Method for producing composite particles

By emulsifying and curing silicone rubber on core particles with a cationic surfactant, the method ensures uniform coating, maintaining core particle shape and size, improving cosmetic performance.

JP2024165522AInactive Publication Date: 2024-11-28SHIN ETSU CHEMICAL CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023081788
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing composite particles with silicone rubber coatings on core particles fail to maintain the shape and size of the core particles, often resulting in agglomeration and uneven coating, which affects the performance of cosmetics.

Method used

A method involving emulsifying a curable liquid silicone composition to form an oil-in-water emulsion, curing it to create silicone rubber spherical particles, adsorbing these particles onto core particles using a cationic surfactant, and then removing moisture to fix the silicone rubber onto the core particle surfaces.

Benefits of technology

The method produces composite particles where silicone rubber adheres to nearly all core particles, maintaining their shape and size, enhancing cosmetic properties such as natural finish, skin adhesion, and drop stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165522000001_ABST
    Figure 2024165522000001_ABST
Patent Text Reader

Abstract

To provide a method for producing composite particles in which multiple core particles are not contained in each composite particle, the shapes and particle diameters of the core particles are mostly maintained without strong aggregation or fixation of the particles, and substantially all of the added silicone rubber adheres to the surfaces of substantially all of the core particles.SOLUTION: A method for producing composite particles in each of which a silicone rubber adheres to the surface of a core particle comprises: a step in which a curable liquid silicone composition is emulsified to make an oil-in-water emulsion, and is subsequently cured to produce an aqueous dispersion of spherical silicone rubber particles; a step in which core particles, the aqueous dispersion, a cationic surfactant and water are mixed to have the silicone rubber particles adsorbed to the surfaces of the core particles; and a step in which water is volatilized and removed from the mixed liquid, thereby fixing the silicone rubber particles to the surfaces of the core particles. In the mixed liquid, the content of the core particles is 1-100 pts.mass per 100 pts.mass of water, and the content of the spherical silicone rubber particles is 0.1-25 pts.mass per 100 pts.mass of the core particles.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing composite particles. [Background technology]

[0002] Various powder treatments have been used to obtain the functions required for makeup cosmetics such as foundations and makeup bases. Powders coated with silicone rubber have been proposed, which are said to have improved light diffusion properties, a natural finish, excellent adhesion to the skin, and a soft, moist feel. In powder cosmetics, they are also said to have excellent drop stability.

[0003] Several methods have been proposed for producing particles in which silicone rubber is attached to and coated on the surface of core particles.

[0004] Patent Document 1 proposes a method of grinding and mixing silica and silicone rubber, but since the silica particles that serve as core particles are ground, it is not possible to obtain particles that maintain their original shape and particle size. In other words, it is not possible to obtain particles with a specific shape such as a sphere, plate, or rod, and it is also difficult to control the particle size.

[0005] Patent Documents 2 and 3 propose a method of mixing core particles with a curable silicone that becomes silicone rubber, and then curing the silicone, but all or some of the particles have a structure in which multiple core particles exist within the particle, which increases the particle size, making it difficult to maintain the shape of the core particles and control the particle size. Also, when the proportion of silicone is low, it is difficult to coat all of the core particles.

[0006] Patent Document 4 proposes a method in which an aqueous dispersion of silica particles and a curable silicone that will become silicone rubber are emulsified and dispersed in water, and then the silicone is cured. However, the particles obtained in powder form have a structure containing multiple silica particles that will become core particles, and the high content of silicone rubber makes it difficult for the properties of the core particles to be expressed.

[0007] Patent Document 5 proposes a method in which a mixture of inorganic particles and an emulsion of a curable silicone that becomes silicone rubber is spray-dried and the silicone is cured at the same time. However, this method can result in particles that contain multiple inorganic particles that become core particles, or particles that consist only of uncoated silicone rubber.

[0008] Patent Document 6 proposes a method of mixing core particles with silicone rubber particles dispersed in a dispersion medium and then evaporating the dispersion medium. However, since the particles aggregate when the dispersion medium is evaporated, it becomes difficult to maintain the shape of the core particles and control the particle size.

[0009] Patent Document 7 proposes a method in which a crosslinking agent is added to a mixture of core particles and an emulsion of slightly crosslinked silicone, followed by centrifugation to form a cake-like mass, which is dried and cured into rubber at the same time; however, the core particles harden together during curing and are difficult to completely loosen, making it difficult to maintain the shape of the core particles and control their particle size. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Japanese Patent Application Publication No. 8-3451 [Patent Document 2] Japanese Patent Application Publication No. 3-294357 [Patent Document 3] JP 2017-214565 A [Patent Document 4] Japanese Patent Application Publication No. 3-281536 [Patent Document 5] Japanese Patent Application Publication No. 5-32914 [Patent Document 6] JP 2010-163375 A [Patent Document 7] International Publication No. WO2018 / 084176 Summary of the Invention [Problem to be solved by the invention]

[0011] In view of the above circumstances, the present invention aims to provide a method for producing composite particles in which silicone rubber is adhered to the surface of a core particle, in which the composite particles do not contain multiple core particles, the particles do not strongly aggregate or adhere to each other, the shape and particle size of the core particles are largely maintained, and almost all of the blended silicone rubber is adhered to the surface of almost all of the core particles. [Means for solving the problem]

[0012] In order to solve the above problems, the present invention provides A method for producing composite particles comprising adhering silicone rubber to the surface of core particles having a volume average particle size of 1 to 50 μm, comprising the steps of: (i) emulsifying a curable liquid silicone composition with a surfactant to prepare an oil-in-water emulsion, and then curing the curable liquid silicone composition to prepare an aqueous dispersion of silicone rubber spherical particles having a volume average particle size of 50 to 1,000 nm; (ii) mixing the core particles, the aqueous dispersion of the silicone rubber spherical particles prepared in step (i), a cationic surfactant, and water to adsorb the silicone rubber particles onto the surfaces of the core particles, thereby preparing a mixture containing the core particles having the silicone rubber particles adsorbed thereon; and (iii) a step of removing water contained in the mixture containing the core particles having the silicone rubber particles adsorbed thereon, produced in step (ii), by volatilization, and fixing the silicone rubber particles adsorbed on the surfaces of the core particles. the amount of the core particles is in the range of 1 to 100 parts by mass relative to 100 parts by mass of water contained in the mixed liquid prepared in step (ii), the amount of the silicone rubber spherical particles is in the range of 0.1 to 25 parts by mass relative to 100 parts by mass of the core particles, and the amount of the cationic surfactant is in the range of 0.02 to 0.9 parts by mass relative to 100 parts by mass of water.

[0013] With this type of manufacturing method for composite particles, it is possible to produce composite particles in which the composite particles do not contain multiple core particles, the particles do not strongly aggregate or adhere to each other, the shape and particle size of the core particles are largely maintained, and almost all of the compounded silicone rubber adheres to the surface of almost all of the core particles.

[0014] The core particles may be made of at least one of inorganic particles and organic particles.

[0015] In this manner, in the method for producing composite particles of the present invention, the core particles can be either inorganic particles or organic particles, or they may be inorganic-organic composite particles, and one type can be used alone or two or more types can be used in appropriate combination.

[0016] The silicone rubber spherical particles preferably have a rubber hardness in the range of 5 to 95, as measured by a type A durometer as specified in JIS K6253.

[0017] If the rubber hardness is 5 or more, the adhesive can have low and good cohesion, and when used in cosmetics, the cosmetic does not lose its slipperiness and spreadability, or becomes twisted. If the rubber hardness is 95 or less, the cosmetic can have good adhesion to the skin, a soft and moist feel, and drop stability when used in cosmetics. Effect of the Invention

[0018] According to the present invention, it is possible to produce composite particles in which the core particles do not contain multiple core particles, the particles are not strongly aggregated or adhered to each other, the shape and particle size of the core particles are roughly maintained, and substantially all of the silicone rubber blended is attached to the surface of substantially all of the core particles. Furthermore, when blended into cosmetics, the composite particles produced by the manufacturing method of the present invention can improve the natural finish feeling due to light diffusion, have excellent adhesion to the skin, provide a soft and moist feel, and, in the case of powder cosmetics, can have excellent drop stability. [Brief description of the drawings]

[0019] [Figure 1] 1 is an electron microscope photograph of the composite particles obtained in Example 6. [Diagram 2] 1 is an electron microscope photograph of the composite particles obtained in Example 7. [Diagram 3] 1 is an electron microscope photograph of the composite particles obtained in Example 8. [Figure 4] 1 is an electron microscope photograph of the composite particles obtained in Example 9. [Diagram 5] 1 is an electron microscope photograph of the composite particles obtained in Example 10. [Figure 6] 1 is an electron microscope photograph of the composite particles obtained in Example 11. [Figure 7] 1 is an electron microscope photograph of the composite particles obtained in Example 12. [Figure 8] 1 is an electron microscope photograph of cellulose particles used in Examples and Comparative Examples. [Figure 9] 1 is an electron microscope photograph of the composite particles obtained in Example 13. [Figure 10] 1 is an electron microscope photograph of the composite particles obtained in Example 18. [Figure 11] 1 is an electron microscope photograph of silica particles used in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] As a result of extensive research into the above-mentioned problems, the inventors discovered that the above-mentioned object could be achieved by a method in which silicone rubber particles are adsorbed onto the surface of core particles in an aqueous solution of a cationic surfactant and then the water is removed, thereby completing the present invention.

