Manufacturing method for chemically strengthened glass, and chemically strengthened glass

By chemically strengthening lithium aluminosilicate glass with a sodium-containing salt of low potassium content, the method addresses production efficiency and fracture issues, resulting in a glass with enhanced strength and weather resistance.

JP2024164238AInactive Publication Date: 2024-11-26AGC INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024146888
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-06-26
Filing Date
2024-08-28
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing chemically strengthened glass technologies face challenges in production efficiency and are prone to explosive fracture due to high internal tensile stress when damaged, and they often suffer from reduced weather resistance after chemical strengthening.

Method used

The use of lithium aluminosilicate glass with a fracture toughness value exceeding 0.80 MPa/m^1/2, chemically strengthened with a sodium-containing salt having a potassium content of less than 5% by mass, to create a compressive stress profile with specific surface and depth values, thereby enhancing strength and weather resistance.

Benefits of technology

The method produces chemically strengthened glass that is resistant to shattering upon damage and maintains excellent weather resistance, suitable for applications requiring high durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164238000001_ABST
    Figure 2024164238000001_ABST
Patent Text Reader

Abstract

To provide a chemically strengthened glass thar is resistant to fracturing upon reception of damage, and is excellent in terms of strength and weatherability and a manufacturing method therefor.SOLUTION: The present invention relates to a chemically strengthened glass with a thickness of t [unit: μm], which is a lithium aluminosilicate glass, wherein a surface compressive stress value (CS0), a compressive stress value at a depth of 50 μm from the glass surface (CS50), DOL [unit: μm], and (CS0×DOL) / K1c [unit: μm / m1 / 2] are each within specified ranges, and wherein the K level on the glass surface is 1 mass% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing chemically strengthened glass and chemically strengthened glass. [Background technology]

[0002] 2. Description of the Related Art Cover glass made of chemically strengthened glass is used for the purpose of protecting display devices such as mobile phones, smartphones, and tablet terminals and enhancing their aesthetic appearance.

[0003] In chemically strengthened glass, the surface compressive stress (value) (CS 0 The strength of the glass increases as the compressive stress layer depth (DOL) increases. On the other hand, the internal tensile stress (value) (CT) occurs inside the glass to balance the compressive stress of the glass surface. 0 The larger the DOL, the larger the CT. Glass with a large CT will have an explosive increase in the number of fractures when damaged, increasing the risk of fragments scattering.

[0004] Patent Document 1 describes that by forming a stress profile represented by a broken line through two-stage chemical strengthening, it is possible to increase the surface compressive stress while suppressing the internal tensile stress. 3 / NaNO 3 Mixed salt is used for the first stage of chemical strengthening, and KNO 3 / NaNO 3 Methods such as using mixed salt for the second stage chemical strengthening have been proposed.

[0005] Patent Document 2 discloses lithium aluminosilicate glass that can obtain a relatively large surface compressive stress and compressive stress layer depth by two-stage chemical strengthening. The lithium aluminosilicate glass can suppress CT and increase CS by a two-stage chemical strengthening treatment using a sodium salt in the first stage and a potassium salt in the second stage. 0 and DOL can both be increased. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] US Patent Application Publication No. 2015 / 0259244 [Patent Document 2] Japan Special Publication No. 2013-520388 Summary of the Invention [Problem to be solved by the invention]

[0007] However, two-stage chemical strengthening is complicated and has problems in terms of production efficiency. In addition, as mentioned above, when compressive stress is generated on the surface layer of glass by chemical strengthening, tensile stress is generated inside the glass, and when the tensile stress exceeds a threshold value (sometimes called the "CT limit"), the number of fractures during damage increases explosively.

[0008] The present inventors have found that by using a high fracture toughness glass as the base glass of chemically strengthened glass, explosive fracture during scratching can be suppressed even when a larger compressive stress is introduced into the glass. In other words, they have found that the CT limit can be increased by increasing the fracture toughness value of the base glass of chemically strengthened glass. By using lithium aluminosilicate glass as the base material of chemically strengthened glass, the fracture toughness value of the base material can be significantly improved. However, when lithium aluminosilicate glass is chemically strengthened, the weather resistance may be significantly reduced compared to before chemical strengthening.

[0009] Therefore, the present invention provides chemically strengthened glass that is resistant to fracture when scratched and has excellent strength and weather resistance, and a method for producing the same. [Means for solving the problem]

[0010] Regarding the above problem, the present inventors have found that the main cause of the deterioration of weather resistance when lithium aluminosilicate glass is chemically strengthened is precipitates formed by a reaction between potassium ions introduced to the glass surface by chemical strengthening using a strengthening salt containing potassium and components in the air. Furthermore, they have found that chemical strengthening using a strengthening salt containing sodium and having a potassium content of less than 5 mass% for lithium aluminosilicate glass having a fracture toughness value of a specific range or more can be used to obtain chemically strengthened glass that is suppressed from fracturing when scratched and has excellent strength and weather resistance. Based on these findings, the present invention has been completed.

[0011] That is, the present invention is as follows. 1. A method for producing chemically strengthened glass, comprising chemically strengthening lithium aluminosilicate glass having a thickness t [unit: μm], The lithium aluminosilicate glass has a fracture toughness value (K1c) of 0.80 MPa / m 1 / 2 That's all. The chemical strengthening is performed using a strengthening salt containing sodium and having a potassium content of less than 5% by mass, The resulting chemically strengthened glass has a surface compressive stress value (CS 0 ) is 500 to 1000 MPa, and A method for producing chemically strengthened glass, in which the depth DOL [unit: μm] at which the compressive stress value becomes zero is 0.06t to 0.2t. 2. The method for producing chemically strengthened glass according to 1 above, wherein the lithium aluminosilicate glass is crystallized glass. 3. The crystallized glass is In mole percent based on oxide, SiO 2 40 to 72% Al 2 O 3 0.5 to 10%, Li 2 Contains 15-50% O 3. A method for producing chemically strengthened glass according to item 2. 4. The method for producing chemically strengthened glass according to 2 or 3 above, wherein the crystallized glass has a visible light transmittance of 85% or more when converted into a glass with a thickness of 0.7 mm. 5. The method for producing chemically strengthened glass according to any one of 2 to 4 above, wherein the crystallized glass contains lithium metasilicate crystals. 6. The lithium aluminosilicate glass is In mole percent based on oxide, SiO 2 40 to 65% Al 2 O 3 15 to 45% Li 2 Contains 2-15% O 2. A method for producing chemically strengthened glass according to claim 1. 7. Chemically strengthened glass having a thickness t [unit: μm], Lithium aluminosilicate glass, Surface compressive stress value (CS 0 ) is 500 to 1000 MPa, Compressive stress value at a depth of 50 μm from the glass surface (CS 50 ) is 150 to 230 MPa, and The depth DOL [unit: μm] at which the compressive stress value becomes zero is 0.06t to 0.2t. (CS 0 ×DOL) / K1c[Unit:μm / m 1 / 2 Chemically strengthened glass having a modulus of 40,000 to 70,000. 8. The chemically strengthened glass according to 7 above, wherein the K concentration on the surface is 1 mass % or less. 9. Chemically strengthened glass having a thickness t [unit: μm], Lithium aluminosilicate glass, Surface compressive stress value (CS 0 ) is 500 to 1000 MPa, Compressive stress value at a depth of 50 μm from the glass surface (CS 50 ) is 150 to 230 MPa, and A chemically strengthened glass having a ratio CT / X of 0.7 to 1, where CT is an internal compressive stress value (unit: MPa) and X is expressed by the following formula: X=√(1 / 2a(1-ν)(t-2×DOL))K1c where a=0.11, ν is the Poisson's ratio [unit: -], DOL is the depth at which the compressive stress value becomes zero [unit: μm]. K1c is the fracture toughness value [unit: MPa / m 1 / 2 ]. 10. The base glass of the chemically strengthened glass has a K1c of 0.85 MPa m 1 / 2 10. The chemically strengthened glass according to any one of 7 to 9 above, which is glass-ceramic. 11. The chemically strengthened glass according to claim 10, wherein the crystallized glass contains lithium metasilicate crystals. 12. The crystallized glass contains, in mole percent based on oxides, SiO 2 40 to 72% Al 2 O 3 0.5 to 10%, Li 2 Contains 15-50% O and K 2 12. The chemically strengthened glass according to 10 or 11 above, which is substantially free of O. 13. The mother glass of the chemically strengthened glass is expressed in mole percentage based on oxides, SiO 2 40-65%, Al 2 O 3 15-45%, Li 2 Contains 2 to 15% O and has a K1c of 0.80 MPa m 1 / 2 10. The chemically strengthened glass according to any one of 7 to 9 above. Effect of the Invention

