Method for producing biodegradable resin extruded foam

By extruding and foaming a mixed resin of polybutylene adipate terephthalate and thermoplastic starch with dimethyl ether and crosslinking using an acrylic polymer, the method addresses shrinkage issues in biodegradable resin foams, resulting in a high-quality foam with reduced shrinkage and lower density.

JP2024165387AActive Publication Date: 2024-11-28JSP CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023081541
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28
Estimated Expiration
2043-05-17

AI Technical Summary

Technical Problem

Extruded biodegradable resin foams containing thermoplastic starch exhibit significant shrinkage, compromising their appearance and utility.

Method used

A method involving the extrusion and foaming of a mixed resin composed of polybutylene adipate terephthalate and thermoplastic starch, using a physical blowing agent like dimethyl ether, and crosslinking with an acrylic polymer having an epoxy group, to produce a foam with reduced shrinkage and improved vegetable content.

Benefits of technology

The method effectively suppresses shrinkage of the extruded foam, enabling the production of a high-quality biodegradable resin foam with lower apparent density and enhanced vegetable content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165387000006
    Figure 2024165387000006
  • Figure 2024165387000007
    Figure 2024165387000007
  • Figure 2024165387000001
    Figure 2024165387000001
Patent Text Reader

Abstract

To provide a method for producing a biodegradable resin extruded foam, which enables the creation of a high-quality foam by the extrusion foaming of a biodegradable resin based on a resin mixture of polybutylene adipate terephthalate and thermoplastic starch.SOLUTION: A method for producing a biodegradable resin extruded foam is a process to produce an extruded foam through the extrusion foaming of a foamable molten resin that has been obtained by mixing a biodegradable resin and a foaming agent using an extruder. The biodegradable resin is based on a resin mixture of polybutylene adipate terephthalate and thermoplastic starch. A physical foaming agent contains dimethyl ether.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an extruded biodegradable resin foam. [Background technology]

[0002] Conventionally, an extruded foam using polybutylene adipate terephthalate as a biodegradable resin has been known (Patent Document 1). However, in recent years, due to growing environmental awareness, there has been a demand for environmentally friendly materials, such as the use of plant-derived raw materials. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 2022-511890 Summary of the Invention [Problem to be solved by the invention]

[0004] However, when thermoplastic starch is added to improve the bio-based content of the extruded biodegradable resin foam, the resulting extruded foam tends to shrink, making it difficult to obtain an extruded foam having a good appearance.

[0005] An object of the present invention is to provide a method for producing an extruded biodegradable resin foam, which is capable of producing a good foam with little shrinkage after extrusion foaming by extruding and foaming a biodegradable resin based on a mixed resin of polybutylene adipate terephthalate and thermoplastic starch. [Means for solving the problem]

[0006] According to the present invention, there is provided a method for producing an extruded biodegradable resin foam as described below. [1] A method for producing an extruded biodegradable resin foam, comprising extruding and foaming a foamable resin melt obtained by kneading a biodegradable resin and a foaming agent in an extruder, The method for producing an extruded biodegradable resin foam is characterized in that the biodegradable resin is based on a mixed resin of polybutylene adipate terephthalate and thermoplastic starch, and the foaming agent is a physical foaming agent containing dimethyl ether. [2] The method for producing an extruded biodegradable resin foam according to item 1 above, wherein the blending ratio of the polybutylene adipate terephthalate to the thermoplastic starch is, in mass ratio, polybutylene adipate terephthalate:thermoplastic starch=30:70 to 90:10. [3] The method for producing a biodegradable resin extruded foam according to item 1 or 2 above, wherein the biodegradable resin is crosslinked with an acrylic polymer having epoxy groups and an epoxy equivalent of 100 g / eq. or more and 600 g / eq. or less, and the gel fraction of the extruded foam is 5% by mass or more and 30% by mass or less. [4] The apparent density of the biodegradable resin extruded foam is 20 kg / m 3 More than 250kg / m 3 3. A method for producing an extruded biodegradable resin foam according to 1 or 2 above, which is as follows: Effect of the Invention

