Resin film, laminate, and bag
A multilayer resin film with specific polypropylene and biomass polyethylene compositions addresses the tearability and sealing challenges of polypropylene films, enhancing environmental sustainability and performance.
Patent Information
- Application Number
- JP2024141091
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-10-24
AI Technical Summary
Polypropylene films used in packaging bags face challenges with reduced tearability due to their inferiority compared to polyethylene films, and substituting a portion of fossil fuel polypropylene with biomass polyethylene leads to reduced sealing properties and film-forming properties.
A multilayer resin film structure is developed, with specific compositions and layer arrangements that include polypropylene and biomass polyethylene, ensuring a polypropylene content of 66% by mass or more and a biomass degree of 5% or more, while maintaining excellent tearability and sealing properties.
The multilayer resin film achieves improved tearability and sealing properties, reducing environmental impact by incorporating biomass materials, and maintaining film-forming capabilities.
Smart Images

Figure 2024164149000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin film, a laminate, and a bag. [Background technology]
[0002] Films made of polypropylene have appropriate flexibility, excellent transparency, oil resistance, moisture resistance, chemical resistance, etc., and are inexpensive, and therefore are used for various packaging bags, etc. Furthermore, polypropylene films have sealing properties, and therefore are used as sealant films for packaging bags, etc. For example, Patent Document 1 proposes a multilayer film including a polypropylene resin layer, and discloses that this multilayer film is used as a sealant film.
[0003] However, although polypropylene film is superior to polyethylene film in terms of heat resistance, it has a drawback in that it is inferior to polyethylene film in terms of tearability, and therefore, when polypropylene film is used for a packaging bag, there is a problem that it is difficult to tear and open the packaging bag.
[0004] In recent years, in order to prevent global warming, there has been a demand for a reduction in carbon dioxide emissions on a global scale. In the field of materials, as in the field of energy, it is desirable to move away from fossil fuels, and the use of biomass has been attracting attention. Biomass is an organic compound that is photosynthesized from carbon dioxide and water, and by using it, it is converted back into carbon dioxide and water, making it a so-called carbon-neutral renewable energy. Recently, the practical application of biomass plastics made from these biomass materials has progressed rapidly, and attempts are being made to produce various resins from biomass materials.
[0005] Regarding polypropylene, biomass polypropylene made from biomass has been put on the market, but the current situation is that biomass polypropylene is much more expensive than fossil fuel polypropylene and is extremely less practical. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2005-335108 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present inventors have considered reducing the amount of fossil fuel polypropylene used and reducing the environmental impact by replacing a portion of fossil fuel polypropylene with relatively inexpensive biomass polyethylene. However, a new problem occurs in that a resin film containing polypropylene as a main component has a reduced sealability and film-forming property when the proportion of polyethylene is increased. As a result of intensive research, the present inventors have found that these problems can be solved by forming the resin film into a multi-layer structure and adjusting the polyethylene content of each layer. In addition, they have found that the tearability of such a multi-layered resin film is unexpectedly improved.
[0008] The present invention has been made in consideration of the above findings, and an object of the present invention is to provide a resin film, laminate, and bag that have a reduced environmental impact, as well as sealing and film-forming properties, and is particularly excellent in tearability. [Means for solving the problem]
[0009] The present invention is a resin film having at least a first layer, a second layer, and a third layer, wherein the first layer and the second layer are laminated directly or via a thermoplastic resin layer, the third layer is laminated to the second layer directly or via a thermoplastic resin layer, the first layer constitutes the innermost layer of the resin film, the resin film contains polypropylene and polyethylene, the resin composition constituting the first layer contains polypropylene as a main component, and the polyethylene content of the first layer is 20 mass% or less, the resin composition constituting the second layer contains polypropylene as a main component and biomass polyethylene, the polypropylene of the second layer is a propylene-ethylene random copolymer, the polyethylene content of the second layer is 5 mass% or more and 35 mass% or less, the resin composition constituting the third layer contains polypropylene as a main component, and the polyethylene content of the third layer is 35 mass% or less, the thickness of the resin film is 15 μm or more and 250 μm or less, and the biomass degree of the resin film is 5% or more.
[0010] In the resin film according to the present invention, the layer constituting the outermost layer of the resin film may have a biomass degree of 30% or less.
[0011] In the resin film according to the present invention, the polypropylene content may be 66% by mass or more.
[0012] In the resin film according to the present invention, the breaking elongation in one direction and in another direction perpendicular to the one direction may each be 500% or more.
[0013] The present invention is a laminate comprising at least one biaxially oriented plastic film and a resin film according to the present invention.
[0014] The present invention is a bag comprising a laminate according to the present invention. Effect of the Invention
[0015] According to the present invention, it is possible to provide a resin film, a laminate, and a bag which have a reduced environmental impact, as well as excellent sealing and film-forming properties, and which are particularly excellent in tearability. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the resin film of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing another example of the resin film of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view showing another example of the resin film of the present invention. [Figure 4] FIG. 4 is a cross-sectional view showing another example of the resin film of the present invention. [Diagram 5] FIG. 5 is a cross-sectional view showing another example of the resin film of the present invention. [Figure 6] FIG. 6 is a cross-sectional view showing another example of the resin film of the present invention. [Figure 7] FIG. 7 is a cross-sectional view showing an example of the laminate of the present invention. [Figure 8] FIG. 8 is a cross-sectional view showing another example of the laminate of the present invention. [Figure 9] FIG. 9 is a cross-sectional view showing another example of the laminate of the present invention. [Figure 10] FIG. 10 is a cross-sectional view showing another example of the laminate of the present invention. [Figure 11] FIG. 11 is a cross-sectional view showing another example of the laminate of the present invention. [Figure 12] FIG. 12 is a front view showing the bag of the present invention. [Figure 13] FIG. 13 is a diagram showing the cutting out of test pieces for measuring the seal strength and low-temperature sealability of the bag of the present invention. [Figure 14] FIG. 14 is a diagram showing how the seal strength and low-temperature sealability are measured using test pieces. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] An embodiment of the present invention will be described with reference to Figures 1 to 14. In the drawings attached to this specification, the scale and aspect ratios have been appropriately changed and exaggerated from those of the actual objects for the convenience of illustration and understanding.
[0018] In addition, terms used in this specification that specify shapes, geometric conditions, and the degree thereof, such as "parallel," "orthogonal," and "same," as well as values of length and angle, are not to be bound by strict meanings, but are to be interpreted to include a range within which similar functions can be expected.
[0019] Resin Film The resin film of the present invention comprises two layers, a first layer and a second layer, and the first layer and the second layer are laminated directly or via a thermoplastic resin layer, with the first layer constituting the innermost layer of the resin film. This allows the resin film to have sealability. In the resin film of the present invention, the innermost layer is a layer located on the side of the contents to be contained when the resin film is used in a bag. The second layer may also constitute the outermost layer of the resin film. In the resin film of the present invention, the outermost layer is a layer located opposite to the innermost layer. The resin film of the present invention further includes a third layer, which may be laminated directly or via a thermoplastic resin layer to the second layer. This can prevent curling in the resin film. The third layer may also constitute the outermost layer of the resin film. Hereinafter, an example of the layer structure of the resin film of the present invention will be described with reference to FIGS.
[0020] 1 is a cross-sectional view showing an example of a resin film 10 of the present invention. The resin film 10 includes a first layer 11 and a second layer 12. The first layer 11 constitutes the innermost layer of the resin film 10. The second layer 12 constitutes the outermost layer of the resin film 10. The first layer 11 and the second layer 12 are directly laminated together.
[0021] 2 is a cross-sectional view showing another example of the resin film 10 of the present invention. The resin film 10 is provided with a first layer 11, a first thermoplastic resin layer 13, and a second layer 12, in that order. The first layer 11 constitutes the innermost layer of the resin film 10. The second layer 12 constitutes the outermost layer of the resin film 10. The first layer 11 and the second layer 12 are laminated with the first thermoplastic resin layer 13 interposed therebetween.
[0022] 3 is a cross-sectional view showing another example of the resin film 10 of the present invention. The resin film 10 includes a first layer 11, a second layer 12, and a third layer 14, in that order. The first layer 11 constitutes the innermost layer of the resin film 10. The third layer 14 constitutes the outermost layer of the resin film 10. The first layer 11 and the second layer 12 are directly laminated to each other. The second layer 12 and the third layer 14 are directly laminated to each other.
[0023] 4 is a cross-sectional view showing another example of the resin film 10 of the present invention. The resin film 10 is provided with a first layer 11, a second layer 12, a first thermoplastic resin layer 13, and a third layer 14, in that order. The first layer 11 constitutes the innermost layer of the resin film 10. The third layer 14 constitutes the outermost layer of the resin film 10. The first layer 11 and the second layer 12 are directly laminated. The second layer 12 and the third layer 14 are laminated with the first thermoplastic resin layer 13 interposed therebetween.
[0024] 5 is a cross-sectional view showing another example of the resin film 10 of the present invention. The resin film 10 is provided with a first layer 11, a first thermoplastic resin layer 13, a second layer 12, and a third layer 14, in that order. The first layer 11 constitutes the innermost layer of the resin film 10. The third layer 14 constitutes the outermost layer of the resin film 10. The first layer 11 and the second layer 12 are laminated with the first thermoplastic resin layer 13 interposed therebetween. The second layer 12 and the third layer 14 are directly laminated.
[0025] 6 is a cross-sectional view showing another example of the resin film 10 of the present invention. The resin film 10 includes a first layer 11, a first thermoplastic resin layer 13, a second layer 12, a second thermoplastic resin layer 15, and a third layer 14, in that order. The first layer 11 constitutes the innermost layer of the resin film 10. The third layer 14 constitutes the outermost layer of the resin film 10. The first layer 11 and the second layer 12 are laminated with the first thermoplastic resin layer 13 interposed therebetween. The second layer 12 and the third layer 14 are laminated with the second thermoplastic resin layer 15 interposed therebetween.
[0026] It is also possible to appropriately combine a plurality of layer structures of the resin film 10 shown in the above-mentioned FIGS.
