Aqueous binder composition for electrodes and method for manufacturing the same
An aqueous binder composition with cationic and anionic polymers improves adhesion in lithium-ion batteries, addressing the low adhesion issues of existing binders and enhancing performance in large electronic devices.
Patent Information
- Application Number
- JP2024135573
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-10-16
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
Existing binders for lithium-ion batteries, such as carbonaceous materials, exhibit low adhesion to active materials, which affects the electrochemical performance and cannot meet the requirements of large electronic devices like electric vehicles and power storage systems.
Development of an aqueous binder composition comprising a cationic copolymer, such as acrylamide copolymers, and an anionic polymer, along with an electrode active material, conductive agent, and dispersant, to form a stable slurry that maintains strong adhesion to current collectors.
The new binder composition enhances the adhesion strength between the electrode active material and current collector, improving the electrochemical performance and stability of lithium-ion batteries, particularly in large electronic devices.
Smart Images

Figure 2024164079000001 
Figure 2024164079000002 
Figure 2024164079000003
Abstract
Description
[Technical field]
[0001] The processes, procedures, methods, manufacture and use of the presently disclosed and / or claimed inventions The present disclosure relates generally to the manufacture, sale, and / or use of battery cells. More specifically, the present invention relates to an aqueous binder composition for use in a liquid crystal display device, and a method for preparing the same. Although not intended to be limiting, the present disclosure relates to a polymerizable composition comprising at least one cationic monomer and at least one and a cationic copolymer derived from the nonionic monomer of The present disclosure further relates generally to an electrode composition including an aqueous binder composition, and The present invention relates to a method for making an electrode, particularly an anode, using the binder composition. [Background technology]
[0002] Lithium-ion batteries (LIBs) are used in medical devices, electric vehicles, airplanes, and most notably are used in a variety of products, including consumer products such as laptops, mobile phones and cameras. Lithium-ion batteries have high energy density, high operating voltage, and low self-discharge. As a result, it has taken the secondary battery market by storm and continues to find new applications in developing industries and products. It is being done.
[0003] Generally, a lithium ion battery comprises an anode, a cathode, and an organic solvent containing a lithium salt. More specifically, either the anode active material or the cathode active material One of the two is mixed with a binder and a solvent to form a paste or slurry, which is then The mixture is coated on a current collector such as aluminum or copper, and dried to form a film on the current collector. Then, the anode and the cathode (collectively, "electrodes") are formed. The electrodes and cathodes are stacked and wound and then placed into a pressurized casing containing an electrolyte material. All of these together form a lithium-ion battery. Summary of the Invention
[0004] To fabricate the electrode, a membrane coated current collector is placed in a pressurized cell casing. Adhesion is sufficient so that contact with the current collector is maintained even when the wire is handled tightly. It is important to select a binder that has the proper properties and chemical characteristics. If the membrane does not maintain sufficient contact with the current collector, the electrochemical properties of the battery may deteriorate. Therefore, the binder is not suitable for the performance of lithium-ion batteries. Styrene butadiene rubber / Carboxymethyl cellulose Existing binders such as cellulose have very low adhesion to active materials. As the use of electronic devices changes from small electronic devices to large electronic devices such as electric vehicles and power storage units, It has high safety, long cycle life, high energy density, and high power. There is a need for better performing anode materials, such as silicon and related materials. Existing binders cannot meet these requirements. Therefore, new aqueous binder compositions need to be developed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0005] Before describing at least one embodiment of the present disclosure in detail, it is important to note that the present disclosure may be used in its application. In accordance with the present invention, the components or elements set forth in the following description or shown in the drawings may be It should be understood that the present invention is not limited to the details of the structure and arrangement of the steps, or to the details of the methodology. The disclosure may be capable of other embodiments or of being practiced or carried out in various ways. Also, the phraseology and terminology used herein is for the purpose of description. It should be understood that these are illustrative and should not be construed as limiting.
[0006] Unless otherwise defined herein, technical terms used in connection with this disclosure will be understood by those of ordinary skill in the art. Further, unless the context otherwise requires, the singular terms includes plural and plural terms include the singular.
