Electrolyte material and forming methods

Halide-based electrolyte materials with controlled crystal irregularities, formed through a specific method, address the limitations of existing solid-state electrolytes by enhancing ionic conductivity and stability, improving the performance of solid-state lithium batteries.

JP2024164039AActive Publication Date: 2024-11-26SAINT GOBAIN CERAMICS & PLASTICS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024126101
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-08-07
Filing Date
2024-08-01
Publication Date
2024-11-26
Estimated Expiration
2041-08-06

AI Technical Summary

Technical Problem

Existing solid-state electrolyte materials lack improved properties such as ionic conductivity, mechanical properties, and stability, which are crucial for enhancing the performance of solid-state lithium batteries.

Method used

The development of halide-based electrolyte materials with controlled irregularities in their crystal structure, including stacking faults and atomic vacancies, which are formed through a specific method involving the reaction of ammonium halides with metal compounds to create a solid electrolyte material with enhanced crystallinity and controlled stacking faults.

Benefits of technology

The resulting halide-based electrolyte materials exhibit improved ionic conductivity, mechanical properties, and stability, making them suitable for use in solid-state lithium batteries with higher energy density and faster recharge times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164039000008
    Figure 2024164039000008
  • Figure 2024164039000009
    Figure 2024164039000009
  • Figure 2024164039000010
    Figure 2024164039000010
Patent Text Reader

Abstract

To provide a solid electrolyte material including a disorder in the crystalline structure and methods of forming the same.SOLUTION: A solid electrolyte material includes a halide-based material having a crystalline structure including a disorder. In an embodiment, the solid electrolyte material includes a crystalline structure including stacking faults. In another embodiment, the solid electrolyte material includes a crystalline phase including a crystalline structure represented by a space group of the hexagonal system or a space group of a rhombohedral lattice system. In another embodiment, the solid electrolyte material includes a crystalline phase including a crystalline structure represented by a monoclinic system space group and a unit cell containing a reduced number of halogen atoms.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The following relates to electrolyte materials and methods of forming the same, in particular to solid-state electrolytes that include irregularities in the crystal structure. The present invention relates to a solution material and a method for forming the same. [Background technology]

[0002] By allowing for a lithium metal anode, solid-state lithium batteries are Compared to lithium-ion batteries, they offer higher energy density and faster recharge times, and are more reliable. The industry continues to seek improved solid electrolyte materials. do. Summary of the Invention

[0003] The present disclosure can be better understood with reference to the accompanying drawings, many of which are incorporated herein by reference. Many features and advantages will become apparent to those skilled in the art. [Brief description of the drawings]

[0004] [Figure 1A] FIG. 1 illustrates a crystal structure of an exemplary solid electrolyte material according to an embodiment. [Figure 1B] FIG. 2 shows another crystal structure. [Figure 1C] FIG. 2 illustrates a crystal structure of another exemplary solid electrolyte material, according to an embodiment. [Figure 2A] FIG. 2 shows further crystal structures. [Figure 2B] FIG. 2 shows another crystal structure. [Figure 2C] FIG. 2 illustrates a crystal structure of another exemplary solid electrolyte material, according to an embodiment. [Figure 2D] FIG. 2 illustrates a crystal structure of another exemplary solid electrolyte material, according to an embodiment. [Diagram 3] FIG. 1 is a diagram showing a crystal structure. [Figure 4]FIG. 2 shows another crystal structure. [Diagram 5] FIG. 1 illustrates different crystal structures. [Figure 6A] This is a simulated powder X-ray diffraction spectrum of a halide-based material. [Figure 6B] This is a simulated powder X-ray diffraction spectrum of a halide-based material. [Figure 6C] This is a simulated powder X-ray diffraction spectrum of a halide-based material. [Figure 7A] 1 is a spectrum of an X-ray diffraction simulation of a halide-based electrolyte material. [Figure 7B] 1 is a simulated X-ray diffraction spectrum of another halide-based electrolyte material. [Figure 7C] 1 is a simulated X-ray diffraction spectrum of another halide-based electrolyte material. [Figure 7D] 1 is a simulated X-ray diffraction spectrum of another halide-based electrolyte material. [Figure 7E] 1 is a simulated X-ray diffraction spectrum of another halide-based electrolyte material. [Figure 8] 1 is a flowchart illustrating a process for forming a solid electrolyte material according to one embodiment. [Figure 9] FIG. 1 includes X-ray diffraction patterns of halide-based electrolyte materials. [Figure 10] This is a crystal structure model of a solid electrolyte material. [Figure 11] This is a crystal structure model of a solid electrolyte material. [Figure 12] This is a crystal structure model of a solid electrolyte material. [Figure 13] This is a crystal structure model of a solid electrolyte material. [Figure 14A] FIG. 2 shows X-ray diffraction patterns of halide-based electrolyte materials. [Figure 14B] FIG. 2 shows X-ray diffraction patterns of halide-based electrolyte materials. [Figure 15]FIG. 2 shows the X-ray diffraction pattern of a sample of a halide-based electrolyte material. [Figure 16] FIG. 2 shows X-ray diffraction patterns of halide-based electrolyte materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0005] Skilled artisans will appreciate that elements in the figures are illustrated for simplicity and clarity and are not necessarily drawn to scale. For example, the dimensions of some of the elements in the drawings may differ from those of the present invention. Some elements may be exaggerated relative to other elements to help better understand the embodiments. The use of the same reference symbols in different drawings indicates similar or identical Shows the item.

[0006] To facilitate an understanding of the teachings disclosed herein, the following description should be read in conjunction with the drawings, in which: The following description provides specific implementations and examples of the teachings. This focus is provided to facilitate explanation of the teachings and to clarify the scope of the teachings. or should not be construed as limiting the applicability of the present disclosure.

[0007] As used herein, "comprises" and "comprises" sing," "includes," "including," "has The terms "has," "having," or any other The variations are intended to cover non-exclusive inclusions. For example, a list of features The process, method, article, or apparatus described herein is not necessarily limited to only those features. Any other features not expressly recited herein or any such process, method, article, or apparatus. Additionally, unless expressly stated to the contrary, "Or" refers to an inclusive or, not an exclusive or. For example, "the condition "A or B" is satisfied by one of the following: A is true (or exists) and A is false (or does not exist) and B is false (or does not exist), A is false (or does not exist) and B is true ( or exists), and both A and B are true (or exist).

[0008] The use of "a" or "an" refers to the elements and components described herein. This is done merely for convenience and to give a general sense of the scope of the invention. This description is made to give a general sense of the It is clear that this should be read as including one more, and is not meant to imply otherwise. Except where expressly stated, the singular includes the plural and vice versa.

[0009] Unless otherwise defined, all technical and scientific terms used herein are intended to be understood as meaning the invention. The terms "material", "method", "method" and "method" have the same meaning as commonly understood by a person skilled in the art to which the term pertains. The methods and examples are illustrative only and are not intended to be limiting.

[0010] The embodiments herein relate to halide systems that contain certain irregularities in their crystal structure. The present invention relates to a solid electrolyte material including a solid-state electrolyte material having disorder. The improved properties include those obtained by applying the same composition to other materials that do not have the same properties. Conductivity, mechanical properties such as deformability and plasticity, electrochemical stability, chemical stability, thermal stability properties, electronic resistivity, particle morphology and / or size, electrode wettability, etc., and / or The solid electrolyte material can be used in electrochemical applications such as solid-state lithium-ion batteries. The present invention can be used in a semiconductor device that ... The present invention relates to a method for forming a solid electrolyte material having a controlled disorder in the crystal structure. This allows for controlled formation of the material while at the same time allowing for control of the crystallinity of the material.

[0011] In one embodiment, the solid electrolyte material is 3ーZ (Me k+ ) f X 3-Z+k*f Represented by The electrolyte may include a halide-based electrolyte material having a structure in which -3≦z<3 and k is Me where k is 2≦k<6, f is 0≦f≦1, M includes an alkali metal, and Me In a further embodiment, X comprises a metal other than an alkali metal and X comprises a halogen. The halogenide-based electrolyte material is a complex metal halide. In certain embodiments, f is not 0. Me may contain two or more metal elements. k can be the average of the sum of the valences of each Me metal element, for example, if Me is equimolar If the element contains a quantity of trivalent and tetravalent elements, k = (3 + 4) / 2 = 3.5. In embodiments, k can be 2 or 3 or 4 or 5.

[0012] Upon reading this application, a person skilled in the art will understand that there exists an atomic vacancy ( It helps to understand the crystal structure. To achieve this, atomic vacancies can be added to the formula of the halide-based material, and the formula including the atomic vacancies becomes , M 3-Z (Me k+ ) f · y X 3-Z+k*fwhere "" represents the unit represents an atomic vacancy in the lattice, and Y represents the vacant atomic position. In certain embodiments, y is the number of * It can be (k-1).

[0013] In one embodiment, M can include at least one of Li and Na. For example, M can be: In another embodiment, M can be Li, Na, K, R In a further embodiment, M may comprise one or more of A, B, C, Cs, or any combination thereof. For example, M can be any of the elements Li, Na, K, Rb, and Cs. The metal oxide may consist essentially of one or more alkali metal elements selected from the group consisting of: In one example, M can consist of Li. In yet another example, M can consist of Li and Na, K, In yet another example, it may be a combination of at least one of Rb and Cs. In another example, M may consist of Na and at least one of Cs and Rb. , M may consist of at least one of Na and Cs.

[0014] In another embodiment, Me is an alkaline earth metal element, a 3d transition metal, a rare earth element, Zn, Z r, Hf, Ti, Sn, Th, Ge, V, Ta, Nb, Mo, W, Sb, Te, In, B For example, Me may include Mg, Alkaline earth metals such as Ca, Sr, or Ba, Zn, Cu, or any combination thereof In another example, Me may include a rare earth element. In a particular implementation, Me may include a rare earth element. In another specific example, Me can be one or more of the elements Y, Ce, , Gd, Er, Zr, La, Cu, Yb, In, Mg, Zn, Sn, or any of them It may include combinations.

[0015] In one embodiment, X can include halogens such as Cl, Br, I, or any combination thereof. In one example, X may include at least one of Cl and Br. In a particular implementation, X can consist of Cl, Br, or a combination thereof. In a particular example, X consists of one The halogens may be any of the above.

[0016] In another embodiment, the halide-based material is NH4 + In certain embodiments, the phase may include So, the halide material is (NH4) n M 3-Z (Me k+ ) f X n+3-Z+k* f (wherein n>0). In the formula of the embodiment of the present specification, M, Me, Symbolic letters such as n, f, Z, X, and k are used. As used in this disclosure, different implementations The same symbol characters shown in the embodiments are intended to refer to the same or similar elements or values. In one embodiment, a particular element or value described with a symbolic character may be expressed with the same symbolic character. When a letter is used, it may apply to another embodiment. For example, The descriptions of M, Me, X, f, z, and k in this and other embodiments of the present disclosure. can be applied to.

[0017] In certain embodiments, the halide-based electrolyte material is Li 3-z Me k+ X 3-z+k When z is not 0, the metal halide complex is said to be nonstoichiometric. When z is 0, the metal halide complex is said to be stoichiometric. In another specific example, Me is Y, Gd, Yb, Zr, In, Sc, Zn, Mg, Ca, Ba, Sn or a combination thereof, and X is Cl, B r or a combination thereof.

[0018] In a further embodiment, the halide-based electrolyte material may be represented by Li3MeBr6. In a further embodiment, the halide-based electrolyte material is represented by Li3MeCl6. In a particular example, Me can be selected from at least one metallic element having a valence of 3. In another particular example, Me can include one or more metal elements, The average valence of the above metallic elements is 3.

[0019] In another particular embodiment, the halide-based electrolyte material is selected from the group consisting of Li, Y, and Cl and B. For example, the halide-based electrolyte material may be , Li, Y, and Cl. In another example, the halide-based electrolyte material can be , Li, Y, and Br. The material can consist of Li, Y, Cl, and Br. In particular examples, the halides The electrolyte material is Li 3X Y 1-X Cl3 or Li 3X Y 1-X Br3 (0 in the formula <x<0 This can be expressed as:

[0020] In another particular embodiment, the halide-based electrolyte material comprises Li, Gd, and Cl and For example, the halide-based electrolyte material may be , Li, Gd, and Cl. In another example, a halide-based electrolyte material The electrodes can consist of Li, Gd, and Br. The electrolyte material can consist of Li, Gd, Cl, and Br. In a particular example, the halogens Lithium ion-based electrolyte materials are 3x Gd 1-x Cl3 or Li 3x Gd 1-x Br3 (in the formula It can be expressed as: 0.01≦x<1.

[0021] Specific examples of halide-based materials include Li3YCl6, Li3YBr6, Li 2. 7Y 0.7 Zr 0.3 Cl6, Li 2.8 Y 0.8 Sn 0.2 Cl6, Li 3.2 Y 0. 8Zn 0.2 Cl6, Li 3.2 Y 0.8 Mg 0.2 Cl6, Li3Y 1 / 3 Zr 1 / 3 Mg 1 / 3 Cl6, Li3Y 1 / 3 Sn 1 / 3 Mg 1 / 3 Cl6, Li3Y 1 / 3 Zr1 / 3 Zinc 1 / 3 Cl6, Li 2.95 Na 0.05 YBr6, Li 2.95 K 0.05 Y Br6, Li 2.95 Cs 0.05 YBr6, Li3Y 0.7 Gd 0.3 Br6, Li3 Y 0.8 Yb 0.2 Br6, Li3Y 0.9 La 0.1 Br6, Li 2.9Y 0.9 Ce 0.1 Examples include Li3Y(Cl,Br)6, Br6, or Li3Y(Cl,Br).