[0021] The present invention will be described in detail below. [Composite particles] The composite particles produced by the method for producing composite particles of the present invention are composite particles having silicone rubber attached to the surface of a core particle.

[0022] Most composite particles have a structure in which the number of core particles in the composite particle is one. The structure can be confirmed by comparative observation of the raw core particle and the manufactured composite particle under an electron microscope. If the shape and size of the composite particle are roughly the same as those of the core particle, it is determined to have the structure.

[0023] When particles are observed overlapping with an electron microscope, it is difficult to distinguish whether they are separate particles or stuck together to form a single particle. In other words, it is difficult to distinguish whether the number of core particles in a composite particle is one structure, or whether multiple structural particles are stuck together to form multiple core particles in a particle. In this case, it can be confirmed by measuring the particle size. If the shape of a particle size distribution diagram with particle size on the horizontal axis and frequency on the vertical axis is roughly the same as that of a core particle, it is determined that the number of core particles in a composite particle is one structure.

[0024] The core particles may be inorganic particles, organic particles, or inorganic-organic composite particles, and may be used alone or in appropriate combination of two or more types, and may be particles that are substantially usable in cosmetics and have a whole range of particle sizes. In addition, as long as the geometric form is one that is usually used in cosmetics, it may be any shape such as spherical, polyhedral, spindle, needle, plate, etc., and may be either non-porous or porous.

[0025] The volume average particle diameter of the core particles is in the range of 1 to 50 μm, and preferably 2 to 30 μm. If the particle diameter is 1 μm or more, the effect of providing a feeling of use such as a silky feeling and smoothness and extensibility can be obtained, and if it is 50 μm or less, a rough feeling does not occur. The volume average particle diameter is measured by the Coulter counter method (electrical resistance method).

[0026] Examples of inorganic particles include particles of titanium oxide, titanium mica, zirconium oxide, zinc oxide, cerium oxide, magnesium oxide, barium sulfate, calcium sulfate, magnesium sulfate, calcium carbonate, magnesium carbonate, talc, cleaved talc, mica, kaolin, sericite, muscovite, synthetic mica, phlogopite, lepidolite, biotite, lithia mica, silicic acid, silica (silicon dioxide), hydrated silicon dioxide, aluminum silicate, magnesium silicate, aluminum magnesium silicate, calcium silicate, barium silicate, strontium silicate, metal tungstate, hydroxyapatite, vermiculite, higilite, bentonite, montmorillonite, hectorite, zeolite, ceramics, secondary calcium phosphate, alumina, aluminum hydroxide, boron nitride, boron nitride, and glass.

[0027] further examples include inorganic pigments, specific examples of which include inorganic red pigments such as iron oxide, iron hydroxide, and iron titanate; inorganic brown pigments such as γ-iron oxide; inorganic yellow pigments such as yellow iron oxide and ochre; inorganic black pigments such as black iron oxide and carbon black; inorganic purple pigments such as manganese violet and cobalt violet; inorganic green pigments such as chromium hydroxide, chromium oxide, cobalt oxide, and cobalt titanate; inorganic blue pigments such as iron blue and ultramarine; colored pigments such as lakes of tar-based pigments and lakes of natural pigments; pearl pigments such as titanium oxide-coated mica, titanium oxide-coated mica, bismuth oxychloride, titanium oxide-coated bismuth oxychloride, titanium oxide-coated talc, fish scale foil, and titanium oxide-coated colored mica; and metal powder pigments such as aluminum powder, copper powder, and stainless steel powder.

[0028] Examples of organic resin particles include particles of polyethylene; polypropylene; polystyrene; divinylbenzene resin; polyvinyl chloride; methacrylic resin; polytetrafluoroethylene; methacrylic-styrene copolymer; polyamide; polycarbonate; polyesters such as polyethylene terephthalate, polybutylene succinate, polyhydroxybutyric acid, and polycaprolactone; cellulose; cellulose derivatives; phenolic resin; melamine resin; benzoguanamine resin; epoxy resin; and polyurethane.

[0029] Further examples include organic dyes. Specific examples include tar dyes such as Red No. 3, Red No. 104, Red No. 106, Red No. 201, Red No. 202, Red No. 204, Red No. 205, Red No. 220, Red No. 226, Red No. 227, Red No. 228, Red No. 230, Red No. 401, Red No. 505, Yellow No. 4, Yellow No. 5, Yellow No. 202, Yellow No. 203, Yellow No. 204, Yellow No. 401, Blue No. 1, Blue No. 2, Blue No. 201, Blue No. 404, Green No. 3, Green No. 201, Green No. 204, Green No. 205, Orange No. 201, Orange No. 203, Orange No. 204, Orange No. 206, and Orange No. 207; and natural dyes such as carminic acid, laccaic acid, carthamine, brazilian, and crocin.

[0030] The inorganic-organic composite particles may be composite particles in which the surfaces of inorganic particles commonly used in cosmetics are coated with organic particles by a publicly known method.

[0031] The particles may be surface-treated with a metal soap, a silane, a silicone, a silicone resin, a fluorine compound, an amino acid, iron oxide, titanium oxide, iron oxide, titanium oxide, or aluminum hydroxide.

[0032] There are no particular limitations on the shape of the silicone rubber adhered to the surface of the core particle, but in the manufacturing method of the present invention, as described below, the shape will be spherical, like fused spherical particles, like a lump, or like a film.

[0033] The density of the rubber attached to the surface of the core particle is not particularly limited. That is, the rubber may be sparsely attached to the surface of the core particle, or may cover the surface of the core particle without any gaps. The shape and density of the attached rubber can be confirmed by an electron microscope.

[0034] The amount of silicone rubber attached to the core particles is in the range of 0.1 to 25 parts by mass, preferably 0.2 to 20 parts by mass, and more preferably 0.5 to 15 parts by mass or more, per 100 parts by mass of the core particles. When the amount attached is 0.1 part by mass or more, it is possible to impart a natural finish feeling due to light diffusion, good adhesion to the skin, a soft and moist feel, and drop stability to the cosmetic. When the amount attached is 25 parts by mass or less, cohesion is low, and there is no decrease in the slipperiness and spreadability of the cosmetic, or wrinkling.

[0035] The rubber constituting the silicone rubber is preferably non-sticky, and its rubber hardness is preferably in the range of 5 to 95, more preferably 10 to 80, as measured by a type A durometer specified in JIS K6253. If the rubber hardness is 5 or more, the cohesiveness is low, and the cosmetic does not suffer from reduced slipperiness or spreadability or from twisting. If the rubber hardness is 95 or less, the cosmetic can be given good adhesion to the skin, a soft and moist feel, and drop stability. The rubber hardness refers to a value measured by preparing a test piece having the shape and dimensions specified in JIS K6253 with the rubber composition.

[0036] Silicone rubber has the formula -(RSiO 2 / 2 ) a Preferably, the cured product has a linear organosiloxane block represented by the formula: R is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 30 carbon atoms, and a is a positive integer of 5 to 5,000.

[0037] The above R has 1 to 30 carbon atoms, preferably 1 to 22, and more preferably 1 to 18. Examples of R include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, decyl, undecyl, dodecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, icosyl, henicosyl, docosyl, tricosyl, tetracosyl, and triacontyl groups; aryl groups such as phenyl, tolyl, and naphthyl groups; benzyl, fluoro, and the like; Examples of such groups include aralkyl groups such as phenylethyl groups, alkenyl groups such as vinyl groups and allyl groups, cycloalkyl groups such as cyclopentyl groups, cyclohexyl groups and cycloheptyl groups, and hydrocarbon groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups have been substituted with atoms such as halogen atoms (fluorine atoms, chlorine atoms, bromine atoms and iodine atoms) and / or substituents such as acryloyloxy groups, methacryloyloxy groups, epoxy groups, glycidoxy groups and carboxyl groups. Preferred are alkyl groups or phenyl groups having 1 to 18 carbon atoms, and it is preferred that 50 mol % or more of all R groups are methyl groups.

