Bulk product composed of carbon fiber agglomerates and method for producing bulk product composed of carbon fiber agglomerates
By mixing recycled and virgin carbon fibers with an organic binder to form carbon fiber agglomerates, the mechanical strength of recycled fibers is enhanced, addressing the strength decrease issue and improving CFRP reinforcement.
Patent Information
- Application Number
- JP2023177109
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2023-10-12
- Publication Date
- 2024-11-21
AI Technical Summary
Recycled carbon fibers from waste composites exhibit a significant decrease in mechanical strength, and their effectiveness as reinforcing materials for CFRP is not fully understood when mixed with virgin carbon fibers.
A method involving the mixing of recycled and virgin carbon fibers, both in short lengths, with an organic binder in water to form carbon fiber agglomerates, where the ratio of virgin carbon fibers to total fibers is less than 50%, enhancing the reinforcing capability of the recycled fibers.
Improves the ability of recycled carbon fibers as reinforcing materials for CFRP without significantly reducing their usage, resulting in improved mechanical properties of the bulk products.
Smart Images

Figure 2024162963000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates primarily to a bulk product of a plurality of carbon fiber agglomerates and a method for producing the bulk product of a plurality of carbon fiber agglomerates. [Background technology]
[0002] CFRP (Carbon Fiber Reinforced Plastic), a fiber-reinforced plastic that uses fiber reinforcement made from carbon fiber, is a lightweight material with excellent mechanical properties that makes it suitable for parts in automobiles, ships, railway vehicles, manned aircraft, unmanned aerial vehicles, and other transportation equipment, and its importance has been increasing in recent years.
[0003] A method for producing carbon fiber pellets is known in which wet continuous carbon fiber bundles containing only virgin carbon fibers as carbon fibers are cut to lengths of about 1 to about 10 mm, mixed with a solution or suspension of a sizing agent, pelletized using a rotary disk pelletizer, and finally dried (Patent Document 1).
[0004] A bulk product made of discontinuous carbon fiber bundles can be manufactured by adding water in which an organic binder is dispersed to dried recycled carbon fibers recovered from waste carbon fiber sheet molding compounds by pyrolysis and stirring the mixture. Such a bulk product can be used as a reinforcing material for CFRP (Patent Document 2). Carbon fiber sheet molding compounds are a type of carbon fiber prepreg, and are manufactured by impregnating a random mat made of chopped carbon fiber bundles with resin. Chopped carbon fiber bundles are short carbon fiber bundles manufactured by cutting continuous carbon fiber bundles made of virgin carbon fibers. Hereinafter, carbon fiber sheet molding compounds may be abbreviated as CF-SMC. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 10-503812 [Patent Document 2] International Publication WO2022 / 265099 Brochure Summary of the Invention [Problem to be solved by the invention]
[0006] It is known that recycled carbon fibers, especially those recovered from waste carbon fiber composites by pyrolysis, have a greater degree of decrease in mechanical strength than virgin carbon fibers. On the other hand, it has not yet been fully investigated how the performance of recycled carbon fibers as CFRP reinforcement materials changes when they are mixed with virgin carbon fibers. The main object of the present invention is to provide a technique for improving the performance of bulk products made of multiple carbon fiber agglomerates using recycled carbon fibers as raw materials as CFRP reinforcement materials without significantly reducing the amount of recycled carbon fibers used. [Means for solving the problem]
[0007] The inventors have unexpectedly found that the ability of a bulk product consisting of a number of carbon fiber agglomerates made from recycled carbon fiber bundles recovered by pyrolysis from waste carbon fiber composites as a reinforcing material for CFRP can be improved by simply mixing in a relatively small amount of virgin carbon fiber into the raw material. The present invention is based on this discovery.
[0008] One aspect of the present invention relates to a bulk product made of a plurality of carbon fiber agglomerates. The bulk product contains a plurality of short carbon fibers including virgin carbon fibers and recycled carbon fibers, and an organic binder, and the ratio of the mass of the virgin carbon fibers to the total mass of the recycled carbon fibers and the virgin carbon fibers is less than 50%. Another aspect of the present invention relates to a method for producing a bulk product made of a plurality of carbon fiber agglomerates. The method includes mixing virgin carbon fibers and recycled carbon fibers, both of which are short carbon fibers, in the presence of water and an organic binder to form a plurality of wet carbon fiber agglomerates, and drying the plurality of wet carbon fiber agglomerates. The ratio of the mass of the virgin carbon fibers to the total mass of the virgin carbon fibers and the recycled carbon fibers is less than 50%. Effect of the Invention
[0009] According to the present invention, a technique is provided for improving the performance of a bulk product made of multiple carbon fiber agglomerates using recycled carbon fiber as a reinforcing material for CFRP, without significantly reducing the amount of recycled carbon fiber used. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram showing an example of the structure of a carbon fiber agglomerate. [Diagram 2] FIG. 2 is a conceptual diagram of a sheet prepreg manufacturing device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the preferred embodiments.
[0012] 1. Bulk Product One embodiment of the present invention relates to a bulk product made of a plurality of carbon fiber agglomerates. The carbon fiber agglomerates constituting this bulk product are formed, for example, by the following procedure. First, short carbon fibers in an unraveled state are prepared. The short carbon fibers are carbon fibers that have been shortened by being intentionally or unintentionally cut. The length of the short carbon fibers is usually 100 mm or less, and may be 90 mm or less, 80 mm or less, 70 mm or less, 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, 20 mm or less, or 10 mm or less. Next, a wet carbon fiber agglomerate is formed by contacting the prepared short carbon fibers with water. Inside the wet carbon fiber agglomerate, the short carbon fibers are in a liquid-bridged state with each other. The organic binder can be contained in the wet carbon fiber agglomerate by dispersing or dissolving the organic binder in advance in the water, or by attaching the organic binder to all or a part of the carbon fibers before contacting with water as an alternative or additional means. When water is removed by evaporation from a wet carbon fiber agglomerate containing an organic binder, a dry carbon fiber agglomerate in which short carbon fibers are bound to each other via the organic binder is obtained. In this specification, the term "carbon fiber agglomerate" simply refers to a dry carbon fiber agglomerate unless otherwise specified.