[0007] All patents, published patent applications, and non-patent publications mentioned herein are incorporated by reference in their entirety to which this disclosure pertains. Any references made in any part of this application are indicative of the level of skill of one of ordinary skill in the art. All patents, published patent applications, and non-patent publications cited herein are incorporated by reference in their entirety. (c) the same extent as if the disclosure were specifically and individually indicated to be incorporated by reference in its entirety. No. 6,313,635, which are expressly incorporated herein by reference.
[0008] All of the articles and / or methods disclosed herein are intended to be illustrative, not limiting, and are not to be construed as limiting the present disclosure. In accordance with the preferred embodiments, the articles and methods of the present disclosure can be made and carried out without the need for a Although described, no particular limitation or exclusion may be imposed on the articles and / or methods without departing from the concept, spirit and scope of the present disclosure. It is understood that variations can be applied to the methods and to the steps or order of steps of the methods described herein. All such similar substitutes and modifications apparent to those skilled in the art. are deemed to be within the spirit, scope and concept of the present disclosure.
[0009] As utilized in accordance with this disclosure, the following terms have the following meanings, unless otherwise specified: Then it should be understood.
[0010] When used in conjunction with the term "comprising," "a The use of the phrase "(one type)(a)" or "one (one type)(an)" means "one (one type)( It can mean "one (one type) or more," but it can also mean "one or more," "at least one," or "one or more." "at least one" and "one (one type) or more" This does not contradict the meaning of "one or more than one." Use of such terms is expressly intended to refer to alternatives only when the alternatives are mutually exclusive. Unless otherwise noted, "and / or" is used to mean, but the disclosure also includes alternatives and "and" Throughout this application, the term "about" is defined to mean "and / or" only. Inherent variation due to error in the quantitative equipment and methods employed to determine the value of It is used to indicate that the variability that exists between subjects is included. However, when using the term "approximately," the value specified is within the limits of plus or minus 12 percent. cents, 11 percent, 10 percent, 9 percent, 8 percent, 7 percent , 6 percent, 5 percent, 4 percent, 3 percent, 2 percent or 1 percent The use of the term "at least one" may indicate a variation in , 1 (one type), but not limited to, 1, 2, 3, 4, 5, 10, 15, 20, It is understood to include any amount greater than or equal to one, including 30, 40, 50, 100, etc. The term "at least one (one type)" means 100, 10, or 10, depending on the term to which it is attached. 00, or even more. Furthermore, the amount 100 / 1000 can be used as a lower or upper limit. Since satisfactory results can be obtained, it is not considered restrictive. The use of the term "at least one of X, Y, and Z" does not include only X alone, Y alone, and Z alone. It is understood that the term includes any combination of X, Y, and Z, but not all of the terms in the sequence number (i.e. The use of terms such as "first," "second," "third," "fourth," etc. is merely intended to distinguish between two or more items. The purpose of this document is to provide a comprehensive understanding of the principles and, unless otherwise stated, the order, hierarchy or ranking of one item relative to another is not implied. No particular order or importance or additional hierarchy is to be implied.
[0011] As used herein, the term "comprising" (and Any form of "comprise" or "comrising", e.g. "prises" etc.), "having" (and the duties of having "include" and "contain" are used in conjunction with "contains" and "contains" "including" (and any form of "containing", e.g. "containing" "includes" and "include", etc.) or "contains" "(and any form of containing, e.g. "containing" The words "contains" and "contains" are inclusive or open It is open-ended and may contain additional, unrecited elements or method steps. As used herein, the term "or a combination thereof" is intended to include, but is not limited to, the following: refers to all permutations and combinations of the items listed before the term. For example, "A, B , C, or a combination thereof" means A, B, C, AB, AC, BC, or ABC, and If the permutation is important in a given context, then BA, CA, CB, CBA, BCA, ACB, BAC or CAB. Continuing this example, BB, AAA, MB, One or more items or terms such as BBC, AAABCCCC, CBBAAA, CABABB Combinations that include repeats are expressly included. Unless otherwise stated, it is understood that there is typically no limit to the number of items or terms in any combination. do.
[0012] As used herein, the term "copolymer" refers to a polymer that is made up of at least two different monomers. It refers to a polymer formed by the polymerization reaction of monomers.
[0013] As used herein, the term "copolymerization" refers to any of random, graft, block, Generally, the copolymers used in accordance with the present disclosure include all types of copolymers. Any suitable copolymerization method, including liquid copolymerization, slurry copolymerization, gas phase copolymerization, and high pressure copolymerization processes, may be used. It can be prepared according to a catalytic polymerization process.
