Rubber composition for bead filler

A rubber composition for bead fillers using isoprene rubber and hydrogenated aromatic vinyl-conjugated diene copolymer with specific additives achieves high hardness, low heat generation, and good processability, enhancing tire performance and efficiency.

JP2024165078APending Publication Date: 2024-11-28THE YOKOHAMA RUBBER CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023080919
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing rubber compositions for bead fillers in tires struggle to achieve a balance between high rubber hardness and low heat build-up while maintaining good processability, with conventional methods either compromising on one or the other.

Method used

A rubber composition for bead fillers comprising 30% to 80% isoprene rubber and 20% to 70% hydrogenated aromatic vinyl-conjugated diene copolymer, with a hydrogenation rate of 60% to 80%, blended with a novolac type phenolic resin, hexamethylenetetramine, and/or melamine derivative, and carbon black, to enhance hardness, reduce heat generation, and maintain processability.

Benefits of technology

The composition achieves improved rubber hardness, reduced heat build-up, and enhanced processability, resulting in a lightweight and fuel-efficient tire with stable production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165078000001
    Figure 2024165078000001
  • Figure 2024165078000002
    Figure 2024165078000002
  • Figure 2024165078000003
    Figure 2024165078000003
Patent Text Reader

Abstract

To provide a rubber composition for bead fillers that exhibits rubber hardness and low heat generation that surpass conventional levels, while ensuring processability.SOLUTION: A rubber composition for bead fillers contains a diene rubber composed of 30 mass% or more of an isoprene rubber and 20-70 mass% of a hydrogenated aromatic vinyl-conjugated diene copolymer, where the hydrogenated aromatic vinyl-conjugated diene copolymer has a hydrogenation rate of 60-80%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition for bead fillers which satisfies both high rubber hardness and low heat build-up. [Background technology]

[0002] In order to reduce the environmental load, there is a demand for tires that are lighter and have lower heat generation. For example, a method is known in which a rubber component with a low glass transition temperature (Tg) is compounded to change the behavior of the loss tangent (tan δ) of the rubber (see, for example, Patent Documents 1 and 2). These methods are mainly used for tread rubber, but there is a limit to how much lowering the heat generation of tires can be achieved by only reducing the tan δ (60°C) of the tread rubber. For example, for bead fillers that use a high-hardness rubber composition to improve the steering stability of tires, technology that achieves both high rubber hardness and low heat generation has not yet been fully developed.

[0003] As a measure to increase the hardness of a bead filler, it has been proposed to compound a resin component into a rubber composition for a bead filler (for example, see Patent Document 3). However, in general, the processability of a rubber composition tends to decrease as the hardness increases by compounding a resin component, so that in order to increase the hardness of a rubber composition, it is required to maintain good processability and achieve a good balance between these performances. Therefore, it is required to improve the rubber hardness and low heat buildup properties to levels higher than those of conventional rubber compositions while maintaining good processability. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2021-035801 [Patent Document 2] Patent Publication No. 2021-066371 [Patent Document 3] JP 2014-118507 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a rubber composition for bead fillers which has excellent rubber hardness and low heat build-up properties beyond conventional levels while ensuring processability. [Means for solving the problem]

[0006] The rubber composition for bead filler of the present invention, which achieves the above object, is characterized in that it contains a diene rubber consisting of 30 mass % or more of an isoprene-based rubber and 20 to 70 mass % of a hydrogenated aromatic vinyl-conjugated diene copolymer, and the hydrogenation rate of the hydrogenated aromatic vinyl-conjugated diene copolymer is 60 to 80%. Effect of the Invention

[0007] The rubber composition for bead fillers of the present invention contains an isoprene-based rubber and a diene-based rubber consisting of a hydrogenated aromatic vinyl-conjugated diene copolymer having a hydrogenation rate of 60 to 80%, so that the rubber hardness and low heat build-up can be improved beyond conventional levels while ensuring processability.

[0008] The rubber composition for bead fillers further contains a novolac type phenolic resin, and hexamethylenetetramine and / or a melamine derivative, and is preferably such that 5 to 50 parts by mass of the novolac type phenolic resin is blended with 100 parts by mass of the diene rubber, and 5 to 20% by mass of the hexamethylenetetramine and / or melamine derivative is blended with respect to the blending amount of the novolac type phenolic resin.

[0009] The hydrogenated aromatic vinyl-conjugated diene copolymer is preferably a hydrogenated styrene-butadiene rubber having a butylene content of 15% or more, which can reduce tan δ at 60° C. and further improve low heat build-up properties.

[0010] A tire having a bead filler made of the above-mentioned rubber composition for bead fillers achieves both light weight and low fuel consumption performance, and can be stably produced as a high-quality tire. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The rubber composition for bead filler of the present invention contains isoprene rubber and hydrogenated aromatic vinyl-conjugated diene copolymer as diene rubber. By containing isoprene rubber, it is possible to obtain a rubber composition with excellent balance between processability and physical properties of unvulcanized rubber. Examples of isoprene rubber include natural rubber and isoprene rubber. The content of isoprene rubber is 30% by mass or more, preferably 30 to 80% by mass, more preferably 35 to 75% by mass, and further preferably 40 to 70% by mass, based on 100% by mass of diene rubber. If the isoprene rubber is less than 30% by mass, the effect of improving processability and physical properties cannot be sufficiently obtained. Also, if it exceeds 80% by mass, the effect of hydrogenated aromatic vinyl-conjugated diene copolymer cannot be sufficiently obtained.

