Thermoplastic resin powder granule

Thermoplastic resin powder granules with a structured outer wall and compressed inner core address the low bulk density and handling issues, enhancing machine feed stability and reducing energy consumption and carbon dioxide emissions.

JP2024165088AActive Publication Date: 2024-11-28NAGASE & CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023080938
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28
Estimated Expiration
2043-05-16

AI Technical Summary

Technical Problem

Thermoplastic resin powders have low bulk density and poor handling properties, leading to insufficient supply to melt-kneading machines and high energy consumption, which increases carbon dioxide emissions.

Method used

The development of thermoplastic resin powder granules with a structured outer wall and compressed inner core, formed through compression granulation without melt-kneading, to enhance bulk density and stability.

Benefits of technology

The granulated resin powder improves feed characteristics to processing machines, reduces energy consumption, and decreases carbon dioxide emissions by eliminating the need for melt-kneading and pelletizing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165088000001_ABST
    Figure 2024165088000001_ABST
Patent Text Reader

Abstract

To provide a granule of thermoplastic resin powder that eliminates the need for a melt-kneading pelletization step for thermoplastic resin powder, while achieving a stable form, high bulk density, better working environment, and excellent feed properties (stability and flowability) for processing equipment, and additionally, reduces power usage required for production, resulting in reduced CO2 emissions.SOLUTION: A powder granule contains thermoplastic resin powder, incorporating an outer wall formed by the melting of at least a part of the thermoplastic resin powder located at the outer edge of the powder granule, wherein the compressed thermoplastic resin powder is contained inside the outer wall.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a granulated product of thermoplastic resin powder. [Background technology]

[0002] Thermoplastic resins may be in a powder form due to their manufacturing process or because they are recycled pulverized products. Such thermoplastic resin powders are usually difficult to handle, so in order to improve the handleability and further increase productivity, they are generally plasticized and melted in a melt extruder, extruded through a die, cooled and solidified, and made into a pellet-like form (hereinafter also referred to as melt-kneaded pellets), which are then supplied to various thermoplastic resin processing machines and commercialized. That is, for powdered thermoplastic resins, melt-kneaded pelletization is usually performed. Summary of the Invention [Problem to be solved by the invention]

[0003] In the process of melt-kneading and pelletizing thermoplastic resin powder, problems such as poor supply to various melt-kneading machines including extruders and low productivity often occur because the powdered thermoplastic resin has a low bulk density.

[0004] Recently, there has been a goal to reduce carbon dioxide, one of the greenhouse gases, and in various processing steps of thermoplastic resins, it has become a major challenge to reduce the amount of energy used in the process and the amount of carbon dioxide generated during the process.

[0005] An object of the present invention is to provide a granulated product of thermoplastic resin powder which has a stable shape and a high bulk density without going through a melt-kneading pelletizing process, improves the working environment, and has excellent feed characteristics (stability, flowability) to a processing machine, and which can contribute to reducing the amount of electricity required for production, i.e., reducing the amount of carbon dioxide generated, compared to melt-kneading pelletizing. [Means for solving the problem]

[0006] (1) A powder granulation product containing a thermoplastic resin powder, the powder granulation product having an outer wall portion formed by melting at least a portion of the thermoplastic resin powder located at the outer edge of the powder granulation product, and compressed thermoplastic resin powder contained inside the outer wall portion. (2) The powder granule according to (1), wherein at least a portion of the compressed thermoplastic resin powder inside the outer wall portion comprises an unmelted compressed powder form. (3) The powder granule according to (1) or (2), wherein at least a part of the compressed thermoplastic resin powder inside the outer wall portion is partially melted. (4) The powder granules according to any one of (1) to (3), wherein the powder granules have a substantially cylindrical or substantially prismatic shape. (5) The powder granule according to any one of (1) to (4), which has an outer wall portion on a side surface of the powder granule. (6) The powder granule according to any one of (1) to (5), having a breaking strength of 2.0 kg or more. (7) The powder granulation product according to any one of (1) to (6), which is a compression granulation product. (8) The powder granule according to any one of (1) to (7), wherein the thermoplastic resin powder contains a thermoplastic resin having a softening onset temperature of 50 to 150°C. (9) The powder granule according to any one of (1) to (8), wherein the thermoplastic resin powder contains a thermoplastic resin having a softening onset temperature of 60 to 90°C. (10) The powder granule according to any one of (1) to (9), wherein the thermoplastic resin powder comprises at least one selected from the group consisting of acrylic resins, methacrylic resins, polyhydroxyalkanoate (PHA) resins, polyolefin resins, polyamide resins, polyacetal resins, polyphenylene ether (PPE) resins, polyphenylene sulfide (PPS) resins, polyether ether ketone (PEEK) resins, polyimide (PI) resins, polyamideimide (PAI) resins, polyester resins, polycarbonate (PC) resins, polystyrene resins, polyketone resins, liquid crystal polymers (LCPs), and core-shell polymers. (11) The powder granule according to any one of (1) to (10), wherein the thermoplastic resin powder contains a PHA-based resin. (12) A method for producing the powder granulated product according to any one of (1) to (11), comprising the steps of: The method includes a compression granulation step of granulating a thermoplastic resin powder by a compression granulation method in which the thermoplastic resin powder is extruded through a die hole, The compression granulation step is carried out under conditions where the granule temperature Tp (°C) immediately after granulation and the softening start temperature Ts (°C) of the thermoplastic resin powder satisfy formula (1), Equation (1): Ts-30≦Tp≦Ts+10. (13) The method according to (12), wherein the die temperature is controlled so that the granule temperature Tp (°C) immediately after granulation and the softening starting temperature Ts (°C) of the thermoplastic resin powder satisfy the condition of formula (1). (14) The method according to (12) or (13), in which the outer wall portion is formed by melting at least a portion of the thermoplastic resin powder at the contact surface with the wall surface of the die hole by frictional heat with the wall surface or heat transfer from the wall surface. (15) The method according to any one of (12) to (14), wherein the compression granulation is carried out using a disk pelletizer type compression granulator. (16) Use of the powder granule according to any one of (1) to (11) as a raw material for a thermoplastic resin compound or a molding material. Effect of the Invention

[0007] The present invention can provide a granulated product of thermoplastic resin powder which has a stable shape and a high bulk density without having to undergo a melt-kneading pelletizing process, improves the working environment, and has excellent feed characteristics (stability, fluidity) to a processing machine. In addition, compared to melt-kneading pelletizing, the granulated product can contribute to reducing the amount of electricity required for production, i.e., reducing the amount of carbon dioxide generated. [Brief description of the drawings]