[0014] As used herein, the terms "aqueous" or "aqueous solvent" refer to water and water and The present invention also includes mixtures containing one or more water-miscible solvents.
[0015] The present disclosure encompasses an aqueous binder composition for the manufacture of lithium ion battery electrodes. In particular, the binder composition includes a cationic copolymer, which is an acrylamide copolymer. Propyltrimethylammonium chloride (APTAC), methacrylamidopropyl trimethylammonium chloride Trimethylammonium chloride (MAPTAC), acryloyloxyethyl trimethyl Ammonium chloride (AETAC), methacryloyloxyethyl trimethylammonium ammonium chloride (MAETAC), N-[2-(acryloyloxy)ethyl]-N-benzo[2-(acryloyloxy)ethyl] Dimethylammonium chloride, acryloyloxyethyltrimethylammonium chloride, and 3-(methacryloylamino)propyl-lauryl-dimethylammonium At least one cationic compound selected from the group consisting of MAPLDMAC Monomers and acrylamide (AM), dimethylacrylamide, diethylacrylamide , Hydroxyethylacrylamide, Dimethylaminopropylacrylamide, Dimethyl Aminopropyl methacrylamide, vinyl acetate (VA), vinyl formamide, acrylic Aronitrile (AN), acrylate, ethylhexyl acrylate, carboxyethyl acrylate Acrylate, Dimethylaminoethyl Methacrylate, and Diethylaminoethyl Methacrylate and at least one nonionic monomer selected from the group consisting of carboxylates. It can be said that.
[0016] The copolymer may have a molecular weight of about 5,000 to about 2,500,000 daltons, or about 8,000 to about 2,000,000, or about 100,000 to about 1,500,000 daltons, or about It has a weight average molecular weight in the range of 300,000 to about 1,000,000 Daltons. can.
[0017] The aqueous binder composition may further comprise at least one anionic polymer. Examples of anionic polymers include, but are not limited to, carboxymethyl cellulose. cellulose; carboxymethyl hydroxyethyl cellulose; carboxymethyl guar Hydroxyalkyl guar, and carboxymethyl hydroxyethyl guar and carboxymethyl Contains carboxyalkyl hydroxypropyl guar such as ethyl hydroxypropyl guar Guar derivatives; Polyacrylic acid; Poly(acrylamido-2-methylpropanesulfonic acid) ); Acrylamide-2-methylpropane and acrylamide, acrylonitrile, acrylonitrile, copolymers derived from acrylic acid or acrylates; alginates; chitosan; carrageenan and 2-acrylamido-2-methyl-1-propanesulfonic acid (AMPS), Derived from acrylic acid, acrylamide, and 3-aroyloxypropylsulfonic acid Mention may be made of tetrapolymers.
[0018] The present disclosure also provides an aqueous slurry comprising an aqueous binder composition, an electrode active material, and a conductive agent. In one non-limiting embodiment, the aqueous slurry composition comprises a dispersant and The aqueous binder composition may further include an aqueous solvent. do.
[0019] The electrode active material can be an anode active material. The anode active material can be a silicon-containing electrode. The active material may be a metal-containing material such as Sn or Ti. In certain embodiments, the silicon-containing material is silicon, silicon-graphene, silicon-carbon nano. The material may be a polysilicon tube, a silicon-based alloy, and combinations thereof.
[0020] The anode active material may also include silicon oxide or carbon-coated silicon oxide. The silicon oxide may be, for example, but is not limited to, a silicon oxide having the formula SiO x (wherein 1≦x<2) Carbon-coated silicon oxide can be represented by the formula SiO x C (wherein 1≦x<2). and the weight ratio of carbon to silicon oxide is at least 50:50, or about 70: 80:10 to about 95:5, or about 90:10 to about 99:1. It can be in the range of 5:5.