[0022] In one embodiment, the halide-based electrolyte material has a crystal structure different from the conventional crystal structure. For example, the crystal structure may have irregularities compared to conventional crystal structures. As used herein, "conventional structure" refers to a halide-based It is intended to refer to the regular crystalline structure of a material. A crystalline structure is a system of crystals, lattices, or spaces. Group, one or more unit cell constants such as unit cell volume, valences a, b, c, or any of them combination, atomic number in a unit cell, stacking order, atomic vacancies, vacancy occupation, or any combination thereof The irregularity may include any change in order related to any of these features. It could be.

[0023] In one embodiment, the halide-based electrolyte material has a layered atomic arrangement that may include disorder. In one embodiment, the crystal structure includes atoms arranged in layers. In one example, the crystal structure may include stacking faults. Defects are occupied or vacant atomic positions (o) that cause the disordering of crystal planes in the crystal structure. vacant atomic position) shift It represents a defect in the crystal structure caused by

[0024] Briefly referring to FIGS. 1A, 1B, and 1C, halide-based materials having the same composition are Different crystal structures of the compound are shown. FIG. 1A is an illustration of a particular crystal structure of one embodiment. FIG. 1B is a conventional crystal structure of a halide-based material. FIG. 1C is an alternative embodiment. 1 is an illustration of a specific crystal structure of an example of the crystal structure 100, 101, and 102. In structure 101, the same atoms in different layers (i.e. That is, the position of atom 110, 120, or 130 remains the same in the stack, and the atom The locations of 110, 120, 130 and voids 140 follow the same pattern across the layers in structure 101. As shown, the structure 101 contains ordered layers of atoms and vacancies. In the structures 100 and 102, at least one of the atoms 110, 120, or 130 At least some of the atomic positions are compared to the positions of the same atoms in different layers or in the structure 100. Since the position of the atoms in the stacking faults is shifted compared to the position of the same atoms in the stacking faults in the present disclosure, Upon reading this, one of ordinary skill in the art will understand that the shift in atomic position across the layers of a crystal structure may be stochastic. and that stacking faults in halide-based materials are the specific examples shown in Figs. 1A and 1C. It can be understood that the present invention is not limited to the above-mentioned halide-based materials. The material has more stacking faults (0% or close to 0%) than the structure shown in FIG. 1B, and is 1C. A person skilled in the art will appreciate that the structure 100, 1 Please note that only a small portion representing 01 and 102 is shown in Figures 1A-1C, respectively. Further understanding is possible.

[0025] In certain embodiments, the halide-based material promotes improved properties of the halide-based material. The crystal structure may contain a certain amount of stacking faults that can cause the powder to break down. The final X-ray diffraction pattern may change, and in particular, only certain X-ray diffraction peaks may become unevenly broadened. Stacking faults are considered to be the solid state ionic s 180(2010) 1652-1659, which is incorporated herein by reference in its entirety. According to the stacking fault quantification method described by TOPAS4.2 or FullProf (version 7.3 released in March 2020) 0), or another equivalent such as TOPAS 4.2 or FullProf version 7.30 By using the version or software of the software, Halide Powder X-ray diffraction analysis of the system materials, DIFFaX simulation, and Rietveld In brief, the quantitative method can be used to determine the The method may include fitting the simulation to an X-ray diffraction pattern of the powder. The solution defines the primary blocks of the crystal structure. These basic blocks can be made up of slabs and inter-slab spaces. Next, we divide the basic blocks into two or more possible stacking vectors. g vector), the stacking vector can be If only one were to occur exclusively, a perfect stack such as structure 101 shown in FIG. % stacking faults). If the stacking vectors are staggered in the stacking direction of the crystal structure, Stacking faults occur. Simulation fitting to X-ray diffraction patterns of halide-based materials A fitting involves changing one or more parameters of the crystal structure (called "parameter refinement"). ", and the least-squares difference minimization algorithm. re difference minimization algorithm) The stacking faults may be identified and quantified. Instead of using the stacking fault quantification method by Boulineau after the Tobeld analysis, the FAULTS software The software can be used.

[0026] In one embodiment, the crystal structure has at least 20% stacking faults (e.g., at least 25%, at least 30%, at least 40%, at least 50%, at least 60%, at least The material may contain at least 70%, at least 80%, or at least 90% stacking faults. In some cases, the stacking of atomic layers is completely disordered. For example, a crystal structure is 100% In another embodiment, the stacking faults are at most 99%, for example at most 95%, Up to 92%, up to 90%, up to 85%, up to 80%, up to 75%, or up to 70%, etc. Additionally, the crystalline structure may be within any of the minimum and maximum percentages set forth herein. In a particular example, the solid electrolyte material may include at least In another specific example, the solid may include a halide-based material having a crystal structure containing 50% The electrolyte material contains halide-based materials with more than 50% and up to 100% stacking faults. It can be seen.

[0027] A specific example of a halide-based material is yttrium bromide containing at least 50% stacking faults. It may contain lithium yttrium bromide.

[0028] In certain embodiments, the halide-based material comprises a monoclinic crystal structure containing stacking faults. In certain embodiments, the crystal structure may be represented by the space group C2 / m. For example, Halide-based materials are yttrium bromide containing a crystal structure represented by C2 / m that contains stacking faults. In another embodiment, the halide-based material may include rhombohedral structures containing stacking faults. It may include a hexagonal or heptagonal lattice crystal structure.

[0029] Another specific example of a halide-based material is one in which the three stacking vectors are (0;0;1), (1 / 2;-1 / 6;1) and (1 / 6;-1 / 6;1) on the c-axis of the monoclinic lattice. Such halide-based materials may contain at least 50% stacking faults in the stacking direction along the A specific example of a material is lithium yttrium bromide. The halide-based material having the specific stacking faults described above has improved properties such as ionic conductivity. For example, the vectors (0;0;1), (1 / 2;-1 / 6;1) and (1 / 6;-1 / 6;1) have at least 50% stacking faults along the c-axis of the monoclinic unit cell Yttrium lithium bromide has higher ionic conductivity than conventional yttrium lithium bromide. The exemplary yttrium lithium halide (li thium yttrium halide has a pH of 1.7 to 3.1 mS / cm at room temperature. It can have ionic conductivity.

[0030] In comparison with FIG. 1B, FIGS. 1A and 1C further show the positions of the atoms 130 and the vacancies 140. As shown, the position of atom 130 is in the structure 100 and 02 is highly intermixed with voids 140. 102 is a position where atoms 130 and vacancies are highly mixed. It is important to understand that this is a novel crystal structure that arises due to the presence of a As shown in the specific example crystal structure 100, an atom 130 is coupled to a vacancy 140. Similarly, in crystal structure 102, atom 130 is highly intermixed with vacancy 140. As shown in the crystal structure 101, the atom 130 is separate from the vacancy 140. When the atoms 130 and vacancies 140 assume their positions, there is an ordering of their positions. is further described later in this disclosure.

[0031] In another embodiment, the halide-based material comprises a crystal structure that differs from conventional crystal structures. In one embodiment, the halide-based material may have a different crystal structure than the conventional crystal structure. In certain embodiments, the solid state electrolyte may include a crystalline phase having a crystal structure represented by a space group. The solution material is a material that is made at the atomic level and the nanometer domain level. A halo comprising a first and a second crystalline phase integrated at the main-level, or both. The closest atomic distances are typically less than 0.5 nm, making them nanometer-sized. The domains of the nuclei are larger than the nearest atomic distance, e.g., larger than 1 nm. In one embodiment, the halide-based material can have a first space group: The first crystal phase has a first crystal structure represented by a second space group different from the first space group. and a second crystalline phase having a second crystal structure represented by at least a first space group. The first crystal structure is different from the conventional crystal structure. In particular, the first space group is different from the conventional crystal structure. This is different from the space group of the structure.

[0032] In certain embodiments, the halide-based material promotes improved properties of the solid electrolyte material. For example, the solid electrolyte material may contain a certain concentration of a first crystalline phase that can The concentration of the system material is at least 1% by weight, for example at least 4% by weight, at least 5% by weight, at least 8% by weight, at least 10% by weight, at least 15% by weight , at least 20% by weight, at least 25% by weight, at least 30% by weight, at least 3 5% by weight, at least 40% by weight, at least 45% by weight, at least 50% by weight, at least at least 60%, at least 70%, at least 80%, or at least 90% by weight In yet another example, the material may include a halide-based material having a first crystalline phase that is 0.1 wt. The halogenide-based material has a concentration of up to 95% by weight, for example up to 90% by weight, up to 85% by weight, %, up to 80% by weight, up to 70% by weight, up to 65% by weight, up to 60% by weight, 55% by weight, up to 50% by weight, up to 45% by weight, up to 40% by weight, up to 30% by weight %, up to 25%, up to 15%, up to 8%, or up to 5% by weight Additionally, the halide-based materials may contain a first phase having the minimum and maximum % content as described herein. The first phase may be present in a range of concentrations including any of the above %.

[0033] In another aspect, the halide-based material may facilitate improving the properties of the solid electrolyte material. In one example, the solid electrolyte material may contain a second phase of a certain concentration that can be used for the solid electrolyte material. The concentration of the compound-based material is at least 1% by weight, for example at least 4% by weight, at least 5% by weight, at least 8% by weight, at least 10% by weight, at least 15% by weight , at least 20% by weight, at least 25% by weight, at least 30% by weight, at least 3 5% by weight, at least 40% by weight, at least 45% by weight, at least 50% by weight, at least at least 60%, at least 70%, at least 80%, or at least 90% by weight In yet another example, the material may include a halide-based material having a second crystalline phase that is 0.1 wt. The halogenide-based material has a concentration of up to 95% by weight, for example up to 90% by weight, up to 85% by weight, %, up to 80% by weight, up to 70% by weight, up to 65% by weight, up to 60% by weight, 55% by weight, up to 50% by weight, up to 45% by weight, up to 40% by weight, up to 30% by weight %, up to 25%, up to 15%, up to 8%, or up to 5% by weight Additionally, the halide-based materials may contain second phases in the range of the minimum and maximum percentages set forth herein. In an exemplary embodiment, the second phase may include a concentration range of at least one of the following: In a further exemplary embodiment, the second phase can have a conventional crystal structure. The second crystal structure may be different from the first crystal structure, and in certain embodiments, the second space group is , the space group of the conventional structure may differ.

[0034] In a further aspect, the halide-based material has a different crystal structure than the second and / or first. The third phase may include a third crystal structure having a third crystal structure that includes a crystal structure characteristic. The crystal structure may be represented by a third space group different from the first and second space groups. In a further aspect, the halide-based material can be described with respect to the concentration of the first or second phase. In yet further embodiments, the halide-based material may include a third phase of any concentration as described above. The concentration of the amorphous phase may be up to 10% by weight, or up to 5% by weight. The concentration of each phase in the halide-based material may be 1% by weight or up to 1% by weight. It is understood that the total may add up to 100% by weight.

[0035] In another embodiment, the halide-based material has a space group different from the space group of conventional crystal structures. The crystal structure may consist essentially of a crystalline phase having a crystal structure represented by:

[0036] In certain embodiments, the solid electrolyte material has a first crystal structure represented by a first space group. The first space group may include a halide-based material including a first phase having a rhombohedral lattice system. The space groups of the rhombohedral lattice systems are R3, R-3, R32, R3m, and R3c. , R-3m, and R-3c space groups. In certain embodiments, the first crystalline phase is In another embodiment, the compound can have a first crystal structure represented by the R-3m space group. , the second crystalline phase can be represented by a monoclinic space group. In certain embodiments, the second phase may include the crystal structure represented by C2 / m. Specific examples of halide-based materials include: Crystal phase having a crystal structure represented by R-3m, crystal having a crystal structure represented by C2 / m A further specific example of a halide-based material is the R-3m phase. The first crystal phase has a crystal structure represented by C2 / m, and the second crystal phase has a crystal structure represented by C2 / m. A further specific example of a halide-based material is a crystal represented by R-3m. A first crystal phase having a structure represented by C2 / m, and a second crystal phase having a crystal structure represented by Fd- The third crystal phase may have a crystal structure represented by Fm-3m or Fm-3m. In a particular example, the halide-based material is a crystal structure represented by R-3m. It may consist of a crystal phase.

[0037] Referring to FIG. 1A, FIG. 1B, and FIG. 1C, FIG. 1A shows an embodiment of a R-3m FIG. 1B is a diagram of a specific example of a crystal structure represented by C2 / m. FIG. 1C is a diagram of the crystal structure of one embodiment, represented in the C2 / m space group. In the case of halide-based electrolyte materials, the crystal structure represented by R-3m is shown in Figure 1A. and a second phase having a crystal structure represented by C2 / m as shown in FIG. 1B. The first and second crystalline phases may include lithium yttrium bromide including In another specific example, the material is integrated at the nanometer domain level, or both. As shown in Figure 1A, halide-based solid electrolyte materials have a crystal structure represented by R-3m. The material may include lithium yttrium bromide which may be comprised of a crystalline phase having a crystal structure.

