Map film
The map film, made of a plastic film with specific polyester resin and digital printing, addresses water resistance and folding stability issues, ensuring clear and durable map information display.
Patent Information
- Application Number
- JP2023081017
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-28
AI Technical Summary
Existing map materials face issues with water resistance, folding stability, and the ability to maintain a folded shape, especially when carrying multiple maps due to space constraints, while also ensuring clear visibility of detailed map information.
A map film composed of a plastic film with a digital printing layer containing map information, using a polyester resin with specific ethylene terephthalate units and amorphous components, allowing a folding retention angle of 90 degrees or less after 24 hours, and protected by multiple plastic films to maintain clarity and durability.
The map film exhibits excellent water resistance, maintains a folded shape, and can clearly display minute map information, even after repeated use and exposure to water, making it suitable for portable maps.
Smart Images

Figure 2024165128000005 
Figure 2024165128000001 
Figure 2024165128000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a map film using a plastic film, and more specifically, to a map film that has excellent folding retention performance after storage for 24 hours in an environment of 20°C and can contain minute, visible map information. [Background technology]
[0002] Conventionally, maps have generally been made of paper with map information printed on it, but this has the drawback of being easily torn when exposed to water or rain.
[0003] Therefore, Patent Document 1 discloses a paper map for outdoor use that is formed by coating a paper core with a glass layer made of a specific material composition, and has excellent water repellency and water resistance.
[0004] Patent Document 2 was proposed to solve the problems of Patent Document 1. That is, when paper having a glass coating layer on the surface is used as the material as in Patent Document 1, the glass coating layer lacks flexibility, so that when folded repeatedly, wrinkles occur, making the printed map difficult to see, and water can penetrate through the wrinkles, making the sheet prone to tearing. Therefore, Patent Document 2 discloses a map-printed sheet in which a map is printed with a waterproof ink on one side of a sheet made of a closed-cell foam having a predetermined cell diameter, in order to provide a map-printed sheet that can recover from wrinkles even when folded repeatedly.
[0005] In Patent Document 2, an elastic sheet made of a closed-cell foam is used as the base material, which has the advantage that it is difficult to develop creases and can be crumpled up and tucked in for storage. However, on the other hand, it is difficult to develop creases and when folded and stored in a clothing pocket or the like, it is difficult to maintain the folded shape, making it difficult to take out after storage, and it is bulky when stored, making it impossible to store other items in the pocket or the like.
[0006] Patent Document 3 discloses a map film that is excellent in retaining its folded shape in order to improve the poor storability caused by the difficulty in retaining the folded shape, which is a problem in Patent Document 2. The map film has the performance of being easily portable, but is often used in a form in which the user carries it in a small storage space such as a pocket, and therefore is required to be compact in size. The present inventors have found that when trying to include a lot of map information on a compact-sized map film, the map information is too small to be printed clearly, resulting in a restriction that only a small amount of map information can be included. In addition, the present inventors have found that in order to include a lot of map information, it becomes necessary to include it in multiple maps, and as a result, the inconvenience caused by using multiple maps occurs. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Utility Model Registration No. 3066036 [Patent Document 2] Utility Model Registration No. 3185924 [Patent Document 3] JP 2019-77094 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made to solve the above-mentioned problems, and its object is to provide a map film that is made of a material that has excellent water resistance against water, rain, etc., has excellent ability to retain its folded shape (folded retention performance) after storage for 24 hours in an environment of 20°C, and is capable of containing tiny, visible map information. [Means for solving the problem]
[0009] The present invention, which has solved the above problems, comprises the following components. 1. A map film having a plastic film and a printed portion consisting of a digitally printed layer containing map information, wherein the printed portion has a folding retention angle of 90 degrees or less after being stored for 24 hours in an environment of 20°C. 2. The map film according to claim 1, wherein the map information includes characters of 4pt or less in size. 3. A map film as described in 1. or 2., having a printed area between two plastic films. 4. A map film according to any one of 1 to 3, wherein the plastic film is a transparent plastic film or a translucent plastic film. 5. A map film according to any one of 1 to 4, wherein the plastic film is a polyester film. 6. The map film described in 5., wherein the polyester film is composed of a polyester resin having 50 mol% or more of ethylene terephthalate units out of 100 mol% of all ester units, and the sum of the proportion of amorphous alcohol components in 100 mol% of all alcohol components and the proportion of amorphous acid components in 100 mol% of all acid components is 12 mol% or more and 30 mol% or less. 7. A map film according to any one of 1 to 6, wherein the map information includes at least one type of information selected from the group consisting of exhibition centres, ski resorts, campsites, tourist destinations, theme parks, amusement parks, golf courses, beaches, swimming pools, baseball stadiums, athletics stadiums, marathon venues, outdoor sports facilities, accommodation facilities and shopping malls. 8. A map film according to any one of 1 to 7, having a folded shape. Effect of the Invention
[0010] According to the present invention, it is possible to provide a map film that has excellent water resistance against water, rain, etc., has excellent folding retention performance after storage for 24 hours in an environment of 20°C, and is capable of containing minute, visible map information. [Brief description of the drawings]
[0011] [Figure 1]FIG. 1 is a diagram showing a method for measuring the folding and holding angle of a map film according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] As a result of extensive investigations conducted by the present inventors to solve the above problems, it was found that the desired object could be achieved by using the above film, and thus the present invention was completed.
[0013] Maps used in expositions, ski resorts, campsites, tourist spots, theme parks, amusement parks, golf courses, beaches, swimming pools, baseball stadiums, athletic stadiums, marathon venues, outdoor sports facilities, accommodation facilities, and shopping malls have map information of limited areas printed on them, and the above maps are carried by users to arrive at their destinations in the above areas. Conventionally, maps with map information printed on the surface of a paper substrate have been used, but maps made of paper have the disadvantage that they are easily damaged by water or rain, and are easily torn and stained, especially when used outdoors. In addition, when a plastic such as synthetic paper is used as the substrate, the folding retention is poor, and when folded and carried, it cannot be stored well in a pocket of clothing, etc. When a plastic substrate with good folding retention is used, if a lot of map information is to be printed, the map information is too small to be printed clearly, so there is a restriction that only a small amount of map information can be printed. In order to print a lot of map information, it is necessary to print it on multiple maps, which results in a problem of not being able to be stored well in a pocket of clothing, etc. when carried. In other words, there is a trade-off between providing a large amount of map information and being easy to store, and no map film has ever been developed that satisfies both. The present invention can solve all of these problems.