[0021] In one non-limiting embodiment, the anode active material comprises a silicon-graphene composition. For example, this disclosure relates to XG Sciences, Inc. (of Michigan) XG-SIG™ silicon-graphene nanocomposite available from Eppendorf (Lansing, MA) was used. In another non-limiting embodiment, the anode active material can be a silicon alloy, such as, for example, Non-limiting examples include silicon titanium nickel alloys (STM) and / or silicon alloys and graphite. More specifically, the anode active material may include a mixture of silicon alloy and fluorite. and graphite, the silicon alloy being about 30-50% by weight, or about 35 to about 45 weight percent, or about 37.5 to about 42.5 weight percent, and about 50 to about 70% by weight, or about 55 to about 65% by weight, or about 57.5 to about 62.5% by weight It is present in the range of % by weight.
[0022] The electrode active material can be a cathode active material. The cathode active material can be a lithium-containing The lithium-containing transition metal oxide may include, consist of, or consist essentially of a lithium-containing transition metal oxide. The cathode active material can be any material comprising a sulphur-containing transition metal oxide. In one non-limiting embodiment, lithium iron phosphate (LiFePO4), lithium cobalt oxide Lithium (LiCoO2), Lithium Nickel Oxide (LiNiO2), Nickel Cobalt Aluminum Lithium cobalt oxide (LiNiCoAlO2), Lithium nickel manganese cobalt oxide (Li NiMnCoO2), lithium manganese oxide (LiMn2O4), and combinations thereof The compound can be selected from the group consisting of:
[0023] In other non-limiting embodiments, the cathode active material can be doped with an element. These include, but are not limited to, boron, magnesium, aluminum, titanium, chromium, etc. Aluminum, iron, zirconium, copper, zinc, gallium, yttrium, fluoride, and combinations thereof In addition, a thin coating material may be applied to the surface of the cathode active material. Coatings such as, but not limited to, ZnO, In2O3, SnO2, Y2O3, La2O3, Li2TiO3, CaTiO3, BaTiO3, SrO, and others Combinations of these may be mentioned.
[0024] The conductive agent includes carbon-based conductive agents, graphite-based conductive agents, metal-based conductive agents, and metal compound-based conductive agents. The agent can be selected from, but is not limited to, the following.
[0025] The carbon-based conductive agent is Super P carbon black (Imerys Graphite & Carbon Switzerland SA), Ketjen Black, Denka Black, Acetylene Black, Carbon Black, Thermal Black Graphite-based conductive agents can be selected from Imerys Gr Commercially available from aphite & Carbon Switzerland SA Can be made with TIMREX® graphite grades such as KS6 or KS15 Carbon nanotubes (CNTs) are a type of material made by Cnano Technology Limited. LB 100 or LB 200 available from Ited (San Jose, Calif.) The metal or metal compound conductive agent may be tin, tin oxide, or phosphorus. The amount of conductive agent in the coating layer can be selected from the slurry composition. In the range of 0.1 to 20% by weight, or in the range of 0.5 to 10% by weight, based on the total weight of the product can be in the range of 1 to 5% by weight.
[0026] The dispersant is a polyacrylate resin; polyethylene oxide; (EO) l (PO) m ( EO) l (wherein EO represents ethylene oxide, PO represents propylene oxide, and and m is in the range of 1 to 500; polyvinyl chloride (PVC) ;Polyvinylpyrrolidone (PVP);Polyacrylic acid (PAA);Acrylonitrile / Br Tadiene / styrene (ABS) polymer; acrylonitrile / styrene / acrylate (ASA) polymers; ABS polymers and propylene carbonate blends; styrene / Acrylonitrile (SAN) copolymer; or methyl methacrylate / acrylonitrile The amount of dispersant can be selected from the group consisting of polybutadiene / butadiene / styrene (MABS) polymers. The range of the dispersant is 0.1 to 20% by weight. In the presence of the dispersant, the conductive agent is uniformly dispersed. It can be distributed among multiple companies.
[0027] The aqueous solvent can be water and / or an aqueous solvent. The solvent is completely dissolved in water. The slurries of the present disclosure have good stability, and the slurries can be used for at least 24 hours or The solution may remain visibly in solution for at least 3 days, or at least 5 days. In an embodiment, the aqueous slurry composition is mixed at 25° C. for about 1 s. -1 ~About 40 seconds -1 In the range of Brookfield shear rates range from about 1,000 mPa·s to about 15,000 mPa·s. or Brook viscosity in the range of about 4,000 mPa·s to about 11,000 mPa·s Field viscosity, or Brookfield viscosity in the range of about 5,500 mPa·s to about 8,500 mPa·s It has a Kfield viscosity.