[0038] In another embodiment, the solid electrolyte material has a crystal structure represented by a hexagonal space group. The hexagonal crystal system may include halide-based materials containing the phase.

number

[0039] In another embodiment, the halide-based material is represented by a hexagonal crystal structure space group. A first crystal phase having a first crystal structure and a space group of a crystal system other than a hexagonal crystal structure. and a second phase having a second crystal structure having a trigonal crystal structure. In certain embodiments, the second phase may have a crystal structure represented by the space group P-3 In a further embodiment, the second phase may have a second crystal structure represented by m1. The compound may have a crystal structure that is expressed in the orthorhombic crystal structure space group. In such a case, the second phase may have a second crystal structure described by the Pnma space group. do.

[0040] In certain embodiments, the halide-based electrolyte material is P63 / mcm or P63 / mm a first phase having a first crystal structure represented by P-3m1 or Pnma; and a second phase having a crystal structure of The inorganic electrolyte material has a first crystal structure represented by P63 / mcm or P63 / mmc. and a second phase having a second crystal structure represented by P-3m1 or Pnma. It can be.

[0041] Referring to FIGS. 2A-2D, FIG. 2A is a diagram of a crystal structure 200 represented by Pnma. 2B is a diagram of a crystal structure 201 designated P-3m1, and FIG. 2C is a diagram of a specific embodiment of the crystal structure 201. FIG. 2D is a diagram of a crystal structure 202 of the example P63 / mcm. FIG. 2 is a diagram of a crystal structure 203 represented by a specific example of P63 / mmc.

[0042] In a particular example, the halide-based electrolyte material is P63 / mcm, as shown in FIG. The first phase has a crystal structure represented by P63 / mmc as shown in Figure 2D, and the second phase has a crystal structure represented by P63 / mmc as shown in Figure 2A. The second compound having a crystal structure represented by Pnma as shown in FIG. 2B or P-3m1 as shown in FIG. and a lithium yttrium chloride having a first crystalline phase and a second crystalline phase. The technology is integrated at the nanometer domain level, at the nanometer domain level, or both. In the example, the halide-based solid electrolyte material is P63 / mcm as shown in FIG. 2C, or The crystal structure may be represented by P63 / mmc, as shown in FIG. 2D. In another specific example, the halide-based solid electrolyte may include lithium yttrium chloride. The material is P63 / mcm as shown in Figure 2C or P63 / mmc as shown in Figure 2D. The first phase has a crystal structure shown in FIG. 2A, and the second phase has a crystal structure shown in FIG. 2B. The second phase has a crystal structure represented by P-3m1, and the second phase can be composed of yttrium chloride. The lithium may be included.

[0043] In one embodiment, the solid electrolyte material has a different structure within the unit cell compared to conventional crystal structures. In one embodiment, the halide-based material may include a halide-based material having a crystal structure including a number of atoms. The material may include a crystal structure that includes a unit cell that is disordered compared to conventional structures. In this embodiment, the irregular unit cell is a unit cell having a number of halogen atoms, a number of M atoms such as Li, a number of Me atoms, etc. the number, the unit cell constant, the volume of a unit cell of a smaller unit cell, etc., or any combination thereof In another embodiment, the halide-based material may have a crystal structure different from that of the conventional one. It may include a crystal structure that includes a unit cell that has a reduced content of halogen atoms compared to the crystal structure.

[0044] In another particular embodiment, the halide-based material is a monohalide material containing less than 12 halogen atoms. In one embodiment, the number of halogen atoms in a unit cell is up to In another embodiment, the units The number of halogen atoms in the lattice is at least 1, at least 2, at least 3, or less. Additionally, the halide-based materials may be any of the minimum and maximum values ​​set forth herein. The present invention may include a crystal structure including a unit cell containing halogen atoms in the range including any of the following: , halide-based materials may contain from 2 to 6 halogen atoms within the unit cell.

[0045] In a further embodiment, the halide-based material is represented by a monoclinic space group and has disorder. In one embodiment, the space group may be C2 / m. In other embodiments, the unit cell may contain less than 12 halogen atoms. Halide materials are represented by the monoclinic space group and are made up of units containing 3 to 5 halogen atoms. It may include a crystal structure that includes a lattice.

[0046] In a further embodiment, the halide-based material is a crystal represented by a hexagonal space group. In one embodiment, the vacancy may include a crystalline structure, and the unit cell may include less than 12 halogens. The intermediate group can be R-3m. In another embodiment, the unit cell contains up to eight halogen atoms. In at least one particular embodiment, the halide-based material has voids in a hexagonal crystal system. The halogen atoms in the unit cell are represented by the halogen groups and include crystal structures containing unit cells with up to six halogen atoms. In another aspect, the halide-based material is represented in the hexagonal space group and has at least Also includes crystal structures containing unit cells having 1.5 halogen atoms.

[0047] In a further embodiment, the halide-based material is represented by a rhombohedral lattice space group. In one embodiment, the unit cell may include less than 12 halogens. , the unit cell may contain up to eight halogen atoms.

[0048] A conventional C2 / m unit cell contains 12 halogen atoms, e.g. Li3YBr6 Conventional Li3MeBr6 contains 12 bromine atoms in the unit cell. Representative examples of 3YBr6 include those having less than 12 bromine atoms, e.g., up to 6 bromine atoms or up to A specific example of Li3YBr6 has four Br atoms. In one embodiment, Li3YBr6 may have a smaller monoclinic unit cell. A specific example may include an R-3m unit cell containing six Br atoms.

[0049] In one embodiment, the solid electrolyte material is a halogen-containing material having a crystal structure with specific unit cell characteristics. In one embodiment, the halide-based material may include a halide-based material having unit lattice constants a, b, and A, B, and C can each independently comprise a unit cell having particular values ​​of A, B, and C. In another aspect, the unit cell can be a cell of a particular volume, a particular normalized volume, or any of these. It may include combinations.

[0050] In certain embodiments, the halide-based material is a crystalline material represented by the rhombohedral space group. The structure can include a structure in which the unit cell constants a and b are equal. Referring to FIG. A rhombohedral unit cell 300 is shown, which includes a, b, and c. The lattice may be in the R-3m space group. In one embodiment, A or B or both contain specific values. For example, A or B may be at least 3.0 angstroms, at least 3.3 angstroms, angstroms, at least 3.6 angstroms, or at least 3.9 angstroms. In another example, A or B may be at most 4.8 angstroms, at most 4. 6 angstroms, up to 4.3 angstroms, up to 4.2 angstroms, or up to 4.0 Angstroms. Further, A or B may be any of the groups described herein. The range can be any of the minimum and maximum values. The genoxide-based material may include a crystal structure that includes a specific C. In one example, C is at least one 5 angstroms, at least 17 angstroms, or at least 19 angstroms In another example, C can be up to 21 Angstroms, up to 20.2 Angstroms, Angstroms, or up to 19.5 Angstroms. It may be within a range including any of the minimum and maximum values ​​set forth in the specification.

[0051] In a further embodiment, the rhombohedral unit cell may include a unit cell volume V having a particular value. For example, V is at least 200 Å and at least 210 Å. Angstroms, at least 230 cubic angstroms, at least 250 cubic angstroms In another example, V can be at least 260 angstroms, or at least 260 cubic angstroms. Up to 320 cubic angstroms, up to 310 cubic angstroms, up to 290 Angstroms cubic, up to 275 Angstroms cubic, or up to 270 Angstroms cubic In certain instances, V can be any of the minimum and maximum values ​​described herein. The range may be inclusive of either.

[0052] In a further embodiment, the rhombohedral unit cell has a unit volume per formula unit V N / FU Includes The normalized volume can be included, V N / FU =V / N FU and N FU is the formula in the unit cell In certain embodiments, the unit cell is a specific V N / FU In one example, The halide-based material is at least 200 cubic angstroms, at least 210 cubic angstroms, at least 230 cubic angstroms, at least 250 cubic on angstroms, or at least 260 cubic angstroms of V N / FU Crystal structure containing In another example, V N / FU is at most 290 cubic angstroms and at most 2 75 cubic angstroms, up to 270 cubic angstroms, or up to 268 cubic In a particular example, V N / FU is the minimum value and The range may be inclusive of either the maximum or minimum value.

[0053] In a further embodiment, the rhombohedral unit cell has a unit volume per halogen atom, V N / AA The normalized volume can include V / NAA =V / N AA and N AA is in the unit cell In certain embodiments, the halide-based material is a material having a specific V N / AA In one example, the crystal structure may include N / AA is at least 30 cubic angstroms mm, at least 34 cubic angstroms, at least 38 cubic angstroms, It may be at least 42 cubic angstroms, or at least 46 cubic angstroms. In another example, V N / AA is a maximum of 50 cubic angstroms and a maximum of 48 cubic on Angstroms, or up to 47 cubic Angstroms. N / AA can be within a range that includes any of the minimum and maximum values ​​described herein. .

[0054] In certain embodiments, the halide-based materials have a unit cell volume that is smaller than that of conventional crystal structures. The crystal structure may include a small monoclinic space group. See FIG. 4, a monoclinic unit cell 400 is shown with parameters a, b, and c, and c are different from each other. In certain embodiments, the unit cell can be in the C2 / m space group. In the formula, A, B, and C may independently include specific values. For example, A may be at least 5. 8 angstroms, at least 6.1 angstroms, at least 6.3 angstroms Angstroms, at least 6.5 Angstroms, at least 6.7 Angstroms, or In another example, A can be at least 6.9 Angstroms. In another example, A can be at most 7.8 Angstroms. Angstroms, up to 7.6 Angstroms, up to 7.3 Angstroms, up to 7 0.2 Angstroms, or up to 7.0 Angstroms. It may be within a range including any of the minimum and maximum values ​​set forth herein. In certain embodiments, B is at least 3.0 angstroms, at least 3.3 angstroms, Angstroms, at least 3.6 Angstroms, or at least 3.9 Angstroms. In another example, B is at most 4.8 angstroms, at most 4.6 angstroms. Angstroms, up to 4.3 Angstroms, up to 4.2 Angstroms, or up to 4.1 In addition, B may be any of the minimum and maximum values ​​described herein. In one example, C is at least 6.1 Angstroms. Angstroms, at least 6.4 Angstroms, or at least 6.8 Angstroms. In another example, C can be at most 7.9 angstroms, at most 7.6 angstroms. The thickness may be up to 7.2 Angstroms, or up to 6.9 Angstroms. Additionally, C may be within a range that includes any of the minimum and maximum values ​​described herein. can.

[0055] In a further embodiment, the monoclinic unit cell can include a unit cell volume V having a particular value. For example, V is at least 110 Å, at least 125 Å. Angstroms, at least 140 cubic angstroms, at least 160 cubic angstroms In another example, V can be at least 170 Å. Large: 500 cubic angstroms, Max: 400 cubic angstroms, Max: 310 cubic angstroms Angstroms, up to 250 cubic angstroms, up to 220 cubic angstroms Angstroms, up to 200 cubic Angstroms, or up to 180 cubic Angstroms In certain instances, V may be in a range that includes any of the minimum and maximum values ​​described herein. It can be within the range.

[0056] In certain embodiments, the monoclinic unit cell has a particular V N / FU In one example, the halo The nitride-based material has a thickness of at least 200 cubic angstroms, at least 210 cubic angstroms. Angstroms, at least 230 cubic angstroms, at least 250 cubic angstroms troms, or at least 260 cubic angstroms of V N / FU The crystal structure includes In another example, V N / FU is at most 320 cubic angstroms and at most 300 Angstroms, up to 280 Angstroms, or up to 270 Angstroms In a particular example, V N / FU are the minimum and maximum values ​​described in this specification. The range may be inclusive of either the greater or lesser value.

[0057] In a further embodiment, the monoclinic unit cell has a unit volume per halogen atom, V N / AA Including The normalized volume can be included, V N / AA =V / N AA and N AA is in the unit cell represents the number of halogen atoms. In certain embodiments, the halide-based material is a material having a specific V N / AA of In one example, the crystal structure may include V N / AA At least 30 cubic angstroms mm, at least 34 cubic angstroms, at least 38 cubic angstroms, at least may be at least 42 cubic angstroms, or at least 44 cubic angstroms. In another example, V N / AA is at most 54 cubic angstroms and at most 51 cubic angstroms. Angstroms, up to 49 cubic angstroms, or up to 47 cubic angstroms, Or up to 45 cubic angstroms. In a specific example, V N / AA This specification The range may include any of the minimum and maximum values ​​set forth in the document.

[0058] The conventional crystal structure of Li3YBr6 is represented by the C2 / m space group and has Two formula units, Li3YBr6, 12 Br atoms, and approximately 534 cubic angstroms of V An exemplary embodiment of Li3YBr6 has a crystal structure represented in the R-3m space group: and 1 formula unit, 6 Br atoms, and approximately 267 + / - 3% cubic angstroms per unit cell. Another exemplary Li3YBr6 of an embodiment may include 100% V per unit cell. The crystal structure is expressed in the C2 / m space group, has 2 / 3 formula units, 4 Br atoms, and approximately 178+ / It may contain -3% cubic angstroms of V.

