Pellicle
By applying tensile strain and a reinforcing body to the pellicle membrane, the issues of sagging and shaking are mitigated, ensuring stable operation of large pellicles during high-speed movements.
Patent Information
- Application Number
- JP2024152958
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing pellicles used in semiconductor and flat panel display manufacturing face issues with sagging and shaking due to their own weight and external forces, leading to potential contact with equipment components, especially when moved at high speeds, and are not suitable for large sizes exceeding 1000 mm.
Applying tensile strain of 1% to 2.5% in the long axis direction and 0.5% to 2% in the short axis direction to the pellicle membrane, combined with a reinforcing body, to stabilize the pellicle membrane and prevent sagging and shaking.
The solution effectively reduces pellicle membrane sway to acceptable levels, minimizing the risk of contact with equipment components even at high speeds, making it suitable for large pellicles exceeding 1000 mm.
Smart Images

Figure 2024164298000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a pellicle used as a dust shield when manufacturing semiconductor devices, printed circuit boards, flat panels, etc., and in particular to a pellicle used in the manufacture of FPD devices such as liquid crystal displays, with at least one side length exceeding 1000 mm. [Background technology]
[0002] In the manufacture of semiconductors such as LSI and VLSI, or flat panel display panels used in liquid crystal displays and organic electroluminescence displays, patterns are created by irradiating ultraviolet light onto a semiconductor wafer or a glass plate for liquid crystal displays coated with photoresist. However, if dust adheres to the photomask used in this process, the dust can block or reflect the ultraviolet light, causing deformation or shorting of the transferred pattern and compromising quality.
[0003] For this reason, these operations are usually performed in a clean room, but even so, it is difficult to keep the photomask clean at all times. Therefore, a pellicle is attached to the surface of the photomask as a dust protection before exposure. In this case, foreign particles do not adhere directly to the surface of the photomask, but to the pellicle, so if the focus is set on the photomask pattern during lithography, the foreign particles on the pellicle will not affect the transfer.
[0004] In a typical pellicle, a transparent pellicle film made of nitrocellulose, cellulose propionate, fluororesin, or the like, which transmits ultraviolet light well, is adhered to the frame surface of a pellicle frame made of aluminum alloy, stainless steel, engineering plastic, etc. Furthermore, an adhesive layer made of polybutene resin, polyvinyl acetate resin, acrylic resin, silicone resin, or the like for mounting on a photomask is provided on the frame surface on the opposite side of the pellicle film, and a release layer (separator) is attached as necessary to protect the adhesive layer.
[0005] As mentioned above, pellicle membranes are generally made of thin resin, so they are stretched over a pellicle frame with an appropriate amount of tension to prevent wrinkles. However, the pellicle membrane also has its own weight, and so no matter what kind of pellicle it is, it will sag downward, even if only slightly.
[0006] Fig. 9 shows a cross-sectional view of a photomask with a pellicle attached. Normally, in an exposure machine, a photomask 91 is placed so that the surface on which an exposure pattern 92 is drawn faces downward. A pellicle 99 is attached to the lower surface of the photomask 91 via a mask adhesive layer 96 so as to cover the exposure pattern 92.
[0007] If the amount of sagging x of the pellicle film 98 due to its own weight is large, the apex y of the pellicle film 98 (usually the center of the pellicle) will protrude downward from the photomask 91, posing the risk of interfering with equipment components inside the exposure machine or foreign object inspection machine (not shown). In the case of a typical exposure machine, taking into account the mounting tolerances of the pellicle itself and each component, the allowable amount of protrusion of the pellicle film is at least 0.8 mm or less, and more preferably 0.6 mm or less. If the exposure machine and foreign object inspection machine use the same optical system, approximately the same value is required for this allowable value even if the pellicle is large.
[0008] However, in recent years, the moving speed of the photomask in the exposure machine has become faster, so the wind pressure that the pellicle film receives during movement and the air bias inside the pellicle due to inertia at the start and stop of movement have become larger. As a result, in addition to the sagging amount x due to its own weight, the swaying of the pellicle film due to operation has become larger, and the risk of the pellicle film contacting the device has increased significantly. As a result, a smaller value of the sagging amount x due to the film's own weight has been required, and in recent years, 0.35 mm or less has been required in general, and in some cases, 0.2 mm or less has been required. In addition, the required value of the film swaying amount cannot be generalized because the requirements differ depending on the applied device and operating conditions, but for example, it is preferable that under any conditions, for a pellicle with a side length of more than 1 m, it is at least 4 mm or less, and for a pellicle with a side length of more than 1.5 m, it is at least 5 mm or less.