[0012] The rubber composition for bead filler contains a hydrogenated aromatic vinyl-conjugated diene copolymer, which can ensure processability while simultaneously achieving both rubber hardness and low heat buildup, and is superior to conventional levels. Furthermore, the tensile strength at break and tensile elongation at break can be improved to levels higher than conventional levels. The hydrogenated aromatic vinyl-conjugated diene copolymer is contained in an amount of 20 to 70 mass%, preferably 25 to 65 mass%, and more preferably 30 to 60 mass% of 100 mass% of diene rubber. If the amount of hydrogenated aromatic vinyl-conjugated diene copolymer is less than 20 mass%, the effect of achieving both rubber hardness and low heat buildup cannot be sufficiently obtained. On the other hand, if the amount exceeds 70 mass%, the viscosity becomes excessively high and processability decreases. In addition, the effect of the isoprene rubber cannot be sufficiently obtained.

[0013] The hydrogenated aromatic vinyl-conjugated diene copolymer is a rubber component obtained by hydrogenating an aromatic vinyl-conjugated diene copolymer. The aromatic vinyl-conjugated diene copolymer is a copolymer of aromatic vinyl and conjugated diene, and is preferably a random copolymer. Examples of aromatic vinyl compounds constituting the aromatic vinyl-conjugated diene copolymer include styrene, methylstyrene, ethylstyrene, t-butylstyrene, α-methylstyrene, α-methyl-p-methylstyrene, chlorostyrene, bromostyrene, methoxystyrene, dimethylaminomethylstyrene, dimethylaminoethylstyrene, diethylaminomethylstyrene, diethylaminoethylstyrene, cyanoethylstyrene, and vinylnaphthalene. Among these, styrene is preferred. Examples of conjugated diene compounds constituting the aromatic vinyl-conjugated diene copolymer include 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, and 1,3-pentadiene. Examples of aromatic vinyl-conjugated diene copolymers include styrene-butadiene rubber (SBR) and styrene-isoprene rubber. Styrene-butadiene rubber is preferred. The aromatic vinyl-conjugated diene copolymer may contain any other copolymerizable monomer in addition to the aromatic vinyl compound and the conjugated diene compound. The aromatic vinyl-conjugated diene copolymer may be polymerized using any of solution polymerization, gas phase polymerization, and bulk polymerization, but solution polymerization is preferred. The polymerization method may be either batch or continuous. The aromatic vinyl-conjugated diene copolymer may have its polymerization initiation end, termination end, side chain, etc. modified with a functional group to increase its affinity with silica and / or carbon black. Preferred examples of such functional groups include epoxy groups, carboxy groups, amino groups, hydroxy groups, alkoxy groups, silyl groups, alkoxysilyl groups, amide groups, oxysilyl groups, silanol groups, isocyanate groups, isothiocyanate groups, carbonyl groups, aldehyde groups, and groups having a polyorganosiloxane structure or an aminosilane structure.

[0014] The method and conditions for the reaction of hydrogenating (hydrogenating) an aromatic vinyl-conjugated diene polymer are not particularly limited. Examples of the method for hydrogenating an aromatic vinyl-conjugated diene polymer include a method using a catalyst mainly composed of an organometallic compound of titanium as a hydrogenation catalyst, a method using a catalyst composed of an organic compound of iron, nickel, or cobalt and an organometallic compound such as alkylaluminum, a method using an organic complex of an organometallic compound such as ruthenium or rhodium, and a method using a catalyst in which a metal such as palladium, platinum, ruthenium, cobalt, or nickel is supported on a carrier such as carbon, silica, or alumina.

[0015] The hydrogenated aromatic vinyl-conjugated diene copolymer preferably has a weight average molecular weight of 200,000 or more, a glass transition temperature of -40°C or less, and a hydrogenation rate of 60% or more. The weight average molecular weight of the hydrogenated aromatic vinyl-conjugated diene copolymer is more preferably 200,000 to 700,000, and even more preferably 250,000 to 600,000. When the weight average molecular weight of the hydrogenated aromatic vinyl-conjugated diene copolymer is 200,000 or more, the rubber hardness and tensile strength at break of the rubber composition can be increased. In addition, when the weight average molecular weight is 700,000 or less, the viscosity increase of the rubber composition for bead filler is suppressed, and both processability and strength are achieved, which is preferable. In this specification, the weight average molecular weight of the hydrogenated aromatic vinyl-conjugated diene copolymer can be a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0016] The hydrogenated aromatic vinyl-conjugated diene copolymer preferably has a glass transition temperature of -40°C or lower, more preferably -80°C to -40°C, and even more preferably -75°C to -40°C. When the hydrogenated aromatic vinyl-conjugated diene copolymer has a glass transition temperature of -40°C or lower, it is preferable that the copolymer can ensure sufficient flexibility even when used in cold regions. In addition, when the glass transition temperature is -80°C or higher, it is preferable that a tire rubber composition having an excellent balance between hardness and flexibility can be obtained. In this specification, the glass transition temperature can be determined as the midpoint temperature of the transition region measured by differential scanning calorimetry (DSC) at a temperature rise rate of 20°C / min.