[0013] Fig. 1 is a schematic diagram illustrating the structure of a carbon fiber agglomerate. As shown in Fig. 1, short carbon fibers are gathered to form bundles in each carbon fiber agglomerate. The number of short carbon fibers contained in one carbon fiber agglomerate can be, for example, within the range of several hundred to several tens of thousands.
[0014] Carbon fiber agglomerates usually have a longitudinal direction, which is along the extension direction of the short carbon fibers contained therein. The length (longitudinal dimension) and external shape of the carbon fiber agglomerate can be affected by the fiber length of the short carbon fibers that compose it. For example, in a carbon fiber agglomerate formed using only short carbon fibers with a fiber length of 6 mm as raw material, the length of the agglomerate may exceed three times the fiber length of the carbon fibers, in which case the shape of the agglomerate will be spindle-like. On the other hand, in a carbon fiber agglomerate formed using only short carbon fibers with a fiber length of 25 mm as raw material, the length of the agglomerate will remain at 1.5 times or less the fiber length of the carbon fibers, and the shape of the agglomerate will be wire-like.
[0015] The bulk product according to the embodiment tends to have a higher bulk density as it contains more short carbon fiber agglomerates, which is advantageous in terms of storage and transportation, and also tends to be less likely to cause bridging in the hopper. Therefore, the fiber length of the short carbon fibers constituting the carbon fiber agglomerates is preferably 60 mm or less, more preferably 50 mm or less, even more preferably 40 mm or less, and even more preferably 30 mm or less, and may be 20 mm or less. In particular, the fiber length of the virgin carbon fibers may be less than 10 mm, and may even be 6 mm or less.
[0016] The bulk product according to the embodiment contains both virgin carbon fiber and recycled carbon fiber as carbon fiber. The ratio of the mass of virgin carbon fiber to the total mass of recycled carbon fiber and virgin carbon fiber is less than 50%. This ratio may be 40% or less, further 30% or less, or even 20% or less. There is no particular lower limit to this ratio, but it is usually 1% or more, preferably 5% or more, and more preferably 10% or more. The ratio of recycled carbon fiber to virgin carbon fiber in each carbon fiber agglomerate constituting the bulk product does not need to be the same as the ratio of recycled carbon fiber to virgin carbon fiber in the entire bulk product.
[0017] In the bulk product according to the embodiment, the fiber length of the virgin carbon fiber may be smaller than the maximum fiber length of the recycled carbon fiber. In other words, there may be no virgin carbon fiber having a fiber length equal to or greater than the longest recycled carbon fiber contained in the bulk product. Most of the recycled carbon fibers contained in the bulk product may have approximately the same fiber length as the longest recycled carbon fiber contained in the same bulk product. For example, 50% by mass or more of the total recycled carbon fibers may have a fiber length that is 90% or more of the longest recycled carbon fiber contained in the same bulk product.
[0018] Generally, the longer the fiber length of carbon fibers, the more effective they are as a reinforcing material for CFRP. From this viewpoint, 60% by mass or more of the recycled carbon fibers contained in the bulk product preferably have a fiber length of 10 mm or more, and may have a fiber length of 20 mm or more. Also, 90% by mass or more of the virgin carbon fibers contained in the bulk product preferably have a fiber length of 1 mm or more, and more preferably have a fiber length of 3 mm or more.
[0019] A typical example of recycled carbon fiber is carbon fiber recovered from waste carbon fiber composites. Examples of waste carbon fiber composites include CFRP extracted from disused CFRP-using products and CFRP discarded as defective or surplus products at CFRP product manufacturing plants. Examples of waste carbon fiber composites also include waste carbon fiber prepreg. Examples of waste carbon fiber prepreg include scraps generated in the manufacturing process of CFRP products using carbon fiber prepreg, and scraps, defective products, and surplus products generated at carbon fiber prepreg manufacturing plants.
[0020] A suitable example of the recycled carbon fiber is a recycled carbon fiber recovered from a waste carbon fiber composite containing chopped carbon fiber bundles impregnated with resin. Almost all of such recycled carbon fibers can have the same fiber length as the carbon fibers constituting the chopped carbon fiber bundles. A typical example of a carbon fiber composite containing chopped carbon fiber bundles impregnated with resin is CF-SMC (carbon fiber sheet molding compound). Waste CF-SMC, both uncured and cured, is a preferred raw material for recycled carbon fibers. Cured CF-SMC includes CFRP molded products manufactured using CF-SMC. When a waste carbon fiber composite contains long carbon fibers and is difficult to use as a raw material for bulk products when recovered at the same length, the waste carbon fiber composite or its dry distillate may be cut or crushed before recovering the carbon fibers.
[0021] The recycled carbon fibers may be recovered from the waste carbon fiber composite by any technique, for example, by a pyrolysis method. In the pyrolysis method, the matrix resin and / or its residue (carbon generated by decomposition of the matrix resin) contained in the waste carbon fiber composite are decomposed by heating in an inert gas atmosphere and / or an oxidizing atmosphere. Examples of the oxidizing atmosphere include an oxygen-containing atmosphere such as an air atmosphere.
[0022] After removing most of the matrix resin from the waste carbon fiber composite by the semiconductor thermal activation method and / or chemical decomposition method, the residue that could not be completely removed by these methods can be decomposed and removed by heating in an oxidizing atmosphere. Recycled carbon fibers can also be recovered by mechanically disintegrating the carbon fiber masses generated by the thermal decomposition of the waste carbon fiber composite.
[0023] The organic binder used in the bulk product according to the embodiment may contain at least one selected from the group consisting of epoxy resin, polyester, epoxy acrylate, polyurethane, polyether and polyamide. These resins or polymers are known as preferred materials for sizing agents used when producing continuous carbon fiber bundles. The sizing agent sometimes used may be preferably used as an organic binder in the bulk product according to the embodiment.
[0024] The bulk product according to the embodiment can be used as a reinforcing material for CFRP. The matrix resin of the CFRP is preferably a cured thermosetting resin. Another use of the bulk product according to the embodiment is a prepreg. A prepreg is a type of intermediate material used when manufacturing a CFRP molded product. Examples of prepregs using the bulk product according to the embodiment include sheet prepregs and bulk molding compounds.
[0025] 2. Sheet Prepreg The bulk product according to the embodiment can be preferably used for producing a sheet prepreg. An example of a method for producing a sheet prepreg includes the following first to fourth steps.
