Release film
A multilayer release film with controlled thickness and viscosity for flexible printed circuit boards addresses the tearing issue by enhancing embeddability and preventing film breakage during hot press molding.
Patent Information
- Application Number
- JP2024074331
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-01
- Publication Date
- 2024-11-27
AI Technical Summary
Conventional release films fail to adequately follow the uneven substrate surfaces during hot press molding, leading to tearing and yield deterioration in flexible printed circuit board production due to increased thickness and step differences in FPCs.
A multilayer release film with controlled thickness standard deviation and shear viscosity differences between resin layers, featuring a cushion layer and release layers, is developed to enhance embeddability and prevent tearing.
The multilayer release film effectively prevents tearing over press objects with steps, improving yield and embedding properties while maintaining film integrity.
Smart Images

Figure 2024164815000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a release film. [Background technology]
[0002] In the heat press process of flexible printed circuit board (FPC) production, a release film is used to prevent the coverlay film and the heat press plate from adhering to each other and to protect the object to be pressed. The release film is placed between the coverlay film and the heat press plate, and conforms to the unevenness of the substrate surface during heat press molding, preventing the adhesive layer of the coverlay film from flowing out (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2004-002593 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, the features and required performance of FPCs have changed as their applications have expanded. As the amount of current required of FPCs increases, the thickness of the copper wiring on the FPC increases, which can lead to larger steps on the board surface. In addition, as FPCs become larger in area and safety requirements increase, the parts (reinforcement plates) attached to reinforce FPCs can become thicker. Due to these trends, the required level of embeddability (ability to conform to unevenness) for release films is increasing. However, conventional release films are unable to conform to large steps on the board surface during hot press molding, which can lead to tears, which can cause a decrease in the yield of FPC production.
[0005] An object of the present invention is to provide a release film that is less likely to tear even when pressed over an object having a step. [Means for solving the problem]
[0006] Disclosure 1 relates to a release film having a multilayer structure in which at least two resin layers are laminated, and in which the standard deviation (σ) of the thickness measured along the width direction perpendicular to the longitudinal direction is 10 μm or less. Disclosure 2 is the release film of Disclosure 1, having a thickness of less than 250 μm. The present disclosure 3 is the release film of the present disclosure 1 or 2, in which the difference in shear viscosity of the resin layers at 250° C. and 100 Hz is 150 Pa·s or less in any two adjacent layers. The present disclosure 4 is the release film of the present disclosure 1, 2, or 3, in which the difference in shear viscosity of the resin layers at 250° C. and 500 Hz is 200 Pa·s or less in any two adjacent layers. Disclosure 5 is the release film of Disclosure 1, 2, 3, or 4, in which the standard deviation (σ) of the thickness measured along the width direction perpendicular to the longitudinal direction is 7 μm or less. A sixth aspect of the present disclosure is the release film of the first, second, third, fourth or fifth aspect of the present disclosure, wherein at least one of the resin layers contains an aromatic polyester resin. Disclosure 7 is the release film of Disclosure 6, wherein the aromatic polyester resin is polybutylene terephthalate. Disclosure 8 is the release film of Disclosure 1, 2, 3, 4, 5, 6, or 7, wherein the at least two resin layers include a cushion layer and two release layers laminated on both sides of the cushion layer. Disclosure 9 is the release film of Disclosure 8, wherein the cushion layer contains a polyolefin resin. The present disclosure 10 is the release film of the present disclosure 8 or 9, wherein the ratio of the sum of the thicknesses of the release layers to the total thickness is 15% or more. Disclosure 11 is the release film of Disclosure 8, 9, or 10, wherein the cushion layer has a thickness of 60 μm or more. The release film of the present disclosure 12 is the release film of the present disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, or 11, which is used in a heat press process in the manufacture of a printed circuit board. The present invention will be described in detail below.
[0007] The present inventors have intensively studied the cause of breakage when pressed on a press object having a step, and found that this is due to slight thickness variation in the release film. Further study revealed that a release film having a multilayer structure in which two or more resin layers are laminated is more likely to have thickness variation than a release film having a single layer structure. Therefore, it was found that by controlling the standard deviation (σ) of the thickness measured along the width direction perpendicular to the longitudinal direction of a multilayer release film to 10 μm or less, breakage when pressed on a press object having a step can be effectively suppressed, and the present invention has been completed.
