High-smoothness CPP thin film for lithium battery packaging aluminum plastic film and preparation method of high-smoothness CPP thin film
By adopting the heat sealing structure of random copolymerized polypropylene, block copolymerized polypropylene and modified silica in aluminum-plastic film, the problem of increased friction coefficient during the shell punching of aluminum-plastic film is solved, and film damage is reduced and Deformation, and simplify production processes and reduce costs.
Patent Information
- Application Number
- CN202411122300.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
The friction coefficient of existing aluminum-plastic films increases during the shell punching process, resulting in adhesion and uneven stress when the shell punching mold and aluminum-plastic film are combined, resulting in damage and deformation of the film. After heat sealing, additional slip agent is required to be applied to increase the process. Complexity and cost.
The composite layer, core layer and heat sealing layer structure are arranged in sequence. The heat sealing layer consists of random copolymer polypropylene, block copolymer polypropylene, and modified silica. The modified silica is alkened and original. Position polymerization modification reduces friction coefficient and improves adhesion resistance, and omits the step of applying slip agent after heat sealing.
It effectively reduces the friction coefficient during aluminum-plastic film shell punching, reduces the damage and deformation of the film during mold shell punching, simplifies the production process, reduces costs, and improves the anti-adhesion and smoothness of the film.
Smart Images

Figure BDA0004995433370000171
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of packaging materials, and in particular to a highly smooth CPP film for lithium battery packaging aluminum-plastic film and a preparation method thereof. Background Art
[0002] Lithium-ion battery is a battery that can be charged and discharged into a load and used in multiple cycles. It consists of one or more electrochemical cells and is the basic power source for many portable telecommunication devices. The rapid development of mobile electronic devices such as mobile phones, laptops and PDAs has brought about an increase in the demand for secondary batteries. Therefore, secondary battery technology has become increasingly important recently and has become a core industry for components of information technology equipment. In addition, there is an increasing demand for lightweight, compact but better-performing electronic devices, which require lighter, smaller, thinner and longer-running secondary batteries. Especially those medium or large mobile devices require a large amount of power consumption to achieve long-lasting operation.
[0003] Currently, there are many kinds of lithium battery packaging materials on the market, such as steel shell, aluminum shell, and plastic shell, but aluminum-plastic film has been widely used in many fields such as 3C electronics due to its advantages of light weight, thin thickness, flexible appearance design, and 360-degree arbitrary placement of soft-pack batteries. Aluminum-plastic composite film (abbreviated as "aluminum-plastic film") is a composite material composed of aluminum foil, various plastics and adhesives (including adhesive resins). It is a key material for soft-pack lithium battery cell packaging. After the single-chip battery is assembled, it is sealed with aluminum-plastic film to protect the contents. It consists of five layers, including outer nylon layer + adhesive + middle layer aluminum foil + adhesive + inner layer heat seal layer, and each layer has relatively high functional requirements.
[0004] There are two main methods for preparing aluminum-plastic film: dry method and hot method. The dry method is to coat the substrate with adhesive and then dry it and then directly compound it with heat-sealing materials. It has low requirements on equipment, but the process is complicated and difficult to operate. The aluminum-plastic film products have good deep forming performance, anti-short circuit performance, excellent appearance (few impurities, pinholes and fish eyes), good electrolyte resistance, water barrier performance and cutting performance, and are used in high energy density, high rate and high capacity batteries; the hot method is to extrude hot-melt resin as adhesive to compound the substrate and heat-sealing materials. It has higher requirements on equipment and can only be imported from abroad. The process is simple, the production efficiency is high, and no waste gas treatment facilities are required. The aluminum-plastic film products have good electrolyte resistance and water barrier performance, poor deep forming performance and short circuit resistance, poor appearance and cutting performance, and are mainly used in batteries with low capacity requirements.
