Hydraulic composition

A cement-free hydraulic composition with specific components and additives addresses the performance gaps in laminates, ensuring excellent retention, smoothness, and lamination, while reducing emissions.

JP2024164511APending Publication Date: 2024-11-27TAISEI CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023080043
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-27

AI Technical Summary

Technical Problem

Existing hydraulic compositions used in laminates for 3D printing lack optimal performance in temporal retention, surface smoothness, and stackability, which are crucial for high-quality laminates.

Method used

A cement-free hydraulic composition comprising pulverized blast furnace slag, pulverized limestone, an expanding agent, slaked lime, fine aggregate, and a thickening admixture, with specific ratios and additives to enhance retention, surface smoothness, and laminability.

Benefits of technology

The composition achieves excellent retention over time, smooth surface, and improved lamination properties, reducing CO2 emissions and avoiding issues like efflorescence and temperature cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164511000001_ABST
    Figure 2024164511000001_ABST
Patent Text Reader

Abstract

To provide: a hydraulic composition, which is excellent in all indices of time retention, surface smoothness, and laminability; a laminate; and a method for manufacturing the laminate.SOLUTION: A hydraulic composition according to the present invention does not contain cement but includes blast furnace slag fine powder, limestone fine powder, an expansive agent, hydrated lime, fine aggregate and a thickening admixture. A laminate according to the present invention is made by laminating the hydraulic composition. A method for manufacturing the laminate according to the present invention includes a step of laminating the hydraulic composition that does not contain the cement but includes the blast furnace slag powder, the limestone fine powder, the expansive agent, the hydrated lime, the fine aggregate, a retardant admixture, and the thickening admixture, using a laminating device that uses a material extrusion method.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hydraulic composition, a laminate formed by laminating hydraulic compositions, and a method for producing a laminate formed by laminating hydraulic compositions. [Background technology]

[0002] In recent years, companies in the construction industry have been working to develop and improve new materials and construction methods with the aim of reducing CO2 emissions. The applicant has proposed a hydraulic composition that contains ground granulated blast furnace slag, an industrial by-product, instead of cement, as shown in Patent Document 1. This hydraulic composition contains a specified amount of stimulant and specifies the amount of calcium hydroxide contained, thereby ensuring material properties such as strength while reducing the amount of cement used and thereby reducing CO2 emissions. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6137850 Summary of the Invention [Problem to be solved by the invention]

[0004] The inventors of the present invention have thoroughly studied hydraulic compositions that do not use cement (see Patent Document 1), and as a result have identified three particularly important indicators for providing high-quality laminates by 3D printing. Specifically, there are three indicators: "retention over time," which is an indicator of whether the material can maintain a state in which it can be appropriately laminated for a long time, "surface smoothness," which is an indicator of the surface properties of the laminate after lamination, and "laminability," which is an indicator of how high it can be laminated. Therefore, the present inventors intended to create a hydraulic composition that is excellent in all of the indices of "retention over time," "surface smoothness," and "laminability" by adjusting the composition of the materials.

[0005] From this viewpoint, an object of the present invention is to provide a hydraulic composition, a laminate, and a method for producing a laminate, which are excellent in all indices of retention over time, surface smoothness, and lamination properties. [Means for solving the problem]

[0006] The above problems can be solved by the following measures. The hydraulic composition according to the present invention is a cement-free hydraulic composition, and contains ground granulated blast furnace slag, ground limestone, an expansive material, slaked lime, fine aggregate, and a thickening admixture. According to the present invention, the hydraulic composition is excellent in all indices of retention over time, surface smoothness, and lamination properties, by specifying the composition. The hydraulic composition according to the present invention preferably has a time period of 60 minutes or more during which the vane shear resistance value, which changes with time after the addition of water, is 0.4 to 0.9 kPa. The hydraulic composition according to the present invention preferably has a water-powder ratio of 30.0% or less. The hydraulic composition according to the present invention preferably contains a retarding admixture, and the thickening admixture is preferably 0.035 to 0.060 parts by mass per 100 parts by mass of the ground granulated blast furnace slag, and the retarding admixture is preferably 0.700 parts by mass or less per 100 parts by mass of the ground granulated blast furnace slag. According to the present invention, the hydraulic composition is more reliably excellent in all indices of retention over time, surface smoothness, and lamination properties. The laminate according to the present invention is obtained by laminating the above hydraulic compositions. According to the present invention, the laminate is produced by laminating hydraulic compositions having excellent retention over time, and thus has a smooth surface and excellent lamination properties. The method for manufacturing a laminate according to the present invention includes a step of laminating a hydraulic composition that does not contain cement and that contains ground granulated blast furnace slag, ground limestone, an expansive material, hydrated lime, fine aggregate, a retarding admixture, and a thickening admixture, using a material extrusion type lamination device. According to the present invention, a laminate having excellent surface smoothness and lamination properties can be produced by laminating a hydraulic composition having excellent retention over time. Effect of the Invention

