binders (activated magnesia, low-reactivity alkaline earth metal oxides, water-soluble organic acid salts, water-soluble inorganic acid salts, etc.), antioxidants, shrinkage relaxation agents, thickeners, organic fibers, etc.
[0025] The alumina particles may be any alumina particles that have been used in conventional amorphous refractory compositions. The alumina particles have a strong cohesive force and have the effect of promoting hardening when the amorphous refractory composition is made into a refractory. The alumina particles also contribute to improving fluidity and physical properties. From the viewpoint of promoting hardening of the refractory by the cohesion of the alumina particles, the average particle size of the alumina particles is preferably less than 10 μm, more preferably less than 5 μm. Two or more types of alumina particles may be included. The particle size of the alumina particles can be measured by a laser diffraction particle size distribution measurement method in accordance with JIS Z 8825:2013, and is the particle size at which the cumulative volume is 50%.
[0026] The silica particles may be any silica particles that have been used in conventional moldable refractory compositions. The particle size of the silica particles is not particularly limited and may be 0.1 μm to 30 μm.
[0027] Examples of the organic fibers include polypropylene fibers, polyethylene fibers, polyester fibers, polyvinyl alcohol fibers, and cellulose fibers. The fiber length of the organic fiber may be 10 μm to 20 mm, and the fiber diameter of the organic fiber may be 0.1 to 20 dtex. In the present disclosure, the fiber length is measured in accordance with JIS L 1015:2010, and the fiber diameter is measured in accordance with JIS L 1015:2010. The organic fibers may be used alone or in combination of two or more. When two or more organic fibers are used in combination, it is preferable to use two or more organic fibers having different fiber lengths. By using two or more organic fibers, the explosion resistance can be further improved, and the flowability can be improved when the amorphous refractory composition is mixed with water to form a clay during construction. For example, it is preferable to use long fibers having a fiber length of 3 mm to 20 mm and short fibers having a fiber length of 10 μm to 3 mm in combination.
[0028] The proportion of the total mass of the solid contents of the refractory aggregate, alumina cement, and silica sol to the total solid contents of the amorphous refractory composition is preferably 99.5 mass% or more, more preferably 99.6 mass% or more, and even more preferably 99.7 mass% or more.
[0029] (Method of manufacturing unshaped refractory composition) The amorphous refractory composition of the present disclosure can be produced by kneading the above-mentioned components by a conventionally known method. For example, an omni mixer, a paddle mixer, a Nauta mixer, an Eirich mixer, a vortex mixer, or a continuous kneader can be used for kneading.
[0030] (Unshaped refractories) The monolithic refractory of the present disclosure is formed from the monolithic refractory composition. The monolithic refractory may be produced by spraying, pouring or casting.
Claims
1. Refractory aggregate and CaO・Al as a hardener 2 O 3 and a silica sol, The ratio of the CaO.Al to the total mass of the alumina cement 2 O 3 The content of is 55% by mass or more, The content of the alumina cement is 1 to 5 parts by mass relative to 100 parts by mass of the refractory aggregate, The amorphous refractory composition, wherein the silica solid content contained in the silica sol is 1 to 30 parts by mass per 100 parts by mass of the refractory aggregate.
2. The amorphous refractory composition according to claim 1, wherein the silica sol has a solids concentration of silica of 10 to 50 mass%.
3. 3. An amorphous refractory composition as described in claim 1 or 2, wherein the total mass of the solid content of the refractory aggregate, alumina cement, and silica sol accounts for 99.5 mass% or more of the total solid content of the amorphous refractory composition.
4. A moldable refractory material formed from the moldable refractory composition according to claim 1 or 2.
Citation Information
Patent Citations
Surface activate supersaturated solid solution alloy for electrode for solution electrolysis and activation treatment method thereof
JP1987096635A
Monolithic refractory for dry spraying and dry spraying construction method using the same
JP7174184B1