[0007] According to the present invention, there is provided a method for extruding and foaming a biodegradable resin having as a base material a mixed resin of polybutylene adipate terephthalate and thermoplastic starch, which method is capable of suppressing shrinkage of the extruded foam after extrusion foaming and producing a good foam. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is an example of a photograph of a cross section of the extruded foam obtained in Example 1. [Diagram 2] FIG. 2 is an example of a photograph of a cross section of the extruded foam obtained in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The method for producing an extruded biodegradable resin foam (hereinafter also referred to as an extruded foam or a foam) of the present invention will be described in detail below. In the production method of the present invention, an extruded foam is produced by extruding and foaming a foamable resin melt obtained by kneading a biodegradable resin and a foaming agent in an extruder.

[0010] The biodegradable resin used in the manufacturing method of the present invention contains a mixed resin of polybutylene adipate terephthalate (hereinafter also referred to as PBAT) and thermoplastic starch as a base material. Polybutylene adipate terephthalate is a copolymer obtained by copolymerizing terephthalic acid, butanediol, and adipic acid, and is a biodegradable thermoplastic resin. Polybutylene adipate terephthalate is generally distributed as a petroleum-derived resin. In this specification, a biodegradable resin refers to a resin that is ultimately decomposed into water and carbon dioxide by the action of microorganisms such as bacteria, fungi, and algae in soil or water, as the molecular bonds of the substance are broken down. Specifically, the biodegradable resin refers to a resin that exhibits biodegradability in at least one of the tests of ISO 9408, ISO 9439, ISO 10707, JIS K 6950, JIS K 6951, JIS K 6953, or JIS K 6955.

[0011] The thermoplastic starch is a processed starch having thermoplastic properties, and has fluidity when heated. For example, starch that has been made fluid by esterifying the hydroxyl groups of starch can be mentioned. Here, starch is a compound with the chemical formula (C6H 10 O5) n It is a carbohydrate (polysaccharide) of plant origin, a natural polymer compound in which many α-glucose molecules are polymerized through glycosidic bonds. By blending thermoplastic starch into the resin, the plant content of the resin can be improved.

[0012] In the biodegradable resin of the present invention, the blending ratio of polybutylene adipate terephthalate to thermoplastic starch is preferably within a range of polybutylene adipate terephthalate: thermoplastic starch=30:70 to 90:10 by mass ratio. If the blending ratio is within this range, the shrinkage of the extruded foam after extrusion foaming is further suppressed, and the effect of improving the bio-based content can be obtained. From this viewpoint, the blending ratio (mass %) is more preferably 40:60 to 85:15, and further preferably 50:50 to 80:20.

[0013] The shrinkage of the resulting extruded foam appears as a phenomenon in which the diameter of the strand becomes smaller in the case of an extruded foam extruded into a strand shape, and as a phenomenon in which the sheet thickness and sheet width become smaller in the case of an extruded foam extruded into a sheet shape.

[0014] Next, the melt properties (melt tension, melt viscosity) of the biodegradable resin will be described. The melt tension of the biodegradable resin is preferably 3 mN to 150 mN, more preferably 5 mN to 110 mN, and even more preferably 8 mN to 50 mN. If the melt tension of the biodegradable resin is within this range, shrinkage of the foam after extrusion foaming can be suppressed, and a foam with a low apparent density (high expansion ratio) can be obtained.

[0015] The melt tension (MT) can be measured, for example, using a Capillograph 1D manufactured by Toyo Seiki Seisakusho Co., Ltd. Specifically, a cylinder with a cylinder diameter of 9.55 mm and a length of 350 mm and an orifice with a nozzle diameter of 2.095 mm and a length of 8.0 mm are used, the set temperature of the cylinder and the orifice is set to 190°C, the required amount of the sample is placed in the cylinder, and after leaving it for 4 minutes, the piston speed is set to 10 mm / min and the molten resin is extruded from the orifice in a string shape, and this string-like material is hung on a tension detection pulley with a diameter of 45 mm, and the take-up speed is increased at a constant rate so that the take-up speed reaches 0 m / min to 200 m / min, and the string-like material is taken up by the take-up roller to obtain the maximum value of the tension just before the string-like material breaks. This operation is performed a total of 5 times, and the maximum values ​​obtained in the 5 times are averaged to obtain the melt tension (mN).