[0008] The release film of the present invention has a multi-layer structure in which at least two resin layers are laminated. Examples of the resin layers include a release layer and a cushion layer. The release layer is disposed on the outermost surface of the release film and is made of a rigid resin to improve releasability, whereas the cushion layer is made of a flexible resin to improve embeddability. The multi-layer structure may be a two-layer structure having a release layer on one side of the cushion layer, or a three-layer structure having release layers on both sides of the cushion layer. As the release film of the present invention, one in which the at least two resin layers include a cushion layer and two release layers laminated on both sides of the cushion layer is preferably used.
[0009] The release film of the present invention has a standard deviation (σ) of thickness measured along the width direction perpendicular to the longitudinal direction of 10 μm or less. By having the above-mentioned standard deviation of thickness of 10 μm or less, the release film of the present invention can prevent stress concentration and tearing at the thin part when pressed on an object to be pressed having a large step. In addition, when the standard deviation of thickness (σ) is 10 μm or less, deterioration of the roll winding appearance due to uneven thickness of the release film (winding deviation due to waviness or meandering, etc.) can be prevented when the release film is wound into a roll. Furthermore, the occurrence of wrinkles during pressing and uneven adhesion during pressing (deterioration of embedding property at the thin part) can be prevented.
[0010] The above-mentioned standard deviation of thickness means the standard deviation of the data obtained when the thickness is measured at 25 mm intervals along the width direction perpendicular to the longitudinal direction of the release film. That is, the above-mentioned standard deviation of thickness represents the thickness distribution in the macroscopic region of the release film, and is different from the surface roughness which represents the thickness distribution in the microscopic region of the release film. The above-mentioned longitudinal direction is preferably the resin flow direction (MD direction). When the longitudinal direction of the release film is unknown, the same measurement is performed in any two orthogonal directions, and the larger standard deviation of the two directions is determined as the longitudinal direction. The standard deviation of the thickness is preferably 7 μm or less, and more preferably 5 μm or less. The smaller the standard deviation of the thickness, the more preferable it is, and the lower limit is not particularly limited, and the standard deviation of the thickness is preferably 0 μm or more.
[0011] The standard deviation of the thickness can be controlled by the kneadability and moldability of the resin (material resin) that is the material for each resin layer constituting the multilayer structure, the material properties of each resin layer, the thickness control function of the film manufacturing equipment, etc.
[0012] (Mixability of resin materials) If the mixture of the resins used in each resin layer is insufficient, the behavior during extrusion becomes unstable. Also, if the compatibility between the resins is low, the film surface after molding becomes rough and the flatness becomes low. Therefore, in order to reduce the standard deviation of the thickness, it is preferable to select materials with high compatibility for the resins used in each resin layer and mix them thoroughly to form the resin layer. As a method of selecting materials with high compatibility, a method of containing the same resin in each resin layer can be mentioned.
[0013] (Fluidity of each resin layer) In the production of multilayer films by melt extrusion molding, a difference in normal stress at the interface occurs due to the flow characteristics (shear viscosity difference) of adjacent resin layers, resulting in the formation of flow marks. Therefore, it is preferable to reduce the difference in shear viscosity between adjacent resin layers when they are melted.
[0014] (Thickness control function for film manufacturing equipment) A thickness gauge may be used to measure the widthwise profile of the release film, and the measurement results may be fed back to a film manufacturing device, and the thickness control function of the device may be used to mechanically control the thickness. For example, in a device that adjusts the gap of the T-die by adjusting the fastening state of bolts arranged at regular intervals (arranged over the entire width at intervals of about 20 to 30 mm), the bolts are heat bolts, and the fastening state of each bolt is adjusted by temperature control, thereby reducing the variation in film thickness and making the standard deviation of thickness smaller.