[0008] [Figure 1] 1 is a photograph showing the appearance of the powder granulated product obtained in Example 1 (acrylic resin powder A1 was used). [Diagram 2] 1 is a cross-sectional photograph of the powder granulated product obtained in Example 1 (acrylic resin powder A1 was used). [Diagram 3] 1 shows the results of DSC measurement of biopolyester powder A2 of Example 4. [Figure 4] 1 is a photograph showing the appearance of the powder granulated product obtained in Example 4 (using biopolyester powder A2). [Diagram 5] 1 is a cross-sectional photograph of the powder granule obtained in Example 4 (using biopolyester powder A2). [Figure 6] 5 is a photograph of an injection-molded article obtained from the powder granulation product obtained in Example 1 (acrylic resin powder A1 was used) in Example 5. [Figure 7] 6 is a photograph of a sheet molded product obtained from the powder granulation product obtained in Example 4 (using biopolyester powder A2). [Figure 8] 1 is a cross-sectional photograph of the powder granule obtained in Example 7 (using biopolyester powder A3). [Figure 9] 1 is a cross-sectional photograph of the powder granule obtained in Example 8 (using biopolyester powder A3). [Figure 10] 1 is a cross-sectional photograph of the powder granule obtained in Example 9 (using biopolyester powder A4). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] A. Overview of thermoplastic resin powder granulation The powder granulation product of the present invention is a powder granulation product containing a thermoplastic resin powder, and has an outer wall portion formed by melting at least a part of the thermoplastic resin powder located at the outer edge of the powder granulation product, and the compressed thermoplastic resin powder is contained inside the outer wall portion. In the powder granulation product of the present invention, the outer wall portion is located at the outer edge of the granulation product. In this specification, the outer wall portion is also referred to as a shell portion. The compressed thermoplastic resin powder is contained inside the outer wall portion, and the thermoplastic resin powder may be at least partially melted or at least partially unmelted. The compressed thermoplastic resin powder inside the outer wall portion may be in an unmelted state. That is, at least a part of the compressed thermoplastic resin powder inside the outer wall portion may include a compressed powder form that is not melted, or may include a partially melted form. The partially melted form refers to a form in which the components of the thermoplastic resin powder are partially melted, but the thermoplastic resin powder is not firmly welded to hold the thermoplastic resin powder like the outer wall portion. In this specification, the inside of the outer wall portion is also referred to as the core portion. The compressed thermoplastic resin powder is contained in the core portion inside the outer wall portion, and in this specification, "compressed" refers to the density of the thermoplastic resin powder located in the core portion being higher than the bulk density of the thermoplastic resin powder before granulation.

[0010] The outer wall (shell) of the granulated product of the thermoplastic resin powder of the present invention has a dense structure containing the molten thermoplastic resin powder, while the core inside has a sparse structure compared to the dense structure (welded structure) of the outer wall containing the molten thermoplastic resin powder, although it is compressed. The thermoplastic resin powder of the present invention has an outer wall made of the molten thermoplastic resin powder, which holds the compressed thermoplastic resin powder present in the core, so that, although it is a powder granulated product, it has a stable structure, little powder falling, excellent handling and safety, and can bring about an improvement in the working environment.

[0011] Therefore, when the powder granules of the present invention are used as a compound raw material in preparing a resin composition, the raw material supply capacity, supply stability, and supply accuracy can be improved, which can contribute to improving productivity. At the same time, since the melt-kneading pelletization process can be omitted, the amount of electric energy required for the process can be reduced, and the amount of carbon dioxide generated during the processing process can be reduced.

[0012] The powder granules of the present invention can be directly supplied to various molding machines such as injection molding machines and extrusion molding machines for thermoplastic resins, or can be used as molding materials. In this case, the melt-kneading pelletizing process can be omitted, so that the amount of carbon dioxide generated in the processing process can be reduced. In addition, the powder granules of the present invention can have a small thermal history because heat sufficient for pelletizing is not applied to the powder granules of the present invention.

[0013] The outer wall (shell) has a welded structure in which at least a part of the thermoplastic resin powder located at the outer edge of the powder granule is melted. The outer wall may be smooth enough to have a glossy surface appearance. The outer wall may be formed by melting a part of the components of the thermoplastic resin powder and partially welding it to the adjacent components, although it is not melted to the extent that it is smooth. As will be described in detail later, the outer wall can be formed by melting at least a part of the thermoplastic resin powder at the contact surface with the die hole, for example, by frictional heat with the wall surface or heat transfer from the wall surface during compression granulation. The thickness of the outer wall can be various depending on the manufacturing conditions of the granules of the thermoplastic resin powder.

[0014] The core portion is a portion located inside the outer wall portion, and is a portion in which the compressed thermoplastic resin powder is contained. The thermoplastic resin powder located in the core portion may be porous, or may have a non-welded structure in which heat is not transferred to the core portion during granulation. Since the core portion is far from the die contact surface, it may have a structure in which the powdered polymer raw material maintains its powder shape (i.e., a non-welded structure or a powder-like structure), or a structure in which the powdered polymer raw material is partially welded but retains its shape.

[0015] In addition, in this specification, the terms "outer wall portion (shell portion)" and "core portion" are used for ease of explanation, but as described above, the outer wall portion is formed by melting the thermoplastic resin powder due to the heat during granulation, so in reality, there is no clear boundary between the outer wall portion (shell portion) and the core portion. The outer wall portion (shell portion) includes a fused structure of the thermoplastic resin powder and refers to a portion that is located on the outer edge of the powder granulation product and contributes to maintaining a certain shape of the powder granulation product, while the core portion refers to a portion located inside the outer wall portion (shell portion).

[0016] The shape of the powder granulation product is preferably substantially cylindrical or substantially prismatic, and the powder granulation product preferably has an outer wall portion on the side surface of the powder granulation product. In the present invention, the powder granulation product preferably has a substantially cylindrical or substantially prismatic shape, and an outer wall portion is preferably formed on the side surface of the powder granulation product having a substantially cylindrical or substantially prismatic shape.

[0017] The powder granulated product of the present invention can be preferably obtained by using a powder compression granulation method, and the details of the production method will be described later.

[0018] The powder granules of the present invention can be used as a raw material for thermoplastic resin in the production of a resin composition by melt compounding. Furthermore, the powder granules can be directly charged into various resin molding machines such as injection molding and extrusion molding to obtain various molded products.

[0019] In the melt compounding of a resin composition, the addition of a powder granulation material can improve productivity. Specifically, since the powder granulation material has a remarkably excellent feeding stability into an apparatus such as an extruder, the use of the powder granulation material can dramatically improve the productivity of the resin composition (compound processing speed per hour). In addition, it can significantly improve the pollution of the working environment due to dust, improve the occupational safety and health environment of the workers, and further, it can significantly reduce the time required for cleaning the equipment when changing over.

[0020] When the powder granulated material is directly fed into various resin molding machines such as injection molding and extrusion molding machines, the "melt-kneading pelletization" process can be omitted, making it possible to significantly reduce the total amount of carbon dioxide generated by the process compared to conventional methods (resin product processing methods that include a melt-kneading pelletizing process).

[0021] The powder granules may have any suitable shape. Typically, the powder is produced by compression granulation of the powder, and when the powder is granulated by passing it through a circular die hole, the basic shape is a cylindrical pellet shape.

[0022] In this specification, the term "die" is a general term for a tool equivalent to a "mold" for compressing and shaping a powder granulated material.

[0023] When the powder granulated product is cylindrical, the diameter of the powder granulated product is, for example, 2 mm to 7 mm, preferably 3 mm to 5 mm. The length (height) of the powder granulated product is, for example, 1 mm to 10 mm, preferably 2 mm to 7 mm. Such a shape makes the powder granulated product easy to handle. The diameter of the powder granulated product can be adjusted, for example, by the diameter of the die hole of the disc plate (die plate) during granulation, and the length can be adjusted by the distance between the disc plate and the cutter. The distance can be any appropriate distance. The distance between the disc plate and the cutter is, for example, 1 mm to 30 mm, more preferably 2 mm to 20 mm, and even more preferably 3 mm to 10 mm.

[0024] The bulk density of the powder granulated product may be any suitable bulk density. The bulk density of the powder granulated product is preferably 0.3 kg / L to 2.0 kg / L, more preferably 0.5 kg / L to 1.0 kg / L. Increasing the bulk density increases the supply speed and supply stability of the powder granulated product to various processing machines. The bulk density is calculated by using a measuring cup, allowing the powder to fall naturally into the measuring cup until it is filled to the brim, weighing out a volume of exactly 1 liter, and measuring the mass (unit: kg / L).