[0016] The melt viscosity of the biodegradable resin is preferably 700 Pa·s or more and 3000 Pa·s or less, and more preferably 800 Pa·s or more and 2900 Pa·s or less. If the melt viscosity of the biodegradable resin is within the above range, an extruded foam can be produced more stably.

[0017] The melt viscosity can be measured, for example, using a measuring instrument such as Capilograph 1D manufactured by Toyo Seiki Seisakusho Co., Ltd. Specifically, a cylinder with a diameter of 9.55 mm and a length of 350 mm and an orifice with a nozzle diameter of 1.0 mm and a length of 10 mm are used, and the set temperatures of the cylinder and orifice are 190° C. 15 g of a sample to be measured is placed in the cylinder, left for 4 minutes to become a molten resin, and then heated at a shear rate of 100 sec -1 The molten resin is extruded from the orifice in a string-like shape, and the viscosity of the molten resin during extrusion is measured; this value is regarded as the melt viscosity.

[0018] The mixed resin of polybutylene adipate terephthalate and thermoplastic starch, which is the base material of the biodegradable resin, is sold as Mater-Bi by Novamont (Italy). Note that in the present invention, it is not necessarily required that the polybutylene adipate terephthalate and thermoplastic starch are melt-mixed and fed into an extruder as a mixed resin, and then heated and melt-kneaded, but it is sufficient that the polybutylene adipate terephthalate and thermoplastic starch are ultimately contained as components constituting the biodegradable resin, and for example, the polybutylene adipate terephthalate and the thermoplastic starch can be separately fed into an extruder, melted, mixed, and extruded and foamed. Mater-Bi has been certified as biodegradable and safe by certification bodies and associations in Japan, Europe, and the United States, and has been confirmed to biodegrade within one year in the ocean.

[0019] The melt properties (melt tension, melt viscosity, etc.) of the biodegradable resin can be adjusted by using a modifier. This makes it possible to further reduce shrinkage after extrusion foaming, even when producing an extruded foam with a lower apparent density. The modifier is preferably one that has the effect of crosslinking the biodegradable resin, and examples of the modifier include acrylic polymers, maleic anhydride-styrene copolymers, dicumyl peroxide, di-tert-butyl peroxide, tert-butyl peroxybenzoate, and the like, as well as their analogs or mixtures thereof, and among these, acrylic polymers are preferred.

[0020] As an example of producing an extruded foam using a modifier, a biodegradable resin can be crosslinked using an acrylic polymer having an epoxy group and an epoxy equivalent of 100 g / eq. or more and 600 g / eq. or less. Specifically, the gel fraction of the resin constituting the extruded foam can be adjusted to 5% by mass or more and 30% by mass or less by feeding the acrylic polymer to the extruder and heating, melting, and kneading the acrylic polymer. In this way, by using the acrylic polymer as a modifier to crosslink PBAT and thermoplastic starch, shrinkage after extrusion foaming can be effectively prevented.

[0021] A specific example of the acrylic polymer is preferably an acrylic polymer containing glycidyl methacrylate as a main component, where the main component means 50% by mass or more of the entire acrylic polymer, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more.

[0022] The above-mentioned phrase "supplying the acrylic polymer to the extruder and heating, melting and kneading" means that a solid acrylic polymer can be supplied to the raw material supply port of the extruder together with a mixed resin of solid PBAT and thermoplastic starch, or that a heated and melted acrylic polymer can be injected through a cylinder into the foamable resin melt flowing in the extruder in the same manner as the injection of a physical foaming agent.

