Hollow resin particles and method for producing the same
Hollow resin particles with a polyolefin and vinyl resin composition improve electrical properties, heat resistance, and flexibility, overcoming the limitations of acrylic resin-based particles by incorporating a polyolefin resin with an olefin and unsaturated carboxylic acid component and a crosslinkable monomer.
Patent Information
- Application Number
- JP2023081729
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing hollow resin particles made of acrylic resin lack sufficient electrical properties, heat resistance, and flexibility, making them unsuitable for applications requiring these qualities, especially when formed into coating films.
Hollow resin particles are composed of a shell containing a polyolefin resin with an olefin component and an unsaturated carboxylic acid component, along with a vinyl resin, which includes a crosslinkable monomer, to enhance electrical properties, heat resistance, and flexibility.
The resulting hollow resin particles exhibit excellent electrical properties, heat resistance, and flexibility when formed into coating films, addressing the limitations of previous acrylic resin-based particles.
Smart Images

Figure 2024165484000001
Abstract
Description
[Technical field]
[0001] The present invention relates to hollow resin particles and a method for producing the same. [Background technology]
[0002] Hollow resin particles having voids inside the particle are excellent in low dielectric properties, heat insulation, light scattering properties, etc., and various types have been developed. Conventionally, hollow resin particles made of inorganic substances such as silica and metal oxides have been used, but inorganic substances have a problem in that they are high in density and are unsuitable for use as particles for applications requiring light weight.
[0003] In light of this background, hollow resin particles made of organic polymers have been studied in recent years. For example, Patent Documents 1 and 2 propose hollow resin particles made of acrylic resin. In general, it is known that acrylic resin has a high dielectric constant and insufficient heat resistance. For this reason, the acrylic hollow resin particles described in Patent Documents 1 and 2 are not suitable for purposes that require excellent electrical properties or heat resistance.
[0004] In recent years, paints and inks containing hollow resin particles have been studied. For example, Patent Document 3 proposes a paint containing hollow resin particles. However, the resin component constituting the hollow resin particles described in Patent Document 3 does not have sufficient flexibility, and there is a problem that cracks and whitening occur in the coating film when the coating film containing the hollow resin particles is folded. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-33503 A [Patent Document 2] JP 2013-221070 A [Patent Document 3] JP 2018-123251 A Summary of the Invention [Problem to be solved by the invention]
[0006] In view of these problems, an object of the present invention is to provide hollow resin particles which are excellent in electrical properties, heat resistance, and flexibility when formed into a coating film. [Means for solving the problem]
[0007] Means for Solving the Problems The present inventors conducted extensive research in order to solve the above problems, and as a result, discovered that hollow resin particles containing a polyolefin resin containing an olefin component and an unsaturated carboxylic acid component as a copolymer component in the shell portion, and a vinyl resin, have excellent electrical properties, heat resistance, and flexibility when formed into a coating film, thereby arriving at the present invention. That is, the gist of the present invention is as follows.
[0008] (1) A hollow resin particle having a shell portion and a hollow portion surrounded by the shell portion, The shell portion contains a polyolefin resin (A) and a vinyl resin (B), The polyolefin resin (A) is a hollow resin particle containing an olefin component and an unsaturated carboxylic acid component as a copolymerization component. (2) The hollow resin particles according to (1), wherein the olefin component contains propylene and an olefin other than propylene, and the propylene content is 60 mass% or more relative to 100 mass% of the olefin component. (3) The hollow resin particles according to (1) or (2), wherein the content of the unsaturated carboxylic acid component is 0.1 to 10.0 parts by mass per 100 parts by mass of the total of propylene and the olefin other than propylene. (4) The hollow resin particles according to any one of (1) to (3), wherein the vinyl resin (B) contains a crosslinkable monomer as a copolymerization component. (5) The hollow resin particles according to any one of (1) to (4), wherein the olefin other than propylene is at least one member selected from the group consisting of ethylene, 1-butene, and 4-methyl-1-pentene. (6) The hollow resin particles according to any one of (1) to (5), having a volume average particle diameter of 0.05 to 20 μm. (7) A method for producing hollow resin particles according to any one of (1) to (6), comprising the following steps (I) and (II): (I) a polyolefin resin containing an olefin component and an unsaturated carboxylic acid component as a copolymerization component, A process of converting a polyolefin resin into an aqueous dispersion by mixing with a basic compound and an aqueous medium. (II) A step of polymerizing a vinyl monomer in the presence of the aqueous dispersion of the polyolefin resin obtained in (I) above. Effect of the Invention
[0009] According to the present invention, hollow resin particles having excellent electrical properties, heat resistance, and flexibility when formed into a coating film can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. The hollow resin particles of the present invention have a shell portion and a hollow portion surrounded by the shell portion. Furthermore, the shell portion contains a polyolefin resin (A) and a vinyl resin (B), and the polyolefin resin (A) contains an olefin component and an unsaturated carboxylic acid component as a copolymerization component.
[0011] In the present invention, "hollow" means a state in which the inside is filled with a substance other than resin, such as a gas or liquid, and preferably means a state in which the inside is filled with gas, in that the effects of the present invention can be more effectively exhibited.
[0012] The shell portion and the hollow portion surrounded by the shell portion may be composed of one hollow region, or may be composed of a plurality of hollow regions.
[0013] The shell and the hollow portion surrounded by the shell may have a porous structure. If the structure is porous, the hollow portion may have one hollow region (continuous pores), multiple hollow regions (independent pores), or a mixture of these.
[0014] <Polyolefin resin (A)> The polyolefin resin constituting the hollow resin particles of the present invention contains an olefin component and an unsaturated carboxylic acid component.
