Solder resist composition, dry film, printed wiring board, and methods for manufacturing the same

A solder resist composition with specific resin and filler combinations addresses reflectance and durability issues in white solder resist layers, ensuring high reflectance and crack resistance, even under harsh conditions, by using a carboxyl group-containing resin, inorganic filler, and mercapto-modified acrylate in dry film and printed wiring boards.

JP2024164127AActive Publication Date: 2024-11-26TAIYO INK MFG CO KOREALTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024139677
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-12-16
Filing Date
2024-08-21
Publication Date
2024-11-26
Estimated Expiration
2041-12-14

AI Technical Summary

Technical Problem

Conventional solder resist layers, particularly white ones, face issues with high reflectance leading to light reflection, halation phenomena, poor HAST resistance, and rapid decrease in reflectance due to copper electrode corrosion, along with challenges in maintaining high reflectance and crack resistance under harsh conditions.

Method used

A solder resist composition comprising a carboxyl group-containing resin without aromatic rings, an inorganic filler, mercapto-modified acrylate, and a resin with aromatic rings, along with optional components like a thermosetting resin, silane coupling agent, and resin with urethane bonds, is used to form a dry film and printed wiring board, enhancing reflectance, crack resistance, and durability.

Benefits of technology

The composition achieves high reflectance, excellent yellowing resistance, and crack resistance, maintaining reflectance after high-temperature reflow and UV treatment, with improved HAST resistance and gloss, resulting in a solder resist layer with enhanced durability and resolution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164127000001_ABST
    Figure 2024164127000001_ABST
Patent Text Reader

Abstract

To provide a solder resist composition, and more specifically, a solder resist composition that achieves high reflectance, excellent yellowing resistance, excellent crack resistance, high resolution and flatness, excellent sensitivity, developability, adhesion, solder heat resistance, pencil hardness, solvent resistance, HAST resistance, and high reflectance and high gloss after a HAST test.SOLUTION: A solder resist composition comprises (A) a carboxyl group-containing resin not containing an aromatic ring, (B) an inorganic filler, (C) a mercapto-modified acrylate and (D) a resin containing an aromatic ring.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solder resist composition, and more particularly to a solder resist composition having high reflectance, excellent yellowing resistance, excellent crack resistance, high resolution and flatness, excellent sensitivity, developability, adhesion, solder heat resistance, pencil hardness, solvent resistance, HAST resistance, and high reflectance and high gloss even after a HAST test; a solder resist layer obtained from the solder resist composition; a dry film and a printed wiring board each including the solder resist composition; and methods for producing the solder resist composition and the solder resist composition. [Background technology]

[0002] In general, in printed wiring boards used in electronic devices, etc., when mounting electronic components on the printed wiring board, a solder resist layer is formed in the area excluding the connection holes on the board on which the circuit pattern is formed in order to prevent solder from adhering to unnecessary areas and to prevent the circuit conductors from being exposed and corroding due to oxidation or humidity.

[0003] In recent years, electronic devices have become lighter, thinner, shorter, and smaller, which has led to higher precision and higher density of printed wiring boards. As a result, solder resist layers are now mainly formed using a so-called photosolder resist, in which a photosensitive resin ink is applied to a board, a pattern is formed by exposure and development, and the patterned resin is then fully cured by heating or light irradiation.

[0004] The liquid photosensitive resin ink as described above has a problem in that the printing and ink drying steps must be repeated during production, resulting in a long working time.

[0005] Therefore, it has been proposed to form a solder resist layer using a so-called photosensitive dry film instead of a liquid photosensitive resin ink, which can omit the drying process after ink application. When a dry film is used for lamination, the working time is shortened, so the manufacturing process is greatly shortened and the productivity is also excellent.

[0006] Such a dry film generally includes a laminate in which a solder resist layer, which is a photosensitive resin layer, is formed on a base film, and a protective film is attached to the layer. When used, the protective film is peeled off, the substrate is heated and pressed, and the substrate is exposed to light, and then the support film is peeled off and developed to form a patterned solder resist layer. When a solder resist layer is formed using a dry film, not only can the ink drying process be omitted compared to the case of using a liquid photosensitive resin ink as described above, but air bubbles are less likely to be mixed between the substrate and the solder resist layer because the dry film is pressed onto the circuit substrate, and the filling of recesses on the substrate surface is also improved. In addition, when a solder resist layer is formed using a dry film, the film has excellent flatness, chips can be efficiently mounted, and high resolution is obtained.

[0007] However, since white solder resist layers have a higher reflectivity than colored solder resist layers, when a solder resist layer is formed using a dry film as described above, there is a problem that light is reflected from the surface of the solder resist layer during exposure, making it difficult for the light to penetrate to the bottom, resulting in a phenomenon called halation in which the top becomes larger at the surface, making it difficult to realize a pattern. Furthermore, white solder resist layers have poor HAST resistance after HAST testing, and there is a problem that the reflectivity drops sharply due to corrosion of the copper electrodes.

[0008] Since the solder resist layer also functions as a permanent protective film for the circuit board, the solder resist composition is required to have various properties such as alkaline developability, solder heat resistance, etc. In addition, the solder resist layer formed from the solder resist composition is also required to have crack resistance, developability, adhesion, solder heat resistance, solvent resistance, etc.

[0009] Furthermore, since the white solder resist layer also functions as a backlight for the display, it is very important to realize a high reflectance. Also, when the white solder resist layer is exposed to harsh environments such as heat, UV, blue light, and HAST, it is very important that the white solder resist layer has a high reflectance, the reflectance does not decrease much during the manufacturing process, and the cured product does not turn yellow even when exposed to heat or light, and maintains a high reflectance. Also, when evaluating the reliability of the white solder resist layer, it is necessary to have characteristics such as high HAST resistance and high reflectance even after the HAST test.

[0010] Patent Document 1 discloses an invention for providing a photosensitive resin composition having a high dielectric constant and excellent resolution, the photosensitive resin composition containing a carboxyl group-containing resin, a photopolymerization initiator, and at least two types of perovskite type compounds, one of which is barium titanate.

[0011] Patent Document 2 is an invention for providing a photosensitive element having a photosensitive layer excellent in resolution and heat resistance, and discloses a photosensitive element having a photosensitive layer, a support, a support film, and a non-photosensitive resin layer, which contains component (A): a resin having a phenolic hydroxyl group, component (B): a photosensitive acid generator, and component (C): at least one compound selected from the group consisting of aliphatic cyclic compounds, aliphatic compounds, and compounds in which a portion of the carbon constituents of these compounds is substituted with a heteroatom, the compound having two or more of at least one selected from the group consisting of methylol groups and alkoxyalkyl groups.

[0012] However, there is a demand for a composition that satisfies not only the basic properties required for a solder resist layer, but also the additional properties required for a white solder resist layer. For example, there is a demand for a solder resist composition that has a higher reflectance than conventional ones, excellent crack resistance, excellent yellowing resistance, and the like, and has excellent HAST resistance and retains a high reflectance even after a HAST test. In particular, there is a demand for a method for producing a dry film and a printed wiring board including a solder resist layer that can solve the specific problems that arise in the process of producing a white solder resist layer. Summary of the Invention [Problem to be solved by the invention]

[0013] An object of the present invention is to provide a solder resist composition which has improved surface hardening and high reflectance, less reduction in reflectance during the manufacturing process, excellent yellowing resistance, excellent crack resistance, and high resolution and flatness compared to conventional solder resist layers, a solder resist layer obtained therefrom, a dry film and a printed wiring board each including the same, and methods for manufacturing the same.

[0014] The object of the present invention is to provide a method for manufacturing a printed wiring board that solves the problem of halation that occurs when manufacturing a printed wiring board including a white solder resist layer, maintains high reflectance when exposed to UV and heat, and has excellent resistance and reflectance even after HAST testing. [Means for solving the problem]

[0015] The present inventors have found that the above problems can be solved by the following solder resist composition, dry film, printed wiring board, and methods for producing the same.

[0016] <1> A solder resist composition comprising: (A) a carboxyl group-containing resin that does not contain an aromatic ring; (B) an inorganic filler; (C) a mercapto-modified acrylate; and (D) a resin that contains an aromatic ring.

[0017] <2> The above <1> The solder resist composition according to claim 1, wherein the solder resist composition is white in color.

[0018] <3> The above <1> The solder resist composition according to claim 1, further comprising a thermosetting resin.

[0019] <4> The above <3> 2. The solder resist composition according to claim 1, wherein the thermosetting resin is an epoxy resin.

[0020] <5> The above <3> In the solder resist composition of claim 1, an equivalent ratio (epoxy group / carboxyl group equivalent ratio) obtained by dividing the equivalent of the epoxy group contained in the epoxy resin by the equivalent of the carboxyl group contained in the carboxyl group-containing resin is 0.5 or more and 1.2 or less.

[0021] <6> The above <1> or <5> The solder resist composition according to claim 1, wherein the content of the mercapto-modified acrylate (C) is 2% by mass to 6% by mass based on the total mass of the composition.

[0022] <7> The above <1> The solder resist composition according to claim 1, wherein the (C) mercapto-modified acrylate is an aliphatic compound having 1 to 15 carbon atoms and substituted with one or more functional groups selected from the group consisting of an acryloyl group, an acryloyloxy group, and an acryloyloxyalkyl group.

[0023] <8> The above <1> A dry film having a solder resist layer formed by applying any one of the solder resist compositions above onto a substrate film and drying the applied composition.

[0024] <9> The above <8> A cured product obtained by curing the solder resist layer of the dry film.

[0025] <10> The above <9> A printed wiring board comprising the cured product.

[0026] <11> A method for producing a dry film, comprising the steps of:

[0027] 1) On a substrate film <1> applying any one of the solder resist compositions of the above;

[0028] 2) drying the applied solder resist composition to form a solder resist layer; and

[0029] 3) The dried solder resist layer is laminated with a protective film.

[0030] <12> A method for manufacturing a printed wiring board, comprising the steps of:

[0031] 1) The solder resist layer is laminated on the substrate. <8> and vacuum laminating the dry film;

[0032] 2) peeling off the base film of the dry film and then exposing the solder resist layer;

[0033] 3) developing the solder resist layer to remove unexposed areas to form a pattern; and

[0034] 4) curing the patterned substrate. Effect of the Invention

[0035] The solder resist composition of the present invention can provide a solder resist layer having excellent sensitivity, developability, adhesion, solder heat resistance and solvent resistance, high reflectance, little decrease in reflectance even after high temperature reflow and UV treatment after final curing, little decrease in reflectance even after 3000 hours of irradiation with blue light, excellent HAST resistance, high reflectance after HAST test, excellent yellowing resistance and crack resistance, excellent flatness and gloss, and high resolution, as well as a dry film and a printed wiring board including the same.

[0036] The dry film including the solder resist layer obtained from the solder resist composition of the present invention can have a high reflectance of 92 to 93% or more, and the reflectance is less decreased compared to normal ink, especially white ink, even after high-temperature reflow and UV treatment after final curing. In addition, the reflectance is less decreased compared to normal ink, especially white ink, and other solder resist layers, even after 3000 hours of irradiation with blue light. Furthermore, the dry film has excellent crack resistance and gloss.

[0037] A printed wiring board including a solder resist layer manufactured by the manufacturing method according to the present invention has high resolution. [Brief description of the drawings]

[0038] [Figure 1] FIG. 1 is a diagram comparing a printed wiring board that was exposed by peeling off the base film before UV exposure and a printed wiring board that was exposed without peeling off the base film before UV exposure.

[0039] [Diagram 2] FIG. 2 is a diagram showing the results of the Erichsen test for Examples 1 to 6 and Comparative Examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0040] Hereinafter, embodiments of the present invention will be described in detail.

[0041] Solder resist composition

[0042] The solder resist composition (hereinafter also referred to as "resin composition") of the present invention is a photosensitive resin composition. The resin composition contains (A) a carboxyl group-containing resin that does not contain an aromatic ring, (B) an inorganic filler, (C) a mercapto-modified acrylate, and (D) a resin that contains an aromatic ring. The resin composition may also contain (E) a silane coupling agent, (F) a resin having a urethane bond, and any other necessary components.

[0043] The solder resist composition of the present invention, by virtue of the combination of the above components (A) to (D), has high reflectance, is subject to little decrease in reflectance during the production process, and has excellent yellowing resistance, excellent crack resistance, excellent sensitivity, developability, adhesion, solder heat resistance, pencil hardness, solvent resistance, HAST resistance, and can maintain high reflectance and high gloss even after a HAST test.

[0044] The solder resist composition of the present invention further contains the above-mentioned (E) in addition to the combination of the above-mentioned (A) to (D), thereby further enhancing the crack resistance, improving the reflectance, and providing more excellent gloss.

[0045] The solder resist composition of the present invention further contains the above-mentioned (F) in addition to the combination of the above-mentioned (A) to (D), thereby increasing flexibility and providing even better resistance to external impacts and cracks when bent, as well as better crack resistance.

[0046] The solder resist composition of the present invention may be white.

