Grinding method for wafer
The wafer grinding method addresses chipping issues by using a thermocompression bonding sheet to protect the reinforcement during grinding, ensuring stable wafer integrity and metal film adhesion.
Patent Information
- Application Number
- JP2023215967
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2023-12-21
- Publication Date
- 2024-11-21
AI Technical Summary
Existing wafer grinding technologies, such as TAIKO grinding, face issues with chipping at the inner periphery of the ring-shaped reinforcement due to the grinding wheel, which can lead to wafer cracking and poor metal film formation during the wet etching process.
A wafer grinding method that involves fixing a thermocompression bonding sheet to the back surface of the wafer, forming a circular recess and ring-shaped reinforcement, and using a grinding unit with a spindle and grinding wheels to grind the wafer while protecting the reinforcement with the bonding sheet, followed by etching and metal film formation.
The method effectively suppresses chipping at the inner circumferential top corner of the ring-shaped reinforcement, preventing wafer cracking and ensuring proper metal film formation and adhesion of the dicing tape.
Smart Images

Figure 2024162989000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for grinding a wafer. [Background technology]
[0002] In grinding the back surface of a wafer having a device region on its surface on which a plurality of devices are formed, a TAIKO (registered trademark) grinding technique is known in which the outer peripheral edge portion of the back surface of the wafer is left uncut, and only the inner portion of the back surface of the wafer corresponding to the device region inside the outer peripheral edge portion is ground to thin the wafer (see, for example, Patent Document 1).
[0003] For example, with the spread of SiP (System in Package) and the like, there is a demand for grinding technology that can thin wafers with good yield, and TAIKO grinding technology is known as one of the grinding technologies for thinning wafers. TAIKO grinding technology forms a ring-shaped reinforcing part that functions as a reinforcing part on the outer peripheral edge part of the wafer. By forming the ring-shaped reinforcing part, for example, warping of the wafer and cracking of the wafer during transportation are suppressed even after the inner part of the wafer is thinned. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2007-019461 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, there was a problem that chipping may occur toward the outer periphery of the wafer at the inner upper corner of the ring-shaped reinforcement part formed by the TAIKO grinding technology when the grinding wheel bites into the wafer. In addition, there was a problem that the chipping may increase and grow even more when the side of the grinding wheel comes into contact with the inner side of the ring-shaped reinforcement part during the formation of the recess after the grinding. The chipping occurring at the inner upper corner of the ring-shaped reinforcement part causes problems such as wafer cracking due to chipping, and the formation of recesses (wavy shape) on the upper surface of the ring-shaped reinforcement part due to the effect of the chemical solution passing through the chipping during the wet etching process, leading to poor metal film formation or poor adhesion of the dicing tape.
[0006] The present invention has been made in consideration of such problems, and its purpose is to provide a wafer grinding method that can suppress chipping formed on the inner upper corners of the ring-shaped reinforcement portion formed by TAIKO grinding. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems and achieve the object, the present invention provides a wafer grinding method for grinding a back surface of a wafer having a device region and a peripheral excess region surrounding the device region on a front surface thereof to form a circular recess and a ring-shaped reinforcing portion surrounding the circular recess, the method including a thermocompression sheet fixing step of fixing a thermocompression sheet to the back surface of the wafer, a holding step of holding the front surface side of the wafer with a chuck table having a rotation shaft on a holding surface thereof, and a ring-shaped base and a plurality of grinding wheels provided on a free end surface of the base, the grinding unit has a spindle with a grinding wheel attached to its tip, the diameter of which is equal to or less than the radius of the wafer, and the grinding wheel is positioned so that the rotational trajectory of the grinding wheel overlaps with the rotational axis of the holding surface, and the grinding unit and the chuck table are moved relatively close to each other in the direction of the rotational axis of the spindle to remove the central portion of the thermo-compression sheet and form the circular recess and the ring-shaped reinforcing portion on the back side of the wafer; and a peeling step of peeling off the thermo-compression sheet fixed to the upper surface of the ring-shaped reinforcing portion.
[0008] The method may further include an etching step of etching a bottom surface of the circular recess after the peeling step, or after the grinding step and before the peeling step, and a metal film formation step of forming a metal film on the bottom surface of the circular recess after the etching step.
[0009] The method may further include a protective member providing step of providing a protective member on the front surface of the wafer.
[0010] The thermocompression sheet may contain a filler.
[0011] The thermocompression sheet may be formed by laminating a filler-containing layer to which a filler has been added and a filler-free layer to which no filler has been added, and the filler-free layer may be laminated on at least one side of the thermocompression sheet.
[0012] In the thermocompression sheet fixing step, the thermocompression sheet may be fixed to the rear surface of the wafer with the surface of the thermocompression sheet on which the filler-free layer is laminated facing the rear surface of the wafer.
[0013] In the thermocompression sheet fixing step, the thermocompression sheet may be fixed to the back surface of the wafer with the surface of the thermocompression sheet on which the filler-free layer is laminated facing away from the back surface of the wafer.
[0014] The thermo-compression sheet may have the filler-free layer laminated on both sides of the thermo-compression sheet, and in the thermo-compression sheet fixing step, the thermo-compression sheet may be fixed to the back surface of the wafer with one side of the thermo-compression sheet on which the filler-free layer is laminated facing the back surface of the wafer and the other side of the thermo-compression sheet on which the filler-free layer is laminated facing the side opposite the back surface of the wafer. Effect of the Invention
[0015] In the present invention, a thermo-compression sheet is fixed to the back side of the wafer, which is the side to be ground, and then TAIKO grinding is performed by penetrating the thermo-compression sheet.As a result, the upper surface of the ring-shaped reinforcement part is ground while being reinforced and protected by the thermo-compression sheet, so chipping that forms on the inner upper corners of the ring-shaped reinforcement part formed by TAIKO grinding can be suppressed. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a flowchart showing an example of a processing procedure of the wafer grinding method according to the first embodiment. [Diagram 2] FIG. 2 is a perspective view illustrating the thermocompression sheet fixing step of FIG. [Diagram 3] FIG. 3 is a side cross-sectional view illustrating the thermocompression sheet fixing step of FIG. [Figure 4] FIG. 4 is a perspective view illustrating the holding step and the grinding step of FIG. [Diagram 5] FIG. 5 is a side cross-sectional view illustrating the holding step and the grinding step of FIG. [Figure 6] FIG. 6 is a perspective view illustrating the grinding step of FIG. [Figure 7] FIG. 7 is a side cross-sectional view illustrating the grinding step of FIG. [Figure 8] FIG. 8 is a side cross-sectional view illustrating a main part of the grinding step in FIG. [Figure 9] FIG. 9 is a side cross-sectional view illustrating a main part of the grinding step in FIG. [Figure 10] FIG. 10 is a side cross-sectional view illustrating the metal film forming step of FIG. [Figure 11] FIG. 11 is a perspective view illustrating the peeling step of FIG. [Figure 12] FIG. 12 is a side cross-sectional view illustrating the peeling step of FIG. [Figure 13] FIG. 13 is a perspective view illustrating a grinding step according to a comparative example. [Figure 14] FIG. 14 is a side cross-sectional view illustrating a grinding step according to a comparative example. [Figure 15] FIG. 15 is a top view illustrating a main part of the grinding step according to the comparative example. [Figure 16] FIG. 16 is a top view illustrating a main part of the grinding step according to the comparative example. [Figure 17] FIG. 17 is a cross-sectional view showing a thermocompression sheet to be thermocompression-bonded in the thermocompression-bonding sheet fixing step of the wafer grinding method according to the second embodiment. [Figure 18] FIG. 18 is a cross-sectional view showing a thermocompression sheet to be thermocompression-bonded in the thermocompression-bonding sheet fixing step of the wafer grinding method according to the third and fourth embodiments. [Figure 19] FIG. 19 is a cross-sectional view showing a thermocompression sheet to be thermocompression-bonded in a thermocompression-bonding sheet fixing step of the wafer grinding method according to the fifth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The form (embodiment) for carrying out the present invention will be described in detail with reference to the drawings. The present invention is not limited to the contents described in the following embodiment. Furthermore, the components described below include those that a person skilled in the art can easily imagine and those that are substantially the same. Furthermore, the configurations described below can be appropriately combined. Furthermore, various omissions, substitutions, or modifications of the configurations can be made without departing from the gist of the present invention.