[0027] The resin film of the present invention contains polypropylene, for example, a propylene-ethylene block copolymer, a propylene-ethylene random copolymer, homopolypropylene, and a mixture of two or more of these.
[0028] Here, "propylene-ethylene block copolymer" refers to a material having the structural formula shown in formula (I) below: In formula (I), m1, m2, and m3 each represent an integer of 1 or more.
[0029] [ka]
[0030] Moreover, the term "propylene-ethylene random copolymer" refers to a material having the structural formula shown in the following formula (II): In formula (II), m and n each represent an integer of 1 or more.
[0031] [ka]
[0032] Moreover, "homopolypropylene" refers to a material having the structural formula shown in the following formula (III): In formula (III), m represents an integer of 1 or more.
[0033] [ka]
[0034] In the resin film of the present invention, the polypropylene content is preferably 66% by mass or more, more preferably 71% by mass or more and 99% by mass or less, and even more preferably 74% by mass or more and 95% by mass or less, which can improve the heat resistance and oil resistance of the resin film.
[0035] In this specification, unless otherwise specified, "propylene" is obtained from raw materials derived from fossil fuels.
[0036] The resin film of the present invention contains polyethylene. This can improve the tearability of the resin film. Examples of polyethylene include high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), and mixtures of two or more of these. From the viewpoint of sealability, the resin film of the present invention preferably contains low density polyethylene, linear low density polyethylene, and mixtures of these, and from the viewpoints of sealability and tearability, it is more preferable to contain low density polyethylene.
[0037] Here, high density polyethylene has a strength of 942 kg / m 3 Medium density polyethylene refers to polyethylene having a density exceeding 925 kg / m 3 Super 942kg / m 3 This refers to polyethylene having the following density: The low-density polyethylene may also be called high-pressure low-density polyethylene, which is a high-pressure ethylene homopolymer and can be obtained by a conventionally known high-pressure radical polymerization method. 3 It is a polyethylene having the following density: Linear low-density polyethylene is a copolymer of ethylene and α-olefins polymerized using a multi-site catalyst such as a Ziegler-Natta catalyst or a single-site catalyst such as a metallocene catalyst, and has a density of 925 kg / m 3 It is a polyethylene having the following density:
[0038] In the resin film of the present invention, the polyethylene content is preferably 29% by mass or less, more preferably 1% by mass or more and 28% by mass or less, and even more preferably 5% by mass or more and 26% by mass or less.
[0039] The polyethylene of the resin film may be fossil fuel polyethylene, biomass polyethylene, or a combination of these. From the viewpoint of reducing the environmental load, the resin film of the present invention preferably contains biomass polyethylene. Hereinafter, biomass polyethylene will be described.
[0040] <Biomass-derived ethylene> The method for producing ethylene derived from biomass, which is a raw material for biomass polyethylene, is not particularly limited, and it can be obtained by a conventionally known method. An example of the method for producing ethylene derived from biomass will be described below.
[0041] Biomass-derived ethylene can be produced using biomass-derived ethanol as a raw material. In particular, it is preferable to use biomass-derived fermented ethanol obtained from a plant raw material. The plant raw material is not particularly limited, and any conventionally known plant can be used. Examples of the plant raw material include corn, sugarcane, beet, and manioc.
[0042] Fermented ethanol derived from biomass refers to ethanol produced by contacting a culture solution containing a carbon source obtained from a plant raw material with an ethanol-producing microorganism or a product derived from its crushed material, and then purifying the ethanol. Conventionally known methods such as distillation, membrane separation, and extraction can be used to purify ethanol from the culture solution. For example, methods include adding benzene, cyclohexane, etc., and removing water by azeotropy or membrane separation.
[0043] In order to obtain the above ethylene, the ethanol may be further subjected to advanced purification at this stage, for example, so that the total amount of impurities in the ethanol is reduced to 1 ppm or less.
[0044] A catalyst is usually used when obtaining ethylene by the dehydration reaction of ethanol, but the catalyst is not particularly limited and any conventionally known catalyst can be used. From the viewpoint of the process, a fixed bed flow reaction is advantageous because it is easy to separate the catalyst from the product, and for example, γ-alumina is preferable.
[0045] Since this dehydration reaction is an endothermic reaction, it is usually carried out under heating conditions. As long as the reaction proceeds at a commercially useful reaction rate, the heating temperature is not limited, but is preferably 100° C. or higher, more preferably 250° C. or higher, and even more preferably 300° C. or higher. There is no particular upper limit, but from the viewpoint of energy balance and equipment, it is preferably 500° C. or lower, more preferably 400° C. or lower.
[0046] In the dehydration reaction of ethanol, the yield of the reaction depends on the amount of water contained in the ethanol supplied as a raw material. In general, when performing a dehydration reaction, it is preferable to have no water in consideration of the efficiency of removing water. However, in the case of the dehydration reaction of ethanol using a solid catalyst, it has been found that the amount of other olefins, especially butene, produced tends to increase if water is not present. It is presumed that this is because ethylene dimerization after dehydration cannot be suppressed if a small amount of water is not present. The lower limit of the allowable water content is 0.1% by mass or more, preferably 0.5% by mass or more. The upper limit is not particularly limited, but from the viewpoint of material balance and heat balance, it is preferably 50% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less.
[0047] By carrying out the dehydration reaction of ethanol in this manner, a mixture of ethylene, water, and a small amount of unreacted ethanol is obtained, but since ethylene is in a gaseous state at room temperature under approximately 5 MPa or less, water and ethanol can be removed from this mixture by gas-liquid separation to obtain ethylene. This can be done by a known method.
[0048] The ethylene obtained by the gas-liquid separation is further distilled. The distillation method, operation temperature, residence time, etc. are not particularly limited, except that the operation pressure at this time is normal pressure or higher.
[0049] When the raw material is biomass-derived ethanol, the obtained ethylene contains trace amounts of carbonyl compounds such as ketones, aldehydes, and esters, which are impurities mixed in during the ethanol fermentation process, and carbon dioxide gas, which is a decomposition product thereof, and nitrogen-containing compounds such as amines and amino acids, which are enzyme decomposition products and impurities, and ammonia, which is a decomposition product thereof. Depending on the use of ethylene, these trace amounts of impurities may be problematic, so they may be removed by purification. The purification method is not particularly limited, and can be performed by a conventionally known method. An example of a suitable purification operation is an adsorption purification method. The adsorbent used is not particularly limited, and a conventionally known adsorbent can be used. For example, a material with a high surface area is preferable, and the type of adsorbent is selected according to the type and amount of impurities in the ethylene obtained by the dehydration reaction of biomass-derived ethanol.
[0050] In addition, a caustic water treatment may be used in combination as a method for purifying impurities in ethylene. When caustic water treatment is used, it is preferable to carry out the treatment before adsorption purification. In that case, it is necessary to carry out a water removal treatment after the caustic treatment and before the adsorption purification.
[0051] <Biomass polyethylene> Biomass polyethylene is formed by polymerizing monomers containing ethylene derived from biomass. It is preferable to use the biomass-derived ethylene obtained by the above-mentioned manufacturing method. Since biomass-derived ethylene is used as the raw material monomer, the polymerized polyethylene is derived from biomass. As the biomass polyethylene, for example, biomass linear low-density polyethylene (product name: SLL318, density: 918 kg / m) manufactured by Braskem is available. 3 , MFR: 2.7g / 10min, biomass content 87%), Braskem biomass low-density polyethylene (product name: SEB853, density: 923kg / m 3 , MFR: 2.7 g / 10 min, biomass content: 95%), etc. The raw material monomer for polyethylene does not have to contain 100% by mass of ethylene derived from biomass.
[0052] As long as the object of the present invention is not impaired, the monomer that is the raw material of the biomass polyethylene may further contain ethylene derived from a fossil fuel.
[0053] In the present invention, the "biomass degree" is represented by the weight ratio of biomass-derived components.
[0054] Carbon dioxide in the atmosphere contains a certain proportion of C14 (105.5 pMC), so it is known that the C14 content in plants that grow by absorbing carbon dioxide from the atmosphere, such as corn, is also about 105.5 pMC. It is also known that fossil fuels contain almost no C14. Therefore, the proportion of carbon derived from biomass can be calculated by measuring the proportion of C14 in the total carbon atoms. In the present invention, the "biomass degree" indicates the weight ratio of biomass-derived components. For example, taking polyethylene terephthalate as an example, polyethylene terephthalate is a polymer of ethylene glycol containing 2 carbon atoms and terephthalic acid containing 8 carbon atoms in a molar ratio of 1:1. Therefore, when only biomass-derived ethylene glycol is used, the weight ratio of biomass-derived components in the polyester is 31.25%, so the theoretical value of the biomass degree is 31.25%. Specifically, the mass of polyethylene terephthalate is 192, of which the mass derived from biomass-derived ethylene glycol is 60, so 60÷192×100=31.25. In addition, the weight ratio of biomass-derived components in a fossil fuel-derived polyester produced using fossil fuel-derived ethylene glycol and fossil fuel-derived dicarboxylic acid is 0%, and the biomass degree of the fossil fuel-derived polyester is 0%. Hereinafter, unless otherwise specified, "biomass degree" refers to the weight ratio of biomass-derived components.
[0055] In the present invention, theoretically, if all biomass-derived ethylene is used as the raw material for polyethylene, the concentration of biomass-derived ethylene is 100%, and the biomass degree of biomass polyethylene is 100%. Also, the concentration of biomass-derived ethylene in fossil fuel polyethylene produced only from raw materials derived from fossil fuels is 0%, and the biomass degree of fossil fuel polyethylene is 0%.
[0056] In the present invention, the biomass polyethylene or the biomass-derived resin layer does not need to have a biomass content of 100%. This is because if even a part of the resin film is made of biomass-derived raw materials, it is in line with the purpose of reducing the amount of fossil fuel used compared to conventional methods.
[0057] The present resin film preferably has a biomass ratio of 5% or more. This allows the environmental load to be further reduced. The biomass ratio of the resin film is more preferably 5% or more and 90% or less, even more preferably 5% or more and 50% or less, and even more preferably 10% or more and 25% or less.