[0014] The map film of the present invention will now be described in detail.
[0015] The map film of the present invention has a plastic film and a printed portion consisting of a digitally printed layer containing map information, and is characterized in that the folding angle after storage for 24 hours in an environment of 20°C is 90 degrees or less.
[0016] As described above, the map film of the present invention satisfies the requirement of a folding retention angle of 90 degrees or less after storage for 24 hours in an environment at 20°C, and therefore, when the film is folded and carried, it can be easily folded by hand and can maintain its shape in the folded state. Strictly speaking, the folding retention property differs depending on the type of plastic film used, but it has been found that, as long as the folding retention angle after storage is controlled to 90 degrees or less, it is possible to achieve both easy folding and shape retention after folding, particularly when folding. Since the map film of the present invention can be firmly folded once, when the map film is carried and used, it can maintain its shape in the folded state even if the map film is repeatedly unfolded and folded, and is very easy to use. The folding retention angle is preferably 80 degrees or less, more preferably 70 degrees or less, and particularly preferably 60 degrees or less. There is no particular restriction on the lower limit of the folding retention angle, but the value that can be actually achieved is generally 20 degrees or more.
[0017] The map film of the present invention also has a printing section made of a digital printing layer containing map information. The digital printing layer is a layer formed by digital printing. Applicable digital printing methods include liquid electrophotography (LEP) and inkjet (IJ) methods. In either method, the digital printing layer is patterned without a plate. An anchor coat layer may be formed to improve the adhesion of the digital printing layer. Toners used in electrophotographic printing are broadly classified into dry toners and wet toners (electrophotographic inks). Electrophotographic inks are suitable for high-precision printing because they scatter less toner particles than dry toners and can be made finer. The method using this electrophotographic ink is called the liquid electrophotography (LEP) method. Hewlett-Packard's Indigo is known as a digital printing device for the LEP method. In the case of the LEP method, the LEP ink and the composition of the primer layer can be, for example, those exemplified in International Publication No. 2016 / 074716. The composition of the LEP ink includes, for example, a colorant such as a pigment or dye, an ionic compound (charge director) for charging the LEP ink, a resin composition such as an acrylic resin, a solvent, and other additives.
[0018] The printing unit includes map information. The map information includes natural landforms such as mountains, seas, and lakes, artificial structures, roads, passages, and the like, and may include their positional relationships and explanatory items. Preferably, the map information includes map symbols defined by the Geospatial Information Authority of Japan, and information on landforms, roads, passages, facilities, vehicles, stations, airports, tourist attractions, pavilions, plazas, stores, stadiums, construction sites, police stations, hospitals, toilets, restaurants, rooms, seating areas, and restricted areas. More preferably, the map information includes one or more types of map information selected from the group consisting of exposition sites, ski resorts, campsites, tourist destinations, theme parks, amusement parks, golf courses, beaches, pools, baseball fields, athletic stadiums, marathon venues, outdoor sports facilities, accommodation facilities, and shopping malls. More preferably, the map information includes at least one type of information selected from the group consisting of pictures, images, figures, letters, and numbers, and more preferably includes letters and / or numbers. When the map information includes letters and / or numbers, it is particularly preferable that the font size of the letters and / or numbers is 4pt or less. Here, 1 pt is 1 / 72 inch, or 0.3528 mm. By having map information with a font size of 4 pt or less, map information including letters and / or numbers can be printed with both the necessary amount of information and a beautiful appearance, even on a map film with a relatively small area, such as A4 size. The font size of 4 pt or less can be achieved by digital printing.
[0019] The map film of the present invention preferably has a printed section containing map information between two plastic films. With the above-mentioned configuration, the printed section is protected and can be used for a long period of time, and even when used in an environment containing water, etc., it is possible to prevent problems such as defective or fallen-off parts occurring in the printed section, making the map information illegible. In particular, when folding, defects are likely to occur in the printed section at the folded part, but with the above-mentioned configuration, it is possible to suppress these defects. The printed section may be one layer, or two or more layers.
[0020] The portion other than the printed portion preferably includes a transparent or translucent portion, and more preferably includes a transparent portion.
[0021] The map film of the present invention is preferably a transparent film or a semi-transparent film, and more preferably a transparent film. In other words, the portion other than the printed portion preferably includes a transparent or semi-transparent portion, and more preferably includes a transparent portion. In the present invention, a film having a haze value of 25% or less in the portion not including the printed portion is defined as a transparent film, a film having a haze value of more than 25% to 50% or less is defined as a semi-transparent film, and a film having a haze value of more than 50% is defined as an opaque film. The haze value is measured in accordance with JIS-K-7105, and the values are measured at three different locations, and the average value is defined as the haze value.
[0022] The type of plastic film constituting the map film of the present invention is not particularly limited as long as the folding angle of the map film after storage for 24 hours in an environment of 20° C. is controlled to 90 degrees or less, and examples include polyester film, polystyrene film, polycarbonate film, etc. In consideration of the printability of the film and material costs, polyester film is preferred.
[0023] The polyester film preferably contains ethylene terephthalate units in an amount of 50 mol% or more, more preferably 60 mol% or more, based on 100 mol% of all ester units. The ethylene terephthalate units contain ethylene glycol and terephthalic acid as main components. By using ethylene terephthalate as the main component in this manner, excellent heat resistance and transparency can be obtained. The upper limit of the ethylene terephthalate units is preferably less than 100 mol%, more preferably 95 mol% or less, even more preferably 90 mol% or less, and most preferably 88 mol% or less.
[0024] Examples of dicarboxylic acid components other than terephthalic acid that constitute the polyester film include aromatic dicarboxylic acids such as isophthalic acid, naphthalenedicarboxylic acid, and orthophthalic acid, aliphatic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, and decanedicarboxylic acid, and alicyclic dicarboxylic acids.