[0047] The white color was produced by laminating a solder resist onto an FR-4 board and exposing it to light at 300 mJ / cm using a SCREEN LEDIA 5 DI exposure tool. 2 The UV exposure was performed with 1% Na 2 CO 3 A 55μm solder resist coating was produced by developing for 1 minute in a solution (developing solution temperature: 30°C) and final curing for 1 hour at 150°C in a box oven, and after passing once under reflow conditions at 260°C for 10 seconds, the L, a, and b values ​​of the coating surface on the board were measured using a spectrophotometer (CM-2600d, Konica Minolta Sensing, Inc.), and the color when the measurement results show that the L value of the spectrophotometer is 70 or more, the a value is -5 or more, and the b value is -5 or more. In this case, L, a, and b do not change depending on the lamination conditions.

[0048] (A) Carboxyl group-containing resin not containing an aromatic ring

[0049] In the solder resist composition of the present invention, the (A) carboxyl group-containing resin not containing an aromatic ring (hereinafter referred to as "resin (A)") may be any resin that is cured by irradiation with active energy rays and exhibits electrical insulation properties, and in particular, in the present invention, a compound not containing a benzene ring is preferably used.

[0050] Resin (A) contains unsaturated double bonds, allowing for radical curing with ultraviolet light, electron beams, or heat, and contains carboxyl groups, allowing for alkaline development. Resin (A) is a carboxyl group-containing aliphatic resin that does not contain aromatic rings, and therefore has excellent resistance to discoloration and yellowing when exposed to heat or UV energy. In addition, the combination of resin (A) and inorganic filler (B) allows for high reflectance, with little loss in reflectance after the reflow process and little loss in reflectance after a 3,000-hour blue light test. Thus, resin (A) has less loss in reflectance due to discoloration and yellowing than other inks, and has excellent resistance to yellowing.

[0051] As the carboxyl group-containing resin (A) that does not contain aromatic ring, any of the photosensitive carboxyl group-containing resins that have one or more photosensitive unsaturated double bonds and the carboxyl group-containing resins that do not have photosensitive unsaturated double bonds can be used, and are not limited to specific ones. In particular, the following resins that do not have aromatic rings (either oligomers or polymers) are preferably used. (1) A carboxyl group-containing resin obtained by copolymerization of an unsaturated carboxylic acid and a compound having an unsaturated double bond; (2) A photosensitive carboxyl group-containing resin obtained by reacting a carboxyl group-containing (meth)acrylic copolymer resin with a compound having an oxirane ring and an ethylenically unsaturated group in one molecule; (3) A photosensitive carboxyl group-containing resin obtained by reacting a copolymer of an unsaturated monocarboxylic acid, a compound having one epoxy group and an unsaturated double bond in one molecule, with a compound having an unsaturated double bond, and then reacting the resulting secondary hydroxyl group-saturated or unsaturated polybasic acid anhydride; and (4) A photosensitive hydroxyl group- and carboxyl group-containing resin obtained by reacting a hydroxyl group-containing polymer with a saturated or unsaturated polybasic acid anhydride, and then reacting the resulting carboxylic acid with a compound having one epoxy group and an unsaturated double bond in one molecule.

[0052] Among these, (a) a carboxyl group-containing (meth)acrylic copolymer resin, which is a photosensitive carboxyl group-containing resin as described above in (2), and (b) a copolymer resin having a carboxyl group obtained by reacting a compound having an oxirane ring and an ethylenically unsaturated group in one molecule are preferred.

[0053] (a) The carboxyl group-containing (meth)acrylic copolymer resin can be obtained by copolymerizing a (meth)acrylic acid ester and a compound having one unsaturated group and at least one carboxyl group in one molecule. Examples of the (meth)acrylic acid ester constituting the copolymer resin (a) include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, and hexyl (meth)acrylate, hydroxyl group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and caprolactone-modified 2-hydroxyethyl (meth)acrylate, and glycol-modified (meth)acrylates such as methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, isooctyloxyethylene glycol (meth)acrylate, phenoxytriethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, and methoxypolyethylene glycol (meth)acrylate. These may be used alone or in a mixture of two or more. In this specification, (meth)acrylate is a term that collectively refers to acrylate and methacrylate, and the same applies to other similar expressions.

[0054] Examples of compounds having one unsaturated group and at least one carboxyl group in one molecule include acrylic acid, methacrylic acid, modified unsaturated monocarboxylic acids in which a chain extends between the unsaturated group and the carboxylic acid, such as β-carboxyethyl (meth)acrylate, 2-acryloyloxyethyl succinic acid, 2-acryloyloxyethyl hexahydrophthalic acid, unsaturated monocarboxylic acids having an ester bond due to lactone modification, modified unsaturated monocarboxylic acids having an ether bond, and those containing two or more carboxyl groups in the molecule, such as maleic acid. These may be used alone or in a mixture of two or more.

[0055] (b) The compound having an oxirane ring and an ethylenically unsaturated group in one molecule may be any compound having an ethylenically unsaturated group and an oxirane ring in one molecule, such as glycidyl (meth)acrylate, α-methylglycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxycyclohexylethyl (meth)acrylate, 3,4-epoxycyclohexylbutyl (meth)acrylate, and 3,4-epoxycyclohexylmethylaminoacrylate. In particular, 3,4-epoxycyclohexylmethyl (meth)acrylate is preferred. Such (b) compounds having an oxirane ring and an ethylenically unsaturated group in one molecule may be used alone or in combination of two or more.

[0056] The carboxyl group-containing resin (A) having no aromatic ring must have an acid value in the range of 30 to 200 mgKOH / g. If the acid value is less than 30 mgKOH / g, it is difficult to remove the unexposed portion of the solder resist composition coating film with a weak alkaline aqueous solution. If the acid value exceeds 200 mgKOH / g, problems such as a decrease in the water resistance and electrical properties of the cured film occur. In addition, the weight-average molecular weight of the carboxyl group-containing resin (A) having no aromatic ring is preferably in the range of 5,000 to 100,000. If the weight-average molecular weight is less than 5,000, the touch dryness of the solder resist composition coating film tends to decrease significantly. In addition, if the weight-average molecular weight exceeds 100,000, problems such as a significant deterioration in the developability and storage stability of the solder resist composition occur, which is not preferable.

[0057] The amount of resin (A) in the solder resist composition of the present invention is in the range of 5 to 25% by mass, preferably 10 to 20% by mass, and more preferably 12 to 19% by mass, based on the total mass of the resin composition. The resin composition contains a solid component and a solvent.

[0058] When the content of resin (A) is within the above range, it is possible to realize excellent yellowing resistance and high reflectance. When the content of resin (A) is below the above range, the solder resist coating film is not formed well, and there is a possibility that there are problems with pencil hardness, adhesion, etc. When the content of resin (A) is above the above range, the touch dryness of the coating film decreases and undercut becomes worse.

[0059] (B) Inorganic filler

[0060] The solder resist composition of the present invention can achieve high reflectance by containing an inorganic filler.

[0061] Examples of inorganic fillers include titanium oxide, zinc oxide, basic carbonates, basic sulfates, sulfates, zinc sulfide, antimony oxide, aluminum hydroxide, silica, and barium sulfate. For example, when a composition is embodied by mixing barium sulfate and silica as an inorganic filler, the L value is 80 or more, the a value is -5 or more, and the b value is -5 or more. Preferably, when a composition is embodied by using a high content of titanium oxide and silica as an inorganic filler, the L value is 90 or more, the a value is -3 or more, and the b value is -3 or more, and the whiteness and reflectance are high. More preferably, when a composition is embodied by using titanium oxide as an inorganic filler, the L value is 95 or more, the a value is -2 or more, and the b value is -1 or more, and the whiteness and reflectance are the highest.

[0062] For example, the method for producing titanium oxide may be either the sulfuric acid method or the chlorine method, and among these, the chlorine method is more preferable.Furthermore, it is preferable not to use sulfuric acid in the production process.Furthermore, the surface treatment of titanium oxide is not particularly limited, but it is preferable that titanium oxide is treated with an acid other than sulfuric acid, such as hydrochloric acid, nitric acid, phosphoric acid, or acetic acid, during neutralization.

[0063] The titanium oxide may be of any of the rutile, anatase, and ramsdellite structures, and may be used alone or in combination of two or more. Among these, the ramsdellite titanium oxide is ramsdellite Li 0.5 TiO 2It can be obtained by carrying out a chemical lithium oxide desorption treatment.

[0064] Among these, the use of rutile titanium oxide is preferable because it can further improve heat resistance, is less likely to discolor due to light irradiation, and can be less likely to deteriorate in quality even in a harsh usage environment. In particular, the use of rutile titanium oxide surface-treated with aluminum oxide such as alumina can improve heat resistance. The content of rutile titanium oxide surface-treated with aluminum oxide in the total titanium oxide is preferably 35% by mass or more, more preferably 55% by mass or more, and the upper limit is 100% by mass or less, that is, the total amount of titanium oxide may be rutile titanium oxide surface-treated with the aluminum oxide. In addition, anatase titanium oxide has a lower hardness than rutile titanium oxide, so that the formability of the composition is improved when anatase titanium oxide is used.

[0065] The amount of the inorganic filler (B) in the solder resist composition of the present invention is in the range of 30 to 70% by mass, preferably 40 to 60% by mass, and more preferably 40 to 50% by mass, based on the total mass of the resin composition. When the content of the inorganic filler (B) is within the above range, it is advantageous for high reflectivity, and when it is less than the above range, the reflectivity decreases, and when it exceeds the above range, there is a risk of cracking.

[0066] Among the (B) inorganic fillers, titanium oxide preferably has a sulfur concentration of 100 ppm or less, more preferably 50 ppm or less. Commercially available titanium oxide with a sulfur concentration of 100 ppm or less may be used, or commercially available titanium oxide with a sulfur concentration of 100 ppm or more may be blended with a reduced sulfur concentration by subjecting it to heat treatment, chemical treatment, or purification treatment such as washing or calcination. Here, the sulfur contained in titanium oxide refers to all sulfur detected by analysis. It includes sulfur adsorbed to titanium oxide and sulfur applied to titanium oxide as an impurity.

[0067] The solder resist composition of the present invention may contain titanium oxide having a sulfur concentration of 100 ppm or more, provided that the effect of the present invention is not impaired. Examples of titanium oxide having a sulfur concentration of 100 ppm or more include CR-58, CR-90, and R-630 manufactured by Ishihara Sangyo Kaisha, Ltd., and R-21 manufactured by Sakai-chem Co., Ltd.

[0068] In addition, rutile-type chlorine-process titanium oxide such as T-550, T-580, R-630, R-820, CR-50, CR-60, R-90, and CR-97 manufactured by Ishihara Sangyo Kaisha, Ltd., Ti PURE R-706 and R-902+ manufactured by DuPont, TR-600, TR-700, and TR-840 manufactured by Fuji Titanium Industry Co., Ltd., and KR-270, KR-310, and KR-380 manufactured by Titanium Industry Co., Ltd. may also be used.

[0069] If the particle size of titanium oxide is too small, the flowability is poor, and if it is too large, the insertability into the small diameter of the substrate is poor. In consideration of these, the median particle size of titanium oxide is in the range of 0.1 to 5 μm, preferably in the range of 0.1 to 1 μm, more preferably in the range of 0.1 to 0.5 μm, and most preferably 0.36 μm. When the particle size of titanium oxide is within the above range, high reflectance can be achieved. The above particle size was measured using a laser diffraction method.

[0070] Among the (B) inorganic fillers, examples of barium sulfate include precipitated barium sulfate #100, precipitated barium sulfate #300, precipitated barium sulfate SS-50, BARIACE B-30, BARIACE B-31, BARIACE B-32, BARIACE B-33, BARIACE B-34, BARIFINE BF-1, BARIACE BF-10, BARIACE BF-20, BARIACE BF-40 (manufactured by Sakai Chemical Industry Co., Ltd.), W-1, W-6, W-10, and C300 (manufactured by Takehara Kagaku Kogyo Co., Ltd.).

[0071] Among the (B) inorganic fillers, silica particles are not particularly limited and can be obtained by methods known to ordinary engineers. For example, they can be produced by burning silicon powder by the VMC (Vap-erized Metal Combustion) method. The VMC method is a method in which a chemical flame is formed by a burner in an oxygen-containing atmosphere, and a metal powder that constitutes a part of the target oxide particles is added into this chemical flame in an amount sufficient to form a dust cloud, causing knocking to obtain oxide particles. Commercially available silica includes the SO series manufactured by Admatechs Co., Ltd. and the HPS series (HPS-0500, HPS-1000, HPS3500, etc.) manufactured by Toagosei Co., Ltd.

[0072] (C) Mercapto-modified acrylate

[0073] The solder resist composition of the present invention uses a mercapto-modified acrylate (C) to enhance surface curing, improve gloss, and achieve high reflectance.

[0074] Furthermore, when the mercapto-modified acrylate (C) of the present invention is used in a solder resist composition together with the inorganic filler (B), the surface hardening of the solder resist layer is improved, and the improved surface hardening can achieve high reflectance and high gloss.