[0015] In the present invention, the polyolefin resin contains an olefin component and an unsaturated carboxylic acid component as a copolymerization component, and the content of the unsaturated carboxylic acid component is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and even more preferably 1 to 4 parts by mass, relative to 100 parts by mass of the olefin component. If the content of the unsaturated carboxylic acid component in the polyolefin resin is out of this range, hollow portions are difficult to form inside the particles in the production of hollow resin particles described below.
[0016] Specific examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, fumaric acid, crotonic acid, etc., as well as half esters and half amides of unsaturated dicarboxylic acids and their anhydrides. Among them, in order to stably disperse the resin in the aqueous dispersion of the resin described below, acrylic acid, methacrylic acid, maleic acid, and maleic anhydride are preferred, and acrylic acid, methacrylic acid, and maleic anhydride are particularly preferred. Two or more of these unsaturated carboxylic acids may be contained in the polyolefin resin.
[0017] The unsaturated carboxylic acid component may be copolymerized in the polyolefin resin in any form, including, for example, random copolymerization, block copolymerization, and graft copolymerization.
[0018] The method of introducing an unsaturated carboxylic acid component into an unmodified polyolefin resin is not particularly limited, and for example, an unmodified polyolefin resin and an unsaturated carboxylic acid can be graft-copolymerized onto the unmodified polyolefin resin by a method of heating and melting the unmodified polyolefin resin and the unsaturated carboxylic acid to a temperature equal to or higher than the melting point of the unmodified polyolefin resin in the presence of a radical generator, and then reacting the unmodified polyolefin resin by heating and stirring in the presence of a radical generator, etc. The former method is particularly preferred from the viewpoint of ease of operation.
[0019] Examples of the radical generator used in the graft copolymerization include peroxides such as di-tert-butyl peroxide, dicumyl peroxide, tert-butyl hydroperoxide, tert-butyl cumyl peroxide, benzoyl peroxide, dilauryl peroxide, cumene hydroperoxide, tert-butyl peroxybenzoate, tert-butyl peroxyisopropyl monocarbonate, ethyl ethyl ketone peroxide, and di-tert-butyl diperphthalate, and azo compounds such as 2,2′-azobisisobutyronitrile. These may be appropriately selected and used depending on the reaction temperature.
[0020] The polyolefin resin in the present invention preferably has a weight average molecular weight of 10,000 or more and less than 250,000, more preferably 15,000 or more and less than 150,000, and even more preferably 20,000 or more and less than 60,000. If the weight average molecular weight of the polyolefin resin is less than 10,000, the strength of the obtained hollow resin particles tends to decrease. On the other hand, if the weight average molecular weight of the polyolefin resin is 250,000 or more, it may be difficult to make an aqueous dispersion in the method for producing hollow resin particles described later.
[0021] In the present invention, the olefin component preferably contains propylene and an olefin other than propylene. The propylene content is preferably 60% by mass or more, more preferably 65% by mass or more, even more preferably 75% by mass or more and 99.5% by mass or less, and particularly preferably 80% by mass or more and 99% by mass or less, based on 100% by mass of the olefin component. If the proportion of propylene in the polyolefin resin is less than 60% by mass, the heat resistance of the resulting hollow resin particles tends to decrease.
[0022] Examples of olefins other than propylene include alkenes such as ethylene, 1-butene, isobutene, 1-pentene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-hexene, 1-octene, and norbornenes, and dienes such as butadiene and isoprene. Among these, ethylene or 1-butene is preferred, and ethylene is more preferred, from the viewpoint of ease of resin production.
[0023] The content of the polyolefin resin in the shell is preferably 25% by mass to 95% by mass, more preferably 35% by mass to 90% by mass, even more preferably 40% by mass to 80% by mass, and particularly preferably 45% by mass to 75% by mass, in order to more effectively exhibit the effects of the present invention. If the content of the polyolefin resin in the shell is below this range, the coating film tends to crack or whiten when the coating film containing the hollow resin particles is folded. If the content of the polyolefin resin in the shell is above this range, the heat resistance of the resulting hollow resin particles tends to decrease.
[0024] The polyolefin resin in the present invention is preferably crystalline. In the present invention, crystalline means that the resin has a crystalline melting point (hereinafter, referred to as melting point) during heating and has a heat of fusion of 0.1 J / g or more when measured using a DSC (differential scanning calorimeter) in accordance with JIS K 7121.
[0025] <Vinyl resin> In the present invention, the vinyl resin (B) is a resin obtained by polymerizing a vinyl monomer.
[0026] In the present invention, the vinyl resin preferably contains a crosslinkable monomer as a copolymerization component. By copolymerizing the crosslinkable monomer, the heat resistance of the obtained hollow resin particles tends to be improved.
[0027] In the present invention, the crosslinkable monomer is a monomer having two or more polymerizable vinyl groups in one molecule.
[0028] The crosslinkable monomer is not particularly limited, and examples thereof include polyfunctional (meth)acrylic acid monomers such as ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, glycerin tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate; polyfunctional (meth)acrylamide monomers such as N,N'-methylene bis(meth)acrylamide and N,N'-ethylene bis(meth)acrylamide; polyfunctional allyl monomers such as diallylamine and tetraallyloxyethane; and styrene-based crosslinkable monomers such as divinylbenzene, divinylnaphthalene, and diallylphthalate. In terms of being able to more effectively exhibit the effects of the present invention, the crosslinkable monomer is preferably a styrene-based crosslinkable monomer, and more preferably divinylbenzene. The crosslinkable monomer may be one type only, or may be two or more types.
[0029] In the present invention, the vinyl resin may contain a monofunctional vinyl monomer as a copolymerization component. As the monofunctional vinyl monomer, a known one can be used, for example, a styrene monomer, a (meth)acrylic acid monomer, a diene monomer, a (meth)acrylamide monomer, etc.
[0030] The styrene-based monomer is not particularly limited, and specific examples include styrene, α-methylstyrene, ethylvinylbenzene, vinyltoluene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, vinylbiphenyl, vinylnaphthalene, and sodium p-styrenesulfonate.