[0025] It is preferable that the polyester film does not contain a polyvalent carboxylic acid having three or more valences (e.g., trimellitic acid, pyromellitic acid, and anhydrides thereof, etc.) This is because films obtained using polyesters containing such polyvalent carboxylic acids may generate foreign matter during film formation by melt extrusion, resulting in poor appearance.
[0026] Examples of diol components other than ethylene glycol that constitute the above polyester film include aliphatic diols such as 1,3-propanediol, 1,4-butanediol, neopentyl glycol, and hexanediol; alicyclic diols such as 1,4-cyclohexanedimethanol; and aromatic diols such as bisphenol A.
[0027] Among these, cyclic diols such as 1,4-cyclohexanedimethanol; and diols having 3 to 6 carbon atoms (for example, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, hexanediol, etc.) are useful as low Tg components, and the glass transition point (Tg) can be adjusted to 60 to 70°C by adding one or more of these components.
[0028] The polyester film preferably contains amorphous components (amorphous alcohol components and amorphous acid components), and the preferred total of the ratio of the amorphous alcohol components in 100 mol% of the total alcohol components and the ratio of the amorphous acid components in 100 mol% of the total acid components is 12 mol% or more and 30 mol% or less. By containing ethylene terephthalate as the main component and 12 mol% or more of a monomer component that can become an amorphous component, the folding holding angle of the film can be easily adjusted to a lower holding angle. More preferably, it is 15 mol% or more, even more preferably 17 mol% or more, and even more preferably 18 mol% or more. On the other hand, if the total of the monomer components that can become an amorphous component exceeds 30 mol%, the tear resistance and heat resistance are likely to be insufficient. In addition, the digital printing layer often has insufficient adhesion to the plastic substrate compared to the printing layer printed by other methods, but the film made of the above-mentioned preferred polyester composition has excellent adhesion to the digital printing layer, and it is possible to ensure adhesion without performing surface treatment or coating to improve adhesion.
[0029] Examples of the amorphous acid component (carboxylic acid component) monomer include isophthalic acid, 1,4-cyclohexanedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid.
[0030] Furthermore, examples of the monomer of the amorphous alcohol component (diol component) include neopentyl glycol, 1,4-cyclohexanedimethanol, 2,2-diethyl-1,3-propanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2-isopropyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, and hexanediol.
[0031] Among these monomer components, neopentyl glycol, 1,4-cyclohexanedimethanol or isophthalic acid is preferred, and neopentyl glycol is particularly preferred.
[0032] It is preferable that the polyester film does not contain a diol having 8 or more carbon atoms (e.g., octanediol, etc.) or a polyhydric alcohol having 3 or more hydricities (e.g., trimethylolpropane, trimethylolethane, glycerin, diglycerin, etc.). If a diol having 8 or more carbon atoms is contained, the mechanical strength of the film may be impaired. If the polyhydric alcohols mentioned above are contained, there is a risk that foreign matter will be generated during the formation of a film by melt extrusion, resulting in a poor appearance.
[0033] The polyester film is preferably used in combination with a polyester elastomer, which increases the degree of amorphousness and improves the folding retention. The polyester elastomer preferably used in the present invention is a polyester block copolymer consisting of a high melting point crystalline polyester segment (hard segment) and a low melting point soft polymer segment (soft segment) having a number average molecular weight of 400 or more.
[0034] The high melting point crystalline polyester segment means a segment whose melting point is 200° C. or higher when the polymer is formed from only its constituent components. Examples of the high melting point crystalline polyester segment include polyesters consisting of residues of aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 1,5-naphthalenedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid, and residues of aliphatic, aromatic, or alicyclic diols such as pentamethylene glycol, 2,2-dimethyltrimethylene glycol, hexamethylene glycol, decamethylene glycol, p-xylene glycol, and cyclohexanedimethanol; Polyesters consisting of residues of oxyacids such as dibenzoic acid pivalolactone, polyether esters consisting of residues of aromatic ether dicarboxylic acids such as 1,2-bis(4,4'-dicarboxymethylphenoxy)ethane, di(4-carboxyphenoxy)ethane and the above-mentioned aliphatic, aromatic or alicyclic diols, polyamide esters consisting of residues of aromatic amide dicarboxylic acids such as bis(N-paracarbethoxyphenyl)terephthalimide and the above-mentioned aliphatic, aromatic or alicyclic diols, etc. Copolymer polyesters using two or more of the above-mentioned dicarboxylic acid residues and / or diol residues can also be used.
[0035] On the other hand, the low melting point soft polymer segment is a segment that is substantially amorphous in the polyester elastomer, and when a polymer is formed from only its constituent components, the segment has a melting point or softening point of 80° C. or lower. The number average molecular weight of the low melting point soft polymer segment is preferably 400 to 8,000, and more preferably 700 to 5,000.
[0036] Examples of the low melting point soft polymer segment include polyethers such as polyethylene oxide glycol, polypropylene oxide glycol, polytetramethylene oxide glycol, glycol of a copolymer of ethylene oxide and propylene oxide, glycol of a copolymer of ethylene oxide and tetrahydrofuran, aliphatic polyesters such as polyneopentyl azelate, polyneopentyl adipate, polyneopentyl sebacate, polylactones such as poly-ε-caprolactone, etc. Considering compatibility with the polyester constituting the polyester film, polyester-based elastomers using polylactones such as poly-ε-caprolactone as the soft segment are preferred. The proportion of the low melting point soft polymer segment in the polyester elastomer is preferably from 1 to 90% by mass, and more preferably from 5 to 80% by mass.
[0037] In the present invention, as the polyester elastomer, an ε-caprolactone polyester elastomer consisting of a copolymer polyester of terephthalic acid, butanediol, and ε-caprolactone is preferably used (see polyester raw material E in Table 1 described later). This increases the degree of amorphousness, and the folding retention performance is further improved. In order to fully exert such effects, the content of the ε-caprolactone polyester elastomer in 100 mol % of the polyester resin constituting the polyester film is preferably 1 to 30 mol %, more preferably 3 to 25 mol %, and even more preferably 5 to 20 mol %. If the content of the ε-caprolactone polyester elastomer is less than 1 mol %, the effect of adding the ε-caprolactone polyester elastomer is not fully exerted. On the other hand, if the content of the ε-caprolactone polyester elastomer exceeds 30 mol %, there is a risk that the physical strength such as tear resistance, strength, and heat resistance of the film cannot be sufficiently obtained.