[0009] In response to this problem, the present inventor previously proposed an invention for a pellicle in which thin linear reinforcements with a thickness of 100 μm or less and made of a material different from the pellicle membrane are stretched between two parallel sides of the pellicle frame, and the thin linear reinforcements are in contact with the outside of the pellicle membrane (Patent Document 1). [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Patent No. 5618888 Summary of the Invention [Problem to be solved by the invention]
[0011] In this invention, the reinforcing body suppresses the self-weight sagging of the pellicle membrane, but since the reinforcing body is defocused, it has no effect on the exposure quality. This method can suppress the self-weight deflection to 0.3 mm even for large pellicles with a side length of over 2000 mm, making it a very effective method for suppressing self-weight sagging. However, there is a problem that the productivity is extremely poor and it is not suitable for mass production.
[0012] Furthermore, the essential purpose of suppressing the amount of deflection x of the pellicle film due to its own weight is to prevent contact of the pellicle film within the apparatus, as described above, but simply reducing the amount of deflection x of the pellicle film due to its own weight is not sufficient to suppress the amount of shaking of the pellicle film caused by external forces when the pellicle attached to the photomask is moved, and the risk of pellicle film contact is not necessarily reduced.
[0013] Furthermore, as described in detail in Patent Document 1, the air flows extremely slowly through the air vent 94 and filter 95, and the self-weight deflection amount x is constantly fluctuating due to changes in air pressure and temperature, and also due to the humidity, depending on the material of the pellicle membrane, causing it to expand and contract, making it somewhat unsuitable as an indicator of safety.
[0014] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a pellicle having at least one side length exceeding 1000 mm, in which the amount of vibration of the pellicle membrane is small when the pellicle attached to a photomask is moved at high speed. [Means for solving the problem]
[0015] After extensive research, the inventors discovered that in order to reduce the amount of vibration of the pellicle membrane when the pellicle attached to the photomask moves, it is important to apply tensile strain to the pellicle membrane while adhering it to the pellicle frame, and that the direction of this strain is important, and thus completed the present invention.
[0016] The solution of the present invention is a pellicle comprising a pellicle frame having at least one side length exceeding 1000 mm and a pellicle membrane bonded to one of the frame-like surfaces, characterized in that a tensile strain of 1% to 2.5% is imparted to the pellicle membrane in a direction parallel to a pair of pellicle frame sides that are parallel and line-symmetric to each other (long axis direction).Furthermore, by imparting a tensile strain of 0.5% to 2% to the pellicle membrane in a direction perpendicular to the pair of pellicle frame sides (short axis direction) and bonding and fixing the pellicle membrane to the pellicle frame, wrinkles in the pellicle membrane can be prevented.
[0017] Furthermore, if the material of the pellicle film is an amorphous fluororesin, the amount of vibration of the pellicle film can be kept small without being affected by environmental changes.
[0018] Furthermore, an invention that adds the features of Patent Document 1 provided by the present inventor to the above-mentioned features of the present invention will also be an effective embodiment in the case of an extra-large pellicle. That is, in this embodiment, at least one linear reinforcement body having a thickness of at most 100 μm is stretched between two opposing sides of the pellicle frame so as to be bonded to the pellicle film to which the tensile strain of the present invention has been applied. Alternatively, in this embodiment, two linear reinforcement bodies having a thickness of at most 100 μm are stretched along the diagonal line of the pellicle frame so as to be bonded to the pellicle film to which the tensile strain of the present invention has been applied. Specific details of these are disclosed in Patent Document 1. Furthermore, the present invention relates to a pellicle-attached photomask having the above-mentioned pellicle attached to a photomask, an exposure method characterized by exposing using the pellicle-attached photomask, and a method for manufacturing a panel for a flat panel display, comprising a step of exposing using the pellicle-attached photomask. Effect of the Invention
[0019] According to the present invention, by applying a tensile strain of 1 to 2.5% in a direction parallel to the long side of the pellicle film (long axis direction) and bonding it to a pellicle frame, the amount of vibration of the pellicle film when moved at high speed can be suppressed to a small amount even for a large pellicle with a side length exceeding 1000 mm. As a result, the risk of the pellicle film coming into contact with equipment parts in an exposure machine or a foreign body inspection machine is reduced. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a plan view showing one embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view taken along line AA of FIG. 1, illustrating one embodiment of the present invention. [Diagram 3] FIG. 1 is an explanatory diagram showing the behavior of a pellicle film when a photomask with a pellicle attached thereto is moved horizontally. [Figure 4] FIG. 1 is a plan view showing one embodiment of the present invention. [Diagram 5] 1 is a cross-sectional view for explaining a method for peeling off a pellicle film using a support frame used in the present invention. FIG. [Figure 6] FIG. 2 is a schematic plan view of a support frame used in the present invention. [Figure 7] FIG. 2 is a perspective view of a support frame tensioning mechanism for use in the present invention; [Figure 8] FIG. 2 is a schematic perspective view of a pellicle produced according to an embodiment. [Figure 9] FIG. 2 is a schematic cross-sectional view of a photomask with a pellicle attached thereto. [Figure 10] FIG. 13 is a schematic plan view of a support frame used in a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The best mode for carrying out the present invention will be described below, but the present invention is not limited thereto.