[0017] The hydrogenated aromatic vinyl-conjugated diene copolymer has a hydrogenation rate (hydrogenation rate) of 60-80%, preferably 62-78%, and more preferably 64-76%. If the hydrogenation rate is less than 60%, it is difficult to achieve both high levels of rubber hardness and low heat buildup. Furthermore, the effect of improving the tensile break strength is not sufficiently obtained. If the hydrogenation rate exceeds 80%, the viscosity increases significantly and the processability decreases. Furthermore, the crosslinking property of the hydrogenated aromatic vinyl-conjugated diene copolymer becomes insufficient. In this specification, the hydrogenation rate refers to the percentage (%) of hydrogenated carbon-carbon bonds in the conjugated diene portion of the aromatic vinyl-conjugated diene copolymer relative to the total of 100% of carbon-carbon double bonds before hydrogenation. A hydrogenation rate of 100% means that the carbon-carbon double bonds in the conjugated diene portion have been completely hydrogenated. The hydrogenation rate is 1 It can be calculated from the spectral reduction rate of the unsaturated bond in the conjugated diene portion of the spectrum obtained by measuring H-NMR.

[0018] The hydrogenated aromatic vinyl-conjugated diene copolymer is preferably hydrogenated styrene butadiene rubber, and the butylene content is preferably 15% or more. Here, the butylene content refers to the amount equivalent to the hydrogenated product of the 1,2-bond butadiene-derived unit (ethylene having an ethyl side chain) in the hydrogenated styrene butadiene rubber. On the other hand, the hydrogenated product of the 1,4-bond butadiene-derived unit is n-butylene, and is measured as two molecules of ethylene. When the butylene content is 15% or more, the tan δ at 60°C can be further reduced, and low heat generation can be achieved. The butylene content of the hydrogenated styrene butadiene rubber is more preferably 15 to 65%, further preferably 20 to 60%, and particularly preferably 25 to 55%. In this specification, when the hydrogenated styrene butadiene rubber is divided into a styrene amount Ms corresponding to units derived from styrene, a butadiene amount Mb1 corresponding to units derived from 1,4-bond butadiene, an n-butylene amount Mb2 corresponding to hydrogenated products of units derived from 1,4-bond butadiene, and a butylene amount Mb3 corresponding to hydrogenated products of units derived from 1,2-bond butadiene, the butylene amount Mb3% is calculated by the following formula. Mb3%=Mb3 / (Ms+Mb1+Mb2+Mb3)×100 In addition, the styrene amount Ms, butadiene amount Mb1, butane amount Mb2, and butylene amount Mb3 of hydrogenated styrene-butadiene rubber can be calculated from the microstructures before and after hydrogenation, 1 It can be measured using H-NMR.

[0019] The rubber composition for bead filler may contain other diene rubbers other than isoprene rubber and hydrogenated aromatic vinyl-conjugated diene copolymer. Examples of other diene rubbers include non-hydrogenated aromatic vinyl-conjugated diene copolymers (such as styrene-butadiene rubber), butadiene rubber, butyl rubber, halogenated butyl rubber, acrylonitrile-butadiene rubber, and the like. These other diene rubbers may be modified diene rubbers having functional groups, and may be used alone or as any blend. Among these, styrene-butadiene rubber is preferred. The content of the other diene rubber is preferably 0 to 40 mass%, more preferably 0 to 30 mass%, in 100 mass% of the diene rubber.

[0020] The rubber composition for bead filler is preferably blended with a thermosetting resin and a curing agent. By blending the thermosetting resin and the curing agent, the rubber hardness and tensile breaking strength of the rubber composition can be increased. Examples of the thermosetting resin include phenolic resin, epoxy resin, polyester resin, urethane resin, urea resin, and melamine resin. In particular, phenolic resin is preferable, and among them, novolac type phenolic resin is preferable.

[0021] As the novolac type phenolic resin, those that are usually blended in rubber compositions for tires can be used. For example, there can be mentioned those produced by condensing phenols such as phenol, cresol, resorcin, and tert-butylphenol, or mixtures thereof, with formaldehyde in the presence of an acid catalyst such as hydrochloric acid or oxalic acid. There can also be mentioned novolac type modified phenolic resins obtained by modifying novolac type phenolic resins with oils, and examples of the oils used to modify novolac type phenolic resins include cashew oil, rosin oil, tall oil, linoleic acid, oleic acid, and linoleic acid. Among them, novolac type cashew modified phenolic resins modified with cashew oil are preferred. These novolac type phenolic resins can be used alone or in any mixture.