[0023] The epoxy equivalent of the acrylic polymer is preferably 100 g / eq. or more and 600 g / eq. or less. Within this range, it is possible to improve the foamability of the biodegradable resin and reduce shrinkage after extrusion foaming. From this viewpoint, the epoxy equivalent is preferably 110 g / eq. or more and 300 g / eq. or less, and more preferably 130 g / eq. or more and 200 g / eq. or less.

[0024] The epoxy equivalent can be measured according to JIS K7236: 2001. Specifically, a precisely weighed sample is dissolved in chloroform, and acetic acid and a tetraethylammonium bromide acetate solution are added, followed by potentiometric titration with a 0.1 mol / L perchloric acid acetate standard solution to determine the gram equivalent (g / eq.).

[0025] The gel fraction of the extruded foam is preferably adjusted to 5% by mass or more and 60% by mass or less. If the gel fraction is within this range, the PBAT and thermoplastic starch constituting the extruded foam are crosslinked, improving the foamability, and shrinkage after foaming is effectively prevented. From the above viewpoint, the gel fraction is preferably 5% by mass or more and 30% by mass or less, and more preferably 8% by mass or more and 20% by mass or less.

[0026] The gel fraction can be adjusted by adjusting the amount of modifier added, preferably from 0.1 to 2 parts by mass, more preferably from 0.5 to 1.5 parts by mass, relative to 100 parts by weight of the biodegradable resin.

[0027] The gel fraction is measured by hot xylene extraction. Specifically, 0.5 g of a foam sample is placed in a 120-mesh wire bag, and the weight including the wire bag is measured. This wire bag is added to a 150 mL flat-bottom flask for a Soxhlet fat extractor together with 100 mL of xylene, a condenser is attached to the flat-bottom flask, and the mixture is refluxed by heating for 8 hours with a mantle heater. After reflux is complete, the flask is cooled by air cooling, the wire bag is removed, and the wire bag is vacuum-dried at 80°C for 3 hours in a vacuum oven. The weight of the dried wire bag is measured, and the difference in weight with the wire bag before reflux is the xylene insoluble matter (gel), and the gel fraction is calculated by the following formula. Gel fraction (%) = [weight of insoluble matter after drying / weight of foam sample] x 100

[0028] The biodegradable resin is based on a mixed resin of polybutylene adipate terephthalate and thermoplastic starch, but may contain other resin components. Examples of other resin components include thermoplastic resins, such as ethylene-based resins such as high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear low-density polyethylene, linear very low-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-acrylic acid ester copolymer, ethylene-methacrylic acid copolymer, and ethylene-methacrylic acid ester copolymer, polystyrene-based resins such as polystyrene, high-impact polystyrene, and styrene-acrylonitrile copolymer, acrylic resins such as polymethyl methacrylate, and polyester-based resins such as polylactic acid and polyethylene terephthalate. In addition, thermoplastic elastomers such as olefin-based elastomers such as ethylene-hexene copolymer and ethylene-propylene-diene copolymer, and styrene-based elastomers such as styrene-butadiene-styrene block copolymer, styrene-isoprene-styrene block copolymer, and hydrogenated products thereof can also be used as the polymer material. These resins, rubbers, or elastomers may be used in combination of two or more kinds. When the other resin components are contained, the total content of the other resin components is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, based on 100% by mass of the biodegradable resin.

[0029] The biodegradable resin may contain additives such as foam nucleating agents, crystal nucleating agents, flame retardants, flame retardant assistants, antistatic agents, antioxidants, ultraviolet inhibitors, light stabilizers, antibacterial agents, colorants, etc. The amount of such additives is preferably 0.1 to 5 parts by mass relative to 100 parts by mass of the biodegradable resin.

[0030] Next, the foaming agent used in the present invention will be described. As the foaming agent, a physical foaming agent containing dimethyl ether is used. By using dimethyl ether, shrinkage of the extruded foam immediately after extrusion foaming can be suppressed. Dimethyl ether has moderate polarity compared to other blowing agents and has excellent solubility and plasticity in PBAT, so it is possible to set the optimal foaming temperature lower, which is thought to suppress shrinkage.

