Stainless steel wire, stainless steel component and wire rod for stainless steel wire

JP2024165475APending Publication Date: 2024-11-28NIPPON STEEL STAINLESS STEEL CORP

Patent Information

Application Number
JP2023081710
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28

AI Technical Summary

Benefits of technology

【0013】 本発明のステンレス鋼線は、成分組成として、低Niではあるものの式(a)のA値を調整し、CuとNを複合添加するとともに、最終伸線における総伸線減面率と最終伸線速度を制御することにより、伸線後の焼鈍を行わずに、高強度·高延性を確保し、製網性を確保できるステンレス鋼線を実現することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165475000001
    Figure 2024165475000001
  • Figure 2024165475000002
    Figure 2024165475000002
  • Figure 2024165475000003
    Figure 2024165475000003
Patent Text Reader

Abstract

To provide a stainless steel wire, a stainless steel component and a wire rod for stainless steel wire in which high strength and high ductility are secured and net-manufacturing property can be secured even in the state where super wire drawing processing is kept being executed.SOLUTION: A stainless steel wire contains Ni:3.0 to 10.0%, Cr:17.0 to 25.0%, N:0.10 to 0.50%, and Cu:0.5 to 4.0%, and has a value A shown by formula (a) of -60 or less, and dislocation density of an austenite phase of a steel wire of 1 to 100×1015 / m2 or less. Tensile strength is 1900 to 4500 MPa, and a percentage reduction of area after rupture is 10% or more. By controlling a total wire drawing reduction rate of area and a final drawing speed in final wire drawing, a stainless steel wire in which high strength and high ductility are secured, and net-manufacturing property can be secured without performing annealing after wire drawing is realized.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stainless steel wire, a stainless steel part, and a wire rod for a stainless steel wire. [Background technology]

[0002] Conventionally, stainless steel fine wire products such as wire mesh, iron cores for communication, and screen mesh have been manufactured by processing and forming austenitic stainless steel wire rods and steel wires, such as SUS304 and SUS316, and then subjecting them to high-temperature heat treatment to ensure ductility. However, in the case of stainless steel fine wire products processed and manufactured from austenitic stainless steel wire rods as described above, the heat treatment time per weight increases during high-temperature heat treatment of the fine wires, resulting in high process costs, long construction periods, and high environmental loads. In addition, the alloy costs of the material are high, so there is a demand for process reduction and alloy reduction.

[0003] The invention described in Patent Document 1 is an inexpensive method for producing highly ductile thin wire, which controls gamma stability by adjusting the component composition, performs strong drawing of 80% or more to a diameter of φ300 μm or less, and performs ultra-short-time strand annealing as annealing after wiredrawing.

[0004] The invention described in Patent Document 2 is a wire rod for ultra-fine wire in which inclusions are controlled by reducing the Al content and performing special melting in a vacuum, and C>3N is controlled for drawability. This wire rod and steel wire can be drawn to ultra-fine wires, and annealing after drawing imparts high strength and high ductility to the wire rod and steel wire.

[0005] The invention described in Patent Document 3 relates to an ultra-fine SUS304 wire containing 0.1 to 0.5% N, in which the austenite structure is refined to a specified grain size or greater by wiredrawing and heat treatment, thereby achieving the target yield strength and elongation values. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 4098171 [Patent Document 2] Patent No. 6491983 [Patent Document 3] Patent No. 4068216 Summary of the Invention [Problem to be solved by the invention]

[0007] Regarding the total wiredrawing reduction in area up to the final wiredrawing when wiredrawing is performed on a wire rod after hot wire rolling and further after solution treatment, or the total wiredrawing reduction in area up to the final wiredrawing in wiredrawing after intermediate strand annealing when preliminary wiredrawing and intermediate strand annealing are performed, when the total wiredrawing reduction in area is 95.0% or more, it is hereinafter referred to as "ultra-wiredrawing".

[0008] The inventions described in the above Patent Documents 1 to 3 are all directed to stainless steel wire rods, fine wires, and ultra-fine wires that are assumed to undergo heat treatment after wiredrawing, and do not consider providing a method for inexpensively producing a high-strength, high-ductility steel wire by ultra-drawing as is, or providing said steel wire or wire rod for said steel wire.