[0012] According to the method for producing chemically strengthened glass of the present invention, lithium aluminosilicate glass having a fracture toughness value of a specific range or more is chemically strengthened using a strengthening salt containing sodium and having a potassium content of less than 5 mass%. This makes it possible to efficiently produce chemically strengthened glass that is suppressed from fracturing when scratched and has superior strength and weather resistance compared to conventional glass. The chemically strengthened glass of the present invention is less likely to fractured when scratched and has superior strength and weather resistance, making it suitable for cover glass. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a diagram showing a stress profile of a chemically strengthened glass according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing an example of a powder X-ray diffraction pattern of the crystallized glass. [Diagram 3] FIG. 3 is a diagram showing an example of a DSC curve of the amorphous glass according to the present invention. [Figure 4] FIG. 4 shows an example of the results of damaging glass, where (A) shows the case of glass with a CT equal to or less than the CT limit, and (B) shows the case of glass with a CT exceeding the CT limit. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The chemically strengthened glass of the present invention will be described in detail below, but the present invention is not limited to the following embodiments, and can be arbitrarily modified and implemented within the scope of the present invention.

[0015] In this specification, "chemically strengthened glass" refers to glass after chemical strengthening treatment. Moreover, "glass for chemical strengthening" refers to glass before chemical strengthening treatment.

[0016] In this specification, the glass composition of the chemically strengthened glass may be referred to as the base composition of the chemically strengthened glass. In chemically strengthened glass, a compressive stress layer is usually formed on the glass surface due to ion exchange, so the glass composition of the non-ion-exchanged portion coincides with the base composition of the chemically strengthened glass. In addition, the concentration of components other than alkali metal oxides does not basically change even in the ion-exchanged portion.

[0017] In this specification, the glass composition is expressed in mole percentage based on oxides, and mole % may be simply written as %. Furthermore, the symbol "~" indicating a numerical range is used to mean that the numerical values ​​before and after it are included as the lower and upper limits.

[0018] In the glass composition, the term "substantially free" means that it is not contained except for unavoidable impurities contained in raw materials, etc., that is, it is not intentionally contained. For example, the content in the glass composition is less than 0.1 mol % except for transition metal oxides that cause coloring.

[0019] In this specification, the term "stress profile" refers to a pattern that expresses compressive stress values ​​with the depth from the glass surface as a variable. A negative compressive stress value means tensile stress. The "depth of compressive stress layer (DOC)" is the depth at which the compressive stress value (CS) is zero. The "internal tensile stress value (CT)" refers to the tensile stress value at a depth of 1 / 2 the glass sheet thickness t.

[0020] Generally, the stress profile is often measured using an optical waveguide surface stress meter (e.g., FSM-6000 manufactured by Orihara Seisakusho Co., Ltd.). However, due to the measurement principle, the optical waveguide surface stress meter cannot measure stress unless the refractive index decreases from the surface toward the inside. As a result, when lithium aluminosilicate glass is chemically strengthened with sodium salt, compressive stress cannot be measured. Therefore, in this specification, the stress profile is measured using a scattered light photoelastic stress meter (e.g., SLP-1000 manufactured by Orihara Seisakusho Co., Ltd.). The scattered light photoelastic stress meter can measure the stress value regardless of the refractive index distribution inside the glass. However, since the scattered light photoelastic stress meter is easily affected by the surface scattered light, it is difficult to accurately measure the stress value near the glass surface. For the surface layer portion up to a depth of 10 μm from the surface, the stress value can be estimated by a method of extrapolation using a complementary error function based on the measurement value of the deeper portion.

[0021] <Chemically strengthened glass> The chemically strengthened glass of this embodiment has a thickness t [unit: μm], Lithium aluminosilicate glass, Surface compressive stress value (CS 0 ) is 500 to 1000 MPa, Compressive stress value at a depth of 50 μm from the glass surface (CS 50 ) is 150 to 230 MPa, and The depth DOL [unit: μm] at which the compressive stress value becomes zero is 0.06t to 0.2t. (CS 0 ×DOL) / K1c[Unit:μm / m 1 / 2 ] is between 40,000 and 70,000. Here, K1c is the fracture toughness value [unit: μm / m 1 / 2 ]. In the present chemically strengthened glass, the K concentration in the glass surface is preferably 1 mass % or less.

[0022] Alternatively, the chemically strengthened glass of this embodiment is A chemically strengthened glass having a thickness t [unit: μm], Lithium aluminosilicate glass, Surface compressive stress value (CS 0 ) is 500 to 1000 MPa, Compressive stress value at a depth of 50 μm from the glass surface (CS 50 ) is 150 to 230 MPa, and The ratio CT / X of the internal compressive stress value CT (unit: MPa) to X represented by the following formula is 0.7 to 1. X=√(1 / 2a(1-ν)(t-2×DOL))K1c where a is 0.11 and ν is Poisson's ratio.

[0023] Fig. 1 is a diagram showing a stress profile of a chemically strengthened glass according to one embodiment of the present invention. In Fig. 1, an example is a stress profile of a chemically strengthened glass according to one embodiment of the present invention (chemically strengthened glass SG5 described later). A reference example is a stress profile of a chemically strengthened glass obtained by subjecting glass G21 described later to two-stage chemical strengthening without crystallization.

[0024] When a glass plate is bent by an impact, if the amount of bending is large, a large tensile stress is applied to the glass surface, causing the glass to break. In this specification, such breakage is referred to as "glass breakage due to bending mode."

[0025] As shown in Fig. 1, the chemically strengthened glass of the present invention has a higher CS at the outermost surface of the glass than the chemically strengthened glass of the Reference Example, and therefore glass breakage in bending mode is suppressed. 50 By keeping the stress at 150 to 230 MPa, the internal tensile stress area (St) can be suppressed, which results in a reduction in CT and suppresses fracture during damage. Here, St is the integral of the tensile stress value in the region from the DOL to the center of thickness t / 2 in the stress profile.

[0026] The thickness (t) of the chemically strengthened glass of the present invention is, for example, 2 mm or less, preferably 1.5 mm or less, more preferably 1 mm or less, even more preferably 0.9 mm or less, particularly preferably 0.8 mm or less, and most preferably 0.7 mm or less. In order to obtain sufficient strength, the thickness is, for example, 0.1 mm or more, preferably 0.2 mm or more, more preferably 0.4 mm or more, even more preferably 0.5 mm or more, and particularly preferably 0.6 mm or more.

[0027] The chemically strengthened glass of the present invention is manufactured by subjecting lithium aluminosilicate glass to an ion exchange treatment. Compared with sodium aluminosilicate glass, which has been widely used as a chemically strengthened glass, lithium aluminosilicate glass has a large fracture toughness value and tends to be less likely to break even if scratched. In addition, the CT limit described later is large, and even if the compressive stress value of the glass surface is increased, severe fracture tends to be less likely to occur.

[0028] The chemically strengthened glass of the present invention is CS 0 is 500 MPa or more, preferably 550 MPa or more, and more preferably 600 MPa or more. 0 By setting the CS to 500 MPa or more, the tensile stress caused by the drop is offset, making the glass less likely to break, and also suppressing breakage due to bending mode. In addition, the total amount of compressive stress in the glass surface layer is constant, and the CS 0 If the temperature is too high, the CS inside the glass 50 Therefore, in order to prevent fragmentation during impact, CS 0 is 1000 MPa or less, preferably 800 MPa or less, and more preferably 750 MPa or less.

[0029] The chemically strengthened glass of the present invention is CS 50 is 150 MPa or more, preferably 160 MPa or more, and more preferably 170 MPa or more. 50 By setting the CS to 150 MPa or more, the strength can be improved. 50If CS is too high, the internal tensile stress CT increases and the material becomes more susceptible to fracture. 50 is 230 MPa or less, preferably 220 MPa or less, and more preferably 210 MPa or less.

