Color-developing UV-curable silicone coating composition and method for using the composition

The color-forming ultraviolet-curable silicone coating composition addresses the challenge of visually confirming curing by using a photochromic dye that changes color upon curing, ensuring efficient application verification and suitability for electronic substrates.

JP2024164924AInactive Publication Date: 2024-11-28SHIN ETSU CHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023080651
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing ultraviolet-curable silicone coatings lack a reliable method for visually confirming completion of curing, especially on complex substrates, which hinders efficient production and requires special inspection equipment.

Method used

A color-forming ultraviolet-curable silicone coating composition containing a photochromic dye that changes color upon curing, allowing visual confirmation of the applied area without special equipment.

Benefits of technology

Enables instant visual verification of coating application, ensuring proper curing without equipment, and prevents issues like color loss or sedimentation, making it suitable for conformal coating on electronic substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164924000001
    Figure 2024164924000001
  • Figure 2024164924000002
    Figure 2024164924000002
  • Figure 2024164924000003
    Figure 2024164924000003
Patent Text Reader

Abstract

To provide a color-developing UV-curable silicone coating composition that undergoes curing via ultraviolet light exposure, enabling easy visual identification of the cured portions.SOLUTION: A color-developing UV-curable silicone coating composition contains (A) an organopolysiloxane with a radical reactive group, (B) a photopolymerization initiator: 0.01-20 mass% relative to the mass of component (A), and (C) a photochromic dye: 10-1,000 ppm relative to the total combined mass of component (A) and component (B).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a color-developing ultraviolet-curable silicone coating composition, and in particular to a color-developing ultraviolet-curable silicone coating composition in which a liquid silicone composition cures upon exposure to ultraviolet light and a photochromic dye develops color, thereby enabling visual inspection of the coated portion. [Background technology]

[0002] Liquid silicone resins have excellent applicability due to their low surface tension, and also have good mechanical strength, excellent insulation, heat resistance, and flame retardancy even after curing, so they are widely used as surface protection agents for substrates and conformal coating agents for electronic substrates. There are many methods for using them, in which the coating agent is applied to the target application area to a thickness of several tens to several hundreds of microns and then cured. Curing methods include condensation curing, addition curing, and ultraviolet curing. Among them, ultraviolet curing coating agents contribute to improving productivity because the resin is instantly cured by irradiation with ultraviolet light.

[0003] On the other hand, since silicone resins generally have high transparency, it is difficult to visually judge whether coating and curing have been performed reliably at the desired location. Although it is possible to add dyes or pigments in advance to color the resin, this may cause the dye to lose color, the pigment to settle, or the deep curing ability of the resin to be impaired by blocking ultraviolet light, making this method unsuitable for ultraviolet-curing coating agents. In addition, after irradiating ultraviolet light to a location where a transparent ultraviolet-curing silicone resin has been applied, it is difficult to visually judge whether the silicone resin has been cured reliably. For this reason, a method is known in which an additive that responds to ultraviolet light is added to the silicone composition, and the resin emits light when irradiated with ultraviolet light. In this case, however, the resin emits light only while it is irradiated with ultraviolet light, so a special inspection device is required, and it is sometimes difficult to judge if the substrate or electronic board has a large unevenness. In addition, there is also a problem that the inspection takes time, which impairs mass production. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5021194 [Patent Document 2] WO 03 / 011967 Summary of the Invention [Problem to be solved by the invention]

[0005] Therefore, an object of the present invention is to provide a color-developing, ultraviolet-curable silicone coating composition that cures when irradiated with ultraviolet light and allows the cured areas to be easily confirmed visually, and a method for confirming the areas where the color-developing, ultraviolet-curable silicone coating composition has been applied to a substrate. [Means for solving the problem]

[0006] The present inventors conducted intensive research to solve the above problems, and as a result, they discovered that when an ultraviolet-curable silicone coating agent composition containing a specific amount of photochromic dye is irradiated with ultraviolet light, the composition cures and at the same time the chemical structure of the photochromic dye in the cured product changes, causing it to instantly develop color, and therefore it is possible to visually determine in a short period of time whether the composition has been applied to a substrate and has been coated in the desired locations, without the need for special inspection equipment, and thus completed the present invention.

[0007] Therefore, the present invention provides the following color-developing UV-curable silicone coating composition and a method for confirming the portion of a substrate to which the color-developing UV-curable silicone coating composition has been applied.