[0015] Among the above-mentioned methods for controlling the standard deviation of thickness, the method of adjusting the difference in shear viscosity of adjacent resin layers when melted to within a certain range is effective, and the method of adjusting any two adjacent layers to within a certain range is particularly effective. In the method of adjusting any two adjacent layers to within a certain range, for example, when the release film has a four-layer structure with a lamination order of A layer / B layer / C layer / D layer, the difference in shear viscosity between A layer and B layer, the difference in shear viscosity between B layer and C layer, and the difference in shear viscosity between C layer and D layer are all adjusted to within a certain range.
[0016] The shear viscosity can be measured by a rheometer (rotational viscometer) based on JIS K 7244-10. Specifically, a cylindrical rotor is placed in the sample, and the torque (shear stress) acting on the cylindrical surface when rotated at a constant speed is measured, whereby the shear viscosity can be calculated by the following formula (1). Shear viscosity = shear stress / shear rate (1) The shear viscosity can be adjusted by the type of material (type of compound) constituting the resin layer, the molecular weight, the molecular structure, etc. The shear viscosity of each resin layer is controlled when producing the release film of the present invention, but it can also be measured after the production of the release film of the present invention by disassembling each resin layer and then melting it.
[0017] In the release film of the present invention, the difference in shear viscosity of the resin layer at 250°C and 100Hz is preferably 150 Pa·s or less in any two adjacent layers. Here, the measurement temperature of the shear viscosity, 250°C, is assumed to be the mold temperature when molding the release film, and the measurement frequency of the shear viscosity, 100Hz, is assumed to be the state of the material resin near the joining point of the material resin (for example, the feed block of the extruder) under general extrusion molding conditions. That is, by having the difference in shear viscosity of the resin layer at 250°C and 100Hz be 150 Pa·s or less, it is possible to suppress the flow of the material resin being disturbed when the material resin joins, thereby preventing unevenness in the thickness, and the thickness accuracy of the release film can be improved. The difference in shear viscosity of the resin layer at 250°C and 100Hz is more preferably 100 Pa·s or less. In addition, it is preferable that the difference in shear viscosity of the resin layer at 250°C and 100Hz is small, and the lower limit is not particularly limited, and it is preferable that it is 0 Pa·s or more.
[0018] In the release film of the present invention, the difference in shear viscosity of the resin layer at 250°C and 500Hz is preferably 200 Pa·s or less between any two adjacent layers. Here, the frequency of 500Hz, which is the measurement frequency of the shear viscosity, is assumed to be the state of the material resin near the die outlet of a general extruder. That is, by making the difference in shear viscosity of the resin layer at 250°C and 500Hz 200 Pa·s or less, it is possible to suppress the disturbance of the flow of the material resin when the flow path of the material resin narrows and the flow becomes fast, and it is possible to improve the thickness accuracy of the release film. It is more preferable that the difference in shear viscosity of the resin layer at 250°C and 500Hz is 100 Pa·s or less. In addition, it is preferable that the difference in shear viscosity of the resin layer at 250°C and 500Hz is small, and the lower limit is not particularly limited, and it is preferable that it is 0 Pa·s or more.
[0019] The thickness of the release film of the present invention is not particularly limited. The thinner the overall thickness of the release film, the more advantageous it is in suppressing the exudation of resin from the cushion layer. The thicker the overall thickness of the release film, the more advantageous it is in conforming to large steps on the substrate surface during heat press molding. The thickness of the release film of the present invention is preferably 70 μm or more, more preferably 90 μm or more. In addition, the thickness of the release film of the present invention is preferably less than 250 μm, more preferably less than 210 μm.
[0020] The size of the release film of the present invention is not particularly limited, but in order to prevent tearing when pressed on the object to be pressed, it is preferably larger than the object to be pressed, and the length in the width direction is preferably 75 mm or more, more preferably 100 mm or more, and from the viewpoint of film formability, it is preferably 3000 mm or less. Also, the length in the longitudinal direction is preferably 75 mm or more, and from the viewpoint of transportation, it is preferably 2000 m or less.
[0021] The resin layer preferably includes at least one release layer.