[0030] If the depth (DOL) at which the compressive stress value becomes 0 is too large relative to the thickness t [unit: μm], it will lead to an increase in CT, so it is 0.2t or less, preferably 0.19t or less, and more preferably 0.18t or less. Specifically, for example, when the plate thickness t is 0.8 mm, the DOL is preferably 160 μm or less. In addition, from the viewpoint of improving strength, the DOL is 0.06t or more, preferably 0.08t or more, more preferably 0.10t or more, and even more preferably 0.12t or more.

[0031] When compressive stress is generated in the surface layer of glass by chemical strengthening, CT occurs inside the glass, and when the CT exceeds the CT limit, the number of fractures during scratching increases explosively. Figure 4 shows an example of the results of scratching glass after chemical strengthening using a Vickers tester by the method described later in the examples. (A) in Figure 4 shows the case of glass with a CT equal to or less than the CT limit, and (B) in Figure 4 shows the case of glass with a CT exceeding the CT limit. Since the total amount of compressive stress in the surface layer is determined by the CT limit, it is possible to suppress fractures during scratching by lowering the CT while keeping the total amount of compressive stress in the surface layer within a certain range, or by raising the CT limit by providing a high fracture toughness.

[0032] The chemically strengthened glass of the present invention is (CS 0 ×DOL) / K1c[Unit:μm / m 1 / 2 ] is 40,000 to 70,000, preferably 42,000 to 58,000, and more preferably 44,000 to 55,000. (CS 0 × DOL) / K1c in the above range improves CS of the surface layer of the glass to suppress fracture in bending mode, improves drop strength, and suppresses St to keep CT low and suppresses fracture when scratched.

[0033] In order to improve the drop strength while suppressing crushing, the value of (t-2×DOL)×CT / 2 [unit: μm·MPa] is preferably 20,000 to 30,000. The value of (t-2×DOL)×CT / 2 [unit: μm·MPa] is more preferably 25,000 or less. (t-2×DOL)×CT / 2 is approximated to the integral value St of the tensile stress.

[0034] Glass with a high fracture toughness value has a high CT limit, so even if a large surface compressive stress is introduced into the glass by chemical strengthening, it is unlikely to fracture violently. From the viewpoint of suppressing fracture when scratched, the chemically strengthened glass of the present invention has a mother glass fracture toughness value of 0.80 MPa m 1 / 2 It is preferable that the viscosity is equal to or higher than 0.85 MPa m. 1 / 2 More preferably, 0.90 MPa m 1 / 2 The fracture toughness value is usually 2.0 MPa m 1 / 2 Typically, it is 1.5 MPa m 1 / 2 The following is the result.

[0035] The fracture toughness value can be measured, for example, by using the DCDC method (Acta metall.mater. Vol.43, pp.3453-3458, 1995). The fracture toughness value can be simply evaluated by the indentation method. As a method for making the fracture toughness value within the above range, for example, a method for adjusting the crystallization rate, fictive temperature, etc. by adjusting the crystallization conditions (time and temperature of heat treatment), glass composition, cooling rate, etc. of the crystallized glass can be mentioned. Specifically, for example, in the case of crystallized glass, the crystallization rate of the crystallized glass described later is preferably 15% or more, more preferably 18% or more, and even more preferably 20% or more. In addition, in order to ensure the transmittance, the crystallization rate of the crystallized glass is preferably 60% or less, more preferably 55% or less, even more preferably 50% or less, and particularly preferably 40% or less.

[0036] The present inventors have experimentally found that the CT limit value is approximately equal to the value of X expressed by the following formula. X=√(1 / 2a(1-ν)(t-2×DOL))K1c where a = 0.11 and ν is Poisson's ratio. In other words, severe fragmentation is unlikely to occur if the ratio of CT to X, CT / X, is 1 or less. Therefore, by setting CT / X to 0.7 to 1, it is possible to increase CS while suppressing fragmentation. In order to prevent crushing, CT / X is preferably 0.95 or less, and more preferably 0.9 or less.

[0037] Chemically strengthened glass obtained by subjecting lithium aluminosilicate glass to a two-stage ion exchange treatment may have a reduced weather resistance compared to before chemical strengthening. The present inventors investigated chemically strengthened glass with reduced weather resistance and found that potassium-containing precipitates were formed on the glass surface. This is presumably because potassium ions present in large amounts on the glass surface react chemically with components in the air to form precipitates. One embodiment of the chemically strengthened glass of the present invention has a large alkali content ratio to alumina in the matrix composition, and is particularly prone to reduced weather resistance.

[0038] The chemically strengthened glass of the present invention has a low K concentration on the glass surface, which prevents chemical reactions with components in the air and exhibits excellent weather resistance. The K concentration on the glass surface of the chemically strengthened glass of the present invention is 1 mass% or less, more preferably 0.8 mass% or less, and even more preferably 0.6 mass% or less.

[0039] In this specification, the "K concentration at the glass surface" refers to the K concentration from the glass surface to a depth of 1 μm. The lower limit of the K concentration at the glass surface is usually 1 / 1000 or more of the K concentration (mass%) originally contained in the glass composition. Here, the K concentration originally contained in the glass composition refers to the K concentration of the glass before chemical strengthening. The K concentration at the glass surface can be measured by EPMA (electron probe micro analyzer).

[0040] The weather resistance of chemically strengthened glass can be evaluated by a weather resistance test. The chemically strengthened glass of the present invention preferably has a difference in haze value before and after standing at 80% humidity and 80°C for 120 hours of 5% or less (i.e., |haze value after test [%]-haze value before test [%]|≦5), more preferably 4% or less, and even more preferably 3% or less. The haze value is measured using a haze meter in accordance with JIS K7136 (2000) under a C light source.

[0041] The shape of the chemically strengthened glass of the present invention may be a shape other than a plate shape depending on the product to which it is applied, the purpose, etc. The glass plate may have a border shape with a different thickness on the periphery. The shape of the glass plate is not limited thereto, and for example, the two main surfaces may not be parallel to each other, and one or both of the two main surfaces may be entirely or partially curved. More specifically, the glass plate may be, for example, a flat glass plate without warping, or a curved glass plate having a curved surface.

[0042] The chemically strengthened glass of the present invention can be used as a cover glass for mobile electronic devices such as mobile phones, smartphones, personal digital assistants (PDAs), and tablet terminals. It is also useful as a cover glass for electronic devices such as televisions (TVs), personal computers (PCs), and touch panels that are not intended to be portable. It is also useful as a building material such as window glass, a tabletop, the interior of automobiles and airplanes, and the like, and as a cover glass for these.

[0043] The chemically strengthened glass of the present invention can be bent or molded into a shape other than a flat plate before or after chemical strengthening, and is therefore useful for applications such as housings having curved surfaces.

[0044] <Lithium aluminosilicate glass> The chemically strengthened glass of the present invention is a lithium aluminosilicate glass. The lithium aluminosilicate glass is SiO 2 , Al 2 O 3 and Li 2The form of the glass is not particularly limited as long as it contains O, and examples thereof include crystallized glass and amorphous glass. Crystallized glass and amorphous glass will be described below.

[0045] <<Glass-ceramics>> When the lithium aluminosilicate glass of the present invention is a crystallized glass, in one embodiment, the lithium aluminosilicate glass is expressed in mole percent based on oxides. SiO 2 40 to 72% Al 2 O 3 0.5 to 10%, Li 2 The O content is preferably 15 to 50%. The crystallized glass preferably contains at least one of lithium silicate crystals, lithium aluminosilicate crystals, and lithium phosphate crystals. As the lithium silicate crystals, lithium metasilicate crystals are more preferable. As the lithium aluminosilicate crystals, petalite crystals or β-spodumene crystals are preferable. As the lithium phosphate crystals, lithium orthophosphate crystals are preferable. To increase transparency, crystallized glass containing lithium metasilicate crystals is more preferable.

[0046] Crystallized glass is obtained by heat-treating and crystallizing amorphous glass, which will be described later. The glass composition of crystallized glass is the same as that of amorphous glass before crystallization, so it will be described in the section on amorphous glass.