[0008] [1] (A) an organopolysiloxane having a radical reactive group, (B) Photopolymerization initiator: 0.01 to 20 mass% based on the mass of component (A), and (C) Photochromic dye: 10 to 1,000 ppm based on the total mass of component (A) and component (B) A color-developing ultraviolet-curable silicone coating composition comprising: [2] The color-developing ultraviolet-curable silicone coating composition according to [1], which is cured by radical polymerization of (meth)acrylic groups or a thiol-ene reaction. [3] The color-developing ultraviolet-curable silicone coating composition according to [1] or [2], wherein component (C) is a photochromic dye having a diarylethene skeleton, a spiropyran skeleton, or a spirooxazine skeleton. [4] The color-developing ultraviolet-curable silicone coating composition according to any one of [1] to [3], which is cured and develops color upon exposure to ultraviolet light. [5] The color-developing ultraviolet-curable silicone coating composition according to any one of [1] to [4], which develops color when irradiated with ultraviolet light and then fades when the ultraviolet light is blocked or when irradiated with visible light. [6] The color-developing ultraviolet-curable silicone coating composition according to any one of [1] to [5], wherein when the light transmittance of the composition before ultraviolet irradiation is taken as 100 for light at 800 nm, the light transmittance of the cured product obtained after ultraviolet irradiation and after standing for 7 days at 23°C is 90 or more for light at 800 nm. [7] A method for confirming the portion on a substrate to which the color-developing ultraviolet-curable silicone coating composition according to any one of [1] to [6] has been applied, the method comprising the steps of: applying the color-developing ultraviolet-curable silicone coating composition on a substrate; irradiating the composition on the substrate with ultraviolet light to cause it to develop color; and visually confirming the portion to which the composition has been applied after the ultraviolet light irradiation is completed. Effect of the Invention

[0009] The color-developing UV-curable silicone coating composition of the present invention undergoes a radical reaction instantaneously by irradiation with UV light, resulting in silicone rubber. In addition, since a photochromic dye is added, the composition develops color at the same time as curing. Therefore, it is possible to visually determine whether the coating has been applied to the desired location, and no special inspection device is required. Furthermore, since the photochromic dye is uniformly dissolved in the silicone polymer matrix, problems such as color loss and sedimentation that occur when dyes or pigments are used are not caused. Therefore, the composition of the present invention is particularly suitable for use as a conformal coating agent for protecting electronic substrates. In addition, the method of the present invention is suitable for checking the coating state of the conformal coating agent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. [Color-developing UV-curable silicone coating composition] Component (A) The component (A) of the present invention is an ultraviolet-curable organopolysiloxane that is rapidly cured when mixed with a photopolymerization initiator, component (B), described below, and then irradiated with ultraviolet light. For example, it is an organopolysiloxane having a radical reactive group that undergoes radical polymerization of (meth)acrylic groups or polymerization by a thiol-ene reaction to rapidly become a silicone cured product, and is preferably at least one of the organopolysiloxanes (i) to (iii) below.

[0011] (i) An organopolysiloxane represented by the following formula (1): [ka] (In formula (1), R 1 each independently represents a substituted or unsubstituted alkyl group, aryl group, or aralkyl group having 1 to 20 carbon atoms; R 2 each independently represents an oxygen atom or an alkylene group having 1 to 20 carbon atoms; R 3each independently represents a radical reactive group, l represents a number satisfying 30 to 1,000, m represents a number satisfying 0 to 20, a and b each independently represent an integer of 0 to 3, and a+b+m is a number of 2 or more.

[0012] R in formula (1) 1 Specific examples of include alkyl groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-hexyl, cyclohexyl, n-octyl, 2-ethylhexyl, and n-decyl groups; aryl groups having 6 to 20 carbon atoms, such as phenyl, tolyl, xylyl, and naphthyl groups; and aralkyl groups having 7 to 20 carbon atoms, such as benzyl and phenylethyl groups. In addition, some or all of the hydrogen atoms bonded to the carbon atoms of these alkyl groups, aryl groups, and aralkyl groups may be substituted with other substituents, and specific examples thereof include halogen-substituted or cyano-substituted alkyl groups, such as chloromethyl, bromoethyl, trifluoropropyl, and cyanoethyl groups. Among these, R 1 As the alkyl group, an alkyl group having 1 to 5 carbon atoms and a phenyl group are preferable, and a methyl group, an ethyl group and a phenyl group are more preferable.