[0038] The polyester raw material used in the present invention may contain various additives as necessary. The additives are not particularly limited, and examples thereof include known additives such as waxes, antioxidants, antistatic agents, crystal nucleating agents, viscosity reducers, heat stabilizers, coloring pigments, coloring inhibitors, and ultraviolet absorbers.
[0039] In addition, it is preferable to add fine particles acting as a lubricant to the polyester raw material in order to improve the workability (slipperiness) of the film. As the fine particles, any type of inorganic or organic fine particles can be selected. Examples of inorganic fine particles include silica, alumina, titanium dioxide, calcium carbonate, kaolin, barium sulfate, etc. Examples of organic fine particles include acrylic resin particles, melamine resin particles, silicone resin particles, crosslinked polystyrene particles, etc. The average particle size of the fine particles is preferably within the range of about 0.05 to 3.0 μm when measured with a Coulter counter.
[0040] The method of blending the above-mentioned fine particles in the polyester raw material is not particularly limited, and for example, they can be added at any stage in the production of the polyester resin, but it is preferable to add them as a slurry dispersed in ethylene glycol or the like at the stage of esterification or after the completion of the transesterification reaction and before the start of the polycondensation reaction, and proceed with the polycondensation reaction. In addition, there is also a method of blending a slurry of particles dispersed in ethylene glycol or water or the like with the polyester resin raw material using a vented kneading extruder, or a method of blending the fine particles dried using a kneading extruder with the polyester resin raw material.
[0041] Furthermore, the polyester film may be subjected to corona treatment, coating treatment, flame treatment, etc., in order to improve the adhesiveness of the film surface.
[0042] The map film of the present invention may be a single layer film or a laminated film of two or more layers. In the case of a single layer film, a printed part including map information can be formed by printing on the front side. In the case of a laminated film, an adhesive layer can be further included. This makes it possible to form a laminated film consisting of multiple layers laminated via an adhesive layer. Specifically, examples of the laminated structure include a plastic film / digital printed part / adhesive / plastic film (No. 1 to 10 in Table 3) in which the printed part side of a plastic film and the adhesive layer side of a plastic film are laminated, as in the laminated film in Table 3 described later, and a plastic film / printed part / digital adhesive / printed part / plastic film (No. 11 in Table 3) in which the printed part sides of the films are laminated together via an adhesive.
[0043] From the viewpoint of providing folding retention performance while favorably exhibiting the design of the pattern or the like applied to the printed portion, for example, a polyurethane adhesive is preferably used as the adhesive used in the present invention. Examples of polyurethane adhesives include dry lamination adhesives such as Takelac (registered trademark) and Takenate (registered trademark) manufactured by Mitsui Chemicals, Inc., and TM-250HV, TM-556S, and TM-265L manufactured by Toyo Ink Co., Ltd. The thickness of the adhesive layer is preferably 1 to 6 μm, and more preferably 2 to 5 μm.
[0044] However, the laminated film does not necessarily have to be produced through an adhesive layer, and it is also possible to produce the laminated film without an adhesive layer by, for example, a co-extrusion method.
[0045] The types of films constituting the laminate film may be such that at least one of them satisfies the requirements of the present invention, and preferably all of the films in the laminate film satisfy the requirements of the present invention, such as the laminate films in Table 3 described below.
[0046] The map film of the present invention preferably has an area that allows it to be folded and carried, which makes it easier to realize the effects of the present invention. The area of the map film of the present invention is 1300 cm, taking into consideration the storage capacity when folded into four or eight and carried in a pocket of a garment. 2 Less than 1000cm is preferable. 2 Less than 700cm is preferable. 2 Less than 650cm is more preferable. 2 The following is particularly preferred. As described above, the map film of the present invention can print small text information with a font size of 4pt or less so that it can be visibly read, so that a sufficient amount of map information can be printed even on a map film with a small area. Not only text information, but also small symbols can be printed so that they can be visibly read.
[0047] The shape of the map film according to the present invention is not particularly limited, and it is possible to adopt shapes such as a triangle, a rectangle, a pentagon, a hexagon, a heptagon, an octagon, a circle, an ellipse, etc., of which a rectangle is preferable, and a rectangle is more preferable.
[0048] The map film of the present invention preferably has a total film thickness (the thickness in the case of a single-layer film, or the total thickness in the case of a laminated film including an adhesive layer) of 5 μm to 200 μm. If the total film thickness is less than 5 μm, the film may not have the stiffness required for a map, and may be difficult to handle when folded. If the total film thickness exceeds 200 μm, folding may be difficult. The total film thickness is preferably 7 μm to 150 μm, and more preferably 10 μm to 120 μm.
[0049] Next, a method for producing a film according to the present invention will be described below. In the following, a polyester film containing a copolymer polyester will be described, but the present invention is not limited thereto.
[0050] The polyester film can be produced by melt-extruding the above-mentioned polyester raw material with an extruder to form an unstretched film, and then uniaxially or biaxially stretching the unstretched film by a predetermined method described below. The polyester can be obtained by polycondensing the above-mentioned suitable dicarboxylic acid component and diol component by a known method. In addition, two or more kinds of chip-like polyesters are usually mixed and used as the raw material for the film.
[0051] First, the raw material resin is melt-extruded. At that time, it is preferable to dry the polyester raw material using a dryer such as a hopper dryer or a paddle dryer, or a vacuum dryer. After the polyester raw material is dried in this manner, it is melted at a temperature of 200 to 300° C. and extruded into a film using an extruder. For extrusion, any existing method such as a T-die method or a tubular method can be used.
[0052] The extruded sheet-like molten resin can then be quenched to obtain an unstretched film. As a method for quenching the molten resin, a method in which the molten resin is cast from a die onto a rotating drum and rapidly cooled and solidified to obtain a substantially unoriented resin sheet can be suitably adopted.
[0053] Next, the unstretched film is stretched. The stretching direction of the film may be either the longitudinal (length) direction or the transverse (width) direction of the film. Below, a biaxial stretching method by transverse stretching-longitudinal stretching in which transverse stretching is performed first and then longitudinal stretching is described, but the order may be reversed (longitudinal stretching-transverse stretching), since only the main orientation direction changes. Alternatively, it is not necessary to perform biaxial stretching as described above, and either transverse stretching or longitudinal stretching may be performed.