[0031] The (meth)acrylic acid monomer is not particularly limited, and examples thereof include acrylic acid, methacrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, and Octyl acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate Examples of the acrylates include acrylates having the formula: acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-(diethylamino)ethyl (meth)acrylate, benzyl (meth)acrylate, allyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, 3-(trimethoxysilyl)propyl (meth)acrylate, 3-(triethoxysilyl)propyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, 2-(perfluorobutyl)ethyl (meth)acrylate, and glycidyl (meth)acrylate.
[0032] The diene monomer is not particularly limited, but examples thereof include butadiene, isoprene, farnesene, and myrcene.
[0033] The (meth)acrylamide monomer is not particularly limited, and examples thereof include (meth)acrylamide, N-isopropyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, and 2-(meth)acrylamide-2-methylpropanesulfonic acid.
[0034] In addition to the above vinyl monomers, any vinyl compound exhibiting polymerizability can be used without particular limitation. For example, vinylpyrrolidone, (meth)acryloylmorpholine, vinyl acetate, (meth)acrylonitrile, 1-vinylimidazole, maleic acid, fumaric acid, itaconic acid, citraconic acid, mesaconic acid, glutaconic acid, aconitic acid, cinnamic acid, maleic acid alkyl esters, fumaric acid alkyl esters, maleic anhydride, itaconic anhydride, aconitic anhydride, etc. can be used.
[0035] In the present invention, the vinyl resin may form a covalent bond with the polyolefin resin.
[0036] In the present invention, the mass ratio of polyolefin resin / vinyl resin constituting the shell of the hollow resin particles is preferably 97 / 3 to 15 / 85, more preferably 85 / 15 to 30 / 70, further preferably 75 / 25 to 35 / 65, and particularly preferably 70 / 30 to 45 / 55. By having the mass ratio of polyolefin resin / vinyl resin within this range, hollow resin particles having both more excellent dielectric properties and flexibility can be obtained.
[0037] The volume average particle diameter of the hollow resin particles of the present invention is preferably 0.05 μm to 20 μm, more preferably 0.05 μm to 5 μm, even more preferably 0.1 μm to 2 μm, and particularly preferably 0.1 μm to 1 μm. If the volume average particle diameter of the hollow resin particles is less than 0.05 μm, the thickness of the shell part becomes relatively thin, so that the hollow resin particles may not have sufficient strength. If the volume average particle diameter of the hollow resin particles exceeds 20 μm, it becomes difficult to reduce the thickness of the resin material in the application in which the hollow resin particles are added to the binder resin to obtain the resin material.
[0038] <Method for producing hollow resin particles> The method for producing hollow resin particles of the present invention preferably includes a step (I) of aqueously dispersing a polyolefin resin, and a step (II) of polymerizing a vinyl monomer in the presence of the aqueous dispersion of the polyolefin resin to obtain an aqueous dispersion of hollow resin particles.
[0039] (Process (I)) In step (I), it is preferable to use, as the polyolefin resin, a resin which contains an olefin component and an unsaturated carboxylic acid component, in which the olefin component contains propylene and an olefin other than propylene, the propylene content is 60 mass% or more relative to 100 mass% of the olefin component, and the unsaturated carboxylic acid content is 0.1 to 10.0 mass parts relative to 100 mass parts of the total of propylene and the olefin other than propylene.
[0040] The aqueous dispersion of the polyolefin resin is carried out by mixing the above-mentioned polyolefin resin with a basic compound and an aqueous medium, and stirring the mixture under a pressure of 0.15 MPa or more. The method for pressurizing the mixture to 0.15 MPa or more is not particularly limited, but may be, for example, a method of heating the mixture in a closed container.
[0041] The aqueous dispersion of the polyolefin resin may be carried out using a mixture of water and an organic solvent as the aqueous medium, and the content of the organic solvent is preferably 50% by mass or less, more preferably 1 to 45% by mass, and even more preferably 2 to 40% by mass of the aqueous medium. If the content of the organic solvent exceeds 50% by mass, the dispersion stability of the polyolefin resin may decrease depending on the type of the organic solvent used.
[0042] In order to obtain a good aqueous dispersion, the organic solvent used for the aqueous dispersion of the polyolefin resin preferably has a solubility in water at 20° C. of 10 g / L or more, more preferably 20 g / L or more, and even more preferably 50 g / L or more. The boiling point of the organic solvent at normal pressure is preferably less than 250° C., more preferably less than 200° C. If the boiling point of the organic solvent exceeds 250° C., it may be difficult to remove the organic solvent in the solvent removal step described below.
[0043] Specific examples of organic solvents include alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-amyl alcohol, isoamyl alcohol, sec-amyl alcohol, tert-amyl alcohol, 1-ethyl-1-propanol, 2-methyl-1-butanol, n-hexanol, and cyclohexanol; ketones such as methyl ethyl ketone, methyl isobutyl ketone, ethyl butyl ketone, and cyclohexanone; ethers such as tetrahydrofuran and dioxane; ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, sec-butyl acetate, and 3-methyl acetate. Examples of the organic solvent include esters such as butyl ether, methyl propionate, ethyl propionate, diethyl carbonate, and dimethyl carbonate, glycol derivatives such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, and ethylene glycol ethyl ether acetate, and further, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, 3-methoxy-3-methyl-1-butanol, methoxybutanol, acetonitrile, dimethylformamide, dimethylacetamide, diacetone alcohol, ethyl acetoacetate, 1,2-dimethylglycerin, 1,3-dimethylglycerin, and trimethylglycerin. These organic solvents may be used alone or in combination of two or more.