[0007] The hydraulic composition according to the present invention is excellent in all indices of retention over time, surface smoothness and lamination properties. The laminate according to the present invention is laminated with a hydraulic composition having excellent retention over time, and has excellent surface smoothness and lamination properties. The method for producing a laminate according to the present invention can produce a hydraulic composition having excellent surface smoothness and lamination properties by laminating a hydraulic composition having excellent retention over time. [Brief description of the drawings]

[0008] [Figure 1] 4 is a graph showing the change over time in vane shear resistance value of a hydraulic composition. [Diagram 2] 1 is a photograph showing the appearance of a laminate of Sample 1. [Diagram 3] 1 is a photograph showing the appearance of the laminate of Sample 2. [Figure 4] 1 is a photograph showing the appearance of a laminate of Sample 3. [Diagram 5] 1 is a photograph showing the appearance of the laminate of Sample 4. [Figure 6] 1 is a photograph showing the appearance of a laminate of Sample 5. [Figure 7] 1 is a photograph showing the appearance of a laminate of Sample 6. [Figure 8] 1 is a photograph showing the appearance of the laminate of Sample 7. [Figure 9] 1 is a photograph showing the appearance of a laminate of Sample 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the hydraulic composition according to this embodiment, a laminate obtained by laminating the hydraulic composition, and a method for producing a laminate obtained by laminating the hydraulic composition will be described. [Hydraulic composition] The hydraulic composition according to this embodiment is a cement-free hydraulic composition (a so-called zero-cement type composition), and includes ground granulated blast furnace slag, ground limestone, an expansive material, slaked lime, fine aggregate, and a thickening admixture, and may further include a retarding admixture. The hydraulic composition according to this embodiment preferably has a vane shear resistance value that satisfies a predetermined requirement, and preferably has a water-powder ratio that is equal to or less than a predetermined value. Each of the constituent elements will be described in detail below.

[0010] (cement) The hydraulic composition according to this embodiment does not contain cement. Here, the cement specifically refers to various Portland cements as specified in JIS R5210:2009. Since the hydraulic composition does not contain cement, it is possible to reduce the amount of CO2 emissions during cement production. Also, since the hydraulic composition does not contain cement, it is possible to avoid the occurrence of "efflorescence (precipitation of calcium carbonate)" after hardening that occurs when cement is used as a material, and the occurrence of "color unevenness" on the surface of the laminate due to said phenomenon. Furthermore, since the hydraulic composition does not contain cement, it is possible to avoid the occurrence of "temperature cracking" caused by heat of hydration that becomes a problem when cement is used as a material.

[0011] (Grained blast furnace slag) Ground granulated blast furnace slag is made by drying and grinding granulated blast furnace slag, or by adding gypsum to this, and is specified in JISA6206:2013. The hydraulic composition does not contain cement, but instead contains ground granulated blast furnace slag, thereby enabling the desired effects (excellent in all indicators of retention over time, surface smoothness, and lamination) to be exhibited while enjoying the above-mentioned advantages of not using cement. (fine limestone powder) Limestone fine powder is made by crushing limestone into powder, and its main component is calcium carbonate. The content of the limestone fine powder is, for example, 5 parts by mass or more, 7 parts by mass or more, 10 parts by mass or more, and 20 parts by mass or less, 15 parts by mass or less, 13 parts by mass or less, relative to 100 parts by mass of the ground granulated blast furnace slag.

