Resin composition having gas barrier properties

A resin composition combining saponified ethylene-vinyl acetate, ethylene-vinyl alcohol, and propylene polymers addresses adhesive and barrier issues in packaging laminates, ensuring strong adhesion and gas barrier performance in a cost-effective, multi-purpose manufacturing process.

JP2024165276APending Publication Date: 2024-11-28TOSOH CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023081328
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing resin compositions for packaging materials face challenges in achieving sufficient adhesive strength and gas barrier properties when used in laminates with polypropylene, leading to issues like gelation, reduced product value, and high equipment costs for multilayer molding.

Method used

A resin composition comprising a saponified ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, and propylene polymer, with specific ratios and properties to enhance adhesiveness and gas barrier properties, using a compatibilizer to improve compatibility and a crosslinking agent for stability.

Benefits of technology

The resin composition achieves excellent adhesiveness to polypropylene layers with high gas barrier properties, suitable for three-layer structures producible on general-purpose molding machines, maintaining mechanical properties and preventing gelation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165276000001
    Figure 2024165276000001
  • Figure 2024165276000002
    Figure 2024165276000002
  • Figure 2024165276000003
    Figure 2024165276000003
Patent Text Reader

Abstract

To provide a resin composition containing a saponified ethylene-vinyl acetate copolymer and an ethylene-vinyl alcohol copolymer, exhibiting superior gas barrier properties and adhesive strength, and a laminate made using the same.SOLUTION: A resin composition contains at least a saponified ethylene-vinyl acetate copolymer with a vinyl acetate content of 0.3-20 mol% and a vinyl alcohol content of 1-20 mol% (A), an ethylene-vinyl alcohol copolymer (B) and a propylene polymer (C).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing at least a saponified ethylene-vinyl acetate copolymer, an ethylene-vinyl alcohol copolymer, and a propylene-based polymer. [Background technology]

[0002] Ethylene-vinyl alcohol copolymer (hereinafter sometimes referred to as EVOH), which has excellent gas barrier properties, aroma retention, solvent resistance, etc., is used in various applications as packaging materials made of thermoplastic resins for food, beverages, medicines, etc., to prevent deterioration of the contents. However, EVOH is hydrophilic, and gas barrier properties, etc., decrease due to moisture absorption, so it is generally known to be used as an intermediate layer in laminates with polyolefins, such as polyethylene and polypropylene, which have excellent water resistance, and laminates made of polypropylene are used in applications requiring particularly high transparency and mechanical properties.

[0003] Since EVOH has many hydroxyl groups in the molecule, it has very low affinity with polypropylene, which does not have polar groups, and the two generally do not adhere to each other. For this reason, methods have been proposed for using graft-modified propylene-based resin compositions grafted with unsaturated carboxylic acids or their derivatives (see, for example, Patent Documents 1 and 2) or ethylene-vinyl acetate copolymer hydrolysates (see, for example, Patent Document 3) as adhesives for EVOH, which is difficult to bond to polypropylene.

[0004] However, the former graft-modified propylene resin composition grafted with unsaturated carboxylic acid or its derivative has excellent adhesiveness, but due to its high reactivity with EVOH, when it is repeatedly kneaded or added to EVOH, the resin that remains in the extruder or die increases in viscosity and becomes discolored and gelled, resulting in the presence of many fish eyes and gel-like substances in the product, which reduces the commercial value. In addition, the latter ethylene-vinyl acetate copolymer hydrolyzate does not discolor or gel even when it is repeatedly kneaded or added to EVOH, and although the adhesiveness to EVOH is improved by adding a tackifying resin to the ethylene-vinyl acetate copolymer hydrolyzate, the effect is small, and it often peels off when subjected to small impacts or friction during transportation or use, and sufficient adhesiveness was not obtained.

[0005] Furthermore, packaging materials containing EVOH must be constructed with at least three types and five layers including a polypropylene layer / adhesive layer / EVOH layer / adhesive layer / polypropylene layer, or four types and six layers including a polypropylene layer / adhesive layer / EVOH layer / adhesive layer / regrind layer / polypropylene layer. However, a multilayer molding machine for producing such a multilayer laminate of five or more layers generally has a problem of very high capital investment costs.

[0006] Therefore, there has been a demand for the production of a laminate that can be produced in a three-layer structure using a general-purpose molding machine.For example, Patent Document 4 proposes a method for producing a three-layer structure by using a hydrolyzate of a melt-kneaded product containing a thermoplastic resin, an ethylene-vinyl ester copolymer having a vinyl ester content 5 mol% or more higher than that of the thermoplastic resin, and a modified product in which the thermoplastic resin and the ethylene-vinyl ester copolymer are grafted, and by blending the hydrolyzate with the EVOH layer, the adhesiveness with the polyolefin resin layer is improved. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2000-167998 A [Patent Document 2] JP 2001-277371 A [Patent Document 3] JP 2001-200124 A [Patent Document 4] JP 2017-210608 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, when a laminate produced by actual film molding, direct blow molding, or the like using the resin composition described in Patent Document 4 was evaluated, a problem occurred in which sufficient adhesive strength and gas barrier properties could not be obtained. The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a resin composition that has excellent adhesiveness to a polypropylene layer and also has gas barrier properties. [Means for solving the problem]

[0009] As a result of intensive investigations aimed at solving the above problems, the present inventors have found that a resin composition containing a specific saponified ethylene-vinyl acetate copolymer, EVOH, and a propylene-based polymer can achieve both good adhesion to the propylene-based polymer and high gas barrier properties, thereby completing the present invention.