[0009] An object of the present invention is to provide a stainless steel wire, a stainless steel part, and a wire rod for a stainless steel wire, which ensures high strength and high ductility even after ultra-wiredrawing and can ensure mesh-forming properties, in order to produce a high-strength, high-ductility stainless steel wire at low cost. [Means for solving the problem]

[0010] That is, the gist of the present invention is as follows. [1] In mass percent, C:0.01~0.20%, Si:0.1~4.0%, Mn:0.1~10.0%, Ni:3.0~10.0%, Cr:17.0~25.0%, Mo:0.1~4.0%, N:0.10~0.50%, Cu:0.5~4.0%, V:0~2.5%, B:0~0.012%, Al:0~2.0%, W:0~2.5%, Ga:0~0.0500%, Co:0~2.5%, Sn:0~2.5%, Ti: 0~1.0%, Nb:0~2.5%, Ta:0~2.5%, Ca:0~0.012%, Mg:0~0.012%, Zr:0~0.012%, REM:0~0.05%, with the remainder being Fe and impurities, The A value represented by the following formula (a) is -60 or less, The dislocation density of the austenite phase of stainless steel wire is 1×10 15 / m 2 ~100×10 15 / m 2 That is, Stainless steel wire. A value=551-462(C+N)-9.2Si―8.1Mn―29(Ni+Cu)-13.7Cr―18.5Mo … (a) However, the element symbol in formula (a) means the content (mass%) of the element in the steel. When the content of an element in formula (a) is 0%, "0" is substituted for the corresponding symbol in the calculation. [2]Further, in mass percent, containing one or more selected from V: 0.001-2.5%, B: 0.001-0.012%, Al: 0.001-2.0%, W: 0.05-2.5%, Ga: 0.0004-0.0500%, Co: 0.05-2.5%, Sn: 0.01-2.5%, Ti: 0.01-1.0%, Nb: 0.01-2.5%, Ta: 0.01-2.5%, Ca: 0.0002-0.012%, Mg: 0.0002-0.012%, Zr: 0.0002-0.012%, and REM: 0.0002-0.05%, [1] The stainless steel wire according to claim 1. [3] The stainless steel wire according to [1] or [2], which has a tensile strength of 1900 to 4500 MPa and a fracture reduction of 10% or more.

[0011] [4] A stainless steel part using the stainless steel wire according to any one of [1] to [3].

[0012] [5] In mass percent, C:0.01~0.20%, Si:0.1~4.0%, Mn:0.1~10.0%, Ni:3.0~10.0%, Cr:17.0~25.0%, Mo:0.1~4.0%, N:0.10~0.50%, Cu:0.5~4.0%, V:0~2.5%, B:0~0.012%, Al:0~2.0%, W:0~2.5%, Ga:0~0.0500%, Co:0~2.5%, Sn:0~2.5%, Ti: 0~1.0%, Nb:0~2.5%, Ta:0~2.5%, Ca:0~0.012%, Mg:0~0.012%, Zr:0~0.012%, REM:0~0.05%, with the remainder being Fe and impurities, The A value represented by the following formula (a) is -60 or less. Wire rod for stainless steel wire. A value=551-462(C+N)-9.2Si―8.1Mn―29(Ni+Cu)-13.7Cr―18.5Mo … (a) However, the element symbol in formula (a) means the content (mass%) of the element in the steel. When the content of an element in formula (a) is 0%, "0" is substituted for the corresponding symbol in the calculation. [6] Further, by weight percent: containing one or more selected from Cu: 0.01-4.0%, V: 0.001-2.5%, B: 0.001-0.012%, Al: 0.001-2.0%, W: 0.05-2.5%, Ga: 0.0004-0.0500%, Co: 0.05-2.5%, Sn: 0.01-2.5%, Ti: 0.01-1.0%, Nb: 0.01-2.5%, Ta: 0.01-2.5%, Ca: 0.0002-0.012%, Mg: 0.0002-0.012%, Zr: 0.0002-0.012%, and REM: 0.0002-0.05%, [5] A wire rod for stainless steel wire. Effect of the Invention

[0013] The stainless steel wire of the present invention has a low Ni content as a chemical composition, but by adjusting the A value in formula (a) and adding Cu and N in combination, and by controlling the total wiredrawing reduction rate and the final wiredrawing speed in the final wiredrawing, it is possible to realize a stainless steel wire that ensures high strength and high ductility and that can ensure mesh-forming properties without annealing after wiredrawing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] In the present invention, a product that has been subjected to final drawing and has not been annealed after the drawing is called a "stainless steel wire." Also, a material for producing the above-mentioned stainless steel wire that has been subjected to hot rolling or further drawing is called a "wire rod for stainless steel wire."