[0059] In another embodiment, the halide-based material has a crystal structure represented by the hexagonal space group. The unit lattice constants a and b are equal. Referring to FIG. 5, the parameters a, A hexagonal unit cell 500 is shown, comprising: The molecule may be represented by the P63 / mcm space group. In another embodiment, the hexagonal unit cell is It can be represented by the P63 / mmc space group.

[0060] In one embodiment, the P63 / mcm unit cell can include a specific A, B, or C. , A or B, or both, are at least 5.0 angstroms, at least 5.5 angstroms angstroms, at least 6.1 angstroms, or at least 6.3 angstroms In another embodiment, A or B or both can be up to 8 angstroms, or is at most 7.5 angstroms, or at most 7.0 angstroms, or at most 6. 5 angstroms. Further, A, B, or both may be any of the maximum lengths described herein. In a further aspect, the halogen atom can be in a range including any of the lower and upper values. The nitride-based material may include a crystal structure that includes a specific C. In one example, C is at least 4. 8 Å, at least 5.3 Å, at least 5.7 Å In one example, C can be at most 6. .9 Angstroms, up to 6.4 Angstroms, or up to 6.1 Angstroms In a further example, C can be any of the minimum and maximum values ​​described herein. The range may be inclusive.

[0061] In a further embodiment, the P63 / mcm unit cell comprises a unit cell volume V having a particular value. For example, V may be at least 150 cubic angstroms, at least 170 cubic angstroms, at least 190 cubic angstroms, at least 205 cubic on In a further example, V is at most 270 cubic angstroms, at most 250 cubic angstroms, at most 2 30 angstroms, or up to 220 angstroms. In examples, V can be within a range that includes any of the minimum and maximum values ​​described herein. can.

[0062] In certain embodiments, the P63 / mcm unit cell has a particular V N / FUIn one example, , the halide-based material is at least 150 cubic angstroms, at least 170 cubic angstroms at least 190 cubic angstroms, at least 200 cubic angstroms angstroms, or at least 210 cubic angstroms of V N / FU Crystal structure containing In another example, V N / FU is at most 270 cubic angstroms, at most 250 cubic angstroms, up to 230 cubic angstroms, or up to 220 cubic In a specific example, V N / FU is the minimum value stated in this specification and the maximum value.

[0063] In a further embodiment, the P63 / mcm unit cell has a unit volume per halogen atom, V N / AA The normalized volume can include N / AA =V / N AA and N AA is the unit represents the number of halogen atoms in the lattice. In certain embodiments, the halide-based material has a particular V N / AA In one example, the crystal structure may include N / AA At least 25 cubic ounces Angstroms, at least 28 cubic angstroms, at least 31 cubic angstroms mm, at least 34 cubic angstroms, or at least 36 cubic angstroms Possibly. In another example, V N / AA is a maximum of 50 cubic angstroms and a maximum of 47 cubic Angstroms, up to 44 cubic angstroms, or up to 41 cubic angstroms Angstroms, or up to 38 cubic Angstroms. N / AA teeth , may be within a range including any of the minimum and maximum values ​​stated herein.

[0064] In one embodiment, the P63 / mmc unit cell can include a specific A, B, or C. , A or B, or both, are at least 2.5 angstroms, at least 2.8 angstroms angstroms, at least 3.2 angstroms, or at least 3.6 angstroms In another embodiment, A or B or both can be up to 5 Angstroms, up to Largest 4.6 angstroms, Maximum 4.3 angstroms, Maximum 4.1 angstroms Angstroms, or up to 3.8 Angstroms. can be within a range including any of the minimum and maximum values ​​described herein. In another embodiment, the halide-based material may include a crystal structure that includes a specific C. , C is at least 4.8 angstroms, at least 5.3 angstroms, It may be at least 5.7 Angstroms, or at least 6.0 Angstroms. In the example, C is at most 6.9 angstroms, at most 6.4 angstroms, or at most In a further example, C can be as small as 6.1 Angstroms. The range may be inclusive of either the value or the maximum value.

[0065] In a further embodiment, the P63 / mmc unit cell comprises a unit cell volume V having a particular value. For example, V may be at least 60 Å or at least 65 Å. angstroms, at least 68 cubic angstroms, or at least 70 cubic angstroms In another example, V may be up to 85 angstroms, up to 82 cubic angstroms, up to 78 cubic angstroms, up to 74 cubic angstroms In a further example, V can be any of the following: The range may include any of the minimum and maximum values ​​set forth in the document.

[0066] In certain embodiments, the P63 / mmc unit cell has a particular V N / FU In one example, The halide-based material is at least 150 cubic angstroms and at least 170 cubic angstroms, at least 190 cubic angstroms, at least 200 cubic on angstroms, or at least 210 cubic angstroms of V N / FU Crystal structure containing In another example, V N / FU is at most 270 cubic angstroms and at most 2 50 cubic angstroms, up to 230 cubic angstroms, or up to 220 cubic In a particular example, V N / FU is the minimum value and The range may be inclusive of either the maximum or minimum value.

[0067] In a further embodiment, the P63 / mmc unit cell has a unit volume per halogen atom V N / AA The normalized volume can include N / AA =V / N AA and N AA is the unit represents the number of halogen atoms in the lattice. In certain embodiments, the halide-based material has a particular V N / AA In one example, the crystal structure may include N / AA At least 25 cubic ounces Angstroms, at least 28 cubic angstroms, at least 31 cubic angstroms mm, at least 34 cubic angstroms, or at least 36 cubic angstroms Possibly. In another example, V N / AA is a maximum of 50 cubic angstroms and a maximum of 47 cubic Angstroms, up to 44 cubic angstroms, or up to 41 cubic angstroms Angstroms, or up to 38 cubic Angstroms. N / AA teeth , may be within a range including any of the minimum and maximum values ​​stated herein.

[0068] The conventional crystal structure of Li3YCl6 is in the Pnma space group, with a single unit cell of the formula Li3YBr contains 4 positions, 24 Cl atoms, and about 875 cubic angstroms of V. Another conventional crystal structure of 6 is represented by the P-3m1 space group, with formula units 3, 18 Cl atoms, and approximately 655 cubic Angstroms of V. Exemplary Li3YCl6 can have a crystal structure represented by P63 / mcm, with the unit lattice Each molecule contains one formula unit, six Cl atoms, and 218+ / -3% Å of V Another exemplary Li3YCl6 of an embodiment is represented in the P63 / mmc space group. The crystal structure may contain 1 / 3 formula units, 2 Cl atoms, and 7 It may contain 3+ / -3% V cubic Angstroms.

[0069] In one embodiment, the solid electrolyte material has atomic disorder in the atomic positions of vacancies and Me. and irregular X1 and X2 atoms (X1 and X2 represent two different halogen atoms). , irregular vacancy sites and M atoms, irregular M and Me atoms, irregular M, Me, and vacancies Halide-based materials that contain irregularities in the crystal structure, such as holes, atoms, or any combination thereof. may include.

[0070] In another embodiment, the halide-based material has at least some of the positions of the vacancies and Me atoms. Crystal structures containing vacancies and Me atoms in which Me is disordered in atomic layers or linear atomic chains. In one embodiment, the halide-based material may include a structure in which the atomic positions of vacancies and Me are atomically It may include a crystal structure that is disordered, the disorder being at least 10%, at least At least 20%, at least 30%, at least 40%, at least 60%, at least 80% , or at least 90%.

[0071] Atomic disorder is revealed by Rietveld refinement of X-ray powder diffraction patterns of halide-based materials. More specifically, the crystallographic sequence including the positions of M atoms, Me atoms and vacancies was refined by the After reading this application, the skilled artisan will be able to determine the crystal structure of the crystalline structure based on the occupancy rate of the crystal structure. The atomic disorder can be understood based on the occupancy of the chemical sites, and the following steps can be taken: Therefore, a decision can be made on a case-by-case basis.

[0072] X-ray diffraction (XRD) analysis was performed on the powdered halide materials, and the XRD patterns were recorded. The simulated XRD patterns can be recorded to obtain the best fit. A set of methods to get the best fit and determine the occupancy of crystallographic sites. The crystal structure parameters (e.g., unit cell parameters, atomic vacancies, and By refining the parameters (and other parameters) the XRD of halide-based materials is fitted. Then, based on the occupancy of the crystallographic sites, The disorder of atoms can be determined.

[0073] Here, Li3MeBr6 is used as an example of a halide material. Vacancies can be included in the formula, and halide-based materials are Li3Me· oct Expressed as 2Br6 The Li3MeBr6 according to the embodiment of the present invention is a crystal represented by the R-3m space group. When the occupancy rate of Me sites is 33.33%, the crystal structure is Octahedral vacancy oct and the position of Me atom is complete It is completely atomically disordered, i.e., 100% Me-vacancy disorder (the origin of vacancies and Me atoms) The molecular positions can be indistinguishable from the X-ray powder diffraction pattern. Li3MeBr6 can have a crystal structure that is represented by the C2 / m space group. To further aid, briefly referring to FIG. 1B, as shown, a Me atom 130 and a vacancy The co-occupancy of crystallographic site 160 by 140 is low (ie, less than 10%).

[0074] As another example, the vacancies in the crystal structure of Li3MeBr6 can be included in the formula, and the halogens Li3Me· oct 2Br6. Li3MeCl6 in the form of Li3MeCl6 has a crystal structure that can be described as the P63 / mcm space group. When the occupancy of the Me site is 33.33%, the crystal structure is an octahedral vacancy. oct and The Me sites are completely atomically disordered, i.e., 100 based on the powder XRD pattern. %Me-vacancy disorder (atomic positions of vacancies and Me atoms cannot be distinguished) do.

[0075] As described in the embodiments herein, halide-based materials can have multiple phases. The atomic disorder can be determined by considering the phase concentration. For example, The halide-based materials are represented by a first space group that is different from the corresponding conventional halide-based materials. A first crystalline phase having a crystal structure and a% atomic disorder (the concentration of the first crystalline phase is b% by weight) (can be expressed as follows) and a crystal structure represented by a second space group and an irregular structure of c% of atoms. and a second crystalline phase having a regularity of d% by weight. The space group may be the same or different from the corresponding conventional halide-based materials. Nitride-based materials are linear total disorder. er) atomic disorder. D LT is the formula D LT =a% * b%+c% * To further aid in understanding, in one example, the first phase is determined by a concentration of 90%. and the atomic disorder can be 96%, and the second phase can have a concentration of 10 wt.% and The atomic disorder of halide-based materials can be as low as 6%. LT =90% * 96%+10% * 6%=87%.

[0076] In another embodiment, the halide-based material has a crystallographic structure in which both Me atoms and vacancies are occupied. In one embodiment, the multiplicity of the crystallographic site is 3. In another embodiment, the crystallographic site can be Wycoff position 3a or 3b.

[0077] In another embodiment, the halide-based material is a crystallographic material dominated by both Me and M atoms. In one embodiment, the atomic disorder may include a crystal structure including Y and Li atoms. In certain embodiments, at least 5% of the Y atoms may be co-occupied, at least 10 %, or at least 20% can co-occupy the Li sites. At most 50%, at most 70%, or at most 90% of the Y atoms may co-occupy the Li sites. In another particular embodiment, the Y atoms present at the Li sites are transferred from one layer to another in the crystal structure. This can be caused by the migration of some Y atoms into the layer of the halide. This can result in a decrease (eg, a slight decrease) in the intensity of the first XRD peak of the nitride-based material.

[0078] In a particular embodiment, the X-ray diffraction pattern of the halide-based material measured with CuK-α radiation is The peaks between 16° and 25° 2θ compared to the corresponding traditional halide-based materials. Specific examples of such halide-based materials are Li, Y, and B. In certain embodiments, X can have a chemical composition comprising: The X-ray diffraction pattern does not necessarily have to have multiple peaks between 2θ of 16° and 25°. In certain embodiments, the X-ray diffraction pattern essentially has peaks between 2θ of 16° and 25°. It does not have to be included.

[0079] Halide-based materials contain XRD patterns that do not have peaks in a specific range of 2θ. It should be understood that the range may vary as the chemical composition is changed. Me may be partially replaced by another Me metal, and the change in the 2θ range is partially This can be inversely correlated with the change in lattice constant caused by the substitution of The lattice constant of the LYB material described in the embodiment is determined by dividing Y by another Me ion having a larger size. The 2θ range of 15.2°C to 23.75°C can be increased by 5% by selective substitution. In another example, the lattice constant of the LYB material is such that Y is more strongly polarized than Y. Partial substitution of Me ions with other Me ions with smaller sizes can reduce the ion concentration by 7%, while 1 There may be no XRD peaks at 2θ between 7.12° and 26.75°. Partial substitution of Me The lattice constants that may be affected by may include A, C, B, or any combination thereof. In some cases, A and C may be equally affected. In other cases, A and C may be slightly different. It can be affected.