[0047] The crystallized glass has a visible light transmittance (total visible light transmittance including diffuse transmitted light) of preferably 85% or more when converted to a thickness of 0.7 mm, so that when used as a cover glass for a mobile display, the display screen is easy to see. The visible light transmittance is more preferably 88% or more, and even more preferably 90% or more. The higher the visible light transmittance, the more preferable it is, but it is usually 93% or less. The visible light transmittance of ordinary amorphous glass is about 90% or more. If the thickness of the glass-ceramic is not 0.7 mm, the transmittance for a thickness of 0.7 mm can be calculated from the measured transmittance using the Lambert-Beer law. In addition, in the case of glass having a sheet thickness t of more than 0.7 mm, the sheet thickness may be adjusted to 0.7 mm by polishing, etching, or the like, and then the actual measurement may be performed.

[0048] Moreover, the haze value, when converted to a thickness of 0.7 mm, is preferably 1.0% or less, more preferably 0.4% or less, even more preferably 0.3% or less, particularly preferably 0.2% or less, and most preferably 0.15% or less. The smaller the haze value, the better, but if the crystallization rate or the crystal grain size is reduced in order to reduce the haze value, the mechanical strength decreases. In order to increase the mechanical strength, the haze value in the case of a thickness of 0.7 mm is preferably 0.02% or more, and more preferably 0.03% or more. The haze value is a value measured according to JIS K7136 (2000). In addition, if the total light visible transmittance of crystallized glass with a thickness of t [mm] is 100×T [%] and the haze value is 100×H [%], then by applying the Beer-Lambert law, it can be written as T=(1-R)2×exp(-αt) using the constant α. Using this constant α, dH / dt ∝ exp(-αt) × (1-H) It can be expressed as: In other words, the haze value can be considered to increase in proportion to the internal linear transmittance as the plate thickness increases. 0.7 is calculated using the following formula: H 0.7 =100×[1-(1-H) {((1-R)2-T0.7) / ((1-R)2-T)} ][%] In addition, in the case of glass having a sheet thickness t of more than 0.7 mm, the sheet thickness may be adjusted to 0.7 mm by polishing, etching, or the like, and then the actual measurement may be performed.

[0049] When tempered glass made of glass-ceramics is used as the cover glass for a mobile display, it is preferable that the tempered glass has a texture and a high-class feel different from that of plastic. Therefore, the refractive index of the glass-ceramics is preferably 1.52 or more at a wavelength of 590 nm, more preferably 1.55 or more, and even more preferably 1.57 or more.

[0050] The crystallized glass is preferably a crystallized glass containing lithium metasilicate crystals. The lithium metasilicate crystals are Li 2 SiO 3 Generally, it is a crystal that shows diffraction peaks at Bragg angles (2θ) of 26.98°±0.2°, 18.88°±0.2°, and 33.05°±0.2° in the powder X-ray diffraction spectrum. Figure 2 shows an example of the X-ray diffraction spectrum of crystallized glass, in which the diffraction peaks of lithium metasilicate crystals can be seen.

[0051] Glass-ceramics containing lithium metasilicate crystals have a higher fracture toughness value than general amorphous glass, and are less likely to break violently even when a large compressive stress is applied by chemical strengthening. In amorphous glass in which lithium metasilicate crystals can precipitate, lithium disilicate may precipitate depending on the heat treatment conditions. Lithium disilicate is Li 2 S 2 O 5 and generally, it is a crystal that exhibits diffraction peaks at Bragg angles (2θ) of 24.89°±0.2°, 23.85°±0.2°, and 24.40°±0.2° in a powder X-ray diffraction spectrum.

[0052] In the case of containing lithium disilicate crystals, the lithium disilicate crystal particle size calculated from the X-ray diffraction peak width by the Scherrer formula is preferably 45 nm or less, since transparency is easily obtained, and more preferably 40 nm or less. Although the Scherrer formula has a shape factor, in this case it is acceptable to represent it by the dimensionless 0.9 (i.e., the crystal grains are assumed to be spherical).

[0053] When lithium metasilicate crystals are contained in the crystallized glass, it is preferable that the crystallized glass does not contain lithium disilicate, since the transparency of the crystallized glass is likely to decrease if lithium disilicate crystals are also contained. Here, "not containing lithium disilicate" means that no diffraction peak of lithium disilicate crystals is detected in the X-ray diffraction spectrum.

[0054] The crystallization rate of the crystallized glass is preferably 5% or more, more preferably 10% or more, even more preferably 15% or more, and particularly preferably 20% or more in order to increase the mechanical strength. In order to increase the transparency, it is preferably 70% or less, more preferably 60% or less, and particularly preferably 50% or less. A small crystallization rate is also excellent in that it is easy to bend and mold by heating.

[0055] The crystallinity can be calculated from the X-ray diffraction intensity by the Rietveld method. The Rietveld method is described in the "Crystal Analysis Handbook" (Kyoritsu Shuppan, 1999, pp. 492-499), edited by the Editorial Committee of the "Crystal Analysis Handbook" of the Japanese Crystallographic Society.

[0056] The average particle size of the precipitated crystals of the crystallized glass is preferably 80 nm or less, more preferably 60 nm or less, even more preferably 50 nm or less, particularly preferably 40 nm or less, and most preferably 30 nm or less. The average particle size of the precipitated crystals is determined from a transmission electron microscope (TEM) image. The average particle size of the precipitated crystals can be estimated from a scanning electron microscope (SEM) image.

[0057] The average thermal expansion coefficient of crystallized glass at 50℃ to 350℃ is 90×10 -7 / °C or more, and more preferably 100×10 -7 / °C or higher, and more preferably 110×10 -7 / °C or more, and particularly preferably 120×10 -7 / ℃ or more, most preferably 130×10 -7 / ℃ or higher.

[0058] If the thermal expansion coefficient is too large, cracks may occur due to the difference in the thermal expansion coefficient during the chemical strengthening process. Therefore, it is preferable to set the thermal expansion coefficient at 160×10 ―7 / ℃ or less, more preferably 150×10 -7 / ℃ or less, more preferably 140×10 -7 / ℃ or less.

[0059] Since crystallized glass contains crystals, it has a high hardness. Therefore, it is difficult to scratch and has excellent abrasion resistance. In order to increase the abrasion resistance, the Vickers hardness is preferably 600 or more, more preferably 700 or more, even more preferably 730 or more, particularly preferably 750 or more, and most preferably 780 or more.

[0060] If the hardness is too high, processing becomes difficult, so the Vickers hardness of the crystallized glass is preferably 1100 or less, more preferably 1050 or less, and even more preferably 1000 or less.

[0061] The Young's modulus of the crystallized glass is preferably 85 GPa or more, more preferably 90 GPa or more, even more preferably 95 GPa or more, and particularly preferably 100 GPa or more, in order to suppress warpage caused by strengthening during chemical strengthening. The crystallized glass may be polished before use. In order to facilitate polishing, the Young's modulus is preferably 130 GPa or less, more preferably 125 GPa or less, and even more preferably 120 GPa or less.

[0062] The fracture toughness value of the crystallized glass is preferably 0.8 MPa m 1 / 2 More preferably, 0.85 MPa m 1 / 2 More preferably, 0.9 MPa m 1 / 2 If the thickness is more than this, then when chemically strengthened, fragments are less likely to scatter when broken, which is preferable.

[0063] When the lithium aluminosilicate glass in the present invention is a crystallized glass, in one embodiment, the glass has a content of SiO in mole percent based on oxides. 2 40-72%, Al 2 O 3 0.5 to 10%, Li 2O 15-50%, P 2 O 5 0-4%, ZrO 2 0-6%, Na 2 O 0-7%, K 2 It is preferable that the content of O is 0 to 5%. That is, the content of O is 0 to 5% by mole of oxide. 2 40-72%, Al 2 O 3 0.5 to 10%, Li 2 O 15-50%, P 2 O 5 0-4%, ZrO 2 0-6%, Na 2 O 0-7%, K 2 It is preferable to crystallize amorphous glass containing 0 to 5% O (hereinafter sometimes referred to as crystallizable amorphous glass) by heat treatment.

[0064] <Crystalline amorphous glass> In one embodiment, the crystallizable amorphous glass of the present invention is a glass having a content of SiO 2 in mole percent based on oxides. 2 40-72%, Al 2 O 3 0.5 to 10%, Li 2 O 15-50%, P 2 O 5 0-4%, ZrO 2 0-6%, Na 2 O 0-7%, K 2 The O content is preferably 0 to 5%. The glass composition will be described below.