[0054] First, the film is stretched in the transverse direction. The stretching in the transverse direction is preferably performed at 65 to 85°C and about 3.5 to 5 times the original length in a tenter (first tenter) with both ends in the width direction of the film held by clips. It is preferable to perform preheating before the transverse stretching, and the preheating may be performed until the film surface temperature reaches 70 to 100°C.
[0055] After the transverse stretching, it is preferable to pass the film through an intermediate zone where no active heating operation is performed. If there is a temperature difference between the transverse stretching zone and the intermediate heat treatment zone of the first tenter, the heat (hot air itself or radiant heat) from the intermediate heat treatment zone may flow into the transverse stretching process, and the temperature of the transverse stretching zone may not be stable, resulting in unstable film quality. Therefore, it is preferable to pass the film after transverse stretching and before intermediate heat treatment through the intermediate zone for a predetermined time, and then perform intermediate heat treatment. In this intermediate zone, if a strip of paper is hung down without passing through the film, the accompanying flow accompanying the running of the film and the hot air from the transverse stretching zone and intermediate heat treatment are blocked so that the paper hangs down almost completely vertically, a film of stable quality can be obtained. The time of passing through the intermediate zone is sufficient for about 1 to 5 seconds. If it is shorter than 1 second, the length of the intermediate zone is insufficient and the heat blocking effect is insufficient. The longer the intermediate zone, the larger the equipment becomes if it is too long, so about 5 seconds is sufficient.
[0056] After passing through the intermediate zone, intermediate heat treatment before longitudinal stretching may or may not be performed. When intermediate heat treatment is performed after transverse stretching, if the temperature of the intermediate heat treatment is increased, the molecular orientation that contributes to foldability is relaxed and crystallization is promoted, resulting in a slight deterioration of foldability. In addition, thickness unevenness is also deteriorated. From this viewpoint, the intermediate heat treatment is preferably performed at 140°C or less. Here, the passing time through the intermediate heat treatment zone is preferably 20 seconds or less. The longer the intermediate heat treatment zone, the more preferable, but about 20 seconds is sufficient. This results in a transverse uniaxially stretched polyester film.
[0057] Next, longitudinal stretching is performed. As described above, longitudinal stretching after transverse stretching is not necessarily required, but longitudinal stretching is preferable because it improves the tensile breaking strength of the film. Specifically, for example, the transversely uniaxially stretched polyester film may be introduced into a longitudinal stretching machine in which a plurality of roll groups are arranged in series. In longitudinal stretching, it is preferable to preheat the film with a preheating roll until the film temperature reaches 65 to 110°C. If the film temperature is lower than 65°C, it becomes difficult to stretch when stretching in the longitudinal direction (i.e., breakage is likely to occur), which is not preferable. On the other hand, if the temperature is higher than 110°C, the film tends to stick to the roll, and the roll becomes easily soiled due to continuous production, which is not preferable.
[0058] When the film temperature reaches the above range, the film is stretched longitudinally. The longitudinal stretching ratio differs depending on whether the main orientation direction is the longitudinal direction or the transverse direction. When the main orientation direction is the longitudinal direction, the longitudinal stretching ratio should be 2 to 5 times. On the other hand, when the main orientation direction is the transverse direction, the longitudinal stretching ratio should be 1.2 to 1.8 times.
[0059] After the longitudinal stretching, it is preferable to once cool the film, and before carrying out the final heat treatment, it is preferable to cool the film with a cooling roll having a surface temperature of 20 to 40° C. Rapid cooling after the longitudinal stretching is preferable because it stabilizes the molecular orientation of the film and reduces the natural shrinkage rate of the film after it is made into a product.
[0060] Next, the film after longitudinal stretching and cooling is introduced into a second tenter for heat treatment (relaxation treatment), where it is subjected to heat treatment (relaxation treatment). The relaxation treatment is a process in which the film is relaxed by 0 to 30% while both ends in the width direction of the film are held by clips. The shrinkage rate in the width direction can be changed by changing the relaxation rate. The lower limit of the relaxation rate is 0% and the upper limit is 99%, but if the relaxation rate is too high, it is undesirable because it has the disadvantage of shortening the width of the film product. Therefore, the upper limit of the relaxation rate is preferably about 30%.
[0061] The temperature of the heat treatment (relaxation treatment) is preferably 65 to 140°C. If the heat treatment temperature is lower than 65°C, the effect of the heat treatment is not effectively exhibited. On the other hand, if the heat treatment temperature is higher than 140°C, the film will crystallize and the film will tend to have poor folding angle retention, which is undesirable. The lower limit of the heat treatment temperature is more preferably 70°C or higher, and even more preferably 75°C or higher. On the other hand, the upper limit of the heat treatment temperature is more preferably 130°C or lower, and even more preferably 120°C or lower.
[0062] Finally, the film is wound up while cutting and removing both ends to obtain a polyester film roll.
[0063] From the viewpoint of easy portability of the map film, the map film of the present invention is preferably in a folded shape. When folding the map film, it is possible to easily fold it by hand, but it is also possible to form it into a tubular shape in advance and fold it at two ends to form a flat tubular body. Examples of methods for producing a tubular body include applying an organic solvent or adhesive to one side of a rectangular film slightly inward from the end, immediately rolling the film, overlapping and gluing the ends to form a label; or applying an organic solvent or adhesive to one side of a rolled film slightly inward from the end, immediately rolling the film, overlapping and gluing the ends to form a tubular body. As the organic solvent for adhesion, cyclic ethers such as 1,3-dioxolane or tetrahydrofuran are preferred. In addition to the above, aromatic hydrocarbons such as benzene, toluene, xylene, trimethylbenzene, etc.; halogenated hydrocarbons such as methylene chloride and chloroform; phenols such as phenol; or mixtures of these can also be used.