[0010] That is, the respective aspects of the present invention are as follows [1] to [8]. [1] A resin composition comprising at least (A) a saponified ethylene-vinyl acetate copolymer having a vinyl acetate content of 0.3 to 20 mol% and a vinyl alcohol content of 1.0 to 20 mol%, (B) an ethylene-vinyl alcohol copolymer having an ethylene content of 27 to 48 mol%, and (C) a propylene-based polymer. [2] The resin composition according to [1], wherein a weight ratio ((A+C) / B) of the total ((A+C)) of the saponified ethylene-vinyl acetate copolymer (A) and the propylene-based polymer (C) to the ethylene-vinyl alcohol copolymer (B) is 80 / 20 to 50 / 50. [3] The resin composition according to [1] or [2], wherein the saponified ethylene-vinyl acetate copolymer (A) is a hydrolysate of a kneaded product containing the following components (a1) to (a3) ​​and crosslinked products of the (a1) to (a3), and has a melt mass-flow rate of 0.3 to 5.0 g / 10 min as measured in accordance with JIS K6922-1: (a1) An ethylene-vinyl acetate copolymer having a vinyl acetate content of 20% by weight or less (a2) Ethylene-vinyl acetate copolymer having a vinyl acetate content of 45% by weight or more (a3) Compatibilizer [4] The resin composition according to any one of [1] to [3], wherein the ethylene-vinyl alcohol copolymer (B) has a melt mass flow rate of 1.5 to 30 g / 10 min as measured at 190°C in accordance with JIS K6922-1. [5] The resin composition according to any one of [1] to [4], wherein the propylene-based polymer (C) includes at least one selected from the group consisting of a propylene homopolymer, a random polypropylene copolymerized with ethylene, a block polypropylene copolymerized with ethylene, a polypropylene terpolymer copolymerized with ethylene and 1-butene, a syndiotactic polypropylene, an atactic polypropylene, and a long-chain branched polypropylene. [6] When the shear rate and apparent shear viscosity were measured using a capillary rheometer at 220°C and an orifice length L / orifice diameter D = 20 / 1, the shear rate was 100-150 sec -1 The resin composition according to any one of [1] to [5], wherein a melt viscosity ratio (A / B) of the component (A) to the component (B) and a melt viscosity ratio (C / B) of the component (C) to the component (B) are 0.20 to 2.0. [7] A laminate comprising a gas barrier resin layer made of the resin composition according to any one of [1] to [6], and at least one propylene-based polymer (C) layer adjacent to the gas barrier resin layer, wherein the propylene-based polymer (C) has a melt mass flow rate of 0.1 to 10 g / 10 min. [8] A laminate having a gas barrier resin layer made of the resin composition according to any one of [1] to [6], and a propylene-based polymer (C) layer on both sides adjacent to the gas barrier resin layer, wherein the propylene-based polymer (C) has a melt mass flow rate of 0.1 to 10 g / 10 min. Effect of the Invention

[0011] When the resin composition of the present invention is made into a film, it has excellent gas barrier properties and adhesiveness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below.

[0013] A resin composition according to one embodiment of the present invention comprises at least a saponified ethylene-vinyl acetate copolymer (A) having a vinyl acetate content of 0.3 to 20 mol % and a vinyl alcohol content of 1 to 20 mol %, an ethylene-vinyl alcohol copolymer (B), and a propylene-based polymer (C).

[0014] The above-mentioned saponified ethylene-vinyl acetate copolymer (A) (hereinafter sometimes abbreviated as (A), (A) component, or component (A)) is a terpolymer mainly composed of ethylene units, vinyl acetate units, and vinyl alcohol units.

[0015] Component (A) can be obtained, for example, by hydrolyzing (saponifying) a portion of the vinyl acetate constituting an ethylene-vinyl acetate copolymer. The method for hydrolyzing the ethylene-vinyl acetate copolymer is not particularly limited, and for example, an ethylene-vinyl acetate copolymer can be produced according to a known method, and then the copolymer can be hydrolyzed to produce component (A). An acid catalyst or an alkali catalyst can be used for hydrolysis of the ethylene-vinyl acetate copolymer, and examples of such methods include a method in which pellets of the ethylene-vinyl acetate copolymer are directly hydrolyzed in an alkali, and a method in which the ethylene-vinyl acetate copolymer is saponified and extruded in a twin-screw extruder.

[0016] The degree of saponification of component (A) can be calculated from the vinyl acetate content of the ethylene-vinyl acetate copolymer before saponification and the saponified ethylene-vinyl acetate copolymer (A) according to the following formula. Formula: Degree of saponification (mol%) = 100 × {(vinyl acetate content of ethylene-vinyl acetate copolymer before saponification) - (vinyl acetate content of saponified ethylene-vinyl acetate copolymer)} / (vinyl acetate content of ethylene-vinyl acetate copolymer before saponification) If the saponification degree of the component (A) is 10 mol % or more, compatibility with EVOH is good, and it is more preferably 20 mol % or more, and most preferably 30 mol % or more.