[0022] 1 and 2 show an embodiment of the present invention. FIG. 1 is a plan view, and FIG. 2 is an AA cross-sectional view of FIG. 1. A pellicle film adhesive layer 12 is provided on the upper frame-shaped surface of a pellicle frame 11, and a pellicle film 13 is adhered to the pellicle frame. A mask adhesive layer 14 is provided on the frame-shaped surface on the opposite side. In this embodiment, the outer shape of the pellicle frame 11 is rectangular, but it may be other shapes similar to this, such as a square or octagon. The pellicle film 13 is adhered to the pellicle frame 11 via the pellicle film adhesive layer 12 in a state where a tensile strain of a predetermined rate is applied in the long axis direction (arrow a direction). This tensile strain is preferably 1% or more and 2.5% or less. Here, the tensile strain is a value expressed by the following formula. Tensile strain (%) = strain amount (tensile amount) (mm) / outer dimension of pellicle membrane in the tensile direction before strain (mm) × 100
[0023] A typical pellicle film is tensioned to a certain extent in order to adhere to the pellicle frame without wrinkles, but this amount is equivalent to about 0.5% in terms of distortion. In addition, in the conventional technology, the tension was adjusted by pulling or pushing the center of the side of the support frame 100 that holds the pellicle film, as shown in Figure 10, so it was not possible to take into account the position, size, or direction.
[0024] The resin pellicle film 13 is stretchable, and by applying tensile strain within the elastic range, resistance to external forces can be increased. The effect of reducing the amount of film sway is greater at tensile strains of 0.5% or more, and from that perspective, the higher the better. In the case of materials that have a yield point against tension, tensile strain can be applied up to near the yield point; for example, in the case of fluororesin, the elongation at the yield point is about 10%, so tensile strain of up to about 9% can be applied.
[0025] However, on the other hand, the higher the tensile strain, the lower the resistance to external damage. Even if the external damage caused by contact or the like is slight, depending on the direction, the cracks that occur may propagate all at once and lead to the total damage of the pellicle membrane. In addition, a large shear stress is constantly applied to the pellicle membrane adhesive layer, which is a concern in terms of the reliability of the adhesion. Considering the balance between the effect of reducing the film vibration, the adhesive strength of the adhesive, and the resistance to external damage, the most suitable range of tensile strain is 1% or more and 2.5% or less. In addition, this tensile strain can be appropriately adjusted depending on the position on the frame. For example, it is also good to particularly increase the tensile strain near the longitudinal central axis where the amount of vibration of the pellicle membrane is large.
[0026] Normally, when a photomask is rectangular, the direction of movement of the photomask inside the exposure machine is the long axis direction. Figure 3 shows the swaying of the pellicle film when a photomask with a pellicle is moved and suddenly stopped. This figure is a cross section on the longitudinal center axis, with the arrow indicating the direction of movement of the photomask with a pellicle, and the two-dot chain line indicating the behavior of the pellicle film when the swaying is greatest.
[0027] The vibration of the pellicle film occurs with the movement of the photomask. Although it is also affected by wind pressure from the outside when passing through a narrow space, the largest vibration occurs when the air inside the pellicle is biased in one direction due to inertia when the movement starts or stops. In the example of Figure 3, the air inside the pellicle moves to the right due to a sudden stop to the right, which causes a recess in part B of the pellicle film and a protrusion in part C. This corresponds to the areas B and C surrounded by dotted lines in the plan view of Figure 1. In the present invention, by applying a large tensile strain in the long axis direction, the resistance to the bias of the air, especially in this direction, is increased, so that the amount of film vibration can be effectively suppressed.