[0025] The breaking strength of the powder granulation product in a Kiya hardness tester is preferably 0.5 kg or more, preferably 1.0 kg or more, preferably 2.0 kg or more, preferably 3.0 kg or more, preferably 4.0 kg or more, preferably 5.0 kg or more, preferably 6.0 kg or more, preferably 7.0 kg or more, preferably 8.0 kg or more, preferably 9.0 kg or more, and preferably 10 kg or more. The upper limit may exceed the measurement limit of the Kiya hardness tester (the measurement limit of Shiro Sangyo's product name "WPF1600-B" is 10 kg). Within this range, a powder granulation product having excellent handling properties and melt processability can be obtained. Here, the breaking strength refers to the average breaking stress (breaking load) measured by crushing 20 or more (preferably 25 or more) of the powder granulation product in a direction perpendicular to the longitudinal direction (extrusion direction) of the powder granulation product. In the case of powder granulation, since the shell is made of molten resin, it is possible to maintain a stable shape as a granulation, even though it is a powder granulation. The diameter of the pressing surface of the pressing attachment of the Kiya hardness tester is, for example, 5 mm.

[0026] The moisture content of the powder granulation product may be any appropriate moisture content. The moisture content of the powder granulation product may be the moisture content originally contained in the raw material powder, or water may be added to the powder to facilitate granulation. The amount of water to be added during granulation will be described later.

[0027] The powder granulated product may be dried after granulation, but the final moisture content is preferably 10% by mass or less, more preferably 5.0% by mass or less, even more preferably 3.0% by mass or less, particularly preferably 1.0% by mass or less, and most preferably 0.5% by mass or less. The final moisture content of the powder granulated product may be appropriately selected depending on the purpose of use.

[0028] It is preferable that the powder granulation material is granulated without adding water. If the moisture content of the powder granulation material is low, a drying process after granulation may not be necessary. If granulation can be performed without using water, the drying process will not be necessary, and the amount of carbon dioxide emitted during the powder granulation process can be significantly reduced.

[0029] The moisture content of the powder granulated product granulated "without adding water" is, for example, 1.0 mass% or less, preferably 0.5 mass% or less, more preferably 0.3 mass% or less, and even more preferably 0.2 mass% or less.

[0030] The moisture content of the powder granulated product is measured using an infrared moisture meter as described below.

[0031] The particle size of the thermoplastic resin powder used in the present invention may be any appropriate particle size depending on the form, as long as the effects of the present invention are obtained. The maximum diameter of the resin powder particles is preferably 5 mm or less, and the minimum diameter is preferably 0.0001 mm or more.

[0032] The average particle diameter of the thermoplastic resin powder is, for example, 0.001 mm to 1.0 mm. The average particle diameter of the thermoplastic resin powder is preferably 1.0 mm or less, more preferably 0.01 mm to 0.8 mm, and particularly preferably 0.1 mm to 0.5 mm. In this specification, the average particle diameter can be measured by a laser diffraction method. The average particle diameter of the resin powder can be a particle diameter (d50) at a cumulative 50% in a cumulative particle size distribution on a volume basis.

[0033] The thermoplastic resin powder may be used alone or in combination of two or more kinds.

[0034] The bulk density of the thermoplastic resin powder may be any appropriate bulk density depending on the form of the powder, as long as the effects of the present invention are obtained. The bulk density of the thermoplastic resin powder is preferably 0.01 kg / L to 1 kg / L, more preferably 0.05 kg / L to 0.8 kg / L, more preferably 0.1 kg / L to 0.8 kg / L, even more preferably 0.1 kg / L to 0.6 kg / L, and particularly preferably 0.2 kg / L to 0.5 kg / L.

[0035] The thermoplastic resin powder may be a powdered resin obtained through the manufacturing process, i.e., may be a powder due to the manufacturing process, or may be a powdered resin obtained by pulverizing a non-powdered resin such as a pelletized resin, a lump resin, or a resin molding. The pulverized powdered resin can be obtained by cooling a molded product, pellet, sprue, runner, etc. generated during injection molding at room temperature or, if necessary, using dry ice or liquid nitrogen, and then using a pulverizer (e.g., Dalton Co., Ltd., product names "Nea Mill, Sylphid Mill, Atomizer, Impact Mill, etc.").

[0036] The thermoplastic resin powder is composed of any suitable thermoplastic resin. Specific examples of the thermoplastic resin include high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), polypropylene (PP), polyvinyl chloride (PVC), polyvinylidene chloride, polystyrene (PS), polyvinyl acetate (PVAc), polyurethane (PUR), fluorine-based resin, general-purpose resins such as ABS resin (acrylonitrile butadiene styrene resin), AS resin, and acrylic resin (PMMA), polyamide (PA), polyacetal (POM), polycarbonate (PC), polyphenylene ether, and modified polyphenylene ether ( Examples of such plastics include engineering plastics such as m-PPE, modified PPE, PPO), polyesters (PET, PBT, etc.), and cyclic polyolefin (COP); super engineering plastics such as polyphenylene sulfide (PPS), polytetrafluoroethylene (PTFE), polysulfone (PSF), polyethersulfone (PES), amorphous polyarylate (PAR), liquid crystal polymer (LCP), polyether ether ketone (PEEK), polyimide (PI), and polyamide imide (PAI); and core-shell rubbers obtained by emulsion polymerization or suspension polymerization.

[0037] The thermoplastic resin may be a biodegradable resin, such as aliphatic polyester resins (e.g., homopolymers or copolymers of polyhydroxyalkanoate (PHA), polycaprolactone, polylactic acid, polyethylene succinate, polybutylene succinate-adipate, polyhydroxyvalerate, etc., or modified products of these homopolymers or copolymers), aliphatic / aromatic polyester resins (e.g., block polymers or random polymers of aliphatic carboxylic acids or hydroxy acids, aromatic dicarboxylic acids and 1,3-propanediol, etc.), and polyvinyl alcohol resins (e.g., polyvinyl alcohol, polyvinyl acetate, polyvinyl butyrate, ethylene-vinyl alcohol copolymers, etc.).

[0038] In the present invention, the particularly preferred thermoplastic resin powder is at least one selected from the group consisting of acrylic resins, methacrylic resins, polyhydroxyalkanoate (PHA) resins, polyolefin resins, polyamide resins, polyacetal resins, polyphenylene ether (PPE) resins, polyphenylene sulfide (PPS) resins, polyether ether ketone (PEEK) resins, polyimide (PI) resins, polyamideimide (PAI) resins, polyester resins, polycarbonate (PC) resins, polystyrene resins, polyketone resins, liquid crystal polymers (LCPs), and core-shell polymers.

[0039] Polyhydroxyalkanoate (PHA) resins can be compounds produced in the body of microorganisms that feed on carbohydrates, oils, fats, etc. Such polyhydroxyalkanoates are primarily extracted as powdered polymers.

[0040] The polyhydroxyalkanoate resin contains hydroxyalkanoic acid, which is a raw material component, as a polymerization component and has at least a repeating unit derived from hydroxyalkanoic acid. The polyhydroxyalkanoate resin may be artificially synthesized or biosynthesized by a microorganism. Examples of hydroxyalkanoic acid include glycolic acid, 3-hydroxybutyrate, 3-hydroxypropionate, 3-hydroxyvalerate, 3-hydroxyhexanoate, 3-hydroxyheptanoate, 3-hydroxyoctanoate, 3-hydroxynanoate, 3-hydroxydecanoate, 3-hydroxytetradecanoate, 3-hydroxyhexadecanoate, 3-hydroxyoctadecanoate, 4-hydroxybutyrate, 4-hydroxyvalerate, 5-hydroxyvalerate, 6-hydroxyhexanoate, etc. The number of carbon atoms of the hydroxyalkanoic acid may be 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, or 8 or more, and is preferably 3 or more. The number of carbon atoms of the hydroxyalkanoic acid may be 15 or less, 12 or less, 10 or less, 8 or less, 6 or less, or 4 or less, preferably 10 or less, particularly preferably 6 or less. The hydroxyalkanoic acid may be used alone or in combination of two or more kinds.

[0041] Preferred examples of the polyhydroxyalkanoate resin include poly(3-hydroxyalkanoate) and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).