[0080] 1A to 1C, as shown in FIG. 1A, the crystal structure represented by R-3m is The positions of Me and vacancies are irregular. The octahedral site 160 is occupied by Me atoms 130 and vacancies 14. 0. As shown, 1 / 3 of the octahedron 160 is occupied by Me. This structure represents a relatively high degree of disorder of the Me vacancies. In comparison with the conventional C2 / m shown in FIG. 1B, the atomic position 160 is nearly empty or nearly full. Therefore, one Me atom 130 and two vacancies 140 are arranged in the order of vacancy / vacancy (unfilled sphere). ) and Filled / Occupied (Partially Filled Balls) Regular or Ordered Putts Within the Site This arrangement represents a low degree of disorder of the Me vacancies (i.e., less than 10%). In Figure 1C, the C2 / m space group unit cell shown is much smaller than the conventional unit cell shown in Figure 1B. The volume is smaller than that of the Me atom, and the vacancy is located at the same position, i.e., 1 / 3 and 2 / 3 of the same position. This configuration also represents a relatively high degree of disorder of the Me vacancies.

[0081] 6A and 6B are diagrams showing yttria bromide having the crystal structures shown in FIGS. 1A and 1B, respectively. The spectrum in Figure 6B includes a simulated powder X-ray diffraction spectrum of lithium. In comparison, the spectrum shown in Figure 6A has no peaks between 16° and 25° 2θ. This indicates that the Y positions and vacancy positions in the crystal structure of R-3m are completely disordered. Similarly, in comparison with the spectrum in FIG. 6B, the spectrum shown in FIG. 6C shows that This shows that the peaks from 6° to 25° 2θ are absent, which is different from the conventional monoclinic crystal. Y in a crystal structure represented by the C2 / m space group with a unit cell approximately three times smaller than the unit cell It is shown that the positions and void positions are quite random.

[0082] 7A to 7E show X-ray diffraction patterns of halide-based materials containing Li, Y, and Cl with different crystal structures. The spectrum of the diffraction simulation is shown in Fig. 7A, which is expressed in Pnma as shown in Fig. 2A. FIG. 7 shows a simulated spectrum of a halide-based material having the crystal structure shown in FIG. B is a halide-based material having a crystal structure represented by P-3m1 as shown in Figure 2B. FIG. 7C is a simulated spectrum of the space group P63 / mc 1 is a simulated spectrum of a halide-based material having a crystal structure represented by m. 2A to 2C, Pnma (FIG. 2A) or P-3m1 (FIG. 2B) The crystal structure of the P63 / mcm (Fig. 2C) has a regular Y-position and vacancy position. The structure is linearly irregular in the Y210 positions and the positions of the vacancies 220. The atomic order of 01 is such that Y210 and vacancies 220 alternate and are regular in a linear chain containing octahedra. The atomic disorder in Figure 2C is shown by the linear 2-chain structure containing octahedra. 30, 50% Y210 and 50% voids 220 are perfectly mixed. In each XRD pattern, linear irregularities are shown in FIG. In comparison with FIG. 7B, the peaks in FIG. 7C are absent from 16.5 to 27.5° 2θ. This is demonstrated by:

[0083] FIG. 7D shows a halo with irregularities in the crystal structure including partial Y migration into the Li channel. 1 is a simulated spectrum of a fluoride-based material. In one example, at least 5 of the Y atoms %, at least 10%, or at least 20% can migrate into the Li channel. FIG. 7E shows a simulation scan of a halide-based material with the crystal structure of P63 / mmc. As shown in FIG. 2D, and in comparison with FIG. 2A and FIG. 2B, P63 / In the crystal structure of mmc, 203, Y is completely mixed with the Li atom, as shown by 240. In a particular example, the halide-based material is lithium yttrium chloride. The disorder in the crystal structure may be a complete mixture of Y and Li sites. In comparison with the spectra shown in FIGS. 7A and 7B, the spectra in FIGS. 7C to 7E At 16.5° to 27.5° 2θ, one or more peaks are missing. The XRD pattern shows that the first XRD peak near 15.5° 2θ is The mark may be completely missing.

[0084] The halide-based material of the embodiments herein may be one or more of the compounds referred to in the embodiments herein. The irregularities in the crystal structure, the average diffracting crystallite size, and the micro-struc- ain), corrected mean FWHM, crystallographic density, or any combination thereof. It is worth noting that the crystallinity characteristics may include one or more irregularities, one or more Certain crystallinity characteristics, or any combination thereof, facilitate improved properties of the solid electrolyte material. Such properties may include, but are not limited to, ionic conductivity, mechanical properties, and the like. However, the properties of plasticity, conformability, compatibility, flexibility, electrochemical stability, chemical stability, and thermal stability are not included. properties, electronic resistivity, particle morphology and / or size, electrode wettability, etc., and / or their Any combination may be included.

[0085] In another embodiment, the solid electrolyte material is a halogen-containing electrolyte having a particular average diffracting crystallite size. The average diffracting crystallite size may be greater than or equal to the coherent X-ray scattering domain size. Also called X-ray diffraction analysis of halide-based materials and Scherrer's method The formula L = (Kλ) / (βcosθ) (where L represents the average diffracting crystallite size and K is close to 1) is a dimensionless form factor with typical values ​​between 0.9 and 1; λ is the X-ray wavelength. β is the half maximum intensity (FWHM) after subtracting the instrumental line broadening. is the linewidth broadening in radians; θ is the Bragg angle) It is possible.

[0086] In one embodiment, the average diffracting crystallite size is at least 20 nm, at least 25 nm, It may be at least 30 nm, at least 35 nm, or at least 40 nm. In the case of , the average diffraction crystallite size is 500nm at maximum, 400nm at maximum, and 300nm at maximum. m, at most 200 nm, or at most 100 nm. The crystallite size can be within a range including any of the minimum and maximum values ​​set forth herein. .

[0087] In further embodiments, the halide-based material may include microstrain. The microstrain ε is , a dimensionless parameter β=4ε tan θ as determined by X-ray diffraction analysis. , Micro distortion is 1% max, 0.6% max, 0.35% max, 0.2% max, or The strain may be at most 0.1%. In another embodiment, the strain may be absent. In some embodiments, the microstrain is at least 0.05%, at least 0.08%, at least It may be at least 0.005%, such as 0.1%, or at least 0.2%. The halogenide-based material may be any of the following microscopic percentages inclusive of the minimum and maximum percentages set forth herein. It may include distortion.

[0088] In a further embodiment, the halide-based material has a diffraction angle 2θ range of 10° to 80°. The correction may include a corrected FWHM averaged over the entire spectrum (referred to as the "corrected average FWHM"). Positive mean FWHM refers to the mean FWHM corrected for instrument broadening. The broadening due to the measurement instrument is performed under the same measurement conditions (diffraction) as the halide-based material being tested. under the geometry of the detector, slits, detector, or other hardware and optical parameters , record the X-ray diffraction pattern of the highly crystalline standard commercial material LaB6 (supplier: NIST). The peak broadening of the standard material can be determined by comparing the peak broadening of the halide-based material. The peak broadening is subtracted to obtain the corrected FWHM as a function of the diffraction angle 2θ. The corrected average FWHM is less than 1.5%, up to 1.4%, up to 1.2%, and up to 1%. , at most 0.8%, or at most 0.5%. In another embodiment, the halide-based material is at least 0.5%, at least 0.8%, or at least 1% corrected mean FWHM Additionally, the corrected average FWHM may include any of the minimum and maximum % values ​​described herein. The range may be inclusive.

[0089] In one embodiment, the halide-based electrolyte material has a specific The crystallographic density can include the crystallographic density of the unit cell, which is given as the ratio of the mass to the volume of the unit cell: The mass of a unit cell is the number of atoms in the unit cell and the mass of each atom in the unit cell. In one embodiment, the halide-based material has a density less than the theoretical crystallographic density. In another embodiment, the halo may have a crystallographic density of at least 95% and up to 100%. The crystallographic density range for fluoride-based electrolyte materials is 2.0 g / cm 3 ~4.2g / cm 3 in There can be.

[0090] In certain embodiments, the crystallographic density range for the halide-based electrolyte material is If yes, 3.0g / cm 3 ~4.2g / cm 3 or 3.4 g / cm 3 ~3.9g / cm 3 In another particular embodiment, the crystallographic The density range is 2.0 g / cm when X is Cl. 3 ~3.2g / cm 3 Or 2.2g / cm 3 ~2.8g / cm 3 It can be said that:

[0091] FIG. 8 illustrates a process for forming a solid electrolyte material that includes a halide-based material 800. The process 800 starts at block 802 with the steps of: n Me k+ X n+k Form In an exemplary embodiment, the process 800 may include the step of: , NH4X, one or more Me metal compounds, one or more M metal compounds, or any of them. In certain implementations, the method may include forming a reaction mixture comprising the combination of starting materials. Metal compounds can be non-hygroscopic. Metal compounds can be oxides, carbonates, sulfides, sulfates, hydrates, etc. The salt may be in the form of a salt, hydroxide, oxalate, acetate, nitrate, or any combination thereof. In a particular embodiment, the starting material is MeO k In certain instances, the starting material may include Earth oxides or hydroxides or carbonates, ZrO2 or Zr(OH)4 or Zr(CO3)2 or Zr(OH)2CO3·ZrO2 or any combination thereof. do.

[0092] In another example, the M metal compound may be a carbonate, such as lithium carbonate, sodium carbonate, cerium carbonate, The metal may include, for example, sodium, sodium, or a combination thereof.

[0093] The starting materials are prepared in a manner that facilitates acid synthesis in aqueous, alcoholic or other polar liquid solutions. The acid may further comprise a carboxylic acid.

[0094] In one example, the metal compound can consist of M metal compounds. Exemplary M Metal Compounds may include halides (e.g., NaCl, CsCl, and LiCl).

[0095] The starting materials may be prepared in a manner that allows for the formation of stoichiometric or non-stoichiometric halide-based materials. The components may be mixed together in such a way that

[0096] In certain exemplary implementations, NH4X, one or more rare earth metal oxides (hereinafter "RE2O3 "), lithium carbonate, and hydrochloric or hydrobromic acid. can.

[0097] In an exemplary embodiment, process 800 can include a step of performing a reaction between starting materials. An exemplary reaction is shown below, focusing on the starting materials and reaction products in aqueous solution. 3 * Li2CO3+RE2O3+12 * HX+6 * NH4X--->2 * (NH4)3 REX6+3 * LiX+6 * H2O+3 * CO2

[0098] In view of the present application, one of ordinary skill in the art may In addition, or instead of RE2O3, different alkali metals such as Na2CO3 or NaCl It is understood that compounds such as MgO or ZrO2 can also be used. Oxides of elements can be added to the reaction. Those skilled in the art will further appreciate that if the starting materials are varied, It will be appreciated that the reaction products may vary accordingly.

[0099] In an exemplary embodiment, the process 800 comprises the steps of: k The moisture in (i.e. Using the reaction illustrated above as an example, The intermediate product can be a hydrated rare earth halide, and the water in the hydrate can be converted to N It can be replaced with H4X to form (NH4)3REX6. The reaction product mixture includes an alkali metal halide such as Lix.

[0100] In one embodiment, the process 800 comprises reacting (NH) n Me k+ X n+k and LiX In certain embodiments, the process 800 may include forming a mixture of (NH4) n M e k+ X n+k and forming a homogenous mixture comprising LiX.

[0101] In one example, the reaction product mixture is filtered to remove larger particles and its The larger particles can be used for either the starting material or the starting These include impurities associated with the remaining particles of the material, carbon, or any combination thereof.

[0102] The process 800 may proceed to block 804. In an exemplary embodiment, the reaction product The product mixture was dried and (NH4) n Me k+ X n+k and alkali metal halides This can promote the solid reaction with MX. Drying can be done in air or dry air and / or can be vacuum or 100mbar, 40mbar, 1mbar or even 0.01mbar The reaction can be carried out under reduced pressure, such as under reduced pressure. Optionally, N2 or Ar can be used to facilitate the removal of water. In another example, heat can be applied to help evaporate the water. The heating temperature may be 100°C to 160°C. The process can be continued until the amount of water contained in the solution becomes very small, for example, 1% by weight to 3% by weight.

[0103] In an exemplary embodiment, the process 800 comprises reacting (NH) n Me k+ X n+k and MX In a particular example, the reaction may include carrying out a solid-state reaction using the reaction product described above. Continuing, the solid reaction of (NH4)3REX6 and LiX was carried out to obtain (NH4) n M 3-Z M e k+ X 3+n+k-z In a further example, the process 100 can include: (NH4) n M 3-Z (Me k+ ) f X 3+n-z+k*f The method may include forming a

[0104] The process 800 proceeds to block 806, where M 3-Z (Me k+ ) f X 3-z+k*f of In an exemplary embodiment, the process 800 comprises decomposing an ammonium halide. In an exemplary embodiment, the solid solution may include a sublimation step of an ammonium halide. To achieve this, the material may be heated to a temperature of at least 150° C. and up to 800° C. The heating temperature can be selected based on the composition of the halide-based material. For relatively volatile halide-based materials, the heating temperature can be relatively low. In the case of the present invention, the heating temperature may be at least 150° C. lower than the melting temperature, and / or the melting temperature The heating may be performed at up to 50°C higher than the reactants and products. For example, the crucible may be made of quartz, alumina, silica-alumina, B The material may be made of N, glassy carbon, or graphite. In certain embodiments, the graphite The sheet may have a pyrolytic carbon coating. The heating may be performed with air or dry air, etc. The process may be carried out in a dry, neutral atmosphere, such as N2 or Ar, to facilitate the process. Inert gas may be used. Heating should be done for at least 15 minutes and up to 12 hours. This may also be the case.