[0026] First step: A step of applying a thermosetting resin paste to the respective surfaces of the first protective film and the second protective film. Second step: A step of scattering the bulk product according to the embodiment onto the surface of the first protective film onto which the resin paste has been applied to form a carbon fiber mat. Third step: A step of overlapping the second protective film with the first protective film, sandwiching the carbon fiber mat therebetween, so that the surfaces onto which the resin paste has been applied face each other, to form a laminate. Fourth step: A step of pressurizing the laminate to impregnate the carbon fiber mat with the resin paste, thereby obtaining a sheet prepreg.
[0027] The production of sheet prepreg by such a method can be carried out using a sheet prepreg production apparatus, the conceptual diagram of which is shown in Fig. 2. The sheet prepreg production apparatus shown in Fig. 2 has a section for applying a resin paste to a first protective film unwound from a roll, a section for forming a carbon fiber mat on the first protective film by spraying the bulk product according to the embodiment, a section for applying a resin paste to a second protective film unwound from a roll, a section for overlaying the second protective film on the first protective film to form a laminate, a section for pressurizing the laminate, and a section for winding up the laminate.
[0028] The first protective film and the second protective film are synthetic resin films, and the material thereof can be appropriately selected from polyolefins such as polyethylene and polypropylene, polyvinylidene chloride, vinyl chloride resins, polyamides, and the like.
[0029] Examples of thermosetting resins that are blended into the resin paste as the base resin include vinyl ester resins, unsaturated polyester resins, epoxy resins, polyimide resins, maleimide resins, and phenolic resins. Two or more of these may be selected and blended into the resin paste. In addition to the hardener blended into the resin paste as an essential component, polymerization inhibitors, thickeners, reactive diluents, low-shrinkage agents, antioxidants, internal mold release agents, colorants, modifiers (e.g., rubber, elastomer, or thermoplastic resin particles), flame retardants, antibacterial agents, and the like may be blended into the resin paste as optional components.
[0030] When a thickener is blended into the resin paste, it is preferable to mature the sheet prepreg after the fourth step until the viscosity of the resin paste becomes sufficiently high.
[0031] The resin paste is preferably solvent-free. In other words, the resin paste is preferably not a varnish. If the resin paste is a varnish, a step of evaporating and removing the solvent is required after impregnating the carbon fiber mat. The reactive diluent is not included in the solvent referred to here.
[0032] A suitable example of the resin paste that is not a varnish is an unsaturated polyester resin-based composition, which contains an unsaturated polyester resin, an ethylenically unsaturated monomer, a thickener, a polymerization initiator, and a polymerization inhibitor. In a suitable example, a vinyl ester resin may be further contained. The ethylenically unsaturated monomer is contained as a reactive diluent. The ethylenically unsaturated monomer preferably includes a monofunctional monomer. A suitable example of the ethylenically unsaturated monomer is a (meth)acrylate. A suitable example of the thickener is a polyisocyanate, but is not limited thereto. A suitable example of the polymerization initiator is an organic peroxide.
[0033] Another suitable example of the resin paste that is not a varnish is an epoxy resin-based composition, which is formulated with an epoxy resin, an epoxy hardener, and a thickener. The epoxy resin preferably contains a diglycidyl ether of bisphenols. The epoxy hardener preferably contains one or more latent hardeners. Suitable examples of the thickener include carboxylic anhydrides, amines, and polyisocyanates. Although carboxylic anhydrides and amines are known as epoxy hardeners, they can act as thickeners when used in small amounts.
[0034] The amount of resin paste applied to the first protective film and the second protective film in the first step and the basis weight of the carbon fiber mat formed on the first protective film in the second step are adjusted taking into account the basis weight and carbon fiber content of the sheet prepreg to be produced.
[0035] The weight of the sheet prepreg can be appropriately designed, for example, 300 g / m 2 More than 500g / m 2 Less than 500g / m 2 More than 1000g / m 2 Less than 1000g / m 2 More than 2000g / m 2 Less than 2000g / m 2 More than 4000g / m 2 Less than 4000g / m 2 More than 6000g / m 2 Less than 6000g / m2 More than 8000g / m 2 Less than 8000g / m 2 More than 10000g / m 2 It can be less than, etc.
[0036] The fiber content of the sheet prepreg can be 20% by mass or more and less than 30% by mass, 30% by mass or more and less than 40% by mass, 40% by mass or more and less than 50% by mass, 50% by mass or more and less than 60% by mass, 60% by mass or more and less than 70% by mass, 70% by mass or more and less than 80% by mass, or 80% by mass or more and less than 90% by mass, etc.
[0037] As a molding method for producing a CFRP product using a sheet prepreg, a press molding method is preferably used, but is not limited thereto. For example, a molding method other than the press molding method, such as an autoclave molding method, can also be used.
[0038] 3. Method for Producing a Bulk Product One embodiment of the present invention relates to a method for producing a bulk product made of a plurality of carbon fiber agglomerates. This method can be preferably used for producing the bulk products according to the above-mentioned embodiments.
[0039] The method according to the embodiment includes mixing virgin carbon fibers and recycled carbon fibers, both of which are short carbon fibers, in the presence of water and an organic binder to form a plurality of wet carbon fiber agglomerates, and drying the plurality of wet carbon fiber agglomerates. The ratio of the mass of the virgin carbon fibers to the total mass of the recycled carbon fibers and the virgin carbon fibers is less than 50%. This ratio may be 40% or less, further 30% or less, or even 20% or less. There is no particular lower limit to the ratio of the mass of the virgin carbon fibers to the total mass of the recycled carbon fibers and the virgin carbon fibers, but it is usually 1% or more, preferably 5% or more, and more preferably 10% or more.
[0040] The fiber length of the virgin carbon fiber may be smaller than the maximum fiber length of the recycled carbon fiber. The maximum fiber length of the recycled carbon fiber is the fiber length of the longest fiber among all the recycled carbon fibers. Most of the recycled carbon fibers may have approximately the same fiber length as the longest fiber. For example, 50 mass% or more of all the recycled carbon fibers may have a fiber length of 90% or more of the longest fiber.