[0044] Among the above organic solvents, ethanol, n-propanol, isopropanol, n-butanol, methyl ethyl ketone, cyclohexanone, tetrahydrofuran, dioxane, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, and diethylene glycol monomethyl ether are preferred because they are highly effective in promoting the aqueous dispersion of the resin, and among these, organic solvents having one hydroxyl group in the molecule are more preferred, and n-propanol, isopropanol, tetrahydrofuran, and ethylene glycol alkyl ethers are even more preferred because they can aqueously disperse the resin with the addition of a small amount.
[0045] Examples of basic compounds used for aqueous dispersion of polyolefin resin include ammonia, triethylamine, isopropylamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, ethylamine, diethylamine, isobutylamine, dipropylamine, 3-ethoxypropylamine, 3-diethylaminopropylamine, sec-butylamine, propylamine, n-butylamine, 2-methoxyethylamine, 3-methoxypropylamine, 2,2-dimethoxyethylamine, monoethanolamine, diethanolamine, triethanolamine, morpholine, N-methylmorpholine, N-ethylmorpholine, pyrrole, pyridine, etc. Examples of basic compounds that can be used include metal hydroxides such as lithium hydroxide, potassium hydroxide, and sodium hydroxide.
[0046] After the aqueous dispersion of the polyolefin resin is completed, a part or all of the organic solvent contained in the aqueous dispersion may be removed by a desolvation treatment generally called "stripping" as necessary. The desolvation treatment can be carried out by a method such as heating or reducing pressure. The desolvation treatment makes it easy to make the medium used have a desired composition when polymerizing a vinyl monomer in the aqueous dispersion of the polyolefin resin.
[0047] The volume average particle diameter of the particles made of polyolefin resin is preferably 0.005 μm to 10 μm, more preferably 0.005 μm to 3 μm, further preferably 0.01 μm to 1.5 μm, and particularly preferably 0.05 μm to 0.8 μm. When the volume average particle diameter of the particles made of polyolefin resin is within this range, the volume average particle diameter of the obtained hollow resin particles is likely to be within the preferred range.
[0048] (Step (II)) In the step (II), a vinyl monomer and a polymerization initiator are added in the presence of the aqueous dispersion of the polyolefin resin to carry out polymerization. The polymerization method is not particularly limited, and examples thereof include dispersion polymerization and emulsion polymerization.
[0049] In the present invention, the dispersion polymerization is a method in which a vinyl monomer is dissolved in a medium, and a polymerization initiator is added to the solution to polymerize the monomer. In the process of obtaining an aqueous dispersion of hollow resin particles by dispersion polymerizing a vinyl monomer in the presence of an aqueous dispersion of a polyolefin resin, it is necessary to use a medium that does not dissolve the polyolefin resin or the vinyl resin produced by polymerization, but can dissolve the raw material vinyl monomer.
[0050] The medium used in the dispersion polymerization is not particularly limited, and examples thereof include water; alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-amyl alcohol, isoamyl alcohol, sec-amyl alcohol, tert-amyl alcohol, 1-ethyl-1-propanol, 2-methyl-1-butanol, n-hexanol, and cyclohexanol; ketones such as methyl ethyl ketone, methyl isobutyl ketone, ethyl butyl ketone, cyclohexanone, and isophorone; ethers such as tetrahydrofuran and dioxane; esters such as ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, sec-butyl acetate, 3-methoxybutyl acetate, methyl propionate, ethyl propionate, diethyl carbonate, and dimethyl carbonate; ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, glycol derivatives such as ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol ethyl ether acetate, diethylene glycol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol ethyl ether acetate, propylene glycol, propylene glycol monomethyl ether, propylene glycol monobutyl ether, and propylene glycol methyl ether acetate; amines such as N,N-dimethylethanolamine, triethylamine, N,N-diethylethanolamine, monoethanolamine, diethanolamine, triethanolamine, morpholine, and pyridine; saturated hydrocarbons such as n-pentane, n-hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclopentane and cyclohexane; aromatic hydrocarbons such as benzene, toluene, ethylbenzene, o-xylene, m-xylene, and p-xylene;Other examples include 3-methoxy-3-methylbutanol, 3-methoxybutanol, acetonitrile, N-methyl-2-pyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide, diacetone alcohol, ethyl acetoacetate, etc., which may be used alone or in combination of two or more kinds.
[0051] When dispersion polymerization of a vinyl monomer is carried out in the presence of an aqueous dispersion of a polyolefin resin, a surfactant and / or a dispersion stabilizer described below can also be used.
[0052] In the present invention, emulsion polymerization is a method in which a vinyl monomer is mixed in a medium, and a polymerization initiator is added to carry out polymerization. In the process of obtaining an aqueous dispersion of hollow resin particles by emulsion polymerization of a vinyl monomer in the presence of an aqueous dispersion of a polyolefin resin, it is necessary to use a medium that does not easily dissolve the vinyl monomer.
[0053] The medium used in the emulsion polymerization is not particularly limited, and examples thereof include water; alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-amyl alcohol, isoamyl alcohol, sec-amyl alcohol, tert-amyl alcohol, 1-ethyl-1-propanol, 2-methyl-1-butanol, n-hexanol, and cyclohexanol; ketones such as methyl ethyl ketone, methyl isobutyl ketone, ethyl butyl ketone, cyclohexanone, and isophorone; ethers such as tetrahydrofuran and dioxane; esters such as ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, sec-butyl acetate, 3-methoxybutyl acetate, methyl propionate, ethyl propionate, diethyl carbonate, and dimethyl carbonate; ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, glycol derivatives such as ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol ethyl ether acetate, diethylene glycol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol ethyl ether acetate, propylene glycol, propylene glycol monomethyl ether, propylene glycol monobutyl ether, and propylene glycol methyl ether acetate; amines such as N,N-dimethylethanolamine, triethylamine, N,N-diethylethanolamine, monoethanolamine, diethanolamine, triethanolamine, morpholine, and pyridine; saturated hydrocarbons such as n-pentane, n-hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclopentane and cyclohexane; aromatic hydrocarbons such as benzene, toluene, ethylbenzene, o-xylene, m-xylene, and p-xylene;Other examples include 3-methoxy-3-methylbutanol, 3-methoxybutanol, acetonitrile, N-methyl-2-pyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide, diacetone alcohol, ethyl acetoacetate, etc., which may be used alone or in combination of two or more kinds.