[0028] The present disclosure includes or consists of an aqueous slurry composition as described above. The electrode comprises an electrode material that consists essentially of the aqueous slurry composition, and a current collector. The electrolyte composition is coated on the surface of the current collector to form a film. about 99% by weight, about 80% by weight, or about 85% by weight to about 95% by weight in the film. and the conductive carbon is present in an amount of from about 0.5 to about 15 weight percent, or from about 2.5 to about 10 weight percent, or from about 1 to about 4 weight percent, and the binder composition is present in the range of about 0.5 to about 15 weight percent, or about It is present in the film in the range of 2.5 to about 10% by weight, or about 4 to about 11% by weight.
[0029] The current collector may be any material that functions as an electrical conductor for either the anode or cathode active material. The current collector can include materials such as aluminum, carbon, copper, stainless steel, nickel, , zinc, silver, and combinations thereof. In one non-limiting embodiment, the current collector for the anode comprises copper foil. In the present embodiment, the cathode current collector includes aluminum foil.
[0030] The present disclosure further provides a method for producing an electrochemical battery comprising: (1) an aqueous binder composition, an electrode active material, a conductive agent, and an optional component. (2) combining the powder with an aqueous solvent to form an aqueous slurry composition; The slurry composition is applied to a current collector to form a coated current collector including a slurry layer on the current collector. (3) drying the slurry layer on the coated current collector to form a current collector. and forming a film on the current collector, the film and the current collector forming an electrode. The present invention includes a method for producing an electrode for use in a liquid crystal display device, an aqueous binder composition, an electrode active material, a conductive agent, a dispersant, and The aqueous solvent is the same as that described above.
[0031] In one non-limiting embodiment, the step (3) of drying the slurry on the current collector is The current collector with the ring is heated to a temperature of about 80 to about 175°C or about 100 to about 150°C. This includes heating for a period of time ranging from 0.5 hours to about 3 hours, or from about 1 hour to about 2 hours.
[0032] The dry film of the electrode is about 20 μm to about 150 μm, or about 30 μm to about 100 μm, or about It has a thickness in the range of 30 μm to 70 μm.
[0033] The film can be bonded to the surface of the current collector to form a bond. The adhesion strength in this case is at least 0.5 as measured by the 90 degree peel adhesion test described below. gf / mm, or at least 0.7 gf / mm, or at least 1.0 gf / mm . EXAMPLES
[0034] <Derived from acrylamidomethylpropanesulfonic acid-acrylamide (AMPS-AM) Preparation of copolymers that Reflex condenser and mechanical stirrer Polymerizations were carried out in a 1 L, four-neck glass reactor equipped with a nitrogen inlet gas port. 0.2 g of AMPS sodium salt solution (15 mol%) and 120 g of AM (85 mol%) The mixture was mixed with 350 g of DI water under nitrogen to form a mixture. This mixture was added to the reactor. The mixture was sparged with nitrogen for about 15 minutes. 0.2% by weight of V, based on the total weight of the monomers, was added. Azo-50 was dissolved in water / ethanol (1:1 weight ratio) to prepare Vazo-50 solution. The reactor was heated to about 55-60°C. The Vazo-50 solution was added to initiate the polymerization. The incubation period lasted about 6 hours. Vazo-50 solution was added at 1 hour, 2 hours, 3 hours, 4 hours and 6 hours. The temperature was maintained at about 50-55°C for 6 hours. Then, the temperature of the reactor is raised to about 65-70°C and the resulting viscous material is stirred for about 10-16 hours. Finally, the reactor was emptied and heated at about 65° C. for about 5 to 7 h under a vacuum of 3 to 5 mm Hg. The solid obtained was used as an anionic polymer (AMPS-AM) described later. It was ground into powder for use.
