Method for forming surface-treated film

A method for forming a surface treatment film on semiconductor substrates with oxidized metal regions using thiols with 8 or fewer carbon atoms addresses overhang issues, ensuring thick films are confined to metal regions and enhancing selective film formation on semiconductor devices.

JP2024165284APending Publication Date: 2024-11-28TOKYO OHKA KOGYO CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023081352
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The formation of insulating films on semiconductor substrates with exposed metal regions leads to overhang or protrusion issues, particularly when the films are thicker than the self-assembled monolayers, which is exacerbated by the miniaturization of semiconductor devices.

Method used

A method involving substrate preparation with oxidized metal regions, exposure to thiols with 8 or fewer carbon atoms, and solvent cleaning to form a surface treatment film that prevents protrusion into insulating regions, using substrates with recessed metal areas and specific insulating materials.

Benefits of technology

The method enables the formation of a thick surface treatment film on metal regions without protruding into insulating regions, maintaining rectangularity and facilitating selective film formation on semiconductor substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165284000002
    Figure 2024165284000002
  • Figure 2024165284000003
    Figure 2024165284000003
  • Figure 2024165284000004
    Figure 2024165284000004
Patent Text Reader

Abstract

To provide a method for forming a surface-treated film on a second region of a substrate having, on the surface thereof, a first region in which an insulator is exposed and a second region in which at least one metal selected from a metal and a conductive metal-containing compound is exposed, and enabling suppression of protrusion to the first region of the surface-treated film even when a film thickness of the surface-treated film is large.SOLUTION: A method for forming a surface-treated film is provided, including: a substrate preparation step of preparing a substrate having, on the surface thereof, a first region in which an insulator is exposed and a second region in which at least one metal selected from a metal and a conductive metal-containing compound is exposed; an oxidation step of oxidizing a surface of the second region; and an exposure step of exposing the surface of the substrate to a surface treatment agent including thiol having eight or less carbon atoms after the oxidation step, thereby forming the surface-treated film on the second region.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for forming a surface treatment film. [Background technology]

[0002] In recent years, there has been a growing trend toward higher integration and miniaturization of semiconductor devices. Accordingly, patterned organic films used as masks and patterned inorganic films produced by etching processes are becoming finer. For this reason, there is a demand for thickness control at the atomic layer level for organic and inorganic films formed on semiconductor substrates. Atomic layer deposition (ALD) is a type of CVD (Chemical Vapor Deposition) known as a method for forming a thin film on a substrate at the atomic layer level. Among CVD (Chemical Vapor Deposition) methods, the ALD method is known to have both high step coverage and film thickness controllability.

[0003] The ALD method is a thin-film formation technology in which two types of gases, the main components of which are the elements that make up the film to be formed, are alternately supplied onto a substrate, and a thin film is formed on the substrate in atomic layer units by repeating this process multiple times to form a film of the desired thickness. The ALD method utilizes a self-limiting growth function in which only the components of the source gas that are sufficient to form one or several atomic layers are adsorbed onto the substrate surface while the source gas is being supplied, while excess source gas does not contribute to growth. For example, when forming an Al2O3 film on a substrate, a source gas made of TMA (TriMethyl Aluminum) and an oxidizing gas containing O are used. When forming a nitride film on a substrate, a nitriding gas is used instead of the oxidizing gas.

[0004] In recent years, attempts have been made to selectively form films on a substrate surface using the ALD method (see Patent Document 1 and Non-Patent Document 1). Accordingly, there is a demand for substrates having surfaces that are selectively modified in areas that can be suitably applied to selectively forming films on the substrate by the ALD method. As a method for obtaining a substrate having such a region-selectively modified surface, for example, a method has been disclosed in which a self-assembled monolayer (SAM) of a sulfur-containing monomer (1-dodecanethiol) is selectively formed on the second (metallic) surface out of a first (dielectric) surface and a second (metallic) surface (see Patent Document 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2003-508897 [Patent Document 2] JP 2018-137435 A [Non-patent literature]

[0006] [Non-Patent Document 1] J.Phys.Chem.C 2014,118,10957-10962 Summary of the Invention [Problem to be solved by the invention]

[0007] As shown in FIG. 1, in a substrate 1 having a first region 11 on its surface where an insulator is exposed, and a second region 12 on its surface where at least one metal selected from metals and conductive metal-containing compounds is exposed (FIG. 1(a)), a SAM 13 using an organic compound having a mercapto group (SH) is formed as a surface treatment film on the second region 12 (FIG. 1(b)), and then an insulator film 14 such as SiO2 can be selectively formed on the first region 11 by a CVD method such as the ALD method (FIG. 1(c)). A thick insulator film 14 may be desired, but if the insulator film 14 formed is significantly thicker than the SAM 13, a problem arises in that the side of the insulator film 14 opposite the first region 11 protrudes towards the second region 12, forming an "overhang" (Figure 1(d)). In order to suppress such overhang of the insulating film 14, it is conceivable to increase the film thickness of the SAM 13 as shown in FIG. 2 (FIG. 2(a)). However, when the thickness of the SAM 13 is increased, a problem occurs in that the SAM 13 protrudes onto the surface of the first region 11 (FIG. 2(b)). This problem becomes prominent particularly when the first region 11 and the second region 12 are minute. FIG. 1 is a schematic cross-sectional view illustrating an overhang, and FIG. 2 is a schematic cross-sectional view illustrating the protrusion of the SAM into the first region.