[0038] Silicone rubber is obtained from a curable liquid silicone composition, and its curing can be exemplified by addition reaction, condensation reaction, radical reaction, etc. The curable liquid silicone composition contains a component having a reactive group for the above curing reaction (one having both reactive groups, or a component having one reactive group and a component having the other reactive group), a curing catalyst, and a radical generator.

[0039] When silicone rubber is produced by curing through an addition reaction, the curable liquid silicone composition can be exemplified by one that contains (A) an organopolysiloxane having alkenyl groups, (B) an organohydrogenpolysiloxane having silicon-bonded hydrogen atoms, and an addition reaction catalyst.

[0040] The component (A) is represented by the following average composition formula (1): R 1 b R 2c SiO (4-b-c) / 2 (1) represented by the formula, and is an organopolysiloxane having at least 2 alkenyl groups in one molecule. In the formula, R 1 are, independently of each other, unsubstituted or substituted monovalent hydrocarbon groups having 1 to 30 carbon atoms and no alkenyl group. R 2 are, independently of each other, alkenyl groups having 2 to 6 carbon atoms. b and c are positive numbers satisfying 0 < b < 3, 0 < c ≤ 3 and 0.1 ≤ b + c ≤ 3.

[0041] One kind of the organopolysiloxane represented by the average composition formula (1) may be used alone or two or more kinds may be used in combination.

[0042] R 1 has 1 to 30 carbon atoms, preferably 1 to 22, more preferably 1 to 18. R 1 is a monovalent hydrocarbon group excluding the alkenyl group among those exemplified for R above, and R 1 is preferably 50 mol% or more methyl group. R 2 includes vinyl group, allyl group, propenyl group, butenyl group, pentenyl group, hexenyl group, and preferably vinyl group. b and c are preferably positive numbers satisfying 0 < b ≤ 2.295, 0.005 ≤ c ≤ 2.3, 0.5 ≤ b + c ≤ 2.3.

[0043] (A) The kinematic viscosity of the component at 25°C is preferably 100,000 mm 2 / s or less, more preferably 10,000 mm 2 / s or less. When the kinematic viscosity is 100,000 mm 2 / s or less, it is particularly easy to obtain silicone fine particles with a narrow particle size distribution in the preparation of the aqueous dispersion of silicone rubber particles described below. The lower limit of the kinematic viscosity is not particularly limited, but 0.7 mm 2 / s or more, particularly 2 mm 2 / s or more is sufficient. In the present invention, the value of the kinematic viscosity can be the value measured using a capillary viscometer at 25°C.

[0044] The structure of component (A) may be linear, cyclic, or branched, with linear or branched structures having fewer branch units being particularly preferred. There are no particular restrictions on the bonding sites of the alkenyl groups, and they may be bonded to silicon atoms on either the side chain or the terminals of the molecule, with bonding to silicon atoms at both terminals of the linear organopolysiloxane being particularly preferred.

[0045] An example of the linear structure is represented by the following general formula (2).

[0046] [ka] (In the formula, R 1 , R 2 is the same as above, d is a positive number, e is 0 or a positive number, and f is 0, 1, 2, or 3, provided that e and f are numbers that satisfy e+2×f≧2.

[0047] Examples of branched structures include R 1 SiO 3 / 2 Examples of the branched units include those represented by the following general formula (3).

[0048] [ka] (In the formula, R 1 , R 2 is the same as above, g is a positive number, h is 0 or a positive number, i is a positive number, and j is 0, 1, 2, or 3, provided that h and j are numbers that satisfy h+j≧1.

[0049] SiO 4 / 2 An example of a structure branched by units is one represented by the following general formula (4).

[0050] [ka] (In the formula, R 1 , R 2is the same as described above, k is a positive number, l is 0 or a positive number, m is a positive number, n is 0, 1, 2, or 3, provided that l and n satisfy l + n ≥ 1.)

[0051] In addition, those represented by the following unit formula (5) and having two or more alkenyl groups per molecule are exemplified.

[0052] [R 1 3SiO 1 / 2 o [R 2 (R 1 )2SiO 1 / 2 p [SiO 4 / 2 q [(OR 3 )SiO 3 / 2 r (5) (In the formula, R 1 , R 2 are the same as described above, R 3 is a hydrogen atom or an unsubstituted monovalent hydrocarbon group having 1 to 6 carbon atoms, o is 0 or a positive number, p is a positive number, and q is a positive number, and r is 0 or a positive number.)

[0053] Component (B) is an organohydrogenpolysiloxane represented by the following average composition formula (6) R 4 s H t SiO (4-s-t) / 2 (6) and has at least two hydrogen atoms bonded to silicon atoms (referred to as SiH groups) in one molecule. In the formula, R 4 are, independently of each other, unsubstituted or substituted monovalent hydrocarbon groups having 1 to 30 carbon atoms and not having an alkenyl group. s and t are numbers satisfying 0 < s < 3, 0 < t ≤ 3, and 0.1 ≤ s + t ≤ 3.)

[0054] One kind of the organopolysiloxane represented by the average composition formula (6) may be used alone or two or more kinds may be used in combination.)

[0055] R 4 ​​​​has 1 to 30 carbon atoms, preferably 1 to 22, more preferably 1 to 18. R 4 is the same monovalent hydrocarbon group as R 1 and preferably 80 mol% or more is a methyl group, more preferably 95% or more is a methyl group. s and t are positive numbers preferably satisfying 0 < s ≦ 2.295, 0.005 ≦ t ≦ 2.3 and 0.5 ≦ s + t ≦ 2.3.

[0056] (B) component has a kinematic viscosity at 25 °C of preferably 100,000 mm 2 / s or less, more preferably 10,000 mm 2 / s or less. When the kinematic viscosity is 100,000 mm 2 / s or less, it is particularly easy to obtain silicone fine particles with a narrow particle size distribution in the preparation of the aqueous dispersion of silicone rubber particles described below. The lower limit of the kinematic viscosity is not particularly limited, but 0.4 mm 2 / s or more, particularly 2 mm 2 / s or more is sufficient.

[0057] Further, the structure of the (B) component may be linear, cyclic, or branched, but linear or branched is particularly preferred. Also, the bonding position of the hydrogen atom bonded to the silicon atom is not particularly limited and may be bonded to any silicon atom in the side chain and the terminal of the molecule.

[0058] Examples of those having a linear structure include those represented by the following general formula (7).

[0059]

Chemical formula

[0060] Examples of the branched structure include R 4 SiO 3 / 2Examples of the branched units include those represented by the following general formula (8).

[0061] [ka] (In the formula, R 4 is the same as above, x is a positive number, y is 0 or a positive number, z is a positive number, and a1 is 0, 1, 2, or 3, provided that y and a1 are numbers that satisfy y+a1≧1.

[0062] SiO 4 / 2 An example of a structure branched by units is one represented by the following general formula (9).

[0063] [ka] (In the formula, R 4 is the same as above, b1 is a positive number, c1 is 0 or a positive number, d1 is a positive number, and e1 is 0, 1, 2, or 3, provided that c1 and e1 are numbers that satisfy c1+e1≧1.

[0064] Also included are those represented by the following formula (10) and having two or more hydrogen atoms bonded to silicon atoms per molecule. [R 4 3SiO 1 / 2 ] f1 [H(R 4 )2SiO 1 / 3 ] g1 [SiO 4 / 2 ] h1 [(OR 5 )SiO 3 / 2 ] i1 (10) In the formula, R 4 is the same as above, and R 5 represents a hydrogen atom or an unsubstituted monovalent hydrocarbon group having 1 to 6 carbon atoms, f1 is 0 or a positive number, g1 is a positive number, h1 is a positive number, and i1 is 0 or a positive number.