[0058] The thickness of the resin film of the present invention is preferably from 15 μm to 250 μm, more preferably from 20 μm to 200 μm, and even more preferably from 20 μm to 150 μm, which can further improve the sealability of the resin film.
[0059] In the resin film of the present invention, the thickness of the second layer is preferably equal to or greater than the thickness of the first layer. This can improve the sealability and tearability of the resin film. The thickness ratio of the first layer:the second layer is preferably 1:8 to 1:1, and more preferably 1:5 to 1:1. In addition, when the resin film has a third layer, the thickness of the second layer is preferably equal to or greater than the thickness of the third layer. This improves the interlayer lamination strength and tear resistance with the multilayer. The thickness ratio of the second layer:the third layer is preferably 8:1 to 1:1, and more preferably 5:1 to 1:1.
[0060] The resin film of the present invention preferably has a breaking elongation of 500% or more in one direction and in the other direction perpendicular to the one direction. The breaking elongation of the resin film in the present invention is measured in accordance with JIS K7127. Using a Tensilon universal material testing machine RTC-1310A (manufactured by A&D Co., Ltd.), the test piece is held for 1 minute in an environment of 25°C temperature and 50% relative humidity, and then measured in an environment of 25°C temperature and 50% relative humidity. The measurement is performed using a rectangular test piece with one side of 15 mm and a direction perpendicular to the one side of 150 mm, the initial gripping tool distance is 100 mm, and the tensile speed is 300 mm / min. As long as the measurement can be performed with the initial gripping tool distance of 100 mm, the length in the direction perpendicular to the one side can be adjusted.
[0061] The breaking elongation (%) of the resin film in the machine direction (MD) is preferably 500% or more. The breaking elongation of the resin film in the machine direction (MD) is preferably 700% or more, more preferably 800% or more. In addition, the breaking elongation of the resin film in the transverse direction (TD) perpendicular to the machine direction is preferably 500% or more. The breaking elongation of the resin film in the transverse direction (TD) is preferably 700% or more, more preferably 800% or less, and even more preferably 900% or more.
[0062] The one direction mentioned above may be a direction different from the machine direction (MD) or the perpendicular direction (TD).
[0063] The first layer, the second layer, the third layer and the thermoplastic resin layer will each be described in detail below.
[0064] (1st layer) The first layer is composed of a resin composition containing polypropylene as a main component. This can improve the heat resistance and oil resistance of the resin film. In this specification, "containing as a main component" and "being a main component" mean that the content is more than 50 mass%. Examples of polypropylene include propylene-ethylene block copolymers, propylene-ethylene random copolymers, homopolypropylenes, and mixtures of two or more of these. From the viewpoint of seal strength, the resin composition constituting the first layer preferably contains a propylene-ethylene block copolymer, and from the viewpoint of low-temperature sealability, it preferably contains a propylene-ethylene random copolymer.
[0065] In the resin composition constituting the first layer, the polypropylene content is preferably 51% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, which can further improve the heat resistance and oil resistance of the resin film.
[0066] The resin composition constituting the first layer may contain polyethylene. This can improve the tearability of the resin film. Examples of polyethylene include high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear low-density polyethylene, and mixtures of two or more of these. From the viewpoint of sealability, the resin composition constituting the first layer preferably contains low-density polyethylene, linear low-density polyethylene, and mixtures of these.
[0067] When a mixture of polypropylene and polyethylene is used as the resin composition constituting the first layer, the resin composition constituting the first layer may have an island-in-sea structure. Here, the "island-in-sea structure" refers to a structure in which polyethylene is discontinuously dispersed within a region in which polypropylene is continuous. By having the island-in-sea structure, the tearability of the resin film can be further improved.
[0068] In the resin composition constituting the first layer, the polyethylene content is 20% by mass or less. This makes it possible to obtain a resin film with sealability. The polyethylene content in the resin composition constituting the first layer is preferably 15% by mass or less, and more preferably 10% by mass or less.
[0069] The polyethylene of the resin composition constituting the first layer may be fossil fuel polyethylene, biomass polyethylene, or a combination thereof. From the viewpoint of reducing the environmental load, it is preferable that the resin composition constituting the first layer contains biomass polyethylene.
[0070] In the resin composition constituting the first layer, the biomass degree is preferably 50% or less. Resins obtained from raw materials derived from biomass have a higher proportion of low molecular weight components than resins obtained from raw materials derived from fossil fuels, and these low molecular weight components may affect the sealability of the resin film. Therefore, by setting the biomass degree of the resin composition constituting the first layer to 50% or less, the effect on the sealability can be reduced. From the viewpoint of reducing the environmental load and sealability, the biomass degree of the resin composition constituting the first layer is preferably 0.1% or more and 25% or less, and more preferably 1% or more and 15% or less.
[0071] The resin composition constituting the first layer preferably has a melt flow rate (MFR) of 1 g / 10 min to 30 g / 10 min, more preferably 3 g / 10 min to 25 g / 10 min, and even more preferably 5 g / 10 min to 20 g / 10 min. The melt flow rate is a value measured by method A under the conditions of a temperature of 190° C. and a load of 21.18 N in the method specified in JIS K7210-2014. If the MFR of the resin composition constituting the first layer is 1 g / 10 min or more, the extrusion load during molding can be reduced. In addition, if the MFR of the resin composition constituting the first layer is 30 g / 10 min or less, the mechanical strength of the resin film can be increased.
[0072] The thickness of the first layer is preferably 5 μm or more and 100 μm or less, more preferably 5 μm or more and 80 μm or less, and even more preferably 10 μm or more and 50 μm or less. This can further improve the sealing property of the resin film. The first layer may be composed of two or more layers.
[0073] As long as the properties of the present invention are not impaired, the resin composition constituting the first layer may contain one or more additives, such as antioxidants, antiblocking agents, lubricants, fillers, plasticizers, antistatic agents, UV absorbers, inorganic particles, organic particles, release agents, and dispersants.
[0074] (2nd layer) The second layer is composed of a resin composition containing polypropylene as a main component and biomass polyethylene. The resin composition constituting the second layer contains polypropylene as a main component, which can improve the heat resistance and oil resistance of the resin film. In addition, the resin composition constituting the second layer contains biomass polyethylene, which can improve the environmental load reduction and tearability of the resin film.
[0075] The resin composition constituting the second layer may have an island-in-a-sea structure, which can further improve the tearability of the resin film.
[0076] In the resin composition constituting the second layer, examples of the polypropylene include a propylene-ethylene block copolymer, a propylene-ethylene random copolymer, a homopolypropylene, and a mixture of two or more of these. From the viewpoint of seal strength, the resin composition constituting the second layer preferably contains a propylene-ethylene block copolymer, and from the viewpoint of low-temperature sealability, it preferably contains a propylene-ethylene random copolymer.
[0077] In the resin composition constituting the second layer, the polypropylene content is preferably 51% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, which can further improve the heat resistance and oil resistance of the resin film.
[0078] In the resin composition constituting the second layer, examples of the biomass polyethylene include biomass high density polyethylene, biomass medium density polyethylene, biomass low density polyethylene, biomass linear low density polyethylene, and mixtures of two or more of these. From the viewpoint of tearability, the resin composition constituting the second layer preferably contains biomass low density polyethylene.
[0079] The resin composition constituting the second layer preferably has a biomass ratio of 5% or more. This allows the resin film to have a further improved environmental load reduction. The resin composition constituting the second layer more preferably has a biomass ratio of 5% or more and 95% or less, and further preferably has a biomass ratio of 10% or more and 50% or less.
[0080] When the second layer constitutes the outermost layer of the resin film, the biomass degree of the resin composition constituting the second layer is preferably 30% or less. Resins obtained from raw materials derived from biomass have a higher proportion of low molecular weight components than resins obtained from raw materials derived from fossil fuels, and these low molecular weight components may affect adhesion with other layers. By setting the biomass degree of the resin composition constituting the second layer to 30% or less, it is possible to reduce the influence on adhesion with other layers. From the viewpoint of reducing environmental load and adhesion, the biomass degree of the resin composition constituting the second layer is preferably 1% or more and 27% or less, and more preferably 5% or more and 20% or less.
[0081] The resin composition constituting the second layer may contain fossil fuel polyethylene, provided that the characteristics of the present invention are not impaired. Examples of fossil fuel polyethylene include fossil fuel high density polyethylene, fossil fuel medium density polyethylene, fossil fuel low density polyethylene, fossil fuel linear low density polyethylene, and mixtures of two or more of these.
[0082] In the resin composition constituting the second layer, the polyethylene content is 35% by mass or less. This allows a resin film to have film-forming properties. The polyethylene content in the resin composition constituting the second layer is preferably 5% by mass or more and 30% by mass or less, and more preferably 15% by mass or more and 30% by mass or less. This allows the tearability of the resin film to be improved.
[0083] The resin composition constituting the second layer preferably has a melt flow rate (MFR) of 1 g / 10 min to 30 g / 10 min, more preferably 3 g / 10 min to 25 g / 10 min, and even more preferably 5 g / 10 min to 20 g / 10 min. If the MFR of the resin composition constituting the second layer is 1 g / 10 min or more, the extrusion load during molding can be reduced. In addition, if the MFR of the resin composition constituting the second layer is 30 g / 10 min or less, the mechanical strength of the resin film can be increased.
[0084] The thickness of the second layer is preferably 10 μm or more and 150 μm or less, more preferably 15 μm or more and 120 μm or less, and even more preferably 20 μm or more and 100 μm or less. This can further improve the sealing property of the resin film. The second layer may be composed of two or more layers.
[0085] As long as the properties of the present invention are not impaired, the resin composition constituting the second layer may contain one or more additives, such as antioxidants, antiblocking agents, lubricants, fillers, plasticizers, antistatic agents, UV absorbers, inorganic particles, organic particles, release agents, and dispersants.
[0086] (3rd layer) The third layer is composed of a resin composition containing polypropylene as a main component. This can improve the heat resistance and oil resistance of the resin film. Examples of polypropylene include propylene-ethylene block copolymers, propylene-ethylene random copolymers, homopolypropylenes, and mixtures of two or more of these. From the viewpoint of seal strength, the resin composition constituting the third layer preferably contains a propylene-ethylene block copolymer, and from the viewpoint of low-temperature sealability, preferably contains a propylene-ethylene random copolymer.
