Method for producing optical film
By temporarily attaching a protective film to the film base material using conductive rolls and applying the coating layer immediately after peeling, the method addresses scratches and defects, ensuring high-quality optical films with uniform alignment and reduced defects.
Patent Information
- Application Number
- JP2024152956
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for forming optical films on film base materials using a roll-to-roll process are prone to scratches and defects due to surface conditions, leading to non-uniform coating thickness and poor alignment of liquid crystal molecules, which can cause optical defects.
A method involving the temporary attachment of a protective film to the film base material using conductive nip rolls to prevent scratches and internal charging, followed by immediate application of a coating layer after peeling off the protective film, ensuring minimal contact with conveyance rolls.
This approach significantly reduces scratches and streak-like defects in the coating layer, maintaining optical uniformity and alignment of liquid crystal molecules, resulting in high-quality optical films with improved display characteristics.
Smart Images

Figure 2024163263000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an optical film. [Background technology]
[0002] Thin coating films are used as optical films that have functions such as optical compensation for liquid crystal displays and anti-reflection of external light for organic electroluminescence devices. Thin films have low self-supporting properties and are difficult to handle as a single unit, so a coating layer is formed by applying a solution onto a support such as a plastic film, and the coating layer is dried or processed while still in close contact with the support.
[0003] For example, Patent Document 1 discloses a method of forming a laminated phase difference film by applying a resin solution onto a support to form a resin coating layer and stretching a laminate of the support and the coating layer. Patent Document 2 discloses a method of preparing an aligned liquid crystal layer by applying a liquid crystal composition onto a stretched film as a support and aligning the liquid crystal compound homogeneously along the stretching direction (alignment direction) of the film. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2004-46068 A [Patent Document 2] WO2016 / 121856 Summary of the Invention [Problem to be solved by the invention]
[0005] In the method of forming a coating layer by coating a solution on a film substrate as a support while conveying it in the longitudinal direction by the roll-to-roll method, scratches on the film substrate can cause defects such as transfer of scratches to the coating layer and poor alignment of liquid crystal molecules. In addition, coating defects caused by the surface condition of the film substrate can cause uneven film thickness and optical properties of the coating layer. [Means for solving the problem]
[0006] One embodiment of the present invention is a method for producing a long optical film, in which a coating layer is formed on a first main surface of a long film substrate having a first main surface and a second main surface.
[0007] First, a long film substrate and a protective film are sandwiched and laminated by a pair of nip rolls to obtain a laminate in which the protective film is peelably attached to the first main surface of the film substrate (lamination process). Both the first roll and the second roll constituting the pair of nip rolls are conductive.
[0008] The laminate of the film substrate and the protective film is transported by rolls along the longitudinal direction to a peeling section (first transport step), where the protective film is peeled off from the first main surface of the film substrate (protective film peeling step). The film substrate from which the protective film has been peeled off is transported along the longitudinal direction of the film substrate from the peeling section to a coating section (second transport step), where a coating is applied onto the first main surface of the film substrate (coating step), to obtain a laminate having a coating layer on the first main surface of the film substrate.
[0009] The coating liquid may be a liquid crystal composition containing a liquid crystal compound. The liquid crystal composition may contain a photocurable liquid crystal compound. After applying the liquid crystal composition containing the photocurable liquid crystal compound onto a film substrate, the liquid crystal compound may be photocured.
[0010] The film substrate may have an alignment regulating force for aligning the liquid crystal molecules in a predetermined direction. The film substrate may be, for example, a stretched film in which the molecules are oriented non-parallel to the longitudinal direction, or an obliquely stretched film.
[0011] The optical film may be one in which another optical layer is laminated on the coating layer by roll-to-roll. The optical layer laminated on the coating layer may include a polarizer. The optical film may be a circular polarizing plate in which the coating layer and a polarizer are laminated. Effect of the Invention
[0012] Since the protective film is temporarily attached to the film substrate until immediately before the coating liquid is applied, the occurrence of scratches on the film substrate due to roll transport is suppressed. In addition, by sandwiching and laminating the film substrate and the protective film between two conductive rolls, internal charging of the laminate is unlikely to occur, and the occurrence of coating defects due to charging of the film substrate is suppressed. Therefore, a coating layer with fewer defects such as scratches and streaks caused by the film substrate can be obtained. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a cross-sectional view of an optical film having a coating layer on a film substrate. [Diagram 2] FIG. 2 is a cross-sectional view of a laminate in which a protective film is temporarily attached onto a film substrate. [Diagram 3] FIG. 2 is a diagram showing an outline of a process for bonding a film substrate and a protective film. [Figure 4] FIG. 1 is a diagram showing an overview of a film-forming apparatus and a film-forming process for forming a coating layer on a film substrate. [Diagram 5] FIG. 2 is a perspective view showing an example of the shape of a pressure roll. [Figure 6] FIG. 1 is a cross-sectional view of an optical film according to an embodiment. [Figure 7] FIG. 1 is a cross-sectional view of an optical film according to an embodiment. [Figure 8] FIG. 1 is a cross-sectional view of an optical film according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] [Process overview] In the present invention, a coating layer is formed by applying a solution onto one main surface of a long film substrate. Fig. 1 is a cross-sectional view of an optical film 9 having a coating layer 3 provided on a first main surface 1A of a film substrate 1. Fig. 2 is a cross-sectional view of a laminate 8 having a protective film 2 peelably attached onto the first main surface 1A of the film substrate 1.
[0015] 3 is a conceptual diagram showing an outline of a lamination device and lamination process for laminating a film substrate 1 and a protective film 2 to obtain a laminate 8. In FIG. 3, a roll 28 in which a long protective film 2 is wound in a roll shape is wound around an unwinding roll 29. The protective film unwound from the roll 28 is continuously transported downstream of a transport path formed along transport rolls 44, 45, and transported to a laminating section 40.
[0016] The laminating section 40 includes a pair of nip rolls 41, 42. The film substrate 1 and the protective film 2 transported from the upstream side (the left side of the figure) are sandwiched between the top and bottom by the pair of nip rolls consisting of the first roll 41 and the second roll 42, and are laminated together, to obtain a laminate 8 in which the protective film 2 is peelably attached onto the film substrate 1 (laminating step). As will be described in detail later, the first roll 41 in contact with the film substrate 1 and the second roll 42 in contact with the protective film 2 are both conductive rolls.
[0017] The laminate of the film substrate 1 and the protective film 2 is continuously transported downstream of a transport path formed along transport rolls 46, 47, and is wound up by a winding roll 49 to obtain a rolled body 80 in which the long film of the laminate 8 is wound into a roll.
[0018] Fig. 4 is a conceptual diagram showing an overview of a film-forming apparatus and film-forming process for forming a coating layer 3 on a film substrate 1. In Fig. 4, a roll 80 of a laminate 8 is wound around an unwinding roll 81. The laminate 8 unwound from the roll 80 moves continuously to the downstream side of a transport path formed along transport rolls 83, 85, and 87, and is transported to a peeling section 10 (first transport step).
[0019] In the peeling section 10, the protective film 2 is peeled off from the film substrate 1 (peeling step). By peeling off the protective film 2, the first main surface 1A of the film substrate 1 is exposed. After the protective film is peeled off, the film substrate 1 is transported from the peeling section 10 to the coating section 30 (second transport step). In the coating section 30, a coating liquid is applied onto the first main surface 1A of the film substrate 1. (coating process).
[0020] A laminate 9 (optical film) in which a coating layer 3 is formed on a first main surface 1A of a film substrate 1 is wound up by a winding roll 91 to obtain a long rolled optical film 90. Heating may be performed in a heating section 50 between the coating section 30 and the winding roll 91. When the coating liquid contains a photopolymerizable component such as a photopolymerizable liquid crystal compound, photocuring may be performed in a curing section 60.
[0021] When a solution is applied to a film substrate while it is being transported by roll-to-roll, scratches are likely to occur along the length of the film substrate due to contact and friction with the transport roll. If scratches exist on the film substrate, when a coating layer is formed on the substrate, the scratches on the film substrate may be transferred to the coating layer, which may cause optical defects. In addition, when a liquid crystal composition is applied on the film substrate, the liquid crystal molecules tend to be aligned along the extension direction of the scratches, which may cause alignment defects.