[0028] Fig. 4 shows a plan view of another embodiment of the present invention. A tensile strain is applied to the pellicle film 43 in the short axis direction (arrow b) in addition to the long axis direction (arrow a) in the embodiment of Fig. 1, and the pellicle film 43 is bonded to the pellicle frame 41 via the pellicle film adhesive layer 42. The tensile strain in the short axis direction is preferably 0.5% to 2%. When a tensile strain is applied to the pellicle film in the long axis direction, shrinkage occurs in the short axis direction due to the Poisson effect, so the purpose is to prevent wrinkles from occurring. Also, from the viewpoint of preventing a decrease in resistance to external damage, it is not necessary to increase the tensile strain applied in the short axis direction.
[0029] In addition, the pellicle film may be made of a known material, such as a cellulose-based resin such as nitrocellulose or cellulose propionate, or an amorphous fluororesin. Among these, it is particularly preferable to use an amorphous fluororesin. Since an amorphous fluororesin does not undergo dimensional changes due to moisture absorption, and does not undergo a decrease in film thickness due to etching even when short-wavelength ultraviolet light with a wavelength of 300 nm or less is used, the applied tensile strain amount can be stably maintained for a long period of time, and no fluctuation occurs in the amount of film vibration. In addition, since it is amorphous, it has the advantage that cracks are relatively difficult to propagate, and it is resistant to external damage even when a large tensile strain amount is applied.
[0030] Next, the method for producing the pellicle of the present invention will be described in detail. A solution of pellicle film material is applied onto a substrate made of smoothly polished quartz, low expansion glass, or the like, by a known coating method such as spin coating or slit coating, and the solvent is completely evaporated using a heating method such as an oven, hot plate, or IR lamp, to obtain a layer of dried pellicle film on the substrate.
[0031] After cooling, the pellicle film is peeled off from the deposition substrate. As shown in the cross-sectional view of FIG. 5, peeling is preferably performed by adhering the film support 52 of the support frame 50 to the end of the pellicle film 54 on the substrate 55, and slowly lifting it from the corner to peel it off. A plan view of the pellicle film supported by the support frame 50 is shown in FIG. 6. The support frame 50 is composed of an outer frame 51, a film support 52, and a tension mechanism 53. In this embodiment, the support frame 50 is adhered and the pellicle film 54 on the substrate 55 is peeled off, but the pellicle film may be peeled off by another means and then the support frame 50 may be attached.
[0032] The outer frame 51 is preferably made of a rigid material and structure so as not to bend when a tensile strain is applied to the pellicle membrane 54. The membrane supports 52 support the periphery of the pellicle membrane by dividing it into sections each having a width of about 20 to 100 mm, and the pellicle membrane 54 is adhered to the membrane by an adhesive applied to the surface, double-sided tape, or other adhesive means (not shown). The narrower the membrane support 52 is, the more finely the tensile strain can be adjusted, but on the other hand, a narrow width also significantly increases the complexity of the work, so it is best to determine the support width by comprehensively taking into consideration the size of the membrane, productivity, the tendency for wrinkles to form, etc.
[0033] The membrane supports 52 are arranged with a gap of 5 mm or less between adjacent ones, and each is supported by the outer frame 51 via a tensioning mechanism 53, and the tension amount can be adjusted individually. A perspective view of the tensioning mechanism 53 is shown in FIG. 7. The tensioning mechanism 53 is mounted on a linear moving means consisting of a rail 71 and a slider 72 that can move in a direction d perpendicular to the tensioning direction c, and can move freely following the displacement of the membrane when tensile strain is applied. As the tensioning means, this embodiment uses a screw mechanism consisting of a female screw portion 73 and a male screw portion 74, but is not limited to this. The membrane support 52 having a membrane adhesive layer 75 on its surface made of adhesive or double-sided tape is attached to the tip of the male screw portion 74 in a state free from the rotation of the male screw portion 74, and the membrane support 52 moves in the tensioning direction c by rotating the male screw portion 74.