[0015] Chemical composition of stainless steel wire and wire rod for stainless steel wire The chemical components of stainless steel wire and wire rod for stainless steel wire are described below. "%" in the chemical composition of steel means mass%. A numerical range expressed using "~" means a range that includes the numerical values ​​before and after "~" as the lower and upper limits. When "over" or "less than" is added to the numerical values ​​before and after "~", the numerical range does not include these numerical values ​​as the lower or upper limit.

[0016] First, reasons for limiting the chemical components of the stainless steel wire and the wire rod for the stainless steel wire according to the present invention will be described below.

[0017] (C: 0.01~0.20%) C is added in an amount of 0.01% or more to ensure the strength of the steel wire after wire drawing. However, if C is added in an amount exceeding 0.20%, the strength becomes too high and the reduction in area at break decreases. Therefore, the upper limit of C is set to 0.20%. The preferred range of C is 0.02 to 0.15%, and the more preferred range is 0.04 to 0.09%.

[0018] (Si: 0.1 to 4.0%) Silicon is added at 0.1% or more to ensure deoxidation and strength. However, if silicon is added in excess of 4.0%, the reduction in area at break decreases, so the upper limit is set at 4.0%. The preferred range of silicon is 0.2-2.0%, and the more preferred range is 0.2-1.0%.

[0019] (Mn: 0.1-10.0%) Mn is added in an amount of 0.1% or more to ensure austenite stability and strength. However, if Mn is added in an amount exceeding 10.0%, the reduction in area at break decreases, so the upper limit is set to 10.0%. The preferred range of Mn is 0.5 to 5.0%, and the more preferred range is 1.0 to 3.0%.

[0020] (Ni: 3.0~10.0%) Ni is added in an amount of 3.0% or more to ensure austenite stability and ductility. However, if the amount exceeds 10.0%, the alloy cost increases and the strength of the stainless steel wire decreases, so the upper limit is set to 10.0%. The preferred range of Ni is 4.0 to 9.0%, and the more preferred range is 5.0 to 8.0%.

[0021] (Cr:17.0~25.0%) Cr is added at 17.0% or more to ensure corrosion resistance and N solubility. However, if it is added at more than 25.0%, the reduction in area at break decreases, so the upper limit is set at 25.0%. The preferred range of Cr is 18.0 to 23.0%, and the more preferred range is 18.5 to 22.0%.

[0022] (Mo: 0.1-4.0%) Mo is added by 0.1% or more to improve the corrosion resistance of stainless steel wire. However, if it is added by more than 4.0%, the alloy cost increases and the reduction in area decreases, so the upper limit is set to 4.0%. The preferred range of Mo is 0.1 to 2.0%, and the more preferred range is 0.1 to 1.0%.

[0023] (N:0.10~0.50%) N is set to 0.10% or more to ensure strength and corrosion resistance. However, if it exceeds 0.50%, the strength and the reduction in area are decreased, so the upper limit is set to 0.50%. The preferred range of N is 0.15 to 0.40%, and the more preferred range is 0.15 to 0.30%.

[0024] (Cu: 0.5-4.0%) Cu is added at 0.5% or more to ensure ductility and austenite stability. However, adding more than 4.0% causes hot work cracking and reduces strength, so the upper limit is set at 4.0%. The preferred range of Cu is 0.8-3.5%, and the more preferred range is 1.4-3.5%.

[0025] By adding N and Cu in combination as described above, the stainless steel wire of the present invention can reduce the dislocation density in the austenite phase after severe working and also suppress the formation of working-induced martensite, thereby ensuring a balance between the strength and ductility of the steel wire.

[0026] The stainless steel wire and the wire rod for a stainless steel wire of the present invention contain the above-mentioned components with the balance being Fe and impurities, and preferably further selectively contain the following components.

[0027] (V:0~2.5%) V is added as necessary to improve the balance between strength and ductility. However, adding more than 2.5% actually reduces the balance between strength and ductility, so the upper limit is set to 2.5%. It is preferably 1.0% or less, more preferably 0.7% or less, and even more preferably 0.5% or less. If the V content is 0.001% or more, the above effects can be achieved.

[0028] (B: 0~0.012%) B is added as necessary to improve the balance between strength and ductility. However, adding more than 0.012% actually reduces the balance between strength and ductility, so the upper limit is set at 0.012%. The above effects can be achieved if the B content is 0.001% or more.

[0029] (Al: 0-2.0%) Al is added as necessary to improve the balance between strength and ductility. However, adding more than 2.0% will actually reduce the balance between strength and ductility, so the upper limit is set to 2.0%. It is preferably 1.0% or less, more preferably 0.5% or less, and even more preferably 0.05% or less. If the Al content is 0.001% or more, the above effects can be achieved.