[0054] When emulsion polymerization of a vinyl monomer is carried out in the presence of an aqueous dispersion of a polyolefin resin, a surfactant and / or a dispersion stabilizer described below can also be used.
[0055] In the present invention, the polymerization initiator used for the purpose of polymerizing the vinyl monomer is not particularly limited, and known azo compounds and peroxides can be used.
[0056] For example, azo compounds include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,3-dimethylbutyronitrile), 2,2'-azobis-(2-methylbutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,3,3-trimethylbutyronitrile), ), 2,2'-azobis(2-isopropylbutyronitrile), 2,2'-azobis[N-(2-hydroxyethyl)-2-methylpropanamide], 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, and the like.
[0057] Examples of peroxides include di-tert-butyl peroxide, dicumyl peroxide, tert-butyl hydroperoxide, tert-butylcumyl peroxide, benzoyl peroxide, dilauryl peroxide, cumene hydroperoxide, tert-butyl peroxybenzoate, methyl ethyl ketone peroxide, di-tert-butyl diperphthalate, cyclohexanone peroxide, diisopropylbenzene hydroperoxide, peracetic acid, sodium persulfate, potassium persulfate, and ammonium persulfate.
[0058] Also, the peroxide can be used as a redox polymerization initiator in combination with a reducing agent. The reducing agent is not particularly limited, but examples thereof include alkali metal salts and ammonium salts such as sulfite, hydrogen sulfite, and pyrosulfite; carboxylic acids such as L-ascorbic acid and tartaric acid; amines such as dimethylaniline; and thiourea dioxide. These reducing agents can be used alone or in combination of two or more. The amount of the reducing agent used is preferably 1 to 1000 parts by mass per 100 parts by mass of the peroxide.
[0059] In the polymerization of the vinyl monomer, the method of adding the vinyl monomer and the polymerization initiator is not particularly limited, and they may be added all at once, may be added in several divided portions, or may be added dropwise. The polymerization atmosphere for the vinyl monomer is not particularly limited, but from the viewpoint of suppressing polymerization inhibition due to oxygen, an inert gas atmosphere such as nitrogen is preferable.
[0060] The polymerization temperature of the vinyl monomer is preferably 0 to 160° C., more preferably 25 to 130° C. If the polymerization temperature is lower than 0° C., the polymerization rate may decrease, which is undesirable from the viewpoint of productivity. If the polymerization temperature exceeds 160° C., the molecular weight of the obtained vinyl resin tends to be small, which tends to decrease the strength of the shell of the obtained hollow resin particles.
[0061] In the method for producing the aqueous dispersion of the polyolefin resin and the aqueous dispersion of the hollow resin particles, a surfactant and / or a dispersion stabilizer can also be used. The method of using a surfactant and a dispersion stabilizer includes a method of including them in a medium, and a method of chemically bonding them to a polyolefin resin and / or a vinyl resin. The mode of bonding between the surfactant and the polyolefin resin and / or the vinyl resin is not particularly limited, but for example, a mode in which a so-called reactive surfactant having a vinyl group capable of radical polymerization in the molecule is copolymerized with the polyolefin resin and / or the vinyl resin by radical polymerization can be exemplified. In addition, the mode of bonding between the dispersion stabilizer and the polyolefin resin and / or the vinyl resin is not particularly limited, but for example, a mode in which the dispersion stabilizer is graft-copolymerized with the olefin resin and / or the vinyl resin can be exemplified.
[0062] The surfactant includes anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants. Examples of the anionic surfactant include alkyl sulfates, polyoxyethylene alkyl ether sulfate salts, alkylbenzene sulfonates, alkylnaphthalene sulfonates, alkyl sulfosuccinates, alkyl diphenyl ether disulfonates, naphthalene sulfonate-formaldehyde condensates, polyoxyethylene polycyclic phenyl ether sulfate salts, polyoxyethylene distyrenated phenyl ether sulfate salts, fatty acid salts, alkyl phosphates, and polyoxyethylene alkyl phenyl ether sulfate salts.
[0063] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyalkylene alkyl ethers, polyoxyethylene polycyclic phenyl ethers, polyoxyethylene distyrenated phenyl ethers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene alkylamines, alkyl alkanolamides, and polyoxyethylene alkyl phenyl ethers.
[0064] Examples of the cationic surfactant include quaternary ammonium salts such as alkyltrimethylammonium bromide, alkylpyridinium bromide, and imidazolinium laurate, pyridinium salts, and imidazolinium salts. Examples of the amphoteric surfactant include lauryl betaine and lauryl dimethylamine oxide.