[0042] The acrylic resin, methacrylic resin, and core-shell type polymer are preferably used in the form of a powder obtained by emulsion polymerization or suspension polymerization. The powdered polymer obtained by emulsion polymerization or suspension polymerization can be used as it is as a thermoplastic resin powder for granulation.

[0043] In the powder granulation product of the present invention, in order to form an outer wall (shell) on the granulation product, it is necessary to melt a part of the components of the thermoplastic resin powder by heat of friction with the powder on the die wall surface or by heat transfer in the granulation process. For this reason, when the softening start temperature of the thermoplastic resin powder is higher than the granulation temperature, it is advantageous to obtain the granulation product by granulating the mixture with other thermoplastic resin powders having a softening start temperature lower than the granulation temperature.

[0044] The powder granules may contain any suitable additives as necessary. The additives may be in powder form or liquid form. Examples of additives include antioxidants, light stabilizers, foaming agents, ultraviolet absorbers, antiblocking agents, heat stabilizers, impact modifiers, antibacterial agents, dispersants, compatibilizers, processing aids, lubricants, coupling agents, crystallization nucleating agents, hydrolysis inhibitors, oxygen scavengers, colorants (dyes and pigments), and binders. The additives may be used alone or in combination of two or more.

[0045] The additive may be in the form of a powder or a liquid.

[0046] The content of the additive in the powder granule is, for example, 10% by mass or less, preferably 5.0% by mass or less, preferably 3.0% by mass or less, and more preferably 1.0% by mass or less.

[0047] The powder granules of this embodiment may contain a binder as an additive. Here, the term "binder" refers to a compound that exists between thermoplastic resin powders other than the components of the raw thermoplastic resin powder, binds the powders together, and exerts an effect of increasing the breaking strength of the granules. However, various compounds that exert a binding effect, preferably water-dispersed or water-soluble polymer compounds, polysaccharides, etc., can be appropriately selected and used as the binder as needed.

[0048] It is preferable to melt and bind a part of the components of the thermoplastic resin powder to form a powder granule, and it is preferable not to mix a binder.

[0049] When a binder is blended in the powder granulation product of this embodiment, the content thereof is typically 10 mass% or less, preferably 5.0 mass% or less, more preferably 3.0 mass% or less, even more preferably 1.0 mass% or less, still more preferably 0.5 mass% or less, particularly preferably 0.1 mass% or less, and most preferably 0 mass% (undetectable), relative to the total mass of the powder granulation product.

[0050] In one embodiment, a dispersant is preferably used as the additive. A surfactant is preferably used as the dispersant. The hydrophilic / hydrophobic balance in the dispersant (surfactant) can be controlled by adjusting the degree of esterification of the compound to be the dispersant, the type of fatty acid (presence or absence of hydroxyl group, saturated or unsaturated fatty acid, alkyl chain length), the degree of polymerization, etc. The use of a dispersant can bring about benefits such as "improving the productivity (discharge speed) of powder granulation," "reducing frictional heat during granulation," and "enhancing the cleaning ability of the granulation device."

[0051] Examples of dispersants include fatty acids, fatty acid metal salts, fatty acid sulfonates, fatty acid amides, acrylamides, polyhydric alcohol fatty acid esters, polyglycerin fatty acid esters, etc. The dispersants may be used alone or in combination of two or more.

[0052] In one embodiment, the dispersant is at least one selected from the group consisting of polyhydric alcohol fatty acid esters, fatty acid amides, polyglycerin fatty acid esters, condensed hydroxy fatty acids, and alcohol esters of condensed hydroxy fatty acids.

[0053] The polyhydric alcohol fatty acid ester is an ester compound composed of a polyhydric alcohol and a fatty acid. For example, esters of polyhydric alcohols such as pentaerythritol and glycerin and fatty acids having 8 or more carbon atoms (preferably 8 to 24 carbon atoms, more preferably 10 to 22 carbon atoms) are used as the polyhydric alcohol fatty acid ester.

[0054] Fatty acid amides are compounds that have a structure formed by dehydration condensation of fatty acid with ammonia or primary or secondary amine. Examples of fatty acid amides include saturated fatty acid monoamides such as lauric acid amide, palmitic acid amide, stearic acid amide, and behenic acid amide.

[0055] Polyglycerol fatty acid esters are ester compounds composed of polyglycerol and fatty acids. Examples of polyglycerol fatty acid esters include diglycerol palmitate, diglycerol stearate, diglycerol oleate, decaglycerol palmitate, decaglycerol stearate, and decaglycerol oleate.

[0056] The content of the dispersant is usually 0.01% by mass to 10% by mass, preferably 0.1% by mass to 7.0% by mass, and more preferably 0.3% by mass to 5.0% by mass, based on the total amount of the powder granulated product.

[0057] In one embodiment, a crystallization nucleating agent is used as an additive. The crystallization nucleating agent is preferably used when the powder granulation product is a granulation product mainly composed of a crystalline thermoplastic resin powder. In particular, the crystallization nucleating agent is preferably added when a biopolyester (e.g., polyhydroxyalkanoates (PHAs)) produced by an organism is used as the thermoplastic resin powder. The use of the crystallization nucleating agent makes it possible to increase the crystallization rate and crystallization degree of the crystalline thermoplastic resin powder (e.g., biopolyester), thereby improving not only rigidity and heat resistance but also productivity. Examples of such crystallization nucleating agents include organic metal salt compounds such as metal phosphate, metal benzoate, metal pimelate, metal rosin, metal oxalate, and metal fatty acid salt, organic compounds such as aliphatic organic ester, triallyl phosphate, polyalkylene glycol or its derivative, aliphatic polyester, and benzylidene sorbitol, dyes and pigments such as quinacridone, cyanine blue, and carbon black, minerals such as talc, mica, kaolin, clay, carbonate minerals, metal oxides, and metal sulfates, and polymer compounds such as ionomers and high-melting polyamides. In one embodiment, talc, mica, kaolin, calcium carbonate, and the like are used as the crystallization nucleating agent. The crystallization nucleating agent may be used alone or in combination of two or more.

[0058] The content of the crystallization nucleating agent is usually 0.01% by mass to 10% by mass, preferably 0.1% by mass to 7.0% by mass, and more preferably 0.3% by mass to 5.0% by mass, based on the total amount of the powder granulated product.

[0059] B. Manufacturing method of powder granulation The powder granule having a core portion and a shell portion of the present invention can be obtained by compressing the powder granule through a "die" and melting the thermoplastic resin powder in the contact area with the die, but preferably can be obtained by a compression granulation method in which the thermoplastic resin powder is extruded from a die hole, and the shell portion is formed when the thermoplastic resin powder is extruded from the die hole, i.e., during extrusion granulation, the components of the thermoplastic resin powder melt at the contact surface with the wall of the die hole due to frictional heat with the wall surface or heat transfer from the wall surface.

[0060] By forming the shell portion, the powder granules can maintain a constant shape (e.g., cylindrical or rectangular), and a powder granule with excellent quality stability (shape stability, uniformity of hardness), low fineness, high hardness, and handleability can be obtained.

[0061] In one embodiment, the powder granulation can be performed without using water, making a drying process unnecessary. This reduces the amount of electricity used for granulation and greatly reduces the amount of carbon dioxide emitted during the process.

[0062] When the powder granulation is extruded, frictional heat may be generated between the wall of the die hole and the powder when the powder passes through the die. At this time, the temperature of the powder granulation increases due to frictional heat, but if the granulation temperature (Tp; unit ° C.) immediately after granulation is too high above the softening start temperature (Ts, Ts corresponds to the melting point or glass transition temperature) of the thermoplastic resin powder, the thermoplastic resin powder melts excessively and sticks to the wall of the die hole, or the die hole becomes clogged, making continuous granulation impossible. On the other hand, if the granulation temperature (Tp) immediately after granulation is too low below the softening start temperature Ts of the resin powder, the raw resin powder does not have a binding force and does not become a granule in the powder state, or the granulation becomes a granulation that easily collapses when compressed, making it difficult to obtain a granulation in a stable shape.