[0065] As described above, component (A) is an organopolysiloxane having two or more alkenyl groups in one molecule, and component (B) is an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms in one molecule. However, the combination of an organopolysiloxane (A) having only two alkenyl groups and an organohydrogenpolysiloxane (B) having only two SiH groups is excluded. This is because the combination of an organopolysiloxane having two alkenyl groups as component (A) and an organohydrogensiloxane having two SiH groups as component (B) results in a sticky cured product, making it impossible to obtain silicone rubber. That is, when component (A) has two alkenyl groups, at least one of components (B) is an organohydrogensiloxane having three or more SiH groups, and when component (B) has two SiH groups, at least one of components (A) is an organosiloxane having three or more alkenyl groups.

[0066] The amount of component (B) relative to component (A) is preferably an amount such that the ratio of the number of SiH groups in component (B) to the number of monovalent alkenyl groups in component (A) is 0.5 to 2, and more preferably an amount such that it is 0.7 to 1.5. When component (B) is blended in an amount such that the ratio of the number of SiH groups falls within the above range, the resulting silicone rubber cured product is not sticky and has appropriate reactivity.

[0067] Examples of the catalyst for the addition reaction include platinum group metal catalysts used in hydrosilylation reactions, such as platinum (including platinum black), rhodium, and palladium; platinum chlorides such as H2PtCl4·XH2O, H2PtCl6·XH2O, NaHPtCl6·XH2O, KHPtCl6·XH2O, Na2PtCl6·XH2O, K2PtCl4·XH2O, PtCl4·XH2O, PtCl2, and Na2HPtCl4·XH2O (wherein X is an integer of 0 to 6, preferably 0 or 6), chloroplatinic acid, and platinum chlorides. Examples of such catalysts include acid salts, alcohol-modified chloroplatinic acid, platinum chloride, complexes of chloroplatinic acid and olefins, complexes of chloroplatinic acid and vinyl group-containing siloxanes, complexes of platinum and vinyl group-containing siloxanes, platinum black, platinum group metals such as palladium supported on supports such as alumina, silica, and carbon, rhodium-olefin complexes, and chlorotris(triphenylphosphine)rhodium (Wilkinson's catalyst). These catalysts may be used alone or in combination of two or more.

[0068] The amount of the platinum group metal catalyst used may be an effective amount as a hydrosilylation reaction catalyst, and the amount of platinum group metal in the platinum group metal catalyst relative to the total amount of components (A) and (B) is usually about 0.1 to 500 ppm, preferably about 0.5 to 200 ppm, and more preferably about 1 to 100 ppm, calculated by mass.

[0069] The silicone rubber may contain silicone oil, organosilane, inorganic powder, organic powder, antioxidant, and the like.

[0070] [Method of manufacturing composite particles] The present invention relates to a composite particle comprising: (i) emulsifying a curable liquid silicone composition with a surfactant to prepare an oil-in-water emulsion, and then curing the curable liquid silicone composition to prepare an aqueous dispersion of silicone rubber spherical particles having a volume average particle size of 50 to 1,000 nm; (ii) mixing the core particles, the aqueous dispersion of the silicone rubber spherical particles prepared in step (i), a cationic surfactant, and water to adsorb the silicone rubber particles onto the surfaces of the core particles, thereby preparing a mixture containing the core particles having the silicone rubber particles adsorbed thereon; and (iii) a step of removing water contained in the mixture containing the core particles having the silicone rubber particles adsorbed thereon, produced in step (ii), by volatilization, and fixing the silicone rubber particles adsorbed on the surfaces of the core particles. The present invention is produced by a method comprising the steps of:

[0071] In addition, in the method for producing composite particles of the present invention, the amount of the core particles per 100 parts by mass of water contained in the mixed liquid prepared in step (ii) is in the range of 1 to 100 parts by mass, and the amount of the silicone rubber spherical particles per 100 parts by mass of the core particles is in the range of 0.1 to 25 parts by mass.

[0072] The preparation of the water dispersion of silicone rubber spherical particles in step (i) can be produced by a known method. The above-mentioned curable liquid silicone composition is emulsified using a surfactant to prepare an oil-in-water emulsion, and then the curable liquid silicone is cured by carrying out an addition reaction, a condensation reaction, a radical reaction, or the like. In order to contain silicone oil, organosilane, inorganic powder, organic powder, and antioxidants in the silicone rubber particles, they may be blended in the curable liquid silicone composition. If the method involves emulsifying this curable liquid silicone composition and then carrying out a curing reaction, the shape of the obtained silicone rubber particles will be spherical.

[0073] When making the water dispersion of silicone rubber spherical particles by curing by addition reaction, the method can be added surfactant and water to the curable liquid silicone composition consisting of (A) the organopolysiloxane having alkenyl group and (B) the organohydrogenpolysiloxane having silicon atom-bonded hydrogen atom, emulsify, make oil-in-water emulsion, and then add platinum group metal catalyst to carry out addition reaction.It is also possible to mix platinum group metal catalyst in advance into the curable liquid silicone composition, but in this case, it is necessary to adjust temperature, adjust catalyst amount, mix regulator, etc. so that the reaction does not proceed before emulsification is completed.

[0074] The surfactant used for emulsification is not particularly limited, and may be a nonionic surfactant, an anionic surfactant, a cationic surfactant, or an amphoteric surfactant. A nonionic surfactant is preferable. These may be used alone or in combination of two or more.

[0075] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene polyoxypropylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyethylene glycol fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene glycerin fatty acid esters, polyglycerin fatty acid esters, propylene glycol fatty acid esters, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, polyoxyethylene hydrogenated castor oil fatty acid esters, polyoxyethylene alkylamines, polyoxyethylene fatty acid amides, polyoxyethylene modified organopolysiloxanes, and polyoxyethylene polyoxypropylene modified organopolysiloxanes.

[0076] Examples of anionic surfactants include alkyl sulfate salts such as sodium lauryl sulfate, polyoxyethylene alkyl ether sulfate salts, polyoxyethylene alkyl phenyl ether sulfate salts, sulfate salts of fatty acid alkylol amides, alkyl benzene sulfonates, polyoxyethylene alkyl phenyl ether sulfonates, α-olefin sulfonates, α-sulfofatty acid ester salts, alkyl naphthalene sulfonates, alkyl diphenyl ether disulfonates, alkanesulfonates, N-acyltaurate salts, dialkyl sulfosuccinates, monoalkyl sulfosuccinates, polyoxyethylene alkyl ether sulfosuccinates, fatty acid salts, polyoxyethylene alkyl ether carboxylates, N-acyl amino acid salts, monoalkyl phosphate salts, dialkyl phosphate salts, and polyoxyethylene alkyl ether phosphate salts.

[0077] Examples of the cationic surfactant include alkyltrimethylammonium salts, dialkyldimethylammonium salts, trialkylmethylammonium salts, polyoxyethylenealkyldimethylammonium salts, dipolyoxyethylenealkylmethylammonium salts, tripolyoxyethylenealkylammonium salts, alkylbenzyldimethylammonium salts, alkylpyridinium salts, monoalkylamine salts, and monoalkylamidoamine salts.

[0078] Examples of amphoteric surfactants include alkyl dimethylamine oxide, alkyl dimethyl carboxybetaine, alkyl amidopropyl dimethyl carboxybetaine, alkyl hydroxysulfobetaine, and alkyl carboxymethyl hydroxyethyl imidazolinium betaine.

[0079] For emulsification, a general emulsifying disperser may be used, and examples of such machines include a high-speed rotating centrifugal radiation type agitator such as a homodisper, a high-speed rotating shear type agitator such as a homomixer, a high-pressure jet type emulsifying disperser such as a homogenizer, a colloid mill, an ultrasonic emulsifying machine, etc. The stirring speed, time, etc. are not particularly limited as long as the emulsification can be performed and the desired particle size can be obtained.

[0080] The volume average particle size of the rubber particles in the aqueous dispersion of silicone rubber spherical particles is preferably smaller than that of the core particles. If it is smaller than the core particles, it is possible to impart to the cosmetic a natural finish due to light diffusion, good adhesion to the skin, a soft and moist feel, and drop stability. The volume average particle size is in the range of 50 to 1,000 nm, and preferably 100 to 500 nm. If it is 1,000 nm or less, it is possible for it to adhere to the core particles. The volume average particle size is measured by a laser diffraction / scattering method.

[0081] The core particles used in step (ii) may be the above-mentioned inorganic particles, organic particles, or inorganic-organic composite particles, and may be used alone or in appropriate combination of two or more kinds. An aqueous dispersion prepared in advance or an aqueous dispersion synthesized in water may be used as it is.