[0065] Examples of reactive surfactants include polyoxyethylene alkyl ether sulfates (commercially available products include Aqualon KH-05, KH-10, and KH-20 manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., Adeka Reasoap SR-10N and SR-20N manufactured by ADEKA Corporation, and Latemul PD-104 manufactured by Kao Corporation), polyoxyalkylene styrenated phenyl ether sulfates (commercially available products include Aqualon AR-10 and AR-20 manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), sulfosuccinates (commercially available products include Latemul S-120, S-120A, S-180P, and S-180A manufactured by Kao Corporation, and Eleminol JS-2 manufactured by Sanyo Chemical Industries, Ltd.), polyoxyethylene alkyl phenyl ether sulfates, and polyoxyethylene alkyl phenyl ether sulfates. anionic reactive surfactants such as oxyethylene alkylphenyl ester sulfates (commercially available products include Aqualon HS-10, HS-20, HS-30, BC-10, and BC-20 manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., and Adeka Reasoap SDX-222, SDX-223, SDX-232, SDX-233, SDX-259, SE-10N, and SE-20N manufactured by ADEKA Corporation), (meth)acrylate sulfates (commercially available products include Antox MS-60 and MS-2N manufactured by Nippon Nyukazai Co., Ltd., and Eleminol RS-30 manufactured by Sanyo Chemical Industries, Ltd.), and phosphates (commercially available products include H-3330PL manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., and Adeka Reasoap PP-70 manufactured by ADEKA Corporation);and nonionic reactive surfactants such as polyoxyethylene alkyl ethers (commercially available products include, for example, Adeka Reasoap ER-10, ER-20, ER-30, and ER-40 manufactured by ADEKA CORPORATION, and Latemul PD-420, PD-430, and PD-450 manufactured by Kao Corporation), polyoxyalkylene styrenated phenyl ethers (commercially available products include Aqualon AN-10 and AN-20 manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), polyoxyethylene alkyl phenyl ethers or alkyl phenyl esters (commercially available products include, for example, Aqualon RN-10, RN-20, RN-30, and RN-50 manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., and Adeka Reasoap NE-10, NE-20, NE-30, and NE-40 manufactured by ADEKA CORPORATION), and (meth)acrylate sulfates (commercially available products include, for example, RMA-564, RMA-568, and RMA-1114 manufactured by Nippon Nyukazai Co., Ltd.);
[0066] Examples of the dispersion stabilizer include, but are not limited to, polyether, polyvinyl alcohol, polyvinylpyrrolidone, poly(vinylpyrrolidone-vinyl acetate) copolymer, polyacrylic acid, starch, gum arabic, gum tragacanth, casein, gelatin, dextrin, carboxylated starch, cationized starch, dextrin, ethyl cellulose, carboxylated methyl cellulose, hydroxyethyl cellulose, and cationized cellulose.
[0067] The above surfactants and dispersion stabilizers can be used alone or in combination of two or more kinds.
[0068] <Applications of hollow resin particles> The hollow resin particles of the present invention can be used in various applications, such as resin compositions for semiconductor members, coating compositions, cosmetics, paper coating compositions, heat insulating compositions, light diffusing compositions, and light diffusing films.
[0069] The above-mentioned resin composition for semiconductor members, coating composition, cosmetic, paper coating composition, heat insulating composition, light diffusing composition, light diffusing film, etc. may contain components other than the hollow resin particles of the present invention, such as binder resins, solvents, coating surface conditioners, flowability conditioners, UV absorbers, light stabilizers, curing catalysts, extender pigments, coloring pigments, metal pigments, mica powder pigments, dyes, etc. EXAMPLES
[0070] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.
[0071] (1) Polyolefin resin composition In orthodichlorobenzene (d4) at 140°C 1 The values were determined by H-NMR and 13C-NMR analysis (JEOL analyzer, 500 MHz). In the 13C-NMR analysis, the measurement was performed using a gated decoupling method in consideration of quantitativeness. The content of the unsaturated carboxylic acid component was calculated from the acid value of the polyolefin resin and the mass of the unsaturated carboxylic acid per 1 g of the polyolefin resin measured by the methods described below, and from these values, the content was calculated by the following formula. Content of unsaturated carboxylic acid component (mass%)=(mass of unsaturated carboxylic acid) / (mass of raw material olefin resin)×100
[0072] <Method for measuring the acid value of polyolefin resin> 0.15g of polyolefin resin was refluxed in 20mL of tetrahydrofuran (THF), and after confirming that the resin was completely dissolved, the temperature of the solution was maintained at 60°C while stirring. A few drops of cresol red indicator were added to this polyolefin resin THF solution, and titrated with a 0.1mol / L potassium hydroxide methanol solution. The acid value of the polyolefin resin was calculated from the titration amount.
[0073] <Calculation of mass of unsaturated carboxylic acid per 1g of polyolefin resin> Mass of unsaturated carboxylic acid (mg / g) = (Acid value of polyolefin resin (mgKOH / g) / Formula amount of KOH) x Molecular weight of unsaturated carboxylic acid* (*If the unsaturated carboxylic acid component is a dicarboxylic acid or its anhydride, use the value obtained by multiplying the molecular weight by 1 / 2.)
[0074] (2) Volume average particle size of particles The volume average particle size was determined using a Microtrac particle size distribution analyzer UPA150 (Model No. 9340) manufactured by Nikkiso Co., Ltd. The refractive index of the resin used to calculate the volume average particle size was set to 1.50.
[0075] (3) Dielectric constant Polyarylate resin (UNIFINER M-2000H manufactured by Unitika Ltd.) was dissolved in cyclohexanone to a solid content of 15% by mass. 0.6 g of each of the particles obtained in the examples and comparative examples was added to 15 g of this cyclohexanone solution of polyarylate resin, and the mixture was degassed and stirred using a planetary centrifugal mixer (ARE-250 manufactured by THINKY Corporation) to prepare a coating material. The prepared coating material was applied to a 5 mm thick glass plate using an applicator to a wet thickness of 250 μm, and then heated at 160° C. for 40 minutes to remove cyclohexanone. After cooling to room temperature, the dielectric constant of the obtained film was measured by a cavity resonance method (measurement frequency: 5 GHz). The dielectric constant of the film that did not contain hollow resin particles was measured and found to be 2.6.
[0076] (4) Heat resistance The heat resistance was evaluated by measuring the 5% thermal weight loss temperature using a differential thermal and thermogravimetric simultaneous measurement device (TG / DTA6200, AST-2, manufactured by SII NanoTechnology Co., Ltd.). The sampling method and temperature conditions were as follows. The bottom of a platinum measuring container was filled with 10.5±0.5 mg of particles without gaps to prepare a sample for measurement. Under a nitrogen gas flow rate of 230 mL / min, the 5% thermal weight loss temperature was measured using alumina as a reference material. The TG / DTA curve was obtained by heating the sample from 30°C to 500°C at a heating rate of 10°C / min. From the obtained curve, the temperature at 5% weight loss was calculated using the analysis software attached to the device, and the heat resistance was evaluated. From the viewpoint of practicality, the temperature at 5% weight loss under these test conditions is preferably 300°C or higher.