[0030] (W:0~2.5%) W is added as necessary to improve the corrosion resistance of stainless steel wire. However, if W is added in excess of 2.5%, wire drawability deteriorates, so the upper limit is set to 2.5%. More preferably, it is 2.0% or less, and even more preferably, it is 1.5% or less. If the W content is 0.05% or more, the above effects can be achieved.

[0031] (Ga: 0 to 0.0500%) Ga is added as necessary for corrosion resistance. However, if it is added in excess of 0.0500%, wire drawability deteriorates, so the upper limit is set to 0.0500%. If the Ga content is 0.0004% or more, the above effects can be achieved.

[0032] (Co: 0-2.5%) Co is added as necessary for corrosion resistance. However, if it is added in excess of 2.5%, wire drawability deteriorates, so the upper limit is set to 2.5%. More preferably, it is 1.0% or less, and even more preferably, it is 0.8% or less. If the Co content is 0.05% or more, the above effects can be achieved.

[0033] (Sn: 0-2.5%) Sn is added as necessary for corrosion resistance. However, if it is added in excess of 2.5%, wire drawability deteriorates, so the upper limit is set to 2.5%. More preferably, it is 1.0% or less, and even more preferably, it is 0.2% or less. If the Sn content is 0.01% or more, the above effects can be achieved.

[0034] (Ti: 0-1.0%) Ti is added as necessary to improve the balance between strength and ductility. However, adding more than 1.0% of Ti results in a decrease in the balance between strength and ductility, so the upper limit is set to 1.0%. It is preferably set to 0.7% or less, and more preferably set to 0.5% or less. If the Ti content is 0.01% or more, the above effects can be achieved.

[0035] (Nb: 0-2.5%) Nb is added as necessary to improve the strength-ductility balance. However, adding more than 2.5% will actually reduce the strength-ductility balance, so the upper limit is set to 2.5%. It is preferably 1.0% or less, more preferably 0.7% or less, and even more preferably 0.5% or less. If the Nb content is 0.01% or more, the above effects can be achieved.

[0036] (Ta: 0~2.5%) Ta is added as necessary to improve the balance between strength and ductility. However, adding more than 2.5% actually reduces the balance between strength and ductility, so the upper limit is set to 2.5%. It is preferably 1.0% or less, more preferably 0.7% or less, and even more preferably 0.5% or less. If the Ta content is 0.01% or more, the above effects can be achieved.

[0037] (Ca: 0~0.012%) Ca is added as necessary for deoxidation. However, if it is added in excess of 0.012%, wire drawability deteriorates, so the upper limit is set to 0.012%. Ca is preferably 0.010% or less, and more preferably 0.005% or less. If the Ca content is 0.0002% or more, the above effects can be achieved.

[0038] (Mg: 0~0.012%) Mg is added as necessary for deoxidation. However, if it is added in excess of 0.012%, wire drawability deteriorates, so the upper limit is set to 0.012%. The content is preferably 0.010% or less, and more preferably 0.005% or less. If the Mg content is 0.0002% or more, the above effects can be achieved.

[0039] (Zr: 0~0.012%) Zr is added as necessary for deoxidation. However, if it is added in an amount exceeding 0.012%, wire drawability deteriorates, so the upper limit is set to 0.012%. It is preferably 0.010% or less, and more preferably 0.005% or less. If the Zr content is 0.0002% or more, the above effects can be achieved.

[0040] (REM: 0~0.05%) REM is added as necessary for deoxidation. However, if added in excess of 0.05%, wire drawability deteriorates, so the upper limit is set to 0.05%. The REM content is preferably 0.010% or less, and more preferably 0.005% or less. If the REM content is 0.0002% or more, the above effects can be achieved.

[0041] (A value: -60 or less) The A value defined by the following formula (a) is an index obtained by investigating the relationship between the volume fraction of stress-induced martensite and the components after wiredrawing, and needs to be controlled in order to prevent the excessive generation of stress-induced martensite in the steel wire after wiredrawing.

[0042] If the A value exceeds -60, excessive deformation-induced martensite phase is generated during wire drawing. In order to suppress deformation-induced martensite, the A value is limited to -60 or less. It is preferably -100 or less, and more preferably -150 or less. In order to prevent high costs due to high alloying, it is preferable to set the lower limit of the A value to -400. A value=551-462(C+N)-9.2Si―8.1Mn―29(Ni+Cu)-13.7Cr―18.5Mo … (a) However, the element symbol in formula (a) means the content (mass%) of the element in the steel. When the content of an element in formula (a) is 0%, "0" is substituted for the corresponding symbol in the calculation.