[0022] In the embodiment of the present invention, the protective film 2 is releasably attached to the first main surface 1A of the film substrate 1. Since the protective film 2 is attached to the first main surface 1A of the film substrate 1 from the unwinding roll 81 until the film substrate reaches the peeling section 10 (first conveying step), the first main surface 1A of the film substrate 1 does not come into direct contact with the conveying roll 87 in the first conveying step. Since the coating liquid is applied onto the first main surface 1A of the film substrate 1 immediately after the protective film 2 is peeled off from the film substrate 1, it is possible to prevent the first main surface of the film substrate from being scratched due to contact with the conveying roll 87, and to suppress the transfer of scratches to the coating layer 3 and poor alignment of liquid crystal molecules.
[0023] In this embodiment, since coating is performed immediately after peeling the protective film 2 from the film substrate 1, the peeling unit 10 and the coating unit 30 are arranged close to each other, and the transport path of the film substrate in the second transport step is short. Therefore, the state of attachment between the film substrate and the protective film, and physical effects such as static electricity when peeling the protective film from the film substrate in the peeling unit 10 may affect the application of the coating liquid in the coating unit 30. Specifically, regions where the coating layer is thin are formed in stripes extending in the width direction, and when the optical film is applied to an image display device, these may be visually recognized as stripe-like unevenness.
[0024] In one embodiment of the present invention, the pair of nip rolls 41, 42 that bond the film substrate 1 and the protective film 2 together are conductive, thereby suppressing the occurrence of streaky unevenness extending in the width direction as described above.
[0025] When a coating liquid was applied to a film substrate immediately after peeling off the protective film, a sample in which streaky unevenness occurred in the coating layer was analyzed, and no thickness unevenness or physical deformation was observed in the film substrate after peeling off the coating layer. Therefore, it is considered that the streaky unevenness in the thickness of the coating layer formed on the film substrate is caused by repelling due to the electrostatic charge of the film substrate when the coating liquid is applied to the surface of the film substrate.
[0026] One cause of the electrostatic charge of the film substrate is the electrostatic charge generated when the protective film is peeled off. However, even when the electrostatic charge of the film substrate after the protective film is peeled off is eliminated by a static elimination bar, the above-mentioned streaky unevenness was not sufficiently eliminated. In order to further examine the electrostatic charge of the film substrate, a toner test was carried out in which a toner was attached to the surface of the film. It was confirmed that the toner was attached in a line extending in the width direction to both the laminate in which the protective film was attached to the film substrate and the film substrate alone. From this result, it is presumed that when the laminate of the film substrate and the protective film is electrostatically charged, the electrostatic state (internal electrostatic charge) of the film substrate is maintained even after the protective film is peeled off, which causes the coating liquid to repel, and the streaky unevenness is formed in the coating layer.
[0027] In the embodiment of the present invention, the first roll 41 and the second roll 42 constituting the pair of nip rolls are conductive, and therefore it is possible to prevent charging of the laminate 8 due to charging of the nip rolls when laminating the film substrate 1 and the protective film 2 in the laminating section 40. Therefore, even after the protective film 2 is peeled off, there is little internal charging of the film substrate 1, which suppresses repelling when applying a coating liquid to the first main surface 1A of the film substrate 1, and it is considered that this makes it possible to prevent the occurrence of streaky thickness unevenness due to poor coating.
[0028] [material] Each material used in this embodiment will be described below.
[0029] <Coating liquid> The coating liquid applied onto the film substrate 1 is a solid component constituting the coating layer 3. It is a solution containing a solute and a solvent that dissolves and disperses the solids. Various resin materials and liquid crystal materials are used as the solids.
[0030] Examples of the resin material for the coating layer include cellulose-based resins such as acetyl cellulose, polyester-based resins, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, maleimide-based resins, polyolefin-based resins, (meth)acrylic-based resins, cyclic polyolefin resins (norbornene-based resins), polyarylate-based resins, polystyrene-based resins, polyvinyl alcohol-based resins, and polysulfone-based resins.
[0031] A liquid crystal composition containing a liquid crystal compound is applied onto a film substrate 1, the liquid crystal compound is aligned in a predetermined direction, and then the aligned state is fixed to form a coating layer (liquid crystal layer) in which the liquid crystal molecules are aligned in a predetermined direction.
[0032] Examples of the liquid crystal compound include rod-shaped liquid crystal compounds and discotic liquid crystal compounds. The rod-shaped liquid crystal compound is preferred as the liquid crystal compound because it is easily homogeneously oriented due to the orientation control force of the film substrate. The rod-shaped liquid crystal compound may be a main chain type liquid crystal or a side chain type liquid crystal. The rod-shaped liquid crystal compound may be a liquid crystal polymer or a polymerized product of a polymerizable liquid crystal compound. As long as the liquid crystal compound (monomer) before polymerization exhibits liquid crystallinity, it may not exhibit liquid crystallinity after polymerization.
[0033] The liquid crystal compound is preferably a thermotropic liquid crystal that exhibits liquid crystallinity upon heating. Thermotropic liquid crystals undergo phase transitions between a crystal phase, a liquid crystal phase, and an isotropic phase with a change in temperature. The liquid crystal compound contained in the liquid crystal composition may be any of nematic liquid crystals, smectic liquid crystals, and cholesteric liquid crystals. Nematic liquid crystals may be provided with cholesteric alignment by adding a chiral agent.
[0034] Examples of rod-shaped liquid crystal compounds exhibiting thermotropic properties include azomethines, azoxys, cyanobiphenyls, cyanophenyl esters, benzoic acid esters, cyclohexanecarboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, and alkenylcyclohexylbenzonitriles.
[0035] Examples of the polymerizable liquid crystal compound include a polymerizable liquid crystal compound in which the alignment state of a rod-shaped liquid crystal compound can be fixed by using a polymer binder, a polymerizable liquid crystal compound having a polymerizable functional group in which the alignment state of a liquid crystal compound can be fixed by polymerization, etc. Among these, a photocurable liquid crystal compound having a photocurable functional group is preferred.
[0036] The photocurable liquid crystal compound (liquid crystal monomer) has a mesogen group and at least one photocurable functional group in one molecule. The temperature at which the liquid crystal monomer exhibits liquid crystallinity (liquid crystal phase transition temperature) is preferably 40 to 200°C, more preferably 50 to 150°C, and even more preferably 55 to 100°C.
[0037] Examples of the mesogenic group of the liquid crystal monomer include cyclic structures such as a biphenyl group, a phenylbenzoate group, a phenylcyclohexane group, an azoxybenzene group, an azomethine group, an azobenzene group, a phenylpyrimidine group, a diphenylacetylene group, a diphenylbenzoate group, a bicyclohexane group, a cyclohexylbenzene group, and a terphenyl group. The terminals of these cyclic units may have a substituent such as a cyano group, an alkyl group, an alkoxy group, or a halogen group.
[0038] Examples of the photocurable functional group include a (meth)acryloyl group, an epoxy group, and a vinyl ether group. Among them, a (meth)acryloyl group is preferable. The photocurable liquid crystal monomer preferably has two or more photocurable functional groups in one molecule. By using a liquid crystal monomer containing two or more photocurable functional groups, a crosslinked structure is introduced into the liquid crystal layer after photocuring, which tends to improve the durability of the optical film.
[0039] Any suitable liquid crystal monomer may be used as the photocurable liquid crystal monomer. For example, see International Publication No. 00 / 37585, U.S. Patent No. 5,211,877, U.S. Patent No. 4,388,453, International Publication No. 93 / 22397, European Patent No. 0,261,712, German Patent No. 19,504,224, German Patent No. 4,408,171, British Patent No. 2,280,445, Japanese Patent Publication No. 2017-206460, International Publication No. 2014 / 126113, International Publication No. 2016 / 114348, International Publication No. 2014 / 010325, Japanese Patent Publication No. 2015 JP-200877A, JP-2010-31223A, WO 2011 / 050896A, JP-2011-207765A, JP-2010-31223A, JP-2010-270108A, WO 2008 / 119427A, JP-2008-107767A, JP-2008-273925A, WO 2016 / 125839A, JP-2008-273925A, etc. By selecting the liquid crystal monomer, it is also possible to adjust the expression of birefringence and the wavelength dispersion of retardation.