[0041] The shorter the fiber length of the carbon fibers used as the raw material, the less likely the carbon fibers are to be entangled with each other, and the easier it is to manufacture bulk products. For this reason, the fiber length of the carbon fibers used as the raw material is preferably 60 mm or less, more preferably 50 mm or less, even more preferably 40 mm or less, even more preferably 30 mm or less, and may be 20 mm or less. In particular, the fiber length of virgin carbon fibers may be less than 10 mm, and may even be 6 mm or less. On the other hand, the longer the fiber length of carbon fibers is, in general, the more effective they are as a reinforcing material for CFRP. From this viewpoint, 60% by mass or more of the recycled carbon fibers used as the raw material preferably have a fiber length of 10 mm or more, and may be 20 mm or more. In addition, it is preferable that 90% by mass or more of the virgin carbon fibers used as the raw material have a fiber length of 1 mm or more, and more preferably have a fiber length of 3 mm or more.
[0042] A typical example of recycled carbon fiber is carbon fiber recovered from waste carbon fiber composites. Examples of waste carbon fiber composites include CFRP extracted from disused CFRP-using products and CFRP discarded as defective or surplus products at CFRP product manufacturing plants. Examples of waste carbon fiber composites also include waste carbon fiber prepreg. Examples of waste carbon fiber prepreg include scraps generated in the manufacturing process of CFRP products using carbon fiber prepreg, and scraps, defective products, and surplus products generated at carbon fiber prepreg manufacturing plants.
[0043] A suitable example of the recycled carbon fiber used in the manufacturing method according to the embodiment is a recycled carbon fiber recovered from a waste carbon fiber composite containing chopped carbon fiber bundles impregnated with resin. Almost all of such recycled carbon fibers can have the same fiber length as the carbon fibers constituting the chopped carbon fiber bundles. A typical example of a carbon fiber composite containing chopped carbon fiber bundles impregnated with resin is CF-SMC (carbon fiber sheet molding compound). Waste CF-SMC, both uncured and cured, is a preferred raw material for recycled carbon fibers. Cured CF-SMC includes CFRP molded products manufactured using CF-SMC. When a waste carbon fiber composite contains long carbon fibers and is difficult to use as a raw material for bulk products when recovered at the same length, the waste carbon fiber composite or its dry distillate may be cut or crushed, and then the carbon fibers may be recovered.
[0044] The recycled carbon fibers may be recovered from the waste carbon fiber composite by any technique, for example, by a pyrolysis method. In the pyrolysis method, the matrix resin and / or its residue contained in the waste carbon fiber composite is heated and decomposed in an inert gas atmosphere and / or an oxidizing atmosphere. Examples of the oxidizing atmosphere include an oxygen-containing atmosphere such as an air atmosphere.
[0045] The pyrolysis method is a technique well known to those skilled in the art, and publicly known documents can be referred to for details. For example, in the method described in JP-A-6-99160, a recycled carbon fiber is recovered by treating a waste carbon fiber composite without burning it in an atmosphere with an oxygen concentration in the range of 3 to 18% by volume and a temperature in the range of 300 to 600°C. As another example, in the method described in JP-A-7-33904, a recycled carbon fiber is recovered by treating a waste carbon fiber composite without burning it in an atmosphere with an oxygen concentration in the range of 0.1 to 25% by volume and a temperature in the range of 300 to 1000°C after dry distillation.
[0046] A typical example of a heating means used in the pyrolysis method is an electric furnace, but means such as microwave heating and induction heating can also be used. The pyrolysis method can also be used to remove residues of matrix resin that could not be completely removed by methods such as semiconductor thermal activation and chemical decomposition. For the procedure for removing resin from waste carbon fiber composites by semiconductor thermal activation, see, for example, International Publication WO2022 / 050281.
[0047] When waste carbon fiber composites are heated in an atmosphere that is sufficiently free of oxygen, carbon fiber agglomerates may be obtained in which the carbon fibers are bound together by residual carbon, which is a decomposition product of the matrix resin. Recycled carbon fibers can also be recovered by mechanically loosening the carbon fiber agglomerates. For example, a stirring mixer with rotating blades, such as a Henschel mixer, can be used to loosen the carbon fiber agglomerates.
[0048] An example of the virgin carbon fiber used in the manufacturing method according to the embodiment is a chopped carbon fiber bundle made of carbon fibers having a fiber length of preferably 1 mm to several cm. In the chopped carbon fiber bundle, the carbon fibers are bound to each other by a sizing agent, so it is preferable to loosen the bundle before use as necessary. As a method for loosening the chopped carbon fiber bundle, in addition to a method of stirring using a stirring mixer having a rotating blade such as a Henschel mixer, there is a method of immersing the bundle in an organic solvent such as acetone to remove the sizing agent.
[0049] Another example of virgin carbon fibers that can be used as a raw material is a wet chopped carbon fiber bundle made of carbon fibers having a fiber length of preferably 1 mm to several cm. The wet chopped carbon fiber bundle does not need to be loosened before use because the carbon fibers are simply bound together by the capillary force of water.
[0050] The organic binder may contain at least one selected from the group consisting of epoxy resin, polyester, epoxy acrylate, polyurethane, polyether and polyamide. These resins or polymers are known as preferred materials for sizing agents used when producing continuous carbon fiber bundles. Sizing agents that are commonly used when producing continuous carbon fiber bundles can be preferably used as organic binders.
[0051] The amount of the organic binder used can be appropriately adjusted so that the content of the organic binder in the produced bulk product is, for example, in the range of 0.5 mass % to 10 mass %. When a sizing agent is attached to the virgin carbon fiber, the sizing agent may remain in the produced bulk product while retaining its function as an organic binder.
[0052] The virgin carbon fiber and the recycled carbon fiber are mixed in the presence of water and an organic binder. The organic binder is preferably dispersed in water using a surfactant and then mixed with the carbon fiber. The amount of water can be appropriately adjusted within a range of, for example, 40 to 100 parts by mass per 100 parts by mass of the carbon fiber, which is the total of the virgin carbon fiber and the recycled carbon fiber. If other conditions are the same, the smaller the mass ratio of water to carbon fiber, the smaller the size of the wet carbon fiber agglomerates formed tends to be.