[0064] It is preferable that the tubular body has a perforation, which allows it to be opened from the perforation and used as a map film. EXAMPLES
[0065] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples, and it is of course possible to carry out the present invention with modifications within the scope of the above and below-mentioned aims, and all of these modifications are included in the technical scope of the present invention. In the following, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0066] In this example, monolayer films 1 to 8 in Table 2 and laminate films No. 1 to 10 in Table 3 (examples of the present invention with map information) using the monolayer films were produced and evaluated by the following method. Furthermore, a tubular film having perforations was produced using the laminate film 1.
[0067] [Folding angle] (For single layer film) Each film was left for 24 hours in a thermostatic chamber at 20°C and 50% RH. Immediately after that, each film was cut into a 10cm x 10cm square in a 20°C and 65% RH environment and folded in four (2.5cm x 2.5cm squares overlapping). Then, a 5kg weight with a bottom size of 3cm x 3cm was placed on the film folded in four for 20 seconds. After removing the weight, as shown in Figure 1, the sample 1 folded in four was placed on the glass plate 2 so that the four corners of the sample 1 were in contact with the glass plate 2 or located near the glass plate 2 [the apex of the fold (the center of the sample 1 before folding in four) was located away from the glass plate 2], and the angle 3 at which the folded monolayer film opened after 1 minute was measured (the completely folded state was taken as 0 degrees) to determine the folding retention angle. The folding retention angles of both the vertical and horizontal directions of the film were measured in the same manner, and the larger angle was taken as the folding retention angle of the film. In the measurement of the folding retention angle, in the case of a film sample in which the longitudinal and transverse directions of the film were unclear, one direction was provisionally defined as the longitudinal direction, and the direction perpendicular to the provisional longitudinal direction was provisionally defined as the transverse direction. In the table, examples in which the folding retention angle is marked "x" indicate that the folded state could not be maintained after 1 second, despite being folded as described above.
[0068] (In the case of laminated film) For the laminated films, the fold retention angle was measured in the same manner as for the monolayer films above, with the following exceptions. Before folding it into four (2.5cm x 2.5cm squares overlapping), it was first folded in half. At that time, the folding angle was measured when folding it in half so that one side (front side) of the laminated film becomes the mountain fold, and the folding angle was measured when folding it in half so that the other side (back side) of the laminated film becomes the mountain fold. The folding angle when folded in half was measured, and the smaller angle was taken as the folding angle.
[0069] [Printability] (Text information visibility) The visibility of printed text information was evaluated for characters with fonts of 4 pt, 6 pt, and 8 pt. Five characters were selected for each font and evaluated for whether they were visible or not. 〇: All 5 characters are visible △: 1 to 4 characters visible ×: All 5 characters are not visible (Color Overlapping) For overlap evaluation, 5 overlapping areas of 6pt size rectangles (framed) of three colors (cyan, magenta, yellow) were created, and the presence or absence of print color misalignment due to overlapping was visually evaluated. 〇: No color shift in all five areas △: Color shift occurs in 1 to 4 places ×: Color misalignment occurs in all five areas
[0070] [Amorphous component content] The content of amorphous components was determined by dissolving about 5 mg of the sampled film in 0.7 mL of a mixed solution of deuterated chloroform and trifluoroacetic acid (volume ratio 9 / 1) and using 1H-NMR (Varian, UNITY50). Specifically, the proton NMR spectrum of the sample solution was measured under the measurement conditions of a temperature of 23°C and an accumulation number of 64 times.
[0071] In this example, the contents of neopentyl glycol (NPG) and 1,4-cyclohexanedimethanol (CHDM) were determined as amorphous components. More specifically, the contents of each amorphous component were calculated as follows. The monomer type of the constituent unit of the polyhydric alcohol component constituting the polyester in the sample solution was identified by the frequency of the proton peak in the NMR spectrum measurement chart. Then, based on the peak intensity value of a specific proton corresponding to each monomer type, the amount of neopentyl glycol or the amount of 1,4-cyclohexanedimethanol in 100 mol % of the polyhydric alcohol component constituting the polyester in the sample solution was calculated as the content (mol %) of the amorphous component.
[0072] <Synthesis of polyester raw materials> [Synthesis of polyester raw material A] In a stainless steel autoclave equipped with a stirrer, a thermometer, and a partial reflux condenser, 100 mol % of dimethyl terephthalate (DMT) as a dicarboxylic acid component and 100 mol % of ethylene glycol (EG) as a polyhydric alcohol component were charged so that the molar ratio of ethylene glycol was 2.2 times that of dimethyl terephthalate, and 0.05 mol % (relative to the acid component) of zinc acetate was used as an ester exchange catalyst to carry out an ester exchange reaction while distilling off the produced methanol outside the system. Then, 0.225 mol % (relative to the acid component) of antimony trioxide was added as a polycondensation catalyst, and a polycondensation reaction was carried out at 280°C under reduced pressure of 26.7 Pa to obtain a polyester raw material A with an intrinsic viscosity of 0.75 dl / g. This polyester raw material A is polyethylene terephthalate. The composition of the monomer components of polyester raw material A is shown in Table 1.
[0073] In Table 1, TPA is terephthalic acid, BD is 1,4-butanediol, NPG is neopentyl glycol, CHDM is 1,4-cyclohexanedimethanol, DEG is diethylene glycol, and ε-CL is ε-caprolactone. In Table 1, the "Acid component" column shows the content of the monomer component (TPA in Table 1) in 100 mol % of all acid components, and the "Polyhydric alcohol component" and "Ester component" columns show the content of each monomer component in the total of 100 mol % of all polyhydric alcohol components and all ester components.
[0074] [Synthesis of polyester raw materials B to F] Polyester raw materials B to F with different monomer components were obtained according to the same procedure as for polyester raw material A. Polyester raw material F was produced by adding SiO2 (Silysia 266 manufactured by Fuji Silysia Corporation) as a lubricant at a ratio of 7,000 ppm to the polyester. Each polyester was appropriately formed into chips. The composition of these monomer components is shown in Table 1. The intrinsic viscosity of each polyester raw material was B: 0.71 dl / g, C: 0.79 dl / g, D: 1.20 dl / g, E: 0.77 dl / g, and F: 0.75 dl / g, respectively.