[0008] The present invention has been made in consideration of the above circumstances, and aims to provide a method for forming a surface treatment film, which forms a surface treatment film on a second region of a substrate having a surface thereof including a first region in which an insulator is exposed and a second region in which at least one metal selected from a metal and a conductive metal-containing compound is exposed, and which can suppress the surface treatment film from protruding into the first region even if the surface treatment film is thick. [Means for solving the problem]

[0009] The present inventors have found that the above-mentioned problems can be solved by a method for forming a surface treatment film, the method including: a substrate preparation step of preparing a substrate having, on its surface, a first region exposing an insulator and a second region exposing at least one metal selected from metals and conductive metal-containing compounds, an oxidation step of oxidizing the surface of the second region, and an exposure step of exposing the surface of the substrate to a surface treatment agent containing a thiol having 8 or less carbon atoms to form a surface treatment film on the second region after the oxidation step, and have completed the present invention. Specifically, the present invention provides the following.

[0010] [1] A substrate preparation step of preparing a substrate having a first region on a surface thereof where an insulator is exposed and a second region on a surface thereof where at least one metal selected from a metal and a conductive metal-containing compound is exposed; an oxidation step of oxidizing a surface of the second region; and an exposure step of exposing the surface of the substrate to a surface treatment agent containing a thiol having 8 or less carbon atoms after the oxidation step, thereby forming a surface treatment film on the second region.

[0011] [2] The method for forming a surface treatment film described in [1] above, wherein the insulator has a recess on the surface of the substrate, and a second region in which the metal is exposed is formed in the recess.

[0012] [3] The insulator is at least one selected from the group consisting of silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, hafnium oxide, tantalum oxide, fluorine-containing silicon oxide, carbon-containing silicon oxide, silicon nitride, boron nitride, silicon carbide, silicon carbonitride, silicon oxynitride, silicon oxycarbonitride, silicon, and silicon doped with at least one selected from phosphorus, boron, and germanium; The method for forming a surface treatment film according to the above [1] or [2], wherein the metal is at least one selected from the group consisting of copper, cobalt, molybdenum and ruthenium.

[0013] [4] The method for forming a surface treatment film according to any one of the above [1] to [3], wherein the thiol includes at least one selected from the group consisting of butanethiol, pentanethiol, hexanethiol, heptanethiol, and octanethiol.

[0014] [5] The method for forming a surface treatment film according to any one of the above [1] to [4], further comprising, after the exposure step, a solvent washing step of washing the substrate on which the surface treatment film has been formed with a solvent.

[0015] [6] The method for forming a surface treatment film according to the above [5], wherein the solvent contains a fatty acid alkyl ester.

[0016] [7] The method for forming a surface treatment film according to any one of the above [1] to [6], wherein the thickness of the surface treatment film is 10 nm or more. Effect of the Invention

[0017] According to the present invention, there can be provided a method for forming a surface treatment film on a second region of a substrate having a surface thereof including a first region in which an insulator is exposed and a second region in which at least one metal selected from a metal and a conductive metal-containing compound is exposed, the method being capable of suppressing the surface treatment film from extending over the first region. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is a schematic cross-sectional view illustrating an overhang. [Diagram 2] FIG. 2 is a schematic cross-sectional view illustrating the protrusion of a SAM into a first region. [Diagram 3] 1A to 1C are schematic cross-sectional views illustrating a method for forming a surface treatment film. [Figure 4] FIG. 11 is a schematic cross-sectional view illustrating another example of the substrate. [Diagram 5] FIG. 2 is a schematic diagram illustrating a substrate used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] <Method of forming surface treatment film> The method for forming a surface treatment film includes a substrate preparation step of preparing a substrate having a surface thereof including a first region in which an insulator is exposed and a second region in which at least one metal selected from a metal and a conductive metal-containing compound is exposed; an oxidation step of oxidizing a surface of the second region; and an exposure step of exposing the surface of the substrate to a surface treatment agent containing a thiol having 8 or less carbon atoms, thereby forming a surface treatment film on the second region, after the oxidation step. Each step will be described below with reference to Fig. 3 and Fig. 4. Fig. 3 is a schematic cross-sectional view illustrating a method for forming a surface treatment film. Fig. 4 is a schematic cross-sectional view illustrating another example of a substrate.

[0020] <Substrate preparation process> In the substrate preparation process, a substrate 1 is prepared having, on its surface, a first region 11 where an insulator is exposed and a second region 12 where at least one metal selected from a metal and a conductive metal-containing compound is exposed (Figure 3(a)). (substrate) The substrate 1 has, on its surface, a first region 11 where an insulator is exposed, and a second region 12 where at least one metal selected from metals and conductive metal-containing compounds is exposed. It is preferable that at least one first region 11 and at least one second region 12 are adjacent to each other in the first region 11 where an insulator is exposed and at least one metal selected from metals and conductive metal-containing compounds is exposed. Here, "adjacent" includes a case where at least one first region 11 and at least one second region 12 are adjacent to each other while sharing a boundary (FIG. 3(a)), or a case where they are adjacent to each other or spaced apart without sharing a boundary. An example of the latter case where they are adjacent to each other or spaced apart without sharing a boundary is a structure in which the second region 12 where metals are exposed is a wiring metal, the second region 12 is covered with a barrier metal (a high-melting-point metal film used to prevent the wiring metal from diffusing into the first region, etc., and causing deterioration in the performance of a semiconductor device, etc.) 20, and this barrier metal 20 is in contact with the first region 11, as shown in FIG. 4(a). In this case, the substrate 1 has, on its surface, a first region 11 where the insulator is exposed, a second region 12 where the metals are exposed, and a region (third region) where the barrier metal 20 is exposed. 4(b), the insulator (first region 11) may have a recess on the surface of substrate 1, and second region 12 may be formed in the recess where metal is exposed. The metal (second region 12) may have a recess on the surface of substrate 1, and first region 11 may be formed in the recess where insulator is exposed. In addition, the first region 11 and the second region 12 are There may be one or more of each. Furthermore, the substrate 1 may have one or more regions other than the first region 11 and the second region 12 (a third region made of a material different from the first region 11 and the second region 12).