[0105] In an exemplary implementation, the sublimation of NH4X is measured by collecting and weighing the escaped NH4X. In certain instances, halide-based materials can essentially convert NH4X into In another specific example, the sublimation can be completed so that it does not contain any amount of NH4X may remain in the halide-based material.

[0106] In an exemplary implementation, after decomposition of NH4X, cooling can be performed. For example, in air, dry Cooling may be performed in dry air or nitrogen. In another example, the cooling temperature is less than 200° C. ( For example, up to 100°C, up to 70°C, up to 50°C, or up to 30°C, etc.), or room temperature (e.g., 20 to 25°C). Optionally, Ar or N2 may be used to facilitate cooling. May be used.

[0107] In one embodiment, at certain cooling rates that can facilitate the formation of halide-based materials, Cooling can be performed. In one example, the cooling rate can be 10 to 100° C. / min.

[0108] Temperature cycling should be done carefully to form halide-based materials with higher stacking fault content. Note that the cooling system should be controlled carefully to prevent, for example, non-monotonous cooling or unintended activation. Annealing can reduce the stacking fault content. , annealing at a temperature less than 0.7Tm, where Tm is greater than 10 minutes. is the melting point of the halide-based material over time (in Kelvin).

[0109] Oxygen-containing species (e.g., oxides, It is further noted that care should be taken to carefully control the number of Note that excess oxygen-containing species may be present in battery components formed using halide-based materials. This can lead to the formation of impurity phases that can reduce certain performance characteristics, such as the ionic conductivity of the For example, solid state or melt reactions may be carried out with less than 10 ppm moisture or limited oxygen levels. In a further example, the reaction can be carried out in a neutral atmosphere using an acid or ammonium halide. The initial amount of halide compounds such as fluorine is and obtaining a complex halide material in a high yield, and an oxygen-containing phase derived from a metal oxide or metal carbonate raw material. To reduce the level of may be higher than the stoichiometric amount based on (e.g., at least 10% higher).

[0110] In another embodiment, the halide-based material has improved ionic conductivity. The on-conductivity can be measured at room temperature (i.e., 20°C to 25°C). , the ionic conductivity is at least 0.001 mS / cm, at least 0.01 mS / cm, At least 0.1mS / cm, at least 0.4mS / cm, at least 0.8mS / cm m, at least 1.2 mS / cm, at least 1.8 mS / cm, or at least 2.2 In another embodiment, the ionic conductivity can be at most 15 mS / cm, at most 13mS / cm, up to 11mS / cm, 8mS / cm, up to 7.2mS / cm, or In addition, the solid electrolyte may have a maximum resistance of 6.2 mS / cm. The material may include halide-based materials having ionic conductivities ranging from and including any of the maximum values. In one embodiment, the ionic conductivity may be primarily bulk.

[0111] In one embodiment, the halide-based materials have the following properties compared to corresponding conventional halide-based materials: The corresponding conventional halide-based materials are of improved purity. The halide-based materials described in the embodiments of the present specification may be represented by the same formula as the halide-based materials described in the embodiments of the present specification. Refers to halide-based materials formed by processes other than those described. In one embodiment, the halide-based material may include a specific content of impurities. For example, impurities may be by-products formed by processes that form halide-based materials. The impurities may include complex compounds of halide-based materials, The skilled artisan will appreciate that impurities may be present in a relatively large amount (i.e., At least 0.3% by weight of the halide-based material is subjected to X-ray diffraction analysis to determine the impurity phase. For example, the spectrum of a halide-based material can be seen to be In a further example, the impurity may be a binary halo. halides (e.g., LiCl, LiBr, YCl3, and / or YBr3), oxyhalides hydrides (e.g., YOCl and / or YOBr), nitrides, or any combination thereof. may include.

[0112] In one embodiment, the halide-based material is characterized by the properties and / or crystal characteristics of the halide-based material. In one embodiment, the composition may include all impurities that may promote improved properties, in a specified total content. The total content of pure matter is up to 15% by weight of the halide-based materials of the embodiments herein. For example, the total content of impurities may be calculated based on the weight of the complex metal halide. up to 14% by weight, for example up to 13% by weight based on the weight of the complex metal halide; Up to 12% by weight, up to 11% by weight, up to 10% by weight, up to 9% by weight, up to 8% by weight %, up to 7% by weight, up to 6% by weight, up to 5% by weight, up to 4% by weight, up to 3 times %, up to 2% by weight, up to 1% by weight, up to 0.5% by weight, up to 0.3% by weight, up to 0.1% by weight at most, 500 ppm at most, 300 ppm at most, 100 ppm at most, 50 ppm at maximum, 40 ppm at maximum, 30 ppm at maximum, 20 ppm at maximum, or In another embodiment, the total impurity content of the halide-based material may be: At least 0.2 ppm by weight of halide-based materials, e.g. at least 0.5 ppm, at least 1 ppm, or at least 2 ppm by weight In another embodiment, the total content of impurities may be less than or equal to the minimum or maximum values ​​described herein. The range can be inclusive of any of the values.

[0113] The content of impurity phases is determined by the characteristic corresponding to the by-product phases (parasitic phases). Quantitative analysis was performed based on the presence of characteristic diffraction peaks, and the XRD analysis was converted into a Rietveld solution. It can be determined by combining refinement by Rietveld refinement ( RR) is a method for determining the shape and position of peaks in an XRD pattern by measuring small increments of 2θ angle. To collect 2θ data in XRD diffraction and convert the XRD data into the ratio of different phases allows the contributions of the various phases to be quantitatively identified.

[0114] In the case of nitride-based impurity phases, the nitride-based impurity phases are present in an amount of less than 0.1% by molar amount or mass. If present, LECO analysis can also be used to determine and quantify the presence of phases. O analysis is performed by combusting the sample and measuring the thermal conductivity of the boiled material gas or the nitrogen (or The method is based on the analysis of the presence of elements such as nitrogen, sulfur, carbon, hydrogen, and oxygen.

[0115] In certain embodiments, the halide-based materials may contain low levels of impurity phases, Phases may not be detected by powder XRD analysis. For example, halide-based materials In the spectrum, the characteristic peaks of the impurity phase may not be discernible. If available, a state-of-the-art diffractometer (e.g., Rigaku SmartLab or Bruker It can be seen that powder XRD can be carried out using a 300 MHz 300 MHz 300 MHz PHASER. Wax.

[0116] In one embodiment, the impurities are metal nitrides, metal oxynitrides, metal carbonitrides, or the like. In further embodiments, the nitride-based compounds may include any combination of halides. The halide-based materials have specific total content that can facilitate improving the properties and / or crystal properties of the halide-based materials. In one embodiment, the total content of the nitride-based impurity phase is Maximum 0.5% by weight based on the weight of the halogenide-based material, e.g. Maximum 0.3% by weight, maximum 0.2% by weight, maximum 0.1% by weight, maximum 50 0ppm, max 300ppm, max 100ppm, max 50ppm, max 40ppm pm, up to 30 ppm, up to 20 ppm, or up to 10 ppm. In an embodiment, the total content of the nitride-based impurity phase is less than the weight of the complex metal halide. 0.2 ppm or less, for example at least 0.5 ppm by weight of the complex metal halide , at least 1 ppm, or at least 2 ppm. The total content of the solid impurity phase is within a range including either the minimum or maximum value described herein. It may be.

[0117] In one embodiment, the halide-based material comprises an alkali metal halide (MX). Specific examples of MX include LiCl, LiBr, NaCl, CsCl, In another embodiment, the halogen atom may include NaBr, CsBr, or any combination thereof. Halide-based materials have certain properties that may facilitate improved properties and / or crystal properties of halide-based materials. In one embodiment, the total content of MX phases is the weight percent of the halide-based material. Maximum 10% by weight of the amount of the halide-based material, e.g., maximum 9% by weight of the halide-based material %, up to 8% by weight, up to 7% by weight, up to 6% by weight, up to 5% by weight, up to 4% by weight %, up to 3% by weight, up to 2% by weight, up to 1% by weight, up to 0.5% by weight, up to 0.3% by weight, max. 0.2% by weight, max. 0.1% by weight, max. 500 ppm, max. 300ppm, max 100ppm, max 50ppm, max 40ppm, max 30 ppm, up to 20 ppm, or up to 10 ppm. In another embodiment, the MX phase The total content of halide-based materials is at least 0.2 ppm by weight, e.g. At least 0.5 ppm, at least 1 ppm, or less by weight of the fluorine-based material In another embodiment, the total content of MX phases is at least 2 ppm. It may be within a range including either the lower or maximum value.

[0118] In one embodiment, the halide-based material comprises a metal oxyhalide (MeOX). It may contain impurities. Examples of MeOX include rare earth oxyhalides. In a further embodiment, the halide-based material is characterized by the properties of the halide-based material and / or The total content of MeOX may be included, which may promote improvement of crystal properties. In one embodiment, the total content of MeOX may be included. The content is up to 5% by weight based on the weight of the complex metal halide, e.g. Maximum 4% by weight, Maximum 3% by weight, Maximum 2% by weight, Maximum 1% by weight of the material , up to 0.5% by weight, up to 0.3% by weight, up to 0.2% by weight, up to 0.1% by weight , up to 500ppm, up to 300ppm, up to 100ppm, up to 50ppm, Maximum 40ppm, maximum 30ppm, maximum 20ppm, maximum 10ppm, etc. In another embodiment, the content of the MeOX phase is based on the weight of the complex metal halide. at least 0.2 ppm by weight of halide-based material, e.g. at least 0. It may be 5 ppm, at least 1 ppm, or at least 2 ppm. The total content of MeOX phases may be within a range including any of the minimum and maximum values ​​set forth herein. In certain embodiments, the halide-based material can be essentially free of MeOX. good.

[0119] In one embodiment, the halide-based material is a metal nitride, Me x Nk Contains impurities including Get. x N k Examples of the nitrides include rare earth nitrides. The halogenide-based materials may facilitate improving the properties and / or crystal properties of the halide-based materials. , a certain total content of Me x N k In one embodiment, the Me x N k The total content of Maximum 0.3% by weight based on the weight of the halide-based material, e.g. Maximum 0.1% by weight, maximum 500 ppm, maximum 300 ppm, maximum 10 0ppm, max 50ppm, max 40ppm, max 30ppm, max 20ppm , or up to 10 ppm, etc. In another embodiment, Me x N k The phase content is At least 0.2 ppm by weight of halogen-based materials, e.g. At least 0.5 ppm, at least 1 ppm, or at least 2 ppm, etc. In another embodiment, Me x N k The total content of the phases is the minimum or maximum value given herein. It may be within a range including either of the greater values.

[0120] In one embodiment, the halide-based material is a metal nitride M x It may contain N-containing impurities. M x Examples of N include alkali metal nitrides. In a further embodiment, halogen Halide-based materials can facilitate improving the properties and / or crystal properties of halide-based materials, particularly The total content of M x In one embodiment, the metal nitride M x The total N content is Maximum 0.3% by weight of halogen-based materials, e.g. Maximum 0.1% by weight, Maximum 500 ppm, Maximum 300 ppm, Maximum 100 ppm, max 50ppm, max 40ppm, max 30ppm, max 20ppm, Or up to 10 ppm, etc. In another embodiment, M x The total N content is At least 0.2 ppm by weight of the inorganic material, e.g., at least 0.2 ppm by weight of the halide material at least 0.5 ppm, at least 1 ppm, or at least 2 ppm, etc. In another embodiment, M x The total N content is either the minimum or maximum value described in this specification. The range may be inclusive.

[0121] Many different aspects and embodiments are possible. Some of these aspects and embodiments are described herein. After reading this specification, those skilled in the art will understand that these aspects and embodiments are It will be understood that these are merely illustrative examples and are not intended to limit the scope of the invention. The embodiment may be according to any one or more of the embodiments listed below.

[0122] Embodiment Embodiment 1. A solid electrolyte material, comprising: M 3-z (Me k+ ) f X 3-z+k*f (wherein, −3≦z<3; 2≦k<6, 0≦f≦1; M includes an alkali metal element; Me includes a divalent metal element, a trivalent metal element, A tetravalent metal element, a pentavalent metal element, a hexavalent metal element, or any combination thereof and X is a halogen. a crystal structure containing at least 20% stacking faults; 1. A solid electrolyte material comprising:

[0123] Embodiment 2. The solid electrolyte material according to embodiment 1, wherein the crystal structure is represented by the C2 / m space group. Fee.