[0075] [Table 1]
[0076] <Production of monolayer film> (Production of Film 1) The polyester raw material A, polyester raw material B, polyester raw material D, and polyester raw material F were mixed in a mass ratio of 5:60:30:5 and fed into an extruder. The mixed resin was then melted at 280°C, extruded from a T-die, and rapidly cooled by being wound around a rotating metal roll cooled to a surface temperature of 30°C to obtain an unstretched film having a thickness of 240 μm. The take-up speed of the unstretched film (the rotation speed of the metal roll) was about 20 m / min. Next, the unstretched film was introduced into a tenter (first tenter) having a transverse stretching zone, an intermediate zone, and an intermediate heat treatment zone in succession. In the intermediate zone, the hot air from the stretching zone and the hot air from the heat treatment zone were controlled to be blocked so that when a strip of paper was hung down without passing through the film, the paper would hang down almost completely in the vertical direction.
[0077] The unstretched film introduced into the first tenter was preheated until the film temperature reached 80°C, then stretched 4 times in the transverse direction at 70°C in the transverse stretching zone, passed through the intermediate zone (passage time = approximately 1.2 seconds), and then introduced into the intermediate heat treatment zone where it was heat-treated at a temperature of 80°C for 8 seconds to obtain a transverse uniaxially stretched film with a thickness of 60 μm.
[0078] The transversely uniaxially stretched film was then introduced into a longitudinal stretching machine having a plurality of rolls arranged in series, preheated on a preheating roll until the film temperature reached 70°C, and then stretched three times. The longitudinally stretched film was then forcibly cooled by a cooling roll whose surface temperature was set to 25°C.
[0079] The cooled film was then introduced into a tenter (second tenter) where it was heat-treated in an atmosphere of 100°C for 10 seconds. Thereafter, it was cooled and both edges were cut and removed, thereby continuously producing a biaxially stretched film having a thickness of 20 μm over a predetermined length, thereby obtaining a film roll made of film 1.
[0080] (Production of Film 2) A film roll made of film 2 having a thickness of 20 μm was obtained in the same manner as film 1, except that polyester raw material B in film 1 was changed to polyester raw material C.
[0081] (Production of Film 3) A film roll made of film 3 having a thickness of 20 μm was obtained in the same manner as film 1, except that polyester raw material D in film 1 was changed to polyester raw material E.
[0082] (Production of Film 4) In the above-mentioned Film 1, the thickness of the unstretched film was changed to 80 μm, and the film was stretched only in the transverse direction without carrying out the longitudinal stretching and final heat treatment, to obtain a film roll made of Film 4 having a thickness of 20 μm.
[0083] (Production of Film 5) A film roll made of film 5 having a thickness of 20 μm was obtained in the same manner as film 1, except that in the above film 1, the weight ratio of polyester raw material B was changed from 60 to 80, and the weight ratio of polyester raw material D was changed from 30 to 10.
[0084] (Production of Film 6) A film roll made of film 6 having a thickness of 20 μm was obtained in the same manner as film 1, except that in the above film 1, the weight ratio of polyester raw material A was changed from 5 to 35, and the weight ratio of polyester raw material B was changed from 60 to 50.
[0085] (Production of Film 7) A film roll made of Film 7 having a thickness of 40 μm was obtained in the same manner as Film 1, except that the film thickness of Film 1 was changed from 20 μm to 40 μm.
[0086] (Production of Film 8) A film roll made of Film 8 having a thickness of 12 μm was obtained in the same manner as Film 1, except that the film thickness of Film 1 was changed from 20 μm to 12 μm.
[0087] (Production of Film 9) The film 9 is a biaxially oriented polyethylene terephthalate film (E5100, manufactured by Toyobo Co., Ltd., thickness 12 μm).
[0088] (Manufacture of Film 10) The film 10 is a biaxially oriented polypropylene film (P2161, manufactured by Toyobo Co., Ltd., thickness 20 μm).
[0089] The properties of the thus obtained films 1 to 10 (single layer films) were evaluated by the above-mentioned methods and are shown in Table 2.
[0090] [Table 2A]
[0091] [Table 2B]
[0092] As shown in Table 2, all of the films 1 to 8 have a folding angle of 80 degrees or less and have good properties. Among these, film 5 in particular has the highest content of amorphous components, so the folding properties are The folding retention angle was 24 degrees, giving it the best folding retention performance. In contrast, Film 9 is a polyethylene terephthalate film that does not contain amorphous components, and has a folded-up angle of 100 degrees, which is inferior to Films 1-8 above in terms of folded-up retention performance. Furthermore, film 10 was also a polypropylene film containing no amorphous components, and even though it was folded, it was unable to maintain the folded state.
[0093] <Manufacturing of laminated film> Using the above films 1 to 10, laminate films No. 1 to 12 with map information applied thereto were manufactured as follows. Of these, No. 1 to 10 and 12 are examples having a single layer of printed area, and No. 11 is an example having a two layer printed area.
[0094] (No.1 Production) The above film 1 was digitally printed with LEP ink using a digital printer Indigo 20000 manufactured by Hewlett-Packard to print map information of the Expo site. This map information includes designs of pavilions, plazas, passageways, entrances and exits, shops, restaurants, toilets, parking lots, stations, bus stops, surrounding roads, etc., and each zone in the site is color-coded. The text information was printed in a size range of 4pt to 8pt, and two overlapping areas of three colors (cyan, magenta, yellow) in a 6pt size medium-filled rectangle were provided for overlapping evaluation. Separately from the above, a urethane-based two-component curing adhesive [Takelac (registered trademark) A525S and Takenate (registered trademark) A50 manufactured by Mitsui Chemicals, Inc.] and ethyl acetate (manufactured by Nacalai Tesque, Inc.) were applied to film 1 in a mass ratio of 13.5:1:8.8 using a wire bar #5 to a thickness of 3 μm, and then the film was left to stand in a 60° C. oven for 30 seconds to evaporate the solvent. Then, using a dry lamination method, the printed side of film 1 with the above printing was bonded to the adhesive layer side of film 1 with the above adhesive applied, and after seasoning at 40°C for 3 days, it was cut into a rectangle of 210 mm x 297 mm (area 623.7 cm2) to produce No. 1 laminated film (map film).
[0095] (Production of No. 2 to 10) Laminated films No. 2 to 10 were produced in the same manner as in No. 1, except that films 2 to 10 were used instead of film 1 in No. 1.