[0075] The mercapto-modified acrylate (C) of the present invention is preferably a monofunctional or polyfunctional acrylate compound, more preferably an aliphatic compound having 1 to 15 carbon atoms and substituted with one or more functional groups selected from the group consisting of an acryloyl group, an acryloyloxy group, and an acryloyloxyalkyl group, such as pentane triacrylate.

[0076] The mercapto-modified acrylate (C) of the present invention is curable, preferably active energy ray-curable, and can be obtained by subjecting a mercapto-modified (meth)acrylate polyfunctional thiol compound and a stoichiometric excess of a difunctional or higher polyfunctional (meth)acrylate compound to a Michael addition reaction. Preferred polyfunctional thiol compounds include polyfunctional thiol compounds that are reaction products of polyisocyanates such as pentaerythritol tetrakis (3-mercaptopropionate) (molecular weight 489 g / mol), trimethylolpropane tris (3-mercaptopropionate) (molecular weight 399 g / mol), and 1,3-bis (2-isocyanato-2-propyl) benzene tetrathiol (thiol) with polyfunctional thiol compounds such as trimethylolpropane tris (3-mercaptopropionate), and polyfunctional thiol compounds such as isophorone diisocyanate and trimethylolpropane tris (3-mercaptopropionate). Examples of the mercapto-modified acrylate include a polyfunctional thiol compound which is a reaction product of a polyisocyanate such as hexamethylene diisocyanate and a polyfunctional thiol compound such as trimethylolpropane tris(3-mercaptopropionate), 1,6-hexanedithiol (molecular weight 150 g / mol), ethylene glycol di-2-mercaptoacetate (molecular weight 210 g / mol), pentaerythritol tetrakis(2-mercaptoacetate) (molecular weight 433 g / mol), trimethylolpropane tris(2-mercaptoacetate), and ethylene glycol bis(3-mercaptopropionate) (molecular weight 238 g / mol). The mercapto-modified acrylate preferably contains two or more mercapto groups. More preferably, it is most preferable that the mercapto-modified acrylate contains three or more mercapto groups. The mercapto-modified (meth)acrylate is contained in the mercapto-modified acrylate component (C) in an amount of preferably 1 to 20 mass %, more preferably 1 to 10 mass %, and most preferably 1 to 7 mass %.In addition, the weight average molecular weight of the mercapto-modified (meth)acrylate is preferably 5,000 or less, more preferably 3,000 or less, and even more preferably 2,000 or less. If the weight average molecular weight is more than 5000, the mobility of the mercapto-modified (meth)acrylate molecule decreases, so that the reactivity of the active energy ray curable coating film formation of the present invention tends to decrease. For example, when the coating film is cured with UV-LED, the tackiness of the cured coating film surface increases, and when a printed matter is placed on the coating film, the possibility of a problem of the printed matter adhering to the coating film increases.

[0077] Of the above, (C) the mercapto-modified acrylate is most preferably a mercapto-modified acrylate.

[0078] The blending amount of (C) mercapto-modified acrylate is in the range of 2 to 6% by mass based on the total resin composition. In this case, (C) mercapto-modified acrylate is a pure monomer (solid content). The resin composition contains solid content and a solvent. When the content of (C) mercapto-modified acrylate is within the above range, the surface hardening is strengthened, the gloss is improved, high reflectance is possible, and there is little decrease in reflectance even after the manufacturing process. In addition, it has excellent crack resistance. When the content of (C) mercapto-modified acrylate is less than the above range, it is not possible to achieve a decrease in gloss due to a decrease in surface hardening and a high reflectance. When the content of (C) mercapto-modified acrylate is more than the above range, the surface is over-hardened, which may increase the cracking tendency of the coating film and decrease the resolution.

[0079] (D) Resin containing an aromatic ring

[0080] The aromatic ring-containing resin (D) of the present invention is a resin that is more excellent in resistance to yellowing than conventionally known resins. The solder resist composition of the present invention has excellent yellowing resistance due to the inclusion of the aromatic ring-containing resin (D).

[0081] The (D) aromatic ring-containing resin of the present invention may be any resin as long as it is cured by heating and exhibits electrical insulation properties, and preferably contains an aromatic ring.

[0082] In the solder resist composition of the present invention, the (D) aromatic ring-containing resin may be a melamine resin, a silicone resin, or a resin having a styrene skeleton, and among these, a resin having a styrene skeleton is most preferred.

[0083] In addition, preferably, the (D) resin containing an aromatic ring may contain a carboxyl group, and it is more preferable to use a carboxyl group-containing resin having a styrene skeleton, and a mixture of carboxyl group-containing resins other than the carboxyl group-containing resin having a styrene skeleton may also be used.

[0084] (D) When the resin containing an aromatic ring is a carboxyl group-containing resin having a styrene skeleton, it does not have a photosensitive group such as an ethylenically unsaturated bond having a carboxyl group in the molecule, has a styrene skeleton in the molecule, has an average molecular weight of 10,000 to 50,000, and has an acid value of 80 to 200 mgKOH / g. Such a carboxyl group-containing resin having a styrene skeleton can be synthesized by copolymerizing styrene as an essential monomer. By using a carboxyl group-containing resin having related physical properties, the cured film made of the photosensitive resin composition of the present invention has excellent touch dryness and flow resistance.

[0085] Specific examples of carboxyl group-containing resins having a styrene skeleton include carboxyl group-containing resins (which may be either oligomers or polymers) obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with a compound containing an unsaturated group selected from styrene, α-methylstyrene, lower alkyl (meth)acrylate, isobutylene, etc. The alkyl group refers to an alkyl group having 1 to 5 carbon atoms.

[0086] In the solder resist composition of the present invention, the weight average molecular weight of the carboxyl group-containing resin having a styrene skeleton varies depending on the resin skeleton, but in the range of 10,000 to 50,000, the flow prevention property is improved. It is preferably 10,000 to 25,000, more preferably 10,000 to 20,000, and even more preferably 10,000 to 17,000. By making the weight average molecular weight 10,000 or more, not only the flow prevention effect is improved, but also the touch dryness (tackiness) is improved, the moisture resistance of the exposed coating film is improved, the reduction of the film during development is suppressed, and the decrease in resolution can be suppressed. In addition, by making the weight average molecular weight 50,000 or less, not only the flow prevention effect is improved, but also the developability and storage stability are improved.

[0087] In the solder resist composition of the present invention, the acid value of the carboxyl group-containing resin having a styrene skeleton is 80 to 200 mgKOH / g. More preferably, it is 100 to 160 mgKOH / g. By making the acid value of the carboxyl group-containing resin having a styrene skeleton 80 mgKOH / g or more, the softening point becomes high, and therefore the tackiness and developability become high. In addition, by making the acid value of the carboxyl group-containing resin having a styrene skeleton 200 mgKOH / g or less, a suitable crosslink density is achieved, so that no stress is generated during curing, and a good coating film can be obtained.

[0088] In the solder resist composition of the present invention, the carboxyl group-containing resin having a styrene skeleton has an aromatic ring due to the presence of the styrene skeleton, and thus the cured product is prevented from decreasing in reflectance and discoloration due to light irradiation and heat, and has excellent developability and dryness to the touch. The proportion of the styrene skeleton in the molecule is preferably 10 to 80 mol%, more preferably 10 to 60 mol%, and most preferably 10 to 50 mol%. That is, when synthesizing the carboxyl group-containing resin having a styrene skeleton, it is preferable to use 30 to 60 mol% of styrene based on the total amount of monomers. When the proportion of the styrene skeleton in the carboxyl group-containing resin having a styrene skeleton is 10 mol% or more in the molecule, the compatibility with other components is good, and when it is 80 mol% or less in the molecule, the developability is good.

[0089] A carboxyl group-containing resin having a styrene skeleton produced by suspension polymerization is a resin having a high molecular weight. As a result, a composition using the resin is preferable in terms of excellent dryness to the touch (tackiness). Generally, when a carboxyl group-containing resin having a styrene skeleton is produced by suspension polymerization, it has a high molecular weight, but considering properties such as screen printing compatibility, dryness to the touch, and developability, it is necessary to limit the weight average molecular weight to the range of 10,000 to 50,000. Therefore, in order to control the molecular weight, it is preferable to use a chain transfer agent when synthesizing a carboxyl group-containing resin having a styrene skeleton.

[0090] In addition, in order to promote polymerization, it is preferable to use a polymerization initiator when synthesizing the carboxyl group-containing resin having a styrene skeleton. Examples of the polymerization initiator include BPO (benzoyl peroxide), t-butylperoxy-2-ethylhexanoate, and AMBN (2,2'-azobis(2-methylbutyronitrile)). Among these, BPO (benzoyl peroxide) is preferable. The amount of the polymerization initiator is preferably 0.1 to 10 mass%, more preferably 0.1 to 6 mass%, calculated as solid content, of 100 mass% of the carboxyl group-containing resin having a styrene skeleton.

[0091] The amount of the resin containing an aromatic ring (D) is in the range of 0.1 to 15% by mass, preferably 1 to 10% by mass, and more preferably 3 to 6% by mass, based on the total amount of the resin composition. The resin composition contains a solid content and a solvent.

[0092] If the content of the resin containing the aromatic ring (D) is less than the above range, the reflectance of the resin composition is decreased and discoloration due to yellowing is large. If the content of the resin containing the aromatic ring (D) is more than the above range, the dryness to the touch is increased. If it is within the above range, the decrease in reflectance and discoloration are suppressed, and the developability and dryness to the touch are excellent. If it is within the above range, the high reflectance and yellowing problems can be improved.

[0093] (E) Silane coupling agent

[0094] The solder resist composition of the present invention contains a silane coupling agent (E), which improves crack resistance, improves reflectance compared to conventional compositions, and also provides excellent gloss.

[0095] The silane coupling agent (E) of the present invention may have an organic group such as a vinyl group, a styrene group, an acrylic group, a methacrylic group, an isocyanurate group, an acid anhydride group, a ureido group, an epoxy group, an amino group, a methacryloxy group, a mercapto group, or an isocyanate group.

[0096] Examples of silane coupling agents having a vinyl group include vinyltrimethoxysilane and vinyltriethoxysilane. Examples of silane coupling agents having a styrene group include p-styrylmethoxysilane. Examples of silane coupling agents having a methacryl group include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyldiethoxysilane, and 3-methacryloxypropyltriethoxysilane. Examples of silane coupling agents having an acrylic group include 3-acryloxypropyltrimethoxysilane. Examples of silane coupling agents having an amino group include N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxy-silyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane. Examples of silane coupling agents having a mercapto group include 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane. Examples of silane coupling agents having an isocyanate group include 3-isocyanatepropyltriethoxysilane. Examples of silane coupling agents having an isocyanurate group include tris-(trimethoxysilylpropyl)isocyanurate. Examples of silane coupling agents having a ureido group include 3-ureidopropyltrialkoxysilane. Examples of silane coupling agents having an acid anhydride group include 3-(trimethoxysilyl)propylsuccinic anhydride. Among the above silane coupling agents, silane coupling agents having an epoxy group are most preferred. Examples include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane.Of these, 3-glycidoxypropyltriethoxysilane is most preferred.

[0097] In the solder resist composition of the present invention, the content of the silane coupling agent (E) is in the range of 0.1 to 5 mass % based on the total composition, preferably in the range of 0.3 to 3 mass %, and more preferably in the range of 0.5 to 2 mass %. The resin composition contains a solid content and a solvent. When the content of the silane coupling agent (E) is within the above range, the resin composition has excellent crack resistance and high reflectance. When the content of the silane coupling agent (E) is less than 0.1 mass %, problems with cracking and adhesion may occur, and when the content exceeds 5 mass %, tackiness increases and film formation does not proceed well.

[0098] (E) The silane coupling agent may be a commercially available product, and examples thereof include KBM-1003, KBE-1003, KBM-303, KBM-402, KBM-403, KBE-402 and KBE-403, KBM-1403, KBM-502, KBM-503, KBE-502, KBE-503, KBM5103, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103P, KBM-573, KBE-573, KBM-575, KBM-9659, KBM-585A, KBM-802, KBM-803, KBE-9007N, and X-12-967C, all of which are manufactured by Shin-Etsu Chemical Co., Ltd.

[0099] (F) Resin containing urethane bonds

[0100] The resin having a urethane bond (F) of the present invention is a resin excellent in flexibility.

[0101] The solder resist composition of the present invention uses a resin having a urethane bond (F), which does not crack even on flexible substrates or thin plates, enables lamination work of a uniform thickness, and has excellent resistance to cracking and cracking when subjected to external impact or bending. Therefore, the solder resist composition of the present invention has superior flexibility and crack resistance compared to other inks and solder resist compositions.

[0102] The resin having a urethane bond (F) of the present invention may include a modified urethane resin. The resin having a urethane bond may be an ester-type urethane resin, an ether-type urethane resin, a modified urethane acrylate resin, a modified urethane epoxy resin, a silicon-modified urethane resin, a fluorine-modified urethane resin, or the like. More preferably, a modified urethane epoxy acrylate resin containing an epoxy group may be used.

[0103] The resin having a urethane bond may be a known compound having a urethane bond, for example, a reaction product of an isocyanate compound (e.g., monoisocyanate, diisocyanate, polyisocyanate) with a compound having an OH group (e.g., monohydric alcohol, polyester polyol, polyether polyol, or other polyhydric alcohol, epoxy (meth)acrylate), or a modified product thereof.