[0022] The amount of modification with cashew oil in the novolac phenolic resin modified with cashew oil is preferably 35 to 45 mass%, more preferably 37 to 42 mass%, based on 100 mass% of the novolac phenolic resin. By setting the amount of modification with cashew oil within this range, the breaking properties can be significantly improved.

[0023] These novolac-type phenolic resins can be commercially available products. Examples of phenolic resins include Sumikanol 620 manufactured by Sumitomo Chemical Co., Ltd. Examples of phenolic resins modified with cashew oil include Sumilite Resin PR-YR-170 and PR-150 manufactured by Sumitomo Bakelite Co., Ltd., and Phenolite A4-1419 manufactured by Dainippon Ink and Chemicals, Inc.

[0024] The novolac phenolic resin is preferably blended in an amount of 5 to 50 parts by mass, more preferably 10 to 30 parts by mass, per 100 parts by mass of diene rubber. When the blending amount of the novolac phenolic resin is 5 parts by mass or more, the rubber strength and tensile strength at break of the rubber composition can be increased. When the blending amount of the novolac phenolic resin is 50 parts by mass or less, low heat buildup can be maintained.

[0025] The rubber composition for bead filler may contain cardanol oligomer in addition to the novolac phenolic resin. The use of cardanol oligomer in combination can further increase the rubber hardness of the rubber composition for bead filler. An example of the cardanol oligomer is cashew oil. Cashew oil is a liquid oil at room temperature obtained from the shell of cashew seeds (cashew nuts). In particular, this refers to industrial cashew oil that is heated after oil extraction to decarbonate the main component anacardic acid, resulting in cardanol being the main component. The industrial cashew oil contains cardol and 2-methyl cardol in addition to cardanol, the main component. Cashew oil is a naturally derived material, and is therefore advantageous in reducing environmental impact.

[0026] The cardanol oligomer is preferably blended in an amount of 7 to 25 parts by mass, more preferably 10 to 20 parts by mass, per 100 parts by mass of diene rubber. When the cardanol oligomer is blended, the cardanol oligomer functions as a processability modifier to improve the processability of the rubber composition, while the hardness of the rubber composition after vulcanization can be increased due to the thermosetting property of the cardanol oligomer. As a result, sufficient hardness and processability can be highly compatible as a rubber composition for bead fillers. Blending 10 parts by mass or more of the cardanol oligomer is preferable because it has the effect of increasing processability and hardness. When the cardanol oligomer is 25 parts by mass or less, the rubber hardness can be appropriately increased and the influence on the tensile strength at break and low heat buildup can be suppressed.

[0027] It is also preferable to incorporate hexamethylenetetramine and melamine derivatives as a hardener for the novolak type phenolic resin. Examples of melamine derivatives include hexamethoxymethylolmelamine, pentamethoxymethylmelamine, hexamethoxymethylmelamine, pentamethoxymethylmelamine, hexaethoxymethylmelamine, hexakis-(methoxymethyl)melamine, N,N',N"-trimethyl-N,N',N"-trimethylolmelamine, N,N',N"-trimethylolmelamine, N-methylolmelamine N,N'-(methoxymethyl)melamine, and N,N',N"-tributyl-N,N',N"-trimethylolmelamine. Of these, hexamethylenetetramine, hexamethoxymethylolmelamine, pentamethoxymethylolmelamine, hexamethoxymethylmelamine, and pentamethoxymethylmelamine are preferred. Hexamethylenetetramine and melamine derivatives can be used alone or in combination.

[0028] An example of hexamethylenetetramine is Sancerer HT-PO manufactured by Sanshin Chemical Industry Co., Ltd. An example of hexamethoxymethylmelamine (HMMM) is CYREZ 964RPC manufactured by Cytec Industries Co., Ltd. An example of pentamethoxymethylmelamine (PMMM) is Sumikanol 507A manufactured by Bara Chemical Co., Ltd.

[0029] The amount of hexamethylenetetramine and / or melamine derivative is preferably 5 to 20 mass % relative to the amount of the novolac phenolic resin, more preferably 8 to 15 mass %. If the amount of hexamethylenetetramine and melamine derivative is less than 5 mass % of the amount of the novolac phenolic resin, the crosslink density of the novolac phenolic resin is low and the heat generation property is also deteriorated. If the amount of hexamethylenetetramine and melamine derivative exceeds 20 mass %, the crosslink density of the novolac phenolic resin becomes too high, making it prone to brittle fracture and deteriorating tire durability.

[0030] The rubber composition for bead filler is preferably blended with carbon black, since it can increase the tensile breaking strength and rubber hardness of the rubber composition. As the carbon black, furnace black, acetylene black, thermal black, channel black, graphite, and other carbon blacks may be blended. Among these, furnace black is preferable, and specific examples thereof include SAF, ISAF, ISAF-HS, ISAF-LS, IISAF, IISAF-HS, HAF, HAF-HS, HAF-LS, FEF, and GPF. Among these, ISAF, HAF, and FEF are more preferable, and HAF is further preferable. These carbon blacks can be used alone or in combination of two or more kinds. In addition, surface-treated carbon blacks obtained by chemically modifying these carbon blacks with various acid compounds and the like can also be used.