[0040] In addition to the liquid crystal monomer, the liquid crystal composition may contain a compound that controls the alignment of the liquid crystal monomer in a predetermined direction. For example, by including a side-chain liquid crystal polymer in the liquid crystal composition, the liquid crystal compound (monomer) can be aligned homeotropically. In addition, by adding a chiral agent to the liquid crystal composition, the liquid crystal compound can be aligned cholesterically.
[0041] The liquid crystal composition may contain a photopolymerization initiator. When the liquid crystal monomer is cured by irradiation with ultraviolet light, the liquid crystal composition preferably contains a photopolymerization initiator (photoradical generator) that generates radicals by irradiation with light in order to promote photocuring. Types of Liquid Crystal Monomer Depending on the type of photocurable functional group, a photocation generator or a photoanion generator may be used. The amount of the photopolymerization initiator used is about 0.01 to 10 parts by weight based on 100 parts by weight of the liquid crystal monomer. In addition to the photopolymerization initiator, a sensitizer or the like may be used.
[0042] A liquid crystal composition can be prepared by mixing a liquid crystal monomer and, if necessary, various alignment control agents, a polymerization initiator, and the like, with a solvent.
[0043] (solvent) The solvent of the coating liquid is not particularly limited as long as it can dissolve the solute and does not corrode the substrate (or has low corrosiveness), and examples of the solvent include halogenated hydrocarbons such as chloroform, dichloromethane, carbon tetrachloride, dichloroethane, tetrachloroethane, trichloroethylene, tetrachloroethylene, chlorobenzene, and orthodichlorobenzene; phenols such as phenol and parachlorophenol; aromatic hydrocarbons such as benzene, toluene, xylene, methoxybenzene, and 1,2-dimethoxybenzene; acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, cyclopentanone, 2-pyrrolidone, and N-methyl- Examples of suitable solvents include ketone solvents such as 2-pyrrolidone, ester solvents such as ethyl acetate and butyl acetate, alcohol solvents such as t-butyl alcohol, glycerin, ethylene glycol, triethylene glycol, ethylene glycol monomethyl ether, diethylene glycol dimethyl ether, propylene glycol, dipropylene glycol, and 2-methyl-2,4-pentanediol, amide solvents such as dimethylformamide and dimethylacetamide, nitrile solvents such as acetonitrile and butyronitrile, ethyl solvents such as diethyl ether, dibutyl ether, and tetrahydrofuran, ethyl cellosolve, and butyl cellosolve. A mixture of two or more solvents may be used.
[0044] The solid content of the coating liquid is usually about 5 to 60% by weight. The coating liquid may contain additives such as a surfactant and a leveling agent.
[0045] <Film substrate> By using a long film substrate 1 as the substrate, a series of steps from application of the coating liquid to drying can be performed by roll-to-roll. When the coating liquid is a liquid crystal composition, operations such as alignment treatment of the liquid crystal molecules after coating and photocuring can also be performed as a series of steps on the film substrate 1. In addition, the process of laminating the coating layer 3 formed on the film substrate 1 to another substrate can also be performed by roll-to-roll, improving the productivity of the optical film.
[0046] The width of the film substrate 1 is preferably 30 cm or more, and may be 50 cm or more, 80 cm or more, 100 cm or more, or 120 cm or more. From the viewpoint of productivity of the optical film, the larger the width of the film substrate 1, the more preferable it is, but it is generally 500 cm or less, and may be 400 cm or less, or 300 cm or less. The length of the film substrate is preferably 100 m or more, and may be 300 m or more, 500 m or more, 800 m or more, 1000 m or more, or 1200 m or more. The upper limit of the length of the film substrate 1 is not particularly limited, but it is generally 10000 m or less, and may be 7000 m or less, or 5000 m or less. The thickness of the film substrate 1 is preferably about 10 to 200 μm.
[0047] The resin material constituting the film substrate 1 is not particularly limited as long as it is insoluble in the solvent of the coating liquid and can withstand processes such as drying, orientation processing, and hardening, and examples of the resin material include polyesters such as polyethylene terephthalate and polyethylene naphthalate; polyolefins such as polyethylene and polypropylene; cyclic polyolefins such as norbornene-based polymers; cellulose-based polymers such as diacetyl cellulose and triacetyl cellulose; acrylic polymers; styrene-based polymers; polycarbonates, polyamides, polyimides, etc.
[0048] Films made of hydrophobic resin materials such as polyolefin, cyclic polyolefin, and acrylic polymers are prone to internal charging when bonded to the protective film 2, which can cause coating defects when a coating liquid is applied after the protective film is peeled off. As described above, the pair of nip rolls 41, 42 that bond the film substrate 1 and the protective film 2 together are conductive, which suppresses charging of the laminate 8, and therefore coating defects can be prevented even when a hydrophobic resin film is used as the film substrate 1.
[0049] The film substrate 1 may have an alignment regulating force for aligning the liquid crystal molecules in a predetermined direction. For example, the film substrate 1 may have an alignment film on the first main surface. An appropriate alignment film may be selected depending on the type of liquid crystal compound, the material of the substrate, and the like. Examples of the alignment film for homogeneously aligning the liquid crystal molecules in a predetermined direction include polyimide-based or polyvinyl alcohol-based alignment films that have been subjected to a rubbing treatment. A photo-alignment film may also be used. A resin film may be subjected to a rubbing treatment without providing an alignment film.
[0050] The film substrate 1 may have an alignment film for homeotropically aligning liquid crystal molecules. Examples of alignment agents for forming an alignment film (vertical alignment film) with homeotropic alignment properties include lecithin, stearic acid, hexadecyltrimethylammonium bromide, octadecylamine hydrochloride, monobasic carboxylate chromium complexes, organic silanes such as silane coupling agents and siloxane compounds, perfluorodimethylcyclohexane, tetrafluoroethylene, polytetrafluoroethylene, and the like.
[0051] A stretched film may be used as the film substrate 1. In a stretched film, the resin material (polymer) constituting the film is oriented in the stretching direction, and has the effect of aligning liquid crystal molecules along the stretching direction. By using a stretched film, even if an alignment film is not formed on the film substrate, it is possible to provide an alignment regulating force for aligning liquid crystal molecules in a predetermined direction. Since it is not necessary to form an alignment film, the manufacturing cost of the optical film can be reduced. Furthermore, by not providing an alignment film, contamination due to rubbing residue and alignment defects can be prevented.
[0052] The stretching direction of the stretched film (the orientation direction of the polymer) is not particularly limited, and may be parallel or non-parallel to the longitudinal direction of the film substrate. By using a stretched film in which the molecules are oriented non-parallel to the longitudinal direction, a liquid crystal layer in which the liquid crystal molecules are oriented non-parallel to the longitudinal direction can be formed as the coating layer 3.
[0053] The stretching ratio of the stretched film may be such that it can exert an orientation control force, for example, about 1.1 to 5 times. The stretched film may be a biaxially stretched film. Even if a biaxially stretched film is used, if the stretching ratios in the longitudinal direction and the transverse direction are different, the liquid crystal molecules can be aligned along the direction with the larger stretching ratio.
[0054] The stretched film may be an obliquely stretched film. Since an obliquely stretched film has an orientation axis in a direction that is neither parallel nor perpendicular to the longitudinal direction (for example, a direction at an angle of 10 to 80° to the longitudinal direction), by using an obliquely stretched film as the film substrate 1, a liquid crystal layer can be formed in which liquid crystal molecules are oriented in a direction that is neither parallel nor perpendicular to the longitudinal direction.
[0055] <Protective film> The protective film 2 temporarily attached to the first main surface 1A of the film substrate 1 preferably has an adhesive layer 292 on one surface of a core material 291 as shown in Fig. 2. The protective film 2 may have an antistatic layer (not shown) on the back surface of the core material 291 (the surface opposite to the surface on which the adhesive layer is formed).