[0096] (Production of No.11) The above film 1 was digitally printed with LEP ink using a digital printer Indigo 20000 manufactured by Hewlett-Packard to print map information of the Expo site. This map information includes designs of pavilions, plazas, passageways, entrances and exits, shops, restaurants, toilets, parking lots, stations, bus stops, surrounding roads, etc., and each zone in the site is color-coded. The text information was printed in a size range of 4pt to 8pt, and two overlapping areas of three colors (cyan, magenta, yellow) in a 6pt size medium-filled rectangle were provided for overlapping evaluation. Separately, the above film 1 was digitally printed with LEP ink using a digital printer Indigo 20000 manufactured by Hewlett-Packard, and arrows indicating the recommended model tour course were printed (printed film 1-2). By superimposing these printed films 1-1 and 1-2, a pattern is formed in which both map information of the exhibition site and information showing a recommended model tour course can be visually recognized.
[0097] A urethane-based two-component curing adhesive [Takelac (registered trademark) A525S and Takenate (registered trademark) A50 manufactured by Mitsui Chemicals, Inc.] and ethyl acetate (manufactured by Nacalai Tesque, Inc.) were applied to the printed side of the above-mentioned printed film 1-1 in a mass ratio of 13.5:1:8.8 using a wire bar #5 to a thickness of 3 μm, and then the coating was left to stand in a 60°C oven for 30 seconds to evaporate the solvent. Then, using a dry lamination method, the printed side of the printed film 1-2 with the above printing was bonded to the adhesive layer side of the printed film 1-1 with the above adhesive applied, and after seasoning at 40°C for 3 days, it was cut into a rectangular shape of 210 mm x 297 mm (area 623.7 cm2) to produce No. 11 laminated film (map film).
[0098] (Production of No.12) On the above film 1, map information of the Expo site was printed by gravure printing using "Shrink Pack" (registered trademark) manufactured by Sakata Inx Corporation as printing ink. This map information includes designs of pavilions, plazas, passageways, entrances and exits, shops, restaurants, toilets, parking lots, stations, bus stops, surrounding roads, etc., and each zone in the site is color-coded. The text information was printed in a size range of 4pt to 8pt, and two overlapping areas of three colors (cyan, magenta, yellow) in a 6pt size medium-filled rectangle were provided for overlapping evaluation.
[0099] The properties of the thus obtained laminated films Nos. 1 to 11 were evaluated by the above-mentioned methods. The results are shown in Table 3.
[0100] [Table 3]
[0101] From Table 3, it can be seen that the laminated films No. 1 to 8 and No. 11 using films 1 to 8 (single layer films) that satisfy the requirements of the present invention all have a folding angle of 80 degrees or less, making them easy to fold and excellent in shape retention after folding. In addition, no defects were observed in the appearance of the printed part of the folded part. Furthermore, when the film was folded in eight and placed in a clothing pocket, then taken out and unfolded, the cycle was repeated 35 times, and the map information was still clearly visible after the repeated test.Furthermore, when the film after the repeated test was immersed in water controlled at 23°C±3°C for 24 hours and then taken out, the map information was still clearly visible.
[0102] In contrast, the laminate films Nos. 9 and 10 using the comparative films 9 and 10 which do not satisfy the requirements of the present invention have the following problems. First, the folding angle of No. 9 was 120 degrees, which was larger than those of Nos. 1 to 8. Therefore, the film was difficult to fold, had poor folding processability, and was poor in shape retention after folding. In addition, a test was conducted in which the film was folded in eighths, placed in a clothing pocket, then taken out and unfolded 35 times. After the repeated tests, wrinkles had appeared in some parts of the film, making some of the map information difficult to see.
[0103] The folding retention angle of No. 10 was rated as ×, and the folded state could not be maintained, similar to the single layer film of Film 10. The above film had poor folding processability because it did not have a crease, and could not retain its shape after folding, so it could not be smoothly taken out or put in a clothing pocket. In addition, after the test was repeated 35 times, the entire surface of the film was wrinkled and the map information was difficult to read. In addition, it was confirmed that the ink peeled off in some of the folded areas.
[0104] For No. 12, the folding angle was good, but the 4pt text information was unclear and unreadable, and misalignment occurred in the overlapping areas. Furthermore, when the above film was folded in eight, put into a clothing pocket, and then taken out and unfolded 35 times, it was confirmed that the ink peeled off in some of the folded areas after the repeated test. [Industrial Applicability]
[0105] According to the present invention, a map film can be obtained that has excellent water resistance against water, rain, etc., and exhibits excellent folded-up retention performance after storage for 24 hours in an environment of 20° C. The map film of the present invention can be suitably used in particular for various portable maps. [Explanation of symbols]
[0106] 1 Sample 2 Glass plate 3 angles
Claims
1. The map film has a plastic film and a printed portion consisting of a digitally printed layer containing map information, and is characterized in that the folded angle of the printed portion is 90 degrees or less after being stored for 24 hours in an environment of 20°C.
2. The map film according to claim 1 , wherein the map information includes characters of a size of 4 pt or less.
3. 2. The map film according to claim 1, further comprising a printed portion between two plastic films.
4. 2. The map film according to claim 1, wherein the plastic film is a transparent or semi-transparent plastic film.
5. 2. The map film of claim 1, wherein said plastic film is a polyester film.
6. The polyester film contains ethylene terephthalate units in an amount of 50 mol % or more based on 100 mol % of all ester units, 6. A map film as described in claim 5, which is composed of a polyester resin in which the sum of the proportion of amorphous alcohol components in 100 mol% of total alcohol components and the proportion of amorphous acid components in 100 mol% of total acid components is 12 mol% or more and 30 mol% or less.
7. 2. The map film according to claim 1, wherein the map information includes at least one type of information selected from the group consisting of exhibition centers, ski resorts, campsites, tourist spots, theme parks, amusement parks, golf courses, beaches, swimming pools, baseball stadiums, athletic stadiums, marathon venues, outdoor sports facilities, accommodation facilities, and shopping malls.
8. 2. The map film of claim 1, having a folded configuration.
Citation Information
Patent Citations
Map film
JP2019077094A
Outdoor goods made of paper with a normal temperature glass coating layer
JP3066036U
Map print sheets and handouts
JP3185924U