[0031] The nitrogen adsorption specific surface area N2SA of the carbon black is preferably 30 to 160 m 2 / g, more preferably 35 to 120m 2 / g, more preferably 60 to 100m 2 / g. The nitrogen adsorption specific surface area of ​​carbon black is 30 m 2 When the carbon black has a nitrogen adsorption specific surface area of ​​160 m / g or more, the rubber strength and hardness of the rubber composition can be ensured, which is preferable. 2 By setting the nitrogen adsorption specific surface area of ​​carbon black to be not more than 1 / g, heat buildup can be reduced, which is preferable. In this specification, the nitrogen adsorption specific surface area of ​​carbon black can be measured in accordance with JIS K6217-2.

[0032] The carbon black is preferably blended in an amount of 5 to 200 parts by mass, more preferably 10 to 150 parts by mass, and further preferably 20 to 100 parts by mass, per 100 parts by mass of diene rubber. By blending 5 parts by mass or more of carbon black, the rubber hardness and tensile strength at break can be increased. Also, by blending 200 parts by mass or less, the effect on heat build-up can be suppressed.

[0033] In addition to carbon black, the rubber composition for bead fillers may contain inorganic fillers such as silica, clay, calcium carbonate, mica, talc, aluminum hydroxide, aluminum oxide, titanium oxide, and barium sulfate.

[0034] In addition to the above components, various compounding agents generally used in rubber compositions for bead fillers, such as vulcanizing or crosslinking agents, vulcanization accelerators, antiaging agents, processing aids, plasticizers, liquid polymers, thermosetting resins, and thermoplastic resins, can be compounded in the rubber composition for bead fillers in a conventional manner. Such compounding agents can be kneaded in a conventional manner to prepare a rubber composition, which can then be used for vulcanization or crosslinking. The compounding amounts of these compounding agents can be conventionally used amounts as long as they do not go against the object of the present invention. The rubber composition for bead fillers can be prepared by mixing the above components using a known rubber kneading machine, such as a Banbury mixer, a kneader, or a roll.

[0035] The rubber composition for bead filler is suitable for forming a bead filler of a tire. A tire having a bead filler formed from the above-mentioned rubber composition has excellent processability while achieving both weight reduction and low fuel consumption performance, and can stably produce a high-quality tire.

[0036] The present invention will be further described below with reference to examples, but the scope of the present invention is not limited to these examples. EXAMPLES

[0037] In the following examples, we used styrene butadiene rubber (SBR) and hydrogenated aromatic vinyl-conjugated diene copolymers (hydrogenated SBR-1 to hydrogenated SBR-5) shown in Table 1. Hydrogenated SBR-1 to hydrogenated SBR-5 were prepared by the following polymerization method.

[0038] [Table 1]

[0039] Polymerization method for hydrogenated SBR-1 In a nitrogen-purged 10L autoclave reactor, 4200g of cyclohexane, styrene (120g, 1.15mol), butadiene (480g, 8.91mol), tetrahydrofuran (0.433g, 6.0mmol) and 2,2-di(2-tetrahydrofuryl)propane (0.604g, 3.28mmol) were charged and stirring was started. After the temperature of the contents in the reaction vessel was raised to 50°C, a hexane solution of n-butyllithium (4.21ml at a concentration of 1.55mol / L, 6.52mmol of n-butyllithium) was added. After the polymerization conversion rate reached almost 100%, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane (0.254g, 0.82mmol) was added and reacted for 30 minutes. After the reaction, methanol (112.1 mg, 3.5 mmol) was added to stop the reaction, and a portion was extracted and dried for analysis. The styrene content was 20 mass%, the vinyl content was 55 mass% in butadiene, and the weight average molecular weight was 300,000. The reaction solution was heated to 80°C or higher and hydrogen was introduced into the system. Next, 0.70 g of a catalyst mainly composed of titanocene dichloride, 1.2 g of diethylaluminum chloride, and 0.30 g of n-butyllithium were added, and the reaction was carried out while maintaining a hydrogen pressure of 1.0 MPa. After reaching a predetermined cumulative hydrogen flow rate, the reaction solution was returned to room temperature and pressure and extracted from the reaction vessel to obtain a polymerization solution. After neutralization, solid rubber was recovered by steam stripping. The obtained solid rubber was dehydrated by a roll and dried in a dryer to obtain hydrogenated SBR-1. The hydrogenation rate was 68% and the butylene content was 44%.