[0022] The resin constituting the release layer is not particularly limited, but polyester, polyolefin or polystyrene is preferred because it improves the releasability of the release film. The polyester preferably contains an aromatic polyester resin. The polyolefin preferably contains poly(4-methyl-1-pentene) or an alicyclic olefin resin. The polystyrene preferably contains a polystyrene resin having a syndiotactic structure. In particular, the release layer more preferably contains an aromatic polyester resin, since it has excellent embedding properties and excellent anti-bleeding properties of the adhesive formed on the coverlay film. That is, it is preferable that at least one of the resin layers contains an aromatic polyester resin.
[0023] The aromatic polyester resin is not particularly limited, but crystalline aromatic polyester resin is preferred.Specific examples include polyethylene terephthalate resin, polybutylene terephthalate resin, polyhexamethylene terephthalate resin, polyethylene naphthalate resin, polybutylene naphthalate resin, terephthalic acid butanediol polytetramethylene glycol copolymer, etc.These aromatic polyester resins may be used alone or in combination of two or more.Among them, polybutylene terephthalate resin is preferred from the viewpoint of balance of heat resistance, releasability, embeddability, etc. Also preferred is a mixed resin of a polybutylene terephthalate resin and a block copolymer of polybutylene terephthalate and an aliphatic polyether. The aliphatic polyether is not particularly limited, and examples thereof include polyethylene glycol, polydiethylene glycol, polypropylene glycol, and polytetramethylene glycol.
[0024] The proportion of the polybutylene terephthalate resin in the resin constituting the release layer is not particularly limited, but is preferably 70% by weight or more. If the proportion of the polybutylene terephthalate resin is 70% by weight or more, the release property of the release film is improved. A more preferable lower limit of the proportion of the polybutylene terephthalate resin in the resin constituting the release layer is 75% by weight.
[0025] Among the above aromatic polyester resins, commercially available examples include "Pelprene (registered trademark)" (manufactured by Toyobo Co., Ltd.), "Hytrel (registered trademark)" (manufactured by DuPont-Toray Co., Ltd.), "Duranex (registered trademark)" (manufactured by Polyplastics Co., Ltd.), and "Novaduran (registered trademark)" (manufactured by Mitsubishi Engineering Plastics Corporation).
[0026] The poly(4-methyl-1-pentene)-containing polyolefin preferably contains 90% by weight or more of poly(4-methyl-1-pentene) resin. As the poly(4-methyl-1-pentene) resin, for example, a commercially available product such as TPX (registered trademark) manufactured by Mitsui Chemicals, Inc. can be used.
[0027] The alicyclic olefin resin is an olefin resin having a cyclic aliphatic hydrocarbon in the main chain or side chain, and from the standpoint of heat resistance, strength, etc., thermoplastic saturated norbornene resin is preferred. Examples of the thermoplastic saturated norbornene resin include resins obtained by hydrogenating ring-opening polymers or ring-opening copolymers of norbornene monomers (after modification such as maleic acid addition or cyclopentadiene addition, if necessary). Other examples include resins obtained by addition polymerization of norbornene monomers, resins obtained by addition polymerization of norbornene monomers and olefin monomers such as ethylene or α-olefin, and resins obtained by addition polymerization of norbornene monomers and cyclic olefin monomers such as cyclopentene, cyclooctene, and 5,6-dihydrodicyclopentadiene. Furthermore, modified products of these resins are also included.
[0028] The polystyrene containing the polystyrene-based resin having a syndiotactic structure preferably contains 70% by weight or more and 90% by weight or less of the polystyrene-based resin having a syndiotactic structure. A polystyrene resin having a syndiotactic structure is a resin having a stereoregular structure in which phenyl groups and substituted phenyl groups, which are side chains, are alternately positioned in opposite directions relative to the main chain formed from carbon-carbon sigma bonds.