[0031] The physical foaming agent used in the present invention may contain other physical foaming agents as long as the object of the present invention is not hindered. Even in this case, the content of dimethyl ether in the physical foaming agent is preferably 50% by mass or more, more preferably 70% by mass or more, and further preferably 80% by mass or more. It is particularly preferable to use only dimethyl ether as the physical foaming agent.

[0032] Other physical blowing agents include, for example, saturated aliphatic hydrocarbons such as propane, n-butane, i-butane, n-pentane, i-pentane, and hexane; saturated aliphatic carbon alcohols such as methanol and ethanol; aromatic hydrocarbons such as benzene, xylene, and toluene; halogenated hydrocarbons such as methyl chloride and Freon (registered trademark); ether compounds other than dimethyl ether such as diethyl ether and methyl ethyl ether; water, carbon dioxide, nitrogen, and other inorganic physical blowing agents.

[0033] As long as the object of the present invention is not hindered, a chemical foaming agent may be used in combination with the foaming agent, such as azodicarbonamide, dinitrosopentamethylenetetramine, hydrazoyldicarbonamide, sodium bicarbonate, etc.

[0034] In the present invention, the amount of dimethyl ether can be adjusted to lower the apparent density (increase the expansion ratio) of the resulting extruded foam and to suppress shrinkage after extrusion foaming. Furthermore, the amount of dimethyl ether can be combined with the type and amount of the modifier to adjust the amount of the resulting extruded foam to lower the apparent density (increase the expansion ratio) and to suppress shrinkage after extrusion foaming.

[0035] It is preferable to add a foam nucleating agent to the biodegradable resin. Examples of the foam nucleating agent include inorganic substances such as talc, calcium carbonate, borax, zinc borate, aluminum hydroxide, alum, etc. The amount of the foam nucleating agent added is preferably 0.001 to 10 parts by weight, more preferably 0.01 to 5 parts by weight, per 100 parts by weight of the biodegradable resin. When a foam nucleating agent is added to a biodegradable resin, the foam nucleating agent can be blended as it is, but it is usually preferable to add the foam nucleating agent as a master batch in consideration of dispersibility and the like.

[0036] The extruder used in the present invention may be a known single screw extruder, a known twin screw extruder, a known tandem extruder, etc. The heating temperature of the extruder is preferably 160°C to 220°C, and the foaming temperature is preferably 105°C to 130°C. There is no limitation on the shape of the resulting extruded biodegradable resin foam, but it is usually extruded into a strand or sheet shape.

[0037] Next, the physical properties of the extruded biodegradable resin foam obtained by the method of the present invention will be described. The apparent density of the extruded foam is 20 kg / m 3 More than 250kg / m 3 In particular, in the production method of the present invention, even an extruded foam that has a low apparent density and is prone to shrinkage can be prevented from shrinking. The apparent density of the extruded foam is preferably 40 kg / m or less. 3 More than 200kg / m 3 Less than 50kg / m is preferable. 3 More than 150kg / m 3 The following is more preferred:

[0038] In the present invention, the apparent density is measured as follows. The apparent density was measured by taking a test piece from the obtained extruded foam, i.e., a foam in the form of a strand (column) or sheet, and multiplying the weight (g) of the test piece by the volume (cm 3The volume of the test piece is determined by submerging the test piece in a graduated container filled with water and measuring the rise in the water level (submersion method).

[0039] The average cell diameter of the extruded foam obtained by the present invention is preferably 100 μm or more and 1800 μm or less. If it is within this range, the foam can withstand the shrinkage force of the extruded foam and is prevented from shrinking. From this viewpoint, the average cell diameter is preferably 800 μm or more and 1600 μm or less.

[0040] The open cell ratio of the extruded foam obtained by the present invention is preferably 60% or more, more preferably 70% or more, further preferably 80% or more, and particularly preferably 90% or more. If the open cell ratio is within this range, the extruded foam will have excellent cushioning properties, and when used as a foam substrate for plant growth, for example, plant roots can penetrate into the extruded foam relatively easily.