[0021] An example of a substrate 1 having, on its surface, a first region 11 where an insulator is exposed and a second region 12 where metals are exposed is a substrate in which an inorganic layer constituting the first region 11 where an insulator is exposed and an inorganic layer constituting the second region 12 where metals are exposed are formed on the surface of a base substrate (not shown), such as a substrate used for manufacturing semiconductor devices. In addition, the substrate 1 having on its surface a first region 11 where an insulator is exposed and a second region 12 where metals are exposed may be a substrate in which the surface of a base substrate is the first region 11 where an insulator is exposed, and an inorganic layer constituting the second region 12 where metals are exposed is formed on the surface of the base substrate. In addition, the substrate 1 having on its surface a first region 11 where an insulator is exposed and a second region 12 where metals are exposed may be a substrate in which the surface of a base substrate is the second region 12 where metals are exposed, and an inorganic layer constituting the first region 11 where an insulator is exposed is formed on the surface of the base substrate. The inorganic layer may be patterned or unpatterned, and the substrate 1 may not have an underlying substrate.

[0022] Examples of the base substrate include substrates used for manufacturing semiconductor devices. Examples of such substrates include silicon (Si) substrates, silicon nitride (SiN) substrates, silicon oxide (Ox) substrates, tungsten (W) substrates, cobalt (Co) substrates, germanium (Ge) substrates, aluminum (Al) substrates, nickel (Ni) substrates, ruthenium (Ru) substrates, copper (Cu) substrates, titanium nitride (TiN) substrates, tantalum nitride (TaN) substrates, silicon germanium (SiGe) substrates, and substrates having a patterned or unpatterned inorganic layer on the substrates. Examples of the inorganic layer include a patterned inorganic layer formed by creating an etching mask on the surface of an inorganic layer present on a substrate by a photoresist method and then performing an etching process, and a patterned inorganic layer formed on the surface of a substrate by an atomic layer deposition method (ALD method). The inorganic layer may be, for example, an inorganic layer formed during the manufacturing process of a semiconductor device. Specific examples of inorganic layers include natural oxide films of elements constituting the substrate, silicon nitride (SiN) formed on the surface of the substrate, silicon oxide film (SiOx), tungsten (W), cobalt (Co), germanium (Ge), aluminum (Al), nickel (Ni), ruthenium (Ru), copper (Cu), silver (Ag), titanium (Ti), gold (Au), chromium (Cr), molybdenum (Mo), aluminum oxide (Al2O3), titanium oxide (TiO2), zirconium oxide (ZrO2), hafnium oxide (HfO2), tantalum oxide (Ta2O5), titanium nitride (TiN), tantalum nitride (TaN), silicon germanium (SiGe), silicon oxide (SiO2), and other inorganic films or layers.

[0023] (first area) The insulator is exposed in the first region 11. That is, the first region 11 has an insulator on its surface. The insulator of the first region 11 is made of one or more insulating compounds selected from the group consisting of oxides, nitrides, carbides, carbonitrides, oxynitrides, oxycarbonitrides, insulating resins, and semiconductors, and is preferably an oxide, a nitride, a carbide, a carbonitride, an oxynitride, or an oxycarbonitride. As the oxide, silicon oxide (SiOx (1≦X≦2)), aluminum oxide (Al2O3), titanium oxide (TiO2), zirconium oxide (ZrO2), hafnium oxide (HfO2), tantalum oxide (Ta2O5), fluorine-containing silicon oxide (SiOF), and carbon-containing silicon oxide (SiOC) are preferable. As the nitride, for example, silicon nitride (SiN) and boron nitride (BN) are preferable. As the carbide, silicon carbide (SiC) is preferable. As the carbonitride, silicon carbonitride (SICN) is preferable. As the oxynitride, silicon oxynitride (SiON) is preferable. The oxycarbonitride is preferably silicon oxycarbonitride (SiOCN).The insulating resin may be polyimide, polyester, plastic resin, etc.The semiconductor may be silicon or silicon doped with at least one element selected from phosphorus, boron, and germanium.

[0024] (Second area) At least one metal selected from metals and conductive metal-containing compounds is exposed in the second region 12. That is, the second region 12 has at least one metal selected from metals and conductive metal-containing compounds on the surface. At least one metal selected from metals and conductive metal-containing compounds in the second region 12 may be defined as a conductor in contrast to the insulator in the first region 11. The metal may be a pure metal consisting of a single metal element or an alloy. As the metals, copper (Cu), cobalt (Co), molybdenum (Mo), ruthenium (Ru), a copper alloy containing 90 at % or more of Cu, a cobalt alloy containing 90 at % or more of Co, and the like are preferable.

[0025] (Pretreatment of the substrate surface) The surface of the substrate 1 is preferably pretreated. The treatment agent used for pretreating the surface of substrate 1 (hereinafter sometimes referred to as "pretreatment agent") is not particularly limited as long as it can remove organic matter present on the surface of substrate 1. Specific examples of the pretreatment agent include peroxides such as hydrogen peroxide, perhalogen acids such as periodic acid, oxo acids such as nitric acid and hypochlorous acid, phosphoric acid, citric acid, acetic acid, and hydrofluoric acid (HF). The pretreatment agent may be appropriately selected depending on the type of substrate used. For example, at least one selected from the group consisting of hydrogen peroxide and perhalogen acids is preferable from the viewpoint of treating the metal surface without damaging inorganic substances such as SiO2 and Al2O3 when the inorganic substances coexist on the substrate surface. On the other hand, in the case of a substrate containing Cu, it is preferable to use an aqueous HF solution, acetic acid, citric acid, phosphoric acid, nitric acid, or the like as the pretreatment agent. The pretreatment agent may be used alone or in combination of two or more kinds.