[0082] In step (ii), the amount of core particles is in the range of 1 to 100 parts by mass, preferably 5 to 50 parts by mass, and more preferably 10 to 30 parts by mass, per 100 parts by mass of water contained in the mixed liquid. When the amount of core particles is 1 part by mass or more, production efficiency is high. On the other hand, when the amount of core particles is 100 parts by mass or less, the kinetic viscosity of the mixed liquid does not become too high, making it easier to attach the silicone rubber particles.

[0083] In step (ii), the amount of the aqueous dispersion of silicone rubber spherical particles should be the amount of silicone rubber to be attached to the surface of the core particles. The amount of silicone rubber spherical particles in the aqueous dispersion of silicone rubber spherical particles is in the same range as the amount of silicone rubber relative to the core particles in the composite particles described above, and is in the range of 0.1 to 25 parts by mass, preferably 0.2 to 20 parts by mass, and more preferably 0.5 to 15 parts by mass or more relative to 100 parts by mass of the core particles.

[0084] The cationic surfactant used in step (ii) has the effect of adsorbing the silicone rubber particles to the core particles. The cationic surfactant is adsorbed to the surface of the silicone rubber particles, increasing the zeta potential (a value that indicates the charged state of a solid surface) of the rubber particle surface, which increases the difference in zeta potential with the core particles, and it is presumed that this causes the silicone rubber particles to be adsorbed to the core particles by electrostatic interaction.

[0085] The cationic surfactant used in step (ii) may be any of those mentioned above. It may be in the form of an aqueous solution, a solution in a water-soluble organic solvent such as an alcohol, or an aqueous solution containing a water-soluble organic solvent.

[0086] The amount of the cationic surfactant used in step (ii) is in the range of 0.02 to 0.9 parts by mass, and more preferably 0.03 to 0.7 parts by mass, per 100 parts by mass of water contained in the mixed liquid. If the amount is 0.02 to 0.9 parts by mass, the silicone rubber particles can be adsorbed onto the surface of the core particles.

[0087] When a cationic surfactant is contained in the aqueous dispersion of silicone rubber spherical particles prepared in step (i) and the amount of cationic surfactant in step (ii) is the desired amount, there is no need to add additional cationic surfactant since the cationic surfactant has already been mixed in. The mixing of the aqueous dispersion of silicone rubber spherical particles prepared in step (i), the cationic surfactant, and water in step (ii) of the present invention also includes such cases.

[0088] In step (ii), a surfactant other than the cationic surfactant or a water-soluble polymer may be contained. The surfactant is the surfactant used for emulsification in the aqueous dispersion of the silicone rubber spherical particles produced in step (i). When the core particles are blended in the form of an aqueous dispersion, a surfactant other than the cationic surfactant or a water-soluble polymer may be contained as a dispersant. In addition, a surfactant other than the cationic surfactant or a water-soluble polymer may be blended in step (ii).

[0089] The surfactant other than the cationic surfactant is not particularly limited, and may be a nonionic surfactant, an anionic surfactant, or an amphoteric surfactant, as described above, with the nonionic surfactant or amphoteric surfactant being preferred.

[0090] Examples of the water-soluble polymer include nonionic water-soluble polymers and anionic water-soluble polymers, with nonionic water-soluble polymers being preferred. It is preferable not to use cationic water-soluble polymers, as they may inhibit the adsorption of silicone rubber particles to the core particle surface.

[0091] Examples of the nonionic water-soluble polymer include polyvinyl alcohol, polyacrylamide, polyvinylpyrrolidone, polyethylene oxide, polymethyl vinyl ether, polyisopropylacrylamide, methyl cellulose, hydroxypropyl methyl cellulose, starch, guar gum, and xanthan gum.

[0092] Examples of the anionic water-soluble polymer include sodium polyacrylate, carboxyvinyl polymer, polysodium styrene sulfonate, sodium naphthalene sulfonate condensate, sodium cellulose sulfate, sodium carboxymethylcellulose, carboxymethyl starch, sodium alginate, gum arabic, carrageenan, and derivatives thereof obtained by copolymerizing monomers having nonionic groups or anionic groups with these.

[0093] In step (ii), the core particles, the aqueous dispersion of silicone rubber spherical particles, the cationic surfactant, and water may be mixed using an agitating blade such as a paddle blade, a propeller blade, a swept-back blade, or an anchor-shaped blade.

[0094] The core particles, the aqueous dispersion of silicone rubber spherical particles, the cationic surfactant, and water are preferably mixed by stirring the core particles, the cationic surfactant, and the water, and then the aqueous dispersion of silicone rubber spherical particles is added while stirring. The core particles, the cationic surfactant, and the water may be added in any order. Alternatively, the core particles and the water are preferably mixed by stirring, and then the aqueous dispersion of silicone rubber spherical particles is added, and then the cationic surfactant is added while stirring.

[0095] When the core particles are used in the form of an aqueous dispersion, the order may be to stir and mix the aqueous dispersion of silicone rubber spherical particles, the cationic surfactant, and water, and then add the aqueous dispersion of core particles while stirring. The aqueous dispersion of silicone rubber spherical particles, the cationic surfactant, and water may be added in any order. Alternatively, the aqueous dispersion of core particles, the aqueous dispersion of silicone rubber spherical particles, and water may be stirred and mixed, and then add the cationic surfactant while stirring. The aqueous dispersion of core particles, the aqueous dispersion of silicone rubber spherical particles, and water may be added in any order.

[0096] In step (ii), the pH of the water may be lowered or raised by adding an acid or alkali. If the change in pH increases the zeta potential difference between the core particles and the silicone rubber spherical particles, this may facilitate the adsorption of the silicone rubber spherical particles to the core particles.

[0097] In step (ii), a water-soluble organic solvent such as alcohol may be added to the mixture for the purpose of facilitating the adsorption of the silicone rubber spherical particles to the core particles.

[0098] The temperature in step (ii) is not particularly limited and may be in the range of 0 to 100°C.

[0099] After mixing the core particles, the aqueous dispersion of silicone rubber spherical particles, the cationic surfactant, and water, it is preferable to continue stirring for a while until the silicone rubber spherical particles are adsorbed onto the core particles.

[0100] In step (iii), the removal by volatilization of water (moisture contained in the mixed liquid) from the mixed liquid containing the core particles having the silicone rubber particles adsorbed thereon produced in step (ii) can be carried out, for example, by heating under normal pressure or reduced pressure, and specific examples include a method of removing moisture by leaving the mixed liquid stationary under heating, a method of removing moisture while stirring and flowing the mixed liquid under heating, a method of spraying and dispersing the mixed liquid in a hot air current as with a spray dryer, a method of using a flowing heat medium, etc. Note that, as a pretreatment for this operation, the mixed liquid may be concentrated by methods such as heating and dehydration, filtration separation such as pressure filtration, centrifugation, decantation, etc.

[0101] When an acid or alkali is added in the step (ii), the mixture may be neutralized by adding an acid or alkali before removing water by evaporation, and may be washed with water, alcohol, or the like, if necessary.

[0102] It is assumed that the adhesion of the silicone rubber particles to the core particle surface in step (iii) is achieved through the following process. When the amount of moisture decreases due to the evaporation of water, a capillary force is generated between the core particle and the silicone rubber spherical particles adsorbed on its surface. The silicone rubber particles are attracted to the core particle surface by the capillary force, and deform so as to spread over the core particle surface, increasing the adhesion area with the core particle. This increases the adhesive force, and the particles remain attached even after the water is removed and the capillary force disappears.

[0103] The shape of the silicone rubber that adheres to the surface of the core particles after the water has evaporated varies depending on the hardness of the rubber. If the rubber hardness is high, it is spherical, if the rubber hardness is lowered, it will take on a shape similar to fused spherical particles, and if the rubber hardness is lowered even further, it will take on a lump-like or film-like shape.

[0104] It is believed that the deformation of the silicone rubber spherical particles due to adhesion to the surface of the core particle is due to the action of capillary forces between the core particle and the silicone rubber spherical particles generated in step (iii) as described above, and that capillary forces also occur between the silicone rubber spherical particles themselves, which is also believed to have an effect.

[0105] In the method for producing composite particles of the present invention, as described above, the produced composite particles have low cohesion, but may be weakly cohesive. In such a case where the particles obtained by removing water from the mixture are cohesive, it is advisable to disintegrate them with a grinding machine such as a jet mill, a ball mill, or a hammer mill.

[0106] The composite particles of the present invention may have their surfaces treated with a silylation agent, silicone oil, waxes, paraffins, organic fluorine compounds, surfactants, or the like in order to impart or improve water repellency or improve dispersibility in oil agents. EXAMPLES

[0107] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the examples, the kinetic viscosity is a value measured using a capillary viscometer at 25° C., and "%" representing the concentration and content indicates "% by mass."