[0104] In the present invention, the compound having a urethane bond is preferably one having an epoxy group having a carboxyl group, or one having a (meth)acryloyl group, and examples thereof include the following carboxyl group-containing resin (1), epoxy group-containing resin (2), and (meth)acryloyl group-containing resin (3), (4), and (5). As shown in the following examples, one resin may have at least two of the carboxyl group, epoxy group, and methacryloyl group.

[0105] (1) A carboxyl group-containing photosensitive polyurethane resin obtained by a polyaddition reaction between a diisocyanate and a monocarboxylic acid compound having an ethylenically unsaturated double bond, such as a bifunctional epoxy resin (meth)acrylate, such as bisphenol A type epoxy resin, hydrogenated bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bixylenol epoxy resin, or phenol type epoxy resin, or a partial anhydride or modified product thereof, and a carboxyl group-containing dialcohol compound and a diol compound.

[0106] (2) A urethane-modified epoxy resin having a urethane bond and two or more epoxy groups in the molecule, obtained by reacting a urethane bond-containing compound having an isocyanate group, obtained by reacting a polyhydroxy compound with a polyisocyanate compound, with a hydroxyl group-containing epoxy compound.

[0107] (3) Urethane resins obtained by polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with diol compounds such as polycarbonate-based polyols, polyether-based polyols, polyester-based polyols, polyolefin polyols, acrylic polyols, epoxy resins having hydroxyl groups (thus giving urethane resins having epoxy groups), bisphenol A-based alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.

[0108] (4) A photosensitive polyurethane resin obtained by replacing a part or all of the diisocyanate in (3) above with a reaction product of isophorone diisocyanate and pentaerythritol triacrylate, or a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, through a polyaddition reaction of such an isocyanate with the diol compound.

[0109] (5) A (meth)acrylate-terminated photosensitive polyurethane resin obtained by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of one of the resins (3) and (4) above.

[0110] Of the resins having a urethane bond, (1) among carboxyl group-containing resins, (2) among epoxy group-containing resins, and (5) among (meth)acryloyl group-containing resins are preferred.

[0111] As the diisocyanate, for example, an aromatic polyisocyanate, an aliphatic polyisocyanate, or an alicyclic polyisocyanate is used. Examples of aromatic polyisocyanates include 4,4'-diphenylmethane diisocyanate, 2,4-diisocyanate-2,6-tolylene diisocyanate, naphthalene-1,5-diisocyanate-o-xylylene diisocyanate, m-xylylene diisocyanate, and 2,4-tolylene dimer. Examples of aliphatic polyisocyanates include tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, 4,4-methylenebis(cyclohexyl isocyanate), and isophorone diisocyanate. A specific example of an alicyclic polyisocyanate is bicycloheptane triisocyanate. Among these, aliphatic isocyanates are most preferred.

[0112] When the compound having a urethane bond (F) is a carboxyl group-containing resin having a urethane bond, the acid value of the carboxyl group-containing resin is preferably in the range of 40 to 200 mgKOH / g, more preferably in the range of 45 to 120 mgKOH / g. When it is in the range of 40 mgKOH / g to 200 mgKOH / g, the adhesion of the cured film is obtained and alkaline development is facilitated, so that dissolution of the exposed area by the developer is suppressed, lines do not become narrower than necessary, and normal resist pattern writing is facilitated.

[0113] When the compound having a urethane bond (F) is a carboxyl group-containing resin having a urethane bond, the weight-average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, but generally, when the weight-average molecular weight is in the range of 2,000 to 150,000, preferably in the range of 5,000 to 50,000, more preferably in the range of 2,000 to 50,000, the tackiness is good, the moisture resistance of the cured film is good, and the coating film is less likely to be reduced during development. In addition, when the weight-average molecular weight is in the above range, the resolution and developability are good, and the storage stability is good.

[0114] As for the carboxyl group-containing resin having a urethane bond, examples of commercially available products of the resin having a urethane bond include UXE-3000 (Nippon Kayaku Co., Ltd.) and EPU-7N (urethane-modified epoxy resin; ADEKA Corporation). Of these, Ebecryl 210 (aromatic urethane acrylate; Daicel-Allnex Co., Ltd.) is the most preferred. The blending amount of the resin is in the range of 0.1 to 15% by mass, preferably in the range of 5 to 13% by mass, more preferably in the range of 8 to 11% by mass, based on the total resin composition. The resin composition contains a solid content and a solvent. When the content of the resin having (F) a urethane bond is within the above-mentioned range, the resin composition has excellent flexibility and crack resistance. When the content of the resin having (F) a urethane bond is less than the above-mentioned range, problems of cracking and flexibility may occur, and when the content of the urethane resin exceeds the above-mentioned range, tackiness increases, and printability and drying properties may become problematic. In the solder resist resin composition of the present invention, the weight average molecular weight of the (F) resin having a urethane bond is preferably in the range of 1,000 to 50,000, and more preferably 6,000 to 30,000. When the (F) resin having a urethane bond has a weight average molecular weight within the above range, it is effective in terms of crack resistance and flexibility.

[0115] Other optional ingredients

[0116] The solder resist composition of the present invention may contain various additives as necessary. Specifically, a thermosetting catalyst, a dispersant, an antioxidant, a photopolymerization initiator, a colorant, a thermosetting resin, an acrylic resin, other various additives, or a mixture of two or more of these may be added. As other optional components, one or more of the following materials may be contained.

[0117] <Photopolymerization initiator>

[0118] In the case where a photocurable resin is used in the solder resist composition of the present invention, it is preferable to add a photopolymerization initiator. Any photopolymerization initiator known as a photopolymerization initiator and a photoradical generator may be used as the photopolymerization initiator.

[0119] Examples of the photopolymerization initiator include bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4'',4''''-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, and bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (BASF Japan Ltd., IRGACURE 819) and other bisacylphosphine oxides; 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphinic acid methyl ester, 2-methylbenzoyldiphenylphosphine oxide, pivaloylphenylphosphinic acid isopropyl ester, 2,4,6-trimethylbenzoyldiphenylphosphine oxide (BASF Japan Ltd., DAROCUR Monoacylphosphine oxides such as 1-hydroxy-cyclohexyl phenyl ketone, 1-4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one and other hydroxyacetophenones; benzoins such as benzoin, benzyl benzoin methyl ether, benzoin ethyl ether, benzo-n-propyl ether, benzoin isopropyl ether, benzo-n-butyl ether and other benzoins; benzoin alkyl ethers; benzophenone, p-methylbenzophenone, Mihirazeketone methylbenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bisdiethylaminobenzophenone and other benzophenones;Acetophenone, 2,2-methoxy-2-phenylacetophenone, 2,2'-diethoxy-2-phenylacetophenone, 1,1'-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-4-(methylthio)phenyl]-2-morpholino-1-propanone-2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-(dimethylamino)-2-[(4-methylphenyl)methyl)-1-[4 -(4-morpholinyl)phenyl]-1-butanone, N,N-dimethylaminoacetophenone and other acetophenones; thioxanthones such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone; anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, anthraquinones such as 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; ketals such as acetophenone dimethyl ketal and benzyl dimethyl ketal; benzoic acid esters such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and p-dimethylbenzoic acid ethyl ester; 1,2-octanedione-1-4-(phenylthio)-2-(O-benzyl)benzoate; oxime esters such as ethanone 1-9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl-1-(0-acetyloxime); titanocenes such as bis(η-5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium and bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium;Examples of the photopolymerization initiator include phenyl disulfide, 2-nitrofluorene, butyroin, anisoin ethyl ether, azobisisobutyronitrile, and tetramethylthiuram disulfide. The above photopolymerization initiators may be used alone or in combination of two or more.

[0120] Among these, acylphosphine oxide-based photopolymerization initiators such as bisacylphosphine oxides and monoacylphosphine oxides are preferred because they are less sticky and have an excellent discoloration suppression effect. In particular, the use of bisacylphosphine oxides is preferred in that it can further improve the sensitivity and reduce stickiness.

[0121] The amount of the photopolymerization initiator is 0.01 to 10% by mass based on the total composition, preferably 0.01 to 7% by mass, and more preferably 0.01 to 5% by mass. By adding the photopolymerization initiator in this range, the photocurability with copper is sufficient, the curability of the coating film is good, the coating film properties such as chemical resistance are improved, and the curability in deep areas is also improved.

[0122] In the solder resist composition of the present invention, the photopolymerization initiator is preferably an oxime ester, phosphine oxide, acetophenone, or benzoate ester photopolymerization initiator, more preferably an oxime ester or phosphine oxide initiator.

[0123] When the content of the photopolymerization initiator is within the above range, undercut is small and resolution is excellent. When the content of the photopolymerization initiator is less than the above range, the coating film is not cured sufficiently or the undercut is large and the deep part is not cured. Also, when the content of the photopolymerization initiator is more than the above range, halation becomes severe and resolution is poor.

[0124] <Thermosetting resin>

[0125] The thermosetting resin of the present invention may be any resin that is cured by heating and exhibits electrical insulation, and examples of such resins include epoxy resins, oxetane compounds, melamine resins, silicone resins, etc. In particular, in the present invention, epoxy resins or oxetane compounds are preferably used, and these may be used in combination.

[0126] The epoxy resin may be a known and commonly used compound having one or more epoxy groups. Among them, a compound having two or more epoxy groups is preferred. For example, monoepoxy compounds such as butyl glycidyl ether, phenyl glycidyl ether, and glycidyl (meth)acrylate, bisphenol A type epoxy resin, bisphenol S type epoxy resin, bisphenol F type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, aliphatic ring epoxy resin, trimethylolpropane polyglycidyl ether, phenyl-1,3-diglycidyl ether, biphenyl-4,4'-diglycidyl ether, 1,6-hexanediol diglycidyl ether, diglycidyl ether of ethylene glycol or propylene glycol, sorbitol polyglycidyl ether, tris(2,3-epoxypropyl)isocyanurate, and triglycidyl tris(2-hydroxyethyl)isocyanurate, each of which may be used alone or in combination according to the required characteristics.

[0127] Specific examples of compounds having two or more epoxy groups include jER828, jER834, jER1001, and jER1004 from Mitsubishi Chemical Corporation, Epicron 840, Epicron 850, Epicron 1050, and Epicron 2055 from DIC Corporation, Epototo D-011, YD-013, YD127, and YD-128 from Nippon Steel & Sumikin Chemical Co., Ltd., and DER317 and DER331 from Dow Chemical Japan Co., Ltd. , DER661, DER664, Sumiepoxy ESA-011, ESA-014, ELA-115, ELA128 from Sumitomo Chemical Co., Ltd., AER330, AER331, AER661, AER664 and other bisphenol A type epoxy resins (all trade names) from Asahi Kasei E-Materials Co., Ltd.; jERYL903 from Mitsubishi Chemical Co., Ltd., Epicron 152, Epicron 165 from DIC Corporation, Nippon Steel & Sumikin Chemical Co., Ltd. Brominated epoxy resins such as Epototo YDE-400 and YDE-500 from Dow Chemical Japan Co., Ltd., DER542 from Dow Chemical Japan Co., Ltd., Sumiepoxy ESB-400 and ESB-700 from Sumitomo Chemical Co., Ltd., AER711 and AER714 from Asahi Kasei E-materials Co., Ltd. (all trade names); jER152 and jER154 from Mitsubishi Chemical Co., Ltd., DEN431 and DEN438 from Dow Chemical Japan Co., Ltd., and E Picron N-730, Epicron N-770, Epicron N-865, Epotohto YDC-701, YDC-704 from Nippon Steel & Sumikin Chemical Co., Ltd., EPPN-201, EPPN-1025, EPPN-1020, EPPN-104S, RE-306, NC-3000 from Nippon Chemical Industry Co., Ltd., Sumiepoxy ESCN-195X, ESCN-220 from Sumitomo Chemical Co., Ltd., AER from Asahi Kasei E-Materials Co., Ltd.Novolac epoxy resins such as ECN-235, ECN-299, YDCN-700-2, YDCN-700-3, YDCN-700-5, YDCN-700-7, YDCN-700-10, YDCN-704, YDCN-704A from Nippon Steel & Sumikin Chemical Co., Ltd., and Epiclon N-680, N-690, and N-695 (all trade names) from DIC Corporation; Epiclon N-690 from DIC Corporation; Bisphenol F type epoxy resins such as Mitsubishi Chemical's jER807, Nippon Steel & Sumikin Chemical's Epotohto YDF-175, YDF-2004 (all trade names); hydrogenated bisphenol A type epoxy resins such as Nippon Steel & Sumikin Chemical's Epotohto ST-2004, ST-2007, ST-3000 (all trade names); Mitsubishi Chemical's jER604, Nippon Steel & Sumikin Chemical's Epotohto YH-434; Sumitomo Chemical's Sumiepoxy ELM-120 (all trade names) and other glycidyl amine type epoxy resins; hydantoin type epoxy resins; alicyclic epoxy resins such as Daicel's Ceroxide 2021 (all trade names); Mitsubishi Chemical's YL-933, Dow Chemical Japan's TENtrihydroxyphenylmethane type epoxy resins such as EPPN-501, EPPN-502 (all trade names); bixylenol type or biphenol type epoxy resins or mixtures thereof such as YL-6056, YX-4000, YL-6121 (all trade names) from Mitsubishi Chemical Corporation; bisphenol S type epoxy resins such as EBPS-200 from Nippon Kayaku Co., Ltd., EPX-30 from ADEKA Corporation, and EXA-1514 (trade name) from DIC Corporation; bisphenol A novolac type epoxy resins such as jER157S (trade name) from Mitsubishi Chemical Corporation; jER Tetraphenylolethane type epoxy resins such as YL-931 (all trade names); heterocyclic epoxy resins such as TEPIC (all trade names) from Nissan Chemical Industries, Ltd.; diglycidyl phthalate resins such as Blenmar DGT from NOF Corp.; tetraglycidyl xylenoylethane resins such as ZX-1063 from Nippon Steel & Sumikin Chemical Co., Ltd.; naphthalene resins such as ESN-190, ESN-360 from Nippon Steel & Sumikin Chemical Co., Ltd., HP-4032, EXA-4750, EXA-4700 from DIC Corp. Examples of epoxy resins include, but are not limited to, epoxy resins containing aryl groups; epoxy resins having a dicyclopentadiene skeleton, such as HP-7200 and HP-7200H from DIC Corporation; glycidyl methacrylate copolymer epoxy resins, such as CP-50S and CP-50M from NOF Corporation; copolymer epoxy resins of cyclohexylmaleimide and glycidyl methacrylate; and CTBN-modified epoxy resins (for example, YR-102 and YR-450 from Nippon Steel & Sumikin Chemical Co., Ltd.). Among these, bisphenol A type epoxy resins, heterocyclic epoxy resins, or mixtures thereof are particularly preferred, as they have excellent resistance to discoloration. These epoxy resins may be used alone or in combination of two or more.