[0065] In crystalline amorphous glass, SiO 2 SiO is a component that forms the network structure of glass. It also increases chemical durability and is a component of lithium silicate crystals and lithium aluminosilicate crystals. 2 The content of SiO is preferably 40% or more. 2 The content of SiO is more preferably 42% or more, and further preferably 45% or more. In order to sufficiently increase the stress due to chemical strengthening, 2The content of SiO is preferably 72% or less. In order to precipitate lithium metasilicate crystals, 2 The content is preferably 60% or less, more preferably 58% or less, and further preferably 55% or less.

[0066] Al 2 O 3 Al is an essential component that increases the surface compressive stress due to chemical strengthening. 2 O 3 The content of Al is preferably 0.5% or more. In order to increase the stress caused by chemical strengthening, 2 O 3 The content of Al is more preferably 1% or more, and further preferably 2% or more. On the other hand, in order to reduce the haze value of the crystallized glass, 2 O 3 The content is preferably 10% or less, more preferably 8% or less, and even more preferably 6% or less.

[0067] Li 2 O is a component that forms surface compressive stress through ion exchange, and is an essential component of lithium silicate crystals, lithium aluminosilicate crystals, and lithium phosphate crystals. 2 The content of O is preferably 15% or more, more preferably 20% or more, and further preferably 25% or more. On the other hand, in order to maintain chemical durability, Li 2 The O content is preferably 50% or less, more preferably 45% or less, and further preferably 40% or less.

[0068] Na 2 O is a component that improves the meltability of glass. 2 O is not essential, but Na is preferred. 2 The content of O is 0.5% or more, more preferably 1% or more, and particularly preferably 2% or more. 2 If there is too much O, it becomes difficult to precipitate lithium metasilicate crystals, or the chemical strengthening properties decrease. 2 The O content is preferably 7% or less, more preferably 6% or less, and further preferably 5% or less.

[0069] K 2 O is Na 2 Like O, it is an ingredient that lowers the melting temperature of glass and may be contained. 2 When O is contained, the content is preferably 0.5% or more, more preferably 1% or more, further preferably 1.5% or more, and particularly preferably 2% or more. 2 If there is too much O, the chemical strengthening properties will decrease. 2 The O content is preferably 5% or less, more preferably 4% or less, further preferably 3% or less, and particularly preferably 2% or less.

[0070] Also Na 2 O and K 2 Total content of Na and O 2 O+K 2 O is preferably 0.5% or more, more preferably 1% or more. 2 O+K 2 The O content is preferably 7% or less, more preferably 6% or less, and even more preferably 5% or less.

[0071] Also Li 2 O and SiO 2 mol% ratio of Li 2 O / SiO 2 is preferably 0.4 or more, more preferably 0.45 or more, and even more preferably 0.5 or more. 2 O / SiO 2 is preferably 0.85 or less, more preferably 0.80 or less, and even more preferably 0.75 or less. This makes it easier for lithium metasilicate crystals to precipitate during heat treatment, making it easier to obtain highly transparent crystallized glass.

[0072] Also, Li 2 O and Na 2 O mol% ratio Li 2 O / Na 2 O is preferably 4 or more, more preferably 8 or more, and even more preferably 12 or more. 2 O / Na 2Furthermore, O is preferably equal to or less than 30, more preferably equal to or less than 28, and even more preferably equal to or less than 25. This makes it easier to obtain a stress profile in which the surface stress is relaxed while a sufficient compressive stress is applied by chemical strengthening.

[0073] P 2 O 5 is not essential for crystallized glass containing lithium silicate or lithium aluminosilicate, but may be contained since it has the effect of promoting phase separation of the glass and accelerating crystallization. Also, it is an essential component for crystallized glass containing lithium phosphate crystals. 2 O 5 When P is contained, the content is preferably 0.5% or more, more preferably 1% or more, and further preferably 1.5% or more. 2 O 5 If the content is too high, phase separation occurs easily when melted, and acid resistance is significantly reduced. 2 O 5 The content is preferably 5% or less, more preferably 4% or less, and further preferably 3% or less.

[0074] ZrO 2 is a component that can form crystal nuclei during crystallization treatment and may be contained. 2 The content of ZrO is preferably 1% or more, more preferably 2% or more, further preferably 2.5% or more, and particularly preferably 3% or more. 2 The content is preferably 6% or less, more preferably 5.5% or less, and even more preferably 5% or less.

[0075] TiO 2 is a component that can form crystal nuclei during crystallization treatment and may be contained. 2 is not essential, but if it is contained, it is preferably 0.5% or more, more preferably 1% or more, further preferably 2% or more, particularly preferably 3% or more, and most preferably 4% or more. On the other hand, in order to suppress devitrification during melting, TiO 2The content is preferably 10% or less, more preferably 8% or less, and even more preferably 6% or less.

[0076] SnO 2 SnO has the effect of promoting the formation of crystal nuclei and may be contained. 2 is not essential, but when contained, it is preferably 0.5% or more, more preferably 1% or more, further preferably 1.5% or more, and particularly preferably 2% or more. On the other hand, in order to suppress devitrification during melting, SnO 2 The content is preferably 6% or less, more preferably 5% or less, further preferably 4% or less, and particularly preferably 3% or less.

[0077] Y 2 O 3 Y is a component that prevents chemically strengthened glass from scattering when broken, and may be included. 2 O 3 The content of Y is preferably 1% or more, more preferably 1.5% or more, further preferably 2% or more, particularly preferably 2.5% or more, and extremely preferably 3% or more. 2 O 3 The content is preferably 5% or less, more preferably 4% or less.

[0078] B 2 O 3 Although not essential, B is a component that improves the chipping resistance and melting property of the glass for chemical strengthening or the chemically strengthened glass, and may be contained. 2 O 3 In the case where B is contained, the content is preferably 0.5% or more, more preferably 1% or more, and further preferably 2% or more in order to improve the melting property. 2 O 3 If the content exceeds 5%, striae will occur during melting and the quality of the glass for chemical strengthening will tend to deteriorate, so the content is preferably 5% or less. 2 O 3 The content is more preferably 4% or less, further preferably 3% or less, and particularly preferably 2% or less.

[0079] BaO, SrO, MgO, CaO, and ZnO are components that improve the melting property of glass and may be contained. When these components are contained, the total content of BaO, SrO, MgO, CaO, and ZnO (BaO+SrO+MgO+CaO+ZnO) is preferably 0.5% or more, more preferably 1% or more, even more preferably 1.5% or more, and particularly preferably 2% or more. On the other hand, since the ion exchange rate decreases, the content of BaO+SrO+MgO+CaO+ZnO is preferably 8% or less, more preferably 6% or less, even more preferably 5% or less, and particularly preferably 4% or less.

[0080] Among these, BaO, SrO, and ZnO may be contained to improve the refractive index of the residual glass and bring it closer to the precipitated crystal phase, thereby improving the transmittance of the crystallized glass and reducing the haze value. In this case, the total content of BaO+SrO+ZnO is preferably 0.3% or more, more preferably 0.5% or more, even more preferably 0.7% or more, and particularly preferably 1% or more. On the other hand, these components may reduce the ion exchange rate. In order to improve the chemical strengthening properties, BaO+SrO+ZnO is preferably 2.5% or less, more preferably 2% or less, even more preferably 1.7% or less, and particularly preferably 1.5% or less.

[0081] In addition, the CEO 2 It may contain CeO 2 has the effect of oxidizing the glass, and may suppress coloring. 2 When CeO is contained, the content is preferably 0.03% or more, more preferably 0.05% or more, and further preferably 0.07% or more. 2 When using CeO as an oxidizing agent, 2 The content is preferably 1.5% or less, and more preferably 1.0% or less, in order to increase transparency.

[0082] When the tempered glass is used after being colored, a coloring component may be added to the glass within a range that does not impede the achievement of the desired chemical strengthening properties. 3 O 4 , MnO 2 , Fe2 O 3 , NiO, CuO, Cr 2 O 3 , V 2 O 5 , Bi 2 O 3 , SeO 2 , Er 2 O 3 , Nd 2 O 3 are mentioned as suitable ones.

[0083] The total content of coloring components is preferably within the range of 1% or less. If it is desired to increase the visible light transmittance of the glass, it is preferable that these components are substantially not contained.

[0084] In addition, SO is used as a fining agent when melting glass. 3 , chloride, fluoride, etc. may be appropriately contained. 2 O 3 It is preferable that Sb is not contained. 2 O 3 When it is contained, it is preferably 0.3% or less, more preferably 0.1% or less, and most preferably not contained.