[0043] Although the present invention has a low Ni content of 10.0% at the upper limit, by limiting the A value to -60 or less as described above, it is possible to suppress the excessive generation of strain-induced martensite phase during wire drawing.

[0044] 《Stainless Steel Wire Quality》 (Dislocation density in the austenite phase: 1×10 15 / m 2 ~100×10 15 / m 2 ) If the dislocation density of the austenite phase is too low, it becomes difficult to ensure strength. Therefore, the lower limit is set at 1×10 15 / m 2 On the other hand, if the dislocation density of the austenite phase is too high, the fracture reduction cannot be ensured, so the upper limit is set at 100 × 10 15 / m 2 Preferably, 3×10 15 / m 2 ~50×10 15 / m 2 , and more preferably 3×10 15 / m 2 ~30×10 15 / m 2 It is.

[0045] (Metal structure) Since the stainless steel wire of the present invention is as drawn and is not annealed after the drawing, the crystal structure of the stainless steel wire exhibits a worked structure. The worked structure can be confirmed by polishing and etching the L-section of the stainless steel wire and then observing the elongation of the crystal grains with an optical microscope.

[0046] The stainless steel wire of the present invention is directly drawn without being annealed after drawing, and as a result, quality excellent in strength and ductility can be achieved with fewer processes.

[0047] The metal structure of the stainless steel wire of the present invention preferably contains an austenite phase. For example, if an FCC diffraction pattern is obtained by X-ray diffraction, it can be said that the stainless steel wire contains an austenite phase. The presence of an austenite phase can be evaluated by the above-mentioned X-ray diffraction or saturation magnetization measurement.

[0048] (Tensile strength: 1900~4500MPa) The stainless steel wire of the present invention preferably has a tensile strength in the range of 1900 to 4500 MPa. By setting the tensile strength to 1900 MPa or more, the high strength that is the object of the present invention can be fully realized. On the other hand, if the tensile strength exceeds 4500 MPa, the fracture reduction cannot be sufficiently ensured. More preferably, the tensile strength is 2000 to 3500 MPa. Further preferably, the tensile strength is 2000 to 3000 MPa.

[0049] (Area at break: 10% or more) The stainless steel wire of the present invention preferably has a fracture reduction of 10% or more. By making the fracture reduction of 10% or more, a steel wire with high ductility can be provided. More preferably, the fracture reduction of 20% or more, and even more preferably, the fracture reduction of 30% or more.

[0050] <<Method of manufacturing stainless steel wire>> Next, a method for producing the stainless steel wire and the wire rod for the stainless steel wire according to the present embodiment will be described. Note that the method for producing the high-strength stainless steel wire and the wire rod for the stainless steel wire according to the present invention is not limited to the conditions described below.

[0051] The steel having the above-mentioned composition is melted and cast into a slab having a predetermined diameter, and then the slab is hot rolled into a wire rod. Thereafter, the slab is appropriately subjected to solution treatment and pickling as necessary to produce a wire rod for stainless steel wire.

[0052] The stainless steel wire according to the present embodiment is obtained by cold drawing the wire rod for stainless steel wire described above. Specifically, a predetermined material before wiredrawing is wiredrawn under the following conditions to manufacture a stainless steel wire. The predetermined material before wiredrawing refers to the above-mentioned wire rod after hot rolling, or a material obtained by subjecting the wire rod to preliminary wiredrawing and then subjecting the steel wire to intermediate strand annealing.

[0053] (Total wire drawing area reduction rate: 95.0~99.98%) The total wiredrawing area reduction in the wiredrawing process is set to 95% or more in order to ensure strength and omit heat treatment. It is preferably set to more than 95.0%. On the other hand, if the total wiredrawing area reduction is too large, the wire breakage rate increases, so the upper limit of the total wiredrawing area reduction is set to 99.98%. It is preferably 96.0 to 99.98%, and more preferably 99.90 to 99.98%. Here, the total wiredrawing area reduction means the total wiredrawing area reduction in the wiredrawing process after intermediate strand annealing, when the preliminary wiredrawing process and intermediate strand annealing are performed.