[0053] There is no limitation on the method for mixing the virgin carbon fiber and the recycled carbon fiber. In order to mix them efficiently in a short time, it is preferable to mix them using a stirring mixer or a stirring granulator. The carbon fibers are bound together by the capillary force of water to form wet carbon fiber agglomerates.
[0054] In a preferred embodiment, the virgin carbon fibers are dispersed in water prior to being mixed with the recycled carbon fibers using a surfactant. Preferred examples of surfactants include, but are not limited to, non-ionic surfactants such as polyoxyalkylene alkyl ethers, including polyoxyethylene alkyl ethers and polyoxyethylene polyoxypropylene alkyl ethers. Both the virgin carbon fibers and the organic binder may be dispersed in the same water.
[0055] Any method can be used to dry the wet carbon fiber agglomerates. In one example, the wet carbon fiber agglomerates may be left at room temperature to dry naturally. In another example, the wet carbon fiber agglomerates may be forced to dry using a dryer such as a hot air dryer or a vacuum dryer.
[0056] 4. Experimental Results The following are the results of experiments conducted by the present inventors.
[0057] 4.1. Material (recycled carbon fiber) Continuous carbon fiber bundles (TR50S15L manufactured by Mitsubishi Chemical Corporation) were cut to produce chopped carbon fiber bundles with a fiber length of 2.5 cm, which were impregnated with a thermosetting matrix resin to form a carbon fiber sheet molding compound, which was then heated at 700°C for 0.5 hours in a nitrogen gas atmosphere, and then further heat-treated at 600°C for 1 hour in an oxygen gas-containing atmosphere to obtain recycled carbon fiber. This recycled carbon fiber was cotton-like, and no adhesion between the carbon fibers due to decomposition products of the matrix resin was observed.
[0058] (Virgin carbon fiber) A wet chopped carbon fiber bundle having a cut length of 3 mm or 6 mm and a water content of 12 mass% was used. The wet chopped carbon fiber bundle having a cut length of 3 mm was made of carbon fibers having a fiber length of 3 mm, and the grade of the carbon fibers was the same as that of the carbon fibers contained in TR50S15L manufactured by Mitsubishi Chemical Corporation. The wet chopped carbon fiber bundle having a cut length of 6 mm was made of carbon fibers having a fiber length of 6 mm, and the grade of the carbon fibers was the same as that of the carbon fibers contained in TR50S15L manufactured by Mitsubishi Chemical Corporation.
[0059] (Organic Binder) An organic binder aqueous dispersion with an organic component content of about 40% by mass was used, which was prepared by kneading a one-terminal acrylic-modified bisphenol A type epoxy resin, an aliphatic urethane acrylate oligomer, and a fumaric acid ester of a bisphenol A-ethylene oxide adduct (average number of moles added: 2) at 80 to 100°C, and dispersing the mixture in water using a nonionic surfactant.
[0060] 4.2. Preparation and evaluation of discontinuous carbon fiber bundles (Experiment 1) A bulk product was prepared by using virgin carbon fiber and recycled carbon fiber in a mass ratio of 14:86 in the following manner. A virgin carbon fiber dispersion was prepared by adding 90 g of an organic binder aqueous dispersion and 94 g of wet chopped carbon fiber bundles with a cut length of 3 mm to 330 g of water and stirring. Next, 514 g of recycled carbon fiber and the entire amount of the above virgin carbon fiber dispersion were put into a 25 L stirring tank of a stirring granulator (SP Granulator SPG-25T manufactured by Dalton Co., Ltd.) equipped with a stirring blade and a chopper, and stirred for 7 minutes. The peripheral speed of the tip of the stirring blade was 4 m / s for the first minute, 9.6 m / s for the next 3 minutes, and 9.6 m / s for the last 3 minutes, and the peripheral speed of the chopper was 11 m / s throughout. The contents were removed from the stirring tank and dried at 120 ° C for 2 hours using a box-type hot air dryer to obtain a bulk product consisting of numerous carbon fiber agglomerates.
[0061] Furthermore, using the manufactured bulk product, sheet prepregs (target basis weight 2000g / m2, target fiber content 53% by mass) were produced by the following procedure. Three 40cm x 40cm polyethylene films (polyethylene films A to C) were prepared, and 47.3g of thermosetting resin paste containing vinyl ester resin, unsaturated polyester resin, styrene, polyisocyanate and radical polymerization initiator was applied to a 30cm x 30cm area on one side of two of them (polyethylene films A and B). 95.4g of the bulk product was scattered on one polyethylene film (polyethylene film C) that was not coated with resin paste, and carbon fiber mats were deposited on it.
[0062] On top of this carbon fiber mat, one of the polyethylene films (polyethylene film A) with the resin paste applied to one side was placed with the resin paste side facing down. The two films were then turned upside down so that polyethylene film C, which had not been coated with resin paste, was on top and polyethylene film A was on the bottom. In this state, another polyethylene film B with paste applied to one side was replaced with polyethylene film C. In this way, a laminate was obtained in which two polyethylene films A and B with resin paste applied were stacked together with the carbon fiber mat sandwiched between them, with the resin paste sides facing each other.
[0063] Next, the laminate was pressed with a roll to impregnate the carbon fiber mat with the resin paste, and then the laminate was left at 25° C. for 7 days to thicken the paste, thereby obtaining a sheet prepreg.
[0064] Two 26cm x 26cm prepreg pieces cut from the prepared sheet prepreg were stacked and placed in a press mold to form a CFRP plate 30cm long and 30cm wide and 2mm thick at a temperature of 140°C, a pressure of 8MPa, and a pressurization time of 2 minutes. The density of the obtained CFRP plate was 1.42g / cm 3 A test piece measuring 8 mm in width and 60 mm in length was cut from this CFRP plate and subjected to a bending test using a universal testing machine (Instron 4465, manufactured by Instron) at a crosshead speed of 2 mm / min and a span of 32 mm (16 times the thickness of the CFRP plate). The average results obtained from the five test pieces showed a bending strength of 233 MPa, a bending modulus of elasticity of 20.2 GPa, and a ratio of bending strength to bending modulus of elasticity of 11.6 x 10 ―3 It was.
[0065] (Experiment 2) A bulk product consisting of carbon fiber agglomerates was produced in the same manner as in Experiment 1, except that wet chopped carbon fiber bundles with a cut length of 6 mm were used instead of wet chopped carbon fiber bundles with a cut length of 3 mm.Furthermore, a sheet prepreg was produced using the bulk product.