[0063] In order to stably obtain a powder granulated product, it is preferable that the granulated product temperature (Tp) immediately after granulation and the softening start temperature (Ts) of the thermoplastic resin powder are within a specific range. That is, the method for producing a powder granulated product according to the present invention includes a compression granulation step of granulating a thermoplastic resin powder by a compression granulation method in which the thermoplastic resin powder is extruded through a die hole, and the compression granulation step is performed under conditions in which the granulated product temperature Tp (°C) immediately after granulation and the softening start temperature Ts (°C) of the thermoplastic resin powder satisfy formula (1), more preferably formula (2), and even more preferably formula (3). Formula (1): Ts-30≦Tp≦Ts+10 Formula (2): Ts-20≦Tp≦Ts+5 Formula (3): Ts-15≦Tp≦Ts

[0064] In formulas (1) to (3), the left and right sides may be arbitrarily combined to create other formulas that define the preferred range of Tp. For example, the compression granulation step can be preferably carried out under conditions that satisfy Ts-20≦Tp≦Ts+10, Ts-15≦Tp≦Ts+10, Ts-30≦Tp≦Ts+5, Ts-15≦Tp≦Ts+5, Ts-30≦Tp≦Ts, and Ts-20≦Tp≦Ts.

[0065] The temperature of the granulated material (Tp) immediately after granulation can be measured by a contact thermocouple. The temperature of the granulated material (Tp) immediately after granulation can be measured by stopping the powder granulation device during granulation after the device is in a state where granulation can be performed stably, directly inserting a thermocouple into the die part or into the powder granulated material inside the die hole, and quickly measuring the temperature. Measurements are performed at least three times (preferably five times), and the average value is taken as Tp. At this time, even if the powder sticks to the die or becomes clogged, making granulation impossible, the thermocouple is similarly inserted directly into the powder to measure the temperature.

[0066] In order to efficiently obtain the powder granules having the core / shell structure of the present invention, it is most effective to control the temperature of the die that comes into direct contact with the powder. That is, it is preferable to control the temperature of the die so as to satisfy the temperature condition of formula (1) by providing a mechanism for heating the die by providing a heater or a heat medium passage for temperature control, and further a mechanism for cooling the die by providing a passage for a cooling medium.

[0067] In general compression granulation equipment, due to the simplicity of the equipment, it is often a simple structure that does not allow control of the die temperature. However, even in this case, the temperature of the granulated material immediately after granulation (Tp) can be changed and controlled by methods such as the rotation speed of the rollers of the granulation equipment, the hole diameter of the die hole, the effective pressurized length of the die hole, the supply speed of the raw material powder, the contact area and contact time between the raw material powder and the die surface, and insulation or cooling of the granulation equipment.

[0068] When there is no temperature control device for the die, the temperature is controlled by balancing the temperature rise due to frictional heat during granulation and heat dissipation to the outside. In order to efficiently obtain a powder granule by satisfying formula (1), the softening onset temperature (Ts) of the thermoplastic resin powder is preferably 50 to 150°C, more preferably 55 to 120°C, and even more preferably 60 to 90°C.

[0069] The thermoplastic resin powder may be a single component or a combination of two or more components. In particular, when the difference between the softening start temperature (Ts) of the target thermoplastic resin powder and the granulated product temperature (Tp) is large and it is difficult to set the granulated product temperature to satisfy any of the conditions of the above formulas (1) to (3), it is advantageous to obtain a granulated product by blending a thermoplastic resin having a softening start temperature lower than the granulated product temperature and granulating the mixture.

[0070] When the thermoplastic resin powder is composed of two or more components, it is preferable to set the condition (e.g., die temperature) such that the granule temperature (Tp) immediately after granulation falls within the range satisfying formula (1) by taking the Ts of the component of the thermoplastic resin powder with the lowest softening onset temperature (Ts) as Ts in formula (1). More preferably, it is preferable to set the condition (e.g., die temperature) such that the softening onset temperatures of all the components of the thermoplastic resin powder satisfy formula (1).

[0071] When the thermoplastic resin powder is composed of two or more components, the component having the lowest softening onset temperature is 50 mass % or less, preferably 30 mass % or less, and more preferably 10 mass % or less, of the total amount of the thermoplastic resin powder.

[0072] In this specification, the softening onset temperature (Ts) of the thermoplastic resin powder means the melting point or glass transition temperature, and can be measured by a differential scanning calorimeter (DSC). In one embodiment, in the DSC measurement, when an endothermic or exothermic peak is observed, the softening temperature corresponds to the melting point, and when a discontinuity in the baseline is observed, the softening temperature corresponds to the glass transition temperature.

[0073] In DSC measurements, a sample of thermoplastic resin powder, usually about 5 mg, is weighed onto a sample dish and heated at 10°C / min in a nitrogen stream to determine the softening onset temperature (Ts).

[0074] In the case of crystalline resins, the intersection of the baseline from the low temperature area and the tangent at the inflection point (the point where the upward convex curve changes to a downward convex curve) on the melting start side where the endothermic peak of crystalline melting is observed is considered to be the "melting point", and this is the softening onset temperature (Ts).

[0075] When a plurality of endothermic peaks of crystal melting appear, the melting point of the peak appearing on the lowest temperature side is regarded as the softening initiation temperature.

[0076] In the case of an amorphous resin, the intersection point of the baseline from the low temperature part and the tangent line at the inflection point is regarded as the glass transition point (Tg), and this is taken as the softening initiation temperature (Ts).

[0077] The powder granulation can be produced by a compression granulator, for example, a disk pelleter system, a screw extrusion system, a briquetting system, a tableting system, etc. Among the above examples, the disk pelleter system is preferably adopted from the viewpoint of granulation productivity and the quality and shape uniformity of the obtained powder granulation. In the disk pelleter system, a "semi-wet granulation method" in which an appropriate amount of moisture is contained may also be adopted, but in the present invention, granulation can be performed without using water, in which case the drying step may be unnecessary. If granulation can be performed without using water, the amount of energy required in the drying step can be reduced, and the amount of carbon dioxide emitted in the process can be greatly reduced.

[0078] When the thermoplastic resin powder is a mixture containing two or more kinds of powder raw materials, it is preferable to mix them uniformly using any appropriate mixer. Examples of the mixer include a Henschel mixer, a Nauta mixer, a powder kneader (KDH, KDA, CKD, CPM) (Dalton), a Spartan mixer (SPM) (Dalton), and an SP granulator (SPG) (Dalton). In order to obtain a preferable mixture with excellent granulation properties, it is preferable that the stirring blades of the mixing and stirring device are appropriate. For example, when using a Henschel mixer type mixer, it is preferable that the mixer blades are a combination of upper and lower blades, and the upper blade is a Y1 blade (trade name, manufactured by Nippon Coke Co., Ltd.) and the lower blade is an S0 blade (trade name, manufactured by Nippon Coke Co., Ltd.). In addition, it is preferable to install a deflector in the stirring tank and mix. In other words, by making it possible to uniformly disperse each component throughout the mixture, it is advantageous to increase the productivity and quality stability of the powder granulated product finally obtained.

[0079] A "semi-wet granulation method" can also be used, but the amount of water can be any appropriate amount depending on the powder properties (water absorption, etc.). In this case, the amount of water is 3 to 30 parts by mass, preferably 5 to 25 parts by mass, and more preferably 5 to 20 parts by mass, per 100 parts by mass of the thermoplastic resin powder. The semi-wet method can be used when the granulation property is not stable in the granulation step.