[0041] In the present invention, the open cell ratio is measured as follows. Test pieces are cut out from the obtained extruded foam, Vx is measured according to procedure C of ASTM-D2856-70 (reapproved in 1976), and the open cell ratio is calculated by the following formula.

[0042] Open cell ratio (%) = 100-{(Vx-W / ρ) x 100 / (Va-W / ρ)} x: True volume of the test piece (the sum of the volume of the closed cell part and the volume of the resin) (cm 3 ) Va: Apparent volume of the test piece determined by the water immersion method (the sum of the volume of the closed cell part, the volume of the open cell part, and the volume of the resin) (cm 3 ) W: weight of test piece (g) ρ: Density of the resin that constitutes the test piece (g / cm 3 )

[0043] The extruded foam obtained by the present invention preferably has a 25% compression set (24 hours) of 10% or less. If the 25% compression set is within this range, it can be suitably used, for example, as a foam substrate for plant growth. From the above viewpoint, the 25% compression set (24 hours) is more preferably 7% or less, even more preferably 5% or less, and particularly preferably 3% or less. If the 25% compression set (24 hours) is within the above range, the extruded foam will be dimensionally stable and will have a flexible shape that is compressible and expandable.

[0044] The 25% compression set (24 hours) is measured as follows. With reference to JIS K 6767, if the foam is in the form of a strand, cut the foam to a length of 25 mm, compress it in the lengthwise direction until it is distorted by 25% from the length in the measurement direction of the test piece, leave it for 22 hours, and measure the thickness 24 hours after the end of compression. When the foam is in sheet form, cut the foam in the extrusion direction or width direction to a length of 25 mm x width of 25 mm, stack the sheets so that the thickness is 25 mm, compress the test piece to a state where it is distorted by 25% from the thickness in the measurement direction, leave it for 22 hours, and measure the thickness after 24 hours. Measurement is performed in the thickness direction.

[0045] The extruded foam of the present invention is expected to be used, for example, as a biodegradable foam for plant growth. EXAMPLES

[0046] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to these examples.

[0047] In the examples and comparative examples, the following raw materials were used. (Raw resin, thermoplastic starch) (1) Abbreviation "Resin 1": "PBAT-thermoplastic starch mixed resin" manufactured by Novamont, product name "Mater-Bi", grade "EF04P" (a mixed resin of PBAT (mass%) and thermoplastic starch (mass%) = 70 / 30 (melting point: 116°C, density: 1.27g / cm3 ) (2) Abbreviation "SGS": "Thermoplastic starch" manufactured by Sankyo Chemical Co., Ltd., product name "SANKYO GOLDEN STARCH (SGS)" (Tg = 58.8 °C, density: 1.32 g / cm 3 ) (3) Abbreviated name "Resin 2": "PBAT" manufactured by BASF, product name "Ecoflex F Blend C1200" (melting point: 117.2°C, density: 1.26g / cm 3 ) and "(2) SGS" mixed resin at 50% by mass:50% by mass

[0048] (Physical foaming agent) (1) Abbreviation "DME": Dimethyl Ether (2) Abbreviation "Butane (Bu)": A mixture of 35% by weight of normal butane and 65% by weight of isobutane

[0049] (Foam nucleating agent) Abbreviation "PO217K": Fine Cell Master "PO217K" (manufactured by Dainichi Seika, LDPE-based): a mixture of citric acid and baking soda

[0050] (Modifier) (1) Abbreviation "G01100": "Epoxy group-containing acrylic polymer" manufactured by NOF Corporation, product name "Marproof G01100" (epoxy equivalent 170g / eq.) (2) Abbreviation "XIRAN": "Maleic anhydride-styrene copolymer" manufactured by Kawahara Oil Chemical Co., Ltd., product name "TDS XIRAN3000P"

[0051] (Extruded foam manufacturing equipment) The manufacturing equipment used was an extruder with an inner diameter of 50 mm, which was provided with a physical foaming agent injection port midway and a die equipped with a resin discharge port (die lip) at its tip.