[0013] In addition, R in formula (1) 2 The alkylene group having 1 to 20 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include methylene, ethylene, propylene, trimethylene, tetramethylene, isobutylene, pentamethylene, hexamethylene, heptamethylene, octamethylene, nonamethylene, and decylene groups. Among these, R 2 As the alkyl group, an oxygen atom, a methylene group, an ethylene group, or a trimethylene group is preferable, and an oxygen atom or an ethylene group is particularly preferable.

[0014] R in formula (1) 3represents a radical reactive group, and is preferably at least one selected from an acryloyloxyalkyl group, a methacryloyloxyalkyl group, an acryloyloxyalkyloxy group, a methacryloyloxyalkyloxy group, an alkenyloxy group, an alkenyloxyalkyl group, and an alkenyl group. Specific examples thereof include, but are not limited to, those represented by the following formula: [ka]

[0015] In formula (1), a and b represent integers of 0 to 3, and the sum with m, a+b+m, is a number equal to or greater than 2. More preferably, a and b are 2, and a+b+m is 4. If a+b+m is less than 2, radical reaction is difficult to occur, and the hardness of the silicone cured product may be insufficient.

[0016] In formula (1), m represents a number satisfying the range of 0 to 20, preferably a number from 0 to 10, and particularly preferably a number from 0 to 5. If m exceeds 20, the silicone cured product becomes hard and brittle, and may crack.

[0017] In formula (1), l represents a number satisfying the range of 30 to 1000, preferably 30 to 500, and particularly preferably 50 to 400. If l is less than 30, the compound is likely to volatilize in the air, whereas if it exceeds 1000, the photopolymerization reaction becomes difficult to occur, and curing does not proceed or does not proceed sufficiently, which may result in the obtained silicone cured product having insufficient hardness.

[0018] The viscosity of component (i) at 23°C is preferably 50 to 10,000,000 mPa·s, and more preferably 1,000 to 100,000 mPa·s. If the viscosity is less than 50 mPa·s, the component will be prone to volatilization under atmospheric pressure or when reduced pressure is applied for degassing, whereas if it exceeds 10,000,000 mPa·s, component (i) will have a high viscosity, which will deteriorate workability and will also make it difficult to mix uniformly with components (B) and (C), which is undesirable. The viscosity here is a value measured using a rotational viscometer.

[0019] Specific examples of component A-(i) include those shown below. Here, "Vi" represents a vinyl group and "Me" represents a methyl group (the same applies below). [ka]

[0020] (ii) An organopolysiloxane represented by the following formula (2): [ka] (In formula (2), R 1 each independently represents a substituted or unsubstituted alkyl group, aryl group, or aralkyl group having 1 to 20 carbon atoms; R 4 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, an aryl group, or a silyl group; R 5 represents an alkylene group having 1 to 20 carbon atoms, n represents a number satisfying 1 to 20, and o is a number satisfying 0 to 20.)

[0021] R in Equation (2) 1 Specific examples of R in the above formula (1) include 1 Specific examples of the alkyl group include those given above, and an alkyl group having 1 to 5 carbon atoms and a phenyl group are preferred, with a methyl group, an ethyl group and a phenyl group being more preferred.

[0022] R in Equation (2) 4 Specific examples of the alkyl group include alkyl groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-hexyl, cyclohexyl, n-octyl, 2-ethylhexyl, and n-decyl groups. 4Specific examples of the aryl group include aryl groups having 6 to 20 carbon atoms, such as phenyl, tolyl, xylyl, and naphthyl groups. In addition, some or all of the hydrogen atoms bonded to the carbon atoms of these alkyl groups or aryl groups may be substituted with other substituents, specific examples of which include halogen-substituted or cyano-substituted alkyl groups such as chloromethyl, bromoethyl, trifluoropropyl, and cyanoethyl groups. 4 Specific examples of the silyl group include trialkylsilyl groups such as trimethylsilyl, triethylsilyl, and tert-butyldimethylsilyl. 4 Preferred are a hydrogen atom, a methyl group, an ethyl group, and a trimethylsilyl group.

[0023] R in Equation (2) 5 The alkylene group having 1 to 20 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include methylene, ethylene, propylene, trimethylene, tetramethylene, isobutylene, pentamethylene, hexamethylene, heptamethylene, octamethylene, nonamethylene, and decylene groups. Among these, R 5 As the alkyl group, an ethylene group or a propylene group is particularly preferred.