[0012] (Expansion material) An expansive agent is an admixture that has the effect of expanding concrete or mortar, and is defined in JISA6202:2017. The content of the expansion material is, for example, 4 parts by mass or more, 7 parts by mass or more, 9 parts by mass or more, and 25 parts by mass or less, 15 parts by mass or less, 13 parts by mass or less, per 100 parts by mass of the ground granulated blast furnace slag. (Slaked lime) Slaked lime is calcium hydroxide (Ca(OH)2). The content of slaked lime is, for example, 4 parts by mass or more, 7 parts by mass or more, 9 parts by mass or more, and 25 parts by mass or less, 15 parts by mass or less, 13 parts by mass or less, relative to 100 parts by mass of the ground granulated blast furnace slag.

[0013] (fine aggregate) Fine aggregates include mountain sand, river sand, sea sand, crushed sand, silica sand, and lime sand, and comply with JISA5005:2020. The content of the fine aggregate is, for example, 70 parts by mass or more, 80 parts by mass or more, 90 parts by mass or more, and 180 parts by mass or less, 150 parts by mass or less, 130 parts by mass or less, per 100 parts by mass of the ground granulated blast furnace slag.

[0014] (Water, water powder ratio) The ultra-high strength concrete according to the present embodiment contains water. Although the water content is not particularly limited, the water-powder ratio (W / P) is, for example, 15.0% or more, 20.0% or more, or 25.0% or more, and 40.0% or less, 35.0% or less, or 30.0% or less. The water is not particularly limited, and tap water, sludge water, etc. can be used.

[0015] (Thickening admixture) A thickening admixture is an admixture added to a hydraulic composition for the main purpose of improving viscosity. Examples of the thickening admixture include cellulose-based thickeners, acrylic-based thickeners, biopolymer-based thickeners, and glycol-based thickeners, and these may be used alone or in combination of two or more. The content of the thickening admixture is preferably 0.033 parts by mass or more, 0.035 parts by mass or more, or 0.039 parts by mass or more relative to 100 parts by mass of the ground granulated blast furnace slag. By having the content of the thickening admixture be equal to or more than a predetermined value, deterioration of the retention over time (and further deterioration of the surface smoothness) due to insufficient viscosity can be reliably avoided. The content of the thickening admixture is preferably 0.063 parts by mass or less, 0.060 parts by mass or less, 0.055 parts by mass or less, or 0.050 parts by mass or less, relative to 100 parts by mass of the ground granulated blast furnace slag. By making the content of the thickening admixture equal to or less than a predetermined value, deterioration of the retention over time (and further deterioration of the surface smoothness) caused by excessive viscosity can be reliably avoided.

[0016] (Retarding admixture) A retarding admixture is an admixture added to a hydraulic composition for the main purpose of delaying setting or hardening. Examples of the retarding admixture include water-reducing agents, air-entraining water-reducing agents, high-performance air-entraining water-reducing agents, and superplasticizers, which are specified as retarding agents in JISA6204:2011, and these may be used alone or in combination of two or more. The content of the retarding admixture is preferably 0.750 parts by mass or less, 0.700 parts by mass or less, 0.650 parts by mass or less, or 0.600 parts by mass or less, relative to 100 parts by mass of the ground granulated blast furnace slag. By making the content of the retarding admixture equal to or less than a predetermined value, it is possible to reliably avoid a situation in which the vane shear resistance value continues to decrease and the retention over time deteriorates (and further, the lamination property deteriorates). The lower limit of the content of the retarding admixture is not particularly limited, and is, for example, 0.010 parts by mass or more, 0.030 parts by mass or more, or 0.060 parts by mass or more relative to 100 parts by mass of the ground granulated blast furnace slag.

[0017] (Vane shear resistance value: requirement) The vane shear resistance of the hydraulic composition according to this embodiment will be described with reference to FIG. FIG. 1 is a graph showing the change over time in vane shear resistance of a hydraulic composition. A hydraulic composition is usually produced by kneading materials other than water and then adding water. As shown in Figure 1, after adding water, the vane shear resistance value first decreases significantly, and then gradually increases. The hydraulic composition preferably has a vane shear resistance value of 0.4 to 0.9 kPa for 60 minutes or more. By satisfying this requirement, the hydraulic composition is more reliably excellent in all indices of retention over time, surface smoothness, and lamination. (Vane shear resistance value: measurement method) The vane shear resistance value can be measured using a general vane testing machine according to the method specified in the "In-situ vane shear test method" of the Geotechnical Society of Japan standard (JGS 1411-012). Moreover, the intervals for measuring the vane shear resistance value may be set at regular intervals (for example, every 3 to 12 minutes, preferably every 5 to 10 minutes) from the time of adding water, and may be changed midway.