[0052] Examples 1 to 5 and Comparative Examples 1 to 5: Production of strand-shaped extruded foams A foaming nucleating agent was added to 100 parts by mass of the resin shown in Tables 1 and 2 in the amounts shown in Tables 1 and 2, and mixed. These raw materials were fed into an extruder, heated, melted, and kneaded by setting the extruder cylinder temperature to 220°C, and a physical foaming agent of the type and amount shown in Tables 1 and 2 was fed from a physical foaming agent injection port provided midway through the extruder. After adjusting to the foaming temperature shown in Tables 1 and 2, the mixture was extruded from the die lip into the atmosphere at the discharge rate shown in Table 1 to produce a strand-shaped extruded foam. The physical properties of the resulting extruded foam are shown in Tables 1 and 2.

[0053] [Table 1]

[0054] [Table 2]

[0055] Examples 6 and 7, Comparative Example 6: Production of strand-shaped extruded foam using modifier A foaming nucleating agent was added to 100 parts by mass of the resin shown in Table 3 in the amount shown in Table 3, and a modifier of the type and amount shown in Table 3 was added and mixed. These raw materials were fed into an extruder, heated, melted, and kneaded by setting the extruder cylinder temperature to 220°C, and a physical foaming agent of the type and amount shown in Table 3 was fed from a physical foaming agent injection port provided midway through the extruder. After adjusting to the foaming temperature shown in Table 3, the mixture was extruded from the die lip into the atmosphere at the discharge rate shown in Table 3 to produce a strand-shaped extruded foam. The physical properties of the resulting extruded foam are shown in Table 3.

[0056] [Table 3]

[0057] Example 8: Production of extruded foam in sheet form The resins shown in Table 4 were mixed and dry blended in an amount of foaming nucleating agent shown in Table 4 to obtain 100 parts by mass. These raw materials were fed into an extruder, heated, melted and kneaded at an extruder cylinder temperature of 220°C, and a physical foaming agent shown in Table 4 was fed from a physical foaming agent injection port provided midway. After adjusting to the foaming temperature shown in Table 4, the mixture was extruded from the die lip into the atmosphere at the discharge rate shown in Table 4 to produce a sheet-like extruded foam. The physical properties of the resulting extruded foam are shown in Table 4.

[0058] [Table 4]

[0059] Example 9: Production of sheet-shaped extruded foam using modifier A foaming nucleating agent and a modifier of a type and amount shown in Table 5 were blended and mixed with 100 parts by mass of the resin shown in Table 5 in the blending amounts shown in Table 5. These raw materials were fed into an extruder, heated, melted, and kneaded at an extruder cylinder temperature of 220°C, and a physical foaming agent shown in Table 5 was fed from a physical foaming agent injection port provided midway. After adjusting to the foaming temperature shown in Table 5, the mixture was extruded from the die lip into the atmosphere at the discharge rate shown in Table 5 to produce a sheet-like extruded foam. The physical properties of the resulting extruded foam are shown in Table 5.

[0060] [Table 5]

[0061] Examples 2 to 5 are examples in which the conditions described in Table 1 were changed from Example 1. The obtained extruded foams were evaluated as having good shrinkage prevention properties. Examples 6 and 7 are examples in which the type and amount of modifier shown in Table 1 was used in comparison with Example 1. By using the modifier, it was possible to prevent shrinkage even when extruded foams having a larger diameter and a lower apparent density were obtained.

[0062] Comparative Examples 1 to 4 are examples in which the physical foaming agent was changed from that of Example 1. When dimethyl ether was not used as the physical foaming agent, the obtained extruded foams showed severe shrinkage after foaming. In Comparative Example 5, only thermoplastic starch was used instead of the biodegradable resin, and no extruded foam could be obtained. Comparative Example 6 is an example in which a modifier was used, but the physical foaming agent was changed. When dimethyl ether was not used as the physical foaming agent, the extruded foam obtained showed severe shrinkage after foaming, even when a modifier was used.