[0026] <Oxidation process> In the oxidation step, the substrate prepared in the substrate preparation step is oxidized. The substrate to be oxidized in the oxidation step may be a substrate prepared in the substrate preparation step on which a natural oxide film is formed by oxidizing metals in the second region 12.

[0027] The oxidation step oxidizes the surface of the metal in the second region 12, or further oxidizes the natural oxide film formed on the surface of the metal in the second region 12, and a metal oxide layer 21 made of a metal oxide obtained by oxidizing the metal is formed on the surface of the second region 12 (FIG. 3(b)). For example, when the metal in the second region 12 is Cu, the oxidation step forms a metal oxide layer 21 made of CuO.

[0028] Although the method for oxidizing the substrate is not particularly limited, it is preferable to use at least one of ozone and hydrogen peroxide as an oxidizing agent. For example, there is a method (UVO3) in which the substrate 1 (and thus the metals in the second region 12 or the natural oxide film formed on the surface of the metals in the second region 12) is oxidized with ozone generated by irradiating an oxygen-containing gas such as air with ultraviolet light or atomic oxygen generated by dissociation of ozone, and a method in which the substrate 1 is oxidized by immersing the substrate 1 in hydrogen peroxide water.

[0029] Here, if a native oxide film is formed on the substrate prepared in the substrate preparation step, the native oxide film may be composed of metal oxides with different valences. For example, if the metal in the second region 12 is Cu, the native oxide film on the substrate surface may contain CuO and Cu2O. According to the above-mentioned method of oxidizing the substrate with ozone generated by irradiating an oxygen-containing gas with ultraviolet light or atomic oxygen generated by ozone dissociation (UVO3), or the method of immersing the substrate in hydrogen peroxide water, a metal oxide layer 21 composed of CuO can be formed. Note that CuO can be easily reduced by a surface treatment agent in the subsequent exposure step.

[0030] <Exposure process> In the exposure step, after the oxidation step, the surface of the substrate is exposed to a surface treatment agent containing a thiol having 8 or less carbon atoms, thereby forming a surface treatment film on the second region. After the oxidation step, the surface of the substrate is exposed to a surface treatment agent containing a thiol having 8 or less carbon atoms, whereby a surface treatment film 22 derived from a thiol having 8 or less carbon atoms is selectively formed on the second region 12 out of the first region 11 and the second region 12, as shown in the examples described below (Figure 3(c)). Even if the surface treatment film 22 formed is thick (for example, the thickness of the surface treatment film 22 is 10 nm or more), as shown in the examples described later, the surface treatment film 22 can be prevented from protruding into the first region 11. Therefore, the surface treatment film 22 having good rectangularity can be formed on the second region 12.

[0031] It is presumed that the protrusion of the surface treatment film 22 into the first region 11 can be suppressed even if the surface treatment film 22 is thick due to the following mechanism. An organic compound having a mercapto group (SH) easily transfers electrons to and from a metal oxide, but does not easily react with an insulator, which does not easily transfer electrons to and from the metal oxide. Therefore, a thiol having 8 or less carbon atoms selectively reacts (e.g., is adsorbed) with the metal oxide layer 21 formed on the surface of the second region 12. The thiol having 8 or less carbon atoms reduces the metal oxide layer 21 to metal and also turns into a disulfide to form a self-assembled monolayer (SAM) on the metal surface of the second region 12. The SAM derived from this thiol having 8 or less carbon atoms improves the contact angle of the surface of the second region 12 with water. A part of the metal generated by reducing the metal oxide layer 21 functions as an adhesive for the SAM. As a result, a structure in which SAM and metal are alternately repeated, including a bond of -SAM-metal-SAM-, can be formed. For this reason, it is considered that the surface treatment film 22 can be made thicker than a monomolecular film of SAM. The surface treatment film 22 can be said to be a multilayer film in which SAMs of thiols having 8 or less carbon atoms are laminated via metals. Here, if the thickness of the surface treatment film 22 is increased, a problem occurs in that the surface treatment film 22 protrudes onto the surface of the first region 11 . However, by using a thiol having 8 or less carbon atoms, the number of carbon atoms can prevent the surface treatment film 22 from spilling out into the first region 11. Even when the first region 11 and the second region 12 are fine (for example, when the narrowest portion of the first region 11 or the second region 12 is 20 nm or more and 80 nm or less when the first region 11 and the second region 12 are viewed in plan), the surface treatment film 22 can be prevented from spilling out into the first region 11. On the other hand, when a thiol having more than 8 carbon atoms is used, the film can be made thick to some extent, but the surface treatment film 22 tends to protrude into the first region 11 to a large extent, and the rectangular shape of the surface treatment film 22 becomes poor.

[0032] (Surface treatment agent) The surface treatment agent used in the exposure step contains a thiol having 8 or less carbon atoms.

[0033] The number of carbon atoms in the thiol contained in the surface treatment agent may be 8 or less, preferably 6 or less, and more preferably 5 or less. There is no particular lower limit to the number of carbon atoms in the thiol contained in the surface treatment agent, but 3 or more is preferred.

[0034] The thiol having 8 or less carbon atoms may be an alkanethiol or an aromatic thiol. The alkyl group of the alkanethiol may be linear or branched, but is preferably linear. Alkanethiols include butanethiol, pentanethiol, hexanethiol, heptanethiol, and octanethiol. Examples of the aromatic thiol include toluene thiol and benzene thiol.

[0035] The thiol having 8 or less carbon atoms may be used alone or in combination of two or more kinds.

[0036] The content of thiol having 8 or less carbon atoms in the surface treatment agent is not particularly limited, but is preferably 0.001% by mass or more and 20% by mass or less, more preferably 0.05% by mass or more and 10% by mass or less, and even more preferably 0.1% by mass or more and 5% by mass or less, relative to the total mass of the surface treatment agent.