[0080] The disk pelletizer has, as a basic structure, one or two disks with many holes of 2 mm to 30 mm, and a roller for pressure-feeding the raw material to the holes of the disk. Thermoplastic resin powder (which may contain moisture) supplied between the disk and the roller, or between two disks, is pressed into the holes of the disk as the roller rotates, and a cylindrical extrudate is formed. The extruded granules are cut by a cutter or the like on the back side of the disk to obtain a pellet-shaped powder granule. The length of the granules can be adjusted by the distance between the back side of the disk and the cutter and the number of rotations of the roller. The distance between the disk plate and the cutter can be any appropriate distance. The distance between the disk plate and the cutter is, for example, 1 mm to 30 mm, more preferably 2 mm to 20 mm, and even more preferably 3 mm to 10 mm.

[0081] More specifically, the disc pelleter type includes a roller disc die type, a roller ring die type, a double die type, a flat die type, etc. An example of a commercially available disc pelleter type granulator is the Disc Pelletter F Series manufactured by Dalton.

[0082] C. Melt compounding using powder granulation In one embodiment, the powder granules are used as a thermoplastic resin compound raw material or molding material. One embodiment of the present invention is the use of the powder granules of the present invention as a thermoplastic resin compound raw material or molding material. For example, a melt compound of the powder granules and other thermoplastic resins can be provided.

[0083] The molten compound may be prepared by any suitable method. For example, a kneader, a Banbury mixer, a roll, or a single-screw or multi-screw extruder having two or more screws may be used. A twin-screw extruder is preferably used. The composition obtained by melt kneading is pelletized.

[0084] In one embodiment, the powder granulated product can be directly charged into a resin processing device such as an injection molding machine or an extrusion molding machine to obtain various resin composition molded articles. EXAMPLES

[0085] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In addition, parts and % are based on mass unless otherwise specified.

[0086] [evaluation] The powder granulated products obtained in the examples and comparative examples were evaluated by the following methods. (1) Granulation property (possibility of granulation) The obtained powder granulated product was confirmed, and the granulation properties were evaluated according to the following criteria. A: A powder granule with a core-shell structure is obtained, and the molten polymer can be clearly observed in the shell portion. B: A powder granule with a core-shell structure was obtained, and molten polymer was partially observed in the shell portion. C: An unstable core-shell structured powder granule is obtained, and a small amount of molten polymer is observed in the shell portion. D: The granules are unstable and tend to crumble. E: "Remains in powder form" or "die clogged" and cannot be granulated.

[0087] (2) Cross-sectional photograph of granulated material From the obtained powder granulated product, a slice (thickness: 0.5 mm) was cut out perpendicular to the extrusion direction from the die using a razor blade, and the cut cross section was observed under an optical microscope.

[0088] (3) Bulk density The dried powder granules were allowed to fall naturally into a 1-liter measure, filled to the brim, and weighed to a volume of exactly 1 liter. The mass was then measured to calculate the bulk density of the powder granules (unit: kg / L).

[0089] (4) Moisture content The amount of moisture (unit: mass%) remaining in the powder granules was measured using an infrared moisture meter (FD-660 manufactured by Kett Electric Laboratory).

[0090] (5) Breaking strength The breaking stress (unit: kg) of the powder granulation was measured using a Kiya hardness tester (manufactured by Shiro Sangyo Co., Ltd., product name "WPF1600-B"). The measured value was the average value of 25 grains of powder granulation. That is, the powder granulation was set in the hardness tester so that the side of the powder granulation was the bottom, and the breaking stress was measured by crushing the side of the powder granulation using a cylindrical presser with a diameter of 5 mm. In other words, the breaking stress was measured by crushing the powder granulation in a direction perpendicular to the longitudinal direction (extrusion direction). A: Breaking strength is 10kg (measurement limit) or more B: Breaking strength is 5.0kg or more and less than 10kg C: Breaking strength is 2.0kg or more and less than 5.0kg D: Breaking strength is 0.5kg or more and less than 2.0kg E: The breaking strength is less than 0.5 kg or the powder granulation product obtained is in powder form.

[0091] (6) Carbon dioxide (CO2) emissions The amount of electricity used in powder granulation was multiplied by the basic emission coefficient of 0.000362 [tons-CO2 / kWh] in the "Greenhouse Gas Emissions Calculation, Reporting, and Disclosure System" issued by the Ministry of the Environment (listed on the website, A0272 Kansai Electric Power's FY2020 Basic Emission Coefficient Actual Value (Announced on January 7, 2022)) to calculate the amount of carbon dioxide (CO2) emitted per unit mass (1 kg) of powder granulation (unit: kg (CO2) / kg).

[0092] [Production Example 1] Acrylic resin powder granulation (Production of acrylic resin powder) Using a polymerization apparatus equipped with a stirrer, reflux condenser, thermometer, nitrogen gas inlet tube and feed pump, 140 parts by mass of water, 0.05 parts by mass of sodium dodecylbenzenesulfonate and 0.1 parts by mass of sodium sulfate were mixed to obtain a mixture. After the mixture was substituted with nitrogen at 80°C, 0.1 parts by mass of potassium persulfate was added, and then, while stirring, a monomer mixture consisting of 90 parts by mass of methyl methacrylate (also referred to as MMA) and 10 parts by mass of butyl acrylate (also referred to as BA) was continuously added over 180 minutes to perform emulsion polymerization. 45 minutes and 90 minutes after the start of addition of the monomer mixture, 0.3 parts by mass of sodium dodecylbenzenesulfonate were added, respectively. After the addition of the monomer mixture was completed, the mixture was further stirred for 1 hour to perform polymerization, and the reaction was terminated to obtain an acrylic copolymer latex.

[0093] The obtained latex was cooled to room temperature, salted out with calcium chloride, coagulated, washed with water and dried to obtain acrylic resin powder A1.

[0094] The obtained acrylic resin powder A1 was sieved through a 10-mesh wire screen (mesh gap is about 2.5 mm) and the powder that passed through was collected. The bulk density of the powder was 0.32 kg / L, and the glass transition temperature (Tg) was measured using a differential scanning calorimeter (DSC, Hitachi High-Tech Science Corporation, product name "DSC6220") and was observed to be 81°C.

[0095] [Example 1] (Production of acrylic resin powder granules) The obtained acrylic resin powder A1 was used as a raw material and fed into a disk pelleter (manufactured by Dalton, product name "Disc Pelleter F-5 / 11-175") to produce a pellet-shaped powder granulation product under the condition of a roller rotation speed of 108 rpm. The thickness of the die plate of the disk pelleter was 15 mm, and the hole diameter was 3 mmφ. The length (referred to as the effective length) over which the powder received compressive stress from the die wall surface inside the die plate was 10 mm.

[0096] The temperature of the powder granulated material immediately after granulation was changed by factors such as the number of rotations of the rollers of the granulating device, the effective pressurizing length of the die hole, and heating or cooling of the die plate.

[0097] The temperature of the granulated material immediately after granulation was measured by stopping the device after granulation stabilized, directly inserting a thermocouple into the die hole, and quickly measuring the temperature of the compressed powder inside the die. This measurement was performed five times, and the average value was taken as the temperature of the granulated material immediately after granulation (Tp). If granulation was impossible due to the powder sticking to the die or clogging, the temperature was measured by directly inserting a thermocouple into the powder in the same manner.

[0098] Example 1 is an example in which the granulated material temperature (Tp) immediately after granulation was -5°C (i.e., the granulated material temperature was 76°C) relative to the softening initiation temperature (81°C) of the raw material acrylic resin powder A1, and a stable, approximately cylindrical granulated material was obtained.

[0099] Figure 1 shows a photograph of the appearance of the powder granulated product of Example 1. As shown in Figure 1, compression granulated products in a roughly cylindrical shape could be stably obtained.