[0018] [Embodiment 1] A wafer grinding method according to a first embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a flow chart showing an example of a processing procedure of the wafer grinding method according to the first embodiment. As shown in Fig. 1, the wafer grinding method according to the first embodiment includes a thermocompression sheet fixing step 1001, a protective member providing step 1002, a holding step 1003, a grinding step 1004, an etching step 1005, a metal film forming step 1006, and a peeling step 1007.
[0019] In the first embodiment, the wafer 100 to be ground in the wafer grinding method according to the first embodiment is a disk-shaped semiconductor wafer or an optical device wafer, etc., with a substrate made of, for example, silicon, sapphire, silicon carbide (SiC), gallium arsenide, etc., as shown in Fig. 2. The wafer 100 has a flat surface 101, and is divided by a plurality of mutually intersecting planned division lines into regions, in which device regions 104 are formed with chip-shaped devices, and a peripheral surplus region 105 in which no devices are formed and which surrounds the device region 104.
[0020] 2 and 3 are respectively a perspective view and a side cross-sectional view for explaining the thermocompression sheet fixing step 1001 in Fig. 1. The thermocompression sheet fixing step 1001 is a step of fixing a thermocompression sheet 110 to a back surface 102 on the back side of a front surface 101 of a wafer 100 by thermocompression bonding, as shown in Fig. 2 and Fig. 3.
[0021] In the first embodiment, the thermocompression sheet 110 fixed to the back surface 102 of the wafer 100 in the thermocompression sheet fixing step 1001 has a shape and size that can sufficiently cover at least the circular recess 107 (see FIGS. 6 and 7) formed in the grinding step 1004 described later in a plan view. That is, in the first embodiment, the thermocompression sheet 110 fixed to the back surface 102 of the wafer 100 in the thermocompression sheet fixing step 1001 has a shape and size that can sufficiently cover at least the inner part of the back surface 102 of the wafer 100 corresponding to the device region 104 in a plan view. In the first embodiment, the thermocompression sheet 110 fixed to the back surface 102 of the wafer 100 in the thermocompression sheet fixing step 1001 is formed in a circle having the same shape and size as the back surface 102 of the wafer 100 in a plan view, that is, the same diameter as the back surface 102 of the wafer 100 in a plan view, as shown in FIGS. 2 and 3.
[0022] In the first embodiment, the thermocompression sheet 110 fixed to the rear surface 102 of the wafer 100 in the thermocompression sheet fixing step 1001 is a thermoplastic resin sheet formed in a sheet shape from a thermoplastic resin, without having a glue layer, which is a layer made of a synthetic resin having adhesive properties such as a pressure-sensitive adhesive. The thermoplastic resin that constitutes the thermocompression sheet 110 fixed to the rear surface 102 of the wafer 100 in the thermocompression sheet fixing step 1001 has a storage modulus of 1×10 at a temperature of 10° C. or more and 30° C. or less. 6 Pa or more 1×10 9 Pa or less, and the storage modulus at temperatures between 80°C and 100°C is 1×10 6 Pa or more 1×10 7 Pa or less.
[0023] The storage modulus, together with the loss modulus (dynamic loss modulus) and loss tangent, is measured by dynamic mechanical analysis (DMA). Specifically, the storage modulus is measured according to any of the following methods: JIS K 7244-4 (non-resonant forced vibration method), JIS K 7244-5 (bending mode), and JIS K 7244-6 (shear mode) of the Japanese Industrial Standards. According to the Japanese Industrial Standards, the storage modulus is 0.01 GPa (1×10 7If the strength is less than 0.01 GPa or less than 5 GPa (1×10 7 Pa or more 5×10 9 Pa or less), it is preferable to measure using a method according to JIS K 7244-4 (non-resonant forced vibration method), and 9 In the case where the compressive strength is greater than 1 Pa, it is preferable to measure using a method in accordance with JIS K 7244-5 (bending mode).
[0024] The storage modulus generally varies depending on the temperature during measurement and the frequency (speed) of deformation applied during measurement. More specifically, the thermoplastic resin constituting the thermocompression sheet 110 has a storage modulus of 1×10 measured under conditions of a temperature of 10° C. or higher and 30° C. or lower and a deformation frequency of 0.01 Hz or higher and 10 Hz or lower. 6 Pa or more 1×10 9 The storage modulus measured under the conditions of a temperature of 80°C to 100°C and a deformation frequency of 0.01Hz to 10Hz is 1×10 6 Pa or more 1×10 7 Pa or less.
[0025] The thermoplastic resin that constitutes the thermocompression sheet 110 fixed to the back surface 102 of the wafer 100 in the thermocompression sheet fixing step 1001 has the storage elastic modulus as described above, and has the property that the storage elastic modulus decreases with an increase in temperature. Therefore, it does not have a glue layer, and can be fixed to the back surface 102 of the wafer 100 by thermocompression bonding by heating. Note that the storage elastic modulus of the resin is 1×10 6 If the storage modulus is less than 1×10 Pa, the resin will be sticky and too adhesive, forming a glue layer. 9 If it is higher than Pa, the resin may be too hard and may not be fixed to the back surface 102 of the wafer 100 .
[0026] The thermocompression sheet 110 fixed to the back surface 102 of the wafer 100 in the thermocompression sheet fixing step 1001 is specifically a polyolefin sheet formed from a polyolefin (Poly Olefine, PO)-based resin compound in a sheet shape, such as a polyethylene sheet formed from polyethylene (Poly Ethylene, PE) in a sheet shape, a polypropylene sheet formed from polypropylene (Poly Propylene, PP) in a sheet shape, or a polystyrene sheet formed from polystyrene (Poly Styrene, PS) in a sheet shape.
[0027] 2 and 3, in the thermocompression sheet fixing step 1001, the wafer 100 is placed on a holding table 10 that is sufficiently larger than the wafer 100 in a plan view with the back surface 102 side exposed facing upward, and a thermocompression sheet 110 is placed on the back surface 102 of the wafer 100 so as to sufficiently cover at least an inner portion of the back surface 102 of the wafer 100 corresponding to the device region 104 in a plan view. Note that the thermocompression sheet fixing step 1001 is not limited to this in the present invention, and the thermocompression sheet 110 may be placed on the holding table 10, and the wafer 100 may be placed on the thermocompression sheet 110 with the back surface 102 side of the wafer 100 facing the thermocompression sheet 110.
[0028] In the thermocompression sheet fixing step 1001, the thermocompression sheet 110 is then heated at a predetermined temperature (for example, 50 to 150° C. in the first embodiment) to soften it, while pressing the wafer 100 and the thermocompression sheet 110 in a direction to approach each other along the thickness direction with a predetermined pressing force (for example, 0.3 MPa or more in the first embodiment) for a predetermined time (for example, 30 seconds or more in the first embodiment), thereby thermocompression-bonding and fixing the thermocompression sheet 110 to the back surface 102 of the wafer 100. In the thermocompression sheet fixing step 1001, the thermocompression sheet 110 may be heated by a heat source provided inside the holding table 10 or inside a pressing member (not shown) having a shape and size sufficient to cover the thermocompression sheet 110 in a plan view, and pressed with this pressing member to thermocompress. In the thermocompression sheet fixing step 1001, the thermocompression sheet 110 may be heated by a heat source provided inside the holding table 10 or inside a pressure roller (not shown), while the pressure roller (not shown) is rotated from one end to the other end on the back surface 102 of the wafer 100 via the thermocompression sheet 110 to press the sheet, thereby performing thermocompression bonding. In the thermocompression sheet fixing step 1001, at least one of the thermocompression sheet 110, the wafer 100, and the holding table 10 may be heated by infrared rays.