[0077] (5) Flexibility of the coating 5g of copolymer polyester resin (Elitell UE-9100, manufactured by Unitika) and 0.2g of epoxy hardener (Denacol EX-614B, manufactured by Nagase ChemteX Corporation) were dissolved in a mixed solvent of toluene and methyl ethyl ketone (mixed mass ratio 1:1) to prepare a solution with a solid content of 25% by mass. 0.6g of each particle obtained in the examples and comparative examples was added to 9g of this solution, and the mixture was degassed and stirred using a rotation / revolution mixer (ARE-250, manufactured by THINKY Corporation) to prepare a coating material. The prepared coating agent was applied to the corona-treated surface of a biaxially oriented polyester film (Unitika Co., Ltd., Emblet S-50, thickness 50 μm) using an applicator to a wet thickness of 150 μm, and then heated at 160 ° C for 40 minutes to remove toluene and methyl ethyl ketone. After cooling to room temperature, the obtained film was folded back so that the coated surface was on the outside, and a load of 10 kg was placed on it while it was sandwiched between rubber plates from above and below. After 1 hour, the load was removed and the film was taken out, the creased part was returned to its original state, and the appearance of the coating film was visually confirmed. Based on the degree of cracking or whitening of the coating film, the flexibility of the coating film was evaluated according to the following criteria. ◯: No cracks or whitening were observed. ×: Cracks and / or whitening are observed.
[0078] Preparation Example 1 Polyolefin resin "P-1" 280 g of propylene-ethylene copolymer (propylene / ethylene=97.9 / 2.1, mass ratio) was heated and melted in a four-neck flask under a nitrogen atmosphere. Then, the temperature in the system was kept at 170°C, and 10.0 g of maleic anhydride as an unsaturated carboxylic acid and 6.0 g of dicumyl peroxide as a radical generator were added over 1 hour while stirring, and then reacted for 1 hour. After the reaction was completed, the obtained reaction product was poured into a large amount of acetone to precipitate a resin. This resin was further washed several times with acetone to remove unreacted maleic anhydride, and then dried under reduced pressure in a vacuum dryer to obtain polyolefin resin "P-1".
[0079] Preparation Example 2 Polyolefin resin "P-2" 280g of propylene-ethylene copolymer (propylene / ethylene=59.0 / 41.0, mass ratio) was heated and melted in a four-neck flask under a nitrogen atmosphere. Then, the temperature in the system was kept at 170°C, and 32.0g of maleic anhydride and 6.0g of dicumyl peroxide as a radical generator were added over 1 hour while stirring, and then reacted for 1 hour. After the reaction was completed, the reaction product was poured into a large amount of acetone to precipitate a resin. This resin was further washed several times with acetone to remove unreacted maleic anhydride, and then dried under reduced pressure in a vacuum dryer to obtain polyolefin resin "P-2".
[0080] Preparation Example 3 Polyolefin resin "P-3" A polyolefin resin "P-3" was obtained in the same manner as in Preparation Example 1, except that a propylene-butene copolymer (propylene / butene=81.6 / 18.4, mass ratio) was used.
[0081] Preparation Example 4 Polyolefin resin aqueous dispersion "E-1" Using a stirrer equipped with a sealable pressure-resistant 1L glass container with a heater and a pressure gauge, 60g of polyolefin resin "P-1", 69g of tetrahydrofuran, 24g of isopropyl alcohol, 15g of cyclohexane, 6g of triethylamine, 3g of N,N-dimethylethanolamine and 123g of distilled water were charged into the glass container. Then, when the stirring blade rotation speed was set to 300 rpm and stirring was performed, no resin precipitation was observed at the bottom of the container and it was confirmed that the resin was in a floating state. Therefore, while maintaining this state, the heater was turned on after 10 minutes and heating was performed. Then, the temperature inside the system was kept at 125 ° C and stirring was performed for another 60 minutes. After that, the mixture was cooled to room temperature (about 25 ° C) by air cooling while stirring at a rotation speed of 300 rpm, and 150g of distilled water was added. This liquid was placed in a 1L eggplant flask, and while immersed in a hot water bath heated to 60 ° C, the pressure was reduced using an evaporator, and 210g of the aqueous medium was distilled off. After cooling, the liquid component in the flask was filtered through a 300 mesh stainless steel filter (wire diameter 0.04 mm, mesh size 0.045 mm) to obtain a milky white, uniform polyolefin resin aqueous dispersion "E-1". The volume average particle size of the polyolefin resin particles in this aqueous dispersion was 0.23 μm.
[0082] Preparation Example 5 Polyolefin resin aqueous dispersion "E-2" A polyolefin resin aqueous dispersion "E-2" was prepared in the same manner as the preparation method of the polyolefin resin aqueous dispersion "E-1", except that the polyolefin resin "P-2" was used. The volume average particle diameter of the polyolefin resin particles in this aqueous dispersion was 0.10 μm.
[0083] Preparation Example 6 Polyolefin resin aqueous dispersion "E-3" A polyolefin resin aqueous dispersion "E-3" was prepared in the same manner as the preparation of the polyolefin resin aqueous dispersion "E-1", except that the polyolefin resin "P-2" was used. The volume average particle size of the polyolefin resin particles in this aqueous dispersion was 0.19 μm.