[0017] The (A) component functions as a compatibilizer between the propylene-based polymer and EVOH described below, and in order to enhance compatibility, the vinyl acetate content is 0.3 to 20 mol% and the vinyl alcohol content is 1 to 20 mol%, preferably the vinyl acetate content is 0.5 to 18 mol% and the vinyl alcohol content is 2 to 20 mol%. Of these, the vinyl acetate content is most preferably 1.0 to 15 mol% and the vinyl alcohol content is 3 to 20 mol%. The total value of the ethylene content, the vinyl acetate content and the vinyl alcohol content is 100 mol%. If the vinyl alcohol content is less than 1.0 mol%, the compatibility with EVOH decreases and the mechanical properties of the resin composition are significantly impaired, and if the vinyl acetate content and / or the vinyl alcohol content exceed 20 mol%, the compatibility with the propylene-based polymer decreases, which is not preferable. The (A) component may be used alone or in combination of two or more types.

[0018] From the viewpoint of molding processability, the (A) component has a melt mass flow rate (hereinafter sometimes abbreviated as MFR) measured in accordance with JIS K6924-1 (under conditions of 190°C and a load of 2160 g) of preferably 0.3 to 5.0 g / 10 min, and most preferably 0.5 to 5.0 g / 10 min.

[0019] The component (A) is preferably a hydrolysate of a kneaded product containing the following components (a1) to (a3) ​​and crosslinked products of the (a1) to (a3). (a1) An ethylene-vinyl acetate copolymer having a vinyl acetate content of 20% by weight or less (a2) Ethylene-vinyl acetate copolymer having a vinyl acetate content of 45% by weight or more (a3) Compatibilizer The component (a1) ethylene-vinyl acetate copolymer having a vinyl acetate content of 20% by weight or less is a copolymer having ethylene units and vinyl acetate units. The method for producing the component (a1) is not particularly limited as long as it is possible to produce an ethylene-vinyl acetate copolymer, and examples of the method include the well-known high-pressure radical polymerization method and ionic polymerization method. Such a resin can be conveniently selected from commercially available products, and an ethylene-vinyl acetate copolymer produced by a high-pressure radical polymerization method is commercially available from Tosoh Corporation under the product name Ultrathene.

[0020] From the viewpoints of molding stability and dispersibility with EVOH, the component (a1) preferably has a melt mass flow rate, measured in accordance with JIS K6924-1 (under conditions of 190°C and a load of 2160 g), of 0.1 to 100 g / 10 min, more preferably 0.1 to 10 g / 10 min, and most preferably 0.5 to 5.0 g / 10 min.

[0021] The component (a2) ethylene-vinyl acetate copolymer has a vinyl acetate content of 45% by weight or more. From the viewpoint of compatibility with the component (a1), the vinyl acetate content is preferably in the range of 45 to 85% by weight, and most preferably in the range of 48 to 80% by weight.

[0022] The method for producing the ethylene-vinyl acetate copolymer in component (a2) is not limited, but examples thereof include known production methods such as high-pressure radical polymerization, solution polymerization, and latex polymerization, and these are commercially available from ARLANXEO under the trade names LEVAPREN and LEVAMELT.

[0023] The compatibilizer constituting the above component (a3) ​​is not particularly limited as long as it can improve the compatibility between (a1) and (a2), and examples thereof include ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-methyl acrylate copolymer, ionomer resin, etc., and is appropriately selected in consideration of the compatibility between (a1) and (a2) and the cost. Among them, it is preferable to use an ethylene-vinyl acetate copolymer having a vinyl acetate content of 21 to 44% by weight from the viewpoint of cost, and one type alone or a combination of two or more types may be used, but using two or more types of ethylene-vinyl acetate copolymers having different vinyl acetate contents reduces the difference in the vinyl acetate content of each component, thereby improving the compatibility between (a1) and (a2). Such ethylene-vinyl acetate copolymers are commercially available from Tosoh Corporation under the trade name Ultrathene, and from ARLANXEO under the trade names LEVAPRENE and LEVAMELT.

[0024] The component (A) is a kneaded product containing the following components (a1) to (a3) ​​and crosslinked products of the (a1) to (a3), which is obtained by crosslinking a composition containing the components (a1) to (a3). The method for crosslinking the composition containing the components (a1) to (a3) ​​is not particularly limited as long as it can be modified by crosslinking, and is appropriately selected in consideration of reactivity, etc., but from the viewpoint of productivity, it is preferable to add a crosslinking agent (a4) to the above components (a1) to (a3), and it is preferable to use an organic peroxide as the crosslinking agent (a4).

[0025] The organic peroxide of the crosslinking agent (a4) is not particularly limited as long as it is an organic peroxide, and examples thereof include dicumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 1,1-di(t-butylperoxy)cyclohexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, 1,3-bis(t-butylperoxyisopropyl)benzene, 1,1-bis(t-butylperoxy)-3,3,5-trimethylperoxide, and the like. Examples of the peroxides include ethylcyclohexane, 1,3-di-(t-butylperoxy)-diisopropylbenzene, n-butyl-4,4-bis(t-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, t-butyl peroxybenzoate, t-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, t-butylcumyl peroxide, etc. These can be used alone or in combination of two or more.