[0029] Alternatively, in the thermocompression sheet fixing step 1001, a roller (not shown) may be rotated from one end to the other end on the back surface 102 of the wafer 100 via the thermocompression sheet 110 to bring the thermocompression sheet 110 into close contact with the back surface 102 of the wafer 100, and then the thermocompression sheet 110 may be heated and softened by blowing hot air of a predetermined temperature (for example, 150°C or higher in embodiment 1) from an industrial dryer against the thermocompression sheet 110 side, thereby thermocompression-bonding and fixing the softened thermocompression sheet 110 to the back surface 102 of the wafer 100 without pressing the thermocompression sheet 110 against the wafer 100, i.e., at a pressing force of 0 MPa.
[0030] In the thermo-compression sheet fixing step 1001, in embodiment 1, the thermo-compression sheet 110 without such an adhesive layer is fixed to the back surface 102 of the wafer 100 by thermo-compression bonding. Therefore, when the central portion 111 of the thermo-compression sheet 110 is scraped off in the grinding step 1004 performed later, there is no risk of a grinding defect such as an adhesive layer adhering to the grinding surface of the grinding stone 34 (see Figure 4, etc.) of the grinding wheel 32 (see Figure 4, etc.). Furthermore, when the outer peripheral portion 112 (see Figures 6 and 7, etc.) of the thermo-compression sheet 110 is peeled off from the upper surface of the ring-shaped reinforcement portion 108 in the peeling step 1007 performed later, there is no risk of a defect such as an adhesive layer remaining on the upper surface of the ring-shaped reinforcement portion 108.
[0031] The protective member providing step 1002 is a step of providing a protective member on the front surface 101 of the wafer 100. In the first embodiment, the protective member provided on the front surface 101 of the wafer 100 in the protective member providing step 1002 is formed, for example, in a circular shape having the same shape and size as the front surface 101 of the wafer 100 in a plan view, that is, the same diameter as the front surface 101 of the wafer 100 in a plan view.
[0032] In the first embodiment, the protective member disposed on the front surface 101 of the wafer 100 in the protective member disposing step 1002 is, for example, an adhesive tape having a base layer and a glue layer (adhesive layer). Here, the glue layer is made of synthetic resin having adhesive properties such as an adhesive, and is laminated on one side of the base layer. The base layer is made of synthetic resin. In the first embodiment, the adhesive layer side of such a protective member which is an adhesive tape is attached to the front surface 101 of the wafer 100. The protective member disposed on the front surface 101 of the wafer 100 in the protective member disposing step 1002 protects the front surface 101 of the wafer 100.
[0033] In addition, in the present invention, the protective member disposed on surface 101 of wafer 100 in protective member disposing step 1002 is not limited to a form having a base material layer and an adhesive layer, and may be a thermoplastic resin sheet formed into a sheet shape from thermoplastic resin without an adhesive layer, similar to thermocompression sheet 110.In this case, in protective member disposing step 1002, the protective member which is a thermoplastic resin sheet is fixed to surface 101 of wafer 100 by thermocompression bonding in a manner similar to that in thermocompression sheet fixing step 1001.
[0034] In the wafer grinding method according to the first embodiment, the protective member disposing step 1002 is performed after the thermocompression sheet fixing step 1001, but the present invention is not limited to this, and the protective member disposing step 1002 may be performed before the thermocompression sheet fixing step 1001, or the protective member disposing step 1002 may be omitted. Note that in the drawings of the present application, illustration of the protective member disposed on the front surface 101 of the wafer 100 in the protective member disposing step 1002 is omitted.
[0035] 4 and 5 are respectively a perspective view and a side cross-sectional view explaining the holding step 1003 and the grinding step 1004 in Fig. 1. The holding step 1003 is a step of holding the front surface 101 side of the wafer 100 by the chuck table 20 having a rotation axis 25 on the holding surface 23, as shown in Figs.
[0036] The chuck table 20 that holds the front surface 101 side of the wafer 100 in the holding step 1003 includes a disk-shaped frame 21 with a recess formed therein and a disk-shaped suction portion 22 fitted into the recess, as shown in Figs. 4 and 5. The suction portion 22 of the chuck table 20 is formed of a porous ceramic or the like with a large number of porous holes, and is connected to a vacuum suction source (not shown) via a vacuum suction path (not shown). The upper surface of the suction portion 22 of the chuck table 20 is a holding surface 23 that suction-holds the placed wafer 100 from below. In the first embodiment, the upper surface of the frame 21 and the holding surface 23 are formed in a conical shape with a slightly lower outer periphery, with the center 24 of the holding surface 23 of the chuck table 20 as the apex, as shown in Fig. 5. The holding surface 23 is not limited to this in the present invention, and may be formed flat.
[0037] The chuck table 20 that holds the front surface 101 side of the wafer 100 in the holding step 1003 is provided so as to be rotatable about a rotation axis 25 that passes through the center 24 of the holding surface 23 and is perpendicular to the bottom surface of the cone that forms the holding surface 23, by a rotation drive source (not shown) connected to the lower side of the frame 21 of the chuck table 20. The chuck table 20 can tilt the rotation axis 25 by an inclination angle within a predetermined range with respect to the Z-axis direction parallel to the vertical direction by an unillustrated rotation axis adjustment unit, and accordingly, the holding surface 23 can be tilted by the same inclination angle with respect to the horizontal plane that is parallel to the XY plane. The chuck table 20 is provided so as to be movable parallel to the horizontal direction within a certain range by an unillustrated movement unit.
[0038] In the holding step 1003, first, after performing the thermocompression sheet fixing step 1001 and the protective member arrangement step 1002, the exposed surface side of the thermocompression sheet 110, which was thermocompression-bonded and fixed to the back surface 102 of the wafer 100 in the thermocompression sheet fixing step 1001, is adsorbed and held from above by a transport pad (not shown), and the wafer is transported onto the holding surface 23 of the chuck table 20, and the adsorption and holding is released on the holding surface 23 of the chuck table 20, thereby placing the wafer 100 on the holding surface 23 of the chuck table 20 with the front surface 101 side of the wafer 100 facing the holding surface 23, as shown in Figures 4 and 5. In a holding step 1003, next, with respect to the wafer 100 placed on the holding surface 23 of the chuck table 20, the front surface 101 side of the wafer 100 is suction-held by the holding surface 23 of the chuck table 20, with the back surface 102 side of the wafer 100 to which the thermocompression sheet 110 was fixed in the thermocompression sheet fixing step 1001 being exposed upward. Note that in the holding step 1003, if a protective member has been provided on the front surface 101 of the wafer 100 by performing the protective member providing step 1002, the front surface 101 side of the wafer 100 is suction-held by the holding surface 23 of the chuck table 20 via the protective member.
[0039] 6 and 7 are respectively a perspective view and a side cross-sectional view explaining the grinding step 1004 in Fig. 1. As shown in Figs. 4, 5, 6 and 7, the grinding step 1004 is a step in which the grinding unit 30 includes a circular base 33 and a plurality of grinding wheels 34 provided on the free end surface of the base 33, and has a spindle 31 attached with a grinding wheel 32 at its tip, the diameter 35 of which is formed by the plurality of grinding wheels 34 and is equal to or smaller than the radius of the wafer 100, and the grinding unit 30 and the chuck table 20 are moved relatively close to each other in the direction of the rotation axis 36 of the spindle 31, thereby grinding off the center portion 111 of the thermocompression sheet 110 and forming a circular recess 107 and a ring-shaped reinforcing portion 108 on the back surface 102 side of the wafer 100.