[0005] When aluminum-plastic film is used for battery molding, the friction coefficient of the polypropylene film surface is too high, which will cause the depth of the aluminum-plastic film to not meet the production requirements, and the heat sealing effect between the polypropylene films is not good during heat sealing, thus affecting the electrolyte resistance of the aluminum-plastic composite film. The lubricant will migrate to the surface of the film to play a lubricating role, thereby reducing the friction coefficient. In existing reports, amides, silicon dioxide, etc. are often added as additives to the polypropylene film layer to reduce the friction coefficient.
[0006] Chinese patent document CN114248523A discloses a cast polypropylene film and an aluminum-plastic film, wherein the cast polypropylene film comprises an adhesive layer, a core layer and a heat-sealing layer stacked in sequence, and the material forming the heat-sealing layer comprises 50 to 60 parts by weight of random copolymer polypropylene, 30 to 40 parts by weight of block copolymer polypropylene, 0.7 to 3.5 parts by weight of a lubricant, and 0.4 to 1.0 parts by weight of silicon dioxide; wherein the lubricant comprises an organic silicone lubricant and an amide lubricant.
[0007] The process of punching the shell of soft-pack lithium batteries in the manufacturing process is to punch the aluminum-plastic film into a certain shape through a punching machine. At present, the compensatory punching method is generally used. This method must ensure that the aluminum-plastic film can slide well during the punching process, so the CPP heat-sealing cover of the punching mold and the aluminum-plastic film is required to have good slipperiness, that is, a low friction coefficient μ≤0.3. The commonly used erucic acid amide lubricant has a low melting point, so it precipitates and volatilizes in large quantities during the aluminum-plastic composite and subsequent aging process. After composite aging, the friction coefficient of the heat-sealing cover will exceed 0.3, which will cause the shell to break or deform. In order to solve this problem, the prior art generally applies a layer of lubricant on the surface after heat sealing. On the one hand, it will increase the process flow and cost, and on the other hand, the coating amount cannot be accurately controlled (if the coating is too little, the friction coefficient will still be high, and if the coating is too much, powder will fall off). Summary of the invention
[0008] In order to solve the deficiencies in the prior art, the purpose of the present invention is to provide a highly slippery CPP film for lithium battery encapsulation aluminum-plastic film and a preparation method thereof, which solves the problem of increased friction coefficient of the CPP film after compounding, inhibits adhesion and uneven force during the aging of the aluminum-plastic film, effectively reduces the damage and deformation of the film during the mold punching process, and omits the process of applying a lubricant after heating and aging the CPP film, thereby saving production costs.
[0009] In order to achieve the above object, the present invention adopts the following technical solution:
[0010] A highly smooth CPP film for lithium battery encapsulation aluminum-plastic film comprises a composite layer, a core layer and a heat-sealing layer which are sequentially stacked. The heat-sealing layer is made of the following components in parts by weight: 40 to 75 parts of random copolymer polypropylene, 2 to 10 parts of block copolymer polypropylene, 10 to 47 parts of EVA and 3 to 12 parts of modified silicon dioxide.
[0011] Preferably, the heat-sealing layer is made of the following components in parts by weight: 60 parts of random copolymer polypropylene, 6 parts of block copolymer polypropylene, 32 parts of EVA, and 9 parts of modified silica.
[0012] Preferably, the core layer is made of the following components in parts by weight: 15 to 40 parts of random copolymer polypropylene, 20 to 40 parts of block copolymer polypropylene, and 20 to 65 parts of POE.
[0013] More preferably, the core layer is made of the following components in parts by weight: 25 parts of random copolymer polypropylene, 30 parts of block copolymer polypropylene, and 55 parts of POE.
[0014] Preferably, the composite layer is made of the following components in parts by weight: 30-60 parts of binary copolymer polypropylene, 10-40 parts of EVA, and 8-30 parts of maleic anhydride grafted polypropylene.
[0015] More preferably, the composite layer is made of the following components in parts by weight: 45 parts of binary copolymer polypropylene, 25 parts of EVA, and 20 parts of maleic anhydride grafted polypropylene.