[0087] In the resin composition constituting the third layer, the polypropylene content is preferably 51% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, which can further improve the heat resistance and oil resistance of the resin film.
[0088] In the resin film of the present invention, the difference between the polypropylene content in the resin film constituting the third layer and the polypropylene content in the resin film constituting the first layer is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, which can further reduce curling of the resin film.
[0089] The resin composition constituting the third layer may contain polyethylene. This can improve the tearability of the resin film. When the resin composition constituting the first layer contains polyethylene, examples of the polyethylene include high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear low-density polyethylene, and mixtures of two or more of these.
[0090] When a mixture of polypropylene and polyethylene is used as the resin composition constituting the third layer, the resin composition constituting the third layer may have an island-in-a-sea structure, which can further improve the tearability of the resin film.
[0091] In the resin composition constituting the third layer, the polyethylene content is 35% by mass or less. This allows a resin film to have film-forming properties. The polyethylene content in the resin composition constituting the third layer is preferably 1% by mass or more and 30% by mass or less, and more preferably 5% by mass or more and 25% by mass or less. This allows the tearability of the resin film to be improved.
[0092] The polyethylene of the resin composition constituting the third layer may be fossil fuel polyethylene, biomass polyethylene, or a combination thereof. From the viewpoint of reducing the environmental load, the resin composition constituting the third layer preferably contains biomass polyethylene.
[0093] When the third layer constitutes the outermost layer of the resin film, the biomass degree of the resin composition constituting the third layer is preferably 30% or less. Resins obtained from raw materials derived from biomass have a higher proportion of low molecular weight components than resins obtained from raw materials derived from fossil fuels, and these low molecular weight components may affect adhesion with other layers. By setting the biomass degree of the resin composition constituting the third layer to 30% or less, it is possible to reduce the influence on adhesion with other layers. From the viewpoint of reducing environmental load and adhesion, the biomass degree of the resin composition constituting the third layer is preferably 1% or more and 25% or less, and more preferably 5% or more and 20% or less.
[0094] The resin composition constituting the third layer preferably has a melt flow rate (MFR) of 1 g / 10 min to 30 g / 10 min, more preferably 3 g / 10 min to 25 g / 10 min, and even more preferably 5 g / 10 min to 20 g / 10 min. If the MFR of the resin composition constituting the third layer is 1 g / 10 min or more, the extrusion load during molding can be reduced. If the MFR of the resin composition constituting the third layer is 30 g / 10 min or less, the mechanical strength of the resin film can be increased.
[0095] The thickness of the third layer is preferably 5 μm or more and 100 μm or less, more preferably 5 μm or more and 80 μm or less, and even more preferably 10 μm or more and 50 μm or less. This can further improve the adhesion to other layers. The third layer may be composed of two or more layers.
[0096] As long as the properties of the present invention are not impaired, the resin composition constituting the third layer may contain one or more additives, such as antioxidants, antiblocking agents, lubricants, fillers, plasticizers, antistatic agents, UV absorbers, inorganic particles, organic particles, release agents, and dispersants.
[0097] (thermoplastic resin layer) The thermoplastic resin layer is a layer formed to bond any two layers together by lamination. The thermoplastic resin layer can be formed by a conventionally known method, for example, a melt extrusion lamination method or a sand lamination method. The material of the thermoplastic resin layer can be a polyolefin resin such as a polyethylene resin or a polypropylene resin, or a cyclic polyolefin resin, or a copolymer resin, modified resin, or mixture (including alloy) containing these resins as main components. Examples of polyolefin resins include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-α-olefin copolymers polymerized using a metallocene catalyst, random or block copolymers of ethylene-polypropylene, ethylene-vinyl acetate copolymers (EVA), ethylene-acrylic acid copolymers (EAA), ethylene-ethyl acrylate copolymers (EEA), ethylene-methacrylic acid copolymers (EMAA), ethylene-methyl methacrylate copolymers (EMMA), ethylene-maleic acid copolymers, ionomer resins, and acid-modified polyolefin resins obtained by modifying the above-mentioned polyolefin resins with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, and itaconic acid in order to improve adhesion between layers. In addition, resins obtained by graft-polymerizing or copolymerizing unsaturated carboxylic acids, unsaturated carboxylic anhydrides, and ester monomers with polyolefin resins can be used. These materials can be used alone or in combination of two or more. Examples of the cyclic polyolefin resin that can be used include cyclic polyolefins such as ethylene-propylene copolymers, polymethylpentene, polybutene, polynorbornene, etc. These resins can be used alone or in combination.
[0098] The thermoplastic resin layer may contain a resin obtained from a raw material derived from biomass, or may contain a resin obtained from a raw material derived from a fossil fuel.
[0099] (Method of manufacturing resin film) The method for producing the resin film of the present invention is not particularly limited, and can be produced by a conventionally known method. The resin film is preferably produced by co-extrusion molding, and the co-extrusion molding is more preferably carried out by a T-die method or an inflation method. Hereinafter, an example of the method for producing the resin film by the T-die method and the inflation method will be described.
[0100] In the T-die method, the raw materials of the resin composition constituting the first layer and the raw materials of the resin composition constituting the second layer are each dried, and then supplied to a melt extruder heated to a temperature (Tm) above their melting points to a temperature of Tm+70°C to melt them and co-extrude them into a sheet from a T-die. The co-extruded sheet is then quenched and solidified on a rotating cooling drum or the like to form a resin film. As the melt extruder, a single screw extruder, a twin screw extruder, a vent extruder, a tandem extruder, etc. can be used depending on the purpose.
[0101] In the inflation method, first, the raw material of the resin composition constituting the first layer and the raw material of the resin composition constituting the second layer are dried, and then fed into a melt extruder heated to a temperature (Tm) to Tm+70°C above their melting points, respectively, to melt them, and co-extrude them into a cylindrical shape through a ring die. At this time, air is fed from below into the cylindrical molten resin to expand the diameter of the cylinder to a predetermined size, and cooling air is fed from below to the outside of the cylinder. This expanded cylindrical body is called a bubble. Next, the bubble is folded into a film shape by a guide plate and a pinch roll, and wound up in a winding section. The folded film may be wound up as it is in a cylindrical shape, or both ends of the cylinder may be removed by a slitter or the like, cut into two films, and then each may be wound up. In this way, a resin film can be formed. As the melt extruder, a single screw extruder, a twin screw extruder, a vent extruder, a tandem extruder, etc. can be used depending on the purpose.
[0102] Laminate Next, the laminate 20 of the present invention will be described. The laminate 20 includes at least one biaxially stretched plastic film and the above-mentioned resin film 10. By including the above-mentioned resin film 10, the laminate can have a reduced environmental load, as well as a sealability and excellent tearability.
[0103] Fig. 7 is a cross-sectional view showing an example of a laminate 20 of the present invention. As shown in Fig. 7, the laminate 20 includes, in this order, a first biaxially stretched plastic film 21, a printed layer 22, a first adhesive layer 23, and the resin film 10. The first biaxially stretched plastic film 21 constitutes an outer surface 20y of the laminate 20, and the resin film 10 constitutes an inner surface 20x.
[0104] Fig. 8 is a cross-sectional view showing an example of the laminate 20 of the present invention. As shown in Fig. 8, the laminate 20 includes, in this order, a first biaxially oriented plastic film 21, a printed layer 22, a first adhesive layer 23, a second biaxially oriented plastic film 24, a second adhesive layer 25, and the resin film 10. The first biaxially oriented plastic film 21 constitutes an outer surface 20y of the laminate 20, and the resin film 10 constitutes an inner surface 20x.
[0105] Fig. 9 is a cross-sectional view showing another example of the laminate 20 of the present invention. As shown in Fig. 9, the laminate 20 includes, in this order, a first biaxially oriented plastic film 21, a printed layer 22, a first adhesive layer 23, a metal foil 26, a second adhesive layer 25, and the resin film 10. The first biaxially oriented plastic film 21 constitutes an outer surface 20y of the laminate 20, and the resin film 10 constitutes an inner surface 20x.
[0106] Fig. 10 is a cross-sectional view showing another example of the laminate 20 of the present invention. As shown in Fig. 4, the laminate 20 includes, in this order, a first biaxially stretched plastic film 21, a printed layer 22, a first adhesive layer 23, a vapor deposition layer 27, a second biaxially stretched plastic film 24, a second adhesive layer 25, and the resin film 10. The first biaxially stretched plastic film 21 constitutes an outer surface 20y of the laminate 20, and the resin film 10 constitutes an inner surface 20x.
[0107] Fig. 11 is a cross-sectional view showing another example of the laminate 20 of the present invention. As shown in Fig. 5, the laminate 20 includes, in this order, a first biaxially stretched plastic film 21, a printed layer 22, a first anchor coat layer 28, a first adhesive resin layer 29, a vapor deposition layer 27, a second biaxially stretched plastic film 24, a second anchor coat layer 30, a second adhesive resin layer 31, and the resin film 10. The first biaxially stretched plastic film 21 constitutes an outer surface 20y of the laminate 20, and the resin film 10 constitutes an inner surface 20x.
[0108] Below, the first biaxially oriented plastic film 21, the second biaxially oriented plastic film 24, the printed layer 22, the metal foil 26, the vapor deposition layer 27, the first adhesive layer 23, the second adhesive layer 25, the first anchor coat layer 28, the second anchor coat layer 30, the first adhesive resin layer 29, and the second adhesive resin layer 31 will each be described in detail.