[0128] Next, the oxetane compound will be described.

[0129] TIFF2024164127000002.tif27127

[0130] (In the formula, R 1represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms), specific examples of the oxetane compound containing an oxetane ring represented by the formula (III) include 3-ethyl-3-hydroxymethyloxetane (manufactured by Toagosei Co., Ltd., product name OXT-101), 3-ethyl-3-(phenoxymethyl)oxetane (manufactured by Toagosei Co., Ltd., product name OXT-211), 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane (manufactured by Toagosei Co., Ltd., product name OXT-212), 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene (manufactured by Toagosei Co., Ltd., product name OXT-121), and bis(3-ethyl-3-oxetanylmethyl)ether (manufactured by Toagosei Co., Ltd., product name OXT-221). In addition, examples include phenol novolac-type oxetane compounds. Such oxetane compounds may be used in combination with the epoxy resin or may be used alone.

[0131] In the solder resist composition of the present invention, the epoxy resin is preferably a bisphenol-based epoxy resin. More preferably, a bisphenol-based epoxy resin having two or more epoxy groups is most preferable. The content of the bisphenol-based epoxy resin having two or more epoxy groups used in the present invention is in the range of 1 to 15% by mass, preferably in the range of 1 to 10% by mass, more preferably in the range of 3 to 10% by mass, based on the total resin composition. The resin composition contains a solid content and a solvent. In the solder resist resin composition of the present invention, the weight average molecular weight of the resin is preferably in the range of 150 to 100,000.

[0132] When the content of the epoxy resin is within the above range, the resin composition has excellent adhesion and excellent heat resistance. When the content of the epoxy resin is less than the above range, the coating film is not cured, and problems may occur in adhesion and pencil hardness of the coating film. When the content of the epoxy resin is more than the above range, yellowing becomes significant and high reflectance cannot be achieved after processing.

[0133] The equivalent ratio (epoxy group / carboxyl group equivalent ratio) obtained by dividing the equivalent of the epoxy groups contained in the epoxy resin by the equivalent of the carboxyl groups contained in the (A) carboxyl group-containing resin having no aromatic ring component may be 0.5 or more and 1.2 or less.

[0134] The epoxy group / carboxyl group equivalent ratio means the ratio obtained by dividing the equivalent of the epoxy group contained in the epoxy resin in the composition calculated as solid content by the equivalent of the carboxyl group contained in the carboxyl group-containing resin:

[0135] - Epoxy group equivalent: mass of solid content of epoxy resin / equivalent of epoxy group of solid content

[0136] -Carboxyl group equivalent: mass of solid content of carboxyl group-containing resin / carboxyl group equivalent of solid content

[0137] In general solder resist compositions, the curing density of the solder resist varies depending on the equivalent ratio of epoxy groups / carboxyl groups, and the difference in curing density leads to differences in HAST resistance, reflectance after HAST, solder heat resistance, adhesion, developability, solvent resistance, crack resistance, etc. When the equivalent ratio of epoxy groups / carboxyl groups is 0.5 or less, the curing density is relatively low, and when the equivalent ratio of epoxy groups / carboxyl groups exceeds 1.2, the curing density is relatively high, so that when the equivalent ratio is in the range of 0.5 or more and 1.2 or less, excellent HAST resistance, reflectance after HAST, developability, solvent resistance, adhesion, solder heat resistance, etc. can be exhibited.

[0138] Preferably, the solder resist composition has an equivalent ratio (epoxy group / carboxyl group equivalent ratio) of 0.5 or more and 1.2 or less, obtained by dividing the equivalent of the epoxy group contained in the epoxy resin by the equivalent of the carboxyl group contained in the carboxyl group-containing resin without an aromatic ring component (A), and the content of the mercapto-modified acrylate (C) may be 2% by mass to 6% by mass based on the total composition. The hardening density and surface hardening property of the solder resist surface differ depending on whether or not the component (C) of the mercapto-modified acrylate composition (C) is contained.

[0139] When the composition contains a mercapto-modified acrylate composition component (C) having an epoxy group / carboxyl group equivalent ratio of 0.5 or more and 1.2 or less, and an amount of the mercapto-modified acrylate composition is 2% by mass to 6% by mass relative to the entire composition, the composition can exhibit better HAST resistance, reflectance after HAST, developability, solvent resistance, adhesion, solder heat resistance, etc.

[0140] <Acrylic resin>

[0141] The acrylic resin is a photocurable resin. The photocurable resin may be any resin that is cured by irradiation with active energy rays and exhibits electrical insulation, and in the present invention, a compound having one or more ethylenically unsaturated bonds in the molecule is preferably used. As the compound having an ethylenically unsaturated bond, a known and commonly used photopolymerizable oligomer, photopolymerizable monomer, and photopolymerizable vinyl monomer are used. Among them, the photopolymerizable oligomer may be an unsaturated polyester oligomer, a (meth)acrylate oligomer, or the like. As the (meth)acrylate oligomer, an epoxy (meth)acrylate such as phenol novolac epoxy (meth)acrylate, cresol novolac epoxy (meth)acrylate, or bisphenol type epoxy (meth)acrylate, a urethane (meth)acrylate, an epoxy urethane (meth)acrylate, a polyester (meth)acrylate, a polyether (meth)acrylate, or a polybutadiene modified (meth)acrylate may be used.

[0142] Examples of the photopolymerizable monomer or photopolymerizable vinyl monomer include known and commonly used ones, for example, styrene derivatives such as styrene, chlorostyrene, and α-methylstyrene; vinyl esters such as vinyl acetate, vinyl butyrate, and vinyl benzoate; ethers such as vinyl isobutyl ether, vinyl-n-butyl ether, vinyl-t-butyl ether, vinyl-n-amyl ether, vinyl isoamyl ether, vinyl-n-octadecyl ether, vinyl cyclohexyl ether, ethylene glycol monobutyl ether, and triethylene glycol monomethyl ether; (meth)acrylamides such as acrylamide, methacrylamide, N-hydroxymethylacrylamide, N-hydroxymethylmethacrylamide, N-methoxymethylacrylamide, N-ethoxymethylacrylamide, and N-butoxymethylacrylamide; aryl compounds such as triallyl isocyanurate diaryl phthalate and diaryl isophthalate; 2-ethylhexyl (meth)acrylate, lauric acid, and the like. (Meth)acrylic acid esters such as aryl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, phenyl (meth)acrylate, and phenoxyethyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and pentaerythritol tri(meth)acrylate; alkoxyalkylene glycol mono(meth)acrylates such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; alkylene polyol poly(meth)acrylates such as ethylene glycol di(meth)acrylate, butanediol di(meth)acrylates, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate;Examples of the polyoxyalkylene glycol poly(meth)acrylates include diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, ethoxylated trimethylolpropane triacrylate, and propoxylated trimethylolpropane tri(meth)acrylate; poly(meth)acrylates such as hydroxypivalic acid neopentyl glycol ester di(meth)acrylate; and isonalate-type poly(meth)acrylates such as tris[(meth)acryloxyethyl]isocyanurate. These may be used alone or in combination of two or more depending on the required properties.

[0143] In the solder resist composition of the present invention, the acrylate resin is preferably an unsaturated polyester oligomer, a (meth)acrylate oligomer, or the like. More preferably, a 6-functional flexible acrylic oligomer is the most preferable. The blending amount of the resin containing the acrylic resin is in the range of 1 to 15% by mass, preferably in the range of 1 to 10% by mass, more preferably in the range of 5 to 10% by mass, based on the total resin composition. The resin composition contains a solid content and a solvent. When the mass ratio of the photopolymerized acrylic resin composition is within the above-mentioned range, the resolution and undercut are excellent. When the mass ratio of the photopolymerized acrylic resin composition is less than the above-mentioned range, the coating film may not be sufficiently cured, and problems such as undercut and uncured coating may occur. In addition, when the mass ratio of the acrylic resin composition exceeds the above-mentioned range, the coating film may be cracked due to overcuring, and the resolution may be poor.

[0144] <Thermosetting catalyst>

[0145] When a thermosetting resin is used in the composition of the present invention, at least one of a curing agent and a curing catalyst may be further added.

[0146] Examples of the curing agent include polyfunctional phenolic compounds, polycarboxylic acids and their acid anhydrides, aliphatic or aromatic primary or secondary amines, polyamide resins, isocyanate compounds, and polymercapto compounds. Among these, polyfunctional phenolic compounds, polycarboxylic acids, and their acid anhydrides are preferably used from the viewpoint of workability and insulation. As the polyfunctional phenolic compound, any compound having two or more phenolic hydroxyl groups in one molecule may be used, and any known and commonly used compound may be used. Specifically, phenol novolac resin, cresol novolac resin, bisphenol A, allylated bisphenol A, bisphenol F, bisphenol A novolac resin, vinylphenol copolymer resin, and the like may be used, and bisphenol A is particularly preferred because of its high reactivity and large effect of increasing heat resistance. These polyfunctional phenolic compounds undergo addition reaction with at least one or both of an epoxy compound and an oxetane compound in the presence of a suitable curing catalyst. Polycarboxylic acids and their acid anhydrides are compounds having two or more carboxyl groups in one molecule and their acid anhydrides, such as copolymers of (meth)acrylic acid, copolymers of maleic anhydride, condensates of dibasic acids, etc. Commercially available products include JONCRYL (product group name) from BASF, SMA Resin (product group name) from Sartomer, and polyazelaic anhydride from New Japan Chemical.

[0147] The curing catalyst is a compound that can be a curing catalyst in the reaction between a thermosetting resin such as an epoxy compound or an oxetane compound and a curing agent, or a compound that can be a polymerization catalyst when no curing agent is used. Specific examples of the curing catalyst include tertiary amines, tertiary amine salts, quaternary ammonium salts, tertiary phosphines, crown ether compounds, and phosphonium ylides, and any of these may be used alone or in combination of two or more.

[0148] Among these, imidazoles such as 2E4MZ, C11Z, C17Z, and 2PZ, imidazole AZINE compounds such as 2MZ-A and 2E4MZ-A, imidazole isocyanurates such as 2MZ-OK and 2PZ-OK, imidazole hydroxymethyl compounds such as 2PHZ and 2P4MHZ (trade names; Shikoku Kasei Kogyo Co., Ltd.), dicyandiamide and its derivatives, melamine and its derivatives, diaminomaleonitrile and its derivatives, diethylenetriamine, triethylenetetramine, tetraethylenediamine ... Preferred examples of the amines include amines such as pentamine, bis(hexamethylene)triamine, triethanolamine, and diaminodiphenylmethane; 1,8-diazabicyclo[5,4,0]undecene-7 (trade name DBU, San-Apro Co., Ltd.); 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro[5,5]undecane (trade name ATU, Ajinomoto Co., Ltd.); and organic phosphine compounds such as triphenylphosphine, tricyclohexylphosphine, tributylphosphine, and methyldiphenylphosphine.

[0149] In the solder resist composition of the present invention, the curing catalyst is preferably an amine-based, phosphine-based, or imidazole-based curing catalyst. More preferably, a melamine-based amine curing catalyst is preferred. The amount of the curing catalyst is in the range of 0.1 to 10% by mass, preferably 1 to 5% by mass, and more preferably 0.1 to 3% by mass, based on the total resin composition.