[0040] The grinding unit 30 performing the grinding step 1004 includes a spindle 31 and a grinding wheel 32, as shown in Figures 4, 5, 6, and 7. The spindle 31 is provided rotatably about a rotation axis 36 parallel to the vertical direction (Z-axis direction), and supports the grinding wheel 32 rotatably about the rotation axis 36 parallel to the vertical direction, the grinding wheel 32 being detachably attached to a tip (lower end) facing downward.
[0041] The grinding wheel 32 includes an annular base 33 and a plurality of grinding wheels 34. The plurality of grinding wheels 34 are provided on a free end surface (lower surface) facing downward of the annular base 33, and are arranged in an annular shape with a diameter 35 equal to or less than the radius of the wafer 100 centered on the rotation axis 36 of the annular base 33 when the grinding wheel 32 is attached to the tip of the spindle 31. Here, the diameter 35 is determined by the distance (length) between the rotation axis 36 and the outer peripheral end of the grinding wheel 34 that is the furthest from the rotation axis 36 in the direction along the free end surface of the base 33. The plurality of grinding wheels 34 have a width roughly equivalent to the radial width of each grinding wheel 34, and draw an annular rotational locus whose outer diameter is equal to the diameter 35, by the grinding wheel 32 being attached to the tip of the spindle 31 and rotating around the rotation axis 36. In the first embodiment, the grinding wheel 34 is formed by fixing abrasive grains such as diamond, cBN (cubic boron nitride), or the like, with a bond material such as a metal bond, a resin bond, or a vitrified bond.
[0042] The grinding unit 30 performing the grinding step 1004 is disposed so that the spindle 31 faces the holding surface 23 of the chuck table 20 in the vertical direction. The rotation axis 25 of the chuck table 20 and the rotation axis 36 of the spindle 31 and grinding wheel 32 of the grinding unit 30 are disposed so as to be shifted in the horizontal direction, and by moving the chuck table 20 parallel to the horizontal direction, it is possible to adjust the horizontal shift between the rotation axis 25 and the rotation axis 36 within the grinding surface on the grinding wheel 34 side of the grinding wheel 32 and the surface to be ground on the back surface 102 side of the wafer 100 when the back surface 102 side of the wafer 100 is ground with the grinding wheel 34 of the grinding wheel 32.
[0043] The grinding unit 30 performing the grinding step 1004 further includes a grinding feed unit (not shown) and a grinding fluid supply unit (not shown). The grinding feed unit performs grinding feed to relatively move the spindle 31 of the grinding unit 30 and the grinding wheel 32 attached to the spindle 31 along a grinding feed direction (Z-axis direction parallel to the vertical direction) relative to the chuck table 20, thereby moving the spindle 31 and the grinding wheel 32 closer to and farther away from the chuck table 20 along the grinding feed direction.
[0044] The grinding feed unit is a known ball screw mechanism having a motor, a ball screw, and a guide. The grinding feed unit is configured to have a ball screw rotatably provided around the axis of the Z axis, a motor that rotates the ball screw around the axis, and a guide that supports the spindle 31 so that it can move in the Z axis direction. The grinding feed unit has a feed speed, a feed amount, and the like controlled by a control unit (not shown) that controls the drive of the motor. Here, the feed speed refers to the speed at which the grinding feed unit moves the spindle 31 and the grinding wheel 32 relatively close to and away from the chuck table 20 along the Z axis direction. The feed amount refers to the amount (height) at which the grinding feed unit moves the spindle 31 and the grinding wheel 32 relatively close to and away from the chuck table 20 along the Z axis direction. The feed speed is the feed amount per unit time.
[0045] The grinding feed unit includes an encoder that reads the rotational position of the motor, detects the relative position of the spindle 31 in the Z-axis direction with respect to the chuck table 20 based on the rotational position of the motor read by the encoder, and outputs the detected relative position to a control unit (not shown). The grinding feed unit detects the relative position of the spindle 31 in the Z-axis direction with respect to the chuck table 20, for example, at regular time intervals (for example, every second) before the start of grinding, during grinding, and after the end of grinding, to detect the feed speed and feed amount, and outputs the detected feed speed and feed amount to a control unit (not shown). The grinding feed unit is not limited to a configuration that detects the relative position of the spindle 31 in the Z-axis direction with respect to the chuck table 20 by an encoder, and may be configured with a linear scale parallel to the Z-axis direction and a reading head that is provided so as to be movable in the Z-axis direction by the grinding feed unit and that reads the graduations of the linear scale.
[0046] The grinding fluid supply unit is connected to a grinding fluid supply source not shown, and supplies grinding fluid (grinding water) such as pure water supplied from the grinding fluid supply source not shown toward the back surface 102 of the wafer 100 held on the chuck table 20.
[0047] In the grinding step 1004, as shown in Figures 4, 5, 6 and 7, first, the chuck table 20 is moved parallel to the horizontal direction to adjust the horizontal deviation between the rotation axis 25 and the rotation axis 36 within the grinding surface on the grinding wheel 34 side of the grinding wheel 32 and the ground surface on the back surface 102 side of the wafer 100 when the grinding wheel 34 of the grinding wheel 32 is used to grind the back surface 102 side of the wafer 100, thereby positioning the annular rotational trajectory of the grinding wheel 34 at a position (referred to as the specified grinding position) that overlaps with the rotation axis 25 of the holding surface 23 of the chuck table 20 and is inscribed in the inner circumference of the outer peripheral edge portion 106, which is an area corresponding to the outer peripheral excess area 105 of the back surface 102 of the wafer 100 held on the chuck table 20.
[0048] In the grinding step 1004, after the rotational trajectory of the grinding wheel 34 is positioned at a predetermined grinding position, next, with the rotational trajectory of the grinding wheel 34 positioned at the predetermined grinding position, the spindle 31 of the grinding unit 30 is rotated around the rotational axis 36 parallel to the vertical direction, thereby rotating the grinding wheel 32 attached to the lower end of the spindle 31 around the rotational axis 36 parallel to the vertical direction, while rotating the chuck table 20 that holds the wafer 100 and is arranged opposite the spindle 31 around the rotational axis 25. While supplying grinding fluid to the wafer 100 held on the rotated chuck table 20 by the grinding fluid supply unit, the rotating grinding wheel 32 is pressed along the grinding feed direction by the grinding feed unit, thereby grinding the back surface 102 side of the wafer 100 held on the chuck table 20 with the grinding wheel 34 of the grinding wheel 32.
[0049] In the grinding step 1004, by grinding in this manner, the back surface 102 of the wafer 100 is ground along the grinding surface of the grinding stone 34 of the grinding wheel 32, and the ground surface on the back surface 102 of the wafer 100 is formed parallel to the grinding surface. In the grinding step 1004, as shown in Figures 6 and 7, the grinding stone 34 of the grinding wheel 32 scrapes off the center portion 111 of the thermocompression sheet 110 fixed by thermocompression to the back surface 102 of the wafer 100, and further, only the inner portion of the back surface 102 of the wafer 100 corresponding to the device region 104 of the wafer 100 is ground to thin it, thereby performing so-called TAIKO (registered trademark) grinding, in which a circular recess 107 and a ring-shaped reinforcing portion 108 surrounding the circular recess 107 are formed on the back surface 102 of the wafer 100.
[0050] Here, the central portion 111 of the thermocompression sheet 110 is a portion of the thermocompression sheet 110 that corresponds to the device region 104 inside the outer circumferential edge portion 106 of the wafer 100. In the grinding step 1004, the circular recess 107 is formed on the back surface 102 side of the wafer 100 in a shape and size corresponding to the device region 104 of the wafer 100 in a plan view, and the ring-shaped reinforcing portion 108 is formed on the back surface 102 side of the wafer 100 in a shape and size corresponding to the outer circumferential edge portion 106 of the wafer 100 in a plan view.