[0109] (First biaxially oriented plastic film and second biaxially oriented plastic film) Examples of resin materials constituting the first biaxially oriented plastic film and the second biaxially oriented plastic film include polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), 1,4-polycyclohexylene dimethylene terephthalate, and terephthalic acid-cyclohexanedimethanol-ethylene glycol copolymers; polyamides such as nylon 6 and nylon 6,6; polyolefins such as polyethylene, polypropylene, and polymethylpentene; vinyl resins such as polyvinyl chloride, polyvinyl alcohol (PVA), polyvinyl acetate, vinyl chloride-vinyl acetate copolymers, polyvinyl butyral, and polyvinylpyrrolidone (PVP); (meth)acrylic resins such as polyacrylate, polymethacrylate, and polymethyl methacrylate; cellulose resins such as cellophane, cellulose acetate, nitrocellulose, cellulose acetate propionate (CAP), and cellulose acetate butyrate (CAB); styrene resins such as polystyrene (PS), and chlorinated resins thereof. Among these, polyolefins, polyesters and polyamides are preferred, and polypropylene, polyethylene terephthalate, nylon 6 and nylon 6,6 are more preferred. In the present invention, "(meth)acrylic" means to include both "acrylic" and "methacrylic", and "(meth)acrylate" means to include both "acrylate" and "methacrylate".
[0110] As long as the properties of the present invention are not impaired, the first biaxially oriented plastic film and the second biaxially oriented plastic film may contain additives such as fillers, plasticizers, antistatic agents, UV absorbers, inorganic particles, organic particles, release agents and dispersants.
[0111] (Printing layer) The printing layer is a layer printed on the first biaxially oriented plastic film to provide product information and aesthetic appeal to the bag. The printing layer expresses letters, numbers, symbols, figures, pictures, etc. Gravure printing inks and flexographic printing inks can be used as materials for the printing layer.
[0112] The ink constituting the printing layer contains a binder and a pigment. The binder contains, for example, polyurethane, as in the first adhesive layer and the second adhesive layer. Polyurethane is a cured product produced by reacting a polyol as a base agent with an isocyanate compound as a curing agent. Details of the polyol and the isocyanate compound will be described in the paragraphs on the first adhesive layer and the second adhesive layer.
[0113] The pigment of the printing layer is a colored powder and exists in the binder at a predetermined distribution density. The color of the pigment is not particularly limited, and various pigments such as red, blue, green, white, and black can be used. For example, the average particle size of the pigment may be 0.1 μm or more and 1 μm or less, or 0.5 μm or more and 1 μm or less. Note that white pigments generally have larger dimensions than pigments of other colors. For example, the average particle size of white pigments is 0.5 μm or more and 1 μm or less. The average particle size of the pigment can be measured by a dynamic light scattering method.
[0114] The printing layer may be composed of a single layer, or may include multiple layers. For example, the printing layer may include a first layer containing a pigment that exhibits a first color, and a second layer containing a pigment that exhibits a second color different from the first color. The thickness of one layer of the printing layer is, for example, 0.5 μm or more and 3 μm or less.
[0115] (Metal foil) As the metal foil, a conventionally known metal foil can be used. From the viewpoints of gas barrier properties that prevent the transmission of oxygen gas, water vapor, etc., and light blocking properties that prevent the transmission of visible light, ultraviolet light, etc., aluminum foil is preferred. The thickness of the metal foil is, for example, 5 μm or more and 15 μm or less.
[0116] (deposited layer) The vapor-deposited layer is a layer provided to enhance the gas barrier properties of the bag. The vapor-deposited layer comprises a vapor-deposited film of one or more inorganic substances or inorganic oxides, such as silicon (Si), aluminum (Al), magnesium (Mg), calcium (Ca), potassium (K), tin (Sn), sodium (Na), boron (B), titanium (Ti), lead (Pb), zirconium (Zr), and yttrium (Y). The vapor-deposited layer may comprise one or more vapor-deposited films.
[0117] The vapor-deposited film can be formed by vapor-depositing the inorganic substance or inorganic oxide on one side of a film such as the biaxially stretched plastic film. Examples of the method for forming the vapor-deposited film include known methods such as vacuum vapor deposition, sputtering, and chemical vapor deposition.
[0118] The thickness of the evaporated film of the inorganic substance or inorganic oxide is 100 Å to 2000 Å, preferably 200 Å to 1000 Å.
[0119] In order to improve the gas barrier property of the vapor deposition layer, a gas barrier coating film may be provided on the vapor deposition film of the inorganic substance and inorganic oxide as described above. The gas barrier coating film is a compound represented by the general formula R 1 n M(OR 2 ) m (In the formula, R 1 , R 2 represents an organic group having 1 to 8 carbon atoms, M represents a metal atom, n represents an integer of 0 or more, m represents an integer of 1 or more, and n+m represents the atomic valence of M. The transparent gas barrier composition contains at least one alkoxide represented by the formula (I) and the above-mentioned polyvinyl alcohol resin and / or ethylene-vinyl alcohol copolymer, and is further polycondensed by a sol-gel method in the presence of a sol-gel catalyst, an acid, water, and an organic solvent.
[0120] (First Adhesive Layer and Second Adhesive Layer) The adhesive layers, such as the first adhesive layer and the second adhesive layer, contain an adhesive for bonding a first biaxially oriented plastic film, a second biaxially oriented plastic film, and the like to each other. The adhesive constituting the adhesive layer is produced from an adhesive composition produced by mixing a first composition containing a base agent and a solvent with a second composition containing a curing agent and a solvent. Specifically, the adhesive contains a cured product produced by the reaction of the base agent and the solvent in the adhesive composition.
[0121] Examples of adhesives include ether-based two-liquid reactive adhesives and ester-based two-liquid reactive adhesives. Examples of ether-based two-liquid reactive adhesives include polyether polyurethane. Polyether polyurethane is a cured product produced by reacting a polyether polyol as a base agent with an isocyanate compound as a curing agent. Examples of ester-based two-liquid reactive adhesives include polyester polyurethane and polyester. Polyester polyurethane is a cured product produced by reacting a polyester polyol as a base agent with an isocyanate compound as a curing agent.
[0122] As isocyanate compounds that react with polyols such as polyether polyols and polyester polyols to produce a cured product, there are aromatic isocyanate compounds and aliphatic isocyanate compounds. Among these, aromatic isocyanate compounds dissolve components that cannot be used for food applications under high temperature environments such as during heat sterilization (retort processing). Meanwhile, the adhesive layer is in contact with the resin film 10 that constitutes the inner surface 20x of the laminate 20, as shown in Figs. 7 to 11. Therefore, when the adhesive layer contains an aromatic isocyanate compound, the components dissolved from the aromatic isocyanate compound may adhere to the contents of the bag 40 formed by the laminate 20.
[0123] Considering these problems, the adhesive that constitutes the adhesive layer is a cured product produced by reacting a polyol as the base agent with an aliphatic isocyanate compound as the curing agent. This makes it possible to prevent the adhesive layer from causing components that cannot be used for food applications from adhering to the contents. Examples of aliphatic isocyanates include hexamethylene diisocyanate (HDI) and isophorone diisocyanate (IPDI).
[0124] In addition, the drop impact resistance can be improved by increasing the molar ratio of the isocyanate group of the aliphatic isocyanate compound to the hydroxy group of the polyol. For example, the molar ratio of the curing agent (aliphatic isocyanate compound) to the hydroxy group of the base agent (polyol) is conventionally about 3. In this embodiment, the molar ratio of the isocyanate group of the aliphatic isocyanate compound to the hydroxy group of the polyol is preferably 3.5 or more, more preferably 4 or more, and even more preferably 4.5 or more. More preferably, the molar ratio of the isocyanate group of the aliphatic isocyanate compound to the hydroxy group of the polyol is greater than 5.
[0125] On the other hand, aliphatic isocyanate compounds are expensive, and increasing the amount of aliphatic isocyanate compounds is not preferable in terms of production costs. Also, the higher the molar ratio of the isocyanate groups of the aliphatic isocyanate compounds to the hydroxyl groups of the polyol, the higher the temperature or the longer the time required to cure the adhesive composition. In consideration of these points, the molar ratio of the aliphatic isocyanate groups to the hydroxyl groups is preferably 7 or less, more preferably 6 or less.
[0126] The adhesive layer is formed by applying an adhesive composition to a first biaxially oriented plastic film, a second biaxially oriented plastic film, a metal foil, or a resin film, and then drying the adhesive composition and curing the adhesive composition through a reaction between the main agent and the solvent in the adhesive composition. In this embodiment, the weight per unit area of the adhesive composition after drying is, for example, 2 g / m 2 More than 5g / m 2 It is preferable that the density is 3 g / m or less. 2 More than 4g / m 2 The thickness of the adhesive layer 60 is preferably 2 μm or more and 5 μm or less, and more preferably 3 μm or more and 4 μm or less.
[0127] (First adhesive resin layer and second adhesive resin layer) The adhesive resin layers, such as the first adhesive resin layer and the second adhesive resin layer, contain a thermoplastic resin for bonding the first biaxially oriented plastic film, the second biaxially oriented plastic film, etc. to each other. The adhesive resin layer is formed by a melt extrusion lamination method using a thermoplastic resin. The thermoplastic resin that can be used for the adhesive resin layer can be the same as the material for the thermoplastic resin layer described above.
[0128] (First anchor coat layer and second anchor coat layer) The anchor coat layers, such as the first anchor coat layer and the second anchor coat layer, are formed to improve the adhesion of the adhesive resin layer. The anchor coat layer can be formed by applying an anchor coat agent to the surface of the layer to be laminated and drying it. The anchor coat agent can be any resin with a heat resistance temperature of 135°C or higher, such as an anchor coat agent made of vinyl modified resin, epoxy resin, urethane resin, polyester resin, etc., and in particular, an anchor coat agent made of a polyacrylic or polymethacrylic resin having two or more hydroxyl groups in the structure and an isocyanate compound as a curing agent can be preferably used. In addition, a silane coupling agent may be used in combination with this as an additive, and nitrocellulose may be used in combination to improve heat resistance.