[0150] When the mass ratio of the curing catalyst is within the above range, the coating film is sufficiently cured to have excellent adhesion, pencil hardness, and heat resistance. However, when it is below the above range, the coating film may not be sufficiently cured, and the curing time may be long. Also, when the mass ratio of the curing catalyst is beyond the above range, the coating film may crack due to over-curing of the solder resist, and problems may occur in developability.

[0151] <Antioxidants>

[0152] The composition of the present invention also preferably contains an antioxidant. By containing an antioxidant, not only can the effect of preventing oxidative deterioration of curable resins and suppressing discoloration be obtained, but also the effect of improving heat resistance and providing good resolution (reproducibility of line width) can be obtained. That is, depending on the type of colorant, the resolution may be deteriorated by reflecting or absorbing light, but by containing an antioxidant, good resolution can be obtained regardless of the type of colorant. The antioxidant includes a radical scavenger that neutralizes the generated radicals and a peroxide decomposition inhibitor that decomposes the generated peroxide into harmless substances and prevents new radicals from being generated, and the like, and may be used alone or in combination of two or more types.

[0153] Specifically, examples of antioxidants that act as radical scavengers include hydroquinone, 4-t-butylcatechol, 2-t-butylhydroquinone, hydroquinone monomethyl ether, 2,6-di-t-butyl-p-cresol, 2,2-methylene-bis(4-methyl-6-t-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3' ,5'-di-t-butyl-4-hydroxybenzyl)-S-triazine-2,4,6-(1H,3H,5H)trione and other phenolic compounds, quinone compounds such as menaquinone and benzoquinone, and amine compounds such as bis(2,2,6,6-tetramethyl-4-piperidyl)-sebacate and phenothiazine. Commercially available products include, for example, IRGANOX1010 (all trade names, BASF Japan Ltd.).

[0154] Examples of antioxidants that act as peroxide decomposers include phosphorus compounds such as triphenyl phosphite, and sulfur compounds such as pentaerythritol tetralauryl thiopropionate, dilauryl thiodipropionate, and distearyl-3,3'-thiodipropionate.

[0155] Among these, the use of a phenol-based antioxidant is preferred in terms of the effect of suppressing discoloration, improving heat resistance, and reproducing better resolution.

[0156] Furthermore, since antioxidants, particularly phenolic antioxidants, may be more effective when used in combination with a heat stabilizer, the resin composition of the present invention may contain a heat stabilizer.

[0157] Examples of the heat stabilizer include phosphorus-based, hydroxylamine-based, and sulfur-based heat stabilizers. The heat stabilizers may be used alone or in combination of two or more. Among these antioxidants, in the present invention, hydroxylamine-based and sulfur-based antioxidants are preferred. More preferably, phenol-based antioxidants are most preferred. When a phenol-based antioxidant is used, its blending amount is preferably 0.01 to 5 mass %, more preferably 0.03 to 3 mass %, based on the total composition. By making the blending amount of the antioxidant 0.01 to 1 mass % or more, the effect of adding the antioxidant can be reliably obtained, and by making the blending amount 1 mass % or less, the photoreaction is not inhibited, good alkaline development can be obtained, and good touch dryness and coating film properties can be secured.

[0158] The solder resist composition of the present invention may contain an organic solvent for the purpose of adjusting the viscosity during production of the composition or during application to a substrate or base film. As the organic solvent, known and commonly used organic solvents such as esters, aliphatic hydrocarbons such as octane and decane, and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha may be used. These organic solvents may be used alone or in combination of two or more kinds.

[0159] The solder resist composition of the present invention may further contain other additives that are well known and commonly used in the field of electronic materials, such as thermal polymerization inhibitors, ultraviolet absorbers, plasticizers, flame retardants, antistatic agents, antioxidants, antibacterial and antifungal agents, defoamers, leveling agents, thickeners, adhesion imparting agents, thixotropic agents, photoinitiator assistants, sensitizers, curing accelerators, release agents, surface treatment agents, dispersants, dispersion assistants, surface modifiers, stabilizers, etc.

[0160] Dry film and its manufacturing method

[0161] The dry film of the present invention has one or more solder resist layers obtained by applying and drying the solder resist composition.

[0162] When forming a dry film, first, the resin composition of the present invention is diluted with an organic solvent to adjust the viscosity to an appropriate level, and then coated on a substrate film to a uniform thickness, for example, in the range of 40 to 60 μm, using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, etc. Thereafter, the coated composition is usually dried at a temperature in the range of 40 to 120° C. for 1 to 30 minutes to form a solder resist layer.

[0163] The thickness of the coating film is not particularly limited, but is usually appropriately selected from the range of 10 to 150 μm, preferably 10 to 80 μm, and more preferably 10 to 60 μm in thickness after drying.

[0164] As the base film, a plastic film is used, and for example, a polyester film such as polyethylene terephthalate (PET), a polyimide film, a polyamideimide film, a polypropylene film, a polystyrene film, etc. may be used. Among these, polyethylene terephthalate is preferred. The thickness of the base film is not particularly limited, but is generally appropriately selected from the range of 10 to 150 μm. It can also be applied to a metal foil such as a copper foil or an aluminum foil. The carrier film used may be subjected to a release treatment such as acrylic or silicone.

[0165] After forming the solder resist layer of the present invention on the substrate film, it is preferable to further laminate a peelable protective film on the surface of the film for the purpose of preventing dust from adhering to the surface of the film. For example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, or surface-treated paper may be used as the peelable protective film. The protective film may have a smaller adhesive force than that between the solder resist layer and the substrate film when peeled off. The thickness of the protective film is not particularly limited, but is preferably, for example, 10 to 150 μm.

[0166] In the present invention, the solder resist composition of the present invention may be applied onto the protective film and dried to form a solder resist layer, and a base film may be laminated on the surface of the solder resist layer. That is, in the present invention, when producing a dry film, the film to which the solder resist composition of the present invention is applied may be either the protective film or the base film.

[0167] The dry film of the present invention can be used to reflect light generated from light-emitting diodes (LEDs) or electroluminescent devices (ELs) used as light sources in backlights of liquid crystal displays of lighting fixtures, mobile terminals, personal computers, televisions, etc. The dry film of the present invention can be applied to LEDs and light-emitting PCBs, etc.

[0168] In order to form a cured film on a printed wiring board using a dry film, the protective film of the dry film is peeled off, and the exposed resin layer of the dry film is placed on a circuit-formed substrate and attached using a laminator or the like to form a resin layer on the circuit-formed substrate. The formed resin layer is then exposed to light, developed, heated, and then cured to form a cured film. The protective film may be peeled off before or after exposure.

[0169] The cured product of the present invention is obtained by curing the solder resist composition of the present invention or the solder resist layer of the dry film of the present invention. The cured product of the present invention can be suitably used for printed wiring boards and electronic components. The cured product of the present invention has excellent crack resistance, high resolution, and dielectric properties including low dielectric constant and low dielectric loss tangent. The cured product of the present invention also has excellent heat resistance and linear expansion coefficient.

[0170] The printed wiring board of the present invention is composed of a cured product obtained from the solder resist composition of the present invention or the solder resist layer of the dry film. The method for producing the printed wiring board of the present invention includes, for example, adjusting the viscosity of the solder resist composition of the present invention to be suitable for the coating method using the organic solvent described above, coating the composition on a substrate by a method such as dip coating, flow coating, roll coating, bar coater, screen printing, or curtain coating, and then evaporating and drying (pre-drying) the organic solvent contained in the composition at a temperature of 60 to 100°C to form a tacky-free resin layer. In addition, in the case of a dry film, the resin layer is attached to a substrate by a laminator or the like so that the resin layer is in contact with the substrate, and then the carrier film is peeled off to form a resin layer on the substrate.

[0171] The above-mentioned substrates include not only printed wiring boards and flexible printed wiring boards with circuits formed with copper or the like, but also materials such as copper foil laminates for high frequency circuits using paper phenol, paper epoxy, glass fiber epoxy, glass polyimide, glass fiber / epoxy, glass fiber / paper epoxy, synthetic fiber epoxy, fluororesin-polyethylene-polyphenylene ether, polyphenylene oxide cyanate, etc. Examples include copper foil laminates of all grades (FR-4, etc.), other metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer substrates, etc.

[0172] Bonding onto the dry film substrate is preferably performed after applying pressure and heating using a vacuum laminator or the like. By using such a vacuum laminator, when a substrate on which a circuit is formed is used, even if the surface of the substrate is uneven, the dry film adheres to the substrate, so that no air bubbles are mixed in and the depressions on the substrate surface are reduced. The pressure condition is preferably about 0.1 to 2.0 MPa, and the temperature condition is preferably 40 to 120°C.

[0173] The volatilization drying carried out after application of the solder resist composition of the present invention may be carried out using a hot air circulation drying oven, an IR furnace, a hot plate, a convection oven or the like (a method in which hot air from inside the dryer is brought into contact with the substrate using a heat source of an air heating method using steam, or a method in which hot air is sprayed from a nozzle onto the substrate).

[0174] After forming a solder resist layer on a substrate, the layer is selectively exposed to active energy rays through a photomask having a predetermined pattern, and the unexposed portions are removed by immersing the layer in a dilute alkaline aqueous solution (e.g., 0.3 to 3 wt. % sodium carbonate, Na 2 CO 3The cured product is then developed with a photoresist solution (aqueous solution) to form a pattern. In the case of a dry film, the support film of the dry film is developed (peeled off) after exposure to form a patterned cured product on the substrate. As long as the properties are not impaired, the support film may be peeled off from the dry film before exposure to expose and develop the exposed resin layer.

[0175] In addition, the cured product is irradiated with active energy rays and then finally cured by heat curing (for example, at 100 to 220°C), or by irradiating active energy rays after heat curing or by heat curing alone, to form a cured film with excellent properties such as adhesion and hardness.

[0176] The exposure device used for the above-mentioned active energy ray irradiation may be a device equipped with a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and irradiates ultraviolet rays in the range of 350 to 450 nm, or may be a direct imaging device (for example, a laser direct imaging device that directly draws CAD data from a computer with a laser). The direct imaging machine lamp light source or laser light source preferably has a maximum wavelength in the range of 350 to 450 nm. The exposure for image formation varies depending on the thickness, etc., but is usually 10 to 1000 mJ / cm. 2 , preferably 20 to 800 mJ / cm 2 may be within the range.

[0177] The developing method may be a dipping method, a shower method, a spray method, a brush method or the like, and the developing solution may be an aqueous alkali solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines or the like.

[0178] Solder resist layer and manufacturing method thereof

[0179] The cured product of the present invention may be formed by curing the solder resist composition of the present invention or the solder resist layer of the dry film of the present invention.

[0180] The solder resist composition of the present invention can be thermally cured, for example, by heating at a temperature of about 100 to 180° C., to form a cured film (cured product) that has excellent properties such as high reflectance, excellent yellowing resistance, and excellent crack resistance.

[0181] Printed wiring board and method for manufacturing same

[0182] The printed wiring board of the present invention may include a cured film obtained by curing the cured product of the solder resist composition of the present invention or the solder resist layer of the dry film of the present invention.

[0183] The printed wiring board of the present invention may include a dry film that includes one or more layers formed from the above-mentioned solder resist composition.

[0184] When forming a printed wiring board, the dry film is placed on a test substrate and vacuum lamination is used to transfer the dry film onto the test substrate.

[0185] The base film is then peeled off, and the substrate with the transferred dry film from which the base film has been peeled off is exposed to UV light using an exposure device. When exposed in this manner, the exposed areas (areas irradiated with light) are hardened. After exposure, the substrate is cooled at room temperature, and then placed in a developing device where the unexposed areas are developed with an alkaline aqueous solution, completing the formation of the resist pattern. The substrate with the pattern formed by development is post-cured in a 150°C oven for one hour, completing the substrate preparation.

[0186] In the method for manufacturing a printed wiring board including a solder resist layer of the present invention, the base film may be peeled off before performing an exposure operation after the lamination process. In the case of a colored solder resist layer, the base film is exposed while attached to the base film. When exposed to light while the base film is attached in this manner, light refracts while passing through the base film, and the surface portion of the pattern is exposed due to the refraction of light, and a reaction occurs due to a highly sensitive photopolymerization initiator. However, the solder resist layer has a high reflectivity, and light is reflected from the surface of the solder resist layer, so that an additional photoreaction occurs on the surface (upper portion) of the solder resist layer due to the reflected light, and an expansion phenomenon (halation) occurs on the upper side of the coating film. Conversely, the lower portion has a relatively small amount of light energy transmitted, and a phenomenon (undercut) occurs in which the side portion becomes narrower.

[0187] Specifically, in the case of the white solder resist layer, a halation occurred at the upper side of the coating film and an undercut occurred at the lower side, whereas this phenomenon did not occur in the case of the blue solder resist layer.

[0188] In this way, when the white solder resist layer is exposed to light with a base film attached, the halation phenomenon becomes severe at the upper side of the coating film, and the halation phenomenon continues to progress, making it difficult to realize the pattern and reducing the resolution.