[0051] In the grinding step 1004, the back surface 102 side of the wafer 100 is ground with the grinding stone 34 of the grinding wheel 32 while the feed amount is detected by the grinding feed unit, so that the depth of the circular recess 107 to be formed in the thickness direction of the wafer 100 can be controlled based on the upper surface of the ring-shaped reinforcing portion 108. Note that, in grinding while controlling the feed amount, there is a risk of an error in the depth of the circular recess 107 due to bending of the grinding unit 30 or wear of the grinding wheel 32, so it is preferable to measure the depth of the circular recess 107 using a separate non-contact thickness measuring device or the like.
[0052] In the grinding step 1004, as shown in Figures 6 and 7, the outer peripheral portion 112, which corresponds to the outer peripheral edge portion 106 of the thermo-compression sheet 110, is not removed, so that the outer peripheral portion 112 of the thermo-compression sheet 110 remains in a fixed state by being thermo-compressed to the upper surface of the ring-shaped reinforcement portion 108.
[0053] 8 and 9 are both side cross-sectional views for explaining the main part of the grinding step 1004 in Fig. 1. In the grinding step 1004, as shown in Fig. 8, the central part 111 of the thermocompression sheet 110 fixed by thermocompression to the back surface 102 of the wafer 100 is scraped off, and when the grinding stone 34 of the grinding wheel 32 bites into the back surface 102 of the wafer 100, the outer peripheral part 112 of the thermocompression sheet 110 reinforces and protects the upper surface of the ring-shaped reinforcing part 108, thereby suppressing the risk of chipping 200 (see Fig. 16) occurring in the inner peripheral upper surface corner of the ring-shaped reinforcing part 108 toward the outer periphery of the wafer 100.
[0054] In addition, in the grinding step 1004, as shown in FIG. 9, when the grinding stone 34 of the grinding wheel 32 bites into the back surface 102 of the wafer 100 and forms a circular recess 107, even when the outer peripheral side surface of the grinding stone 34 comes into contact with the inner peripheral side surface of the ring-shaped reinforcement portion 108, the outer peripheral portion 112 of the thermocompression sheet 110 reinforces and protects the upper surface of the ring-shaped reinforcement portion 108, while also coming into contact with the outer peripheral side surface of the grinding stone 34 on the inner peripheral surface side, thereby suppressing the risk of chipping 200 at the corners of the inner upper surface of the ring-shaped reinforcement portion 108 increasing and increasing toward the outer periphery of the wafer 100.
[0055] In this way, the grinding step 1004 suppresses the risk of chipping 200 occurring toward the outer periphery of the wafer 100, as well as the risk of the chipping 200 toward the outer periphery of the wafer 100 increasing and expanding, thereby suppressing cracking of the wafer 100 due to the chipping 200 and suppressing the risk of a recess (wavy shape) being formed on the upper surface of the ring-shaped reinforcement portion 108 due to the influence of the chemical solution passing through the chipping 200 when wet etching is performed in the subsequent etching step 1005, thereby suppressing the risk of poor formation of the metal film 120 (see Figure 10) formed in the subsequent metal film formation step 1006 and poor adhesion of the dicing tape.
[0056] The etching step 1005 is a step of etching the bottom surface 109 of the circular recess 107 formed in the grinding step 1004. In the etching step 1005, in the first embodiment, for example, wet etching is performed to supply a chemical solution to the bottom surface 109 of the circular recess 107, and the bottom surface 109 of the circular recess 107 is etched with the chemical solution to remove the grinding marks formed on the bottom surface 109 of the circular recess 107 in the grinding step 1004, and the bottom surface 109 of the circular recess 107 is modified to a surface state in which the metal film 120 can be suitably formed in the metal film forming step 1006 performed subsequently. Note that the etching step 1005 is not limited to wet etching using a chemical solution in the present invention, and may be, for example, plasma etching using plasma.
[0057] Fig. 10 is a side cross-sectional view for explaining the metal film forming step 1006 in Fig. 1. The metal film forming step 1006 is a step of forming a metal film 120 on the bottom surface 109 of the circular recess 107 as shown in Fig. 10 after the etching step 1005. In the metal film forming step 1006, in the first embodiment, the metal film 120 is formed on the bottom surface 109 and side surfaces of the circular recess 107 by, for example, metal vapor deposition or sputtering.
[0058] In the first embodiment, after the grinding step 1004 and before the peeling step 1007, the etching step 1005 and the metal film forming step 1006 are performed in a state in which the outer peripheral portion 112 of the thermocompression sheet 110 is thermocompression-bonded and fixed to the upper surface of the ring-shaped reinforcement portion 108, so that the outer peripheral portion 112 of the thermocompression sheet 110 can function as a mask that maintains the upper surface of the ring-shaped reinforcement portion 108 in a state in which the wet etching chemical is not supplied and in a state in which the metal film 120 is not formed. Here, when the metal film 120 is formed on the outer peripheral portion 112 of the thermocompression sheet 110 in the metal film forming step 1006, the metal film 120 formed on the outer peripheral portion 112 of the thermocompression sheet 110 is peeled off together with the outer peripheral portion 112 of the thermocompression sheet 110 in the peeling step 1007 performed later, so that the risk of the metal film 120 peeling off in places on the outer peripheral portion 112 of the thermocompression sheet 110 is suppressed. In the first embodiment, the etching step 1005 and the metal film forming step 1006 are performed after the grinding step 1004 and before the peeling step 1007, but the present invention is not limited to this and may be performed after the peeling step 1007.
[0059] 11 and 12 are respectively a perspective view and a side cross-sectional view for explaining the peeling step 1007 in Fig. 1. As shown in Fig. 11 and Fig. 12, the peeling step 1007 is a step of peeling off the thermocompression sheet 110 fixed to the upper surface of the ring-shaped reinforcing part 108. In the peeling step 1007, the outer periphery 112 of the thermocompression sheet 110 fixed by thermocompression to the upper surface of the ring-shaped reinforcing part 108 remaining in the grinding step 1004 is peeled off from the upper surface of the ring-shaped reinforcing part 108.
[0060] 13 and 14 are respectively a perspective view and a side cross-sectional view explaining the grinding step according to the comparative example. Both of FIG. 15 and FIG. 16 are top views explaining the main part of the grinding step according to the comparative example. FIG. 15 is a top view showing the entire back surface 102 side of the wafer 100 after the grinding step according to the comparative example is performed, and FIG. 16 is an enlarged view of the part shown in XVI of FIG. 15. In order to explain the first embodiment more clearly, a comparative example based on the conventional technology will be explained in comparison with the first embodiment. In the comparative example, the thermocompression sheet fixing step 1001 and the peeling step 1007 performed in conjunction with the thermocompression sheet fixing step 1001, which are the main parts of the first embodiment, are omitted in the first embodiment, and a grinding step similar to the grinding step 1004 is performed. In such a comparative example, as shown in Figures 13 and 14, if the grinding stone 34 of the grinding wheel 32 is used to grind and thin only the inner portion of the back surface 102 of the wafer 100 to which the thermocompression sheet 110 is not fixed, when the grinding stone 34 of the grinding wheel 32 bites into the back surface 102 of the wafer 100, there is a risk that chipping 200 will occur in the inner upper corner of the ring-shaped reinforcement portion 108 toward the outer periphery of the wafer 100, as shown in Figure 16. Also, when the grinding stone 34 of the grinding wheel 32 bites into the back surface 102 of the wafer 100 and forms the circular recess 107, when the outer peripheral side surface of the grinding stone 34 comes into contact with the inner peripheral side surface of the ring-shaped reinforcement portion 108, there is a risk that the chipping 200 formed in the inner upper corner of the ring-shaped reinforcement portion 108 toward the outer periphery of the wafer 100 will increase and increase.