[0037] The surface treatment agent may contain a solvent, but may not substantially contain a solvent. From the viewpoint of ease of surface treatment of a substrate by immersion, spin coating, or the like, it is preferable that the surface treatment agent contains a solvent. When the surface treatment agent does not substantially contain a solvent, the content of the solvent in the surface treatment agent is 5% by mass or less, preferably 1% by mass or less, and more preferably 0.1% by mass or less. When the surface treatment agent contains a solvent, the amount of the solvent may be appropriately adjusted, for example, within the range of more than 5 mass% and not more than 99.99 mass%. For example, the amount of the solvent may be the remainder of the thiol having 8 or less carbon atoms contained in the surface treatment agent. When the surface treatment agent contains a solvent, the blending amount of the solvent is preferably from 80% by mass to 99.9% by mass, more preferably from 90% by mass to 99.5% by mass.

[0038] The solvent may be an organic solvent or water. Specific examples of organic solvents include sulfoxides, sulfones, amides, lactams, imidazolidinones, dialkyl glycol ethers, monoalcohol solvents, (poly)alkylene glycol monoalkyl ethers, (poly)alkylene glycol monoalkyl ether acetates, other ethers, ketones, other esters, lactones, linear, branched, or cyclic aliphatic hydrocarbons, aromatic hydrocarbons, and terpenes.

[0039] The sulfoxides include dimethyl sulfoxide.

[0040] Examples of sulfones include dimethyl sulfone, diethyl sulfone, bis(2-hydroxyethyl) sulfone, and tetramethylene sulfone.

[0041] Examples of amides include N,N-dimethylformamide, N-methylformamide, N,N-dimethylacetamide, N-methylacetamide, and N,N-diethylacetamide.

[0042] Examples of lactams include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-propyl-2-pyrrolidone, N-hydroxymethyl-2-pyrrolidone, and N-hydroxyethyl-2-pyrrolidone.

[0043] Examples of imidazolidinones include 1,3-dimethyl-2-imidazolidinone, 1,3-diethyl-2-imidazolidinone, and 1,3-diisopropyl-2-imidazolidinone.

[0044] Examples of dialkyl glycol ethers include dimethyl glycol, dimethyl diglycol, dimethyl triglycol, methyl ethyl diglycol, diethyl glycol, and triethylene glycol butyl methyl ether.

[0045] Examples of monoalcohol solvents include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-pentanol, isopentanol, 2-methylbutanol, sec-pentanol, tert-pentanol, 3-methoxybutanol, 3-methyl-3-methoxybutanol, n-hexanol, 2-methylpentanol, sec-hexanol, 2-ethyl-1-butanol, sec-heptanol, 3-heptanol, 1-octanol, and the like. Examples of the alcohols that can be used include ethanol, 2-ethylhexanol, sec-octanol, n-nonyl alcohol, 2,6-dimethyl-4-heptanol, n-decanol, sec-pentadecyl alcohol, trimethylnonyl alcohol, sec-tetradecyl alcohol, sec-heptadecyl alcohol, methyl isobutyl carbinol, phenol, cyclohexanol, methylcyclohexanol, 3,3,5-trimethylcyclohexanol, benzyl alcohol, phenylmethylcarbinol, diacetone alcohol, and cresol.

[0046] Examples of (poly)alkylene glycol monoalkyl ethers include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol monomethyl ether, and tripropylene glycol monoethyl ether.

[0047] Examples of the (poly)alkylene glycol monoalkyl ether acetates include ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate.

[0048] Examples of other ethers include dimethyl ether, diethyl ether, methyl ethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, diisoamyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol monobutyl ether, diethylene glycol diethyl ether, tetraethylene glycol dimethyl ether, and tetrahydrofuran.

[0049] Examples of ketones include methyl ethyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, and 2,6-dimethyl-4-heptanone.

[0050] Other esters include, for example, alkyl lactate esters such as methyl lactate and ethyl lactate; ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, 3-methoxybutyl acetate, 3-methyl-3-methoxy-1-butyl acetate, 3-methyl-3-methoxybutylpropionate, ethyl acetate, and acetic acid. Examples of the ethyl acetate include n-propyl, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-pentyl acetate, n-hexyl acetate, n-heptyl acetate, n-octyl acetate, n-pentyl formate, isopentyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, butyl butyrate, methyl n-octanoate, methyl decanoate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl 2-oxobutanoate, dimethyl adipate, and propylene glycol diacetate.

[0051] Examples of lactones include propylolactone, γ-butyrolactone, and 6-pentyrolactone.

[0052] Examples of linear, branched, or cyclic aliphatic hydrocarbons include n-hexane, n-heptane, n-octane, n-nonane, methyloctane, n-decane, n-pentane, n-dodecane, 2,2,4,6,6-pentamethylheptane, 2,2,4,4,6,8,8-heptamethylnonane, cyclohexane, and methylcyclohexane.

[0053] Examples of aromatic hydrocarbons include benzene, toluene, benzotrifluoride, xylene, 1,3,5-trimethylbenzene, naphthalene, and decahydronaphthalene.

[0054] Examples of terpenes include p-menthane, diphenylmenthane, limonene, terpinene, bornane, norbornane, and pinane.