[0124] Embodiment 3. A solid electrolyte material, comprising: M 3-z (Me k+ ) f X 3-z+k*f (In the formula, -3≦z<3;2≦k<6;0≦f ≦1; M includes an alkali metal element; Me includes a divalent metal element, a trivalent metal element, a tetravalent metal element, X is a valent metal element, a pentavalent metal element, a hexavalent metal element, or any combination thereof; rogens) and A crystal structure represented by a rhombohedral space group; 1. A solid electrolyte material comprising:

[0125] Embodiment 4. The method according to embodiment 3, comprising the step of: Solid electrolyte material.

[0126] Embodiment 5. A method for producing a crystal structure comprising the steps of: The solid electrolyte material according to any one of aspects 3 to 4.

[0127] Embodiment 6. A solid electrolyte material comprising: X 3-z (Me k+ ) f X 3ーz+k*f (wherein, −3≦z<3; 2≦k<6, 0≦f≦1; M includes an alkali metal element; Me includes a divalent metal element, a trivalent metal element, A tetravalent metal element, a pentavalent metal element, a hexavalent metal element, or any combination thereof and X is a halogen. A crystal structure represented by a hexagonal space group; 1. A solid electrolyte material comprising:

[0128] Embodiment 7. A crystal comprising a crystal structure represented by the P63 / mcm or P63 / mmc space group. 7. The solid electrolyte of embodiment 6, comprising a phase.

[0129] Embodiment 8. A crystal comprising a crystal structure represented by the P63 / mcm or P63 / mmc space group. 8. The solid electrolyte material of embodiment 6 or 7, consisting essentially of a phase.

[0130] Embodiment 9. The present invention relates to a crystalline phase having a crystal structure represented by the P-3m1 or Pnma space group. 7. The solid electrolyte material according to embodiment 1, 3 or 6.

[0131] Concentration of a crystalline phase comprising a crystalline structure represented by the P-3m1 or Pnma space group. However, up to 70% by weight, up to 50% by weight, up to 25% by weight, up to 15% by weight, up to 10. The solid electrolyte material of embodiment 9, wherein the SiO 2 content is 8 wt. %, or at most 5 wt. %.

[0132] Concentration of a crystalline phase comprising a crystalline structure represented by the P-3m1 or Pnma space group. At least 1% by weight, at least 4% by weight, at least 10% by weight, at least 25% by weight %, at least 50% by weight, or at least 70% by weight. The solid electrolyte material according to claim 1,

[0133] Embodiment 12. A solid electrolyte material comprising: M 3-z (Me k+ ) f X 3-z+k*f (wherein, −3≦z<3; 2≦k<6, 0≦f≦1; M includes an alkali metal element; Me includes a divalent metal element, a trivalent metal element, A tetravalent metal element, a pentavalent metal element, a hexavalent metal element, or any combination thereof and X comprises a halogen; Has a unit cell containing 3 to 5 halide atoms a crystal structure represented by a monoclinic space group; 1. A solid electrolyte material comprising:

[0134] Embodiment 13. The method of embodiment 1, comprising the steps of: 3, 6, or 12. A solid electrolyte material according to any one of claims 3, 6, and 12.

[0135] Embodiment 14. The concentration of a crystalline phase having a crystalline structure represented by the C2 / m space group is at most 70 %, up to 50%, up to 25%, up to 15%, up to 8%, or is up to 5 wt. %.

[0136] Embodiment 15. The concentration of a crystalline phase comprising a crystalline structure represented by the C2 / m space group is at least 1% by weight, at least 4% by weight, at least 10% by weight, at least 25% by weight, 50% or at least 70% by weight of the solid according to embodiment 13 or 14. Electrolyte materials.

[0137] Embodiment 16. A solid-state battery according to any one of embodiments 1 to 15, comprising a layered atomic arrangement. solute material.

[0138] Embodiment 17. A represents the value of the unit lattice constant a, B represents the value of the unit lattice constant b, and A= The solid electrolyte material according to any one of embodiments 3 to 8, wherein B is B.

[0139] Embodiment 18. A represents the value of the unit lattice constant a, B represents the value of the unit lattice constant b, and A or A or B is at least 3.0 angstroms, or at least 3.3 angstroms Angstroms, or at least 3.6 Angstroms, or at least 3.9 Angstroms The solid electrolyte material according to any one of embodiments 3 to 5 and 17, which is a polymerizable compound.

[0140] Embodiment 19. A or B or both are at most 4.8 Angstroms, or at most 4.6 Angstroms, or up to 4.3 Angstroms, or up to 4.2 Angstroms Angstroms, or up to 4.0 Angstroms, in embodiments 3-5, 17 and 18. The solid electrolyte material according to claim 1,

[0141] Embodiment 20. C represents the value of the unit cell constant c, and C is at least 17 Angstroms. , at least 18 angstroms, or at least 19 angstroms; 20. The solid electrolyte material according to any one of aspects 3 to 5 and 17 to 19.

[0142] 21.C is up to 21 Angstroms, up to 20.2 Angstroms; or up to 19.5 angstroms. 1. The solid electrolyte material according to claim 1.

[0143] In embodiment 22, A represents the value of the unit lattice constant a, B represents the value of the unit lattice constant b, and A or A or B is at least 5.0 angstroms, or at least 5.5 angstroms Angstroms, or at least 6.1 Angstroms, or at least 6.3 Angstroms The solid electrolyte material according to any one of embodiments 6 to 8, which is a polymerizable compound.

[0144] Embodiment 23. A or B or both are at most 8 Angstroms, or at most 7. 5 angstroms, or up to 7.0 angstroms, or up to 6.5 angstroms The solid electrolyte material according to embodiments 6 to 8 and 22, which is ROHM.

[0145] Embodiment 24. C represents the value of the unit cell constant c, and C is at least 4.8 Angstroms. Angstroms, at least 5.3 Angstroms, at least 5.7 Angstroms, or less In any one of embodiments 6 to 8, 22 and 23, the thickness is at least 6.0 angstroms. The solid electrolyte material described herein.

[0146] C is at most 6.9 Angstroms, at most 6.4 Angstroms; or at most 6.1 angstroms. The solid electrolyte material according to any one of claims 1 to 5.

[0147] Embodiment 26: The solid electrolyte material according to any one of embodiments 3 to 8, A lattice volume V, V being at least 200 cubic angstroms and at least 210 cubic angstroms, at least 230 cubic angstroms, at least 250 cubic on Angstroms, at least 260 cubic angstroms.

[0148] Embodiment 27. The solid electrolyte material according to any one of embodiments 3 to 8, The volume V is 290 Å and 275 Å. Angstroms, up to 250 cubic angstroms, up to 230 cubic angstroms, or A solid electrolyte material that is up to 220 cubic angstroms.

[0149] Embodiment 28. Formula unit FU and unit cell volume V normalized for each FU N / FU Including , V N / FU = V / FU, and V N / FUis at least 200 cubic angstroms, at least 210 angstroms, at least 230 angstroms, or As described in any one of embodiments 1 to 27, which is at least 250 cubic angstroms. Solid electrolyte material.

[0150] Embodiment 29. Formula unit FU and unit cell volume V normalized for each FU N / FU Including , V N / FU =V / N FU and N FU represents the number of formula units, and V N / FU Maximum is 290 cm Angstroms, up to 275 cubic angstroms, up to 270 cubic angstroms 30 or at most 268 cubic angstroms. The solid electrolyte material according to claim 1,

[0151] Embodiment 30. The normalized unit cell volume V for each atom of halogen N / AA Including V N / AA = V / AA and AA is V N / AA At least 30 cubic angstroms, at least At least 34 cubic angstroms, at least 38 cubic angstroms, or at least The solid electrolyte according to any one of embodiments 1 to 29, wherein the thickness of the electrolyte is at least 42 cubic angstroms. quality material.

[0152] 31. Normalized unit cell volume V per atom of halogen N / AA Including V N / AA = V / AA and AA is V N / AA is at most 50 cubic angstroms, and at most 46 cubic angstroms, max 42 cubic angstroms, max 38 cubic angstroms 31. The solid electrolyte material according to any one of embodiments 1 to 30, which is a trompe.

[0153] Embodiment 32. The average diffracting crystallite size is at least 20 nm, at least 25 nm, At least 30 nm, at least 35 nm, or at least 40 nm. 32. The solid electrolyte material according to any one of claims 1 to 31.

[0154] Embodiment 33. The average diffracting crystallite size is at most 500 nm, at most 400 nm, at most Any of embodiments 1 to 32, wherein the thickness is at most 300 nm, at most 200 nm, or at most 100 nm. 13. The solid electrolyte material according to claim 12,

[0155] Embodiment 34. The minute distortion is 1% at most, 0.6% at most, 0.35% at most, 0.2% or at most 0.1%. Electrolyte materials.

[0156] 35. Corrected average FWHM is less than 1.5%, at most 1.4%, at most 1.2%; Any of embodiments 1 to 34, wherein the .alpha.-to-.alpha. ratio is at most 1%, at most 0.8%, or at most 0.5%. 1. The solid electrolyte material according to claim 1.

[0157] Embodiment 36. The corrected mean FWHM is at least 0.5%, at least 0.8%, or less The solid electrolyte material according to any one of embodiments 1 to 35, wherein the number of the first and second electrodes is at least 1.

[0158] Embodiment 37. A method according to claim 3, wherein the crystallographic density is 2.0 g / cm 3 ~4.2g / cm 3 is within the range of The solid electrolyte material according to any one of embodiments 1 to 36.

[0159] Embodiment 38. The solid electrolyte material according to embodiment 37, When X is Br, the crystallographic density of the solid electrolyte material is 3.0 g / cm 3 ~4.2g / cm 3 or 3.4 g / cm 3 ~3.9g / cm 3 or When X is Cl, the crystallographic density of the solid electrolyte material is 2.0 g / cm 3 ~3.2g / cm 3 or 2.2 g / cm 3 ~2.8g / cm 3 In the range of Solid electrolyte material.

[0160] Embodiment 39. A solid electrolyte material according to any one of Examples 1 to 38, comprising a crystal structure but, Atomically disordered vacancies and Me atoms; Irregular X1 and X2 atoms (X1 and X2 represent two different halogen atoms); Irregular vacancy positions and M atoms; Disordered M and Me atoms; Disordered M, Me and vacancy atoms; or any combination thereof, 1. A solid electrolyte material comprising:

[0161] Embodiment 40: Atomically disordered vacancies and Me atoms are formed in an atomic layer or linear atomic chain. 40. The solid electrolyte material of embodiment 39, wherein the solid electrolyte material is partially disordered.

[0162] Embodiment 41: The solid electrolyte material according to any one of embodiments 1 to 9 and 20. and the atomic disorder is at least 10%, at least 20%, at least 30%, at least 40%, at least 60%, at least 80%, or at least 90% Body electrolyte material.

[0163] Embodiment 42. The crystal structure has crystallographic sites occupied by both Me atoms and vacancies. The solid electrolyte material according to any one of embodiments 1 to 41, comprising:

[0164] Embodiment 43. A solid electrolyte according to embodiment 42, wherein the multiplicity of the crystallographic site is 3. material.

[0165] Embodiment 44. Embodiment 42, in which the crystallographic site is Wycoff position 3a or 3b 44. A solid electrolyte material according to claim 43.

[0166] In the X-ray diffraction pattern measured with CuKα radiation, the diffraction angle is 16° to 25°. The solid electrolyte material according to any one of embodiments 1 to 44, wherein no peak exists between θ. .

[0167] Embodiment 46. Any of embodiments 1 to 45, wherein M contains at least one of Li and Na. 10. The solid electrolyte material according to claim 9,

[0168] Embodiment 47. The solid electrolyte according to any one of embodiments 1 to 46, wherein M comprises Li. material.

[0169] Embodiment 48. Me is an alkaline earth metal element, a 3d transition metal, Mg, Ca, Ba, Z n, Zr, Hf, Ti, Sn, Th, Ge, V, Ta, Nb, Mo, W, Sb, In, B Any one of embodiments 1 to 47, including i, Al, Ga, or any combination thereof. The solid electrolyte material described herein.

[0170] Embodiment 49. The embodiment in which Me comprises a rare earth element, Zr, Sn, or any combination thereof. The solid electrolyte material according to any one of the first to eighteenth embodiments.

[0171] Embodiment 50. Me is Y, Ce, Gd, Er, Zr, La, Yb, In, Mg, Zn , Sn, or any combination thereof. Body electrolyte material.

[0172] Embodiment 51. A solid electrolyte according to any one of embodiments 1 to 50, wherein Me comprises Y. material.

[0173] Embodiment 52. An embodiment in which X comprises F, Cl, Br, I, or any combination thereof. 52. The solid electrolyte material according to any one of embodiments 1 to 51.

[0174] Embodiment 53. Any of embodiments 1 to 52, wherein X comprises Cl, Br, or a combination thereof. 13. The solid electrolyte material according to claim 12,

[0175] Embodiment 54. The solid electrolyte of any one of embodiments 1 to 53, wherein X comprises Br. material.

[0176] Any one of embodiments 1 to 54, consisting of Li, Y, Cl, and Br. The solid electrolyte material according to claim 1,

[0177] Embodiment 56. The crystal structure has at least 20% stacking faults, at least 30%, or less At least 40%, at least 50%, at least 60%, at least 70%, at least 80% %, or at least 90% stacking faults. Solid electrolyte material.