[0035] <Preparation of silicon slurry for viscosity test and adhesion test> A slurry was prepared using the ingredients listed in Table 1. Anode active materials listed in Table 1 Regarding 650mAh / g SiO, BTR Energy Materials A powder mixture of graphite and silicon oxide, commercially available from Shenzhen Graphite Co., Ltd., China. 680mAh / g SiO is the equivalent of graphite (BTR Energy (commercially available from Materials Co., LTD.) and SiO x (Osaka Titanium Co., Ltd. (commercially available from Mu Technologies, Amagasaki, Hyogo, Japan) at 75:25 At a weight ratio of (graphite to silicon oxide), it has an initial capacity of about 350 mAh / g. Conductive carbon C-NERGY(TM) Super C65 (Imerys Gr (commercially available from Aphite & Carbon, Bodio, Switzerland) are listed in Table 1. The listed conductive agents were used. The content of each component is given based on the total weight of the slurry. .
[0036] [Table 1]
[0037] N-Hance™ SP100: Acrylamidopropyltrimonium chloride / Acrylamide copolymer, commercially available from Ashland LLC N-DurHance™ AA200: (3-acrylamidopropyl) trimethyl Highly charged homopolymer of ammonium chloride, commercially available from Ashland LLC Prasetol™ 644BC: Acrylamidopropyltrimonium chloride / Acrylamide copolymer, commercially available from Solenis LLC Prasetol™ 611BC: Acrylamidopropyltrimonium chloride / Acrylamide copolymer, commercially available from Solenis LLC Prasetol™ 610BC: Acrylamidopropyltrimonium chloride / Acrylamide copolymer, commercially available from Solenis LLC Prasetol™ 852BC: Acrylamidopropyltrimonium chloride / Acrylamide copolymer, commercially available from Solenis LLC N-Hance™ 4572: Guar and Guar Derivatives, Ashland LLC Available from N-Hance™ 3215: Guar hydroxypropyltrimonium chloride, Available from Ashland LLC XxtraDura(TM) FLA 3766: Fluid Loss Additive, Ashland L Commercially available from LC CMC 7LF: Aqualon™ sodium carboxymethylcellulose, A Available from shland LLC CMC 7HO: Blanose™ sodium carboxymethylcellulose, A Available from shland LLC CMC MAC 350: Sunrose® carboxymethylcellulose, Available from Nippon Paper Group Inc. (Japan) * Includes 1.3% by weight of Zeon® BM-480B: styrene butadiene Enlatex, commercially available from Zeon Corporation (Tokyo, Japan)
[0038] <Slurry rheology measurement> The viscosities of the slurry compositions listed in Table 1 were determined by Brookfield Engineers Manufactured by ing Laboratories, Inc. (Middleboro, Massachusetts) Using a Brookfield® viscometer, spindle 4 The measurements were performed at 3 rpm and 30 rpm using a 17 mL vial immediately after mixing and 3 days after mixing. The viscosity was measured directly in the bottle. The results are listed in Table 2. The stability of the slurry is also listed in Table 2. As shown in.
[0039] [Table 2]
[0040] <Adhesion measurement> The slurry composition was coated on a copper current collector and dried to form an electrode. The adhesion was measured by a peel test. The 90 degree peel test was performed using a peel test fixture manufactured by Norwood, Pennsylvania. The pole is 2.5 to 3.5 mg / cm 2 Load and 4.0-5.0mg / cm 2 Tested with a load of Individual electrode samples were obtained from 3M Corporation (St. Paul, Minnesota). After attaching it to a stainless steel plate using 3M (registered trademark) double-sided Scotch tape, The membrane attached to the tape was then spun at a speed of 1 ft / min using an Instron® instrument. Peeling and the force required to peel the film from the current collector with the Instron® instrument The results are listed in Table 3.
[0041] [Table 3]
Claims
1. Acrylamidopropyltrimethylammonium chloride (APTAC), Methacrylic Amidopropyltrimethylammonium chloride (MAPTAC), acryloyloxy Ethyltrimethylammonium chloride (AETAC), methacryloyloxyethyl Trimethylammonium chloride (MAETAC), N-[2-(acryloyloxy)ethyl ethyl]-N-benzyldimethylammonium chloride, acryloyloxyethyl trime ethyl ammonium chloride, and 3-(methacryloylamino)propyl-lauryl-di At least one selected from the group consisting of methyl ammonium chloride (MAPLDMAC) One cationic monomer and acrylamide (AM), dimethylacrylamide, diene ethyl acrylamide, hydroxyethyl acrylamide, dimethylaminopropyl acrylamide amide, dimethylaminopropyl methacrylamide, vinyl acetate (VA), vinyl formate amide, acrylonitrile (AN), acrylate, ethylhexyl acrylate, carboxyethyl acrylate, dimethylaminoethyl methacrylate, and diethylaminoethyl At least one nonionic monomer selected from the group consisting of ethyl methacrylate and an aqueous binder for an electrode of a lithium ion battery, comprising a cationic copolymer derived from - Composition.