[0066] Furthermore, the prepared sheet prepreg was used to mold a CFRP plate in the same manner as in Experiment 1. The density of the obtained CFRP plate was 1.44 g / cm 3 In the same manner as in Experiment 1, test pieces were cut out from the CFRP plate and subjected to bending tests. The average results obtained from the five test pieces were 238 MPa in bending strength, 21.5 GPa in bending modulus, and 11.1 × 10 ―3 It was.
[0067] (Experiment 3) A bulk product consisting of carbon fiber agglomerates was produced in the same manner as in Experiment 1, except that a wet chopped carbon fiber bundle having a cut length of 12 mm was used instead of the wet chopped carbon fiber bundle having a cut length of 3 mm. Furthermore, a sheet prepreg was produced using the bulk product.
[0068] Furthermore, the prepared sheet prepreg was used to mold a CFRP plate in the same manner as in Experiment 1. The density of the obtained CFRP plate was 1.43 g / cm 3 In the same manner as in Experiment 1, test pieces were cut out from the CFRP plate and subjected to bending tests. The average results obtained from the five test pieces were 202 MPa in bending strength, 19.8 GPa in bending modulus, and 10.3 × 10 ―3 It was.
[0069] (Experiment 4) A bulk product consisting of carbon fiber agglomerates was produced in the same manner as in Experiment 1, except that a wet chopped carbon fiber bundle having a cut length of 25 mm was used instead of the wet chopped carbon fiber bundle having a cut length of 3 mm.Furthermore, a sheet prepreg was produced using the bulk product.
[0070] Furthermore, the prepared sheet prepreg was used to mold a CFRP plate in the same manner as in Experiment 1. The density of the obtained CFRP plate was 1.41 g / cm 3 In the same manner as in Experiment 1, test pieces were cut out from the CFRP plate and subjected to bending tests. The average results obtained from the five test pieces were 207 MPa in bending strength, 17.6 GPa in bending modulus, and 11.8 × 10―3 It was.
[0071] (Experiment 5) A bulk product consisting of carbon fiber agglomerates was produced in the same manner as in Experiment 1, except that the mass ratio of virgin carbon fiber to recycled carbon fiber used was changed to 33:67.Furthermore, a sheet prepreg was produced using this bulk product.
[0072] Furthermore, the prepared sheet prepreg was used to mold a CFRP plate in the same manner as in Experiment 1. The density of the obtained CFRP plate was 1.43 g / cm 3 In the same manner as in Experiment 1, test pieces were cut out from the CFRP plate and subjected to bending tests. The average results obtained from the five test pieces were 253 MPa in bending strength, 23.8 GPa in bending modulus, and 10.8 × 10 ―3 It was.
[0073] (Experiment 6) A bulk product consisting of carbon fiber agglomerates was produced in the same manner as in Experiment 1, except that wet chopped carbon fiber bundles with a cut length of 12 mm were used instead of wet chopped carbon fiber bundles with a cut length of 3 mm, and the mass ratio of virgin carbon fiber to recycled carbon fiber used was changed to 33:67.Furthermore, a sheet prepreg was produced using this bulk product.
[0074] Furthermore, the prepared sheet prepreg was used to mold a CFRP plate in the same manner as in Experiment 1. The density of the obtained CFRP plate was 1.46 g / cm 3 In the same manner as in Experiment 1, test pieces were cut out from the CFRP plate and subjected to bending tests. The average results obtained from the five test pieces were , bending strength is 221 MPa, bending modulus is 20.2 GPa, and the ratio of bending strength to bending modulus is 11.0 × 10 ―3 It was.
[0075] (Experiment 7) A bulk product made of carbon fiber agglomerates was produced in the same manner as in Experiment 1, except that the virgin carbon fiber dispersion was changed to a mixture of 390 g of water not containing virgin carbon fiber and 90 g of an organic binder aqueous dispersion, and the amount of recycled carbon fiber used was changed to 600 g. Furthermore, a sheet prepreg was produced in the same manner as in Experiment 1, using the bulk product using only recycled carbon fiber as the carbon fiber.
[0076] Furthermore, the prepared sheet prepreg was used to mold a CFRP plate in the same manner as in Experiment 1. The density of the obtained CFRP plate was 1.47 g / cm 3 In the same manner as in Experiment 1, test pieces were cut out from the CFRP plate and subjected to bending tests. The average results obtained from the five test pieces were 182 MPa in bending strength, 18.6 GPa in bending modulus, and 9.9 × 10 ―3 It was.
[0077] 5. Summary of the embodiments The present invention includes at least the following. [Embodiment 1] A bulk product made of a plurality of carbon fiber agglomerates, the bulk product containing a plurality of short carbon fibers including virgin carbon fibers and recycled carbon fibers and an organic binder, wherein the ratio of the mass of the virgin carbon fibers to the total mass of the recycled carbon fibers and the virgin carbon fibers is less than 50%. [Embodiment 2] A bulk product according to embodiment 1, in which the length of the plurality of short carbon fibers is 100 mm or less, and may be 90 mm or less, 80 mm or less, 70 mm or less, or 60 mm or less. [Embodiment 3] A bulk product according to embodiment 1 or 2, in which the ratio is 1% or more and less than 50%, and may be 5% or more and 35% or less, or 10% or more and 20% or less. [Embodiment 4] A bulk product according to any one of embodiments 1 to 3, in which the fiber length of the virgin carbon fibers is shorter than the maximum fiber length of the recycled carbon fibers. [Embodiment 5] The bulk product according to any one of embodiments 1 to 4, in which the fiber length of the recycled carbon fibers is 60 mm or less, preferably 50 mm or less, more preferably 40 mm or less, and even more preferably 30 mm or less. [Embodiment 6] The bulk product according to any one of embodiments 1 to 5, in which 60% by mass or more of the recycled carbon fibers have a fiber length of 10 mm or more, and may even have a fiber length of 20 mm or more. [Embodiment 7] The bulk product according to any one of embodiments 1 to 6, in which the virgin carbon fibers have a fiber length of less than 10 mm. [Embodiment 8] The bulk product according to embodiment 7, in which the virgin carbon fibers have a fiber length of 6 mm or less. [Embodiment 9] The bulk product according to any one of embodiments 1 to 8, in which 90% by mass or more of the virgin carbon fibers have a fiber length of 1 mm or more. [Embodiment 10] The bulk product according to any one of embodiments 1 to 9, in which 90% by mass or more of the virgin carbon fibers have a fiber length of 3 mm or more. [Embodiment 11] The bulk product according to any one of embodiments 1 to 10, wherein the recycled carbon fiber comprises carbon fiber recovered from a waste carbon fiber composite. A pyrolysis method may be used for recovery. [Embodiment 12] The bulk product according to embodiment 11, wherein the waste carbon fiber composite comprises either or both of an uncured carbon fiber sheet molding compound and a cured carbon fiber sheet molding compound.[Embodiment 13] A bulk product according to any one of embodiments 1 to 12, wherein the organic binder contains at least one selected from the group consisting of epoxy resin, polyester, epoxy acrylate, polyurethane, polyether, and polyamide. [Embodiment 14] A CFRP using the bulk product according to any one of embodiments 1 to 13 as a reinforcing material. [Embodiment 15] A prepreg using the bulk product according to any one of embodiments 1 to 13. [Embodiment 16] A method for producing a CFRP product using the prepreg according to embodiment 15. [Embodiment 17] A method for producing a sheet prepreg, comprising forming a carbon fiber mat using the bulk product according to any one of embodiments 1 to 13, and impregnating the carbon fiber mat with a thermosetting resin paste. [Embodiment 18] A sheet prepreg produced by the production method according to embodiment 17. [Embodiment 19] A method for producing a CFRP product using the sheet prepreg according to embodiment 18.