[0016] Preferably, the total thickness of the CPP film is 20 to 100 μm;
[0017] Specifically, the total thickness of the CPP film can be 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, or 100 μm;
[0018] Preferably, the thickness of the composite layer is 10% to 30% of the total thickness of the CPP film;
[0019] Specifically, the thickness of the composite layer may be 10%, 15%, 20%, 25%, or 30% of the total thickness of the CPP film;
[0020] Preferably, the thickness of the heat-sealing layer is 10% to 30% of the total thickness of the CPP film.
[0021] Specifically, the thickness of the heat-sealing layer may be 10%, 15%, 20%, 25%, or 30% of the total thickness of the CPP film.
[0022] Preferably, the weight percentage of ethylene in the random copolymer polypropylene is 1-7%, and the melting point is 135-145°C; the weight percentage of ethylene in the block copolymer polypropylene is 7-15%, and the melting point is 155-165°C.
[0023] Preferably, the preparation method of the modified silicon dioxide comprises the following steps:
[0024] (1) dispersing silica in an ethanol / water mixture, then adding 3-(methacryloyloxy)propyltrimethoxysilane, stirring for reaction, filtering, washing, and drying the product to obtain olefinated silica;
[0025] (2) dispersing olefinated silica in methyl isobutyl ketone, then adding perfluoroalkyl ethyl acrylate, allyl acrylate, and erucic acid amide, ultrasonically treating, slowly adding azobisisobutyronitrile under stirring, introducing nitrogen to remove air, heating to carry out polymerization reaction, precipitating the product with n-hexane, washing, and freeze-drying to obtain the modified silica.
[0026] Preferably, in step (1), the particle size of the silicon dioxide is 30 to 100 nm.
[0027] Specifically, in step (1), the particle size of the silicon dioxide can be 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, or 100 nm.
[0028] Preferably, in step (1), the ethanol / water mixture is obtained by mixing anhydrous ethanol and deionized water in a volume ratio of 10:4-8, and the amount ratio of silicon dioxide, ethanol / water mixture and 3-(methacryloyloxy)propyltrimethoxysilane is 10g:100mL:1-5g.
[0029] Preferably, in step (1), the stirring reaction condition is 50-65° C. for 1-4 h.
[0030] Specifically, in step (1), the stirring reaction temperature can be 50°C, 53°C, 56°C, 59°C, 62°C, or 65°C;
[0031] Specifically, in step (1), the stirring reaction time can be 1 h, 2 h, 3 h, or 4 h.
[0032] Preferably, in step (2), the ultrasonic treatment time is 10 to 30 minutes, and the polymerization reaction conditions are polymerization at 50 to 65° C. for 12 to 20 hours.
[0033] Specifically, in step (2), the ultrasonic treatment time can be 10 min, 20 min, or 30 min.
[0034] Specifically, in step (2), the polymerization reaction temperature can be 50°C, 53°C, 56°C, 59°C, 62°C, or 65°C; and the polymerization reaction time can be 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, or 20h.
[0035] Preferably, in step (2), the mass ratio of olefinated silica, perfluoroalkylethyl acrylate, allyl acrylate and erucamide is 10:2-6:0.5-3:3-8; and the amount of azobisisobutyronitrile is 0.1-1% of the total mass of the monomers.
[0036] The present invention also claims protection for a method for preparing a highly smooth CPP film for lithium battery encapsulation aluminum-plastic film, comprising the following steps: melting the raw materials according to the formula through three single-screw extruders respectively, and then passing through a batching block connector, a die head for co-extrusion, and cast film formation. The product is subsequently cooled and shaped, thickness detected, online slitting, winding and packaging to obtain the anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] 1) The present invention provides a high-smooth CPP film for lithium battery encapsulation aluminum-plastic film, which is made of a composite layer, a core layer, and a heat-sealing layer stacked in sequence. The heat-sealing layer adopts block copolymer polypropylene, random copolymer polypropylene, TPE, and modified silica. The block copolymer polypropylene is formed by alternating polymerization of propylene and ethylene segments and has good low-temperature impact resistance. The random copolymer polypropylene is a random copolymer of propylene and ethylene. The addition of ethylene monomer in the polypropylene molecular chain can improve its impact resistance and transparency. The random copolymer polypropylene with a melting point between 135 and 145°C and the random copolymer polypropylene with a melting point between 155 and 165°C are used. ℃ block copolymer polypropylene, after the two are mixed at high temperature, the regular polymer chain segments are disrupted, and the polymer crystallinity decreases after cooling, resulting in a lower melting point of the mixed mixture, thereby enabling the heat-sealing layer to maintain a suitable initial heat-sealing temperature; modified silica can give the CPP film excellent anti-adhesion, smoothness and mechanical strength, and significantly reduce the precipitation and volatilization of the lubricant during the heat sealing and aging process, thereby solving the problem of increased friction coefficient of the CPP film after compounding, inhibiting the adhesion and uneven force of the aluminum-plastic film during aging, and effectively reducing the damage and deformation of the film during the mold shell punching process.