[0084] Example 1 In a glass tube, 2g of olefin resin aqueous dispersion "E-1", 0.1g of divinylbenzene (DVB-960, manufactured by Nippon Steel Chemical & Material Co., Ltd.), 0.4g of styrene (St), 2.6mg of 2,2'-azobis[N-(2-hydroxyethyl)-2-methylpropanamide] (VA-086, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator, and 10.5g of distilled water were charged, and after nitrogen replacement, the glass tube was sealed and emulsion polymerization was carried out for 24 hours while shaking at 100 cycles / min in a shaker equipped with a 90°C oil bath. After polymerization, the mixture was cooled to room temperature to obtain an aqueous dispersion. The aqueous dispersion thus obtained was diluted with pure water, and the solid matter was collected by centrifugation, and the solid matter thus obtained was redispersed in pure water. This series of steps consisting of centrifugation and redispersion of the solid matter thus obtained in pure water was repeated three times in total, and then the aqueous dispersion was dried at 50°C to obtain hollow resin particles (H-1). The volume average particle diameter of the hollow resin particles (H-1) in this aqueous dispersion was 0.40 μm.
[0085] Example 2 In a glass tube, 2g of polyolefin resin aqueous dispersion "E-1", 0.4g of styrene, 0.1g of ethylene glycol dimethacrylate as a crosslinking monomer, 2.6mg of 2,2'-azobis[N-(2-hydroxyethyl)-2-methylpropanamide] (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., VA-086) as a polymerization initiator, and 10.5g of distilled water were charged, and after nitrogen replacement, the glass tube was sealed and emulsion polymerization was carried out for 24 hours while shaking at 100 cycles / min in a shaker equipped with a 90°C oil bath. After polymerization, the contents were cooled to room temperature to obtain an aqueous dispersion. The aqueous dispersion thus obtained was diluted with pure water, and the solid matter was collected by centrifugation, and the solid matter thus obtained was redispersed in pure water. This series of steps consisting of centrifugation and redispersion of the solid matter thus obtained in pure water was repeated three times in total, and then the aqueous dispersion was dried at 50°C to obtain hollow resin particles (H-2). The volume average particle diameter of the hollow resin particles (H-2) in this aqueous dispersion was 0.43 μm.
[0086] Example 3 Except for using the polyolefin resin aqueous dispersion "E-2", hollow resin particles (H-3) were produced in the same manner as in Example 1. The volume average particle diameter of the hollow resin particles (H-3) in this aqueous dispersion was 0.16 μm.
[0087] Example 4 Except for using the polyolefin resin aqueous dispersion "E-3", hollow resin particles (H-4) were produced in the same manner as in Example 1. The volume average particle diameter of the hollow resin particles (H-4) in this aqueous dispersion was 0.34 μm.
[0088] Comparative Example 1 An oil phase was prepared by mixing 1.65 g of methyl methacrylate, 1.8 g of dipentaerythritol hexaacrylate, 2.4 g of toluene, 0.126 g of polystyrene (mass average molecular weight 300,000), and 0.104 g of lauroyl peroxide. Next, 38 g of pure water and 0.045 g of sodium dodecyl sulfate as a surfactant were mixed to prepare an aqueous phase. The oil phase was added to the aqueous phase, and a dispersion was prepared using an ultrasonic homogenizer (Hielscher), and the resulting dispersion was heated at 70° C. for 4 hours to carry out polymerization. The aqueous dispersion thus obtained was diluted with pure water, and the solid matter was collected by centrifugation, and the solid matter thus obtained was redispersed in pure water. This series of steps consisting of centrifugation and redispersion of the solid matter thus obtained in pure water was repeated three times in total, and then the aqueous dispersion was dried at 50°C to obtain hollow resin particles (H-4). The volume average particle diameter of the hollow resin particles (H-4) in this aqueous dispersion was 0.42 μm.
[0089] The hollow resin particles obtained in the examples and comparative examples and their evaluation results are shown in Table 1.
[0090] [Table 1] The hollow resin particles obtained in Examples 1 to 4 were excellent in heat resistance, low dielectric properties, and coating film flexibility. On the other hand, the hollow resin particles obtained in Comparative Example 1 did not contain a polyolefin resin but were composed only of a vinyl resin, and therefore had poor flexibility when formed into a coating film.
Claims
1. A hollow resin particle having a shell portion and a hollow portion surrounded by the shell portion, The shell portion contains a polyolefin resin (A) and a vinyl resin (B), The hollow resin particles include a polyolefin resin (A) containing an olefin component and an unsaturated carboxylic acid component as a copolymerization component.
2. 2. The hollow resin particle according to claim 1, wherein the olefin component contains propylene and an olefin other than propylene, and the propylene content is 60% by mass or more relative to 100% by mass of the olefin component.
3. 3. The hollow resin particle according to claim 1, wherein the content of the unsaturated carboxylic acid component is 0.1 to 10.0 parts by mass per 100 parts by mass of the total of propylene and the olefin other than propylene.
4. 3. The hollow resin particle according to claim 1, wherein the vinyl resin (B) contains a crosslinkable monomer as a copolymerization component.
5. 3. The hollow resin particle according to claim 1, wherein the olefin other than propylene is at least one member selected from the group consisting of ethylene, 1-butene, and 4-methyl-1-pentene.
6. 3. The hollow resin particles according to claim 1, having a volume average particle size of 0.05 to 20 μm.
7. 3. A method for producing the hollow resin particles according to claim 1 or 2, comprising the following steps (I) and (II): (I) a polyolefin resin containing an olefin component and an unsaturated carboxylic acid component as a copolymerization component, A process of converting a polyolefin resin into an aqueous dispersion by mixing with a basic compound and an aqueous medium. (II) A step of polymerizing a vinyl monomer in the presence of the aqueous dispersion of the polyolefin resin obtained in (I) above.
Citation Information
Patent Citations
Hollow polymer minute particle and method for producing the same
JP2013221070A
Coating composition and multilayer coating film
JP2018123251A
Resin particle
JP2020033503A