[0029] The polystyrene resin having the syndiotactic structure is not particularly limited. For example, polystyrene having a syndiotacticity of 75% or more in racemic diad or 30% or more in racemic pentad, poly(alkylstyrene), poly(arylstyrene), poly(halogenated styrene), poly(halogenated alkylstyrene), poly(alkoxystyrene), poly(vinyl benzoate ester), etc. can be mentioned. In addition, hydrogenated polymers of these, mixtures of these, copolymers containing these as main components, etc. can be mentioned. The polystyrene resin having the syndiotactic structure can be commercially available, such as XAREC (registered trademark) manufactured by Idemitsu Kosan Co., Ltd.
[0030] The release layer may contain a rubber component. When the release layer contains a rubber component, embeddability of the release film is improved. The rubber component is not particularly limited, and examples thereof include natural rubber, styrene-butadiene copolymer, polybutadiene, polyisoprene, acrylonitrile-butadiene copolymer, ethylene-propylene copolymer (EPM, EPDM), polychloroprene, butyl rubber, acrylic rubber, silicone rubber, urethane rubber, etc. Examples of the rubber component include olefin-based thermoplastic elastomer, styrene-based thermoplastic elastomer, vinyl chloride-based thermoplastic elastomer, ester-based thermoplastic elastomer, amide-based thermoplastic elastomer, etc.
[0031] The release layer may contain a stabilizer. The stabilizer is not particularly limited, and examples thereof include hindered phenol-based antioxidants and heat stabilizers. The hindered phenol-based antioxidant is not particularly limited, and examples thereof include 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 3,9-bis{2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)-propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, and the like. The heat stabilizer is not particularly limited, and examples thereof include tris(2,4-di-t-butylphenyl)phosphite, trilauryl phosphite, 2-t-butyl-α-(3-t-butyl-4-hydroxyphenyl)-p-cumenylbis(p-nonylphenyl)phosphite, dimyristyl 3,3'-thiodipropionate, distearyl 3,3'-thiodipropionate, pentaerythryl tetrakis(3-laurylthiopropionate), ditridecyl 3,3'-thiodipropionate, and the like.
[0032] The release layer may further contain conventionally known additives such as fibers, inorganic fillers, flame retardants, ultraviolet absorbing agents, antistatic agents, inorganic substances, and salts of higher fatty acids.
[0033] The thickness of the release layer is not particularly limited. The thinner the release layer, the more advantageous it is in that the embeddability of the release film is easily ensured. The thicker the release layer, the more advantageous it is in that it is less likely to break during pressing, and is also advantageous in that it ensures the releasability of the release film and reduces heat shrinkage to improve dimensional stability before and after the heat pressing process. The thickness of the release layer is preferably 5 μm or more, more preferably 7 μm or more. In addition, the thickness of the release layer is preferably less than 100 μm, more preferably less than 50 μm. When the thickness of the release layer is less than 50 μm, the effect of improving embeddability can be sufficiently obtained.
[0034] In addition, the release film of the present invention preferably has a ratio of the total thickness of the release layers to the total thickness of 15% or more. By ensuring the ratio of the rigid release layers, the tensile strength is relatively increased, making the film less likely to break during pressing.
[0035] The resin layer preferably includes a cushion layer. The cushion layer can improve the embeddability of the release film. In the manufacturing process of a flexible printed circuit board or the like, when a heat press is performed with a release film disposed between the coverlay film and the heat press plate, the release layer that is in direct contact with the coverlay film and the heat press plate is required to have excellent releasability, so there are certain restrictions on improving the embeddability. The embeddability of the release film can be improved by providing a soft layer as the cushion layer, and it becomes easy to obtain a release film that is excellent in both releasability and embeddability.
[0036] Examples of the resin constituting the cushion layer include polyolefin, polystyrene, polyvinyl chloride, polyamide, polycarbonate, polysulfone, polyester, etc., and among these, polyolefin is preferably used. That is, the cushion layer preferably contains a polyolefin resin.
[0037] The polyolefin resin is not particularly limited, and examples thereof include polyethylene resins (e.g., high-density polyethylene, low-density polyethylene, linear low-density polyethylene), polypropylene resins, ethylene-vinyl acetate copolymers, etc. Also included are ethylene-acrylic monomer copolymers such as ethylene-methyl methacrylate copolymers, ethylene-ethyl acrylate copolymers, and ethylene-acrylic acid copolymers. These polyolefin resins may be used alone or in combination of two or more kinds. Among them, polypropylene resins are preferred because they easily achieve both embeddability and heat resistance.