2. Carboxymethylcellulose; Guar derivatives; Polyacrylic acid; Poly(acrylamide -2-methylpropanesulfonic acid); acrylamido-2-methylpropanesulfonic acid and Copolyesters derived from acrylic acid, acrylamide, acrylonitrile, acrylic acid or acrylate alginate; chitosan; carrageenan; and acrylamidomethylpropylsulfur acrylate (AMPS), acrylic acid, acrylamide, and 3-allyloxy-2-hydroxybutyric acid. and tetrapolymers derived from hydroxypropylsulfonic acid. The aqueous binder composition of claim 1 further comprising an ionic polymer.
3. The cationic copolymer has a molecular weight ranging from about 5,000 to about 1,000,000 Daltons. The aqueous binder composition of claim 1 having a weight average molecular weight of
4. The aqueous binder composition according to claim 1 ; An electrode active material; A conductive agent; A dispersant; An aqueous solvent; 1. An aqueous slurry composition comprising:
5. 5. The aqueous slurry composition of claim 4, wherein the electrode is an anode.
6. The electrode active material is one or more chemical elements selected from the group consisting of Si, Sn, and Ti. The aqueous slurry composition of claim 4 comprising:
7. The Si-containing electrode active material is SiO x / Graphite, SiC, SiO x , SiO x C , Si-graphene, Si-based alloys, and combinations thereof; The aqueous slurry composition of claim 6.
8. The conductive agent is a carbon-based conductive agent, a graphite-based conductive agent, a metal-based conductive agent, or a metal compound-based conductive agent.
5. The aqueous slurry composition of claim 4, wherein the conductive agent is selected from the group consisting of:
9. The aqueous binder composition is based on the total weight of the aqueous slurry composition on a dry weight basis.
5. The aqueous slurry composition of claim 4, wherein the aqueous slurry composition is present in the range of about 0.25 to about 12 weight percent.
10. The aqueous slurry composition is mixed for about 1 to about 40 s. -1 At shear rates in the range of about 1 4. The composition of claim 1, further comprising a Brookfield viscosity in the range of about 1,000 to about 15,000 mPa·s.
5. The aqueous slurry composition according to claim 4.
11. The aqueous slurry composition according to claim 5 ; A current collector; 1. An electrode for a lithium ion battery comprising:
12. The aqueous slurry composition is coated on the current collector to form a film.
12. The electrode of claim 11.
13. The current collector is selected from the group consisting of aluminum, copper, and combinations thereof. The electrode of claim 11 comprising a metal.
14. The electrode of claim 12, wherein the membrane has a thickness in the range of about 10 μm to about 150 μm. 。
15. 12. The electrode of claim 11 which is an anode.
16. The surface of the film and the surface of the current collector have at least about The electrodes according to claim 11, which are adhered to each other with an adhesion strength of 0.3 gf / mm.
17. A lithium ion battery comprising an anode, a cathode, and an electrolyte, 12. A lithium ion battery, wherein the anode is the electrode of claim 11.
18. A method for producing an electrode for a lithium ion battery, comprising the steps of: The aqueous binder composition according to claim 1, an electrode active material, a conductive agent, a dispersant, and an aqueous and a solvent to form an aqueous slurry composition; The aqueous slurry composition is applied to a current collector to form a coating including a slurry layer on the current collector. forming a current collector with a ring; Drying the slurry layer on the coated current collector to form a film on the current collector. The process and Including, The method, wherein the membrane and the current collector constitute the electrode.
19. Based on the total weight of the aqueous slurry composition, the aqueous binder composition is in the aqueous slurry composition in the range of about 0.25 to about 12 weight percent of the electrode active material, The material is present in the aqueous slurry composition in a range of about 80% to about 99.5% on a dry weight basis. The method according to claim 17 .
Citation Information
Cited By
Aqueous binder composition, aqueous slurry composition, electrode, and method for manufacturing an electrode.
JP2026150178A