[0039] 2) The present invention provides a modified silica. First, 3-(methacryloyloxy)propyltrimethoxysilane is used to organically modify silica, and organic long chains and unsaturated double bonds are grafted onto the surface of nano-silica. Then, methyl isobutyl ketone is used as a solvent, allyl acrylate is used as a cross-linking agent, and azobisisobutyronitrile is used as an initiator to cause perfluoroalkyl ethyl acrylate and erucic acid amide to be in situ polymerized on the surface of nano-silica. The introduced erucic acid amide is a commonly used lubricant, which can quickly migrate to the surface of the CPP film to form a lubricating film, thereby reducing the friction coefficient of the film surface and reducing the mutual adhesion between the films. Adhesion; the introduced fluoroalkyl group has good anti-sticking and weather resistance, and can cooperate with erucamide to increase the lubricity of the film, further improving the anti-sticking and slippery properties of the CPP film; nano-silica is modified by in-situ polymerization, and a large number of organic functional groups are introduced on its surface, which can significantly improve the compatibility between the inorganic powder and the resin matrix, so that it can be evenly dispersed in the polypropylene, thereby giving full play to the slippery effect of erucamide and fluoroalkyl groups, and effectively avoiding the migration and precipitation of erucamide and the poor durability problems, which can effectively solve the damage and deformation problems of the film during the aluminum-plastic composite curing process. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0041] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from commercial sources or synthesized from raw materials purchased from commercial sources.
[0042] Maleic anhydride grafted polypropylene was purchased from Coase Chemical Co., Ltd., model B1A;
[0043] The binary copolymer polypropylene was provided by Samsung of South Korea, with the trade name RF402;
[0044] EVA was purchased from Shanghai Fuchen Plastic Raw Materials Co., Ltd., brand number Japan Mitsui 420;
[0045] POE was purchased from Mitsui Chemicals, brand DF840.
[0046] A method for preparing a highly smooth CPP film for lithium battery encapsulation aluminum-plastic film, comprising the following steps:
[0047] (1) dispersing 10 g of silica into 100 mL of an ethanol / water mixture (prepared by mixing anhydrous ethanol and deionized water in a volume ratio of 10:4-8), then adding 1-5 g of 3-(methacryloyloxy)propyltrimethoxysilane, stirring and reacting at 50-65° C. for 1-4 h, filtering, washing, and drying the product to obtain olefinated silica;
[0048] (2) dispersing 10 g of olefinated silica in 100-200 mL of methyl isobutyl ketone, then adding 2-6 g of perfluoroalkyl ethyl acrylate, 0.5-3 g of allyl acrylate, and 3-8 g of erucic acid amide, ultrasonically treating for 10-30 min, slowly adding azobisisobutyronitrile (in an amount of 0.1-1% of the total mass of the monomer) under stirring, introducing nitrogen to remove air, heating to 50-65° C. for polymerization for 12-20 h, precipitating the product with n-hexane, washing, and freeze-drying to obtain the modified silica;
[0049] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain the anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film.