[0038] The content of the polyolefin resin in the cushion layer is not particularly limited, but the preferred lower limit is 50% by weight, and the preferred upper limit is 90% by weight. If the content of the polyolefin resin is 50% by weight or more, the flexibility of the cushion layer is sufficient, and the embedding property of the release film is improved. If the content of the polyolefin resin is 90% by weight or less, the adhesion between the release layer and the cushion layer is improved. The more preferred lower limit of the content of the polyolefin resin is 60% by weight, and the even more preferred lower limit is 65% by weight. The more preferred upper limit of the content of the polyolefin resin is 80% by weight, and the even more preferred upper limit is 75% by weight.
[0039] The cushion layer preferably contains the resin that constitutes the release layer. The cushion layer contains the resin constituting the release layer, so that the adhesion between the release layer and the cushion layer is improved. The cushion layer more preferably contains the main component resin of the release layer, and further preferably contains the main component resin of the release layer and a polyolefin resin. Here, the main component resin of the release layer means the resin with the highest content among the resins contained in the release layer.
[0040] The content of the resin constituting the release layer in the cushion layer is not particularly limited, but the preferred lower limit is 10% by weight, and the preferred upper limit is 50% by weight. If the content of the resin constituting the release layer is 10% by weight or more, the adhesion between the release layer and the cushion layer is improved. If the content of the resin constituting the release layer is 50% by weight or less, the flexibility of the cushion layer is sufficient, and the embedding property of the release film is improved. The more preferred lower limit of the content of the resin constituting the release layer is 20% by weight, and the even more preferred lower limit is 25% by weight. The more preferred upper limit of the content of the resin constituting the release layer is 40% by weight, and the even more preferred upper limit is 35% by weight.
[0041] The cushion layer may further contain additives such as fibers, inorganic fillers, flame retardants, ultraviolet absorbing agents, antistatic agents, inorganic substances, and salts of higher fatty acids.
[0042] The cushion layer may have a single-layer structure made of a single layer, or a multi-layer structure made of a laminate of multiple layers. When the cushion layer has a multi-layer structure, the multiple layers may be laminated together via an adhesive layer.
[0043] The thickness of the cushion layer is not particularly limited, but the preferred lower limit is 15 μm, and the preferred upper limit is 200 μm. If the thickness of the cushion layer is 15 μm or more, the embeddability of the release film is further improved. If the thickness of the cushion layer is 200 μm or less, the exudation of resin from the cushion layer that occurs at the film end during the heat pressing process can be suppressed. The more preferred lower limit of the thickness of the cushion layer is 30 μm, and the even more preferred lower limit is 60 μm. That is, in the release film of the present invention, the thickness of the cushion layer is preferably 60 μm or more. The more preferred upper limit of the thickness of the cushion layer is 170 μm.
[0044] The method for producing the release film of the present invention is not particularly limited, and examples thereof include a method for producing a film by a coextrusion T-die method, a method for preparing a film by a water-cooled or air-cooled coextrusion inflation method, a solvent casting method, a hot press molding method, etc. Among these, the method for producing a film by a coextrusion T-die method is preferred because of its excellent controllability of the thickness of each layer.
[0045] The release film of the present invention is not likely to break even when pressed against an object having a large step, and is therefore preferably used in a heat press process, particularly preferably in a heat press process in the manufacture of printed circuit boards. Conditions for the heat press process in which the release film of the present invention is used include, for example, a temperature of 100 to 220° C. and a pressure of 0.5 to 100 MPa.