[0129] (Specific examples of layer structure of laminate) Specific examples of the laminate 20 shown in Figs. 7 to 11 are shown below. Note that " / " represents the boundary between layers. The leftmost layer is the layer that constitutes the outer surface 20y of the laminate 20, and the rightmost layer is the layer that constitutes the inner surface 20x of the laminate 20. In addition, "biaxially oriented PET film" means a biaxially oriented polyethylene terephthalate film, "biaxially oriented PP film" means a biaxially oriented polypropylene film, and "AC" means an anchor coat layer. (1) Biaxially oriented PET film / printing layer / adhesive layer / resin film (2) Biaxially oriented PET film / printing layer / adhesive layer / biaxially oriented nylon film / adhesive layer / resin film (3) Biaxially oriented PET film / printing layer / adhesive layer / biaxially oriented PET film / adhesive layer / resin film (4) Biaxially oriented PET film / printed layer / adhesive layer / metal foil / adhesive layer / resin film (5) Biaxially oriented PET film / printed layer / adhesive layer / vapor deposition layer / biaxially oriented PET film / adhesive layer / resin film (6) Biaxially oriented polypropylene film / printed layer / AC / adhesive resin layer / vapor deposition layer / biaxially oriented PET film / AC / adhesive resin layer / resin film
[0130] (Method of manufacturing laminate) The method for producing the laminate is not particularly limited, and the laminate can be produced by a conventionally known method such as a dry lamination method, a melt extrusion lamination method, or a sand lamination method.
[0131] bag Next, the bag 40 of the present invention will be described. Fig. 12 is a front view showing the bag 40 according to this embodiment. The bag 40 includes a storage section 40a for storing contents. The configuration of the bag 40 will be described below.
[0132] Bag 40 includes an upper portion 41, a lower portion 42, and a side portion 43, and has a generally rectangular outline in a front view. Note that names such as "upper portion," "lower portion," and "side portion," as well as terms such as "above" and "below," merely indicate the relative positions and directions of bag 40 and its components. The position, etc., of bag 40 during transportation or use is not limited by the names and terms used in this specification.
[0133] 12, the bag 40 includes a surface film 44 constituting the surface and a back film 45 constituting the back surface. The surface film 44 and the back film 45 are each composed of the laminate 20 described above.
[0134] The above-mentioned terms "front film" and "back film" merely divide the films according to their positional relationships, and the above-mentioned terms do not limit the method of providing the films when manufacturing bag 40. For example, bag 40 may be manufactured using a single film in which front film 44 and back film 45 are continuously provided.
[0135] The inner surfaces of the front film 44 and the back film 45 are joined together by a sealed portion. In the front view of the bag 40 shown in Figure 12, the sealed portion is hatched.
[0136] As shown in Fig. 12, the sealed portion has an outer edge sealed portion that extends along the outer edge of the bag 40. The outer edge sealed portion includes an upper sealed portion 41a that extends along the upper portion 41, a lower sealed portion 42a that spreads over the lower portion 42, and a pair of side sealed portions 43a that extend along a pair of side portions 43. Note that, in the bag 40 before it is filled with the contents (a state in which the contents are not filled), an opening (not shown) is formed in the upper portion 41 of the bag 40. Then, after the contents are placed in the bag 40, the inner surface of the front film 44 and the inner surface of the back film 45 are joined at the upper portion 41 to form the upper sealed portion 41a and seal the bag 40.
[0137] The upper seal portion 41 a, the lower seal portion 42 a and the side seal portion 43 a are seal portions formed by joining the inner surface of the front film 44 and the inner surface of the back film 45 together.
[0138] There are no particular limitations on the method for forming the sealed portion, so long as it is possible to join opposing films together and seal bag 40. For example, the sealed portion may be formed by melting the inner surfaces of the films by heating or the like and fusing the inner surfaces together, i.e., by heat sealing.
[0139] (Easy-to-open means) The front film 44 and the back film 45 may be provided with easy-open means 47 for tearing the front film 44 and the back film 45 to open the bag 40. For example, as shown in Fig. 12, the easy-open means 46 may include a notch 47 that serves as a starting point for tearing and is formed in the side seal portion 43a of the bag 40. Also, a half-cut line formed by laser processing, a cutter, or the like may be provided as the easy-open means 46 in a portion that serves as a path for tearing the bag 40.
[0140] Although not shown, the easy-open means 46 may include a group of cuts or scars formed in the area where the seal portion is formed in the front film 44 and the back film 45. The group of scars may include, for example, a plurality of through holes formed so as to penetrate the front film 44 and / or the back film 45. Alternatively, the group of scars may include a plurality of holes formed on the outer surface of the front film 44 and / or the back film 45 so as not to penetrate the front film 44 and / or the back film 45.
[0141] (Bag manufacturing method) First, a surface film 44 and a back film 45 made of the laminate 20 described above are prepared. Then, the inner surfaces of the films are heat-sealed to form seals such as a bottom seal 42a and a side seal 43a. The films joined together by heat sealing are cut into an appropriate shape to obtain a bag 40 as shown in FIG. 12. Next, the bag 40 is filled with contents through an opening (not shown) in the upper part 41. The contents are, for example, chocolate. After that, the upper part 41 is heat-sealed to form an upper seal 41a. In this manner, a bag 40 containing and sealed with contents can be obtained.
[0142] Other Aspects Another aspect of the present invention is a resin film having at least two layers, a first layer and a second layer, the first layer and the second layer being laminated directly or via a thermoplastic resin layer, the first layer constituting the innermost layer of the resin film, the resin film comprising polypropylene and polyethylene, the resin composition constituting the first layer containing polypropylene as a main component, the polyethylene content of the first layer being 20 mass% or less, and the resin composition constituting the second layer containing polypropylene as a main component and biomass polyethylene, the polyethylene content of the second layer being 35 mass% or less. In a resin film according to another aspect of the present invention, the resin film further comprises a third layer, the third layer being laminated to the second layer directly or via a thermoplastic resin layer, the resin composition constituting the third layer containing polypropylene as a main component, and the polyethylene content of the third layer may be 35 mass% or less. In the resin film according to another embodiment of the present invention, the biomass ratio may be 5% or more. In the resin film according to another embodiment of the present invention, the layer constituting the outermost layer of the resin film may have a biomass degree of 30% or less. In the resin film according to another embodiment of the present invention, the polypropylene content may be 66% by mass or more. In the resin film according to another embodiment of the present invention, the breaking elongation in one direction and in another direction perpendicular to the one direction may each be 500% or more. Another aspect of the invention is a laminate comprising at least one biaxially oriented plastic film and a resin film according to another aspect of the invention. Another aspect of the invention is a bag comprising a laminate according to another aspect of the invention. EXAMPLES
[0143] Next, the present invention will be described more specifically with reference to examples. However, the present invention is not limited to the description of the following examples as long as it does not depart from the gist of the present invention.
[0144] [Example 1-1] As the raw material of the resin composition constituting the first layer, a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 (Biomass content: 0%) was melted. Next, as a raw material for the resin composition constituting the second layer, 85 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3, biomass content: 0%), and 15 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 (biomass content: 87%) was melted separately. These melts were co-extruded through a T-die to produce an unstretched resin film with a layer thickness ratio of 1:4 (first layer:second layer) and a thickness of 50 μm. The polypropylene content in the resin film was 88 mass %, and the biomass ratio of the resin film was 10%.
[0145] Next, a biaxially oriented polyethylene terephthalate film having a thickness of 12 μm (manufactured by Toyobo Co., Ltd., product name: E5100) was prepared as the first biaxially oriented plastic film 21. Then, a printed layer 22 was formed on this first biaxially oriented plastic film 21. The printed layer 22 had a thickness of 1.0 μm. In addition, a biaxially oriented polyethylene terephthalate film having a thickness of 12 μm (manufactured by Toyobo Co., Ltd., product name: E5100) was prepared as the second biaxially oriented plastic film 24.
[0146] Next, the first biaxially oriented plastic film 21, the print layer 22, the first adhesive layer 23, the second biaxially oriented plastic film 24, the second adhesive layer 25, and the resin film 10 were laminated in this order by dry lamination to produce the laminate 20 shown in FIG. 8. As the first adhesive layer 23 and the second adhesive layer 25, a two-liquid polyurethane adhesive (main agent: RU-40, hardener: H-4) manufactured by Rock Paint Co., Ltd. was used. The main agent RU-40 is polyester polyol. The thicknesses of the first adhesive layer 23 and the second adhesive layer 25 were each 3.0 μm. In the laminate 20, the first layer of the resin film 10 constitutes the innermost layer.
[0147] Next, the bag 40 shown in Fig. 12 was produced. Specifically, first, a front surface film 44 and a back surface film 45 were produced from the obtained laminate 20. Next, the front surface film 44 and the back surface film 45 were overlapped such that the resin film 10 of the front surface film 44 and the resin film 10 of the back surface film 45 were in contact with each other.
[0148] Then, an upper sealed portion 41a, a lower sealed portion 42a, and a side sealed portion 43a were formed by heat sealing according to the shape of each bag 40. The heat sealing was performed under the following conditions. (Heat seal conditions) Heat sealing device: Heat sealer (Tester Sangyo Co., Ltd., product name: TP-701-A) Heat seal temperature: 200℃, 190℃, 180℃, 170℃, 160℃, 150℃ Heat seal pressure: 0.1MPa Heat seal time: 1 second
[0149] Next, the heat-sealed area was cut to match the shape of each bag 40, thereby producing the bags 40 shown in Fig. 14. Furthermore, in the produced bags 40, notches 47 were formed as easy-open means 46.
[0150] The produced bag 40 had a height S1 (see FIG. 12) of 140 mm, a width S2 of 120 mm, and widths S3 of upper sealed portion 41a, S4 of lower sealed portion 42a and S5 of side sealed portion 43a of 5.0 mm.
[0151] [Example 1-2] As the raw material of the resin composition constituting the second layer, 80 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 20 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 A resin film was produced in the same manner as in Example 1-1, except that a polypropylene film having a biomass ratio of 87% was used. The layer thickness ratio was 1:4 (first layer:second layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 84 mass%, and the biomass ratio of the resin film was 14%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 1-1.
[0152] [Examples 1-3] As the raw material of the resin composition constituting the second layer, 70 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 30 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 A resin film was produced in the same manner as in Example 1-1, except that a polypropylene film having a biomass ratio of 87% was used. The layer thickness ratio was 1:4 (first layer:second layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 76 mass%, and the biomass ratio of the resin film was 21%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 1-1.