[0026] Among them, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane and 1,1-di(t-butylperoxy)cyclohexane are preferably used from the viewpoint of reactivity. In addition, a crosslinking assistant such as triallyl isocyanurate or divinylbenzene may be used together with the above crosslinking agent, if necessary. The amount of the crosslinking agent (a4) is preferably in the range of 0.005 to 1 part by weight per 100 parts by weight of the total of the components (a1) to (a3), which can improve the compatibility of the saponified ethylene-vinyl acetate copolymer (A) with the propylene polymer and EVOH. A specific example of a production process for the component (A), which is a hydrolysate of a kneaded product containing the components (a1) to (a3) ​​and crosslinked products of (a1) to (a3), is as follows.

[0027] A dry blend of the components (a1) to (a3) ​​and the crosslinking agent (a4) is fed into the hopper of an extruder. At least a portion of the components (a1) to (a3) ​​and the crosslinking agent (a4) may be added from a side feeder or the like. Furthermore, two or more extruders may be used to sequentially melt-knead in stages. When mixing in advance, a Henschel mixer, a V blender, a ribbon blender, a tumbler, or the like may be used.

[0028] Furthermore, component (A) may contain additives, such as crosslinking aids, antioxidants, lubricants, neutralizing agents, antiblocking agents, surfactants, slip agents, and odor trapping agents, that are typically used in thermoplastic resins, as required.

[0029] The EVOH (B) (hereinafter sometimes abbreviated as (B), (B) component, or component (B)) is a copolymer mainly composed of ethylene units and vinyl alcohol units. The ethylene content of the (B) component is 27 to 48 mol% from the viewpoint of film formation stability and gas barrier properties. The saponification degree of the EVOH is preferably 96 mol% or more. By keeping the ethylene content and saponification degree in the EVOH within the above ranges, good gas barrier properties can be maintained. In addition to the ethylene units and vinyl alcohol units, the EVOH may contain other structural units in small amounts, and the (B) component can be used alone or in a mixture of two or more types. Such EVOH is commercially available under the trade name EVAL from Kuraray Co., Ltd. and under the trade name Soarnol from Mitsubishi Chemical Corporation.

[0030] From the viewpoints of high gas barrier property and molding process stability, the MFR of component (B) (value measured at 190° C. under a load of 2160 g) is preferably 1.5 to 30 g / 10 min, and most preferably 1.5 to 20 g / 10 min.

[0031] The propylene polymer (C) (hereinafter sometimes abbreviated as (C), (C) component, or component (C)) is not particularly limited as long as the object of the present invention is achieved, and examples thereof include propylene homopolymer, random polypropylene in which ethylene is randomly copolymerized, block polypropylene in which ethylene is block copolymerized, polypropylene terpolymer in which ethylene and 1-butene are copolymerized, syndiotactic polypropylene, atactic polypropylene, and long-chain branched polypropylene. Such polypropylene (4) is sold under the trade name Prime Polypro by Prime Polymer Co., Ltd., under the trade names Novatec PP, Wintech, Newcon, and Newstrene by Japan Polypropylene Corporation, and under the trade names Noblen, Excellen, and Sumitic by Sumitomo Chemical Co., Ltd. Such polypropylenes may be used alone or in combination of two or more kinds.

[0032] The MFR of the propylene polymer measured according to JIS K7210 (under conditions of 230°C and 2160g load) is preferably 0.1 to 10g / 10min, more preferably 0.2 to 8.0g / 10min, from the viewpoint of molding processability. When the MFR of the propylene polymer is 10g / 10min or less, the melt viscosity ratio matches with that of component (B), and good gas barrier properties are obtained. When the MFR of the propylene polymer is 0.1g / 10min or more, productivity is excellent.

[0033] The resin composition according to one embodiment of the present invention contains at least the above-mentioned components (A), (B), and (C), and from the viewpoint of maintaining adhesiveness, it is preferred that components (A) and (C) are formed as a matrix (sea component) and component (B) is formed as a domain (island component). A part of component (A) also acts as a compatibilizer for components (B) and (C).

[0034] The weight ratio ((A+C) / B) of the total ((A+C)) of the saponified ethylene-vinyl acetate copolymer (A) and the propylene-based polymer (C) to the ethylene-vinyl alcohol copolymer (B) is preferably 80 / 20 to 50 / 50, more preferably 75 / 25 to 50 / 50, and most preferably 70 / 30 to 50 / 50 (the total of A, B, and C is 100 parts by weight). It is preferable that each of the components (A) and (C) is contained in an amount of 10 parts by weight or more.

[0035] In order to achieve high gas barrier properties, it is preferable that component (B) has a structure in which the component is dispersed in a layered form, or a part of the layered domain is three-dimensionally connected, when the resin is cut and observed in a direction perpendicular to the flow direction (MD). From the viewpoint of maintaining gas barrier properties, it is preferable that 50% or more of component (B) is a layered domain, or a network structure in which a part of the layered domain is three-dimensionally connected. To form such a dispersed structure, it is preferable that component (A) / component (B) or component (C) / component (B) have an appropriate melt viscosity ratio.