[0054] (Final wire drawing speed: 50~1000m / min) The final wiredrawing speed in the wiredrawing process is set to a range of 50 to 1000 m / min. By setting the final wiredrawing speed in the wiredrawing process to 50 m / min or more, in combination with the combined addition of Cu and N in the composition, it is possible to achieve both high strength and high ductility without annealing after the final wiredrawing, despite performing ultra-wiredrawing with a total wiredrawing reduction rate of 95.0% or more. On the other hand, if the final wiredrawing speed exceeds 1000 m / min, the frequency of wire breakage increases, so the upper limit of the final wiredrawing speed is set to 1000 m / min. The final wiredrawing speed is preferably set to a range of 100 to 1000 m / min, and more preferably set to a range of 300 to 1000 m / min.

[0055] (Synergistic effect of ingredient composition and manufacturing method) In the present invention, by adding Cu and N in combination to the composition and further setting the final drawing speed to 50 m / min or more as described above, the total wire drawing reduction is 95.0% or more, and by not performing final annealing, the dislocation density of the austenite phase can be controlled within the preferred range of the present invention, thereby achieving both high strength and high ductility. Since no final annealing is performed, it is possible to suppress the high cost, long construction period, and high environmental load of the process.

[0056] (Stainless steel wire diameter) The stainless steel wire of the present invention can be suitably used in the range of wire diameter from 0.01 to 4.0 mm. In particular, in a fine wire having a wire diameter of 0.5 mm or less, and further in an ultra-fine wire having a wire diameter of 0.1 mm or less, the absence of final annealing can greatly reduce process costs, shorten the construction period, and reduce the environmental load.

[0057] Stainless steel parts The stainless steel wire of the present invention can be used to produce stainless steel parts. Examples of stainless steel parts include wire mesh, ropes, springs, iron cores for communication, etc. The stainless steel wire of the present invention has excellent strength and ductility, and therefore can be suitably used as a material for the above stainless steel parts. EXAMPLES

[0058] Examples of the present invention will be described below, but the conditions in the examples are merely examples of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to the conditions used in the following examples. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.

[0059] Table 1 shows the chemical compositions of the steels of the examples (steel types A to AU) and the A values ​​in formula (a). Note that the underlines in Table 1 indicate those outside the range of the present invention.

[0060] [Table 1]

[0061] The steel with these chemical compositions was melted in a 100 kg vacuum melting furnace and cast into a φ180 mm slab, assuming AOD melting, a low-cost stainless steel melting process. The resulting slab was heated at 1100°C for 200 minutes, then hot-rolled to a φ5.5 mm wire rod, and the hot rolling was completed at 1050°C. Immediately after that, in-line heat treatment was performed at 1050°C for 3 minutes as a solution treatment, followed by water cooling and pickling to produce wire rod for stainless steel wire.

[0062] The wire was then cold drawn to a diameter of 0.15 mm to produce a stainless steel wire. The total wire drawing reduction was 99.93%, and the final wire drawing speed was 400 m / min. No heat treatment was performed after the wire drawing.

[0063] The steel wires produced by the above method were evaluated for dislocation density in the austenite phase, tensile strength, and reduction in area at break according to the following methods.

[0064] [Dislocation density in the austenite phase] The dislocation density of the austenite phase of the steel wire was measured by X-ray line profile analysis. Measurement was performed on the L section of the steel wire (section (longitudinal section) in the rolling direction of the steel wire) using X-ray diffraction with CuKα radiation to measure the half-value widths of (111), (200), (220), and (311). The obtained half-value widths were then substituted into the following formula (E) (modified Williamson-Hall equation). ΔK=0.9 / D+((πM 2 b 2 ρ) / 2) 1 / 2 K.C. 1 / 2 +O(K 2 C) (E) In formula (E), D is the crystallite size (nm), ρ is the dislocation density (m -2 ), b is the magnitude of the Burgers vector (nm), M is a constant related to the dislocation density ρ and the interaction distance Re (nm), and C is the average contrast factor of dislocations. In addition, K and ΔK are as follows: K=2sinθ / λ, ΔK=2βcosθ / λ In the above formula, β, θ, and λ are the half-width (rad) of each diffraction line, the Bragg reflection angle (rad), and the X-ray wavelength (CuKα=0.15405 nm), respectively.

[0065] Here, we square both sides of equation (E) and obtain the higher-order term O(K 2 C) is ignored, and α = (0.9 / D) 2 , γ=πM 2 b 2 If we set it to ρ / 2, we obtain equation (F). [(ΔK) 2 -α] / K 2 = γC (F)

[0066] In the above formula, C=C h00 (1-qH 2 ) · · · (G) And q is a parameter that includes the type and ratio of dislocations, H(=(h 2 k 2 +h 2 l 2 +k 2 l 2 ) / (h 2 +k 2 +l 2 ) 2 ) · · · (H) is a function of the indices h, k, and l of the diffraction lines (hkl). C h00 =C e h00 +S(C s h00 -C e h00 ) · · · (I) and C e h00 ,C s h00 is the contrast factor for 100% edge and screw dislocations, and is a constant calculated from the elastic constant. The above q value is determined as follows, and the screw dislocation fraction S of austenite can be calculated from the following relational expression (J). S = (qq e ) / (q s -q e )...Equation (J) In the above formula, q e andq s are the q values ​​for a 100% edge dislocation and a screw dislocation, respectively, and are constants determined by the elastic constants.