[0085] <<Highly tough amorphous glass>> The lithium aluminosilicate glass in the present invention may be a highly tough amorphous glass. Examples of highly tough amorphous glass include SiO 2 40-65%, Al 2 O 3 15-45%, Li 2 Glass containing 2 to 15% O is an example. High toughness amorphous glass is Y 2 O 3 , La 2 O 3 , Nb 2 O 5 , Ta 2 O 5 and W.O. 3 It is preferable that the total content of one or more components selected from the above is 1 to 15%.

[0086] In tough amorphous glass, SiO 2 SiO is a component that forms the network structure of glass. It also increases chemical durability. 2 The content of SiO is preferably 40% or more. 2 The content of SiO is more preferably 42% or more, and further preferably 45% or more. In order to sufficiently increase the stress due to chemical strengthening, 2 The content is preferably 65% ​​or less, more preferably 60% or less, and further preferably 55% or less.

[0087] Al 2 O 3 Al is an essential component that increases the surface compressive stress due to chemical strengthening. 2 O 3 The content of Al is preferably 15% or more. In order to increase the fracture toughness value, 2 O 3 The content of Al is more preferably 20% or more, further preferably 22% or more, and particularly preferably 25% or more. 2 O 3 The content is preferably 45% or less, more preferably 40% or less, and even more preferably 35% or less.

[0088] Li 2 O is an essential component that forms surface compressive stress through ion exchange. 2 The content of O is preferably 2% or more, more preferably 4% or more, and further preferably 7% or more. On the other hand, in order to maintain chemical durability, Li 2 The O content is preferably 15% or less, more preferably 13% or less, and further preferably 11% or less.

[0089] The glass of the present invention is 2 O 3 , La 2 O 3 , Nb 2 O 5 , Ta 2 O 5 and W.O. 3In order to lower the devitrification temperature, it is preferable for the glass to contain one or more components selected from the above in a total amount of 1% or more, more preferably 2% or more, and even more preferably 3% or more.

[0090] Y 2 O 3 , La 2 O 3 , Nb 2 O 5 , Ta 2 O 5 and W.O. 3 are cations with large field strength. Field strength is calculated by dividing the valence of a cation by its ionic radius, and is the strength with which it attracts surrounding oxygen ions. These components increase the oxygen packing density, and therefore have the effect of improving Young's modulus and fracture toughness.

[0091] If the Young's modulus is too high, the processing becomes more difficult, resulting in a lower yield. 2 O 3 , La 2 O 3 , Nb 2 O 5 , Ta 2 O 5 and W.O. 3 The total content of one or more components selected from is preferably 15% or less in order to keep the improvement in Young's modulus within an appropriate range. Such a content is more preferably 13% or less, even more preferably 12% or less, and particularly preferably 11% or less.

[0092] In the glass composition of the present invention, Y 2 O 3 , La 2 O 3 , Nb 2 O 5 , Ta 2 O 5 and W.O. 3 The total content of Al 2 O 3 The ratio of the content ([Y 2 O 3 ]+[La 2 O 3 ]+[Nb2 O 5 ]+[Ta 2 O 5 ]+[WO 3 ]) / [Al 2 O 3 In order to form a glass structure with high packing density, [Y 2 O 3 ]+[La 2 O 3 ]+[Nb 2 O 5 ]+[Ta 2 O 5 ]+[WO 3 ]) / [Al 2 O 3 In order to prevent the glass from having an unnecessarily high Young's modulus, ] is preferably 0.6 or less, more preferably 0.55 or less, and even more preferably 0.5 or less.

[0093] La 2 O 3 , Nb 2 O 5 , Ta 2 O 5 and W.O. 3 is not an essential component, but has a significant effect on the brittleness of the glass and may be contained in order to adjust the properties of chipping and scratch tests.

[0094] Li 2 O, Na 2 O and K 2 Alkali metal oxides such as O (collectively R 2 O) are components which lower the melting temperature of the glass, although none of them is essential, and one or more of them may be contained.

[0095] The glass transition temperature Tg of the amorphous glass is preferably 390° C. or higher, more preferably 410° C. or higher, and even more preferably 420° C. or higher. If the glass transition temperature Tg is high, stress relaxation during chemical strengthening is unlikely to occur, and high strength is likely to be obtained. On the other hand, if the Tg is too high, it is difficult to mold the glass, so the Tg is preferably 650° C. or lower, and more preferably 600° C. or lower.

[0096] The average thermal expansion coefficient of amorphous glass at 50℃ to 350℃ is 90×10 -7 / ℃ or more is preferable, and 100×10 -7 / ℃ or more is more preferable, and 110×10 -7 On the other hand, if the thermal expansion coefficient is too large, the glass is likely to break during molding. -7 / ℃ or less is preferable, and 140×10 -7 / ° C. or less is more preferable. If the difference in thermal expansion coefficient between the amorphous glass and the lithium metasilicate crystal is large, cracks are likely to occur during the crystallization process due to the difference in thermal expansion coefficient.

[0097] Amorphous glass is crushed and the glass transition temperature (Tg DSC The difference between the DSC curve and the crystallization peak temperature (Tc) appearing in the lowest temperature range is defined as (Tc-Tg). The (Tc-Tg) of amorphous glass is preferably 80°C or higher, more preferably 85°C or higher, even more preferably 90°C or higher, and particularly preferably 95°C or higher. If (Tc-Tg) is large, the crystallized glass can be easily reheated and bent. (Tc-Tg) is preferably 150°C or lower, and more preferably 140°C or lower.

[0098] Figure 3 shows an example of a DSC curve for amorphous glass. DSC may not coincide with the glass transition point (Tg) determined from the thermal expansion curve. DSC Since the glass is crushed and measured, the measurement error is likely to be large. However, in order to evaluate the relationship with the crystallization peak temperature, it is better to use the Tg obtained by the same DSC measurement rather than the Tg obtained from the thermal expansion curve. DSC It is appropriate to use

[0099] The Young's modulus of the amorphous glass is preferably 75 GPa or more, more preferably 80 GPa or more, and even more preferably 85 GPa or more.

[0100] The Vickers hardness of the amorphous glass is preferably 500 or more, and more preferably 550 or more.

[0101] <Method of manufacturing chemically strengthened glass> The chemically strengthened glass of the present invention is produced by heat-treating the above-mentioned crystallizable amorphous glass to obtain crystallized glass, and then chemically strengthening the obtained crystallized glass, or by chemically strengthening the above-mentioned high-toughness amorphous glass.

[0102] (Production of amorphous glass) The amorphous glass can be produced, for example, by the following method. Note that the production method described below is an example of the case of producing a plate-shaped chemically strengthened glass.

[0103] Glass raw materials are mixed so as to obtain glass of a desired composition, and are heated and melted in a glass melting furnace. The molten glass is then homogenized by bubbling, stirring, adding a clarifier, etc., and formed into a glass plate of a predetermined thickness by a known forming method, and slowly cooled. Alternatively, the molten glass may be formed into a block shape, slowly cooled, and then cut into a plate shape.

[0104] Examples of the forming method of plate glass include the float method, the press method, the fusion method, and the down-draw method. In particular, when producing a large glass plate, the float method is preferred. In addition, continuous forming methods other than the float method, such as the fusion method and the down-draw method, are also preferred.

[0105] (Crystallization treatment) When the lithium aluminosilicate glass in the present invention is crystallized glass, the crystallized glass can be obtained by heat-treating the crystallizable amorphous glass obtained by the above procedure.

[0106] The heat treatment is preferably a two-stage heat treatment in which the temperature is raised from room temperature to a first treatment temperature and held for a certain period of time, and then the temperature is held for a certain period of time at a second treatment temperature that is higher than the first treatment temperature.

[0107] In the case of two-stage heat treatment, the first treatment temperature is preferably in a temperature range where the crystal nucleation rate is high in the glass composition, and the second treatment temperature is preferably in a temperature range where the crystal growth rate is high in the glass composition. In addition, the holding time at the first treatment temperature is preferably long so that a sufficient number of crystal nuclei are generated. By generating a large number of crystal nuclei, the size of each crystal becomes small, and a highly transparent crystallized glass is obtained.