[0036] The specific melt viscosity ratio is a shear rate of 100 to 150 sec when the shear rate and apparent shear viscosity of the components (A) and (B) constituting the gas barrier resin layer are measured using a capillary rheometer under the conditions of 190°C, orifice length L / orifice diameter D = 20 / 1. -1 The melt viscosity ratio (A / B) of component (A) to component (B) and the melt viscosity ratio (C / B) of component (C) to component (B) are preferably 0.20 to 2.0, and more preferably 0.30 to 1.8.

[0037] The aspect ratio (major axis / minor axis) of the lamellar domains derived from component (B) formed in the matrix-forming component (A) is preferably at least 5, more preferably at least 10, and most preferably at least 20. From the viewpoint of maintaining the appearance of the film, the minor axis of the lamellar domains of component (B) is preferably at most 10 μm, more preferably at most 5 μm, and most preferably at most 2.5 μm.

[0038] The method of melt-kneading the resin composition (components (A) to (C)) is not particularly limited as long as the melt-kneading device can uniformly disperse each component, and production can be performed using a melt-kneading device that is commonly used for resins. Examples of melt-kneading devices include a single-screw extruder, a multi-screw extruder, a Banbury mixer, a pressure kneader, a rotating roll, and a Labo Plastomill. The melting temperature is preferably about 180 to 260°C. The resin composition (components (A) to (C)) is not necessarily melt-kneaded, and may be simply dry-blended. Examples of dry-blending methods include a Henschel mixer, a V blender, a ribbon blender, and a tumbler.

[0039] Furthermore, the above resin composition may contain additives, such as crosslinking assistants, antioxidants, lubricants, neutralizing agents, antiblocking agents, surfactants, slip agents, odor trapping agents, and the like, which are usually used in thermoplastic resins, as long as the object of the present invention is not impaired.

[0040] A laminate which is one embodiment of the present invention has a gas barrier resin layer made of the above-mentioned resin composition, and at least one propylene-based polymer layer adjacent to the gas barrier resin layer, or at least one propylene-based polymer layer adjacent to the gas barrier resin layer on both sides.

[0041] Since the resin composition has excellent gas barrier properties, it is possible to use the resin composition as a gas barrier resin layer of a laminate. For example, if necessary, at least one propylene-based polymer layer may be disposed on the gas barrier resin layer made of the resin composition, or propylene-based polymer layers may be disposed on both sides of the gas barrier resin layer.

[0042] The components constituting the propylene-based polymer layer are similar to those exemplified for component (C), and include, for example, propylene homopolymer, random polypropylene in which ethylene is randomly copolymerized, block polypropylene in which ethylene is block copolymerized, polypropylene terpolymer in which ethylene and 1-butene are copolymerized, syndiotactic polypropylene, atactic polypropylene, long-chain branched polypropylene, etc., and are not particularly limited as long as the object of the present invention is achieved. Such propylene-based polymers are sold under the trade names Prime Polypro by Prime Polymer Co., Ltd., Novatec PP, Wintech, Newcon, and Newstrene by Japan Polypropylene Corporation, and Noblen, Excellen, and Sumitic by Sumitomo Chemical Co., Ltd. Such polypropylenes may be used alone or in combination of two or more kinds.

[0043] From the viewpoint of molding processability, the MFR of the propylene polymer measured based on JIS K7210 (under conditions of 230°C and 2160g load) is preferably 0.1 to 10g / 10min, more preferably 0.2 to 8.0g / 10min. If the MFR of the polyolefin resin exceeds 10g / 10min, the melt viscosity ratio does not match that of the gas barrier resin layer, which may cause unstable fluidization and deteriorate the appearance of the laminate. If the MFR of the polyolefin resin is less than 0.1g / 10min, the productivity may decrease.

[0044] The propylene-based polymer used in the propylene-based polymer layer may contain additives, such as crosslinking aids, antioxidants, lubricants, neutralizing agents, antiblocking agents, surfactants, slip agents, odor trapping agents, and the like, which are generally used in thermoplastic resins, as long as the object of the present invention is not impaired. In addition, inorganic fillers and dyes and pigments may be contained as necessary for the purpose of reinforcement, weight increase, coloring, and the like. Examples of inorganic fillers and dyes and pigments include calcium carbonate, talc, clay, synthetic silicon, titanium oxide, carbon black, and barium sulfate.

[0045] The laminate can be produced by any known method, including, for example, various coextrusion moldings such as coextrusion blow molding, coextrusion sheet molding, coextrusion cast molding, coextrusion inflation molding, coextrusion lamination molding, and coinjection molding, and can be molded into any shape such as a sheet, film, pipe, block, etc. In addition, by adopting a laminate structure with other materials, it is possible to impart the properties of the other materials, such as gas barrier properties, water vapor barrier properties, mechanical properties, oil resistance, and weather resistance, to the laminate.