[0078] [Embodiment 20] A method for producing a bulk product consisting of a plurality of carbon fiber agglomerates, comprising mixing virgin carbon fibers and recycled carbon fibers, both of which are short carbon fibers, in the presence of water and an organic binder to form a plurality of wet carbon fiber agglomerates, and drying the plurality of wet carbon fiber agglomerates, wherein the ratio of the mass of the virgin carbon fibers to the total mass of the recycled carbon fibers and the virgin carbon fibers is less than 50%. [Embodiment 21] The method according to embodiment 20, wherein the length of the virgin carbon fibers and the recycled carbon fibers is 100 mm or less, and may be 90 mm or less, 80 mm or less, 70 mm or less, or 60 mm or less. [Embodiment 22] The method according to embodiment 20 or 21, wherein the ratio is 1% or more and less than 50%, and may be 5% or more and 35% or less, or 10% or more and 20% or less. [Embodiment 23] The method according to any one of embodiments 20 to 22, wherein the fiber length of the virgin carbon fibers is shorter than the maximum fiber length of the recycled carbon fibers. [Embodiment 24] The method according to any one of embodiments 20 to 23, wherein the recycled carbon fibers have a fiber length of 60 mm or less, preferably 50 mm or less, more preferably 40 mm or less, and even more preferably 30 mm or less. [Embodiment 25] The method according to any one of embodiments 20 to 24, wherein 60% by mass or more of the recycled carbon fibers have a fiber length of 10 mm or more, and may even have a fiber length of 20 mm or more. [Embodiment 26] The method according to any one of embodiments 20 to 25, wherein the virgin carbon fibers have a fiber length of less than 10 mm. [Embodiment 27] The method according to embodiment 26, wherein the virgin carbon fibers have a fiber length of 6 mm or less. [Embodiment 28] The method according to any one of embodiments 20 to 27, wherein 90% by mass or more of the virgin carbon fibers have a fiber length of 1 mm or more. [Embodiment 29] The method according to any one of embodiments 20 to 28, wherein 90% by mass or more of the virgin carbon fibers have a fiber length of 3 mm or more. [Embodiment 30] The method according to any one of embodiments 20 to 29, wherein the recycled carbon fibers include carbon fibers recovered from a waste carbon fiber composite. The recovery may be performed by pyrolysis.[Embodiment 31] The method according to embodiment 30, wherein the waste carbon fiber composite comprises either or both of an uncured carbon fiber sheet molding compound and a cured carbon fiber sheet molding compound. [Embodiment 32] The method according to any one of embodiments 20 to 31, wherein the organic binder contains at least one selected from the group consisting of epoxy resin, polyester, epoxy acrylate, polyurethane, polyether and polyamide. [Embodiment 33] The method according to any one of embodiments 20 to 32, wherein the virgin carbon fiber is dispersed in the water before being mixed with the recycled carbon fiber. [Embodiment 34] A bulk product produced by the method according to any one of embodiments 20 to 33. [Embodiment 35] A CFRP using the bulk product according to embodiment 34 as a reinforcing material. [Embodiment 36] A prepreg using the bulk product according to embodiment 34. [Embodiment 37] A method for producing a CFRP product using the prepreg according to embodiment 36. [Embodiment 38] A method for producing a sheet prepreg, comprising forming a carbon fiber mat using the bulk according to embodiment 34, and impregnating the carbon fiber mat with a thermosetting resin paste. [Embodiment 39] A sheet prepreg produced by the production method according to embodiment 38. [Embodiment 40] A method for producing a CFRP molded product using the sheet prepreg according to embodiment 39.
[0079] Although the present invention has been described above with reference to specific embodiments, each embodiment is presented as an example and does not limit the scope of the present invention. Each embodiment described in this specification can be modified in various ways within the scope of the effects of the invention, and can be combined with features described in other embodiments within the scope of feasibility. [Industrial Applicability]
[0080] The discontinuous carbon fiber bundles and sheet prepregs according to the embodiments can be preferably used when producing various CFRP products used in automobiles, motorcycles, bicycles, ships, railway vehicles, manned aircraft, unmanned aircraft and other transportation equipment, sporting goods, leisure goods, home appliances, agricultural machinery, building materials, etc.
Claims
1. A bulk product consisting of a plurality of carbon fiber agglomerates, the bulk product containing a plurality of short carbon fibers including virgin carbon fibers and recycled carbon fibers, and an organic binder, wherein the ratio of the mass of the virgin carbon fibers to the total mass of the recycled carbon fibers and the virgin carbon fibers is less than 50%.