[0055] The relative dielectric constant of the solvent is preferably 35 or less, and more preferably 20 or less. Examples of solvents having such a low dielectric constant include methanol (dielectric constant: 33), isopropanol (IPA) (dielectric constant: 18.3), diethylene glycol monobutyl ether (BDG) (dielectric constant: 13.70), propylene glycol monomethyl ether (PE) (dielectric constant: 12.71), benzyl alcohol (dielectric constant: 13.70), 2-heptanone (dielectric constant: 11.74), ethylene glycol monobutyl ether acetate (dielectric constant: 8.66), tert-butanol (dielectric constant: 12.5), 1-octanol (dielectric constant: 10.21), isobutanol (dielectric constant: 18.22), benzotrifluoride (dielectric constant: 9.18), decahydronaphthalene (dielectric constant: 2.16), cyclohexane (dielectric constant: 13.70), and 2-heptanone (dielectric constant: 11.74). Dielectric constant: 1.99), decane (dielectric constant: less than 1), ethyl lactate (EL) (dielectric constant: 13.22), diethylene glycol monomethyl ether (dielectric constant: 15.76), 1-nonanol (dielectric constant: 9.13), toluene (dielectric constant: 2.37), propylene glycol monomethyl ether acetate (PM) (dielectric constant: 9.4), methyl isobutyl carbinol (MIBC) (dielectric constant: 10.47), 2,6-dimethyl-4-heptanol (dielectric constant: 2.98), 2-ethyl-1-butanol (dielectric constant: 12.6), 2-butanone oxime (dielectric constant: 2.9), n-dibutyl ether (dielectric constant: 3.33), butyl butyrate (dielectric constant: 4.55), 2,6-dimethyl-4-heptanone (dielectric constant: 9.82), etc.

[0056] The solvent may be used alone or in combination of two or more kinds.

[0057] (Other ingredients) Examples of other components that may be incorporated into the surface treatment agent include acids, basic nitrogen-containing compounds, pH adjusters, antioxidants, ultraviolet absorbers, viscosity adjusters, and antifoaming agents.

[0058] (Method of manufacturing surface treatment agent) The surface treatment agent can be obtained by mixing a thiol having 8 or less carbon atoms, a solvent containing the thiol as necessary, and other components by a known method.

[0059] (exposure) The method for exposing the surface of the substrate to the surface treatment agent may be a liquid phase method or a gas phase method. Examples of liquid phase methods include a method in which the surface treatment agent is applied (eg, coated) to the surface of the substrate and exposed by means of, for example, an immersion method or a coating method such as a spin coating method, a roll coating method, or a doctor blade method. An example of the gas phase method is a method in which the surface of the substrate is exposed to vapor containing a thiol having 8 or less carbon atoms as a surface treatment agent. The atmosphere in which the vapor is exposed may be either atmospheric pressure or reduced pressure, and reduced pressure is preferred.

[0060] The exposure temperature is, for example, 10°C or higher and 90°C or lower, preferably 20°C or higher and 80°C or lower, more preferably 20°C or higher and 70°C or lower, and even more preferably 20°C or higher and 30°C or lower. From the viewpoint of thickening the surface treatment film to be formed, the exposure time is preferably 20 seconds or more, more preferably 30 seconds or more, and even more preferably 45 seconds or more. The upper limit of the exposure time is not particularly limited, but is, for example, 2 hours or less, typically 1 hour or less, preferably 15 minutes or less, more preferably 5 minutes or less, and particularly preferably 2 minutes or less.

[0061] <Solvent cleaning process> After the exposure step, a solvent cleaning step may be performed in which the substrate 1 on which the surface treatment film 22 has been formed is cleaned with a solvent. By washing the substrate 1 on which the surface treatment film 22 is formed with a solvent, it is possible to remove the surface treatment film 22 on the first region 11 when the surface treatment film 22 is formed on the first region 11 in the exposure process, i.e., when the surface treatment film 22 protrudes onto the first region 11 in the exposure process.

[0062] The solvent used in the solvent washing step includes alcohol and fatty acid alkyl ester. Alcohols include methanol, ethanol, 1-propanol, 2-propanol (IPA), 1-butanol, 2-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 4-methyl-2-pentanol, 2,2-dimethyl-1-propanol, benzyl alcohol, and phenethyl alcohol. Examples of fatty acid alkyl esters include ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-pentyl formate, isopentyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, and ethyl 2-oxobutanoate.

[0063] The solvent used for washing in the solvent washing step may be one type or two or more types. When two or more kinds of solvents are used, a mixed solvent of two or more kinds of solvents may be used, or the substrate may be washed with one kind of solvent, dried as necessary, and then washed with another solvent. For example, washing with alcohol may be followed by washing with a fatty acid alkyl ester.

[0064] <Drying process> A drying step of drying the substrate may be included as necessary after the exposure step, cleaning step, etc. Drying is performed by, for example, blowing nitrogen.

[0065] According to the above-described method for forming a surface treatment film, even if the film thickness is large, the surface treatment film 22 can be selectively formed on the second region 12 in such a manner that the surface treatment film 22 is prevented from spilling over into the first region 11. The thickness of the surface treatment film 22 can be, for example, 10 nm or more. Therefore, when a CVD film is formed on the first region 11 by a CVD method such as an ALD method after the surface treatment film 22 is formed on the second region 12, overhang of the CVD film can be suppressed even if the CVD film is thick (for example, even if it is 20 nm or more). In addition, since the surface treatment film 22 is prevented from spilling over into the first region 11, the surface treatment film 22 is prevented from interfering with the formation of a CVD film on the first region 11, and the CVD film can be formed more selectively on the first region 11.

[0066] <Method for selectively forming a film on a substrate surface> Using the above-mentioned method for forming a surface treatment film, a film can be formed selectively in regions on the surface of a substrate by a CVD method such as an ALD method. Such an area-selective film formation method on a substrate surface includes a surface treatment film formation step of forming a surface treatment film on the second region by the above-mentioned surface treatment film formation method, and a CVD film formation step of forming a CVD film by a chemical vapor deposition method (CVD method) after the surface treatment film formation step, in which more material of the CVD film is deposited on the first region than on the second region.