[0046] A laminate in which the above-mentioned resin composition is used as a gas barrier resin layer can be used in molding machines that have a limit on the number of layers, and can be used not only for food, beverages, pharmaceuticals, agriculture, and cosmetics applications in which high gas barrier properties are required, but also for a wide variety of applications in which it is desirable to avoid releasing odors or fragrance components to the outside. EXAMPLES

[0047] The resin composition of the present invention will be described in more detail below based on examples carried out to clarify the effects of the resin composition of the present invention. Note that the resin composition of the present invention is not limited by the following examples and comparative examples. <Saponification degree> The vinyl acetate content of the ethylene-vinyl acetate copolymer or saponified ethylene-vinyl acetate copolymer (A) obtained in the examples was measured in accordance with JIS K7192 (1999), and the degree of saponification (mol%) was calculated according to the following formula. Saponification degree (mol%) = 100 × {(vinyl acetate content of ethylene-vinyl acetate copolymer before saponification) - (vinyl acetate content of saponified ethylene-vinyl acetate copolymer)} / (vinyl acetate content of ethylene-vinyl acetate copolymer before saponification) <mfr> The MFR was measured in accordance with JIS K6922-1, JIS K6924-2, ISO1183-3, and JIS K7210. <Preparation of Laminate> The resin composition constituting the gas barrier resin layer was fed to the extruder (25 mmφ) forming the intermediate layer of a three-layer cast molding machine (manufactured by Plastics Engineering Research Institute Co., Ltd.) having a screw of 32 / 25 / 25 mmφ, and the propylene-based polymer constituting the propylene-based polymer layer was fed to two extruders (32 mmφ and 25 mmφ) forming the inner layer and the outer layer, and all layers were extruded at 230°C and taken up at a take-up speed of 10 m / min to obtain a 50 μm thick laminate (two-kind three-layer film) with a propylene-based polymer layer / gas barrier resin layer / propylene-based polymer layer=20 μm / 10 μm / 20 μm. The obtained two-kind three-layer film was used to evaluate the oxygen permeability and heat seal strength. Note that the / above means adjacent. <Oxygen permeability> The oxygen permeability was measured in accordance with ISO 15105-2 using the two-type three-layer film (thickness 50 μm) obtained in the examples with a MOCON OX-TRAN 2 / 22 L at 23°C and humidity 65%, and the unit is cc / (m 2 An oxygen permeability of less than 75 was judged as "good," while an oxygen permeability of 75 or more but less than 150 was judged as "good," and an oxygen permeability of 150 or more was judged as "bad." <Heat seal strength> The heat seal strength of the two-kind three-layer film was measured by cutting the two-kind three-layer film obtained in the examples to 100 mm in the horizontal direction (TD direction) and 200 mm in the vertical direction (MD direction), overlapping the inner layers of the film, and heat sealing was performed with a heat seal tester TP-701B (manufactured by Tester Sangyo Co., Ltd.) at a set temperature of 180°C, double-sided heating, air pressure of 0.2 MPa, and heat seal time of 1 second using a seal bar with a width of 10 mm and a length of 300 mm. This test piece was cut to a width of 15 mm and a peel test was performed using a tensile tester Tensilon RTE-1210 (manufactured by Orientec Co., Ltd.) at a tensile speed of 300 mm / min and T-type peeling to measure the heat seal strength (N / 15 mm). A heat seal strength of 10 or more was marked as "◯", less than 10 and 5 or more was marked as "△", and less than 5 was marked as "X". <Production Example> [Production example of saponified ethylene-vinyl acetate copolymer (A1)] 70 parts by weight of ethylene-vinyl acetate copolymer (manufactured by Tosoh Corporation, trade name Ultrathene 626) (a1-1) having a melt mass flow rate of 3.0 g / 10 min and a vinyl acetate content of 15 wt%, 10 parts by weight of ethylene-vinyl acetate copolymer (manufactured by ARLANXEO, trade name LEVAPREN500) (a2) having a melt mass flow rate of 5.0 g / 10 min and a vinyl acetate content of 50 wt%, 20 parts by weight of a compatibilizer (a3) ​​shown below, and 100 ppm of an organic peroxide (manufactured by NOF Corporation, trade name Perhexa 25B) as a crosslinking agent (a4) were dry-blended at a melt resin temperature of 190°C using a twin-screw extruder to obtain a pellet-shaped sample. Next, this sample was hydrolyzed in a 5 wt% sodium hydroxide methanol solution at 65°C for 5 hours to obtain an ethylene-vinyl acetate copolymer saponification product (A1) having a saponification degree of 50 mol% and MFR of 3.0 g / 10 min. Detailed results are shown in Tables 1 and 2. (Constitution of the Compatibilizer (a3)) The following four types of ethylene-vinyl acetate copolymers were dry-blended in equal amounts (1 / 1 / 1 / 1) to prepare the compatibilizer (a3). Ethylene-vinyl acetate copolymer with a melt mass flow rate of 20 g / 10 min and a vinyl acetate content of 20% by weight (manufactured by Tosoh Corporation, product name Ultrathene 633) Ethylene-vinyl acetate copolymer with a melt mass flow rate of 18 g / 10 min and a vinyl acetate content of 28% by weight (manufactured by Tosoh Corporation, product name Ultrathene 710) Ethylene-vinyl acetate copolymer with a melt mass flow rate of 30 g / 10 min and a vinyl acetate content of 32% by weight (manufactured by Tosoh Corporation, product name Ultrathene 750) Ethylene-vinyl acetate copolymer with a melt mass flow rate of 70 g / 10 min and a vinyl acetate content of 42% by weight (manufactured by Tosoh Corporation, product name Ultrathene 760) [Production example of saponified ethylene-vinyl acetate copolymer (A2)] A saponified ethylene-vinyl acetate copolymer (A2) with a saponification degree of 65 mol% and MFR of 0.5 g / 10 min was obtained by the same method as (A1), except that 50 parts by weight of (a1-1), 30 parts by weight of (a2), and 150 ppm of crosslinking agent (a4) were dry-blended and hydrolysis treatment was carried out for 7 hours. Detailed results are shown in Tables 1 and 2. [Production example of saponified ethylene-vinyl acetate copolymer (A3)] A saponified ethylene-vinyl acetate copolymer (A3) with a saponification degree of 46 mol% and MFR of 14 g / 10 min was obtained by the same method as (A1), except that 65 parts by weight of ethylene-vinyl acetate copolymer (a1-2) with a melt mass flow rate of 30 g / 10 min and a vinyl acetate content of 15 wt%, 12 parts by weight of (a2), and 23 parts by weight of (a3) ​​were used, and hydrolysis was carried out for 5 hours at a reaction temperature of 55°C using 1 part by weight of sodium hydroxide methanol solution. Detailed results are shown in Tables 1 and 2. [Production example of saponified ethylene-vinyl acetate copolymer (A4)] A saponified ethylene-vinyl acetate copolymer (A5) with a saponification degree of 5 mol% and MFR of 3.5 g / 10 min was obtained in the same manner as (A1), except that 70 parts by weight of (a1-1), 10 parts by weight of (a2), and 20 parts by weight of (a3) ​​were dry-blended and hydrolyzed with 1 part by weight of a methanol solution of sodium hydroxide at a reaction temperature of 40°C for 2 hours. Detailed results are shown in Tables 1 and 2.