[0061] In contrast to such comparative examples, in embodiment 1, a thermo-compression sheet fixing step 1001 is performed before performing the grinding step 1004, and a thermo-compression sheet 110 is fixed by thermo-compression to the back surface 102 of the wafer 100, which is the surface to be ground by the grinding stone 34 of the grinding wheel 32 in the grinding step 1004. Therefore, in embodiment 1, when the grinding wheel 34 of the grinding wheel 32 bites into the back surface 102 of the wafer 100, and when the grinding wheel 34 of the grinding wheel 32 bites into the back surface 102 of the wafer 100 and forms a circular recess 107, when the outer peripheral side surface of the grinding wheel 34 contacts the inner peripheral side surface of the ring-shaped reinforcement portion 108, the outer peripheral portion 112 of the thermocompression sheet 110 reinforces and protects the upper surface of the ring-shaped reinforcement portion 108, and further contacts the outer peripheral side surface of the grinding wheel 34 on the inner peripheral surface side, thereby suppressing the risk of chipping 200 occurring at the inner peripheral upper corner of the ring-shaped reinforcement portion 108 toward the outer periphery of the wafer 100, and the risk of chipping 200 increasing and increasing at the inner peripheral upper corner of the ring-shaped reinforcement portion 108 toward the outer periphery of the wafer 100.
[0062] In the wafer grinding method of embodiment 1 having the above-mentioned configuration, the thermo-compression sheet 110 is fixed to the back surface 102, which is the surface to be ground, of the wafer 100, and TAIKO grinding is performed by penetrating the thermo-compression sheet 110. As a result, the upper surface of the ring-shaped reinforcing portion 108 is ground while being reinforced and protected by the thermo-compression sheet 110, which has the effect of suppressing chipping 200 formed at the inner upper corners of the ring-shaped reinforcing portion 108 formed by TAIKO grinding.
[0063] Moreover, the wafer grinding method according to the first embodiment further includes an etching step 1005 and a metal film forming step 1006 after the peeling step 1007, or after the grinding step 1004 and before the peeling step 1007. Therefore, the wafer grinding method according to the first embodiment can further suppress the risk of a recess (wavy shape) being formed on the upper surface of the ring-shaped reinforcing part 108 due to the influence of a chemical solution passing through the chipping 200 when wet etching is performed in the etching step 1005, and thus suppress the risk of a defective formation of the metal film 120 formed in the metal film forming step 1006.
[0064] Moreover, the wafer grinding method according to the first embodiment further includes a protective member providing step 1002 of providing a protective member on the front surface 101 of the wafer 100. Therefore, the wafer grinding method according to the first embodiment can further protect the front surface 101 of the wafer 100 on which the chip-like devices are formed, during the implementation of the holding step 1003 and subsequent steps.
[0065] [Embodiment 2] A wafer grinding method according to embodiment 2 of the present invention will be described with reference to the drawings. Fig. 17 is a cross-sectional view showing a thermocompression sheet 110-2 to be thermocompressed in a thermocompression sheet fixing step 1001 of the wafer grinding method according to embodiment 2. In Fig. 17, the same parts as those in embodiment 1 are denoted by the same reference numerals, and the description thereof will be omitted.
[0066] The wafer grinding method of embodiment 2 is similar to embodiment 1 in that the thermo-compression sheet 110 fixed to the back surface 102 of the wafer 100 in the thermo-compression sheet fixing step 1001 is changed to the thermo-compression sheet 110-2 shown in FIG. 17 .
[0067] 17, the thermocompression sheet 110-2 used in the second embodiment is the thermocompression sheet 110 used in the first embodiment to which a filler 130 has been added. Specifically, the thermocompression sheet 110-2 used in the second embodiment is a filler-containing thermoplastic resin sheet obtained by forming a thermoplastic resin containing the filler 130 into a sheet shape, the thermoplastic resin being the same as the thermoplastic resin constituting the thermocompression sheet 110 used in the first embodiment, to which the filler 130 has been added.
[0068] The filler 130 added to the thermocompression sheet 110-2 in the second embodiment has a size of, for example, 0.1 nm or more and 400 nm or less. The filler 130 added to the thermocompression sheet 110-2 in the second embodiment is granular, but the present invention is not limited to this, and may have a shape such as a columnar shape like fiber. In this specification, the size of the filler 130 is defined by the particle diameter of the filler 130. There are known methods for expressing the particle diameter, such as a geometric diameter and an equivalent diameter. The geometric diameter includes the Feret diameter, the maximum diameter in a certain direction (i.e., Krummbein diameter), the Martin diameter, the sieve diameter, etc., and the equivalent diameter includes the diameter equivalent to a circle with a projected area (i.e., Heywood diameter), the diameter equivalent to a sphere with an equal surface area, the diameter equivalent to a sphere with an equal volume, the Stokes diameter, the light scattering diameter, etc. Even when the filler 130 has a shape such as a columnar shape like fiber, the size of the filler 130 can be defined in the same manner as when the filler 130 is granular.
[0069] The filler 130 added to the thermocompression sheet 110-2 in the second embodiment is preferably an inorganic filler, and specifically, fused silica, crystalline silica, alumina, calcium carbonate, calcium silicate, barium sulfate, talc, clay, magnesium oxide, aluminum oxide, beryllium oxide, iron oxide, titanium oxide, aluminum nitride, silicon nitride, boron nitride, mica, glass, quartz, mica, etc. may be preferably used. The filler 130 added to the thermocompression sheet 110-2 in the second embodiment may be a mixture of two or more of the above. The filler 130 added to the thermocompression sheet 110-2 in the second embodiment is preferably a silica such as fused silica or crystalline silica among the above inorganic fillers, and in this case, the cost of the filler 130 can be suitably suppressed.
[0070] In the thermocompression sheet 110-2, the content (mixing ratio) of filler 130 in the thermoplastic resin can be changed in the range of 0.01 wt% to 90 wt%, and the higher the content of filler 130, the higher the dressing effect will be, in which the bond material covering the abrasive grains of the grinding wheel 34 is removed by grinding with the grinding wheel 34, causing the abrasive grains to protrude, sharpening the grinding wheel 34, and improving the grinding quality of the grinding wheel 34. However, if the content of filler 130 is too high, it may become difficult for the thermocompression sheet 110-2 to be thermocompressed to the back surface 102 of the wafer 100, or the entire sheet may become brittle, so an appropriate ratio is selected.
[0071] The grinding step 1004 of the wafer grinding method according to the second embodiment is a modification of the grinding step 1004 of the wafer grinding method according to the first embodiment, in which instead of grinding off the central portion 111 of the thermo-compression bonded sheet 110, the central portion 111 of the thermo-compression bonded sheet 110-2 to which the filler 130 has been added is ground off. In the wafer grinding method according to the second embodiment, when the central portion 111 of the thermo-compression bonded sheet 110-2 to which the filler 130 has been added is ground by the grinding wheel 34 in the grinding step 1004, a dressing effect of dressing the grinding wheel 34 is obtained by the filler 130 added and mixed in the thermo-compression bonded sheet 110-2.
[0072] The wafer grinding method according to the second embodiment having the above-mentioned configuration is obtained by changing the thermocompression sheet 110 fixed to the back surface 102 of the wafer 100 in the thermocompression sheet fixing step 1001 in the first embodiment to a thermocompression sheet 110-2 to which the filler 130 is further added. Therefore, the wafer grinding method according to the second embodiment has the same effect as the first embodiment, and further, when the center portion 111 of the thermocompression sheet 110-2 to which the filler 130 is added is ground by the grinding wheel 34 in the grinding step 1004, the grinding wheel 34 is dressed by the filler 130 added and mixed in the thermocompression sheet 110-2, thereby suppressing deterioration of the grinding quality of the grinding wheel 34, and thereby, it has an effect of more suitably suppressing chipping 200 formed at the inner circumferential upper surface corner portion of the ring-shaped reinforcing portion 108 formed by TAIKO grinding.