[0034] With the pellicle film 54 supported by the support frame 50, the tension mechanism 53 is operated to impart a desired amount of tensile strain to the pellicle film 54. The more the film support 52 is moved back, the greater the amount of tensile strain to be imparted, but the amount of movement is operated so that the opposing film supports 52 are the same amount. It is preferable to operate the film first in the long axis direction, which imparts the greatest amount of tensile strain, and then in the short axis direction. Finally, it is confirmed that no wrinkles have occurred in the pellicle film 54, and then, in the same manner as in the normal pellicle manufacturing method, the pellicle film 54 is adhered to the pellicle film adhesive layer of the pellicle frame to complete the pellicle. EXAMPLES
[0035] Examples of the present invention will be described below, but the present invention is not limited to these examples. EXAMPLES
[0036] A pellicle 80 shown in the perspective view of FIG. 8 was manufactured. The pellicle frame 81 was a rectangle manufactured by machining using A5052 aluminum alloy, with outer dimensions of 1526×1748 mm and inner dimensions of 1493×1715 mm, with a height of 6.0 mm and corner shapes of inner R2 and outer R6. In addition, two recessed holes 82 with a diameter of 2.5 mm and a depth of 2 mm were provided on each of the long outer sides for handling purposes, a groove 83 with a height of 2 mm and a depth of 3 mm was provided on the short outer side, and similarly, grooves 84 with a height of 2 mm and a depth of 3 mm were provided on three of the long outer sides. In addition, eight ventilation holes 85 with a diameter of 1.5 mm and eight filters 86 were provided on each of the long sides. Finally, the surface was sandblasted and then black anodized.
[0037] This pellicle frame 81 was brought into a clean room, thoroughly washed with a surfactant and pure water, and dried. Then, a silicone adhesive was applied to one frame-shaped surface of the pellicle frame as a pellicle film adhesive layer 88, and a silicone adhesive (manufactured by Shin-Etsu Chemical Co., Ltd.) was diluted with toluene and applied to the other frame-shaped surface as a mask adhesive layer 87 to a thickness of 2 mm using an air-pressurized dispenser, and cured by heating.
[0038] Next, a pellicle film material solution in which an amorphous fluororesin (product name: Cytop, manufactured by Asahi Glass Co., Ltd.) was dissolved was applied to a smoothly polished quartz substrate 55 of 1620×1780×thickness 17 mm by a slit die coater. The amount of application was set so that the film thickness after drying would be 3.9 μm. Next, this was heated to 180° C. in an oven to dry off the solvent.
[0039] A support frame 50 was attached to the pellicle film 54 on the substrate 55 as shown in Fig. 5. The tension mechanism of the support frame 50 has the structure shown in Fig. 7. A film adhesive layer 75 made of a double-sided silicone tape provided on the lower surface of the film support 52 was attached to the pellicle film 54 at the edge of the substrate, and then the support frame 50 was slowly lifted up from the corner. Fig. 6 is a plan view showing the state after peeling.
[0040] Next, the tension mechanism 53 was operated to move the membrane support 52 toward the center of the membrane, and the position where the pellicle membrane began to loosen was determined. Using this position as a reference, the opposing tension mechanisms 53 arranged on the short sides were simultaneously operated to apply a tensile strain in the long axis direction to the pellicle membrane. The amount of stretch applied at this time was 41 mm, which was a tensile strain of about 2.3% in terms of elongation, and the operation was performed sequentially from the center of the short side to the outside. Next, the tension mechanism 53 arranged on the long side was operated in the same way, and a tensile strain of 30 mm in the short axis direction, which was a tensile strain of about 1.9% in terms of elongation, was applied. Finally, the entire membrane was visually observed to confirm that no wrinkles had occurred.
[0041] The support frame 50 supporting the pellicle film 54 to which tensile strain was imparted in the long axis and short axis directions was then moved, and as shown in Fig. 8, a pellicle film 89 was adhered to the pellicle film adhesive layer 88 on the pellicle frame 81 produced as described above, and the excess film around the pellicle was cut off with a cutter to complete the pellicle 80. In this Example 1, the tensile strain was imparted in the directions a and b shown in Fig. 4.