[0056] (Core material) The material of the core material 291 of the protective film 2 is not particularly limited as long as it has flexibility, and metal foil, resin film, etc. are used. Resin film is preferable because the material is inexpensive and has excellent processability. Specific examples of the resin material constituting the core material 291 include those mentioned above as the resin material of the film substrate 1. The core material 291 may be a stretched film. The thickness of the core material 291 is not particularly limited. From the viewpoint of achieving both self-supporting properties and flexibility, the thickness of the core material 291 is preferably about 10 to 100 μm.
[0057] (Adhesive layer) The adhesive layer 292 may be made of an adhesive used in general adhesive tapes, etc., as long as it can be attached to the film substrate 1 and can be peeled off from the film substrate 1. The protective film 2 may be a self-adhesive film in which the resin material constituting the core material 291 and the resin material of the adhesive layer 292 are integrally molded by multilayer extrusion.
[0058] The composition of the adhesive constituting the adhesive layer 292 is not particularly limited, and an adhesive having an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyvinyl ether, a vinyl acetate / vinyl chloride copolymer, a modified polyolefin, an epoxy-based polymer, a fluorine-based polymer, a rubber-based polymer such as natural rubber, synthetic rubber, or the like as a base polymer can be appropriately selected and used. In particular, an acrylic adhesive having an acrylic polymer as a base polymer is preferably used, since the adhesive strength (peeling strength) is easily adjusted and little adhesive is left behind on the film substrate 1 as an adherend.
[0059] The acrylic base polymer preferably has a main skeleton of a monomer unit of (meth)acrylic acid alkyl ester. The (meth)acrylic acid alkyl ester having an alkyl group with 1 to 20 carbon atoms is preferably used as the (meth)acrylic acid alkyl ester. The content of the (meth)acrylic acid alkyl ester is preferably 40% by weight or more, more preferably 50% by weight or more, and even more preferably 60% by weight or more, based on the total amount of the monomer components constituting the base polymer. The acrylic polymer may be a copolymer of a plurality of (meth)acrylic acid alkyl esters. The arrangement of the constituent monomer units may be random or block.
[0060] The acrylic base polymer preferably contains a monomer component having a crosslinkable functional group as a copolymerization component. Examples of the monomer having a crosslinkable functional group include a hydroxyl group-containing monomer and a carboxyl group-containing monomer. Among them, it is preferable that the base polymer contains a hydroxyl group-containing monomer such as 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate as a copolymerization component. The hydroxyl group and carboxyl group of the base polymer become reaction sites with the crosslinking agent. By introducing a crosslinked structure into the base polymer, the cohesive strength of the adhesive is improved, and the adhesive shows an appropriate adhesive strength to the film substrate as the adherend, and the peeling force when peeling the protective film 2 from the film substrate 1 tends to decrease.
[0061] The molecular weight of the base polymer is appropriately adjusted so that the pressure-sensitive adhesive layer 292 has a desired adhesive strength, and for example, the weight average molecular weight in polystyrene equivalent is about 50,000 to 2 million, preferably about 70,000 to 1.8 million, more preferably about 100,000 to 1.5 million, and even more preferably about 200,000 to 1 million. When a crosslinked structure is introduced into the base polymer, it is preferable that the molecular weight of the base polymer before the introduction of the crosslinked structure is in the above range.
[0062] A crosslinked structure may be introduced into the base polymer for the purpose of adjusting the adhesive strength of the adhesive layer 292. For example, a crosslinked structure is introduced by adding a crosslinking agent to a solution obtained after polymerization of the base polymer, and heating the solution as necessary.
[0063] Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, carbodiimide-based crosslinking agents, and metal chelate-based crosslinking agents. Among them, isocyanate-based crosslinking agents and epoxy-based crosslinking agents are preferred because they are highly reactive with the hydroxyl group and carboxyl group of the base polymer and can easily introduce a crosslinked structure. The amount of the crosslinking agent used may be appropriately adjusted according to the composition and molecular weight of the base polymer, the desired adhesive properties, and the like. In order to provide the adhesive with an appropriate cohesive force and adjust the peeling force when peeling the protective film from the adherend to an appropriate range, the amount of the crosslinking agent used is preferably 0.5 parts by weight or more, more preferably 1 part by weight or more, and even more preferably 1.5 parts by weight or more, relative to 100 parts by weight of the base polymer. In order to provide an appropriate adhesive property to the adherend, the amount of the crosslinking agent used is preferably 20 parts by weight or less, more preferably 15 parts by weight or less, and even more preferably 10 parts by weight or less, relative to 100 parts by weight of the base polymer.
[0064] By introducing a crosslinked structure into the base polymer, the gel fraction of the adhesive increases, and as the viscous behavior decreases, the peeling force when peeling the protective film from the adherend tends to decrease. The gel fraction of the adhesive layer 292 is preferably 70.0% or more, more preferably 80.0% or more, and even more preferably 90.0% or more. If the gel fraction of the adhesive layer 292 is excessively large, the wettability to the adherend may decrease and the adhesive force may become insufficient. Therefore, the gel fraction of the adhesive layer 292 is preferably 99% or less, and more preferably 98% or less. The gel fraction can be determined as the insoluble content in a solvent such as ethyl acetate, and specifically, it is determined as the weight fraction (unit: weight %) of the insoluble content after immersing the adhesive layer in ethyl acetate at 23° C. for 7 days relative to the sample before immersion. In general, the gel fraction of a polymer is equal to the degree of crosslinking, and the more crosslinked parts in the polymer, the higher the gel fraction.
[0065] The adhesive layer 292 may contain additives such as a silane coupling agent, a tackifier, a plasticizer, a softener, an anti-deterioration agent, a filler, a colorant, an ultraviolet absorber, an antioxidant, a surfactant, and an antistatic agent.
[0066] The thickness of the adhesive layer 292 is not particularly limited, but from the viewpoint of achieving both adhesive strength to the adherend and ease of releasability from the adherend, the thickness of the adhesive layer 292 is preferably 1 to 50 μm, more preferably 2 to 40 μm, and even more preferably 3 to 35 μm. The thinner the adhesive layer 292 is, the more easily it is releasable from the adherend.
[0067] The peeling force when peeling the protective film 2 from the film substrate 1 is preferably 1.5 N / 50 mm or less, and may be 1.0 N / 50 mm or less or 0.8 N / 50 mm or less. The peeling force is a measured value in a peeling test in which the protective film is peeled from the film substrate under the conditions of a peeling angle of 180° and a pulling speed of 10 m / min. By reducing the peeling force, it is possible to suppress zipping when peeling the protective film from the film substrate. In addition, since the vibration of the film substrate 1 caused by the peeling force of the protective film 2 is reduced, the running state of the film substrate 1 in the coating section 30 (on the backup roll 31) is stabilized, and uneven coating of the coating liquid can be suppressed.
[0068] From the viewpoint of suppressing zipping and uneven coating, it is preferable that the peeling force of the protective film 2 is small. On the other hand, if the peeling force is too small, when the laminate of the film substrate and the protective film is transported by rolls, the protective film may be unintentionally peeled off from the film substrate, which may cause transport defects. Therefore, the peeling force when peeling the protective film from the film substrate is preferably 0.05 N / 50 mm or more, and may be 0.1 N / 50 mm or more, 0.15 N / 50 mm or more, or 0.2 N / 50 mm or more.
[0069] (Antistatic layer) The protective film 2 may have an antistatic layer on the back surface of the core material 291. By providing the antistatic layer, the surface resistance of the back surface 2A of the protective film 2 is reduced, and charging can be more effectively suppressed when the film substrate 1 and the protective film 2 are bonded together. Furthermore, by providing the protective film 2 with an antistatic layer, charging of the film substrate 1 when the protective film 2 is peeled off from the film substrate 1 can be prevented, and adhesion of dust to the film substrate 1 and coating defects caused by static electricity can be suppressed.