[0178] Embodiment 57. The ionic conductivity is at least 0.001 mS / cm, at least 0.0 1mS / cm, at least 0.1mS / cm, at least 0.4mS / cm, at least 0.8 mS / cm, at least 1.2 mS / cm, at least 1.8 mS / cm, or less 57. The solid electrolyte according to any one of embodiments 1 to 56, wherein the electrical conductivity is at least 2.2 mS / cm. material.

[0179] 58. The ionic conductivity is at most 15 mS / cm, at most 13 mS / cm, at most 11mS / cm, up to 8mS / cm, up to 7.2mS / cm, or up to 6.2m 39. The solid, ionically conductive material of any one of embodiments 1 to 38, wherein the conductivity is .S / cm.

[0180] example Example 1 A representative lithium yttrium bromide sample (Li3YBr6) is used in the embodiments herein. The decomposition of NH4Br was carried out at 400°C to 600°C. The samples were further ground in an automatic agate mortar to obtain finer powder particles. No milling was used. The crystal structure and crystallinity characteristics of the final particles formed are as follows: This is shown in Table 1. [Table 1]

[0181] Example 2 Representative Li3YBr6 samples were formed using the processes described in the embodiments herein. FIG. 9 includes an X-ray diffraction spectrum recorded with CuKα radiation. Curve 910 indicates the X-ray diffraction spectrum of the sample. The X-ray diffraction pattern is shown, with bars indicating the peaks expected for the conventional crystal structure. The sample does not show a peak between 16° and 25° 2θ.

[0182] Example 3 Representative Li3YBr6 samples were formed using the processes described in the embodiments herein. Figure 10 includes a structural model of the sample. The yttrium lithium bromide sample was R-3m. It has the crystal structure shown in FIG.

[0183] Example 4 Representative Li3YBr6 samples were formed using the processes described in the embodiments herein. Figure 11 contains a structural model of the sample. As shown in the figure, the sample is composed of new small C2 / It has a crystal structure described by the m space group.

[0184] Example 5 Representative Li3YCl6 samples were formed using the processes described in the embodiments herein. Figure 12 includes a structural model of the sample. As shown in the figure, the sample is composed of P63 / mcm voids. It has a crystal structure represented by the intermetallic group.

[0185] Example 6 Representative Li3YCl6 samples were formed using the processes described in the embodiments herein. Figure 13 includes a structural model of the sample. As shown in the figure, the sample is a P63 / mmc void. It has a crystal structure represented by the intermetallic group.

[0186] Example 7 Using the processes described in the embodiments herein, lithium yttrium bromide Li3YB The decomposition of NH4Br was carried out at 450°C to 650°C. The chemical properties are shown in Table 2 below. [Table 2]

[0187] Comparing Sample 7-1 with Samples 1-1 to 1-3, the average crystallite size of Sample 7 is larger than that of Sample 1. Increasing the decomposition temperature helps to increase the crystallinity, as shown by the increase in Note that it is possible to

[0188] Example 8 After grinding in an automatic agate mortar, the mixture was subjected to additional energy boiling in a rolling mill at 400 rpm for 2 hours. A typical odor was obtained by the same method as described in Example 1, except that a mill was applied to obtain a superfine powder. The lithium yttrium hydride Li3YBr6 sample was formed. The final formed particle crystals The structural and crystalline properties are presented in Table 3 below. [Table 3]

[0189] Example 9 The method according to the embodiment herein, which includes a liquid acidic reaction in addition to ammonium complexation, Thus, a representative lithium yttrium bromide Li3YBr6 (sample 10-1) was formed. Further investigation was carried out by direct solid-state reaction of LiBr and YBr3 at 450 °C for 24 h. The resulting lithium yttrium bromide Li3YBr6 (sample 10-2) was formed.

[0190] FIG. 14A shows the powder X-ray diffraction pattern of sample 10-1 and the XRD pattern of conventional Li3YBr6. The scans are overlaid for comparison. The folded pattern and the XRD scan of conventional Li3YBr6 are overlaid for comparison. Sample 10-1 is the same as the conventional Li3YBr6 and sample 10-2 in terms of XRD scan. Compared to the overlay, there are no peaks within 16 to 25 degrees (2θCu-K-α). Note that sample 10-1 contains approximately 83% + / - 5% stacking faults, and sample 10 -2 contains approximately 15% + / - 5% stacking faults. Quantification of stacking fault values ​​is described in the embodiments of this specification. As described in the report, the FAULTS software released in 2020 was used It is executed.

[0191] The crystal structure and crystallinity properties of Sample 10-2 are further presented in Table 4 below. [Table 4]

[0192] Example 10 Additional samples were prepared using the synthesis methods described in Table 5 below. The impurity contents of the materials are listed in Table 1. The XRD analysis was precisely analyzed by Rietveld refinement. In combination with the synthesis, characteristic The phases of each impurity were detected by quantitative analysis based on the presence of distinct diffraction peaks. Approximately 22°C) with an AC frequency of 3MHz to 10Hz and a peak-to-peak of 10 to 50mV Electrochemical impedance analysis using a gold blocking electrode under sinusoidal AC voltage signal conditions The ionic conductivity of the samples was determined using an optical technique. The ionic conductivity referred to herein is the Barrier Conductivity. The bulk particle conductivity appears at the highest frequencies, whereas the double layer capacitance The barrier that can be separated from the grain boundaries and electrode contacts is related to the minimum value of resistivity. The conductivity from the bulk particles contributes. [Table 5]

[0193] The synthesis by high energy ball milling was carried out to clarify the synthesis reaction and the molecular structure of the main metal halide complex phase. Note that the decomposition reaction may occur in parallel. Therefore, the high-energy ball mill synthesis is effective to remove the impurities present near the main Li3YX6 phase. The content of simple compounds such as LiX and YX3 can be significantly increased. If the content is high, the crystallinity of the halide-based material may decrease. However, annealing can be performed to partially restore the crystallinity, but annealing Stacking faults in metallic materials may also be significantly reduced.

[0194] In a solid-state reaction at atmospheric pressure of 1 bar, ammonium halide was added to produce oxide (Y Starting from Li2O3 or carbonate materials (Li2CO3), a single phase of Li3YX6 is synthesized. Note also that the rare earth metal (e.g., Y in the Li3YX6 example) is not At least two chemical reactions can occur to convert them to halogen compounds. In the reaction, YX3 is synthesized, which can further react to form the Li3YX6 phase. The second reaction can result in the formation of YOX, which is a stable compound and can be easily converted to Li3 Impurities in the final product of YX6. High levels of rare earth oxynitride in halide-based materials. The formation of a halide phase (i.e., at least 6 wt%) is characteristic of an impurity phase. Quantification of stacking faults based on XRD spectra, which may result in extra XRD peaks may not be reliable.

[0195] Example 11 Additional representative halide-based materials are the same as those described for Sample 10-1 in Example 9. The formulas of each sample are shown in Table 6. The stacking fault content of each sample was determined by the method described in Example 9. Each sample is expected to have 30-85% stacking faults. can be. [Table 6]

[0196] FIG. 15 shows the XRD spectrum of sample 11-6 and the XRD scan of conventional Li3YBr6. The XRD scans of Li3YBr3 and Li3YBr3 are overlaid for comparison. In comparison, the specific peak between 15° and 25° 2θ associated with Cu-Kα radiation was observed in sample 11-6. Note that this is not present in the spectrum of

[0197] Example 12 Powder XRD measurements of sample 10-1 were performed using sealed Kapton capillary tubes in transmission geometry. and a conventional powder sample holder. Figure 16 shows the XRD spectra obtained during the test. Both spectra show the conventional XRD peaks of Li3YBr3. Compared to the bar position, there is no specific peak between 15° and 25° 2θ for CuK-α radiation. Note that this indicates that

[0198] Example 13 Lithium yttrium bromide Li3YBr6 can be prepared by the process described in the embodiments herein. The reaction mixture is heated to 650 °C for 30 min. Heat and hold for 15 minutes for decomposition of NH4Br, then cool to room temperature over 1 hour. Rapid cooling from high temperatures may promote the formation of stacking faults. The abundance is estimated to be about 50%.

[0199] Example 14 Lithium yttrium bromide Li3YBr6 can be prepared by the process described in the embodiments herein. The decomposition of NH4Br was continued for at least 1.5 hours at 350°C before cooling. The temperature range is from 400°C to 440°C. The stacking fault content of the samples is expected to be 10-20%.

[0200] Benefits, other advantages, and solutions to problems have been described above with regard to specific embodiments. while giving rise to benefits, advantages, solutions to problems, and any benefits, advantages, or solutions Any feature or features which may render the invention more pronounced may be recited in any or all of the claims. They should not be construed as critical, necessary, or essential features. When referring to a material that contains more than one ingredient, it means that the material consists essentially of one or more of the ingredients identified. The term "consisting essentially of" may be interpreted to include at least one embodiment that consists of The term includes the specified material and excludes minor inclusions that do not significantly change the properties of the material (e.g., "contains impurities, etc." Alternatively, in certain non-limiting embodiments, the compositions identified herein may be None may be essentially free of material not expressly disclosed. In the embodiment, various amounts of a particular component are included in the material, and the component included in a given material It will be understood that the contents of total 100%.

[0201] The specification and drawings of the embodiments described herein provide a general understanding of the structure of the various embodiments. The present specification and drawings are intended to provide a method and apparatus for producing a semiconductor device using the structures or methods described herein. serve as a comprehensive and comprehensive description of all elements and features of the devices and systems Also, separate embodiments are not intended to be combined into a single embodiment. Conversely, various features that are described in the context of a single embodiment for brevity may be provided. The features may also be provided separately or in any subcombination. A reference to a range of values ​​includes any and all values ​​within that range. Many other embodiments will be apparent to those skilled in the art. Other embodiments may be incorporated into the present disclosure, such as by making logical substitutions, logical substitutions, or other changes. can be used and derived. Accordingly, this disclosure is illustrative rather than limiting. should be considered.

Claims

1. M 3-z (Me k+ ) f X 3-z+k*f (Wherein, −3≦z<3; 2≦k<6, 0≦f≦1; M includes an alkali metal element; Me includes a divalent metal element, a trivalent a tetravalent metal element, a pentavalent metal element, a hexavalent metal element, or any combination thereof and X is a halogen; a crystal structure containing at least 20% stacking faults; 1. A solid electrolyte material comprising:

2. The solid electrolyte material according to claim 1 , wherein the crystal structure is represented by a C2 / m space group.

3. M 3-z (Me k+ ) f X 3-z+k*f (Wherein, −3≦z<3; 2≦k<6, 0≦f≦1; M includes an alkali metal element; Me includes a divalent metal element, a trivalent a tetravalent metal element, a pentavalent metal element, a hexavalent metal element, or any combination thereof and X comprises a halogen; A crystal structure represented by a rhombohedral space group; 1. A solid electrolyte material comprising:

4. The solid electrolyte according to claim 3, comprising a crystalline phase having a crystalline structure represented by the R-3m space group. material.

5. P6 3 / mcm or P6 3 The present invention relates to a crystalline phase having a crystal structure represented by the / mmc space group. The solid electrolyte material according to claim 3.

6. The present invention relates to a method for producing a crystalline phase comprising the steps of:

4. The solid electrolyte material according to claim 3.

7. A solid electrolyte material, M 3-z (Me k+ ) f X 3-z+k*f (Wherein, −3≦z<3; 2≦k<6, 0≦f≦1; M includes an alkali metal element; Me includes a divalent metal element, a trivalent a tetravalent metal element, a pentavalent metal element, a hexavalent metal element, or any combination thereof and X comprises a halogen; Represented by the monoclinic space group with a unit cell containing 3 to 5 halide atoms. A crystal structure having the structure 1. A solid electrolyte material comprising:

8. Any of claims 1, 3 and 7, comprising a crystalline phase having a crystalline structure represented by a C2 / m space group.

3. The solid electrolyte material according to claim 1 .

9. The solid electrolyte material according to any one of claims 1 to 8, comprising a layered atomic arrangement.

10. A represents the value of the unit lattice constant a, B represents the value of the unit lattice constant b, and A=B. Item 7. The solid electrolyte material according to any one of items 3 to 6.

11. The average diffracting crystallite size is at least 20 nm, at least 25 nm, at least 30 nm m, at least 35 nm, or at least 40 nm, or at least 500 nm; The solid electrolyte material according to any one of claims 1 to 10.

12. The X-ray diffraction pattern of the solid electrolyte material measured with CuKα radiation is 16° to 25°. The solid electrolyte material according to any one of claims 1 to 11, which does not include a peak between θ.

13. The compound according to any one of claims 1 to 12, wherein M comprises at least one of Li and Na. Solid electrolyte material.

14. 14. The method of claim 1, wherein Me comprises a rare earth element, Zr, Sn, or any combination thereof. The solid electrolyte material according to any one of claims 1 to 7.

15. According to any one of claims 1 to 14, X comprises Cl, Br, or a combination thereof. Solid electrolyte material.

Citation Information

Patent Citations

  • Solid electrolyte material and battery

    WO2019135316A1

  • Solid electrolyte material, and battery

    WO2019135342A1