[0046] The use of the release film of the present invention is not particularly limited, but it can be suitably used in the manufacturing process of printed boards such as flexible printed boards (FPCs), printed wiring boards, and multilayer printed wiring boards, and can be particularly suitably used in the manufacturing process of printed boards for in-vehicle use. Specifically, for example, in the manufacturing process of an FPC, the release film of the present invention can be used when hot press bonding a coverlay film to a flexible circuit board main body having a copper circuit formed thereon via a thermosetting adhesive or a thermosetting adhesive sheet. The release film of the present invention can also be suitably used in the production of FPCs by the roll-to-roll method, which requires high releasability. Effect of the Invention
[0047] According to the present invention, it is possible to provide a release film that is less likely to tear even when pressed over an object having a step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0048] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0049] Example 1 Polybutylene terephthalate (PBT) was used as the resin composition for the release layer. A mixture of 20 parts by weight of polybutylene terephthalate (PBT), 40 parts by weight of polyethylene (PE) and 40 parts by weight of ethylene-methyl methacrylate copolymer (EMMA, "Acryft WD106" manufactured by Sumitomo Chemical Co., Ltd.) was used as the resin composition for the cushion layer.
[0050] The resin composition for the release layer and the resin composition for the cushion layer were extruded into a three-layer structure at a molding temperature of 250°C and a T-die width of 400mm using an extruder (GM Engineering, GM30-28 (screw diameter 30mm, L / D28)) and the extruded molten resin was cooled by a cooling roll (temperature 90°C, arithmetic mean surface roughness Ra 0.1μm). As a result, a release film having a three-layer structure (first layer: release layer, second layer: cushion layer, third layer: release layer) with a release layer on each side of the cushion layer and a width of 1700mm was obtained. The thickness of each release layer was 17μm, the thickness of the cushion layer was 86μm, and the thickness of the entire film was 120μm.
[0051] The extruder is equipped with heat bolts and a thickness gauge arranged at intervals of about 20 to 30 mm across the entire width of the film. The measurement results of the thickness gauge are fed back to the extruder, and the heat bolts are tightened by temperature control to adjust the gap of the T-die and adjust the thickness of the release film. During cooling, the contact time between the molten resin and the cooling roll is 1.0 second, and the elongation stress when cooling the molten resin by the cooling roll is 450 kPa.
[0052] Example 2 A multilayer release film having a three-layer structure was obtained in the same manner as in Example 1, except that the thicknesses of the release layer and the cushion layer were changed as shown in Table 1 below.
[0053] Example 3 A three-layer multilayer release film was obtained in the same manner as in Example 1, except that a mixture of 30 parts by weight of polybutylene terephthalate (PBT), 30 parts by weight of polyethylene (PE), and 40 parts by weight of ethylene-methyl methacrylate copolymer (EMMA, "Acryft WD106" manufactured by Sumitomo Chemical Co., Ltd.) was used as the resin composition for the cushion layer.
[0054] Example 4 A multilayer release film having a three-layer structure was obtained in the same manner as in Example 3, except that the thicknesses of the release layer and cushion layer were changed as shown in Table 1 below.
[0055] Example 5 A three-layer multilayer release film was obtained in the same manner as in Example 1, except that a mixture of 30 parts by weight of polybutylene terephthalate (PBT), 30 parts by weight of polypropylene (PP) and 40 parts by weight of ethylene-methyl methacrylate copolymer (EMMA, "Acryft WD106" manufactured by Sumitomo Chemical Co., Ltd.) was used as the resin composition for the cushion layer.
[0056] Example 6 A multilayer release film having a three-layer structure was obtained in the same manner as in Example 5, except that the thicknesses of the release layer and the cushion layer were changed as shown in Table 1 below.
[0057] Comparative Example 1 A multilayer release film having a three-layer structure was obtained in the same manner as in Example 1, except that polypropylene (PP) was used as the resin composition for the cushion layer.
[0058] Comparative Example 2 A multilayer release film having a three-layer structure was obtained in the same manner as in Example 1, except that polycarbonate (PC) was used as the resin composition for the cushion layer.
[0059] Comparative Example 3 A multilayer release film having a three-layer structure was obtained in the same manner as in Example 1, except that polyethylene (PE) was used as the resin composition for the cushion layer.
[0060] The release films obtained in the examples and comparative examples were measured by the following methods.