[0067] To determine the q value, use formulas (F) and (G). The variables on the X and Y axes are H 2 and (ΔK 2 -α 2 ) / K 2 And H 2 Determine the α that optimizes linearity for, and calculate the q value from the slope and intercept of the linear function above as q = -slope / intercept. Calculate the S value from equation (J) and the C value from equation (G).

[0068] Next, the profile of each diffractive surface is Fourier transformed to obtain the modified Warren-Averbach equation (K), where L is the Fourier length.

number

number

[0069] The reason for limiting the evaluation of dislocation density to "in the austenite phase" is that it is a factor necessary for ensuring the balance between strength and ductility of the steel wire. Also, the dislocation density of the austenite phase can be evaluated by the above evaluation.

[0070] The dislocation density of the austenite phase was evaluated using the above procedure and listed in Tables 2 and 3. 15 / m 2 More than 30×10 15 / m 2 "Excellent" is less than "dislocation density" is 1×10 15 / m 2 More than 3×10 15 / m 2 Less than or equal to 30 x 10 15 / m 2 More than 100 x 10 15 / m 2 "Good" is below, and dislocation density is 1×10 15 / m 2 Less than or 100 x 10 15 / m 2 The judge ruled super unacceptable.

[0071] [Tensile strength] The tensile strength of the steel wire was evaluated by the tensile strength in the tensile test of JIS Z 2241. The tensile strength was evaluated as follows: 2000 MPa or more and less than 3000 MPa: ◎; 1900 MPa or more and less than 2000 MPa, or 3000 MPa or more and less than 4500 MPa: ○; and less than 1900 MPa or more than 4500 MPa: △. These are shown in Tables 2 and 3.

[0072] [Break drawing] The reduction in area of ​​the stainless steel wire at fracture was evaluated as the reduction in area of ​​the fractured surface after the tensile test. The reduction in area of ​​the stainless steel wire at fracture was evaluated as 30% or more, 10% or more but less than 30%, ◯, and less than 10%, △, as shown in Tables 2 and 3.

[0073] The evaluation results are shown in Table 2. Items outside the scope of the present invention are underlined.

[0074] [Table 2]

[0075] As shown in Table 2, in the steel wires of Inventive Examples 1 to 33, the dislocation density of the austenite phase was within the range of the present invention, the tensile strength was ◯ or ◎, and the breaking elongation was ◯ or ◎. On the other hand, in the steel wires of Comparative Examples 34 to 47, the dislocation density of the austenite phase did not reach the target, and both the tensile strength and the breaking elongation were △, not reaching the preferred range.

[0076] Next, the influence of manufacturing conditions was investigated.

[0077] Using the steel type M shown in Table 1, stainless steel wire rods having various diameters were manufactured by the same method as above, and used as wire rods for stainless steel wire before wire drawing. The prepared wire rods for stainless steel wire were used to perform wire drawing under the wire drawing conditions (total wire drawing reduction, final wire drawing speed) shown in Table 3, and stainless steel wires of φ0.17 mm were produced without performing heat treatment after wire drawing. In each example, the diameter of the wire rod for stainless steel wire was adjusted so that the final wire diameter of the stainless steel wire was φ0.17 mm. Then, the dislocation density of the austenite phase, tensile strength, and reduction in area of ​​fracture were measured and evaluated for the obtained steel wires by the same method as above. The evaluation results are shown in Table 3. Items outside the scope of the present invention and values ​​outside the preferred manufacturing conditions of the present invention are underlined.

[0078] [Table 3]

[0079] The steel wires of the present invention shown in Test Nos. 48 to 56 had a total wire drawing reduction rate and a final wire drawing speed within the preferred range of the present invention, a dislocation density of the austenite phase within the preferred range of the present invention, a tensile strength of ◯ or ◎, and a breaking elongation of ◯ or ◎. On the other hand, of the steel wires of Comparative Examples 57 to 60, Comparative Examples 58 and 60 were not subjected to quality evaluation because breakage occurred during wire drawing. For Comparative Examples 57 and 59, the dislocation density of the austenite phase did not reach the target, and both the tensile strength and the breaking elongation were △, not reaching the preferred range.