[0070] The antistatic layer may be, for example, a layer formed by incorporating an antistatic component into a binder resin. As the binder resin, various types of resins such as a thermosetting resin, an ultraviolet-curing resin, an electron beam curing resin, and a two-liquid mixed resin may be adopted. As the antistatic component, an organic or inorganic conductive substance, various antistatic agents, and the like may be used. As the organic conductive substance, conductive polymers such as polyaniline, polypyrrole, polythiophene, polyethyleneimine, and allylamine polymers may be used. As the inorganic conductive substance, various metals, alloys, and conductive metal oxides may be used. The inorganic conductive substance is preferably contained in the antistatic layer as fine particles having a particle diameter of 0.1 μm or less (typically 0.01 μm to 0.1 μm). The antistatic component may be a cationic antistatic agent, an anionic antistatic agent, an amphoteric antistatic agent, a nonionic antistatic agent, and the like.
[0071] The surface resistance of the back surface 2A of the protective film 2 is 1×10 10 Ω / sq or less, 5×10 9 Ω / sq or less, 1×10 9 Ω / sq or less, or 5×10 8 The surface resistance may be Ω / sq or less. The surface resistance is generally 1×10 3 Ω / sq or more, 1×10 4 Ω / sq or more, or 1×10 5 The smaller the surface resistance of the back surface 2A of the protective film 2, the more likely it is that charging will be suppressed when the film substrate 1 and the protective film 2 are attached to each other and when the protective film 2 is peeled off from the film substrate 1.
[0072] [Optical film fabrication] A laminate 8 is formed by laminating an adhesive layer 292 of a protective film 2 to one surface of a film substrate 1, and the protective film 2 is peeled off from the film substrate 1 of the laminate 8, and a coating layer 3 is formed on a first main surface 1A of the film substrate 1, thereby obtaining a laminate (optical film) 9 including a coating layer 3 on the film substrate 1. Each step will be described below, focusing on a case where a liquid crystal composition containing a liquid crystal compound is used as the coating liquid and an aligned liquid crystal layer is formed as the coating layer 3.
[0073] <Lamination process> As shown in FIG. 3, while the film substrate 1 and the protective film 2 are each transported by rolls, the film substrate 1 and the protective film 2 are sandwiched and laminated by a pair of nip rolls 41, 42 in a laminating section 40 to form a laminate 8. The laminating step may be performed continuously with the manufacturing step of the film substrate 1. For example, when the film substrate 1 is a stretched film, the protective film 2 may be laminated on the film substrate 1 by roll-to-roll before the stretched film is wound into a roll. By laminating the protective film 2 continuously with the manufacturing step of the film substrate 1, the number of times the rolls come into contact with the first main surface 1A of the film substrate 1 can be reduced, and the occurrence of scratches can be suppressed.
[0074] As described above, the first roll 41 and the second roll 42 constituting the pair of nip rolls are both conductive. Examples of conductive rolls include metal rolls and conductive rubber rolls. The conductive roll only needs to have a conductive surface in contact with the film substrate 1 and the protective film 2, and may be a coated roll in which the outer peripheral surface of an insulating material is coated with a conductive material. The surface resistance of the conductive roll is, for example, 1×10 10 Ω / sq or less, 1×10 9 Ω / sq or less, 1×10 8 Ω / sq or less or 1×10 7 It may be Ω / sq or less.
[0075] The metal roll may be an insulating material (e.g., a resin material) with a metal coating applied to the outer circumferential surface. The conductive rubber roll may be a metal roll or a resin roll with a conductive rubber coating on the outer circumferential surface. Examples of the conductive rubber material constituting the conductive rubber roll include rubber materials such as natural rubber, butadiene rubber, acrylic rubber, silicone rubber, urethane rubber, and fluororubber mixed with a conductive material such as carbon black.
[0076] The first roll 41 in contact with the film substrate 1 and the second roll 42 in contact with the protective film 2 may be the same type of roll or different types of rolls. For example, the nip rolls 41 and 42 may both be metal rolls, both may be conductive rubber rolls, or one may be a metal roll and the other a conductive rubber roll. From the viewpoint of suppressing bonding defects such as air bubbles at the bonding interface, it is preferable that at least one of the rolls 41 and 42 is a conductive rubber roll. Both the rolls 41 and 42 may be conductive rubber rolls. Silicone rubber is particularly preferable as the rubber material for the conductive rubber roll because it is easy to adjust the hardness and to uniformize the distribution of the nip pressure in the width direction.
[0077] <First conveying process> The laminate 8 in which the protective film 2 is laminated to the first main surface 1A of the film substrate 1 is once wound up as a roll-shaped wound body 80 and set on an unwinding roll 81. The laminate 8 unwound from the wound body 80 set on the unwinding roll 81 moves continuously to the downstream side of a transport path formed along transport rolls 83, 85, and 87, and is transported to a peeling section 10.
[0078] 3 and 4, the laminate 8 of the film substrate 1 and the protective film 2 is once wound into a roll-shaped wound body, but the step of bonding the film substrate 1 and the protective film 2 to form the laminate 8 (the bonding step described above) and the first transport step may be carried out consecutively. For example, after bonding the film substrate 1 and the protective film 2, the laminate 8 may be transported directly to the peeling section 10 without being wound up.
[0079] <Peeling process> In the peeling step, the protective film 2 is peeled off from the laminate 8 transported to the peeling section 10, and the first main surface 1A of the film substrate 1 is exposed. The method of peeling off the protective film is not particularly limited, but a method of peeling on the peeling roll 11 is common. If the transport rolls 13 and 23 downstream of the peeling roll 11 are arranged so that the wrap angle of the protective film 2 with respect to the peeling roll 11 is larger than the wrap angle of the film substrate 1 with respect to the peeling roll 11, the protective film 2 can be peeled off from the film substrate 1 on the peeling roll 11. The peeling roll may be a pair of nip rolls that sandwich the laminate 8 from above and below. The protective film 2 peeled off from the first main surface of the film substrate 1 is transported along the transport path by the transport rolls 23 and 25, and is taken up as a roll 20 by the take-up roll 21.
[0080] <Second conveying process> In the second conveying step, the film substrate 1 after the protective film 2 is peeled off is conveyed to the coating section 30. While the film substrate 1 after the protective film 2 is peeled off in the peeling section 10 is conveyed from the peeling section 10 to the coating section 30, the first main surface 1A of the film substrate 1 is exposed. In this embodiment, the conveying path of the film substrate 1 in the second conveying step is short and there is little opportunity for the first main surface 1A of the film substrate 1 to come into contact with the conveying roll, so that the frequency of occurrence of scratches on the film substrate in the second conveying step is low.
[0081] By preventing the transport roll from coming into contact with the first main surface 1A of the film substrate 1 while transporting the film substrate 1 from the peeling section 10 (peeling roll 11) to the coating section 30 (backup roll 31), it is possible to prevent scratches on the first main surface 1A of the film substrate 1 during the second transport process.
[0082] 4, in the second conveying step, a roll 15 may come into contact with the first main surface 1A of the film substrate 1. When the roll 15 comes into contact with the first main surface 1A of the film substrate 1, a force acts on the film substrate 1 pressing it from the first main surface side (the lower side in the figure) toward the upper side in the figure. This reduces vibration of the film substrate 1 caused by the peeling force of the protective film 2, and can suppress uneven application of the coating liquid.
[0083] In the transport path (second transport step) of the film substrate 1 from when the protective film 2 is peeled off in the peeling section 10 until when the coating liquid is applied in the application section 30, the roll 15 in contact with the first main surface 1A of the film substrate 1 can act as a “pressure roll” for the film substrate 1.
[0084] The pressure roll does not need to be in contact with the entire width of the film substrate 1 as long as it can suppress vibration of the film substrate 1 caused by peeling of the protective film 2 at the peeling section 10. The pressure roll may be in contact with only both ends of the film substrate 1 in the width direction and not in contact with the center portion in the width direction. For example, a barbell-shaped roll 151 as shown in FIG. 5 can be used as the pressure roll 15 that contacts the first main surface 1A of the film substrate 1.