[0063] Example 8 is an example of producing a sheet-like foam. By using dimethyl ether as a physical foaming agent, the obtained extruded foam had a high expansion ratio and was evaluated as having good shrinkage prevention properties. Example 9 is an example of producing a sheet-shaped foam using a modifier. By using the modifier, the obtained extruded foam had a larger thickness and a lower apparent density.

[0064] The melt viscosities and melt tensions in Tables 1 to 5 were measured using the raw material resin itself in the case of raw material resins, and when modified with a modifier, measurements were performed using a separately modified sample.

[0065] The various physical properties in Tables 1 to 5 were measured as follows.

[0066] The strand diameter was determined by measuring the maximum diameter of a cross section of a strand-shaped extruded foam with a vernier caliper and calculating the arithmetic average value of at least 10 points.

[0067] The thickness of the sheet was determined as an average thickness by measuring the thickness at a plurality of specific locations on the sheet at 10 mm intervals across the width direction with a vernier caliper and calculating the arithmetic mean of these values.

[0068] The apparent density was calculated by dividing the weight of the test piece (g) by the volume of the test piece (cm 3) and convert to units to obtain the arithmetic average value of the five locations.

[0069] The open cell ratio was measured by the above-mentioned method and calculated as the arithmetic average value of five samples.

[0070] Cross-sectional photographs of the extruded foam were taken by cutting the strand-shaped extruded foam in a direction perpendicular to the longitudinal direction, and then photographing the cut surface as an enlarged photograph of the entire cut surface using a microscope such as a scanning electron microscope.

[0071] The 25% compression set (24 h) was measured by the above-mentioned method (n=5).

[0072] The gel fraction was measured by the method described above.

[0073] (Shrinkage evaluation) The diameter D0 of the extruded foam immediately after it is extruded from the die lip and the diameter D of the extruded foam after 24 hours 24 The shrinkage rate (%) was calculated from the following formula (n=5). Shrinkage rate (%) = [(D0-D 24 ) / D0]×100

[0074] The obtained shrinkage rate (%) was used to evaluate the shrinkage property according to the following criteria. ⊚: The shrinkage rate is 15% or less. Good: The shrinkage rate is greater than 15% and less than or equal to 20%. ×: Shrinkage rate is more than 20%.

Claims

1. A method for producing an extruded biodegradable resin foam, comprising extruding and foaming a foamable resin melt obtained by kneading a biodegradable resin and a foaming agent in an extruder, The method for producing an extruded biodegradable resin foam is characterized in that the biodegradable resin is based on a mixed resin of polybutylene adipate terephthalate and thermoplastic starch, and the foaming agent is a physical foaming agent containing dimethyl ether.

2. The method for producing a biodegradable resin extruded foam according to claim 1, wherein the blending ratio of the polybutylene adipate terephthalate to the thermoplastic starch is, in mass ratio, polybutylene adipate terephthalate:thermoplastic starch=30:70 to 90:

10.

3. 3. The method for producing a biodegradable resin extruded foam according to claim 1 or 2, wherein the biodegradable resin is crosslinked with an acrylic polymer having an epoxy group and an epoxy equivalent of 100 g / eq. to 600 g / eq., and the gel fraction of the extruded foam is 5% by mass to 30% by mass.

4. The apparent density of the extruded biodegradable resin foam is 20 kg / m 3 More than 250kg / m 3 The method for producing an extruded biodegradable resin foam according to claim 1 or 2, wherein the method is as follows:

Citation Information

Patent Citations

  • Method for manufacturing aliphatic-aromatic copolyester resin foam, and foamed sheet

    JP2004058352A

  • Biodegradable and industrially compostable injection-molded microflexible foams and methods for their manufacture

    JP2021524408A

  • Biodegradable foam substrate for plant growth, plant system using same, and method for manufacturing same