[0189] Figure 1 compares a printed wiring board that was exposed by peeling off the base film before UV exposure with a printed wiring board that was exposed without peeling off the base film before UV exposure. When the base film was not peeled off before UV exposure, light was reflected on the surface of the white solder resist layer, causing the upper part to become larger (halation).

[0190] However, when the substrate film is peeled off and then exposed to light as in the present invention, the photopolymerization initiator reacts with oxygen, inhibiting the reaction of the photopolymerization initiator on the surface and reducing the phenomenon of the upper portion becoming enlarged. As a result, the solder resist pattern can be satisfactorily realized even in the white solder resist layer.

[0191] Specifically, in the absence of a substrate film, oxygen prevents the photoinitiator from forming radicals, preventing the chain reaction and thus reducing the halation phenomenon, whereas in the presence of a substrate film, the substrate film prevents contact between oxygen and the photoinitiator, allowing the radical chain reaction to continue and thus intensifying the halation phenomenon.

[0192] <Example>

[0193] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples.

[0194] <Synthesis Example 1 (alkali-soluble resin A, copolymer resin)>

[0195] In a flask equipped with a thermometer, a stirrer, a dropping funnel, and a reflux condenser, 325.0 parts by weight of dipropylene glycol monomethyl ether as a solvent was heated to 110°C, and a mixture of 174.0 parts by weight of methacrylic acid, 174.0 parts by weight of ε-caprolactone-modified methacrylic acid (average molecular weight 314), 77.0 parts by weight of methyl methacrylic acid, 222.0 parts by weight of dipropylene glycol monomethyl ether, and 12.0 parts by weight of t-butylperoxy-2-ethylhexanoate (Perbutyl-O from NOF Corp.) as a polymerization catalyst was added dropwise over 3 hours, and the mixture was stirred at 110°C for 3 hours, after which the polymerization catalyst was deactivated to obtain a resin solution. After cooling this resin solution, 289.0 parts by weight of Cyclomer M100 from Daicel Corporation, 3.0 parts by weight of triphenylphosphine, and 1.3 parts by weight of hydroquinone monomethyl ether were added, the temperature was raised to 100°C, and the mixture was stirred to carry out a ring-opening addition reaction of the epoxy group ring, yielding resin solution A. The solid content of the resulting resin solution A was 55% by weight, and the acid value of the solid content was 79.8 mgKOH / g.

[0196] <Synthesis example 2, D resin solution>

[0197] 200 parts by weight of deionized water and 0.3 parts by weight of sodium sulfate were poured into a pressure vessel equipped with a thermometer, a cooling tube, and a stirrer, and it was confirmed that they were dissolved. Then, 5 parts by weight of BPO (benzoyl peroxide) as a polymerization initiator and 5 parts by weight of MSD (α-methylstyrene dimer) as a chain transfer agent were added to a monomer mixture consisting of 10.4 parts by weight of MMA (methyl methacrylate), 5 parts by weight of n-BA (n-butyl acrylate), 24.6 parts by weight of MAA (methacrylic acid), and 60 parts by weight of Stylene (styrene), and then thoroughly dissolved. Then, a dispersant was added to a concentration of 300 ppm, and the inside of the vessel was replaced with nitrogen by thoroughly stirring, and the temperature was raised to perform suspension polymerization. After the polymerization was completed, the obtained suspension liquid was filtered through a 30 μm mesh and dried with hot air at 40 ° C. to obtain a particulate resin. The granular resin (copolymer resin) thus obtained was sufficiently dissolved in an organic solvent DPM (dipropylene glycol methyl ether) so that the solid content concentration was 50% by weight, to obtain resin solution D. The acid value of the solid content was 160 mgKOH / g.

[0198] <Synthesis Example 3, F resin solution>

[0199] 0.5g of triphenolphosphine and 183g (1.2mol) of tetrahydrophthalic anhydride were added to 433g of a 53% by weight solution of epoxy acrylate containing a urethane bond or a bisphenol AD ​​skeleton, and reacted at 110°C for 5 hours while stirring. As a result, epoxy acrylate resin solution F containing a carboxyl group and having a urethane bond and a bisphenol skeleton was obtained. The solid content of the obtained resin solution F was 51% by weight, the acid value of the solid content was 85mgKOH / g, and the Tg obtained by DSC measurement was 19.2°C.

[0200] (Method of analyzing sulfur concentration)

[0201] The sulfur concentration was measured by the following method. 0.25 g of each component was weighed out and used as the measurement sample. As a pretreatment, each measurement sample was subjected to combustion treatment by the quartz tube combustion method using a sample combustion device: Model QF-02 manufactured by Mitsubishi Chemical Corporation under the following conditions.

[0202] 1. Combustion conditions

[0203] (1) Temperature rise conditions (temperature rise section): Room temperature → (5°C / min.) → 200°C → (10°C / min.) → 500°C → (5°C / min.) → 900°C, maintained for 5 min.

[0204] (2) Combustion conditions (combustion section) Inlet: 850°C, Outlet: 900°C

[0205] (3) Burn time 40 min. (total)

[0206] 2. Gas conditions (all values ​​indicated by the flow meter on the device body)

[0207] (1) Oxygen SUB 100ml / min.

[0208] (2) Oxygen MAIN 200ml / min.

[0209] (3) Argon / oxygen 100ml / min. (converted at 700℃)

[0210] (4) Total flow rate: 400ml / min.

[0211] 3.Gas conditions during combustion

[0212] (1) Heating section up to 700°C: Argon, after 700°C: Oxygen

[0213] (2) Combustion area up to 900°C: oxygen

[0214] 4. Absorption solution: 15ml of 0.3% hydrogen peroxide (after combustion treatment, increase to 25ml)

[0215] The ion content of the absorption liquid after the above-obtained filling up was measured by ion chromatography under the following conditions, and the sulfur concentration of each component was determined.

[0216] Ion chromatograph: ICS-1500 (manufactured by Thermo Fisher Scientific) Eluent: 2.7 mM Na 2 CO 3 / 0.3mM NaHCO 3

[0217] Column: Ion Pac AS12A (Thermo Fisher Scientific)

[0218] Flow rate: 1ml / min.

[0219] Suppressor: ASRS300

[0220] Injection volume: 25μl

[0221] Production of solder resist resin composition

[0222] Table 1-1. Content of each component of the solder resist composition (unit: mass% based on the total composition, (C) mercapto-modified acrylate content is pure monomer (solid content))

[0223] TIFF2024164127000003.tif233149

[0224] Table 1-2. Content of each component of the solder resist composition (unit: mass% based on the total composition, (C) mercapto-modified acrylate content is pure monomer (solid content))

[0225] TIFF2024164127000004.tif235146

[0226] Table 1-3. Content of each component of the solder resist composition (unit: mass% based on the total composition, (C) mercapto-modified acrylate content is pure monomer (solid content))

[0227] TIFF2024164127000005.tif236154

[0228] Manufacturing of dry film including solder resist layer

[0229] In a dust-free room, the resin compositions of each Example and Comparative Example were applied to a uniform thickness (40-60 μm) on a substrate film (PET film) (Toray XD-500P, film thickness: 25 μm) using a comma coater. (2) The applied resin compositions were dried in four temperature chambers (Chamber 1: 60°C, Chamber 2: 80°C, Chamber 3: 100°C, Chamber 4: 100°C) ranging from 40 to 120°C. (3) The appropriately dried coating film on the substrate film was laminated with a protective film (PP film) to produce a dry film. At this time, the thickness of the dried coating film was set to be in the range of 40 μm to 60 μm.

[0230] Dry Film Evaluation

[0231] <Sensitivity>

[0232] The dry films prepared in each of the examples and comparative examples were laminated onto a substrate (lamination conditions - measurement equipment: vacuum laminator (Nikko Materials CVP-300); 1st chamber: temperature 60°C, vacuum time 10 seconds, vacuum degree 3hPa, pressure 0.2MPa, pressure time 10 seconds; 2nd chamber: temperature 70°C, pressure 6kgf / cm 2 After leaving the plate to cool to room temperature (pressure for 20 seconds), the PET film was peeled off. A Kodak Step Tablet No. 0.2 (41 steps) was used as a photomask, and the exposure was performed with a Screen Inc. DI exposure device at a light intensity of 300 mJ / cm2 on an integrated light meter. 2 The film was exposed to light at 30°C in 1% Na 2 CO 3 The aqueous solution was sprayed at a pressure of 0.2 MPa for 60 seconds for development, and the gloss level of the cured coating film was visually confirmed.

[0233] <Developability>

[0234] The dry films prepared in each of the examples and comparative examples were laminated on a substrate, dried at 90° C. for 0 to 20 minutes, cooled to room temperature, and then immersed in 1% NaCl at 30° C.2 CO 3 The aqueous solution was used for development at a spray pressure of 0.2 MPa for 60 seconds, and the presence of any residue on the substrate was confirmed.

[0235] PASS: No residue on the measurement substrate.

[0236] NG: × Residue present on the measurement substrate.

[0237] <Adhesion>

[0238] The dry film prepared in each Example and Comparative Example was laminated onto a substrate, and the PET film was peeled off. Using a DI exposure device manufactured by Screen, the integrated light meter was set to 300 mJ / cm 2 The film was exposed to light using a Kodak Step Tablet No. 0.2 (41 steps) as a photomask to give 23 steps, and then incubated at 30°C with 1% Na 2 CO 3 The aqueous solution was developed for 60 seconds under a spray pressure of 0.2 MPa, and the substrate was finally cured in a 150°C oven. 1 mm squares (10 x 10) were made on the substrate, transparent adhesive tape was completely attached to the squares, and one end of the tape was immediately peeled off in an instant while maintaining a right angle to the substrate, and the number of squares that remained incompletely were counted. The results were reported using the number of remaining squares as the numerator and the total number of squares (100) as the denominator.

[0239] ○: 100% of the grid remains.

[0240] △: 95 to 99% of the grid remains.

[0241] ×: Less than 95% of the grid remains.

[0242] <Solder heat resistance>

[0243] The substrate prepared in the same manner as above was immersed in a solder bath at 260° C. for 10 seconds, and then a peeling test was carried out in the same manner as in the adhesion evaluation, and the coating state was evaluated according to the following criteria.

[0244] ○: 100% of the grid remains.

[0245] △: 95 to 99% of the grid remains.

[0246] ×: Less than 95% of the grid remains.

[0247] <Pencil hardness>

[0248] Using a substrate prepared in the same manner as described above, pencils ranging from B to 9H, each with a lead tip ground flat, were pressed at an angle of approximately 45°, and the hardness of the pencil at which the coating did not peel off was recorded.

[0249] <Solvent resistance>

[0250] Substrates prepared in the same manner as above were immersed in a mixture of isopropyl alcohol and distilled water (75%:25%) for 15 minutes, and then the coating state was evaluated according to the following criteria.

[0251] Pass: There is no swelling, discoloration or peeling on the solder resist.

[0252] NG: Bulging, discoloration, and peeling are observed on the solder resist.

[0253] <HAST resistance>

[0254] The dry films prepared in the examples and comparative examples were laminated onto a substrate on which a comb-shaped electrode (line / space = 50 μm / 50 μm) was formed, and the total light intensity was measured at 300 mJ / cm 2 The film was exposed to light at 30°C in 1% Na 2 CO 3An aqueous solution was developed for 60 seconds under the condition of a spraying pressure of 0.2 MPa and cured in an oven at 150 °C for 60 minutes to form a dry film cured coating film, and a HAST evaluation substrate was fabricated. This evaluation substrate was placed in a high-temperature and high-humidity chamber with a temperature of 110 °C and a humidity of 85%, charged with a voltage of 20 V, and subjected to an in-chamber HAST (Highly Accelerated Stress Test) for 250 hours. After 250 hours, the discoloration and elution of the cured coating film of the dry film were evaluated according to the following criteria (equipment manufacturer: Espec, Ion migration system, equipment name: NY IM1064).

[0255] ○: No peeling, discoloration or elution

[0256] △: There are peeling, discoloration or elution

[0257] ×: Many peeling, discoloration and elution phenomena are visually confirmed

[0258] <Reflectance after HAST test>

[0259] After the in-chamber HAST test was performed on the HAST evaluation substrate, the reflectance was measured (equipment manufacturer: Espec, Ion migration system, equipment name: NY IM1064). The initial reflectance was 91%.

[0260] 〇: Reflectance exceeds 85%

[0261] △: Reflectance is 80% or more and less than 85%

[0262] ×: Reflectance is less than 80%

[0263] Table 2-1. Reliability evaluation results

[0264] JPEG2024164127000006.jpg87160

[0265] In the cases of Examples 1 to 6, the sensitivity, developability, adhesion, and solder heat resistance were excellent, the film coating was hard, and the solvent resistance was also excellent. In contrast, in the cases of Comparative Examples 1 to 3, the sensitivity and solder heat resistance were low, and the film was more brittle than Examples 1 to 6. As a result of the solvent resistance test, swelling, discoloration, and peeling were observed on the solder resist.

[0266] Table 2-2. Reliability evaluation results

[0267] JPEG2024164127000007.jpg59160

[0268] In the cases of Examples 7 to 9, the HAST resistance was excellent, the reflectance after the HAST test did not decrease significantly, there was no problem with the developability, and the adhesion, solder heat resistance, and solvent resistance were also excellent.