[0100] The side of the powder granule obtained in Example 1 had an outer wall structure (shell structure) containing the melted components of the thermoplastic resin powder, and unmelted powder traces were confirmed inside the outer wall structure (core portion). Figure 2 shows a cross-sectional photograph of the powder granule obtained in Example 1 in a plane perpendicular to the longitudinal direction (extrusion direction).

[0101] The powder granulated product of Example 1 had a bulk density of 0.58 kg / L, a moisture content of 0.12 mass%, and a granulated product breaking strength of 6.9 kg, and was a powder granulated product with excellent handleability.

[0102] [Example 2] Example 2 is an example in which the granule temperature (Tp) immediately after granulation was -15°C (i.e., the granule temperature was 66°C) relative to the softening start temperature (81°C) of the raw material acrylic resin powder A1. The granule temperature was controlled by lowering the roller rotation speed. The obtained powder granule had a core-shell structure, similar to Example 1.

[0103] The powder granulated product of Example 2 had a bulk density of 0.52 kg / L, a moisture content of 0.2 mass%, and a granulated product breaking strength of 5.1 kg, and was a powder granulated product with excellent handleability.

[0104] [Example 3] Example 3 is an example in which the granule temperature (Tp) immediately after granulation was -26°C (i.e., the granule temperature was 55°C) relative to the softening start temperature (81°C) of the raw material acrylic resin powder A1. The granule temperature was controlled by further reducing the roller rotation speed and forcibly cooling by blowing air onto the disc plate. The obtained powder granule had a core-shell structure, similar to Example 1.

[0105] The powder granulated product of Example 3 had a bulk density of 0.6 kg / L, a moisture content of 0.15 mass%, and a breaking strength of the granulated product of 2.7 kg, and was a powder granulated product with excellent handleability.

[0106] Table 1 shows the production conditions for the powder granulated products obtained in Examples 1 to 3 and various measurement results for the powder granulated products.

[0107] [Comparative Example 1] Comparative Example 1 is an example in which the granule temperature (Tp) immediately after granulation was -41°C (i.e., the granule temperature was 40°C) relative to the softening start temperature (81°C) of the raw material acrylic resin powder A1. The granule temperature was controlled by changing the effective die length to 5 mm and forcibly cooling the disk plate.

[0108] In Comparative Example 1, the acrylic resin powder A1 passed through the die holes in the powder state, and no granules could be obtained.

[0109] [Comparative Example 2] Comparative Example 2 is an example in which the temperature of the granulated product immediately after granulation was +14°C (i.e., the granulated product temperature was 95°C) higher than the softening start temperature (81°C) of the raw material acrylic resin powder A1. The granulated product temperature was controlled by forcibly heating the disk plate using an external heater.

[0110] In Comparative Example 2, the acrylic resin powder A1 caused clogging in the die holes, and no granules could be obtained.

[0111] The powder granulated products obtained in Examples 1 to 3 and Comparative Examples 1 and 2 were evaluated, and the results are shown in Table 1.

[0112] [Table 1]

[0113] [Example 4] Biopolyester powder granules Pellets of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHBH), a type of PHA and a copolymer polyester of 3-hydroxybutyric acid and 3-hydroxyhexanoic acid (manufactured by Kaneka Corporation, product name "Green planet X131A", hexanoate content 6%) were crushed and sieved through a 10-mesh wire screen to obtain biopolyester powder A2.

[0114] The DSC measurement of the biopolyester powder A2 revealed that the softening onset temperature (Ts) was 80° C. As shown in FIG. 3, the softening onset temperature (Ts) was determined from the temperature at the intersection of the baseline from the low temperature part and the tangent to the inflection point on the melting onset side of the first observed crystal melting endothermic peak.

[0115] The biopolyester powder A2 was charged into a disk pelletizer in the same manner as in Example 1 to obtain a powder granulated product.

[0116] In Example 4, the granule temperature (Tp) immediately after granulation was 81°C, which was 1°C different from the softening onset temperature (Ts: 80°C), but a stable, approximately cylindrical granule was obtained. The side of the obtained powder granule had an outer wall structure (shell structure) made of molten polymer formed by melting the components of the thermoplastic resin powder, and an unmelted powder-like appearance was confirmed inside the outer wall structure (core part). A photograph of the appearance of the powder granule of Example 4 is shown in Figure 4. A cross-sectional photograph of the powder granule of Example 4 is shown in Figure 5.

[0117] The powder granulated product of Example 4 had a bulk density of 0.50 kg / L, a moisture content of 0.48 mass%, and a breaking strength of the granulated product of 10 kg or more, and was a powder granulated product with excellent handleability.

[0118] [Example 5] Injection molding using powder granulation The powder granules made of the acrylic resin powder A1 obtained in Example 1 were put into an injection molding machine (manufactured by Shibaura Corporation, product name "EX75SX"), and a business card size molded body (88 mm x 53 mm, three-stage plate with thicknesses of 1, 2, and 3 mm) was obtained at a resin temperature of 240°C, a mold temperature of 60°C, and a cooling time of 30 seconds. A photograph of the obtained injection molded body is shown in FIG. 6.

[0119] [Example 6] Sheet extrusion using powder granules The powder granules made of biopolyester powder A2 (PHBH) obtained in Example 4 were fed into a sheet extruder (manufactured by Technobel Co., Ltd., product name "KTZ15") and extruded through a T-shaped die at an extrusion speed of 2 kg / Hr to obtain a single-layer extruded sheet having a thickness of 0.5 mm and a width of 100 mm. The roll temperature was 20°C and the winding speed was 5 m / min.

[0120] In Example 6, extrusion molding was performed without the "melt kneading pelletization", but a sheet molding was obtained that was almost equivalent to the case where melt kneading pelletization was used. A photograph of the obtained sheet molding is shown in Figure 7.

[0121] [Example 7] Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHBH) pellets (manufactured by Kaneka Corporation, product name "Green planet X151A", hexanoate content 11%) were pulverized, and the pulverized material was sieved through a 10-mesh wire screen to obtain biopolyester powder A3.

[0122] For the biopolyester powder A3, DSC measurement was carried out in the same manner as in Example 4, and the softening onset temperature (Ts) was measured and found to be 80°C.

[0123] 100 parts by mass of biopolyester powder A3 were placed into an FM mixer (manufactured by Nippon Coke and Engineering Co., Ltd., product name "5FM5C / I"; processing volume: 5 L), and while rotating the stirring blades at a rotation speed of 2,000 rpm, 20 parts by mass of clean water (tap water) was continuously sprayed and injected into the biopolyester powder A3 in a spray form over a period of 10 minutes to obtain a water-containing powder mixture.

[0124] The FM mixer had a combination of upper and lower blades, with the upper blade being a Y1 blade (product name, manufactured by Nippon Coke Co., Ltd.) and the lower blade being an S0 blade (product name, manufactured by Nippon Coke Co., Ltd.). A baffle plate (also called a deflector) was installed in the mixing vessel.

[0125] This water-containing powder was charged into a disk pelleter in the same manner as in Example 1, to obtain a roughly cylindrical granulated material precursor.

[0126] Example 7 is a semi-wet granulation method. The presence of an appropriate amount of moisture increases the bulk density of the powder, improves the powder's ability to fit into the die holes, and also suppresses excessive heat generation during granulation and prevents the die from clogging. As a result of these actions and effects, the granulation speed was improved, and the granulation speed of the granule precursor granules reached 88 kg / Hr.

[0127] In Example 7, the temperature of the granulated precursor immediately after granulation was 54°C, which was -26°C lower than the softening starting temperature (80°C) of the raw material biopolyester powder A3 (i.e., the granulated temperature was 54°C). In Example 7, cylindrical granulated products could be stably obtained.

[0128] The obtained granulated material precursor was dried at 140° C. using a hot air circulation type dryer (manufactured by Espec, product name "PH-402") until the moisture content became 0.5 wt % or less, to obtain a powdered granulated material.