[0048] [Table 1]

[0049] [Table 2]

[0050] Example 1 As a resin composition constituting the gas barrier resin layer, 50 parts by weight of saponified ethylene-vinyl acetate copolymer (A1), 25 parts by weight of an ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name EVAL C109B) (B1) having a melt mass flow rate of 8.5 g / 10 min and an ethylene content of 35 mol%, as an ethylene-vinyl alcohol copolymer, and 25 parts by weight of a propylene homopolymer (manufactured by Japan Polypropylene Corporation, product name Novatec FB3B) (C1) having a melt mass flow rate of 7.5 g / 10 min as a propylene polymer, were dry blended, and then melt blended at a molten resin temperature of 230°C using a single-screw extruder.

[0051] As the propylene-based polymer constituting the propylene-based polymer layer, C1 was used.

[0052] Using the above-mentioned three-layer cast molding machine, the resin composition constituting the gas barrier resin layer was supplied to the extruder (25 mmφ) forming the intermediate layer, and the propylene-based polymer constituting the propylene-based polymer layer was supplied to two extruders (32 mmφ and 25 mmφ) forming the inner and outer layers, and molded at 220°C to obtain a 50 μm-thick laminate with inner layer / intermediate layer / outer layer=20 / 10 / 20 μm. The oxygen permeability and heat seal strength of the obtained laminate were evaluated, and the results are shown in Table 3.

[0053] Example 2 A laminate was produced in the same manner as in Example 1, except that the amount of saponified ethylene-vinyl acetate copolymer (A1) was 25 parts by weight, the amount of ethylene-vinyl alcohol copolymer (B1) was 25 parts by weight, and the amount of propylene-based polymer (C1) was 50 parts by weight. The oxygen permeability and heat seal strength of the obtained laminate were evaluated, and the results are shown in Table 3.

[0054] Example 3 Except for using the saponified ethylene-vinyl acetate copolymer (A2), a laminate was produced in the same manner as in Example 2. The oxygen permeability and heat seal strength of the obtained laminate were evaluated, and the results are shown in Table 3.

[0055] Example 4 A laminate was produced in the same manner as in Example 2, except that the amount of saponified ethylene-vinyl acetate copolymer (A3) was 25 parts by weight, the amount of an ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name EVAL F171B) (B2) having a melt mass flow rate of 1.7 g / 10 min and an ethylene content of 32 mol% as an ethylene-vinyl alcohol copolymer was 50 parts by weight, and the amount of a propylene-based polymer (C1) was 25 parts by weight. The oxygen permeability and heat seal strength of the obtained laminate were evaluated, and the results are shown in Table 3.

[0056] [Table 3]

[0057] Example 5 A laminate was produced in the same manner as in Example 2, except that the amount of saponified ethylene-vinyl acetate copolymer (A1) was 40 parts by weight, the amount of ethylene-vinyl alcohol copolymer (B1) was 20 parts by weight, and the amount of propylene-based polymer (C1) was 40 parts by weight. The oxygen permeability, heat seal strength, and film appearance of the obtained laminate were evaluated, and the results are shown in Table 4. Example 6 A laminate was produced in the same manner as in Example 2, except that the amount of saponified ethylene-vinyl acetate copolymer (A1) was 20 parts by weight, the amount of ethylene-vinyl alcohol copolymer (B1) was 60 parts by weight, and the amount of propylene-based polymer (C1) was 20 parts by weight. The oxygen permeability and heat seal strength of the resulting laminate were evaluated, and the results are shown in Table 4. Example 7 A laminate was produced in the same manner as in Example 2, except that a polypropylene terpolymer (manufactured by Japan Polypropylene Corporation, product name Novatec FW4BA) (C2) in which ethylene and 1-butene were copolymerized and had a melt mass flow rate of 7.0 g / 10 min was used as the propylene polymer. The oxygen permeability and heat seal strength of the obtained laminate were evaluated, and the results are shown in Table 4.