[0050] The heat-sealing layer is made of the following components in parts by weight: 40-75 parts of random copolymer polypropylene, 2-10 parts of block copolymer polypropylene, 10-47 parts of EVA, and 3-12 parts of modified silicon dioxide; the thickness of the heat-sealing layer is 10%-30% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 15-40 parts of random copolymer polypropylene, 20-40 parts of block copolymer polypropylene, and 20-65 parts of POE; the composite layer is made of the following components in parts by weight: 30-60 parts of binary copolymer polypropylene, 10-40 parts of EVA, and 8-30 parts of maleic anhydride grafted polypropylene, and the thickness of the composite layer is 10%-30% of the total thickness of the CPP film.
[0051] The present invention will be further described below through specific embodiments.
[0052] Example 1
[0053] A method for preparing a highly smooth CPP film for lithium battery encapsulation aluminum-plastic film, comprising the following steps:
[0054] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (anhydrous ethanol and deionized water were mixed in a volume ratio of 10:8), and then 5 g of 3-(methacryloyloxy)propyltrimethoxysilane was added, and the mixture was stirred at 65° C. for 1 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0055] (2) 10 g of olefinated silica was dispersed in 150 mL of methyl isobutyl ketone, and then 6 g of perfluoroalkyl ethyl acrylate, 3 g of allyl acrylate, and 8 g of erucic acid amide were added, and ultrasonic treatment was performed for 30 min. 0.15 g of azobisisobutyronitrile was slowly added under stirring, and nitrogen was introduced to remove air. The temperature was raised to 65° C. and polymerized for 12 h. The product was precipitated with n-hexane, washed, and freeze-dried to obtain the modified silica;
[0056] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain the 61 μm anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film.
[0057] The heat-sealing layer is made of the following components in parts by weight: 60 parts of random copolymer polypropylene, 6 parts of block copolymer polypropylene, 32 parts of EVA, and 12 parts of modified silica; the thickness of the heat-sealing layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 25 parts of random copolymer polypropylene, 30 parts of block copolymer polypropylene, and 55 parts of POE; the composite layer is made of the following components in parts by weight: 45 parts of binary copolymer polypropylene, 25 parts of EVA, and 20 parts of maleic anhydride grafted polypropylene, and the thickness of the composite layer is 30% of the total thickness of the CPP film.
[0058] Example 2
[0059] A method for preparing a highly smooth CPP film for lithium battery encapsulation aluminum-plastic film, comprising the following steps:
[0060] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (anhydrous ethanol and deionized water were mixed in a volume ratio of 10:6), and then 4 g of 3-(methacryloyloxy)propyltrimethoxysilane was added, and the mixture was stirred at 60° C. for 2 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0061] (2) 10 g of olefinated silica was dispersed in 150 mL of methyl isobutyl ketone, and then 5 g of perfluoroalkyl ethyl acrylate, 2 g of allyl acrylate, and 7 g of erucic acid amide were added, and ultrasonic treatment was performed for 20 min. 0.1 g of azobisisobutyronitrile was slowly added under stirring, and nitrogen was introduced to remove air. The temperature was raised to 60° C. and polymerized for 14 h. The product was precipitated with n-hexane, washed, and freeze-dried to obtain the modified silica;
[0062] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain the 54 μm anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film.
[0063] The heat-sealing layer is made of the following components in parts by weight: 60 parts of random copolymer polypropylene, 6 parts of block copolymer polypropylene, 32 parts of EVA, and 9 parts of modified silica; the thickness of the heat-sealing layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 25 parts of random copolymer polypropylene, 30 parts of block copolymer polypropylene, and 55 parts of POE; the composite layer is made of the following components in parts by weight: 45 parts of binary copolymer polypropylene, 25 parts of EVA, and 20 parts of maleic anhydride grafted polypropylene, and the thickness of the composite layer is 30% of the total thickness of the CPP film.