[0129] The obtained powder granules had a core-shell structure, similar to that of Example 1. A cross-sectional photograph of the powder granules of Example 7 is shown in FIG.

[0130] The powder granulated product of Example 7 had a bulk density of 0.49 kg / L, a moisture content of 0.27 mass%, and a breaking strength of the granulated product of 10.0 kg or more, and was a powder granulated product with excellent handleability.

[0131] [Example 8] The biopolyester powder A3 used in Example 7 was charged into a disk pelleter to obtain a powder granulated product in the same manner as in Example 1. In Example 8, unlike Example 7, no water was added.

[0132] The obtained powder granules had a core-shell structure, similar to that of Example 1. A cross-sectional photograph of the powder granules of Example 8 is shown in FIG.

[0133] The powder granulated product of Example 8 had a bulk density of 0.53 kg / L, a moisture content of 0.52 mass%, and a granulated product breaking strength of 10.0 kg or more, and was a powder granulated product with excellent handleability.

[0134] [Example 9] Polyhydroxyalkanoate (PHA) pellets (manufactured by Danimer Scientific, USA, product name "DAH-04267") were pulverized, and the pulverized material was sieved through a 10-mesh wire screen to obtain biopolyester powder A4.

[0135] For the biopolyester powder A4, DSC measurement was carried out in the same manner as in Example 4, and the softening onset temperature (Ts) was measured and found to be 85°C.

[0136] Example 9 is an example in which biopolyester powder A4 was used and granulation was carried out by mixing 20 parts by mass of tap water in the same manner as in Example 7.

[0137] In Example 9, the granulation speed of the granulated material was 39 kg / Hr, and the temperature of the granulated material precursor immediately after granulation was 76° C., which was 9° C. lower than the softening starting temperature (85° C.) of the raw material biopolyester powder A3 (i.e., the granulated material temperature was 76° C.). In Example 9, a granulated material precursor having a substantially cylindrical shape could be stably obtained.

[0138] The obtained granulated material precursor was dried at 140°C in a hot air circulation type dryer until the moisture content was 0.5 wt% or less, as in Example 7, to obtain a powder granulated material. The obtained powder granulated material had a core-shell structure. A cross-sectional photograph of the powder granulated material of Example 9 is shown in Figure 10.

[0139] The powder granules of Example 9 had a bulk density of 0.35 kg / L, a moisture content of 0.30 mass%, and a breaking strength of the granules of 10.0 kg or more, and were therefore excellent in handleability.

[0140] The evaluation results of Examples 4 and 7 to 9 are shown in Table 2.

[0141] [Table 2]

[0142] [Comparative Example 3] The biopolyester powder A3 used in Example 7 was continuously fed into a twin-screw extruder (manufactured by Nippon Steel Corporation, product name "TEX44αII", L / D = 42, cylinder set temperature: 140°C) and melt-kneaded to produce pellets of a thermoplastic resin composition.

[0143] Biopolyester powder A3 was quantitatively fed into the extruder at the hopper position at the most upstream part via a gravimetric feeder. The screw was rotated at 81 rpm, and a strand was drawn out from the die at the tip of the extruder, cooled with water at 60°C, and pelletized into pellets of about 3 mm length using a pelletizer (manufactured by Isuzu Motors, product name "HSCR-150") to obtain "melt-kneaded pellets" of biopolyester powder A3.

[0144] The feeding rate of biopolyester powder A3 into the extruder was gradually increased, and granulation was performed at the feed rate that maximized the compound processing speed per hour (i.e., the maximum feed rate at which stable production is possible without causing a feed neck of the raw material powder into the extruder). As a result, the maximum discharge rate was only 60 kg / Hr.

[0145] The obtained melt-kneaded pellets were dried at 80° C. using a hot air circulation type dryer until the moisture content became 0.2 wt % or less, in the same manner as in Example 7, to obtain melt-kneaded pellets.

[0146] The power consumption and the amount of carbon dioxide generated in each process (calculated values) per unit mass (per 1 kg) of granules were calculated in the same manner as in Example 7. The results are shown in Table 3.

[0147] Comparison of Examples 7 and 8 with Comparative Example 3 shows that the "powder polymer granules" of the present invention significantly reduces the amount of CO2 emitted during the process compared to the "melt-kneaded pellets" that use a twin-screw extruder that uses a large heat source heater and power.

[0148] [Table 3]

Claims

1. A powder granulation product containing thermoplastic resin powder, the powder granulation product having an outer wall portion formed by melting at least a portion of the thermoplastic resin powder located at the outer edge of the powder granulation product, and compressed thermoplastic resin powder being contained inside the outer wall portion.

2. 2. The powder granulation of claim 1, wherein at least a portion of the compressed thermoplastic resin powder inside the outer wall comprises unmelted compressed powder-like forms.

3. The powder granule according to claim 1 , wherein at least a portion of the compressed thermoplastic resin powder inside the outer wall portion is in a partially melted state.

4. The powder granulated product according to claim 1 , wherein the powder granulated product has a substantially cylindrical or substantially prismatic shape.

5. The powder granulated product according to claim 4, which has an outer wall portion on a side surface of the powder granulated product.

6. The powder granulated product according to claim 5, having a breaking strength of 2.0 kg or more.

7. The powder granule according to claim 1 , wherein the powder granule is a compressed granule.

8. The powder granule according to claim 1, wherein the thermoplastic resin powder contains a thermoplastic resin having a softening onset temperature of 50 to 150°C.

9. The powder granule according to claim 1, wherein the thermoplastic resin powder contains a thermoplastic resin having a softening onset temperature of 60 to 90°C.

10. The thermoplastic resin powder is selected from the group consisting of acrylic resins, methacrylic resins, polyhydroxyalkanoate (PHA) resins, polyolefin resins, polyamide resins, polyacetal resins, polyphenylene ether (PPE) resins, polyphenylene sulfide (PPS) resins, polyether ether ketone (PEEK) resins, polyimide (PI) resins, polyamideimide (PAI) resins, polyester resins, polycarbonate (PC) resins, polystyrene resins, polyketone resins, liquid crystal polymers (LCPs), and core-shell polymers. The powder granule according to claim 1, which contains at least one selected from the group consisting of polyphenylene ether (PPE) resins, polyphenylene sulfide (PPS) resins, polyether ether ketone (PEEK) resins, polyimide (PI) resins, polyamideimide (PAI) resins, polyester resins, polycarbonate (PC) resins, polystyrene resins, polyketone resins, liquid crystal polymers (LCPs), and core-shell polymers.

11. The powder granulated product according to claim 1 , wherein the thermoplastic resin powder comprises a PHA-based resin.

12. A method for producing the powder granulated product according to any one of claims 1 to 11, The method includes a compression granulation step of granulating a thermoplastic resin powder by a compression granulation method in which the thermoplastic resin powder is extruded through a die hole, The compression granulation step is carried out under the condition that the granulated product temperature Tp (°C) immediately after granulation and the softening starting temperature Ts (°C) of the thermoplastic resin powder satisfy the formula (1). Equation (1): Ts-30≦Tp≦Ts+10.

13. The method according to claim 12, wherein the die temperature is controlled so that the granule temperature Tp (°C) immediately after granulation and the softening starting temperature Ts (°C) of the thermoplastic resin powder satisfy the condition of formula (1).

14. The method according to claim 12, wherein the outer wall portion is formed by melting at least a portion of the thermoplastic resin powder at a contact surface with a wall surface of the die hole by frictional heat with the wall surface or heat transfer from the wall surface.

15. The method according to claim 14, wherein the compression granulation is carried out using a disk pelleter type compression granulator.

16. Use of the powder granule according to any one of claims 1 to 11 as a raw material for a thermoplastic resin compound or as a molding material.

Citation Information

Patent Citations

  • Method for producing composite particle

    JP2003025325A

  • Raw mix powder composition and method for making same

    JP2005326846A