[0024] In the formula (2), n represents a number satisfying 1 to 20, preferably a number of 1 to 10, and particularly preferably a number of 3 to 10. If n is less than 3, sufficient rubber strength may not be obtained.

[0025] The above o represents a number satisfying a range of 0 to 20, and is preferably a number of 0 to 10, and particularly preferably a number of 0 to 5. If o exceeds 20, sufficient rubber strength may not be obtained.

[0026] Specific examples of the A-(ii) component include the following. Here, "OTMS" represents a trimethylsiloxy group (hereinafter the same). [ka]

[0027] (iii) An organopolysiloxane represented by the following average formula (3), having a number average molecular weight (Mn) of 3,000 to 100,000 as determined by GPC measurement (standard polystyrene equivalent) using THF solvent: [ka] (In formula (3), R 1 is the same as above, A is a siloxane unit satisfying the following formula (4) or (5), and p, q, and r are numbers that respectively satisfy p>0, q>0, and r>0, and (p+q+r)=1. [ka] (In formulas (4) and (5), R 1 , R 2 , and R 3 is the same as above, c represents an integer of 1 to 3, and s represents a number of 0 to 10.

[0028] Specific examples of the A-(iii) component include the following. [ka]

[0029] In the formula (4), c represents an integer of 1 to 3, preferably 1 or 2, and particularly preferably 1.

[0030] In formula (3), p, q, and r are numbers that satisfy p>0, q>0, and r>0, respectively, and that satisfy (p+q+r)=1.

[0031] The ratio (p+q) / r of M units to Q units in the component (iii) is preferably from 0.3 to 2.0, and more preferably from 0.5 to 1.0.

[0032] The number average molecular weight of the component (iii) is preferably 3,000 to 100,000, and more preferably 2,000 to 10,000.

[0033] Since component (iii) may be in a solid state at 25° C., it may be dissolved in an organopolysiloxane such as component (i) above before use.

[0034] The component (A) may be used alone or in combination of two or more. In particular, when the component (i) is an organopolysiloxane containing only an alkenyl group, an alkenyloxy group, or an alkenyloxyalkyl group, the component (i) alone does not undergo ultraviolet curing (radical polymerization), so the components (i) and (ii) are used in combination for curing (ene-thiol reaction). In this case, the ratio of the amount of the alkenyl group, the alkenyloxy group, or the alkenyloxyalkyl group contained in the component (i) to the amount of the thiol group contained in the component (ii) is preferably 1:0.5 to 1:10, more preferably 1:0.8 to 1:3. In addition, the component (iii) may be in a solid state at 25°C. Therefore, it may be dissolved in an organopolysiloxane or a liquid organic compound containing a (meth)acrylic group as shown in the component (i) before use. The weight ratio of component (iii) to component (i) or the (meth)acrylic group-containing liquid organic compound when dissolved is preferably 1:0.1 to 1:10, more preferably 1:0.2 to 1:2. The viscosity of the solution at 25°C is preferably 100,000 mPa·s or less (usually 1 to 100,000 mPa·s), more preferably 10,000 mPa·s or less (for example, 5 to 10,000 mPa·s). If the viscosity at 25°C exceeds 100,000 mPa·s, the fluidity is low, and handling and coating may be difficult.

[0035] In the composition of the present invention, the component (A) is preferably from 70 to 99 mass %, and more preferably from 80 to 99 mass %.

[0036] (B) Component The component (B) of the present invention is a photopolymerization initiator that generates organic radical species upon absorbing ultraviolet light, and serves as the starting point for a radical polymerization reaction. Specific examples of photopolymerization initiators that can be used in the present invention include 2,2-diethoxyacetophenone, 2,2-dimethoxy-1,2-diphenylethan-1-one (Omnirad 651, manufactured by IGM Resins BV), 1-hydroxy-cyclohexyl-phenyl-ketone (Omnirad 184, manufactured by IGM Resins BV), ethyl phenyl(2,4,6-trimethylbenzoyl)phosphinate (Omnirad TPO-L, manufactured by IGM Resins BV), 2-hydroxy-2-methyl-1-phenyl-propan-1-one (Omnirad 1173, manufactured by IGM Resins BV), 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propan-1-one (Omnirad 1213, manufactured by IGM Resins BV), and the like. 127), 2-(dimethylamino)-2-(4-methylbenzyl)-1-(4-morpholinophenyl)butan-1-one (Omnirad 379, manufactured by IGM Resins BV), and phenylglyoxylic acid methyl ester (Omnirad MBF, manufactured by IGM Resins BV). Among these, from the viewpoint of compatibility with the components (A) and (B), 2,2-diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one (Omnirad 1173 manufactured by IGM Resins BV), and ethyl phenyl(2,4,6-trimethylbenzoyl)phosphinate (Omnirad TPO-L manufactured by IGM Resins BV) are preferred. The component (B) may be used alone or in combination of two or more.