[0153] [Examples 1-4] As the raw material of the resin composition constituting the first layer, 90 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 10 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 The raw material for the resin composition constituting the second layer was 70 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 30 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3A resin film was produced in the same manner as in Example 1-1, except that a polypropylene film having a biomass ratio of 87% was used. The layer thickness ratio was 1:4 (first layer:second layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 74 mass%, and the biomass ratio of the resin film was 23%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 1-1.
[0154] [Examples 1-5] As the raw material of the resin composition constituting the second layer, 85 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%), and 15 parts by mass of biomass low-density polyethylene (manufactured by Braskem, product name: SEB-853, MFR: 2.7 g / 10 min, density: 923 kg / m 3 A resin film was produced in the same manner as in Example 1-1, except that a polypropylene film having a biomass ratio of 95% was used. The layer thickness ratio was 1:4 (first layer:second layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 88% by mass, and the biomass ratio of the resin film was 11%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 1-1.
[0155] [Examples 1-6] As the raw material of the resin composition constituting the second layer, 70 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%), and 30 parts by mass of biomass low-density polyethylene (manufactured by Braskem, product name: SEB-853, MFR: 2.7 g / 10 min, density: 923 kg / m 3A resin film was produced in the same manner as in Example 1-1, except that a polypropylene film having a biomass ratio of 95% was used. The layer thickness ratio was 1:4 (first layer:second layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 76 mass%, and the biomass ratio of the resin film was 23%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 1-1.
[0156] [Examples 1-7] The raw materials for the resin composition constituting the second layer were 70 parts by mass of a propylene-ethylene block copolymer (manufactured by Prime Polymer Co., Ltd., product name: J715M, MFR: 9.0 g / 10 min, biomass content: 0%) and 30 parts by mass of a biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 A resin film was produced in the same manner as in Example 1-1, except that a polypropylene film having a biomass ratio of 87% was used. The layer thickness ratio was 1:4 (first layer:second layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 76% by mass, and the biomass ratio of the resin film was 21%. The configuration of the resin film of this example is shown in Table 1. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 1-1.
[0157] [Comparative Example 1-1] Propylene-ethylene random copolymer (Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 (biomass content: 0%) was melted, and the melt was extruded through a T-die to produce an unstretched resin film with a thickness of 50 μm. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 1-1.
[0158] [Comparative Example 1-2] Only the propylene-ethylene block copolymer (manufactured by Prime Polymer Co., Ltd., product name: J715M, MFR: 9.0 g / 10 min, biomass content: 0%) was melted, and the melt was extruded through a T-die to produce an unstretched resin film with a thickness of 50 μm. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 1-1.
[0159] [Comparative Example 1-3] As the raw material of the resin composition constituting the first layer, 70 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 30 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 The raw material for the resin composition constituting the second layer was 70 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 30 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 A resin film was produced in the same manner as in Example 1-1, except that a polypropylene film having a biomass ratio of 87% was used. The layer thickness ratio was 1:4 (first layer:second layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 70 mass%, and the biomass ratio of the resin film was 26%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 1-1.
[0160] [Comparative Example 1-4] As the raw material of the resin composition constituting the first layer, a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m3 (Biomass content: 0%) was melted. Next, as a raw material for the resin composition constituting the second layer, 60 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 40 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 (biomass content: 87%) was melted separately. These melts were co-extruded using a T-die, but the resin composition could not be formed into a film.
[0161] Details of each layer and the resin film in Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-4 are shown in Tables 1 and 2. In Table 1, "petroleum-based random PP" means propylene-ethylene random copolymer, "petroleum-based block PP" means propylene-ethylene block copolymer, "bio-LLDPE" means biomass linear low-density polyethylene, and "bio-LDPE" means biomass low-density polyethylene. The contents in Tables 1 and 2 are all based on mass.
[0162] [Table 1]
[0163] [Table 2]
[0164] [Example 2-1] As the raw material of the resin composition constituting the first layer, a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 (Biomass content: 0%) was melted. Next, as a raw material for the resin composition constituting the second layer, 80 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 20 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 (biomass content: 87%) was melted separately. Next, as the raw material of the resin composition constituting the third layer, a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 (biomass content: 0%) was melted separately. These melts were co-extruded through a T-die to produce an unstretched resin film with a layer thickness ratio of 1:3:1 (first layer: second layer: third layer) and a thickness of 50 μm. The polypropylene content in the resin film was 88 mass %, and the biomass ratio of the resin film was 10%.
[0165] Next, a biaxially oriented polyethylene terephthalate film having a thickness of 12 μm (manufactured by Toyobo Co., Ltd., product name: E5100) was prepared as the first biaxially oriented plastic film 21. Then, a printed layer 22 was formed on this first biaxially oriented plastic film 21. The printed layer 22 had a thickness of 1.0 μm. In addition, a biaxially oriented polyethylene terephthalate film having a thickness of 12 μm (manufactured by Toyobo Co., Ltd., product name: E5100) was prepared as the second biaxially oriented plastic film 24.
[0166] Next, the first biaxially oriented plastic film 21, the print layer 22, the first adhesive layer 23, the second biaxially oriented plastic film 24, the second adhesive layer 25, and the resin film 10 were laminated in this order by dry lamination to produce the laminate 20 shown in FIG. 8. As the first adhesive layer 23 and the second adhesive layer 25, a two-liquid polyurethane adhesive (main agent: RU-40, hardener: H-4) manufactured by Rock Paint Co., Ltd. was used. The main agent RU-40 is polyester polyol. The thicknesses of the first adhesive layer 23 and the second adhesive layer 25 were each 3.0 μm. In the laminate 20, the first layer of the resin film 10 constitutes the innermost layer.
[0167] Next, the bag 40 shown in Fig. 12 was produced. Specifically, first, a front surface film 44 and a back surface film 45 were produced from the obtained laminate 20. Next, the front surface film 44 and the back surface film 45 were overlapped such that the resin film 10 of the front surface film 44 and the resin film 10 of the back surface film 45 were in contact with each other.
[0168] Then, an upper sealed portion 41a, a lower sealed portion 42a, and a side sealed portion 43a were formed by heat sealing according to the shape of each bag 40. The heat sealing was performed under the following conditions. (Heat seal conditions) Heat sealing device: Heat sealer (Tester Sangyo Co., Ltd., product name: TP-701-A) Heat seal temperature: 200℃, 190℃, 180℃, 170℃, 160℃, 150℃ Heat seal pressure: 0.1MPa Heat seal time: 1 second
[0169] Next, the heat-sealed area was cut to match the shape of each bag 40, thereby producing the bags 40 shown in Fig. 14. Furthermore, in the produced bags 40, notches 47 were formed as easy-open means 46.
[0170] The produced bag 40 had a height S1 (see FIG. 12) of 140 mm, a width S2 of 120 mm, and widths S3 of upper sealed portion 41a, S4 of lower sealed portion 42a and S5 of side sealed portion 43a of 5.0 mm.
[0171] [Example 2-2] As the raw material of the resin composition constituting the second layer, 70 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 30 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 A resin film was produced in the same manner as in Example 2-1, except that polypropylene (1st layer: 2nd layer: 3rd layer) and biomass degree: 87% were used. The layer thickness ratio was 1:3:1 (1st layer: 2nd layer: 3rd layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 82 mass%, and the biomass degree of the resin film was 16%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 2-1.
[0172] [Example 2-3] As the raw material of the resin composition constituting the first layer, 90 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 10 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 The raw material for the resin composition constituting the second layer was 70 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3, biomass content: 0%) and 30 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 A resin film was produced in the same manner as in Example 2-1, except that a polypropylene film having a biomass ratio of 87% was used. The layer thickness ratio was 1:3:1 (first layer:second layer:third layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 80 mass %, and the biomass ratio of the resin film was 17%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 2-1.
[0173] [Example 2-4] As the raw material of the resin composition constituting the first layer, 90 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 10 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 The raw material for the resin composition constituting the second layer was 70 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 30 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 The raw material for the resin composition constituting the third layer was 80 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 20 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3A resin film was produced in the same manner as in Example 2-1, except that polypropylene was used (biomass ratio: 87%). The layer thickness ratio was 1:3:1 (first layer:second layer:third layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 76 mass%, and the biomass ratio of the resin film was 21%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 2-1.
[0174] [Example 2-5] As the raw material of the resin composition constituting the second layer, 80 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%), and 20 parts by mass of biomass low-density polyethylene (manufactured by Braskem, product name: SEB-853, MFR: 2.7 g / 10 min, density: 923 kg / m 3 A resin film was produced in the same manner as in Example 2-1, except that a polypropylene film having a biomass ratio of 95% was used. The layer thickness ratio was 1:3:1 (first layer:second layer:third layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 88% by mass, and the biomass ratio of the resin film was 11%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 2-1.
[0175] [Example 2-6] As the raw material of the resin composition constituting the second layer, 70 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%), and 30 parts by mass of biomass low-density polyethylene (manufactured by Braskem, product name: SEB-853, MFR: 2.7 g / 10 min, density: 923 kg / m 3A resin film was produced in the same manner as in Example 2-1, except that a polypropylene film having a biomass ratio of 95% was used. The layer thickness ratio was 1:3:1 (first layer:second layer:third layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 82% by mass, and the biomass ratio of the resin film was 17%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 2-1.
[0176] [Example 2-7] The raw material of the resin composition constituting the first layer was a propylene-ethylene block copolymer (manufactured by Prime Polymer Co., Ltd., product name: J715M, MFR: 9.0 g / 10 min, biomass ratio: 0%), and the raw material of the resin composition constituting the second layer was a mixture of 70 parts by mass of a propylene-ethylene block copolymer (manufactured by Prime Polymer Co., Ltd., product name: J715M, MFR: 9.0 g / 10 min, biomass ratio: 0%) and 30 parts by mass of a biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 A resin film was produced in the same manner as in Example 2-1, except that a propylene-ethylene block copolymer (manufactured by Prime Polymer Co., Ltd., product name: J715M, MFR: 9.0 g / 10 min, biomass degree: 0%) was used as the raw material for the resin composition constituting the third layer. The layer thickness ratio was 1:3:1 (first layer:second layer:third layer), and the thickness of the resin film was 50 μm. The polypropylene content of the resin film was 82 mass %, and the biomass degree in the resin film was 16%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 2-1.