[0085] The roll 151 has cylindrical rolls 15R and 15L at both ends, and the rolls 15R and 15L at both ends are connected via a connecting shaft 15C having a smaller diameter than the rolls. When this roll 151 is used, the roll 151 comes into contact with only both ends in the width direction of the film substrate, and does not come into contact with the center of the film substrate in the width direction.
[0086] In the second conveying step, scratches may be formed on the first main surface of the film substrate at both ends in the width direction (areas where the rolls 15R and 15L contact) of the film substrate due to contact with the rolls 15. However, if these areas are designated as non-product areas and only the center in the width direction that does not contact the rolls 15 is designated as the product area, an optical film (coating layer 3) with fewer defects due to scratches on the film substrate 1 can be obtained. For example, if the coating liquid is applied only to the center in the width direction of the film substrate 1 and a coating layer is not formed on both ends in the width direction of the film substrate, only the center in the width direction becomes the product area. In addition, at an appropriate stage after the formation of the coating layer, the areas at both ends may be cut and removed from the product by a method such as punching the film or slitting the ends, and only the center in the width direction of the film substrate may be designated as the product area.
[0087] In this manner, when the roll contacts the first main surface 1A of the film substrate 1 in the second conveying step, it is preferable that the pressing roll contacts the first main surface 1A at both ends in the width direction and does not contact the first main surface in the center in the width direction. In this embodiment, vibration of the film substrate 1 caused by peeling of the protective film 2 is suppressed, uneven application of the coating layer 3 can be reduced, and a coating layer 3 with fewer defects caused by scratches on the film substrate 1 can be obtained.
[0088] At each of both ends of the film substrate 1, the width of the portion where the film substrate and the pressure roll contact each other is, for example, 1 to 50 cm. If the width of the portion where the film substrate and the pressure roll contact each other is too small, the vibration suppression effect of the film substrate may be insufficient, or the running property of the film substrate may be deteriorated. If the width of the portion where the film substrate and the pressure roll contact each other is too large, the width of the non-product region of the optical film becomes large, which causes a decrease in production efficiency and yield. The width of the portion where the film substrate and the pressure roll contact each other may be 2 cm or more, 3 cm or more, or 5 cm or more, or may be 30 cm or less, 25 cm or less, 20 cm or less, 15 cm or less, or 10 cm or less.
[0089] The pressure rolls may be disposed so as to extend outward from both ends in the width direction of the film substrate 1, or may be disposed more inward than both ends in the width direction. When the pressure rolls are disposed more inward than both ends in the width direction of the film substrate 1, the distance from the ends in the width direction of the film substrate to the pressure rolls may be within 30 cm, within 20 cm, within 15 cm, within 10 cm, within 5 cm, within 3 cm, or within 1 cm.
[0090] After the protective film 2 is peeled off in the peeling section 10, the pressing roll in contact with the first main surface 1A of the film substrate 1 before the coating liquid is applied in the coating section 30 may be any pressing roll capable of suppressing vibration of the film substrate by pressing both ends of the film substrate, and the shape of the pressing roll is not limited to the barbell shape shown in FIG. 5. For example, two rolls may be arranged separately at both ends in the width direction. The pressing roll in contact with the first main surface 1A of the film substrate 1 may be a nip roll that is paired with a roll in contact with the second main surface 1B of the film substrate 1 and holds the film substrate 1 between them. Two or more pressing rolls in contact with the first main surface 1A of the film substrate 1 may be provided between the peeling section 10 and the coating section 30.
[0091] In the second conveying step, the means for suppressing vibration of the film substrate 1 by pressing the film substrate from the first main surface 1A side of the film substrate 1 does not necessarily have to be a rotating body. For example, a pin or the like for pressing the film substrate from the first main surface side (the lower side in the figure) toward the second main surface side may be disposed between the peeling unit 10 and the coating unit 30 as a film pressing mechanism.
[0092] In the second conveying step, both ends of the film substrate may be held by tenter clips. In this case, the regions of both ends in the width direction of the film substrate are pressed from both the first and second main surfaces without contacting the width direction central portion of the film substrate with a roll or the like, thereby suppressing vibration of the film substrate 1 caused by peeling of the protective film 2. In this case, the lower clip in contact with the first main surface of the film substrate acts as a film pressing mechanism.
[0093] As shown in FIG. 4, in the second conveying step between the peeling section 10 and the coating section 30, by bringing the roll 13 into contact with the second main surface 1B of the film substrate 1, the film substrate 1 is pressed from the second main surface 1B side as well, so that vibration of the film substrate 1 caused by the peeling force of the protective film 2 can be more effectively suppressed.
[0094] The roll 13 in contact with the second main surface 1B of the film substrate 1 may be in contact with only both ends of the film substrate, or may be in contact with the entire width of the film substrate. From the viewpoint of transportability of the film substrate, it is preferable that the roll 13 be in contact with the entire width of the second main surface of the film substrate.
[0095] <Coating process> A coating liquid is applied onto the first main surface 1A of the film substrate 1 transported to the coating unit 30. In the embodiment shown in Fig. 4, the coating liquid discharged from a die 33 is applied onto the first main surface 1A of the film substrate 1 with the second main surface 1B of the film substrate 1 in contact with the backup roll 31.
[0096] There is no particular limitation on the method for applying the coating liquid onto the film substrate 1. In addition to die coating, examples of the application method include kiss roll coating, gravure coating, reverse coating, spray coating, Mayer bar coating, knife roll coating, and air knife coating. The thickness of the coating liquid is preferably adjusted so that the thickness of the coating layer 3 after drying the solvent is about 0.1 to 20 μm.
[0097] In this embodiment, the protective film 2 is temporarily attached to and protected on the first main surface 1A of the film substrate 1 until immediately before the coating step, so that the occurrence of scratches on the first main surface 1A of the film substrate 1 due to roll transport is suppressed. Furthermore, by sandwiching and bonding the film substrate 1 and the protective film 2 between two conductive rolls 41, 42, internal charging of the laminate 8 is unlikely to occur, and the occurrence of coating defects due to charging of the film substrate 1 after peeling off the protective film 2 is suppressed. Therefore, it is possible to form a coating layer 3 with few defects such as scratches and streaks caused by the film substrate 1.
[0098] <Post-coating process> The film substrate 1 after the coating liquid is applied may be heated in a heating section 50. The heating section 50 includes, for example, a heating furnace 55, and while the film substrate 1 is transported through the heating furnace 55, the film substrate 1 and the coating liquid applied thereon are heated. For example, the solvent of the coating liquid can be removed by heating.
[0099] When the coating liquid is a liquid crystal composition and the liquid crystal compound contained in the liquid crystal composition is a thermotropic liquid crystal, the liquid crystal composition layer is heated to a liquid crystal phase, and the liquid crystal compound is aligned in a predetermined direction. Specifically, the liquid crystal composition applied on the film substrate is heated to a temperature equal to or higher than the N (nematic phase)-I (isotropic liquid phase) transition temperature to be in an isotropic liquid state. From there, the liquid crystal composition is gradually cooled as necessary to express the nematic phase. At this time, it is desirable to hold the temperature at which the liquid crystal phase is exhibited once, and grow the liquid crystal phase domain to form a monodomain. Alternatively, after applying the liquid crystal composition, the temperature may be held for a certain period of time within the temperature range at which the nematic phase is expressed to align the liquid crystal molecules in a predetermined direction.
[0100] The heating temperature for aligning the liquid crystal compound in a predetermined direction may be appropriately selected depending on the type of liquid crystal composition, and is usually about 40 to 200°C. If the heating temperature is too low, the transition to the liquid crystal phase tends to be insufficient, and if the heating temperature is too high, alignment defects may increase. The heating time may be adjusted so that the liquid crystal phase domain grows sufficiently, and is usually about 30 seconds to 30 minutes.
[0101] After the liquid crystal compound is oriented by heating, it is preferable to cool the liquid crystal compound to a temperature equal to or lower than the glass transition temperature. The cooling method is not particularly limited, and may be, for example, by removing the liquid crystal compound from the heated atmosphere to room temperature. Forced cooling such as air cooling or water cooling may also be performed.