[0058] Example 8 A laminate was produced in the same manner as in Example 2, except that a polypropylene homopolymer (manufactured by Japan Polypropylene Corporation, product name Novatec FY4) (C3) having a melt mass flow rate of 4.0 g / 10 min was used as the propylene-based polymer. The oxygen permeability and heat seal strength of the obtained laminate were evaluated, and the results are shown in Table 4.

[0059] [Table 4]

[0060] Comparative Example 1 A laminate was produced in the same manner as in Example 1, except that saponified ethylene-vinyl acetate copolymer (A4) was used. The oxygen permeability and heat seal strength of the resulting laminate were evaluated, and the results are shown in Table 5. The laminate of this comparative example had poor heat seal strength.

[0061] Comparative Example 2 A laminate was produced in the same manner as in Example 1, except that the amount of saponified ethylene-vinyl acetate copolymer (A1) was 70 parts by weight and the amount of ethylene-vinyl alcohol copolymer (B1) was 30 parts by weight. The oxygen permeability and heat seal strength of the resulting laminate were evaluated, and the results are shown in Table 5. The laminate of this comparative example had poor heat seal strength.

[0062] Comparative Example 3 A laminate was produced in the same manner as in Example 1, except that the ethylene-vinyl alcohol copolymer (B1) was 30 parts by weight and the propylene-based polymer (C1) was 70 parts by weight. The oxygen permeability and heat seal strength of the resulting laminate were evaluated, and the results are shown in Table 5. The laminate of this comparative example had poor heat seal strength.

[0063] [Table 5] < / mfr>

Claims

1. The resin composition comprises at least a saponified ethylene-vinyl acetate copolymer (A) having a vinyl acetate content of 0.3 to 20 mol % and a vinyl alcohol content of 1.0 to 20 mol %, an ethylene-vinyl alcohol copolymer (B) having an ethylene content of 27 to 48 mol %, and a propylene-based polymer (C).

2. The resin composition according to claim 1, wherein a weight ratio ((A+C) / B) of the total ((A+C)) of the saponified ethylene-vinyl acetate copolymer (A) and the propylene-based polymer (C) to the ethylene-vinyl alcohol copolymer (B) is 80 / 20 to 50 / 50.

3. The resin composition according to claim 1, wherein the saponified ethylene-vinyl acetate copolymer (A) is a hydrolyzate of a kneaded product containing the following components (a1) to (a3) ​​and crosslinked products of the (a1) to (a3), and has a melt mass flow rate of 0.3 to 5.0 g / 10 min as measured in accordance with JIS K6922-1: (a1) Ethylene-vinyl acetate copolymer having a vinyl acetate content of 20% by weight or less (a2) Ethylene-vinyl acetate copolymer having a vinyl acetate content of 45% by weight or more (a3) Compatibilizer

4. The resin composition according to claim 1, wherein the ethylene-vinyl alcohol copolymer (B) has a melt mass flow rate of 1.5 to 30 g / 10 min measured at 190° C. according to JIS K6922-1.

5. The resin composition according to claim 1, wherein the propylene-based polymer (C) comprises at least one selected from the group consisting of a propylene homopolymer, a random polypropylene copolymerized with ethylene, a block polypropylene copolymerized with ethylene, a polypropylene terpolymer copolymerized with ethylene and 1-butene, a syndiotactic polypropylene, an atactic polypropylene, and a long-chain branched polypropylene.

6. Using a capillary rheometer, the shear rate and apparent shear viscosity were measured under the conditions of 220°C, orifice length L / orifice diameter D = 20 / 1. -1 The resin composition according to claim 1, wherein the melt viscosity ratio (A / B) of the component (A) to the component (B) and the melt viscosity ratio (C / B) of the component (C) to the component (B) are 0.20 to 2.

0.

7. 7. A laminate comprising a gas barrier resin layer made of the resin composition according to any one of claims 1 to 6, and at least one propylene-based polymer (C) layer adjacent to the gas barrier resin layer, wherein the propylene-based polymer (C) has a melt mass flow rate of 0.1 to 8.0 g / 10 min.

8. 7. A laminate comprising a gas barrier resin layer made of the resin composition according to any one of claims 1 to 6, and a propylene-based polymer (C) layer on both sides adjacent to the gas barrier resin layer, wherein the propylene-based polymer (C) has a melt mass flow rate of 0.1 to 8.0 g / 10 min.

Citation Information

Patent Citations

  • Laminated body and manufacture thereof

    JP2000167998A

  • Fuel container

    JP2001200124A

  • Method for preparing laminated body

    JP2001277371A

  • Adhesive and laminate containing the same

    JP2017210608A