[0037] The amount of the photopolymerization initiator added is within the range of 0.01 to 20% by mass relative to the total mass of the component (A). If it is less than 0.01% by mass, the curability is insufficient, and if it is added in an amount exceeding 20% ​​by mass, the curability in deep areas is deteriorated.

[0038] (C) Component The component (C) of the present invention is a photochromic dye, preferably a photochromic dye having a spiropyran skeleton, a spirooxazine skeleton, or a diarylethene skeleton. These dyes are colorless or have a slight color when dispersed in a silicone composition, but when exposed to ultraviolet light, they instantly develop a strong color. In addition, it is known that these dyes fade when the ultraviolet light irradiation is stopped or when exposed to visible light, so they are useful even when the silicone cured product has a problem of coloring.

[0039] Specific examples of the photochromic dye having a spiropyran skeleton, a spirooxazine skeleton, or a diarylethene skeleton include, but are not limited to, those shown below. [ka]

[0040] In the present invention, the component (C) may be used alone or in combination with a plurality of different compounds. Most of the compounds exemplified above as the component (C) are solid, so when they are added, they may be dissolved and diluted in a solvent such as acetone or toluene. The amount of the additive is preferably 10 to 1000 ppm, more preferably 10 to 500 ppm, and even more preferably 30 to 300 ppm, relative to the total amount of components (A) and (B). If the amount is less than 10 ppm, the color is weak and difficult to visually confirm. If the amount is more than 1000 ppm, the additive may precipitate from the silicone, causing poor appearance and poor application, and may compete with the photodecomposition reaction of component (B) during UV irradiation, resulting in poor curing.

[0041] Other Ingredients In addition to the components (A) to (C), the ultraviolet-curable silicone composition of the present invention may contain other components, such as those exemplified below, as long as the object of the present invention is not impaired.

[0042] For example, organic compounds having an adhesive group such as a carbonyl group, an epoxy group, or an alkoxysilyl group in one molecule to impart adhesiveness to the substrate; organopolysiloxanes having a condensation curing group such as a silanol group or an alkoxysilyl group; metal catalysts such as organic titanium, organic zirconium, or organic bismuth that activate the adhesive group or catalyze the condensation curing reaction; thixotropy control agents such as fumed silica; reinforcing agents such as crystalline silica; antioxidants; light stabilizers; heat resistance improvers such as metal oxides and metal hydroxides; flame retardant agents such as platinum group metal catalysts; thermal conductivity imparting fillers such as alumina and crystalline silica; viscosity adjusters such as non-reactive silicone oils that do not have reactive functional groups; and electrical conductivity imparting agents such as metal powders such as silver and gold. The ultraviolet-curable silicone composition of the present invention may optionally contain dyes and pigments as necessary within a range that does not affect its purpose and effect, but it is preferable that the composition does not contain black pigments such as carbon black when it is difficult to visually recognize the hue change associated with the color development of the photochromic dye.

[0043] [Method of manufacturing a color-developing UV-curable silicone coating composition] The method for producing the color-developing ultraviolet-curable silicone coating composition of the present invention is not particularly limited, and the composition can be produced by mixing components (A), (B), and (C) as well as other components that are added as necessary in a conventional manner.

[0044] [Use of color-developing UV-curable silicone coating composition] The color-developing UV-curable silicone coating composition of the present invention has the characteristics of silicone resin, such as excellent applicability, good mechanical strength even after curing, excellent insulation, heat resistance and flame retardancy, and when irradiated with UV rays, it cures and develops color, and then gradually fades when UV rays are blocked or when irradiated with visible light. Therefore, the part where the composition of the present invention is applied can be easily confirmed visually after UV irradiation is completed, so it can be used as a method for confirming the applied part. In addition, since it fades after confirmation, it can also be used for parts where coloring is not desirable in use. That is, as one aspect of the present invention, A step of applying the color-forming ultraviolet-curable silicone coating composition of the present invention onto a substrate; Irradiating the composition-applied portion of the substrate with ultraviolet light; and A step of visually checking the composition-applied portion on the substrate. The method includes a method for confirming the applied portion of the composition.