[0042] The completed pellicle 80 was attached to a quartz substrate measuring 1620 mm x 1780 mm x 17 mm thick, and then mounted on a motion mechanism consisting of a linear guide and a slider. It was then moved horizontally as shown in Figure 3, and the amount of film vibration during the movement was measured using a laser distance sensor. The results were a speed of 1300 mm / s and an acceleration of 2940 mm / s. 2 , deceleration 2940mm / s 2 Under these conditions, the maximum vibration of the pellicle membrane on the protruding side was approximately 2.3 mm, which was a value that did not cause any concern about membrane contact. EXAMPLES
[0043] Pellicle were produced in the same manner as in the above-mentioned Example, by changing the amount of strain applied to the pellicle membrane. The amount of stretch applied was a tensile strain of 19 mm in the long axis direction, or about 1.1%, and 10 mm in the short axis direction, or 0.6%, in terms of stretch rate. When the amount of membrane sway of the completed pellicle was evaluated under exactly the same conditions as in the above-mentioned Example, the maximum amount of sway of the pellicle membrane was about 3.7 mm, which was practically a level at which there was no concern about membrane contact. Comparative Example
[0044] As in Example 1, a pellicle film material solution in which amorphous fluororesin (product name Cytop, manufactured by Asahi Glass Co., Ltd.) was dissolved was applied by a slit die coater on a smoothly polished quartz substrate of 1620 x 1780 x 17 mm thickness, and the solution was dried. A support frame 100 as shown in FIG. 10 was attached to the periphery of the pellicle film on the substrate, and the pellicle film 101 was obtained by slowly peeling it off from the corner. In the above Examples 1 and 2, the pellicle film was peeled off and held by the support frame 50, and tensile strain was applied by the tension mechanism, but the support frame 100 in this comparative example does not have a tension mechanism. In order to prevent wrinkles, the center of each long side and each short side of the pellicle film 101 was pulled outward as shown by the arrows in the figure, and while maintaining this state, it was adhered to the pellicle film adhesive layer on the pellicle frame manufactured in the same manner as in Examples 1 and 2 above, and the excess film around the frame was cut off with a cutter to complete the pellicle. In this case, when the center of the side of the support frame 100 is pulled, the whole side bends and pulls the membrane, and the amount of tension of the long side and the short side influence each other. Therefore, the amount of tension cannot be simply compared with the above example, but for reference, when the tensile strain was measured at the center of the side, it was about 0.5% for both the long side and the short side.
[0045] When the amount of film swaying of the completed pellicle was evaluated under exactly the same conditions as in Examples 1 and 2 above, the maximum amount of swaying of the pellicle membrane was approximately 5.2 mm on the protruding side, which was at a level that raised concerns that the pellicle membrane might come into contact with other parts of the device. [Explanation of symbols]
[0046] 11 Pellicle frame 12 Pellicle membrane adhesive layer 13 Pellicle membrane 14 Mask adhesive layer 15 Photomask 41 Pellicle Frame 42 Pellicle membrane adhesive layer 43 Pellicle membrane 50 Support slots 51 Outer Frame 52 Membrane support 53 Tension Mechanism 54 Pellicle membrane 55 Substrate 71 Rail 72 Slider 73 Female thread 74 Male thread 75 Membrane adhesive layer 80 Pellicle 81 Pellicle Frame 82 Hole 83 Groove (short side) 84 Groove (long side) 85 Ventilation Hole 86 Filters 87 Mask adhesive layer 88 Pellicle membrane adhesive layer 89 Pellicle Membrane 91 Photomask 92 Exposure Pattern 93 Pellicle Frame 94 Ventilation holes 95 Filters 96 Mask adhesive layer 97 Pellicle membrane adhesive layer 98 Pellicle Membrane 99 Pellicle 100 Support Slots 101 Pellicle membrane A Long axis center B Area with large membrane vibration (concave) C Area with large membrane vibration (convex) a Tensile direction (longitudinal direction) b Tensile direction (minor axis direction) c Tensile direction d Perpendicular to the tensile direction x Deflection of the pellicle membrane due to its own weight y Apex (center) of pellicle membrane
Claims
[Claim 1] A pellicle comprising a pellicle frame having at least one side length exceeding 1000 mm and a pellicle membrane adhered to one of the frame-shaped surfaces, characterized in that a tensile strain of 1% or more and 2.5% or less is imparted to the pellicle membrane in a direction parallel to a pair of pellicle frame sides that are parallel and line-symmetric to each other.
Citation Information
Patent Citations
Photomask housing device, projection aligner, projection aligning method and semiconductor equipment
JP2002268203A
Method of manufacturing pellicle, and pellicle
JP2013195852A
Mahjong tile
JP1981018888A