[0108] The first treatment temperature is, for example, 450° C. to 700° C., and the second treatment temperature is, for example, 600° C. to 800° C. After being held at the first treatment temperature for 1 to 6 hours, the second treatment temperature is held for 1 to 6 hours.

[0109] The crystallized glass obtained by the above procedure is ground and polished as necessary to form a crystallized glass plate. When the crystallized glass plate is cut into a predetermined shape and size or chamfered, it is preferable to perform the cutting or chamfering before the chemical strengthening treatment, because a compressive stress layer is formed on the end surface by the subsequent chemical strengthening treatment.

[0110] <Method of manufacturing chemically strengthened glass> The chemically strengthened glass of the present invention is produced by chemically strengthening lithium aluminosilicate glass. The preferred embodiment of the lithium aluminosilicate glass in this production method is the same as that described above. The lithium aluminosilicate glass in this production method preferably has the composition described above.

[0111] Lithium aluminosilicate glass can be produced by a conventional method. For example, the raw materials of the glass components are mixed and heated and melted in a glass melting furnace. The glass is then homogenized by a known method, formed into a desired shape such as a glass plate, and slowly cooled.

[0112] Examples of glass forming methods include the float method, the press method, the fusion method, and the down-draw method. In particular, the float method, which is suitable for mass production, is preferred. Continuous forming methods other than the float method, such as the fusion method and the down-draw method, are also preferred.

[0113] Thereafter, the molded glass is ground and polished as necessary to form a glass substrate. When the glass substrate is cut into a predetermined shape and size or chamfered, it is preferable to cut or chamfer the glass substrate before carrying out the chemical strengthening treatment described later, since a compressive stress layer is formed on the end surface by the subsequent chemical strengthening treatment.

[0114] In the method for producing chemically strengthened glass of the present invention, the chemical strengthening is performed using a strengthening salt containing sodium and less than 5 mass% of potassium. In the method for producing chemically strengthened glass of the present invention, the chemical strengthening treatment may be performed in two or more stages, but one-stage strengthening is preferred in order to increase productivity.

[0115] According to the method for producing chemically strengthened glass of the present invention, K1c is 0.80 MPa / m 1 / 2 The lithium aluminosilicate glass described above is chemically strengthened using the strengthening salt to obtain CS 0 In this way, chemically strengthened glass having a compressive strength of 500 to 1000 MPa and a DOL (unit: μm) of 0.06t to 0.2t relative to the glass thickness t (unit: μm) can be obtained.

[0116] The chemical strengthening treatment is carried out, for example, by immersing the glass sheet for 0.1 to 500 hours in a molten salt such as sodium nitrate heated to 360 to 600° C. The heating temperature of the molten salt is preferably 375 to 500° C., and the immersion time of the glass sheet in the molten salt is preferably 0.3 to 200 hours.

[0117] The strengthening salt used in the method for producing chemically strengthened glass of the present invention is a strengthening salt that contains sodium and has a potassium content of less than 5 mass% in terms of potassium nitrate. The potassium content is preferably less than 2 mass%, and more preferably is substantially free. "Substantially free of potassium" means that potassium is not contained at all, or potassium may be contained as an impurity that is inevitably mixed in during production.

[0118] Examples of the reinforcing salt include nitrates, sulfates, carbonates, and chlorides. Examples of the nitrates include lithium nitrate and sodium nitrate. Examples of the sulfates include lithium sulfate and sodium sulfate. Examples of the carbonates include lithium carbonate and sodium carbonate. Examples of the chlorides include lithium chloride, sodium chloride, cesium chloride, and silver chloride. These reinforcing salts may be used alone or in combination.

[0119] Appropriate conditions for the chemical strengthening treatment may be selected in consideration of the composition (characteristics) of the glass, the type of molten salt, and the desired chemical strengthening characteristics. EXAMPLES

[0120] The present invention will be described below using examples, but the present invention is not limited thereto. G1 to G26 are amorphous glasses, and GC1 to GC19 are crystallized glasses. SG1 to SG21, SG25, SG31, and SG32 are examples of chemically strengthened glasses of the present invention, and SG22 to SG24 and SG26 to SG30 are comparative examples. In addition, blanks in the tables indicate that no measurements were taken.

[0121] [Preparation and evaluation of amorphous glass] Glass raw materials were mixed to obtain the glass compositions shown in Tables 1 to 3 in terms of oxide-based mole percentages, and then melted and polished to produce glass plates. As glass raw materials, general glass raw materials such as oxides, hydroxides, and carbonates were appropriately selected and weighed out to obtain 900 g of glass. The mixed glass raw materials were placed in a platinum crucible, melted at 1700°C, and degassed. The glass was poured onto a carbon board to obtain a glass block. Using a portion of the obtained block, the Young's modulus, Vickers hardness, and fracture toughness of the amorphous glass were evaluated, and the results are shown in Tables 1 to 3. Blanks in the tables indicate that no evaluation was performed.

[0122] (Young's Modulus) The Young's modulus was measured by an ultrasonic method.

[0123] (Vickers hardness) The Vickers hardness was measured in accordance with the test method specified in JIS-Z-2244 (2009) (ISO6507-1, ISO6507-4, ASTM-E-384) using a Vickers hardness tester (MICRO HARDNESS TESTER HMV-2) manufactured by Shimadzu Corporation under normal temperature and humidity conditions (in this case, the room temperature was maintained at 25°C and the humidity was maintained at 60% RH). Measurements were performed at 10 points per sample, and the average was taken as the Vickers hardness of the prototype. The Vickers indenter was pressed with a load of 0.98 N for 15 seconds.

[0124] (Fracture toughness value) The fracture toughness value was measured by the DCDC method using a sample measuring 6.5 mm x 6.5 mm x 65 mm, with a 2 mm diameter through hole drilled in the 65 mm x 6.5 mm surface of the sample.

[0125] [Table 1]

[0126] [Table 2]

[0127] [Table 3]

[0128] [Preparation of glass-ceramics] The obtained glass block was processed to 50 mm x 50 mm x 1.5 mm, and then heat-treated under the conditions shown in Tables 4 and 5 to obtain crystallized glass. In the crystallization condition column of the table, the upper row indicates the nucleation treatment conditions, and the lower row indicates the crystal growth treatment conditions. For example, if 550-2 is written in the upper row and 730-2 is written in the lower row, it means that the glass was held at 550°C for 2 hours, and then at 730°C for 2 hours. Using a part of the obtained crystallized glass, it was confirmed by powder X-ray diffraction that it contained lithium metasilicate.

[0129] The obtained crystallized glass was processed and mirror-polished to obtain a crystallized glass plate with a thickness t of 0.7 mm (700 μm). A part of the remaining crystallized glass was crushed and used for the analysis of precipitated crystals. The evaluation results of the crystallized glass are shown in Tables 4 and 5. Blanks indicate that no evaluation was performed.

[0130] (Visible light transmittance) A 150 mm integrating sphere unit was used as a detector for a spectrophotometer (PerkinElmer; LAMBDA950), and the crystallized glass plate was placed in close contact with the integrating sphere to measure the transmittance at wavelengths of 380 to 780 nm. The average transmittance, which is the arithmetic mean value of the transmittances, was taken as the visible light transmittance (unit: %).

[0131] (Haze value) The haze value (unit: %) was measured using a haze meter (HZ-V3 manufactured by Suga Test Instruments Co., Ltd.) under light source C.

[0132] (X-ray diffraction: precipitated crystals and crystallization rate) The precipitated crystals were identified by powder X-ray diffraction under the following conditions. The crystallization rate was calculated from the obtained diffraction intensity by the Rietveld method. Measurement equipment: Rigaku SmartLab X-ray used: CuKα ray Measurement range: 2θ=10°~80° Speed: 10° / min Step: 0.02°

[0133] The detected crystals are shown in the columns for main crystals in Tables 4 and 5. In the tables, LS stands for lithium metasilicate.

[0134] [Table 4]

[0135] [Table 5]

[0136] [Preparation of chemically strengthened glass] GC1 to GC19 and G22 to 26 were subjected to chemical strengthening treatment under the strengthening conditions shown in Tables 6 to 9 to obtain tempered glasses SG1 to SG32. SG1 to SG21, SG25, SG31, and SG32 are examples, and SG22 to SG24 and SG26 to SG30 are comparative examples. In Tables 6 to 9, "Na100%" indicates a molten salt of 100% sodium nitrate, "Na99.7%Li0.3%" indicates a molten salt of 99.7 wt% sodium nitrate mixed with 0.3 wt% lithium nitrate, and "K100%" indicates a molten salt of 100% potassium nitrate. The results of evaluation of the obtained chemically strengthened glasses are shown in Tables 6 to 9. Blanks indicate no evaluation.