[0108] [Example 1] (Step (i): Preparation of an aqueous dispersion of silicone rubber spherical particles) The kinetic viscosity shown by the following formula (11) is 10 mm 2 313 g of a vinyl group-containing dimethylpolysiloxane (A1) having a kinematic viscosity of 117 mm3 / s, 287 g of methylhydrogenpolysiloxane (B1) with 1.0% alcohol / s (amount of hydrosilyl groups per vinyl group) and 0.1 g of dl-α-tocopherol (antioxidant) were charged into a 1-liter glass beaker and mixed and dissolved using a homomixer. 45 g of polyoxyethylene lauryl ether (product name: Emulgen 109P, Kao Corporation) and 150 g of water were added and stirred using a homomixer, and thickening was observed. Stirring was continued for another 15 minutes. Next, 402 g of water was added to dilute the mixture, and the mixture was passed through a homogenizer at a pressure of 100 MPa to obtain a uniform white emulsion. 498.5 g of this emulsion was transferred to a 1-L glass flask equipped with an anchor-shaped stirring blade stirrer, and the temperature was adjusted to 20-25°C. After that, a mixed solution of 0.5 g of an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) and 1 g of polyoxyethylene lauryl ether (product name: Emulgen 109P, manufactured by Kao Corporation) was added with stirring at the same temperature for 24 hours, yielding an aqueous dispersion of silicone rubber spherical particles.

[0109] The volume average particle size of the silicone rubber spherical particles was measured using a laser diffraction / scattering particle size distribution analyzer LA-960 (manufactured by Horiba, Ltd.) and was found to be 320 nm.

[0110] Separately from the preparation of the aqueous dispersion of silicone rubber spherical particles, vinyl group-containing dimethylpolysiloxane (A1) represented by the following formula (11), methylhydrogenpolysiloxane (B1) represented by the following formula (12), and an isododecane solution of platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) were mixed in the above-mentioned mixing ratio, poured into an aluminum petri dish to a thickness of 10 mm, left at 25° C. for 6 hours, and then heated in a thermostatic chamber at 50° C. for 1 hour. The resulting cured product was a non-sticky rubber elastic body, and its hardness was measured with a durometer A hardness tester to be 73.

[0111] (A1): Dimethylpolysiloxane containing vinyl groups [ka]

[0112] (B1): Methylhydrogenpolysiloxane [ka]

[0113] [Example 2] (Step (i): Preparation of an aqueous dispersion of silicone rubber spherical particles) The kinetic viscosity, as shown in the following formula (13), is 61 mm 2 343 g of a vinyl group-containing dimethylpolysiloxane (A2) having a kinematic viscosity of 30 mm 2 57 g of methylhydrogenpolysiloxane (B2) with 1.0% alcohol / s (amount of hydrosilyl groups per vinyl group) and 0.1 g of dl-α-tocopherol (antioxidant) were placed in a 1-liter glass beaker and mixed and dissolved using a homomixer. 30 g of polyoxyethylene lauryl ether (product name: Emulgen 109P, manufactured by Kao Corporation) and 40 g of water were added and stirred using a homomixer, resulting in thickening to a state where stirring was no longer possible. The thickened material was kneaded for 15 minutes using a homodisper. 527 g of water was then added and mixed using a homomixer, resulting in a uniform white emulsion. This emulsion was transferred to a 1-L glass flask fitted with an anchor-shaped stirring device, and the temperature was adjusted to 20-25°C. After that, a mixed solution of 1 g of an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) and 2 g of polyoxyethylene lauryl ether (product name: Emulgen 109P, manufactured by Kao Corporation) was added with stirring and stirred at the same temperature for 24 hours to obtain an aqueous dispersion of silicone rubber spherical particles.

[0114] The volume average particle size of the silicone rubber spherical particles was measured using a laser diffraction / scattering particle size distribution analyzer LA-960 (manufactured by Horiba, Ltd.) and was found to be 330 nm.

[0115] Separately from the preparation of the aqueous dispersion of silicone rubber spherical particles, vinyl-containing dimethylpolysiloxane (A2) represented by the following formula (13), methylhydrogenpolysiloxane (B2) represented by the following formula (14), and an isododecane solution of platinum-vinyl-containing disiloxane complex (platinum content 0.5%) were mixed in the above-mentioned proportions, poured into an aluminum petri dish to a thickness of 10 mm, left at 25° C. for 6 hours, and then heated in a thermostatic chamber at 50° C. for 1 hour. The resulting cured product was a non-sticky rubber elastic body, and its hardness was measured with a durometer A hardness tester to be 50.

[0116] (A2): Dimethylpolysiloxane containing vinyl groups [ka]

[0117] (B2): Methylhydrogenpolysiloxane [ka]

[0118] [Example 3] (Step (i): Preparation of an aqueous dispersion of silicone rubber spherical particles) The kinetic viscosity, as shown in the following formula (15), is 125 mm 2 365 g of a vinyl group-containing dimethylpolysiloxane (A3) having a kinematic viscosity of 30 mm 235 g of methylhydrogenpolysiloxane (B2) with 1.0% by weight (amount of hydrosilyl groups per vinyl group) and 0.1 g of dl-α-tocopherol (antioxidant) were placed in a 1-liter glass beaker and mixed and dissolved using a homomixer. 30 g of polyoxyethylene lauryl ether (product name: Emulgen 109P, manufactured by Kao Corporation) and 35 g of water were added and stirred using a homomixer, resulting in thickening to a state where stirring was no longer possible. The thickened material was kneaded for 15 minutes using a homodisper. Next, 532 g of water was added and mixed using a homomixer, resulting in a uniform white emulsion. This emulsion was transferred to a 1-L glass flask fitted with an anchor-shaped stirring device, and the temperature was adjusted to 20-25°C. After that, a mixed solution of 1 g of an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) and 2 g of polyoxyethylene lauryl ether (product name: Emulgen 109P, manufactured by Kao Corporation) was added with stirring and stirred at the same temperature for 24 hours to obtain an aqueous dispersion of silicone rubber spherical particles.

[0119] The volume average particle size of the silicone rubber spherical particles was measured using a laser diffraction / scattering particle size distribution analyzer LA-960 (manufactured by Horiba, Ltd.) and was found to be 310 nm.

[0120] Separately from the preparation of the aqueous dispersion of silicone rubber spherical particles, vinyl-containing dimethylpolysiloxane (A3) represented by the following formula (15), methylhydrogenpolysiloxane (B2) represented by the above formula (14), and an isododecane solution of platinum-vinyl-containing disiloxane complex (platinum content 0.5%) were mixed in the above-mentioned proportions, poured into an aluminum petri dish to a thickness of 10 mm, left at 25° C. for 6 hours, and then heated in a thermostatic chamber at 50° C. for 1 hour. The resulting cured product was a non-sticky rubber elastic body, and its hardness was measured with a durometer A hardness tester to be 43.

[0121] (A3): Dimethylpolysiloxane containing vinyl groups [ka]

[0122] [Example 4] (Step (i): Preparation of an aqueous dispersion of silicone rubber spherical particles) The kinetic viscosity, as shown in the following formula (16), is 600 mm 2 384 g of a vinyl group-containing dimethylpolysiloxane (A4) having a kinematic viscosity of 30 mm 2 16 g of methylhydrogenpolysiloxane (B2) with 1.0% by weight per vinyl group (amount of hydrosilyl groups per vinyl group) and 0.1 g of dl-α-tocopherol (antioxidant) were placed in a 1-liter glass beaker and mixed and dissolved using a homomixer. 32 g of polyoxyethylene lauryl ether (product name: Emulgen 109P, Kao Corporation) and 36 g of water were added and stirred using a homomixer, resulting in thickening to a state where stirring was impossible. The thickened material was kneaded for 15 minutes using a homodisper. 530 g of water was then added and mixed using a homomixer, resulting in a uniform white emulsion. This emulsion was transferred to a 1-L glass flask equipped with an anchor-shaped stirring device, and the temperature was adjusted to 20-25°C. After that, a mixed solution of 0.6 g of an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) and 1 g of polyoxyethylene lauryl ether (product name: Emulgen 109P, manufactured by Kao Corporation) was added with stirring at the same temperature for 24 hours, yielding an aqueous dispersion of silicone rubber spherical particles.