[0061] <Standard deviation of thickness> For a release film with a width of 1700 mm, the thickness was measured at 25 mm intervals along the width direction perpendicular to the longitudinal direction over a length of 1700 mm using a thickness meter (Digimatic Indicator) (Mitsutoyo Corporation, (Model) ID-C112CX). The standard deviation of the obtained 67 thickness data was calculated, and the obtained values are shown in Table 1 below.
[0062] <Shear viscosity> The shear viscosity at 250°C and 100 Hz and the shear viscosity at 250°C and 500 Hz of the resin composition for the release layer constituting the first and third layers were measured using a rotational viscometer (model number HAAKE MARS, manufactured by Thermo Fisher Scientific), and the measurement results are shown in Table 1 below. The shear viscosity at 250° C. and 100 Hz and the shear viscosity at 250° C. and 500 Hz of the resin composition for the cushion layer constituting the second layer were measured, and the measurement results are shown in Table 1 below. From the above measurement results, the difference in shear viscosity between the first layer and the second layer, and the difference in shear viscosity between the second layer and the third layer were calculated, and the obtained values are shown in Table 1 below.
[0063] The release films obtained in the examples and comparative examples were evaluated by the following methods. The results are shown in Table 1.
[0064] <Heat press evaluation> A coverlay film (10cm x 10cm, polyimide thickness 25μm, epoxy adhesive layer thickness 35μm) was laminated on the copper foil surface of a copper clad laminate (CCL) (10cm x 10cm, polyimide thickness 25μm, copper foil thickness 35μm) so that the epoxy adhesive layer was in contact with the copper foil surface. Furthermore, FR-4 (Flame Retardant Type 4), a glass epoxy resin plate measuring 15mm length x 25mm width, was laminated on the center of the copper foil surface of the coverlay film. Furthermore, a release film (15cm x 15cm) was laminated by aligning the centers of the FR-4 and the release film so that the release layer was in contact with the FR-4. This laminate was heated at 175°C and 20kgf / cm 2 The sample was heat-pressed for 50 seconds under the conditions of 1. After that, the release film was peeled off and the release film was visually inspected for tears. An evaluation was performed using FR-4 with a thickness of 2 mm (evaluation 1), and an evaluation was performed using FR-4 with a thickness of 4 mm (evaluation 2).
[0065] [Table 1] [Industrial Applicability]
[0066] According to the present invention, it is possible to provide a release film that is less likely to tear even when pressed over an object having a step.
Claims
1. A release film having a multilayer structure in which at least two resin layers are laminated, A release film having a standard deviation (σ) of thickness measured along a width direction perpendicular to the longitudinal direction of the film of 10 μm or less.
2. The release film of claim 1 having a thickness of less than 250 μm.
3. 3. The release film according to claim 1, wherein the difference in shear viscosity between any two adjacent resin layers at 250° C. and 100 Hz is 150 Pa·s or less.
4. 3. The release film according to claim 1, wherein the difference in shear viscosity of the resin layers at 250° C. and 500 Hz is 200 Pa·s or less between any two adjacent resin layers.
5. 3. The release film according to claim 1, wherein the standard deviation (σ) of the thickness measured along the width direction perpendicular to the longitudinal direction is 7 μm or less.
6. The release film according to claim 1 or 2, wherein at least one of the resin layers contains an aromatic polyester resin.
7. The release film according to claim 6 , wherein the aromatic polyester resin is polybutylene terephthalate.
8. The release film according to claim 1 or 2, wherein the at least two resin layers include a cushion layer and two release layers laminated on both sides of the cushion layer.
9. The release film according to claim 8 , wherein the cushion layer comprises a polyolefin resin.
10. The release film according to claim 8 , wherein the ratio of the sum of the thicknesses of the release layers to the total thickness is 15% or more.
11. The release film according to claim 8 , wherein the cushion layer has a thickness of 60 μm or more.
12. 3. The release film according to claim 1, which is used in a heat pressing step in the production of printed circuit boards.
Citation Information
Patent Citations
sheet
JP2004002593A
Cited By
Method for manufacturing release film and molded product
JP2026148109A
Method for manufacturing release film and molded product
JP7838693B1
Release film and method for producing molded article
WO2026186514A1