[0040] Polymerization method for hydrogenated SBR-2 In a nitrogen-purged 10L autoclave reactor, 4200g of cyclohexane, styrene (30g, 0.29mol), butadiene (570g, 10.58mol), tetrahydrofuran (0.433g, 6.0mmol) and 2,2-di(2-tetrahydrofuryl)propane (0.147g, 0.80mmol) were charged and stirring was started. After the temperature of the contents in the reaction vessel was raised to 50°C, a hexane solution of n-butyllithium (3.11ml at a concentration of 1.55mol / L, 4.82mmol of n-butyllithium) was added. After the polymerization conversion rate reached almost 100%, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane (0.254g, 0.82mmol) was added and reacted for 30 minutes. After the reaction, methanol (80.1 mg, 2.5 mmol) was added to stop the reaction, and a portion was extracted and dried for analysis. The styrene content was 5 mass%, the vinyl content was 40 mass% in butadiene, and the weight average molecular weight was 390,000. The reaction solution was heated to 80°C or higher and hydrogen was introduced into the system. Next, 0.70 g of a catalyst mainly composed of titanocene dichloride, 1.2 g of diethylaluminum chloride, and 0.30 g of n-butyllithium were added, and the reaction was carried out while maintaining a hydrogen pressure of 1.0 MPa. After reaching a predetermined cumulative hydrogen flow rate, the reaction solution was returned to room temperature and pressure and extracted from the reaction vessel to obtain a polymerization solution. After neutralization, solid rubber was recovered by steam stripping. The obtained solid rubber was dehydrated by a roll and dried in a dryer to obtain hydrogenated SBR-2. The hydrogenation rate was 74% and the butylene content was 38%.

[0041] Polymerization method for hydrogenated SBR-3 In a nitrogen-purged 10L autoclave reactor, 4200g of cyclohexane, styrene (180g, 1.73mol), butadiene (420g, 7.79mol), tetrahydrofuran (0.433g, 6.0mmol) and 2,2-di(2-tetrahydrofuryl)propane (0.037g, 0.20mmol) were charged and stirring was started. After the temperature of the contents in the reaction vessel was raised to 50°C, a hexane solution of n-butyllithium (3.57ml at a concentration of 1.55mol / L, 5.54mmol of n-butyllithium) was added. After the polymerization conversion rate reached almost 100%, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane (0.254g, 0.82mmol) was added and reacted for 30 minutes. After the reaction, methanol (92.9 mg, 2.9 mmol) was added to stop the reaction, and a portion was extracted and dried for analysis. The styrene content was 30% by mass, the vinyl content was 25% by mass in butadiene, and the weight average molecular weight was 340,000. The reaction solution was heated to 80°C or higher and hydrogen was introduced into the system. Next, 0.70 g of a catalyst mainly composed of titanocene dichloride, 1.2 g of diethylaluminum chloride, and 0.30 g of n-butyllithium were added, and the reaction was carried out while maintaining a hydrogen pressure of 1.0 MPa. After reaching a predetermined cumulative hydrogen flow rate, the reaction solution was returned to room temperature and pressure and extracted from the reaction vessel to obtain a polymerization solution. After neutralization, solid rubber was recovered by steam stripping. The obtained solid rubber was dehydrated by a roll and dried in a dryer to obtain hydrogenated SBR-3. The hydrogenation rate was 70% and the butylene content was 17.5%.

[0042] Polymerization method for hydrogenated SBR-4 In a nitrogen-purged 10L autoclave reactor, 4200g of cyclohexane, styrene (180g, 1.73mol), butadiene (420g, 7.79mol), tetrahydrofuran (0.433g, 6.0mmol) and 2,2-di(2-tetrahydrofuryl)propane (0.022g, 0.12mmol) were charged and stirring was started. After the temperature of the contents in the reaction vessel was raised to 50°C, a hexane solution of n-butyllithium (3.57ml at a concentration of 1.55mol / L, 5.54mmol of n-butyllithium) was added. After the polymerization conversion rate reached almost 100%, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane (0.254g, 0.82mmol) was added and reacted for 30 minutes. After the reaction, methanol (92.9 mg, 2.9 mmol) was added to stop the reaction, and a portion was extracted and dried for analysis. The styrene content was 30% by mass, the vinyl content was 20% by mass in butadiene, and the weight average molecular weight was 330,000. The reaction solution was heated to 80°C or higher and hydrogen was introduced into the system. Next, 0.70 g of a catalyst mainly composed of titanocene dichloride, 1.2 g of diethylaluminum chloride, and 0.30 g of n-butyllithium were added, and the reaction was carried out while maintaining a hydrogen pressure of 1.0 MPa. After reaching a predetermined cumulative hydrogen flow rate, the reaction solution was returned to room temperature and pressure and extracted from the reaction vessel to obtain a polymerization solution. After neutralization, solid rubber was recovered by steam stripping. The obtained solid rubber was dehydrated by a roll and dried in a dryer to obtain hydrogenated SBR-4. The hydrogenation rate was 71% and the butylene content was 14%.