[0123] The volume average particle size of the silicone rubber spherical particles was measured using a laser diffraction / scattering particle size distribution analyzer LA-960 (manufactured by Horiba, Ltd.) and was found to be 320 nm.

[0124] Separately from the preparation of the aqueous dispersion of silicone rubber spherical particles, vinyl-containing dimethylpolysiloxane (A4) represented by the following formula (16), methylhydrogenpolysiloxane (B2) represented by the above formula (14), and an isododecane solution of platinum-vinyl-containing disiloxane complex (platinum content 0.5%) were mixed in the above-mentioned proportions, poured into an aluminum petri dish to a thickness of 10 mm, left at 25° C. for 6 hours, and then heated in a thermostatic chamber at 50° C. for 1 hour. The resulting cured product was a non-sticky rubber elastic body, and its hardness was measured to be 27 using a durometer A hardness tester.

[0125] (A4): Dimethylpolysiloxane containing vinyl groups [ka]

[0126] [Example 5] (Step (i): Preparation of an aqueous dispersion of silicone rubber spherical particles) The kinetic viscosity, as shown in the following formula (17), is 5,060 mm 2 393 g of vinyl group-containing dimethylpolysiloxane (A5) having a kinematic viscosity of 30 mm 2 7 g of methylhydrogenpolysiloxane (B2) with 1.0% alcohol / s (amount of hydrosilyl groups per vinyl group) and 0.1 g of dl-α-tocopherol (antioxidant) were placed in a 1-liter glass beaker and mixed and dissolved using a homomixer. Polyoxyethylene lauryl ether (trade name: Emulgen 109P, manufactured by Kao Corporation) When 42g of the emulsion and 35g of water were added and stirred using a homomixer, the emulsion thickened to the point where it could not be stirred. The thickened emulsion was kneaded for 15 minutes using a homodisper. Next, 521g of water was added and mixed using a homomixer, resulting in a uniform white emulsion. This emulsion was transferred to a 1-liter glass flask equipped with an anchor-type stirring blade stirrer, and the temperature was adjusted to 20-25°C. After that, a mixed solution of 0.6g of an isododecane solution of a platinum-vinyl group-containing disiloxane complex (platinum content 0.5%) and 1g of polyoxyethylene lauryl ether (trade name: Emulgen 109P, manufactured by Kao Corporation) was added under stirring, and the mixture was stirred at the same temperature for 24 hours to obtain an aqueous dispersion of silicone rubber spherical particles.

[0127] The volume average particle size of the silicone rubber spherical particles was measured using a laser diffraction / scattering particle size distribution analyzer LA-960 (manufactured by Horiba, Ltd.) and was found to be 300 nm.

[0128] Separately from the preparation of the aqueous dispersion of silicone rubber spherical particles, vinyl-containing dimethylpolysiloxane (A5) represented by formula (17) below, methylhydrogenpolysiloxane (B2) represented by formula (14) above, and an isododecane solution of platinum-vinyl-containing disiloxane complex (platinum content 0.5%) were mixed in the above-mentioned proportions, poured into an aluminum petri dish to a thickness of 10 mm, left at 25° C. for 6 hours, and then heated in a thermostatic chamber at 50° C. for 1 hour. The resulting cured product was a non-sticky rubber elastic body, and its hardness was measured with a durometer A hardness tester to be 20.

[0129] (A5): Dimethylpolysiloxane containing vinyl groups [ka]

[0130] [Example 6] (Steps (ii) and (iii): Adsorption and adhesion of silicone rubber particles to the surface of cellulose particles (core particles)) In a 1-liter glass flask equipped with an anchor-shaped stirring blade, 75 g (amount of cellulose particles of 17.9 parts by mass per 100 parts by mass of water) of core particles (trade name: CELLULOBEADS D5, manufactured by Daito Kasei Kogyo Co., Ltd., shape = spherical, volume average particle size = 12 μm, electron microscope photograph: FIG. 8) were charged, 2.8 g (amount of lauryl trimethyl ammonium chloride of 0.2 parts by mass per 100 parts by mass of water) of 30% aqueous solution of lauryl trimethyl ammonium chloride (trade name: CATION BB, manufactured by NOF Corp.) and 412.2 g of water were charged. The pH of the liquid at this time was 6.6. Under impeller stirring, 10 g of the aqueous dispersion of silicone rubber spherical particles obtained in Example 1 was added (amount of silicone rubber particles of 5.3 parts by mass per 100 parts by mass of cellulose particles) and stirred for 2 hours. The liquid temperature at this time was 25°C.

[0131] The resulting mixture was filtered using a pressure filter with a filter paper with a retention particle size of 4 μm (product name: quantitative filter paper No. 5B, manufactured by Toyo Roshi Kaisha, Ltd.) to separate the particles. The filtrate was colorless and transparent, and it was determined that the silicone rubber particles had not passed through the filter paper, and it was possible that the silicone rubber particles were adsorbed on the surface of the cellulose particles. The resulting water-containing particles were placed in a stainless steel tray, and the water was volatilized and removed at a temperature of 105°C in a hot air flow dryer. The dried material was crushed using a jet mill to obtain particles.

[0132] When the obtained particles were observed under an electron microscope, it was confirmed that spherical particles with a size of about 300 nm were attached to the entire surface of particles with the same shape and diameter as the cellulose particles, and that they were composite particles made of cellulose particles with silicone rubber attached to the surface. An electron microscope image is shown in Figure 1. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and diameter of the cellulose particles were maintained.

[0133] The volume average particle size of the obtained composite particles was measured using an electrical resistance particle size distribution analyzer (Multisizer 3, Beckman Coulter, Inc.) and found to be 12 μm. The particle size distribution was approximately the same as that of the cellulose particles, and it was determined that the shape and particle size of the cellulose particles were maintained.

[0134] [Examples 7 to 12] (Steps (ii) and (iii): Adsorption and adhesion of silicone rubber particles to the surface of cellulose particles (core particles)) Particles were obtained in the same manner as in Example 6, except that the type of cationic surfactant, the type and amount of the aqueous dispersion of silicone rubber particles, and the amount of water were as shown in Table 1.

[0135] Table 1 shows the results of observing the appearance of the filtrate obtained by filtering the mixture through a filter paper, observing the adhesion of silicone rubber to the surfaces of the cellulose particles (core particles) using an electron microscope, and measuring the volume average particle size.

[0136] The particles obtained in Example 7 were observed under an electron microscope, and it was confirmed that spherical particles of about 300 nm in size and particles of a shape similar to that of cellulose particles fused together were attached to the entire surface of the particles, and that the particles were composite particles formed by attaching silicone rubber to the surface of the cellulose particles. The electron microscope photograph is shown in Figure 2. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and particle size of the cellulose particles were maintained.

[0137] The particles obtained in Example 8 were observed under an electron microscope, and it was confirmed that spherical particles of about 300 nm in size and particles of a shape similar to that of cellulose particles fused together were attached to the entire surface of the particles, and that the particles were composite particles formed by attaching silicone rubber to the surface of the cellulose particles. The electron microscope photograph is shown in Figure 3. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and particle size of the cellulose particles were maintained.

[0138] The particles obtained in Example 9 were observed under an electron microscope to have a nodular coating attached to the entire surface of the particles, which had the same shape and particle size as the cellulose particles, and were confirmed to be composite particles with silicone rubber attached to the surface of the cellulose particles. An electron microscope photograph is shown in Figure 4. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and particle size of the cellulose particles were maintained.

[0139] The particles obtained in Example 10 were observed under an electron microscope to have a nodular coating attached to the entire surface of the particles, which had the same shape and particle size as the cellulose particles, and were confirmed to be composite particles with silicone rubber attached to the surface of the cellulose particles. An electron microscope photograph is shown in Figure 5. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and particle size of the cellulose particles were maintained.

[0140] The particles obtained in Example 11 were observed under an electron microscope, and it was confirmed that spherical particles of about 300 nm in size were sparsely attached to the surface of particles with the same shape and diameter as the cellulose particles, and that the particles were composite particles formed by attaching silicone rubber to the surface of the cellulose particles. An electron microscope photograph is shown in Figure 6. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and diameter of the cellulose particles were maintained.

[0141] When the particles obtained in Example 12 were observed under an electron microscope, sparse nodules were observed on the surface of the particles, which had the same shape and particle size as the cellulose particles, and it was confirmed that the particles were composite particles in which silicone rubber was attached to the surface of the cellulose particles. An electron microscope photograph is shown in Figure 7. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and particle size of the cellulose particles were maintained.