[0137] (Stress Profile) The stress value was measured using a measuring instrument SLP-2000 manufactured by Orihara Seisakusho Co., Ltd., and the compressive stress value CS of the glass surface was calculated. 0 [Unit: MPa], compressive stress value CS at a depth of 50 μm 50 The results of reading the stress [unit: MPa] and the depth DOL [unit: μm] at which the compressive stress value becomes zero are shown in Tables 6 to 9.

[0138] The stress profile of SG5 is shown in Figure 1. The reference example in Figure 1 is a stress profile of chemically strengthened glass obtained by two-stage chemical strengthening without crystallizing G21 (amorphous glass) shown in Table 2. The conditions for the two-stage chemical strengthening were a first stage of chemical strengthening using 100% sodium nitrate at 450°C for 2.5 hours, followed by a second stage of chemical strengthening using 100% potassium nitrate at 450°C for 1.5 hours.

[0139] (EPMA surface K concentration) The K concentration on the glass surface was measured using an EPMA (JXA-8500F manufactured by JEOL Ltd.). After chemical strengthening, the sample was embedded in resin and the cross section perpendicular to the main surface was mirror polished. Since it is difficult to accurately measure the concentration on the outermost surface, it was assumed that the K signal intensity at the position where the signal intensity of Si, which is thought to have almost no change in content, is half the signal intensity at the center of the plate thickness corresponds to the K concentration on the outermost surface, and the signal intensity at the center of the plate thickness corresponds to the glass composition before strengthening, and the K concentration on the outermost surface was calculated.

[0140] (Weather resistance test) The haze value was measured after leaving the specimen at 80% humidity and 80°C for 120 hours. The haze value does not change due to chemical strengthening treatment, but increases when left at 80% humidity and 80°C for 120 hours. The difference from the haze value before the test (i.e., |Haze value after test [%] - Haze value before test [%]|) is shown in the table as [Haze change (%)].

[0141] (Number of crushed pieces) Using a Vickers testing machine, a Vickers indenter with a 90° tip angle was driven into the center of the test glass plate to break it, and the number of broken pieces was recorded as the number of pieces. (If the glass plate breaks into two, the number of broken pieces is 2.) If very fine pieces were generated, the number of pieces that did not pass through a 1 mm sieve was counted and recorded as the number of broken pieces. The test was started with a Vickers indenter impact load of 3 kgf. If the glass plate did not break, the impact load was increased by 1 kgf and the test was repeated until the glass plate broke. The number of pieces that broke the first time was counted.

[0142] (Drop test) For the drop test, the obtained glass sample of 120 x 60 x 0.6 mmt was fitted into a structure whose mass and rigidity were adjusted to the size of a typical smartphone currently in use, and then a mock smartphone was prepared and allowed to freely drop onto #180SiC sandpaper. The drop height was 5 cm. If the sample did not break, it was dropped from a height of 5 cm and then dropped again, and this process was repeated until the sample broke. The average height of the 10 samples at which the sample first broke is shown in Tables 6 to 9.

[0143] [Table 6]

[0144] [Table 7]

[0145] [Table 8]

[0146] [Table 9]

[0147] As shown in Tables 6 to 9, the chemically strengthened glass of the present invention is 0 and C.S. 50 It was found that the chemically strengthened glass of the present invention had a lower haze change rate in a weather resistance test than the comparative example, and was also excellent in weather resistance.

[0148] Although the present invention has been described in detail and with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2019-118969) filed on June 26, 2019, the contents of which are incorporated herein by reference.

Claims

1. A chemically strengthened glass having a thickness of 1 mm or less, Lithium aluminosilicate glass, The lithium aluminosilicate glass is a crystallized glass, The crystallized glass has a visible light transmittance of 90% or more when converted into a glass having a thickness of 0.7 mm; Surface compressive stress value (CS 0 ), expressed using the depth DOL at which the compressive stress value becomes zero and the fracture toughness value (K1c) (CS 0 ×DOL) / K1c [unit: μm / m 1/2 ] is 40,000 to 70,000, The glass of the non-ion-exchanged portion of the chemically strengthened glass has a K1c of 0.85 MPa m 1/2 That's it, chemically strengthened glass.

2. A chemically strengthened glass having a thickness t [unit: μm], Lithium aluminosilicate glass, The lithium aluminosilicate glass is a crystallized glass, The crystallized glass has a crystallization rate of 15% or more and The visible light transmittance when converted to a thickness of 0.7 mm is 85% or more, The depth DOL [unit: μm] at which the compressive stress value becomes zero is 0.10t or more, Chemically strengthened glass, wherein the value of (t-2 × DOL) × CT / 2 [unit: μm MPa] expressed using the t, the DOL, and the internal compressive stress value CT [unit: MPa] is 20000 to 30000.

3. The chemically strengthened glass according to claim 1 or 2, wherein a surface K concentration is 1 mass% or less.

4. The chemically strengthened glass according to claim 1 or 2, wherein the average particle size of the precipitated crystals of the crystallized glass is 80 nm or less.

5. The average thermal expansion coefficient of the crystallized glass at 50° C. to 350° C. is 90×10 -7 / ℃ or more 160 x 10 -7 The chemically strengthened glass according to claim 1 or 2, wherein the temperature is 0.15 to 1.5 ° C. or less.

6. SiO 2 40 to 72% Al 2 O 3 を0.5~10%、 Li 2 Contains 15-50% O and K 2 The chemically strengthened glass according to claim 1 or 2, which substantially does not contain O.

7. The chemically strengthened glass according to claim 1 or 2, wherein the crystallized glass contains lithium metasilicate crystals.

8. Surface compressive stress value CS 0 The chemically strengthened glass according to claim 1 or 2, wherein the compressive strength is 500 MPa or more.

9. A method for producing chemically strengthened glass, comprising chemically strengthening a lithium aluminosilicate glass having a thickness t [unit: μm], The lithium aluminosilicate glass is obtained by subjecting amorphous glass to a two-stage heat treatment, and has a fracture toughness value (K1c) of 0.85 MPa m 1/2 The above crystallized glass is The chemical strengthening is a chemical strengthening using a strengthening salt containing sodium and having a potassium content of less than 5% by mass, The crystallized glass has a visible light transmittance of 85% or more when converted into a glass having a thickness of 0.7 mm; The depth DOL [unit: μm] at which the compressive stress value of the chemically strengthened glass becomes zero is 0.10t or more, and The value of (t-2 × DOL) × CT / 2 [unit: μm MPa] expressed using the t, the DOL, and the internal compressive stress value CT [unit: MPa] is 20000 to 30000. A method for producing chemically strengthened glass.

10. The method for producing chemically strengthened glass according to claim 9, wherein a K concentration on a surface of the chemically strengthened glass is 1 mass% or less.

11. The method for producing chemically strengthened glass according to claim 9, wherein the average particle size of the precipitated crystals of the crystallized glass is 80 nm or less.

12. The average thermal expansion coefficient of the crystallized glass at 50° C. to 350° C. is 90×10 -7 / ℃ or more 160 x 10 -7 The method for producing chemically strengthened glass according to claim 9, wherein the temperature is 0.15 to 1.5° C. or less.

13. SiO 2 40 to 72% Al 2 O 3 を0.5~10%、 Li 2 Contains 15-50% O and K 2 The method for producing chemically strengthened glass according to claim 9, which substantially does not contain O.

14. The method for producing chemically strengthened glass according to claim 9, wherein the crystallized glass contains lithium metasilicate crystals.

15. The surface compressive stress value CS of the chemically strengthened glass 0 The method for producing chemically strengthened glass according to any one of claims 9 to 14, wherein the compressive strength is 500 MPa or more.

Citation Information

Patent Citations

  • Inorganic composition article

    JP2008254984A

  • High-strength glass ceramic having a petalite and lithium silicate structure

    JP2017530933A

  • High strength glass ceramic having lithium disilicate and β-spodumene structure

    JP2019081705A

  • Chemically strengthened glass and production method therefor

    WO2019022035A1

  • Chemically strengthened glass

    JP2013520388A