Claims

1. In mass percent, C: 0.01-0.20%, Si: 0.1 to 4.0%, Mn: 0.1 to 10.0%, Ni: 3.0 to 10.0%, Cr: 17.0-25.0%, Mo: 0.1 to 4.0%, N: 0.10 to 0.50%, Cu: 0.5-4.0%, V: 0 to 2.5%, B: 0 to 0.012%, Al: 0-2.0%, W: 0 to 2.5%, Ga: 0 to 0.0500%, Co: 0 to 2.5%, Sn: 0 to 2.5%, Ti: 0 to 1.0%, Nb: 0 to 2.5%, Ta: 0 to 2.5%, Ca: 0-0.012%, Mg: 0 to 0.012%, Zr: 0 to 0.012%, REM: 0-0.05%, with the remainder being Fe and impurities, The A value represented by the following formula (a) is −60 or less, The dislocation density of the austenite phase of the stainless steel wire is 1×10 15 / m 2 ~100 x 10 15 / m 2 That is, Stainless steel wire. A value=551-462(C+N)-9.2Si-8.1Mn-29(Ni+Cu)-13.7Cr-18.5Mo... (a) In the formula, the symbol of an element means the content (mass%) of the element in the steel. When the content of an element in formula (a) is 0%, "0" is substituted for the corresponding symbol in the calculation.

2. Further, in mass percent, V: 0.001 to 2.5%, B: 0.001-0.012%, Al: 0.001-2.0%, W: 0.05-2.5%, Ga: 0.0004-0.0500%, Co: 0.05-2.5%, Sn: 0.01 to 2.5%, Ti: 0.01 to 1.0%, Nb: 0.01-2.5%, Ta: 0.01-2.5%, Ca: 0.0002-0.012%, Mg: 0.0002-0.012%, Zr: 0.0002 to 0.012% and REM: Contains one or more selected from 0.0002 to 0.05%; 2. The stainless steel wire according to claim 1.

3. 3. The stainless steel wire according to claim 1, having a tensile strength of 1900 to 4500 MPa and a fracture reduction of 10% or more.

4. A stainless steel part, comprising the stainless steel wire according to claim 1 or 2.

5. In mass percent, C: 0.01-0.20%, Si: 0.1 to 4.0%, Mn: 0.1 to 10.0%, Ni: 3.0 to 10.0%, Cr: 17.0-25.0%, Mo: 0.1 to 4.0%, N: 0.10 to 0.50%, Cu: 0.5-4.0%, V: 0 to 2.5%, B: 0 to 0.012%, Al: 0-2.0%, W: 0 to 2.5%, Ga: 0 to 0.0500%, Co: 0 to 2.5%, Sn: 0 to 2.5%, Ti: 0 to 1.0%, Nb: 0 to 2.5%, Ta: 0 to 2.5%, Ca: 0-0.012%, Mg: 0 to 0.012%, Zr: 0 to 0.012%, REM: 0-0.05%, with the remainder being Fe and impurities, The A value represented by the following formula (a) is −60 or less: Wire rod for stainless steel wire. A value=551-462(C+N)-9.2Si-8.1Mn-29(Ni+Cu)-13.7Cr-18.5Mo... (a) In the formula (a), the symbol of an element means the content (mass%) of the element in the steel. When the content of an element in the formula (a) is 0%, "0" is substituted for the corresponding symbol in the calculation.

6. Further, in mass percent, Cu: 0.01-4.0%, V: 0.001 to 2.5%, B: 0.001-0.012%, Al: 0.001-2.0%, W: 0.05-2.5%, Ga: 0.0004-0.0500%, Co: 0.05-2.5%, Sn: 0.01 to 2.5%, Ti: 0.01 to 1.0%, Nb: 0.01-2.5%, Ta: 0.01-2.5%, Ca: 0.0002-0.012%, Mg: 0.0002-0.012%, Zr: 0.0002 to 0.012% and REM: Contains one or more selected from 0.0002 to 0.05%; The wire rod for stainless steel wire according to claim 5.

Citation Information

Patent Citations

  • Electroslag welding method

    JP1989091983A

  • High strength stainless steel extra fine wire

    JP4068216B2

  • Method for producing inexpensive stainless steel fine wire with excellent elongation characteristics

    JP4098171B2

Cited By

  • Stainless steel wire in as-drawn state, heat-treated stainless steel wire, and wire for stainless steel wire

    WO2026105635A1