[0102] When the liquid crystal compound has a curing property, it is preferable to perform curing in the curing section 60. For example, when the liquid crystal compound has a photocuring property, photocuring is performed in a state where the photocurable liquid crystal compound (liquid crystal monomer) has liquid crystal regularity. The light irradiated from the light source 61 may be any light capable of polymerizing the photocurable liquid crystal compound, and typically, ultraviolet or visible light having a wavelength of 250 to 450 nm is used. When the liquid crystal composition contains a photopolymerization initiator, light having a wavelength to which the photopolymerization initiator is sensitive may be selected. As the irradiation light source, a low pressure mercury lamp, a high pressure mercury lamp, an extra-high pressure mercury lamp, a metal halide lamp, a xenon lamp, an LED, a black light, a chemical lamp, or the like is used. In order to promote the photocuring reaction, it is preferable to perform the light irradiation under an inert gas atmosphere such as nitrogen gas.
[0103] During photocuring, the liquid crystal compound can be aligned in a predetermined direction by using polarized light in a predetermined direction. As described above, when the liquid crystal compound is aligned by the alignment regulating force of the film substrate 1, the irradiated light may be unpolarized (natural light).
[0104] The irradiation intensity may be appropriately adjusted depending on the composition of the liquid crystal composition, the amount of the photopolymerization initiator added, etc. The irradiation energy (accumulated irradiation light amount) is usually 20 to 10,000 mJ / cm 2 Approximately 50 to 5000 mJ / cm 2 is preferable, and 100 to 800 mJ / cm 2 In order to promote the photocuring reaction, the photoirradiation may be carried out under heating conditions.
[0105] The polymerized product obtained by photocuring the liquid crystal monomer is non-liquid crystal, and transition between liquid crystal phase, glass phase, and crystal phase does not occur due to temperature change. Therefore, the liquid crystal layer photocured in a state in which the liquid crystal monomer is aligned in a predetermined direction is unlikely to undergo change in molecular orientation due to temperature change. In addition, the liquid crystal layer has a significantly larger birefringence than a film made of a non-liquid crystal material, so the thickness of an optically anisotropic element having a desired retardation can be significantly reduced.
[0106] The optical properties of the coating layer (liquid crystal layer) 3 are not particularly limited. The in-plane retardation and thickness retardation of the coating layer 3 may be appropriately set according to the application. When the liquid crystal molecules are homogeneously aligned, the in-plane retardation of the coating layer 3 is, for example, about 20 to 1000 nm. When the coating layer 3 is a quarter-wave plate, the in-plane retardation is preferably 100 to 180 nm, more preferably 120 to 150 nm. When the coating layer 3 is a half-wave plate, the in-plane retardation is preferably 200 to 340 nm, more preferably 240 to 300 nm. When the liquid crystal is homeotropically aligned, the in-plane retardation of the coating layer 3 is approximately 0 (for example, 5 nm or less, preferably 3 nm or less), and the absolute value of the thickness retardation is about 30 to 500 nm.
[0107] The retardation of the coating layer 3 such as a liquid crystal layer is proportional to the thickness. When applying the coating liquid, if a portion with a locally small thickness is formed due to repelling on the surface of the film substrate, the retardation of that portion becomes small, resulting in optical unevenness in the display device. As described above, in this embodiment, the film substrate and the protective film are sandwiched and bonded together by a nip roll composed of two conductive rolls, so that internal charging during bonding is unlikely to occur, and the occurrence of streaky thickness unevenness due to coating defects is suppressed. Therefore, retardation unevenness due to thickness unevenness of the optical film (coating layer) is unlikely to occur, and the optical uniformity is excellent.
[0108] The orientation direction of the liquid crystal molecules in the coating layer (liquid crystal layer) 3 may be parallel or non-parallel to the longitudinal direction of the film substrate 1 (the roll-to-roll transport direction). As described above, by utilizing the orientation regulating force of an obliquely stretched film or the like, a liquid crystal layer in which the liquid crystal molecules are oriented non-parallel to the longitudinal direction can be formed. When the liquid crystal molecules are oriented non-parallel to the longitudinal direction, if there is a scratch on the film substrate along the longitudinal direction, the liquid crystal layer formed thereon will have the liquid crystal molecules oriented in the longitudinal direction along the scratch, causing poor orientation. As described above, by applying a liquid crystal composition onto the film substrate 1 immediately after peeling off the protective film 2 temporarily attached to the film substrate 1, it is possible to suppress the occurrence of scratches on the film substrate and reduce poor orientation of the liquid crystal layer.
[0109] <Optical film processing> A laminate 9 (optical film) in which a coating layer 3 is formed on a first main surface 1A of a film substrate 1 is wound up on a winding roll 91 to obtain a long rolled optical film 90. This laminate 9 can be used as an optical film as is. The regions at both ends in the width direction of the film substrate 1 are non-product regions, and therefore may be cut and removed by slitting after the coating layer 3 is formed and before the film substrate 1 is wound up on the winding roll 91, or at an appropriate stage after the film substrate 1 is wound up on the winding roll 91. Alternatively, the film may be punched out to cut out a sheet of product so as not to include the regions at both ends in the width direction.
[0110] The laminate 9 in which the coating layer 3 is formed on the first main surface 1A of the film substrate 1 may be used as an optical film as it is, or the film substrate 1 may be peeled off and only the coating layer 3 may be used as the optical film. When the coating layer 3 is a resin layer, the laminate of the film substrate 1 and the coating layer 3 may be stretched to impart optical anisotropy to the coating layer 3.
[0111] Other layers may be laminated on the coating layer 3. For example, the optical layer 4 is bonded onto the coating layer 3 via an adhesive layer 5, thereby obtaining a laminate 96 shown in FIG.
[0112] The optical layer 4 laminated on the coating layer 3 is not particularly limited, and an optically isotropic or optically anisotropic film generally used as an optical film can be used without any particular limitation. Specific examples of the optical layer 4 include transparent films such as retardation films and polarizer protective films, and functional films such as polarizers, viewing angle widening films, viewing angle limiting (peeping prevention) films, and brightness enhancing films. The optical layer 4 may be a single layer or a laminate. The optical layer 4 may be a liquid crystal layer. The optical layer 4 may be a polarizing plate having a transparent protective film attached to one or both sides of a polarizer. When the polarizing plate has a transparent protective film on one side, the polarizer and the coating layer may be attached to each other, or the transparent protective film and the coating layer may be attached to each other.
[0113] The adhesive constituting the adhesive layer 5 is not particularly limited in material so long as it is optically transparent, and examples thereof include epoxy resin, silicone resin, acrylic resin, polyurethane, polyamide, polyether, polyvinyl alcohol, etc. The thickness of the adhesive layer 5 is appropriately set depending on the type of adherend, the adhesive material, etc. When using a curing type adhesive that exhibits adhesiveness by a crosslinking reaction after application, the thickness of the adhesive layer 5 is preferably 0.01 to 5 μm, more preferably 0.03 to 3 μm.
[0114] The adhesive may be in any of various forms, such as a water-based adhesive, a solvent-based adhesive, a hot melt adhesive, an active energy ray curable adhesive, etc. Among these, a water-based adhesive or an active energy ray curable adhesive is preferred, since it allows the thickness of the adhesive layer to be reduced.
[0115] An adhesive is applied to either or both of the surface of the coating layer 3 and the surface of the optical layer 4, and then cured, so that the coating layer 3 and the optical layer 4 are laminated via the adhesive layer 5. The curing method of the adhesive may be appropriately selected depending on the type of adhesive. For example, a water-based adhesive can be cured by heating. An active energy ray curable adhesive can be cured by irradiation with active energy rays such as ultraviolet rays.
[0116] A laminate 96 in which the optical layer 4 is bonded to the coating layer 3 on the film substrate 1 via the adhesive layer 5 may be used as an optical film as it is. In this case, the film substrate 1 constitutes a part of the optical film. As shown in Fig. 7, the film substrate may be peeled off from the coating layer 3. An appropriate pressure-sensitive adhesive layer 6 may be laminated on the surface of the coating layer 3 exposed by peeling off the film substrate, as shown in Fig. 8.