[0045] [Coating process] The substrate used in the confirmation method of the present invention is not particularly limited, but examples thereof include various substrates such as glass, various organic resins, metals, and alloys. The method for applying the color-developing ultraviolet-curable silicone coating composition of the present invention to a substrate is not particularly limited, but examples thereof include wet coating methods (wet application methods) such as brush coating, immersion (dip coating), flow coating, spin coating, and spray coating. The color-developing ultraviolet-curable silicone coating composition of the present invention may be applied to a substrate in a thickness desired for the application. [Ultraviolet irradiation process] In the ultraviolet irradiation process, ultraviolet light is irradiated onto the liquid silicone composition. As a light source of ultraviolet light, a 365 nm UV-LED lamp, a metal halide lamp, a high pressure mercury lamp, etc. can be used, and as an ultraviolet light irradiation method, a method of irradiating an appropriate amount of ultraviolet light onto the composition can be mentioned, but when it is performed on a transparent substrate such as glass or a resin film, ultraviolet light may be irradiated through the glass or film. When irradiating ultraviolet light, it may be performed under air, or in order to suppress the effect of curing inhibition by oxygen, it may be performed under a nitrogen or argon atmosphere. For ultraviolet irradiation, light having a wavelength of preferably 200 to 500 nm, more preferably 200 to 350 nm is used. From the viewpoint of preventing discoloration, the irradiation temperature is preferably 20 to 40°C, and the irradiation intensity is preferably 30 to 2,000 mW / cm. 2 is preferable, and the exposure dose is 150 to 100,000 mJ / cm 2 is preferred. [Confirmation process] In the confirmation step, the applied portion is visually confirmed. The color-developing UV-curable silicone coating composition of the present invention is colorless or has a slight color before the UV irradiation step, but hardens and develops color by the UV irradiation step, so that it is possible to visually confirm whether the composition has been applied to the desired portion by observing the change in color tone without the need for a special inspection device.

[0046] The color-developing UV-curable silicone coating composition of the present invention is preferably one in which there is little change in light transmittance between the composition before UV irradiation and the cured product which has been irradiated with UV light to develop a color and then blocked from UV light or has been irradiated with visible light to fade. For example, when the sample thickness is kept under the same conditions for light transmittance measurement, and the light transmittance at 800 nm before UV irradiation is taken as 100, it is preferred that the cured product obtained after UV irradiation has a light transmittance at 800 nm of 90 or more after being left at 23°C for 7 days under visible light irradiation.

[0047] The color-developing UV-curable silicone coating composition of the present invention can be suitably used as a surface protective agent for substrates or as a conformal coating agent for electronic substrates. EXAMPLES

[0048] [Examples 1 to 6, Comparative Examples 1 to 3, Table 1] The following components were mixed in the amounts shown in Table 1 to prepare an ultraviolet-curable silicone composition. In Table 1, the amounts of component (A), component (B), and nanosilica are expressed in parts by mass, and the amount of component (C) is expressed as a ratio (ppm) to the total mass of components (A) and (B). To prepare an ultraviolet-curable silicone composition, each component was mixed and thoroughly degassed, and then the silicone composition was irradiated with a UV-LED lamp having a wavelength of 365 nm at an irradiation intensity of 100 mW / cm under a nitrogen environment. 2 and a dose of 3,000 mJ / cm 2 After curing, the appearance of the cured product of the UV-curable silicone composition was visually inspected and the results are shown in Table 1. In addition, "Vi" represents a vinyl group, "Me" represents a methyl group, and "OTMS" represents a trimethylsiloxy group.

[0049] [Summary of added ingredients] (A)-(i)-1 A linear dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups and having a viscosity of 5000 mPa s at 23°C, as represented by the following formula: ViMe2Si (OMe2Si) 430 OSiMe2Vi

[0050] (A)-(i)-2 A linear dimethylpolysiloxane capped at both ends with propenyloxy groups and having a viscosity of 5000 mPa s at 23°C, as represented by the following formula: [ka]

[0051] (A)-(i)-3 A linear organopolysiloxane terminated at both molecular chain ends with acryloyloxy groups and having a viscosity of 3,000 mPa·s at 23°C, as represented by the following formula: [ka] (wherein the arrangement of the siloxane units in the parenthesized main chain is random)