[0043] Polymerization method for hydrogenated SBR-5 In a nitrogen-purged 10L autoclave reactor, 4200g of cyclohexane, styrene (180g, 1.73mol), butadiene (420g, 7.79mol), tetrahydrofuran (0.433g, 6.0mmol) and 2,2-di(2-tetrahydrofuryl)propane (0.037g, 0.20mmol) were charged and stirring was started. After the temperature of the contents in the reaction vessel was raised to 50°C, a hexane solution of n-butyllithium (3.57ml at a concentration of 1.55mol / L, 5.54mmol of n-butyllithium) was added. After the polymerization conversion rate reached almost 100%, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1-aza-2-silacyclopentane (0.254g, 0.82mmol) was added and reacted for 30 minutes. After the reaction, methanol (92.9 mg, 2.9 mmol) was added to stop the reaction, and a portion was extracted and dried for analysis. The styrene content was 30% by mass, the vinyl content was 25% by mass in butadiene, and the weight average molecular weight was 340,000. The reaction solution was heated to 80°C or higher and hydrogen was introduced into the system. Next, 0.70 g of a catalyst mainly composed of titanocene dichloride, 1.2 g of diethylaluminum chloride, and 0.30 g of n-butyllithium were added, and the reaction was carried out while maintaining a hydrogen pressure of 1.0 MPa. After reaching a predetermined cumulative hydrogen flow rate, the reaction solution was returned to room temperature and pressure and extracted from the reaction vessel to obtain a polymerization solution. After neutralization, solid rubber was recovered by steam stripping. The obtained solid rubber was dehydrated by a roll and dried in a dryer to obtain hydrogenated SBR-5. The hydrogenation rate was 90% and the butylene content was 17.5%.

[0044] In preparing the rubber compositions for bead fillers (Examples 1-8, Comparative Examples 1-5) having the common compounding formulation shown in Table 4 and the formulations shown in Tables 2 and 3, the components except for sulfur, vulcanization accelerator, and curing agent were weighed and kneaded for 5 minutes in a 1.7-liter closed Banbury mixer, and the master batch was discharged outside the mixer and cooled at room temperature. This master batch was fed to the Banbury mixer, and sulfur, vulcanization accelerator, and curing agent were added and mixed to obtain a rubber composition for bead fillers. The compounding formulations in Table 4 are listed in parts by mass relative to 100 parts by mass of the diene rubber listed in Tables 2 and 3.

[0045] The Mooney viscosity of the rubber composition for bead filler obtained above was measured by the following method. The rubber composition for bead filler was vulcanized at 170°C for 15 minutes in a mold of a predetermined shape to prepare an evaluation sample. The obtained evaluation sample was used to measure the rubber hardness at 23°C, tensile elongation at break, and dynamic viscoelasticity (loss tangent tanδ) by the following methods.

[0046] Mooney Viscosity (Processability) Mooney viscosity (ML) of rubber composition for bead filler 1+4 ) was measured in accordance with JIS K6300-1:2001 using a Mooney viscometer with an L-type rotor (diameter 38.1 mm, thickness 5.5 mm) under conditions of a preheating time of 1 minute, a rotor rotation time of 4 minutes, 100°C, and 2 rpm. The results are shown in the "Processability" column in Table 2 as an index with the value of Comparative Example 1 set to 100, and in Table 3 as an index with the value of Comparative Example 2 set to 100. The smaller the index, the lower the Mooney viscosity and the better the processability.

[0047] Rubber hardness at 23℃ (lightweight tires) Using the obtained evaluation sample of the rubber composition for bead filler, rubber hardness was measured at a temperature of 23°C with a type A durometer in accordance with JIS K6253. The obtained results are shown in the "rubber hardness" column as an index with the value of Comparative Example 1 set to 100 in Table 2, and as an index with the value of Comparative Example 2 set to 100 in Table 3. A higher index means that the tire can be made lighter.

[0048] Tensile elongation at break Using the obtained evaluation sample of the rubber composition for bead filler, a JIS No. 3 dumbbell-shaped test piece was cut out in accordance with JIS K6251. The tensile elongation at break was measured in accordance with JIS K6251, and the obtained results are shown in Table 1 as an index with the value of Comparative Example 1 being 100 in Table 2, and the value of Comparative Example 2 being 100 in Table 3. A higher index indicates better tire durability.

[0049] Dynamic viscoelasticity (loss tangent tanδ) The dynamic viscoelasticity of the evaluation sample of the obtained rubber composition for bead filler was measured using a viscoelasticity spectrometer manufactured by Iwamoto Seisakusho Co., Ltd. under conditions of an elongation deformation strain rate of 10±2%, a vibration frequency of 20 Hz, and a temperature of 60°C, and tan δ(60°C) was calculated. The obtained tan δ(60°C) values ​​are shown in the column "tan δ(60°C)" in Table 2 as an index with the value of Comparative Example 1 set to 100, and in Table 3 as an index with the value of Comparative Example 2 set to 100. The smaller this index, the smaller the heat buildup and the lower the rolling resistance.