[0073] [Embodiment 3] A wafer grinding method according to embodiment 3 of the present invention will be described with reference to the drawings. Fig. 18 is a cross-sectional view showing a thermocompression sheet 110-3 to be thermocompressed in the thermocompression sheet fixing step 1001 of the wafer grinding method according to embodiment 3 and embodiment 4. In Fig. 18, the same parts as those in embodiment 1 and embodiment 2 are denoted by the same reference numerals, and the description thereof will be omitted.
[0074] The wafer grinding method of embodiment 3 is similar to embodiments 1 and 2 in that the thermo-compression sheet 110, 110-2 fixed to the back surface 102 of the wafer 100 in the thermo-compression sheet fixing step 1001 is changed to the thermo-compression sheet 110-3 shown in FIG. 18, and the thermo-compression sheet 110-3 is fixed to the back surface 102 of the wafer 100 with the surface on which the filler-free layer 132 of the thermo-compression sheet 110-3 is laminated facing the back surface 102 of the wafer 100; other configurations are the same as those of embodiments 1 and 2.
[0075] The thermocompression sheet 110-3 used in the third embodiment is formed by laminating a filler-containing layer 131 and a filler-free layer 132 as shown in Fig. 18, and the filler-free layer 132 is laminated on at least one surface side of the thermocompression sheet 110-3. Here, the filler-containing layer 131 is formed in a sheet shape (layer shape) of a thermoplastic resin containing a filler 130, which is a thermoplastic resin similar to the thermoplastic resin constituting the thermocompression sheet 110 used in the first embodiment, to which the filler 130 is added, in the same manner as the thermoplastic resin constituting the thermocompression sheet 110 used in the first embodiment, as in the thermoplastic resin containing a filler 130, in which the filler 130 is not added, in the same thermoplastic resin constituting the thermocompression sheet 110 used in the first embodiment. The filler-free layer 132 is formed in a sheet shape (layer shape) of a thermoplastic resin without a filler 130, which is a thermoplastic resin without a filler 130, which is a thermoplastic resin similar to the thermoplastic resin constituting the thermocompression sheet 110 used in the first embodiment, in which the filler 130 is not added.
[0076] In the example shown in Figure 18, the thermo-compression sheet 110-3 used in embodiment 3 is formed by laminating one filler-containing layer 131 and one filler-free layer 132, but the present invention is not limited to this, and as long as at least one filler-containing layer 131 and one filler-free layer 132 are laminated and the filler-free layer 132 is laminated on at least one side of the thermo-compression sheet 110-3, multiple filler-containing layers 131 may be laminated, or multiple filler-free layers 132 may be laminated.
[0077] In the wafer grinding method of embodiment 3, the filler-containing layer 131 does not come into contact with the back surface 102 of the wafer 100, and the filler 130 does not come into contact with the back surface 102 of the wafer 100, thereby reducing the risk of the filler 130 contaminating the back surface 102 of the wafer 100.
[0078] The grinding step 1004 of the wafer grinding method according to the embodiment 3 is a modification of the grinding step 1004 of the wafer grinding method according to the embodiment 1, in which instead of grinding off the central portion 111 of the thermocompression bonded sheet 110, the central portion 111 of the filler-containing layer 131 to which the filler 130 of the thermocompression bonded sheet 110-3 is added and the filler-free layer 132 to which the filler 130 is not added is ground off. In the wafer grinding method according to the embodiment 3, when the central portion 111 of the filler-containing layer 131 to which the filler 130 is added is ground by the grinding wheel 34 in the grinding step 1004, a dressing effect of dressing the grinding wheel 34 is obtained by the filler 130 added and mixed in the filler-containing layer 131.
[0079] The wafer grinding method of embodiment 3 having the above-mentioned configuration is a modification of embodiments 1 and 2 in which the thermo-compression sheets 110, 110-2 fixed to the back surface 102 of the wafer 100 in the thermo-compression sheet fixing step 1001 are changed to a thermo-compression sheet 110-3 formed by laminating a filler-containing layer 131 and a filler-free layer 132, with the filler-free layer 132 laminated on at least one side, and the thermo-compression sheet 110-3 is fixed to the back surface 102 of the wafer 100 with the side on which the filler-free layer 132 of the thermo-compression sheet 110-3 is laminated facing the back surface 102 of the wafer 100. For this reason, the wafer grinding method of embodiment 3 achieves the same effects as those of embodiments 1 and 2, and further achieves the effect of preventing deterioration of the grinding quality of the grinding wheel 34 by dressing the grinding wheel 34 when grinding the filler-containing layer 131 with the grinding wheel 34 in the grinding step 1004, while preventing the filler 130 from contacting the back surface 102 of the wafer 100 by the filler-free layer 132, thereby reducing the risk of contamination of the back surface 102 of the wafer 100 by the filler 130.
[0080] [Embodiment 4] A method for grinding a wafer according to a fourth embodiment of the present invention will be described with reference to the drawings. The method for grinding a wafer according to the fourth embodiment is modified from the third embodiment in that, instead of fixing the filler-free layer 132 side of the thermocompression bonding sheet 110-3 facing the back surface 102 of the wafer 100 in the thermocompression bonding sheet fixing step 1001, the thermocompression bonding sheet 110-3 is fixed to the back surface 102 of the wafer 100 with the filler-free layer 132 side of the thermocompression bonding sheet 110-3 facing the surface opposite to the back surface 102 of the wafer 100, and other configurations are the same as those of the third embodiment.
[0081] In the wafer grinding method of embodiment 4, in holding step 1003, the filler-free layer 132 side of the thermo-compression bonded sheet 110-4, which has been fixed by thermo-compression bonding to the back surface 102 of the wafer 100 in thermo-compression sheet fixing step 1001, is adsorbed and held from above by a transport pad, and transported onto the holding surface 23 of the chuck table 20. Therefore, the filler-containing layer 131 does not come into contact with the transport pad, and the filler 130 does not come into contact with the transport pad, thereby reducing the risk of the transport pad being contaminated by the filler 130.
[0082] The wafer grinding method of embodiment 4, like the wafer grinding method of embodiment 3, in grinding step 1004, when the central portion 111 of the filler-containing layer 131 of the thermocompression bonded sheet 110-3 to which the filler 130 has been added is ground with the grinding wheel 34, a dressing effect is obtained in which the grinding wheel 34 is dressed by the filler 130 added and mixed into the filler-containing layer 131.
[0083] The wafer grinding method of embodiment 4 having the above-mentioned configuration is a modification of embodiment 3, in which in the thermo-compression sheet fixing step 1001, instead of fixing the filler-free layer 132 side of the thermo-compression sheet 110-3 facing the back surface 102 of the wafer 100, the filler-free layer 132 side of the thermo-compression sheet 110-3 is fixed to the back surface 102 of the wafer 100 with the filler-free layer 132 side of the thermo-compression sheet 110-3 facing the surface opposite the back surface 102 of the wafer 100. For this reason, the wafer grinding method according to the fourth embodiment has the same effects as those of the first and second embodiments, and further has the effect of preventing deterioration of the grinding quality of the grinding wheel 34 by dressing the grinding wheel 34 when grinding the filler-containing layer 131 with the grinding wheel 34 in the grinding step 1004, while preventing the filler 130 from coming into contact with the transport pad that adsorbs and holds the exposed side of the wafer 100 opposite the back surface 102 from above by the filler-free layer 132, thereby preventing contamination of the transport pad by the filler 130.