[0064] Example 3
[0065] A method for preparing a highly smooth CPP film for lithium battery encapsulation aluminum-plastic film, comprising the following steps:
[0066] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (anhydrous ethanol and deionized water were mixed in a volume ratio of 10:6), and then 3 g of 3-(methacryloyloxy)propyltrimethoxysilane was added, and the mixture was stirred at 55° C. for 3 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0067] (2) 10 g of olefinated silica was dispersed in 150 mL of methyl isobutyl ketone, and then 3 g of perfluoroalkylethyl acrylate, 1 g of allyl acrylate, and 4 g of erucic acid amide were added, and ultrasonic treatment was performed for 20 min. 0.05 g of azobisisobutyronitrile was slowly added under stirring, and nitrogen was introduced to remove air. The temperature was raised to 55° C. and polymerized for 18 h. The product was precipitated with n-hexane, washed, and freeze-dried to obtain the modified silica;
[0068] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain the 52 μm anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film.
[0069] The heat-sealing layer is made of the following components in parts by weight: 60 parts of random copolymer polypropylene, 6 parts of block copolymer polypropylene, 32 parts of EVA, and 6 parts of modified silica; the thickness of the heat-sealing layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 25 parts of random copolymer polypropylene, 30 parts of block copolymer polypropylene, and 55 parts of POE; the composite layer is made of the following components in parts by weight: 45 parts of binary copolymer polypropylene, 25 parts of EVA, and 20 parts of maleic anhydride grafted polypropylene, and the thickness of the composite layer is 30% of the total thickness of the CPP film.
[0070] Example 4
[0071] A method for preparing a highly smooth CPP film for lithium battery encapsulation aluminum-plastic film, comprising the following steps:
[0072] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (anhydrous ethanol and deionized water were mixed in a volume ratio of 10:4), and then 1 g of 3-(methacryloyloxy)propyltrimethoxysilane was added, and the mixture was stirred at 50° C. for 4 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0073] (2) 10 g of olefinated silica was dispersed in 150 mL of methyl isobutyl ketone, and then 2 g of perfluoroalkyl ethyl acrylate, 0.5 g of allyl acrylate, and 3 g of erucic acid amide were added, and ultrasonic treatment was performed for 10 min. 0.05 g of azobisisobutyronitrile was slowly added under stirring, and nitrogen was introduced to remove air. The temperature was raised to 50° C. and polymerized for 20 h. The product was precipitated with n-hexane, washed, and freeze-dried to obtain the modified silica;
[0074] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain the 58 μm anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film.
[0075] The heat-sealing layer is made of the following components in parts by weight: 60 parts of random copolymer polypropylene, 6 parts of block copolymer polypropylene, 32 parts of EVA, and 3 parts of modified silica; the thickness of the heat-sealing layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 25 parts of random copolymer polypropylene, 30 parts of block copolymer polypropylene, and 55 parts of POE; the composite layer is made of the following components in parts by weight: 45 parts of binary copolymer polypropylene, 25 parts of EVA, and 20 parts of maleic anhydride grafted polypropylene, and the thickness of the composite layer is 30% of the total thickness of the CPP film.
[0076] Comparative Example 1
[0077] A method for preparing a highly smooth CPP film for lithium battery encapsulation aluminum-plastic film, comprising the following steps:
[0078] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (anhydrous ethanol and deionized water were mixed in a volume ratio of 10:8), and then 5 g of 3-(methacryloyloxy)propyltrimethoxysilane was added, and the mixture was stirred at 65° C. for 1 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0079] (2) dispersing 10 g of olefinated silica in 150 mL of methyl isobutyl ketone, then adding 6 g of perfluoroalkyl ethyl acrylate and 3 g of allyl acrylate, ultrasonically treating for 30 min, slowly adding 0.15 g of azobisisobutyronitrile under stirring, introducing nitrogen to remove air, heating to 65° C. for polymerization for 12 h, precipitating the product with n-hexane, washing, and freeze-drying to obtain the modified silica;
[0080] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain the 60 μm anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film.
[0081] The heat-sealing layer is made of the following components in parts by weight: 60 parts of random copolymer polypropylene, 6 parts of block copolymer polypropylene, 32 parts of EVA, and 12 parts of modified silica; the thickness of the heat-sealing layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 25 parts of random copolymer polypropylene, 30 parts of block copolymer polypropylene, and 55 parts of POE; the composite layer is made of the following components in parts by weight: 45 parts of binary copolymer polypropylene, 25 parts of EVA, and 20 parts of maleic anhydride grafted polypropylene, and the thickness of the composite layer is 30% of the total thickness of the CPP film.