[0050] [Table 2]

[0051] [Table 3]

[0052] The types of raw materials used in Tables 2 and 3 are shown below. NR: Natural rubber, TSR20 SBR: Styrene butadiene rubber, Zeon Nipol 1502 Hydrogenated SBR-1 to Hydrogenated SBR-5: Hydrogenated aromatic vinyl-conjugated diene copolymers listed in Table 1 CB-1: Carbon black, Seast KH manufactured by Tokai Carbon Co., Ltd., with a nitrogen adsorption specific surface area of ​​93 m 2 / g CB-2: Carbon black, Seast F manufactured by Tokai Carbon Co., Ltd., with a nitrogen adsorption specific surface area of ​​41m 2 / g Phenolic resin: Novolac type cashew modified phenolic resin, Sumiresin PR-NR-1 manufactured by Sumitomo Bakelite Co., Ltd. Cardanol oligomer: CD-5L manufactured by Tohoku Kako Co., Ltd. Hexamethylenetetramine: Noccela H manufactured by Ouchi Shinko Chemical Industry Co., Ltd. HMMM: Hexamethoxymethylmelamine, CYREZ 964RPC manufactured by CYTEC INDUSTRIES

[0053] [Table 4]

[0054] The types of raw materials used in Table 4 are shown below. Zinc oxide: Three types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd. Stearic acid: Stearic acid beads manufactured by NOF CORPORATION Anti-aging agent: LANXESS VULKANOX 4020 Sulfur: Tsurumi Chemical Industry Co., Ltd. Kinkaji oil-filled fine sulfur Vulcanization accelerator: Noccela CZ-G manufactured by Ouchi Shinko Chemical Co., Ltd.

[0055] As is clear from Tables 2 and 3, the rubber compositions for bead fillers of Examples 1 to 8 were confirmed to have low Mooney viscosity and excellent processability, as well as excellent rubber hardness at 23° C., tensile elongation at break, and low heat buildup (tan δ at 60° C.). Regarding the Mooney viscosity of Examples 4 and 5, a rubber composition containing hydrogenated SBR usually has an increased Mooney viscosity as in Comparative Example 3, whereas in Examples 4 and 5, the increase in Mooney viscosity is suppressed, and the rubber hardness at 23° C., tensile elongation at break, and low heat buildup (tan δ at 60° C.) are improved without excessively impairing processability.

[0056] As is clear from Table 2, the rubber composition for bead filler in Comparative Example 1 does not contain hydrogenated SBR, and therefore is inferior to Example 1 in processability (high Mooney viscosity), rubber hardness, tensile elongation at break, and low heat build-up property (tan δ at 60°C). As is clear from Table 3, in the rubber composition for bead filler of Comparative Example 3, the hydrogenation rate of the hydrogenated SBR-5 exceeds 80%, so that the Mooney viscosity increases, the tensile elongation at break decreases, and the low heat build-up property (tan δ at 60°C) cannot be improved. In the rubber composition for bead fillers of Comparative Example 4, the hydrogenated SBR-1 is less than 20 parts by mass, so the effect of improving tan δ(60° C.) is not sufficient, and the balance with rubber hardness cannot be improved. The rubber composition for bead fillers in Comparative Example 5 contains less than 30 parts by mass of natural rubber and more than 70 parts by mass of hydrogenated SBR-1, so that the Mooney viscosity increases and processability deteriorates.

[0057] The present invention includes the following inventions. Invention [1] A rubber composition for bead fillers, comprising a diene rubber consisting of 30% by mass or more of an isoprene-based rubber and 20 to 70% by mass of a hydrogenated aromatic vinyl-conjugated diene copolymer, the hydrogenation rate of the hydrogenated aromatic vinyl-conjugated diene copolymer being 60 to 80%. Invention [2] The rubber composition for bead filler according to invention [1] further comprises a novolac phenolic resin, and hexamethylenetetramine and / or a melamine derivative, wherein 5 to 50 parts by mass of the novolac phenolic resin are blended per 100 parts by mass of the diene rubber, and the hexamethylenetetramine and / or melamine derivative is blended in an amount of 5 to 20% by mass relative to the blending amount of the novolac phenolic resin. Invention [3] The rubber composition for bead fillers according to invention [1] or [2], characterized in that the hydrogenated aromatic vinyl-conjugated diene copolymer is a hydrogenated styrene butadiene rubber having a butylene content of 15% or more. Invention [4] A tire comprising a bead filler made of the rubber composition for bead fillers according to any one of Inventions [1] to [3].

Claims

1. A rubber composition for bead fillers comprising a diene rubber comprising 30% by mass or more of an isoprene rubber and 20 to 70% by mass of a hydrogenated aromatic vinyl-conjugated diene copolymer, the hydrogenation rate of the hydrogenated aromatic vinyl-conjugated diene copolymer being 60 to 80%.

2. The rubber composition for bead fillers according to claim 1, further comprising a novolac phenolic resin, and hexamethylenetetramine and / or a melamine derivative, wherein 5 to 50 parts by mass of the novolac phenolic resin is blended with respect to 100 parts by mass of the diene rubber, and 5 to 20% by mass of the hexamethylenetetramine and / or melamine derivative is blended with respect to the blending amount of the novolac phenolic resin.

3. 3. The rubber composition for bead fillers according to claim 1, wherein the hydrogenated aromatic vinyl-conjugated diene copolymer is a hydrogenated styrene-butadiene rubber having a butylene content of 15% or more.

4. A tire comprising a bead filler made of the rubber composition for bead fillers according to claim 1 or 2.

Citation Information

Patent Citations

  • Rubber composition for tire bead filler and pneumatic tire using the same

    JP2014118507A

  • Pneumatic tire

    JP2021035801A

  • Pneumatic tire

    JP2021066371A