[0067] The CVD film is made of a material different from that of the surface treatment film 22, and is formed of, for example, an insulating material such as SiO2. The surface treatment film 22 formed on the second region 12 by the above-mentioned method for forming a surface treatment film can be made thick. Therefore, even if the CVD film formed on the first region 11 is thick, overhang of the CVD film can be suppressed. Furthermore, the surface treatment film 22 formed on the second region 12 by the above-mentioned method for forming a surface treatment film is prevented from spilling over into the first region 11, so that the surface treatment film 22 is prevented from interfering with the formation of a CVD film on the first region 11, and the CVD film can be selectively formed on the first region 11. Hereinafter, film formation by the ALD method (ALD film formation) will be described as an example of the CVD method.

[0068] (Film formation by ALD method) Although the film formation method using the ALD method is not particularly limited, it is preferably a thin film formation method by adsorption using at least two gas phase reactants (hereinafter simply referred to as "precursor gases"). The adsorption using the precursor gas is preferably chemical adsorption. Specifically, the method includes a method including the following steps (a) and (b), which are repeated at least once (one cycle) until a desired film thickness is obtained. (a) exposing a substrate on which a surface treatment film has been formed by the method for forming a surface treatment film to a pulse of a first precursor gas; (b) following step (a) above, exposing the substrate to a pulse of a second precursor gas.

[0069] After the above step (a) and before the above step (b), a plasma treatment step, a step of removing or evacuating (purging) the first precursor gas and its reactants using a carrier gas, a second precursor gas, etc., may or may not be included. After the above step (b), a plasma treatment step, a step of removing or purging the second precursor gas and its reactants with a carrier gas or the like, and the like may or may not be included. The carrier gas may be an inert gas such as nitrogen gas, argon gas, or helium gas.

[0070] Preferably, each pulse per cycle and each layer formed is self-limiting, and more preferably, each layer formed is a monolayer. The thickness of the monoatomic layer can be, for example, 5 nm or less, preferably 3 nm or less, more preferably 1 nm or less, and further preferably 0.5 nm or less.

[0071] Examples of the first precursor gas include organic metals, metal halides, and metal oxide halides, and specific examples thereof include tantalum pentaethoxide, tetrakis(dimethylamino)titanium, pentakis(dimethylamino)tantalum, tetrakis(dimethylamino)zirconium, tetrakis(dimethylamino)hafnium, tetrakis(dimethylamino)silane, copper hexafluoroacetylacetonate vinyltrimethylsilane, Zn(C2H5)2, Zn(CH3)2, TMA (trimethylaluminum), TaCl5, WF6, WOCl4, CuCl, ZrCl4, AlCl3, TiCl4, SiCl4, and HfCl4.

[0072] The second precursor gas may be a precursor gas capable of decomposing the first precursor or a precursor gas capable of removing a ligand of the first precursor, such as H2O, H2O2, O2, O3, NH3, H2S, H2Se, PH3, AsH3, C2H4, or Si2H6.

[0073] The exposure temperature in step (a) is not particularly limited, but is, for example, 25°C or higher and 800°C or lower, preferably 50°C or higher and 650°C or lower, more preferably 100°C or higher and 500°C or lower, and even more preferably 150°C or higher and 375°C or lower.

[0074] The exposure temperature in step (b) is not particularly limited, but may be a temperature substantially equal to or higher than the exposure temperature in step (a). Films formed by the ALD method are not particularly limited, and examples thereof include films containing pure elements (e.g., Si, Cu, Ta, W), films containing oxides (e.g., SiO2, GeO2, HfO2, ZrO2, Ta2O5, TiO2, Al2O3, ZnO, SnO2, Sb2O5, B2O3, In2O3, WO3), films containing nitrides (e.g., Si3N4, TiN, AlN, BN, GaN, NbN), films containing carbides (e.g., SiC), films containing sulfides (e.g., CdS, ZnS, MnS, WS2, PbS), films containing selenides (e.g., CdSe, ZnSe), films containing phosphides (GaP, InP), films containing arsenides (e.g., GaAs, InAs), and mixtures thereof. EXAMPLES

[0075] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0076] [Example 1] (Preparation of Surface Treatment Agent) A surface treatment agent was prepared by dissolving 1-octanethiol in n-octanol (organic solvent) so that the amount of the 1-octanethiol was 2 mass % relative to the total mass of the surface treatment agent.

[0077] (Pretreatment, surface treatment) A substrate 1 having Cu and SiO2 on its surface was prepared (substrate preparation step). As shown in Fig. 5(a), the surface of the substrate 1 has a pattern shape in which a plurality of first regions 11 made of rectangular SiO2 with a width a1 of 50 nm and a plurality of second regions 12 made of rectangular Cu with a width a2 of 50 nm are alternately arranged in lines when viewed from above. Fig. 5 is a schematic diagram of the substrate 1 used in the example, Fig. 5(a) is a plan view, and Fig. 5(b) is a cross-sectional view taken along the line A-A' in Fig. 5(a). The prepared substrate having Cu and SiO2 on its surface was subjected to a surface treatment using the obtained surface treatment agent according to the following method. Specifically, the substrates having Cu and SiO2 on the surface were pretreated by immersing them in a 0.5% by mass HF aqueous solution at 25°C for 1 minute without stirring. After the pretreatment, each substrate was washed with deionized water (DIW) for 1 minute. After washing with water, the substrate was dried for 1 minute with a nitrogen gas flow. After drying, the substrate was placed for 10 minutes in an atmosphere in which ozone was generated by irradiating air with ultraviolet light using a Hg lamp, thereby oxidizing the Cu on the substrate surface and forming a CuO layer on the substrate surface (oxidation process). Next, the substrate was immersed in the surface treatment agent at 25° C. for 1 minute without stirring to expose the substrate to the surface treatment agent (exposure step). Thereafter, the substrate was immersed in isopropanol (IPA) at 25° C. for 1 minute without stirring, and then dried for 1 minute in a nitrogen stream to obtain a substrate on which a surface treatment film was formed.