[0177] [Comparative Example 2-1] Propylene-ethylene random copolymer (Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3The molten material was extruded through a T-die to produce an unstretched resin film with a thickness of 50 μm. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 2-1.
[0178] [Comparative Example 2-2] Only the propylene-ethylene block copolymer (manufactured by Prime Polymer Co., Ltd., product name: J715M, MFR: 9.0 g / 10 min, biomass content: 0%) was melted, and the melt was extruded through a T-die to produce an unstretched resin film with a thickness of 50 μm. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 2-1.
[0179] [Comparative Example 2-3] As the raw material of the resin composition constituting the first layer, 70 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 30 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 The raw material for the resin composition constituting the second layer was 70 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 30 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 A resin film was produced in the same manner as in Example 2-1, except that polypropylene was used (biomass ratio: 87%). The layer thickness ratio was 1:3:1 (first layer:second layer:third layer), and the thickness of the resin film was 50 μm. The polypropylene content in the resin film was 76 mass%, and the biomass ratio of the resin film was 21%. Moreover, using the obtained resin film, a laminate and a bag were produced in the same manner as in Example 2-1.
[0180] [Comparative Example 2-4] As the raw material of the resin composition constituting the first layer, a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 (Biomass content: 0%) was melted. Next, as a raw material for the resin composition constituting the second layer, 60 parts by mass of a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 , biomass content: 0%) and 40 parts by mass of biomass linear low-density polyethylene (manufactured by Braskem, product name: SLL-318, MFR: 2.7 g / 10 min, density: 918 kg / m 3 (biomass content: 87%) was melted separately. Next, as the raw material of the resin composition constituting the third layer, a propylene-ethylene random copolymer (manufactured by Prime Polymer Co., Ltd., product name: F219DA, MFR: 8.0 g / 10 min, density: 910 kg / m 3 (biomass content: 0%) was melted separately. These melts were co-extruded using a T-die, but the resin composition could not be formed into a film.
[0181] Details of each layer and the resin film in Examples 2-1 to 2-7 and Comparative Examples 2-1 to 2-4 are shown in Tables 3 and 4. In Table 3, "petroleum-based random PP" means propylene-ethylene random copolymer, "petroleum-based block PP" means propylene-ethylene block copolymer, "bio-LLDPE" means biomass linear low-density polyethylene, and "bio-LDPE" means biomass low-density polyethylene. The contents in Tables 3 and 4 are all based on mass.
[0182] [Table 3]
[0183] [Table 4]
[0184] <<Seal strength test>> A seal strength test was conducted using bags 40 according to Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-3, and Examples 2-1 to 2-7 and Comparative Examples 2-1 to 2-3, which had a heat seal temperature of 200° C. The seal strength was measured in accordance with JIS Z 0238:1998 under an environment of a temperature of 25° C. and a relative humidity of 50%, using a tensile tester SA-1150 manufactured by Orientec Co., Ltd. Specifically, as shown in FIG. 13, a rectangular test piece 50 was cut out having one side S6 of 15 mm and another side S7 extending in a direction perpendicular to the one side of 50 mm, so as to include the side seal portion 43a. Next, as shown in FIG. 14, the non-sealed portion of the front film 44 and the non-sealed portion of the back film 45 in the test piece 50 were arranged so that they were in the opposite directions in the direction perpendicular to the surface direction of the sealed portion, i.e., in a T-shape, and then the end of the non-sealed portion of the front film 44 and the end of the non-sealed portion of the back film 45 were fixed to the grippers 51 and 52, respectively. The chuck distance (S8) was set to 50 mm, and the grippers 51 and 52 were pulled at a speed of 300 mm / min in the opposite directions in the direction perpendicular to the surface direction of the sealed portion of the test piece 50, and the maximum value of the tensile stress was measured. This operation was performed five times in total using the test pieces 50 cut out from different bags 40, and the average value of the maximum value of the tensile stress five times was taken as the seal strength. The evaluation results are shown in Tables 5 and 6. (Evaluation Criteria) Good: The seal strength was 40N / 15mm or more. Pass: The seal strength was 20N / 15mm or more and less than 40N / 15mm. · Unacceptable: The seal strength was less than 20N / 15mm.
[0185] <<Low temperature sealability test>> A low-temperature sealability test was carried out using bags 40 according to Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-3, and Examples 2-1 to 2-7 and Comparative Examples 2-1 to 2-3, each of which had a heat seal temperature of 150°C, 160°C, 170°C, 180°C, and 190°C. In the low-temperature sealability test, similarly to the seal strength test, the seal strength was measured in an environment of a temperature of 25°C and a relative humidity of 50% in accordance with JIS Z 0238:1998, and a tensile tester SA-1150 manufactured by Orientec Co., Ltd. was used as the measuring instrument. Specifically, as shown in FIG. 13, a rectangular test piece 50 was cut out so as to include the side seal portion 43a, with one side S6 being 15 mm and the other side S7 extending in a direction perpendicular to the one side being 50 mm. Next, as shown in FIG. 14, the non-sealed portion of the front film 44 and the non-sealed portion of the back film 45 in the test piece 50 were arranged so that they were in the opposite directions in the direction perpendicular to the surface direction of the sealed portion, i.e., in a T-shape, and then the end of the non-sealed portion of the front film 44 and the end of the non-sealed portion of the back film 45 were fixed to the grippers 51 and 52, respectively. The chuck distance (S8) was set to 50 mm, and the grippers 51 and 52 were pulled at a speed of 300 mm / min in the opposite directions in the direction perpendicular to the surface direction of the sealed portion of the test piece 50, and the maximum value of the tensile stress was measured. This operation was performed five times in total using the test pieces 50 cut out from different bags 40, and the average value of the maximum value of the tensile stress five times was taken as the seal strength. The evaluation results are shown in Tables 5 and 6. (Evaluation Criteria) Good: For bags with a heat seal temperature of 150°C or higher, the seal strength was 20N / 15mm or higher. Pass: For bags with a heat seal temperature of 170°C or higher, the seal strength was 20N / 15mm or higher. - Unacceptable: The seal strength was less than 20N / 15mm when the bag was heat sealed at 190℃.
[0186] <<Tearability test>> A tear property test was conducted using bags 40 according to Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-3, and Examples 2-1 to 2-7 and Comparative Examples 2-1 to 2-3, all of which had a heat sealing temperature of 200° C. The tear property test was conducted by holding a sample of bag 40 of each Example and Comparative Example in the left hand so that notch 47 of bag 40 was on the left side and facing sideways, and tearing bag 40 by pulling it toward oneself with the right hand while keeping the left hand fixed. The evaluation results are shown in Tables 5 and 6. (Evaluation Criteria) Good: Bag 40 could be torn in a straight line. Acceptable: Although not in a straight line, bag 40 could be torn. · Unacceptable: Bag 40 could not be torn.
[0187] <<Film-forming evaluation>> The film-forming properties were evaluated based on whether or not a resin film could be formed in Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-4, as well as Examples 2-1 to 2-7 and Comparative Examples 2-1 to 2-4. The evaluation results are shown in Tables 5 and 6. (Evaluation Criteria) Good: The resin composition was formed into a film. · Unacceptable: The resin composition could not be made into a film.
[0188] [Table 5]
[0189] [Table 6]
[0190] As is clear from the above table, the resin film, laminate, and bag of the present invention have a reduced environmental impact, as well as excellent sealability, film-forming properties, and tearability. [Explanation of symbols]
[0191] 10 Resin film 11 1st layer 12 2nd layer 13 First thermoplastic resin layer 14 3rd layer 15 Second thermoplastic resin layer 20 Laminate 20x inner surface 20y external surface 21 First biaxially stretched plastic film 22 Printing layer 23 First adhesive layer 24 Second biaxially oriented plastic film 25 Second adhesive layer 26 Metal foil 27 Deposited layer 28 First Anchor Coat Layer 29 First adhesive resin layer 30 Second Anchor Coat Layer 31 Second adhesive resin layer 40 bags 40a Storage section 41 Top 41a Upper seal part 42 Lower 42a Lower seal part 43 Side 43a Side seal 44 Surface Film 45 Back film 46 Easy-to-open means 47 Notch 50 test pieces 51,52 Gripping tool
Claims
1. A resin film having at least a first layer, a second layer, and a third layer, The first layer and the second layer are laminated directly or via a thermoplastic resin layer, the third layer is laminated to the second layer directly or via a thermoplastic resin layer; the first layer constitutes an innermost layer of the resin film; The resin film contains polypropylene and polyethylene, The resin composition constituting the first layer contains polypropylene as a main component, The polyethylene content of the first layer is 20% by mass or less, The resin composition constituting the second layer contains polypropylene as a main component and biomass polyethylene, The polypropylene of the second layer is a propylene-ethylene random copolymer; The polyethylene content of the second layer is 5% by mass or more and 35% by mass or less, The resin composition constituting the third layer contains polypropylene as a main component, The third layer has a polyethylene content of 35% by mass or less, The thickness of the resin film is 15 μm or more and 250 μm or less, The resin film has a biomass ratio of 5% or more.
2. The resin film according to claim 1 , wherein the layer constituting the outermost layer of the resin film has a biomass degree of 30% or less.
3. The resin film according to claim 1 or 2, wherein the polypropylene content is 66 mass % or more.
4. The resin film according to claim 1 , wherein the resin film has a breaking elongation of 500% or more in one direction and in another direction perpendicular to the one direction.
5. A laminate comprising at least one biaxially stretched plastic film and the resin film according to any one of claims 1 to 4.
6. A bag comprising the laminate of claim 5.
Citation Information
Patent Citations
Stretched polypropylene film
JP2018065267A
Laminated film and food packaging bag
WO2018163835A1
Laminated film and food packaging bag
WO2018163836A1
Multilayer film and food-packaging bag
WO2019131168A1
Multilayer film and its laminate
JP2005335108A