2. 2. The bulk product of claim 1, wherein the length of the plurality of short carbon fibers is 100 mm or less, and may be 90 mm or less, 80 mm or less, 70 mm or less, or 60 mm or less.
3. 3. The bulk product according to claim 1 or 2, wherein the ratio is between 1% and less than 50%, and may be between 5% and 35% or between 10% and 20%.
4. The bulk product according to any one of claims 1 to 3, wherein the fiber length of the virgin carbon fibers is smaller than the maximum fiber length of the recycled carbon fibers.
5. The bulk product according to any one of claims 1 to 4, wherein the recycled carbon fibers have a fiber length of 60 mm or less, preferably 50 mm or less, more preferably 40 mm or less, and even more preferably 30 mm or less.
6. The bulk product according to any one of claims 1 to 5, wherein 60 mass% or more of the recycled carbon fibers have a fiber length of 10 mm or more, and may further have a fiber length of 20 mm or more.
7. The bulk product according to any one of claims 1 to 6, wherein the virgin carbon fibers have a fiber length of less than 10 mm.
8. 8. The bulk product of claim 7, wherein the virgin carbon fibers have a fiber length of 6 mm or less.
9. The bulk product according to any one of claims 1 to 8, wherein 90% by mass or more of the virgin carbon fibers have a fiber length of 1 mm or more.
10. The bulk product according to any one of claims 1 to 9, wherein 90% by mass or more of the virgin carbon fibers have a fiber length of 3 mm or more.
11. The bulk product of any one of claims 1 to 10, wherein the recycled carbon fibre comprises carbon fibre recovered from waste carbon fibre composites.
12. 12. The bulk product of claim 11, wherein the waste carbon fiber composite comprises one or both of uncured carbon fiber sheet molding compound and cured carbon fiber sheet molding compound.
13. The bulk product according to any one of claims 1 to 12, wherein the organic binder contains at least one selected from the group consisting of epoxy resins, polyesters, epoxy acrylates, polyurethanes, polyethers and polyamides.
14. A CFRP using the bulk product according to any one of claims 1 to 13 as a reinforcing material.
15. A prepreg using the bulk product according to any one of claims 1 to 13.
16. A method for producing a CFRP product, using the prepreg according to claim 15.
17. A method for producing a sheet prepreg, comprising forming a carbon fiber mat using the bulk product according to any one of claims 1 to 13, and impregnating the carbon fiber mat with a thermosetting resin paste.
18. A sheet prepreg produced by the production method according to claim 17.
19. A method for producing a CFRP product, using the sheet prepreg according to claim 18.
20. A method for producing a bulk product of a plurality of carbon fiber agglomerates, the method comprising: mixing virgin carbon fibers and recycled carbon fibers, both of which are short carbon fibers, in the presence of water and an organic binder to form a plurality of wet carbon fiber agglomerates; and drying the plurality of wet carbon fiber agglomerates. and wherein the ratio of the mass of the virgin carbon fibers to the total mass of the recycled carbon fibers and the virgin carbon fibers is less than 50%.
21. 21. The method of claim 20, wherein the virgin carbon fibers and the recycled carbon fibers have a length of 100 mm or less, and may be 90 mm or less, 80 mm or less, 70 mm or less, or 60 mm or less.
22. 22. The method according to claim 20 or 21, wherein the ratio is ≧1% and less than 50%, and may be ≧5% and less than 35%, or ≧10% and less than 20%.
23. The method according to any one of claims 20 to 22, wherein the fiber length of the virgin carbon fibers is less than the maximum fiber length of the recycled carbon fibers.
24. The method according to any one of claims 20 to 23, wherein the fiber length of the recycled carbon fibers is 60 mm or less, preferably 50 mm or less, more preferably 40 mm or less, and even more preferably 30 mm or less.
25. The method according to any one of claims 20 to 24, wherein 60% by mass or more of the recycled carbon fibers have a fiber length of 10 mm or more, and may further have a fiber length of 20 mm or more.
26. The method according to any one of claims 20 to 25, wherein the virgin carbon fibres have a fibre length of less than 10 mm.
27. 27. The method of claim 26, wherein the virgin carbon fibers have a fiber length of 6 mm or less.
28. The method according to any one of claims 20 to 27, wherein 90% by mass or more of the virgin carbon fibers have a fiber length of 1 mm or more.
29. The method according to any one of claims 20 to 28, wherein 90% by mass or more of the virgin carbon fibers have a fiber length of 3 mm or more.
30. The method of any one of claims 20 to 29, wherein the recycled carbon fibers comprise carbon fibers recovered from waste carbon fiber composites.
31. 31. The method of claim 30, wherein the waste carbon fiber composite comprises one or both of uncured carbon fiber sheet molding compound and cured carbon fiber sheet molding compound.
32. The method according to any one of claims 20 to 31, wherein the organic binder contains at least one selected from the group consisting of epoxy resins, polyesters, epoxy acrylates, polyurethanes, polyethers and polyamides.
33. A method according to any of claims 20 to 32, wherein the virgin carbon fibres are dispersed in the water before being mixed with the recycled carbon fibres.
34. A bulk product produced by the method according to any one of claims 20 to 33.
35. CFRP using the bulk product according to claim 34 as a reinforcing material.
36. A prepreg using the bulk product according to claim 34.
37. A method for producing a CFRP product using the prepreg according to claim 36.
38. 35. A method for producing a sheet prepreg, comprising forming a carbon fiber mat using the bulk according to claim 34, and impregnating the carbon fiber mat with a thermosetting resin paste.
39. A sheet prepreg produced by the production method according to claim 38.
40. A method for producing a CFRP molded product, using the sheet prepreg according to claim 39.
Citation Information
Patent Citations
Profile fiber-reinforced plastic
JP1997012730A
Carbon fiber sheet material, prepreg, molded article, carbon fiber sheet material production method, prepreg production method, and molded article production method
WO2020040289A1
Self-assembled carbon fiber bundles, method for producing same, prepreg and method for producing same
WO2022265099A1
Method for producing fiber assembly and method for producing prepreg sheet
WO2022265100A1
Method for producing carbon fiber pellets, high density streamlined pellets obtained therefrom, and method for producing reinforced thermoplastics using said pellets
JP1998503812A
Cited By
Sheet molding compound, method for manufacturing same, and carbon fiber reinforced plastic