[0117] The adhesive constituting the adhesive layer 6 is not particularly limited, and an adhesive having an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyether, a fluorine-based polymer, a rubber-based polymer, or the like as a base polymer can be appropriately selected and used. In particular, adhesives such as acrylic adhesives and rubber-based adhesives that have excellent transparency, moderate wettability, cohesiveness, and adhesiveness, and excellent weather resistance, heat resistance, and the like are preferred. The thickness of the adhesive layer is appropriately set depending on the type of adherend, and is generally about 5 to 500 μm.
[0118] The adhesive layer 6 is laminated on the coating layer 3, for example, by attaching an adhesive previously formed into a sheet shape to the surface of the coating layer 3. After applying an adhesive composition onto the coating layer 3, the adhesive layer 6 may be formed by drying the solvent, crosslinking, photocuring, etc. In order to increase the adhesive strength (anchor strength) between the coating layer 3 and the adhesive layer 6, the surface of the coating layer 3 may be subjected to a surface treatment such as a corona treatment or a plasma treatment, or an easy-adhesion layer may be formed, and then the adhesive layer 6 may be laminated.
[0119] A separator 7 is preferably temporarily attached to the surface of the pressure-sensitive adhesive layer 6. The separator 7 protects the surface of the pressure-sensitive adhesive layer 6 until the optical film is bonded to another member. As a constituent material of the separator, a plastic film such as acrylic, polyolefin, cyclic polyolefin, polyester, etc. is preferably used. The thickness of the separator is usually about 5 to 200 μm. The surface of the separator is preferably subjected to a release treatment. Examples of the release agent include silicone-based materials, fluorine-based materials, long-chain alkyl-based materials, and fatty acid amide-based materials.
[0120] Another optical layer may be laminated via an appropriate adhesive or pressure-sensitive adhesive layer on the exposed surface of the coating layer 3 after peeling off the film substrate 1. For example, another optical layer may be laminated on the coating layer 3 via an appropriate adhesive layer, and a pressure-sensitive adhesive layer may be further laminated on top of that.
[0121] The optical film having the coating layer can be used, for example, as an optical film for an image display device. An example of an optical film having another optical layer 4 laminated onto the coating layer 3 is a circular polarizing plate in which an aligned liquid crystal layer as the coating layer 3 and a polarizing plate are laminated.
[0122] The polarizing plate may be composed of only one layer of polarizer, or as described above, a transparent protective film may be attached to one or both sides of the polarizer. Examples of polarizers include hydrophilic polymer films such as polyvinyl alcohol films, partially formalized polyvinyl alcohol films, and partially saponified ethylene-vinyl acetate copolymer films, which are uniaxially stretched after adsorbing dichroic substances such as iodine or dichroic dyes, and polyene-based oriented films such as dehydrated polyvinyl alcohol and dehydrochlorinated polyvinyl chloride.
[0123] Among them, polyvinyl alcohol (PVA) polarizers are preferred because they have a high polarization degree, and are formed by adsorbing a dichroic substance such as iodine or a dichroic dye onto a polyvinyl alcohol film such as polyvinyl alcohol or partially formalized polyvinyl alcohol, and aligning the film in a predetermined direction. For example, a PVA polarizer can be obtained by dyeing a polyvinyl alcohol film with iodine and stretching the film. A PVA resin layer may be formed on a resin substrate, and the laminate may be dyed with iodine and stretched.
[0124] In a circular polarizing plate in which a polarizing plate and a liquid crystal layer are laminated, it is preferable that the liquid crystal molecules in at least one liquid crystal layer are homogeneously aligned. In the circular polarizing plate, the liquid crystal molecules are arranged so that the alignment direction of the liquid crystal molecules in the liquid crystal layer in which the liquid crystal molecules are homogeneously aligned is neither parallel nor perpendicular to the absorption axis direction of the polarizer.
[0125] For example, when the circular polarizing plate has only one liquid crystal layer, the liquid crystal layer as the coating layer 3 is a quarter-wave plate, and the angle between the absorption axis direction of the polarizer and the alignment direction of the liquid crystal molecules (generally the slow axis direction) is set to 45°. The angle between the absorption axis direction of the polarizer and the alignment direction of the liquid crystal molecules may be 35 to 55°, 40 to 50°, or 43 to 47°.
[0126] In a structure in which the polarizing plate 4 and the coating layer 3 as a quarter-wave plate are laminated so that the angle between the optical axes of the two is 45°, the liquid crystal molecules are further aligned vertically to the substrate surface. The polarizing plate may have a liquid crystal layer with a homeotropic alignment (homeotropic alignment). By laminating a coating layer 3 as a quarter-wave plate and a homeotropic liquid crystal layer functioning as a positive C plate in this order on the polarizing plate, a circular polarizing plate capable of blocking reflected light even from external light coming from an oblique direction can be formed. A homeotropically aligned liquid crystal layer (positive C plate) and a homogeneously aligned liquid crystal layer (quarter-wave plate that is a positive A plate) may be laminated in this order on the polarizing plate.
[0127] In a circular polarizer in which a plurality of liquid crystal layers are laminated on a polarizer, all of the liquid crystal layers may be homogeneously aligned liquid crystal layers. In this case, it is preferable that the liquid crystal layer disposed closer to the polarizer 4 is a half-wave plate, and the liquid crystal layer disposed farther from the polarizer is a quarter-wave plate. In this laminated structure, it is preferable that the half-wave plate is arranged so that the angle between the slow axis direction and the absorption axis direction of the polarizer is 75°±5°, and the angle between the slow axis direction and the absorption axis direction of the polarizer is 15°±5°. A circular polarizer having such a laminated structure functions as a circular polarizer over a wide wavelength range of visible light, and thus can reduce coloring of reflected light.
[0128] As described above, in the embodiment of the present invention, the protective film is temporarily attached to the surface of the film substrate until immediately before the coating liquid is applied, so that the occurrence of scratches on the film substrate is suppressed, and there are few defects in the coating layer caused by scratches on the film substrate. In addition, even if the coating layer is an oriented liquid crystal layer and the liquid crystal molecules are oriented non-parallel to the longitudinal direction of the film substrate, there are few alignment defects. Furthermore, since coating defects caused by bonding the film substrate and the protective film are suppressed, the in-plane uniformity of the coating layer is high, and good display characteristics can be realized. [Explanation of symbols]
[0129] 1 Film substrate 2 Protective film 291 Core material 292 Adhesive layer 3 Coating layer (liquid crystal layer) 4 Optical layer (polarizing plate) 5 Adhesive layer 6 Adhesive layer 7 Separator 8 Laminate 9,96,97,98 Laminates (Optical Films) 29,81 Unwinding roll 21,49,91 Winding roll 40 Lamination section 41,42 Nip roll 10 Peeling part 11 Peeling roll 30 Application section 31 Backup Role 33 Dice 50 Heating section 55 Heating Furnace 60 Hardened part 61 Light source 44, 45, 46, 47 Transport roll 83,85,87 Transport roll 13 Transport roll 15,151 Presser roll 71, 73, 75, 77, 79 Transport roll
Claims
[Claim 1] A method for producing a long optical film, comprising the steps of: a lamination step of sandwiching and laminating a long film substrate having a first main surface and a second main surface and a protective film between a pair of nip rolls consisting of a first roll and a second roll, thereby obtaining a laminate in which the protective film is peelably attached to the first main surface of the film substrate; a first conveying step of conveying the laminate by rolls along a longitudinal direction of the film substrate to a peeling section; a protective film peeling step of peeling the protective film from the first main surface of the film substrate in the peeling section; a second transport step of transporting the film substrate after the protective film has been peeled off from the peeling section to a coating section along a longitudinal direction of the film substrate; and A coating step of applying a coating liquid onto the first main surface of the film substrate in the coating section to obtain a laminate having a coating layer on the first main surface of the film substrate. having The first roll and the second roll are both electrically conductive. A method for producing an optical film.
Citation Information
Patent Citations
Method for manufacturing birefringent layer, and optical film including the birefringent layer
JP2004046068A
Multilayer film, use thereof, and production method thereof
WO2016121856A1