[0052] (A)-(ii)-1 Thiol-containing dimethylpolysiloxane represented by the following formula: [ka]

[0053] (A)-(iii)-1 The average unit formula is: (ViMe2SiO 1 / 2 ) 0.07 (Me3SiO 1 / 2 ) 0.39 (SiO 4 / 2 )0.54 A dimethylpolysiloxane solution of a vinyl group-containing siloxane resin represented by the formula (weight ratio: resin / dimethylpolysiloxane polymer (A)-(i)-1 component=1 / 1)

[0054] (B) Component 2-Hydroxy-2-methyl-1-phenyl-propan-1-one (Omnirad 1173, IGM Resins BV)

[0055] (C) Component (C-1) DAE-0001 (diarylethene skeleton type) manufactured by Yamada Chemical Industry Co., Ltd. (C-2) Yamada Chemical Industry Co., Ltd. DAE-0068 (diarylethene skeleton type) (C-3) TPC-0021 (spiropyran skeleton type) manufactured by Yamada Chemical Industry Co., Ltd. (C-4) TPC-0073 (spiropyran skeleton type) manufactured by Yamada Chemical Industry Co., Ltd. Note: The above (C-1) to (C-4) are 5% by mass solutions of each photochromic dye in toluene.

[0056] Other ingredients: Nanosilica (reinforcing agent)

[0057] [Table 1]

[0058] [Whether or not visual confirmation of thin film is possible] Each composition shown in Table 1 was applied to a thickness of 100 μm on a glass slide substrate, and then irradiated with ultraviolet light under the same conditions as above to cure. The applied area was visually confirmed to be distinguishable by the change in color tone before and after ultraviolet light irradiation. The results are shown in Table 2.

[0059] [Table 2]

[0060] The laminates prepared in Table 2 above, in which each composition was cured and laminated to a thickness of 100 μm on a slide glass, were measured for transmittance at 800 nm using a spectroscopic hardness meter, and the laminates were then left to stand under visible light irradiation at 23° C. for one week, and the presence or absence of fading (change in color tone) and changes in light transmittance were confirmed. The results are shown in Table 3.

[0061] [Table 3]

Claims

1. (A) an organopolysiloxane having a radical reactive group, (B) Photopolymerization initiator: 0.01 to 20% by mass based on the mass of component (A), and (C) Photochromic dye: 10 to 1,000 ppm based on the total mass of component (A) and component (B) A color-developing ultraviolet-curable silicone coating composition comprising:

2. 2. The color-developing ultraviolet-curable silicone coating composition according to claim 1, which is cured by radical polymerization of (meth)acrylic groups or by a thiol-ene reaction.

3. 2. The color-developing ultraviolet-curable silicone coating composition according to claim 1, wherein component (C) is a photochromic dye having a diarylethene skeleton, a spiropyran skeleton, or a spirooxazine skeleton.

4. 2. The color-developing ultraviolet-curable silicone coating composition according to claim 1, which is cured and develops color upon exposure to ultraviolet light.

5. 2. The color-developing ultraviolet-curable silicone coating composition according to claim 1, which develops color when irradiated with ultraviolet light and then fades when the ultraviolet light is blocked or when irradiated with visible light.

6. 2. The color-developing ultraviolet-curable silicone coating composition according to claim 1, wherein the light transmittance of the composition before ultraviolet irradiation to light at 800 nm is taken as 100, and the cured product obtained after ultraviolet irradiation has a light transmittance of 90 or more after being allowed to stand for 7 days at 23°C.

7. A method for confirming the portion on a substrate to which the color-developing ultraviolet-curable silicone coating composition according to any one of claims 1 to 6 has been applied, the method comprising the steps of: applying the color-developing ultraviolet-curable silicone coating composition on a substrate; irradiating the composition on the substrate with ultraviolet light to cause it to develop color; and visually confirming the portion to which the composition has been applied after the ultraviolet light irradiation is completed.

Citation Information

Patent Citations

  • Photochromic curable composition, cured product thereof, and laminate including said cured product

    JP2017052869A

  • Method for producing active energy ray-curable water-soluble resin composition containing photochromic dye and coating composition, and cured article

    JP2022037865A

  • Free radical polymerizable adhesion-promoting interlayer compositions and methods of use

    US20210402748A1

  • Coating product and coating system

    WO2013001992A1

  • Crane maneuvering assistance

    WO2013006625A2