[0018] (Application) The hydraulic composition according to this embodiment can be suitably used as a material for 3D printing, and is therefore preferably used as a material for 3D printing. In addition, the proportion of cement in mortar that does not contain coarse aggregate is greater than that in general concrete. Therefore, the hydraulic composition according to the present embodiment is preferably mortar. This is because the above-mentioned advantages of not using cement (especially the reduction in CO2 emissions) can be more effectively enjoyed.

[0019] (others) The hydraulic composition according to this embodiment may appropriately contain conventionally known materials (chemical admixtures, fibers, etc.) used in mortar, as long as the desired effects of the present invention are not impaired. Examples of chemical admixtures include the thickening admixtures and retarding admixtures described above, as well as separation reducing agents, air content adjusting agents, shrinkage reducing agents, setting accelerators, defoamers, high performance water reducing agents, high performance AE water reducing agents, hardening accelerators, etc. Any one of the chemical admixtures may be used alone, or two or more may be used in combination. Examples of fibers include metal fibers, organic fibers, and composite fibers made by mixing organic fibers and metal fibers. Examples of metal fibers include steel fibers, stainless steel fibers, titanium fibers, and aluminum fibers. Examples of organic fibers include polypropylene fibers, polyvinyl alcohol fibers, aramid fibers, polyethylene fibers, ultra-high strength polyethylene fibers, polyethylene terephthalate fibers, rayon fibers, nylon fibers, polyvinyl chloride fibers, polyester fibers, acrylic fibers, and alkali-resistant glass fibers.

[0020] [Laminate] The laminate according to this embodiment is formed by laminating the above-mentioned hydraulic compositions, and is produced by the method for producing a laminate described later. The laminate according to this embodiment is produced by laminating the hydraulic composition having excellent retention over time, and therefore has a smooth surface and excellent lamination properties.

[0021] [Method of manufacturing laminate] The method for producing the laminate according to this embodiment includes a step of laminating the hydraulic composition using a lamination device of a material extrusion type. The material extrusion type lamination device may be a general 3D printing device, for example, a device consisting of a hopper for storing the hydraulic composition, a nozzle for discharging the hydraulic composition to a specified location, and a transfer mechanism for transferring the hydraulic composition in the hopper to the nozzle. In the method for producing the laminate according to this embodiment, it is preferable to laminate the hydraulic composition in a state where the vane shear resistance value of the hydraulic composition, which changes over time after addition of water, satisfies 0.4 to 0.9 kPa. EXAMPLES

[0022] [material] The composition of each sample used in the examples is shown in Table 1, and the details of each material used are shown in Table 2. Each sample shown in Table 1 is a zero-cement type material (mortar for 3D printers).

[0023] [Table 1]

[0024] [Table 2]

[0025] [Method of measuring vane shear resistance] After mixing the materials shown in Table 1, the vane shear resistance value, which changes with time from the addition of water, was measured. In detail, the materials were mixed in a mixer according to the following steps (1) to (6). (1) Mix all ingredients except water for 3 minutes. (2) Add water and knead for 2 minutes. (3) Scraping (4) Mix for 2 minutes (5) Leave it for 5 minutes (6) Mix for 1 minute After the kneading, the material was kept in the mixer and the vane shear resistance was measured by repeating the following steps (7) and (8). (7) Leave it for 5 minutes (8) After stirring for 2 minutes, measure the vane shear resistance. After the vane shear resistance value of the material became 0.9 kPa or less, the material was placed in the hopper of the 3D printer, and the material was poked with a scraping rod as needed, and the vane shear resistance value was measured approximately every 10 minutes. The vane shear resistance was measured according to the method specified in the "In-situ vane shear test method" of the Geotechnical Society of Japan standard (JGS 1411-012).

[0026] [Layering method] As described above, for each sample, when the vane shear resistance value became 0.9 kPa or less, the sample was put into the hopper of the 3D printer, and lamination was started, and lamination was continued for about 50 to 70 minutes. The 3D printer used was a material extrusion (ME) type stacking device.