[0078] [Example 2] The same procedure as in Example 1 was carried out, except that 1-hexanethiol was used instead of 1-octanethiol.

[0079] [Example 3] The same procedure as in Example 1 was carried out, except that 1-butanethiol was used instead of 1-octanethiol.

[0080] [Example 4] The substrate was immersed in isopropanol (IPA) at 25° C. for 1 minute without stirring, then dried in a nitrogen stream for 1 minute, and then immersed in butyl butyrate at 25° C. for 1 minute without stirring, washed with deionized water for 1 minute, and then dried in a nitrogen stream for 1 minute. The same operations as in Example 3 were performed.

[0081] [Example 5] The same procedure as in Example 1 was carried out, except that p-toluenethiol was used instead of 1-octanethiol.

[0082] [Comparative Example 1] The same procedure as in Example 3 was carried out, except that the oxidation step was not carried out.

[0083] [Comparative Example 2] The same procedure as in Example 1 was carried out, except that 1-dodecanethiol was used instead of 1-octanethiol.

[0084] [Comparative Example 3] The same procedure as in Example 1 was carried out, except that 1-decanethiol was used instead of 1-octanethiol.

[0085] (Measurement of the thickness of the surface treatment film) For each of the obtained substrates, the thickness of the surface treatment film formed on Cu was measured by fluorescent X-ray analysis and evaluated according to the following criteria. The results are shown in the "Film Thickness" column of Table 1. ○: The thickness of the surface treatment film is 10 nm or more. ×: The thickness of the surface treatment film is less than 10 nm.

[0086] (Evaluation of rectangularity (extension of surface treatment film onto SiO2)) The surface treatment film of each of the obtained substrates was observed by AFM (atomic force microscope) analysis (instrument name: Dimension Icon, manufactured by Bruker), and the rectangularity was evaluated according to the following criteria. The results are shown in Table 1. ◎: Very good rectangular shape ◯: Good rectangular shape ×: Defective shape is observed

[0087] (Selectivity evaluation) For each of the obtained substrates, the adhesive force on the second region (Cu) 12 and the adhesive force on the first region (SiO2) 11 were measured by AFM (atomic force microscope) analysis (instrument name: Dimension Icon, manufactured by Bruker) under the measurement conditions of an observation area of ​​1 μm × 1 μm and 256 scans, and the difference in adhesive force was calculated using the following formula. The larger the difference in adhesive force, the higher the selectivity, which means that a surface treatment film is selectively formed on the Cu surface out of Cu and SiO2. The results are shown in Table 1. Difference in adhesive force [nN] = adhesive force on first area [nN] - adhesive force on second area [nN]

[0088] [Table 1]

[0089] As shown in Table 1, the surface treatment films of Examples 1 to 5 formed by the method for forming a surface treatment film including a substrate preparation step of preparing a substrate having a surface with a first region where an insulator (SiO2) is exposed and a second region where a metal (Cu) is exposed, an oxidation step of oxidizing the surface of the second region, and an exposure step of exposing the surface of the substrate to a surface treatment agent containing a thiol having 8 or less carbon atoms to form a surface treatment film on the second region after the oxidation step can suppress the protrusion of the surface treatment film into the first region and have excellent rectangularity even when the surface treatment film has a thickness of 10 nm or more. It can also be seen that the surface treatment films of Examples 1 to 5 are selectively formed on the surface of metals (Cu). On the other hand, the surface-treated film of Comparative Example 1, which did not undergo an oxidation process, and the surface-treated films of Comparative Examples 2 and 3, in which the thiol contained in the surface treatment agent had more than 8 carbon atoms, had a large amount of protrusion into the first region and poor rectangularity. [Explanation of symbols]

[0090] 1 Board 11 First area 12 Second area 21 Metal oxide layer 22 Surface treatment film

Claims

1. a substrate preparation step of preparing a substrate having a surface thereof including a first region in which an insulator is exposed and a second region in which at least one metal selected from a metal and a conductive metal-containing compound is exposed; an oxidation step of oxidizing a surface of the second region; and an exposure step of exposing the surface of the substrate to a surface treatment agent containing a thiol having 8 or less carbon atoms after the oxidation step, thereby forming a surface treatment film on the second region.

2. 2. The method for forming a surface treatment film according to claim 1, wherein the insulator has a recess on the surface of the substrate, and the second region where the metal is exposed is formed in the recess.

3. the insulator is at least one selected from the group consisting of silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, hafnium oxide, tantalum oxide, fluorine-containing silicon oxide, carbon-containing silicon oxide, silicon nitride, boron nitride, silicon carbide, silicon carbonitride, silicon oxynitride, silicon oxycarbonitride, silicon, and silicon doped with at least one selected from phosphorus, boron, and germanium; 2. The method for forming a surface treatment film according to claim 1, wherein the metal is at least one selected from the group consisting of copper, cobalt, molybdenum and ruthenium.

4. The method for forming a surface treatment film according to claim 1 , wherein the thiol includes at least one selected from the group consisting of butanethiol, pentanethiol, hexanethiol, heptanethiol, and octanethiol.

5. 2. The method for forming a surface treatment film according to claim 1, further comprising, after the exposure step, a solvent washing step of washing the substrate on which the surface treatment film has been formed with a solvent.

6. The method for forming a surface treatment film according to claim 5 , wherein the solvent contains a fatty acid alkyl ester.

7. 7. The method for forming a surface treatment film according to claim 1, wherein the surface treatment film has a thickness of 10 nm or more.

Citation Information

Patent Citations

  • Method for producing fine metallic particle

    JP2002294309A

  • Film formation method

    JP2021057563A

  • Film forming method and film forming device

    JP2021108336A

  • Film deposition method and film deposition apparatus

    JP2022055462A

  • A bottomless deposition method for barrier layers in integrated circuit metallization schemes

    JP2003508897A