[0269] In contrast, in the case of Comparative Example 4, the adhesion of the cured coating film after the HAST test was reduced, the HAST resistance was poor, the reflectance after the HAST test was greatly reduced, and the solvent resistance and solder heat resistance were also poor. In addition, the developability was poor in Comparative Examples 5 and 6. In the cases of Comparative Examples 7 to 9, the HAST resistance was poor, the reflectance after the HAST test was greatly reduced, and the solder heat resistance was also poor.

[0270] <Reflectance>

[0271] The dry film prepared in each Example and Comparative Example was laminated onto a substrate, and the PET film was peeled off. Using a DI exposure device manufactured by Screen, the integrated light meter was set to 300 mJ / cm 2 The film was exposed to light using a Kodak Step Tablet No. 0.2 (41 steps) as a photomask to give 23 steps, and then incubated at 30°C with 1% Na 2 CO 3The aqueous solution was developed for 60 seconds under a spray pressure of 0.2 MPa, and then cured in an oven at 150°C for 60 minutes to obtain a substrate. The reflectance of the coating surface on the obtained substrate was measured at a wavelength of 450 nm using a spectrophotometer (CM-2600d, Konica Minolta Sensing, Inc.) (Table 3). Reflow was carried out 1 to 3 times at 260°C, and the reflectance was measured (Table 4). In addition, after the final curing, UV was irradiated at 500 mJ / cm using an integrated actinometer. 2 The reflectance was measured after passing the sample once to three times under the above conditions (Table 5).

[0272] Table 3. Reflectance evaluation after final curing

[0273] JPEG2024164127000008.jpg91160

[0274] As a result of the measurement in Examples 1 to 12, the L value of the spectrophotometer was 80 or more, the a value was −5 or more, and the b value was −5 or more.

[0275] Table 4. Reflectance evaluation after reflow

[0276] JPEG2024164127000009.jpg226158

[0277] In the cases of Examples 1 to 6, the average reflectance (reflow was performed 0, 1, 2, and 3 times) and the reflectance at 450 nm were higher than those of Comparative Examples 1 to 3. In particular, in the cases of Examples 1 to 6, even after performing reflow three times, the reflectance at 450 nm decreased within a range of 1.81% to 3.61%, confirming that the decrease in reflectance was small even after reflow. In contrast, in the cases of Comparative Examples 1 to 3, the reflectance decreased by 5.85%, 4.20%, and 5.8%, respectively, confirming that the decrease in reflectance after reflow was greater than that of Examples 1 to 6.

[0278] On the other hand, in the cases of Examples 1 to 6, the b values ​​before and after reflow were smaller than those of Comparative Examples 1 to 3. This indicates that Examples 1 to 6 were less yellowed than Comparative Examples 1 to 3.

[0279] Table 5. Evaluation of reflectance after UV treatment after final curing

[0280] JPEG2024164127000010.jpg226146

[0281] In the cases of Examples 1 to 6, the average reflectance (reflow was performed 0, 1, 2, and 3 times) and the reflectance at 450 nm were higher than those of Comparative Examples 1 to 3. Furthermore, in the cases of Examples 1 to 6, even after performing UV treatment three times after final curing, the average reflectance and the reflectance at 450 nm each decreased within a range of 1.78% to 2.54%, confirming that there was little decrease in reflectance even after UV treatment after final curing.

[0282] In contrast, in the cases of Comparative Examples 1 to 3, the reflectance decreased by 4.89%, 5.22%, and 6.13%, respectively, and it was confirmed that the decrease in reflectance after the UV treatment following final curing was greater than that in the cases of Examples 1 to 6.

[0283] On the other hand, in the cases of Examples 1 to 6, the b values ​​before and after reflow were smaller than those of Comparative Examples 1 to 3. This indicates that Examples 1 to 6 were less yellowed than Comparative Examples 1 to 3.

[0284] <Blue light test>

[0285] The dry films prepared in Examples 1 and 2 and Comparative Example 1 were laminated, and the irradiated light was 300 mJ / cm 2 using an integrating light meter. 2 The film was exposed to light at 30°C in 1% Na 2 CO 3 The aqueous solution was developed for 60 seconds under a spray pressure of 0.2 MPa, and then cured in an oven at 150°C for 60 minutes to obtain a substrate. The reflectance of the coating surface of the obtained substrate was measured at a wavelength of 450 nm using a spectrophotometer (CM-2600d, Konica Minolta Sensing, Inc.). The results are shown in Table 6. (Blue light test conditions: After leaving for 3000 hours of measurement, measurements were made at 450 nm for each time period, measurement equipment: Blue light tester, output 15.9 mW, emission wavelength 450 nm, measurement area: 0.708 cm) 2)

[0286] Table 6. Reflectance evaluation after 3000 hours of blue light

[0287] JPEG2024164127000011.jpg55160

[0288] In Examples 1 and 2, the reflectance at 450 nm for each time period was higher than that of Comparative Example 1. In addition, in Examples 1 and 2, the reflectance decreased by 1.76% and 1.11%, respectively, even after 3000 hours of irradiation with blue light, whereas in Comparative Example 1, the reflectance decreased by 11.81%, and it was confirmed that in Examples 1 and 2, the decrease rate of the reflectance after 3000 hours of irradiation with blue light was lower than that of Comparative Example 1.

[0289] <Tested in a chamber with a temperature of 85℃ and humidity of 85%, and reflectance test in a HS chamber>

[0290] The dry film prepared in Example 2 was laminated, and the luminance was 300 mJ / cm 2 using an integrated light meter. 2 The film was exposed to light at 30°C in 1% Na 2 CO 3 The aqueous solution was developed for 60 seconds under a spray pressure of 0.2 MPa, and then cured in a 150°C oven for 60 minutes to obtain a substrate. The obtained substrate was placed in a chamber (ETAC's HIFLEX, Temperature and Humidity chamber) with a temperature of 85°C and humidity of 85% and left for 1000 hours. The reflectance at a wavelength of 450 nm of the substrate left in the HS chamber for 1000 hours was measured using a spectrophotometer (CM-2600d, Konica Minolta Sensing, Inc.). The results are shown in Table 7.

[0291] Table 7. Reflectance evaluation after being left in a chamber at 85°C and 85% humidity

[0292] JPEG2024164127000012.jpg38160

[0293] In Example 2, even when evaluated for a long period of time under high temperature and high humidity conditions, the average reflectance and reflectance at 450 nm decreased by only 0.64% after 500 hours and 2.88% after 1000 hours, confirming that there was little decrease in reflectance even under high temperature and high humidity conditions.

[0294] <Crack resistance evaluation results (Erichsen test)>

[0295] The dry films (55 μm) produced in each of the Examples and Comparative Examples were laminated on Cu substrates (1600 μm), exposed to light, developed, and cured for 60 minutes in an oven at 150° C. to produce substrates. The coating surfaces of the obtained substrates were measured for the presence or absence of cracks, and the results are shown in Tables 8-1 and 8-2.

[0296] Evaluation of the presence or absence of cracks

[0297] ◯: Slight cracks occur.

[0298] ×: Severe cracking occurs.

[0299] Table 8-1. Crack resistance evaluation

[0300] JPEG2024164127000013.jpg26156

[0301] Table 8-2. Crack resistance evaluation

[0302] JPEG2024164127000014.jpg20156

[0303] 2 shows the results of the Erichsen test for Examples 1 to 9 and Comparative Examples 1 to 9. In the cases of Examples 1 to 9, slight cracks were generated, whereas in the cases of Comparative Examples 1 to 4, severe cracks were generated.

[0304] <Gloss evaluation>

[0305] The dry films prepared in each Example and Comparative Example were laminated, exposed, developed, and cured in an oven at 150°C for 60 minutes to prepare substrates. The gloss of the coating surface of the obtained substrate was measured at an angle of 60° using a gloss colorimeter (BYK E-4430). The results are shown in Tables 9-1 and 9-2.

[0306] Gloss rating

[0307] Pass: Glossiness is 80 or higher.

[0308] NG: Glossiness is 80 or less.

[0309] Table 9-1. Gloss evaluation results

[0310] JPEG2024164127000015.jpg27158

[0311] Table 9-2. Gloss evaluation results

[0312] JPEG2024164127000016.jpg21157

[0313] In the cases of Examples 1 to 9, the gloss level was higher than in the cases of Comparative Examples 1 to 3.

[0314] Evaluation of manufacturing methods for printed wiring boards including solder resist layers

[0315] Example 6

[0316] (1) The test substrate was buffed, cleaned, and then dried.

[0317] (2) The dry film prepared in Example 1 was peeled off from the protective PP film, placed on a test substrate, and then vacuum laminated using a vacuum lamination device (Nikko Materials Co., Ltd.) to transfer the dry film onto the test substrate. (Vacuum lamination conditions: 1st chamber -60℃, 3.0hpa, 10sec. / 0.2Mpa, 10sec, 2nd chamber -70℃)

[0318] (3) The PET film was peeled off.

[0319] (4) The substrate with the PET film peeled off and the dry film transferred was exposed to 300 mJ / cm 2 using a pattern film from Taiyo Ink Co., Ltd. of Korea, in a DI exposure device manufactured by Screen Co., Ltd. 2 (DI UV Exposure: SCREEN LEDIA 5, 300 mJ / cm 2 )

[0320] (5) After cooling the substrate at room temperature, it was placed in a developing device and developed (development conditions: 1 wt% Na 2 CO 3 , 30℃, 0.2MPa, 60 seconds).

[0321] (6) The solder resist pattern formation is completed.

[0322] (7) The substrate on which the pattern was formed by development was finally cured in an oven at 150° C. for 1 hour to complete the substrate preparation.

[0323] Comparative Example 3

[0324] The preparation of a printed wiring board was completed in the same manner as in Example 6, except that the PET film was not peeled off before UV exposure, and exposure was performed with the PET film attached.

[0325] <Evaluation of printed wiring boards>

[0326] The substrates produced in Example 6 and Comparative Example 3 were examined, and the results are shown in FIG.

[0327] Figure 1 is a diagram comparing a printed wiring board that was exposed by peeling off the base film before UV exposure and a printed wiring board that was exposed without peeling off the base film before UV exposure. The numbers in Figure 1 refer to the spacing between lines, also called Line / Space. That is, 100 / 100 means that the line is 100 μm thick and there is a 100 μm spacing between the lines, and the smaller this value, the better the resolution.

[0328] The printed wiring board of Example 6 was exposed to UV light after the PET film was peeled off, so the solder resist pattern was well formed and had high resolution. In contrast, the printed wiring board of Comparative Example 3 was exposed to UV light without peeling off the PET film, so the solder resist pattern was not formed and the resolution was very low (Figure 1).

Claims

1. A solder resist composition comprising (A) a carboxyl group-containing resin that does not contain an aromatic ring, (B) an inorganic filler, (C) a mercapto-modified acrylate, and (D) a resin that contains an aromatic ring.

2. 2. The solder resist composition according to claim 1, which is white.

3. The solder resist composition according to claim 1 , further comprising a thermosetting resin.

4. 4. The solder resist composition according to claim 3, wherein the thermosetting resin is an epoxy resin.

5. 4. The solder resist composition according to claim 3, wherein an equivalent ratio (epoxy group / carboxyl group equivalent ratio) obtained by dividing an equivalent of an epoxy group contained in the epoxy resin by an equivalent of a carboxyl group contained in the carboxyl group-containing resin is 0.5 or more and 1.2 or less.

6. 6. The solder resist composition according to claim 1, wherein the content of the mercapto-modified acrylate (C) is 2 to 6% by mass based on the total mass of the composition.

7. 2. The solder resist composition according to claim 1, wherein the mercapto-modified acrylate (C) is an aliphatic compound having 1 to 15 carbon atoms and substituted with one or more functional groups selected from the group consisting of an acryloyl group, an acryloyloxy group, and an acryloyloxyalkyl group.

8. 2. A dry film having a solder resist layer formed by applying the solder resist composition of claim 1 onto a substrate film and drying the applied composition.

9. A cured product obtained by curing the solder resist layer of the dry film according to claim 8.

10. A printed wiring board comprising the cured product of claim 9.

11. A method for producing a dry film, comprising the steps of: 1) applying the solder resist composition of claim 1 onto a substrate film; 2) drying the applied solder resist composition to form a solder resist layer; and 3) A step of laminating the dried solder resist layer with a protective film.

12. A method for manufacturing a printed wiring board, comprising the steps of: 1) a step of laminating the dry film of claim 8 on a substrate so that the solder resist layer is laminated thereon, and performing vacuum lamination; 2) peeling off the base film of the dry film and then exposing the solder resist layer; 3) developing the solder resist layer to remove unexposed areas to form a pattern; and 4) curing the patterned substrate.

Citation Information

Patent Citations

  • Photocurable / thermosetting resin composition and printed wiring board using the same

    JP2008134621A

  • Photocurable resin composition, ink, and coating material

    JP2019019291A

  • Curable composition for transparent base material, dry film, cured material, light-shielding member and member for display

    JP2020138992A