[0027] [Evaluation item: Retention over time] The vane shear resistance of each sample was measured using the above-mentioned method, and the vane shear resistance was plotted on a graph with the vertical axis representing the vane shear resistance (kPa) and the horizontal axis representing the time (minutes) from the addition of water. Then, each plot was connected with a straight line to create a graph like that shown in Figure 1. Then, for each sample, the time at which the vane shear resistance value was 0.4 to 0.9 kPa was derived. When this time was 60 minutes or more, it was evaluated as "excellent in retention over time (marked with ○ in the table)".

[0028] [Evaluation item: surface smoothness] After lamination, each sample was visually inspected for surface smoothness of the laminate. When almost no roughness or cracks were observed on the surface of the laminate, it was evaluated as "excellent surface smoothness (marked with ○ in the table)". [Evaluation item: Lamination] After lamination, the height of the laminate was measured for each sample. When the laminate could be laminated to a length of 40 cm or more, it was evaluated as having "excellent lamination properties (marked with ◯ in the table)".

[0029] [Consideration of the results] 2 to 9 are photographs showing the appearance of Samples 1 to 8. In the samples 1 to 5, the hydraulic composition satisfied the requirements of the present invention, and the results showed that the hydraulic composition was excellent in terms of retention over time, surface smoothness, and lamination. In addition, as shown in Figures 2 to 6, it was confirmed that the surface of the laminate was smooth and that it could be laminated highly. In addition, Samples 1 to 5 did not contain cement, and therefore had a white appearance. As a result, in Samples 1 to 5, the occurrence of the "efflorescence phenomenon" that is a problem when using materials containing cement, and the occurrence of "color unevenness" on the surface due to the phenomenon, was not confirmed.

[0030] On the other hand, the vane shear resistance of sample 6 dropped below 0.4 kPa and did not return to 0.4 kPa or higher even 100 minutes after water was added. This is presumably because the content of retarding admixture (super retarder) was high, causing a significant delay in setting. As a result, sample 6 was found to have poor retention over time and lamination properties. The external photograph of sample 6 in Figure 7 also clearly shows that it does not have excellent lamination properties. In addition, for sample 7, after the vane shear resistance value dropped below 0.4 kPa, it rose relatively quickly to exceed 0.9 kPa, and the time to reach 0.4 to 0.9 kPa was less than 60 minutes. This is presumably because the content of retarding admixture (super retarder) was low and the content of thickening admixture (thickener) was high. As a result, sample 7 was found to have poor retention over time and poor surface smoothness. It is also clear from the external photograph of sample 7 in FIG. 8 that the surface smoothness is poor. Also, in the case of Sample 8, like Sample 7, the time during which the vane shear resistance value reached 0.4 to 0.9 kPa was less than 60 minutes. This is presumably because the content of the thickening admixture (thickener) was low. As a result, Sample 8 was found to have poor retention over time and poor surface smoothness. It is also clear from the external view of Sample 8 in FIG. 9 that the surface smoothness is not excellent.

Claims

1. A cement-free hydraulic composition comprising: A hydraulic composition comprising ground granulated blast furnace slag, ground limestone, an expansive material, slaked lime, fine aggregate, and a thickening admixture.

2. 2. The hydraulic composition according to claim 1, wherein the time required for the vane shear resistance value, which changes with time after the addition of water, to reach 0.4 to 0.9 kPa is 60 minutes or more.

3. 3. The hydraulic composition according to claim 1, wherein the water-powder ratio is 30.0% or less.

4. Includes retarding admixture, The thickening admixture is 0.035 to 0.060 parts by mass relative to 100 parts by mass of the ground granulated blast furnace slag; 3. The hydraulic composition according to claim 1, wherein the amount of the retarding admixture is 0.700 parts by mass or less per 100 parts by mass of the ground granulated blast furnace slag.

5. A laminate comprising the hydraulic composition according to claim 1 or 2 laminated thereon.

6. A method for manufacturing a laminate, comprising a step of laminating a hydraulic composition that does not contain cement and that contains ground granulated blast furnace slag, ground limestone, an expansive material, slaked lime, fine aggregate, a retarding admixture, and a thickening admixture, using a material extrusion type lamination device.

Citation Information

Patent Citations

  • Reticulated bondable polymer resin and its use as binder component in coating agent