[0082] Comparative Example 2
[0083] A method for preparing a highly smooth CPP film for lithium battery encapsulation aluminum-plastic film, comprising the following steps:
[0084] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (anhydrous ethanol and deionized water were mixed in a volume ratio of 10:8), and then 5 g of 3-(methacryloyloxy)propyltrimethoxysilane was added, and the mixture was stirred at 65° C. for 1 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0085] (2) 10 g of olefinated silica was dispersed in 150 mL of methyl isobutyl ketone, and then 3 g of allyl acrylate and 8 g of erucic acid amide were added, and the mixture was ultrasonically treated for 30 min. 0.15 g of azobisisobutyronitrile was slowly added under stirring, and nitrogen was introduced to remove air. The mixture was heated to 65° C. and polymerized for 12 h. The product was precipitated with n-hexane, washed, and freeze-dried to obtain the modified silica.
[0086] (3) The raw materials are melted by three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain the 56 μm anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film.
[0087] The heat-sealing layer is made of the following components in parts by weight: 60 parts of random copolymer polypropylene, 6 parts of block copolymer polypropylene, 32 parts of EVA, and 12 parts of modified silica; the thickness of the heat-sealing layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 25 parts of random copolymer polypropylene, 30 parts of block copolymer polypropylene, and 55 parts of POE; the composite layer is made of the following components in parts by weight: 45 parts of binary copolymer polypropylene, 25 parts of EVA, and 20 parts of maleic anhydride grafted polypropylene, and the thickness of the composite layer is 30% of the total thickness of the CPP film.
[0088] Comparative Example 3
[0089] A method for preparing a highly smooth CPP film for lithium battery encapsulation aluminum-plastic film, comprising the following steps:
[0090] (1) 10 g of silica was dispersed in 100 mL of an ethanol / water mixture (anhydrous ethanol and deionized water were mixed in a volume ratio of 10:8), and then 5 g of 3-(methacryloyloxy)propyltrimethoxysilane was added, and the mixture was stirred at 65° C. for 1 h. The product was filtered, washed, and dried to obtain olefinated silica;
[0091] (2) The raw materials are melted through three single-screw extruders according to the formula, and then co-extruded through a batching block connector and a die head, and cast into a film. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up, and packaged to obtain the 56 μm anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film.
[0092] The heat-sealing layer is made of the following components in parts by weight: 60 parts of random copolymer polypropylene, 6 parts of block copolymer polypropylene, 32 parts of EVA, and 12 parts of olefinic silica; the thickness of the heat-sealing layer is 20% of the total thickness of the CPP film; the core layer is made of the following components in parts by weight: 25 parts of random copolymer polypropylene, 30 parts of block copolymer polypropylene, and 55 parts of POE; the composite layer is made of the following components in parts by weight: 45 parts of binary copolymer polypropylene, 25 parts of EVA, and 20 parts of maleic anhydride grafted polypropylene, and the thickness of the composite layer is 30% of the total thickness of the CPP film.
[0093] The performance tests were conducted on the CPP films prepared in Examples 1 to 4 and Comparative Examples 1 to 3. The tensile strength and elongation at break were tested with reference to GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets"; the initial static friction coefficient of the film and the static friction coefficient after storage at 60°C for 30 days were tested with reference to GB / T 10006-2021 "Determination of friction coefficient of plastic films and sheets"; the CPP film stored at 80°C for 30 days was compounded into an aluminum-plastic film and formed into a double pit shape with a single pit length of 4.5 cm × 11.5 cm × 6 mm, and the chamfer of the finished product was observed for pinholes, cracks or delamination. Specific data are shown in Table 1.