[0084] [Embodiment 5] A wafer grinding method according to embodiment 5 of the present invention will be described with reference to the drawings. Fig. 19 is a cross-sectional view showing a thermocompression sheet 110-4 to be thermocompressed in a thermocompression sheet fixing step 1001 of the wafer grinding method according to embodiment 5. In Fig. 19, the same parts as those in embodiment 1, embodiment 2, embodiment 3, and embodiment 4 are denoted by the same reference numerals, and the description thereof will be omitted.
[0085] The wafer grinding method of embodiment 5 is similar to that of embodiments 1, 2, 3, and 4, except that the thermo-compression sheets 110, 110-2, and 110-3 fixed to the rear surface 102 of the wafer 100 in the thermo-compression sheet fixing step 1001 are changed to a thermo-compression sheet 110-4 shown in FIG. 19, and the other configurations are the same as those of embodiments 1, 2, 3, and 4.
[0086] The thermocompression sheet 110-4 used in the fifth embodiment is formed by laminating a filler-containing layer 131 and a filler-free layer 132, and the filler-free layer 132 is laminated on both sides of the thermocompression sheet 110-4, as shown in Fig. 19. Note that the thermocompression sheet 110-4 used in the fifth embodiment is formed by laminating one filler-containing layer 131 and two filler-free layers 132 in the example shown in Fig. 19, but the present invention is not limited to this, and as long as at least one filler-containing layer 131 is laminated and the filler-free layer 132 is laminated on both sides of the thermocompression sheet 110-4, a plurality of filler-containing layers 131 may be laminated, or three or more filler-free layers 132 may be laminated.
[0087] In the wafer grinding method according to the fifth embodiment, as in the third embodiment, the filler-containing layer 131 does not contact the back surface 102 of the wafer 100, and the filler 130 does not contact the back surface 102 of the wafer 100, so that it is possible to suppress the risk of the back surface 102 of the wafer 100 being contaminated by the filler 130. Also, in the wafer grinding method according to the fifth embodiment, as in the fourth embodiment, in the holding step 1003, the filler-free layer 132 side of the thermocompression-bonded sheet 110-4 fixed by thermocompression to the back surface 102 of the wafer 100 in the thermocompression-bonded sheet fixing step 1001 is adsorbed and held from above by the conveying pad, and conveyed onto the holding surface 23 of the chuck table 20. Therefore, the filler-containing layer 131 does not contact the conveying pad, and the filler 130 does not contact the conveying pad, so that it is possible to suppress the risk of the conveying pad being contaminated by the filler 130.
[0088] The wafer grinding method of embodiment 5, like the wafer grinding methods of embodiments 3 and 4, in grinding step 1004, when the central portion 111 of the filler-containing layer 131 of the thermocompression bonded sheet 110-4 to which the filler 130 has been added is ground with the grinding wheel 34, a dressing effect is obtained in which the filler 130 added and mixed into the filler-containing layer 131 dresses the grinding wheel 34.
[0089] The wafer grinding method of embodiment 5 having the above-mentioned configuration is the same as embodiments 1, 2, 3 and 4, except that the thermocompression sheets 110, 110-2 and 110-3 fixed to the back surface 102 of the wafer 100 in the thermocompression sheet fixing step 1001 are changed to a thermocompression sheet 110-4. For this reason, the wafer grinding method according to the fifth embodiment has the same effects as those of the first and second embodiments, and further maintains the ability to suppress deterioration of the grinding quality of the grinding wheel 34 by dressing the grinding wheel 34 when grinding the filler-containing layer 131 with the grinding wheel 34 in the grinding step 1004. Similarly to the third embodiment, the filler-free layer 132 prevents the filler 130 from contacting the back surface 102 of the wafer 100, thereby suppressing the risk of contamination of the back surface 102 of the wafer 100 by the filler 130. Similarly to the fourth embodiment, the filler-free layer 132 prevents the filler 130 from contacting the transport pad that adsorbs and holds the exposed side of the wafer 100 opposite the back surface 102 from above, thereby suppressing the risk of contamination of the transport pad by the filler 130.
[0090] It should be noted that the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the gist of the present invention. [Explanation of symbols]
[0091] 20 Chuck table 23 Holding surface 25 Rotational Axis 30 Grinding unit 31 Spindle 32 Grinding Wheel 33 Foundation 34 Grinding Wheel 35 diameter 36 Rotational Axis 100 wafers 101 Surface 102 Back side 104 Device Area 105 Surplus outer area 107 Circular recess 108 Ring-shaped reinforcement 109 Bottom 110, 110-2, 110-3, 110-4 Heat-sealed sheet 111 Central part 120 Metal Film 130 Filler 131 Filler-containing layer 132 Filler-free layer 1001 Thermocompression sheet fixing step 1002 Protective member disposing step 1003 Retention Step 1004 Grinding step 1005 Etching step 1006 Metal film formation step 1007 Peeling step
Claims
1. A method for grinding a wafer, the method comprising grinding a back surface of a wafer having a device region and a peripheral excess region surrounding the device region on a front surface thereof, to form a circular recess and a ring-shaped reinforcing portion surrounding the circular recess, the method comprising the steps of: a thermocompression sheet fixing step of fixing a thermocompression sheet to the back surface of the wafer; a holding step of holding the front surface side of the wafer by a chuck table having a rotation axis on a holding surface; a grinding step in which a grinding unit includes an annular base and a plurality of grinding wheels provided on a free end surface of the base, the grinding wheel being formed by the plurality of grinding wheels and having a spindle attached to its tip, the grinding wheel having a diameter equal to or smaller than the radius of the wafer, and the grinding unit and the chuck table are moved relatively close to each other in the direction of the rotation axis of the spindle while the grinding unit is positioned at a position where the rotation path of the grinding wheel overlaps with the rotation axis of the holding surface, thereby grinding away a central portion of the thermocompression sheet and forming the circular recess and the ring-shaped reinforcing portion on the back side of the wafer; a peeling step of peeling off the thermocompression sheet fixed to the upper surface of the ring-shaped reinforcing portion; A method for grinding a wafer comprising the steps of:
2. After the peeling step, or after the grinding step and before the peeling step, an etching step of etching a bottom surface of the circular recess; a metal film forming step of forming a metal film on a bottom surface of the circular recess after the etching step; The method of claim 1 further comprising:
3. a protective member providing step of providing a protective member on the front surface of the wafer; 3. The method for grinding a wafer according to claim 1, further comprising:
4. 2. The method for grinding a wafer according to claim 1, wherein the thermocompression sheet contains a filler.
5. 2. The wafer grinding method according to claim 1, wherein the thermocompression sheet is formed by laminating a filler-containing layer to which a filler has been added and a filler-free layer to which no filler has been added, and the filler-free layer is laminated on at least one side of the thermocompression sheet.
6. 6. The wafer grinding method according to claim 5, wherein in the thermocompression sheet fixing step, the surface of the thermocompression sheet on which the filler-free layer is laminated faces the back surface of the wafer, and the thermocompression sheet is fixed to the back surface of the wafer.
7. The wafer grinding method according to claim 5, wherein in the thermocompression sheet fixing step, the surface of the thermocompression sheet on which the filler-free layer is laminated is faced opposite the back surface of the wafer, and the thermocompression sheet is fixed to the back surface of the wafer.
8. The thermocompression sheet has the filler-free layer laminated on both sides of the thermocompression sheet, 6. The wafer grinding method of claim 5, wherein in the thermocompression sheet fixing step, the thermocompression sheet is fixed to the back surface of the wafer with one surface of the thermocompression sheet on which the filler-free layer is laminated facing the back surface of the wafer and the other surface of the thermocompression sheet on which the filler-free layer is laminated facing the side opposite the back surface of the wafer.
Citation Information
Patent Citations
Method for processing wafer and wafer
JP2007019461A