[0094] Table 1 Film performance test results
[0095]
[0096] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A highly smooth CPP film for lithium battery encapsulation aluminum-plastic film, comprising a composite layer, a core layer and a heat-sealing layer stacked in sequence, characterized in that: The heat sealing layer is made of the following components in parts by weight: 40 to 75 parts of random copolymer polypropylene, 2 to 10 parts of block copolymer polypropylene, 10 to 47 parts of EVA, and 3 to 12 parts of modified silicon dioxide.
2. The highly smooth CPP film for lithium battery encapsulation aluminum-plastic film according to claim 1, characterized in that: The core layer is made of the following components in parts by weight: 15 to 40 parts of random copolymer polypropylene, 20 to 40 parts of block copolymer polypropylene, and 20 to 65 parts of POE.
3. The highly smooth CPP film for lithium battery encapsulation aluminum-plastic film according to claim 1, characterized in that: The composite layer is made of the following components in parts by weight: 30-60 parts of binary copolymer polypropylene, 10-40 parts of EVA, and 8-30 parts of maleic anhydride grafted polypropylene.
4. The highly smooth CPP film for lithium battery encapsulation aluminum-plastic film according to claim 1, characterized in that: The total thickness of the CPP film is 20-100 μm; the thickness of the composite layer is 10%-30% of the total thickness of the CPP film; and the thickness of the heat-sealing layer is 10%-30% of the total thickness of the CPP film.
5. The highly smooth CPP film for lithium battery encapsulation aluminum-plastic film according to claim 1, characterized in that: The preparation method of the modified silicon dioxide comprises the following steps: (1) dispersing silica in an ethanol / water mixture, then adding 3-(methacryloyloxy)propyltrimethoxysilane, stirring for reaction, filtering, washing, and drying the product to obtain olefinated silica; (2) dispersing olefinated silica in methyl isobutyl ketone, then adding perfluoroalkyl ethyl acrylate, allyl acrylate, and erucic acid amide, ultrasonically treating, slowly adding azobisisobutyronitrile under stirring, introducing nitrogen to remove air, heating to carry out polymerization reaction, precipitating the product with n-hexane, washing, and freeze-drying to obtain the modified silica.
6. The highly smooth CPP film for lithium battery encapsulation aluminum-plastic film according to claim 5, characterized in that: In step (1), the ethanol / water mixture is obtained by mixing anhydrous ethanol and deionized water in a volume ratio of 10:4-8, and the amount ratio of silicon dioxide, ethanol / water mixture and 3-(methacryloyloxy)propyltrimethoxysilane is 10g:100mL:1-5g.
7. The highly smooth CPP film for lithium battery encapsulation aluminum-plastic film according to claim 5, characterized in that: In step (1), the stirring reaction condition is 50-65° C. for 1-4 h.
8. The highly smooth CPP film for lithium battery encapsulation aluminum-plastic film according to claim 5, characterized in that: In step (2), the ultrasonic treatment time is 10 to 30 minutes, and the polymerization reaction conditions are polymerization at 50 to 65° C. for 12 to 20 hours.
9. The highly smooth CPP film for lithium battery encapsulation aluminum-plastic film according to claim 5, characterized in that: In step (2), the mass ratio of olefinated silica, perfluoroalkylethyl acrylate, allyl acrylate and erucamide is 10:2-6:0.5-3:3-8; and the amount of azobisisobutyronitrile is 0.1-1% of the total mass of the monomers.
10. A method for preparing a highly smooth CPP film for lithium battery encapsulation aluminum-plastic film as claimed in any one of claims 1 to 9, characterized in that: The method comprises the following steps: the raw materials are melted respectively through three single-screw extruders according to the formula, and then co-extruded and cast into films through a batching block connector and a die head. The product is subsequently cooled and shaped, thickness tested, slit online, rolled up and packaged to obtain the anti-adhesion CPP film for lithium battery encapsulation aluminum-plastic film.
Citation Information
Cited By
Aluminum-plastic film for long-life lithium battery and production process of aluminum-plastic film
CN122025940A
Anti-sticking smooth master batch for cast film and preparation method of anti-sticking smooth master batch
CN122037398A