[0142] [Comparative Example 1] (Steps (ii) and (iii): Adsorption and adhesion of silicone rubber particles to the surface of cellulose particles (core particles)) In a 1-liter glass flask equipped with an anchor-shaped impeller stirrer, 75 g of the above-mentioned cellulose particles as core particles (an amount of 17.8 parts by mass of cellulose particles per 100 parts by mass of water) and 415.0 g of water were charged. The pH of the liquid at this time was 6.4. No cationic surfactant was added. With impeller stirring, 10 g of the silicone rubber spherical particle aqueous dispersion obtained in Example 1 was added (an amount of 5.3 parts by mass of silicone rubber particles per 100 parts by mass of cellulose particles), and the mixture was stirred for 2 hours. The liquid temperature at this time was 25°C.

[0143] The resulting mixture was filtered using a pressure filter with filter paper with a particle retention size of 4 μm (product name: Quantitative Filter Paper No. 5B, manufactured by Toyo Roshi Kaisha, Ltd.) to separate the particles. The filtrate was cloudy, indicating that the silicone rubber particles had passed through the filter paper, which means that at least the silicone rubber particles that had permeated the filter paper were not adsorbed onto the surfaces of the cellulose particles.

[0144] The obtained water-containing particles were placed in a stainless steel tray, and the water was removed by volatilization in a hot air flow dryer at a temperature of 105° C. The dried material was crushed in a jet mill to obtain particles.

[0145] When the resulting particles were observed under an electron microscope, no adhesion of silicone rubber to the surface of the cellulose particles was observed.

[0146] [Table 1] (Note 1) Cationic surfactant D-1: 30% aqueous solution of lauryltrimethylammonium chloride (product name: Cation BB, manufactured by NOF Corporation) D-2: 30% cetyltrimethylammonium chloride aqueous solution (product name: Coatamin 60W, manufactured by Kao Corporation) D-3: 25% stearyltrimethylammonium chloride aqueous solution (product name: CATION AB-250AQ, manufactured by NOF Corporation) (Note 2) Nonionic surfactant: Polyoxyethylene lauryl ether contained in the aqueous dispersion of silicone rubber spherical particles

[0147] [Example 13] (Steps (ii) and (iii): Adsorption and adhesion of silicone rubber particles to the surface of silica (core particles)) In a 1-liter glass flask equipped with an anchor-shaped stirring blade, 75 g (amount of silica of 17.8 parts by mass per 100 parts by mass of water) of silica (trade name: SILICA MICRO BEAD P-1500, manufactured by JGC Catalysts and Chemicals Co., Ltd., shape = spherical, volume average particle size = 16 μm, electron microscope photograph: FIG. 11), 2.8 g (amount of lauryl trimethyl ammonium chloride of 0.2 parts by mass per 100 parts by mass of water) of 30% aqueous solution of lauryl trimethyl ammonium chloride (trade name: CATION BB, manufactured by NOF Corp.), and 412.2 g of water were charged. The pH of the liquid at this time was 6.8. While stirring with the blade, 10 g of the aqueous dispersion of silicone rubber particles obtained in Example 2 was added (amount of silicone rubber particles of 5.3 parts by mass per 100 parts by mass of silica), and stirring was performed for 2 hours. The liquid temperature at this time was 25°C.

[0148] The resulting suspension was filtered using a pressure filter with filter paper with a retention particle size of 4 μm (product name: Quantitative Filter Paper No. 5B, manufactured by Toyo Roshi Kaisha, Ltd.) to separate the particles. The filtrate was colorless and transparent, and it was determined that the silicone rubber particles had not passed through the filter paper, suggesting that the silicone rubber particles were possibly adsorbed onto the silica surface.

[0149] The obtained water-containing particles were placed in a stainless steel tray, and the water was removed by volatilization in a hot air flow dryer at a temperature of 105° C. The dried material was crushed in a jet mill to obtain particles.

[0150] When the obtained particles were observed under an electron microscope, it was confirmed that spherical particles with a size of about 300 nm were attached to the entire surface of particles with the same shape and diameter as silica, and that they were composite particles with silicone rubber attached to the silica surface. An electron microscope image is shown in Figure 9. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and diameter of the silica were maintained.

[0151] The volume average particle size of the obtained composite particles was measured using an electrical resistance particle size distribution measuring device (Multisizer 3, manufactured by Beckman Coulter, Inc.) and found to be 16 μm. The particle size distribution was approximately the same as that of silica, and it was determined that the shape and particle size of the silica was maintained.

[0152] [Examples 14 to 20, Comparative Examples 2 to 4] (Steps (ii) and (iii): Adsorption and adhesion of silicone rubber particles to the surface of silica (core particles)) Particles were obtained in the same manner as in Example 13, except that the type of cationic surfactant, the type and amount of the aqueous dispersion of silicone rubber particles, and the amount of water were as shown in Tables 2 and 3.

[0153] Tables 2 and 3 show the results of observing the appearance of the filtrate obtained by filtering the mixture through a filter paper, observing the adhesion of silicone rubber to the surfaces of the silica particles (core particles) using an electron microscope, and measuring the volume average particle size.

[0154] When the particles obtained in Example 18 were observed under an electron microscope, nodules were observed on the entire surface of the particles, which had the same shape and particle size as silica, and it was confirmed that the particles were composite particles with silicone rubber attached to the silica surface. An electron microscope photograph is shown in Figure 10. Furthermore, no adhesion between the composite particles was observed, and it was determined that the shape and particle size of the silica were maintained.

[0155] The particles obtained in Examples 14 to 17, 19, and 20 also had the properties shown in Tables 2 and 3, and were determined to maintain the shape and particle size of the silica, similar to the particles obtained in Example 18.

[0156] When the particles obtained in Comparative Examples 2 to 4 were observed under an electron microscope, no adhesion of silicone rubber to the surfaces of the silica particles was observed.

[0157] [Table 2] (Note 3) Cationic surfactants D-1: 30% aqueous solution of lauryltrimethylammonium chloride (product name: Cation BB, manufactured by NOF Corporation) D-4: 75% dialkyl (C12-C18) dimethyl ammonium chloride in isopropyl alcohol (product name: Coatamin D-2345P, manufactured by Kao Corporation) D-5: 80% trioctylmethylammonium chloride aqueous solution (product name: TOMAC 80% aqueous solution, manufactured by Nippon Specialty Chemical Industry Co., Ltd.) D-6: 20% tri(polyoxyethylene)stearyl ammonium chloride aqueous solution (Catinal SPC-20V-S, Toho Chemical Industry Co., Ltd.) D-7: 50% benzalkonium chloride aqueous solution (Nikkol CA-101, manufactured by Nikko Chemicals Co., Ltd.)

[0158] [Table 3]

[0159] In Examples 6 to 22, the composite particles did not contain multiple core particles, the particles did not strongly aggregate or adhere to each other, the shape and particle size of the core particles were roughly maintained, and composite particles in which almost all of the silicone rubber blended was attached to the surface of almost all of the core particles were produced. On the other hand, in Comparative Examples 1 and 2, since no cationic surfactant was blended in step (ii), no silicone rubber was attached to the surface of the core particles, and the desired composite particles could not be produced. In Comparative Example 3, the amount of cationic surfactant in step (ii) was insufficient, and in Comparative Example 4, the amount of cationic surfactant in (ii) was excessive, so no silicone rubber was attached to the surface of the core particles, and the desired composite particles could not be produced.

[0160] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.

Claims

1. A method for producing composite particles comprising adhering silicone rubber to the surface of core particles having a volume average particle size of 1 to 50 μm, comprising the steps of: (i) emulsifying a curable liquid silicone composition with a surfactant to prepare an oil-in-water emulsion, and then curing the curable liquid silicone composition to prepare an aqueous dispersion of silicone rubber spherical particles having a volume average particle size of 50 to 1,000 nm; (ii) mixing the core particles, the aqueous dispersion of the silicone rubber spherical particles prepared in step (i), a cationic surfactant, and water to adsorb the silicone rubber particles onto the surfaces of the core particles, thereby preparing a mixture containing the core particles having the silicone rubber particles adsorbed thereon; and (iii) a step of removing water contained in the mixture by volatilization from the mixture containing the core particles having the silicone rubber particles adsorbed thereon, prepared in the step (ii), and fixing the silicone rubber particles adsorbed on the surfaces of the core particles. wherein the amount of the core particles is in the range of 1 to 100 parts by mass relative to 100 parts by mass of water contained in the mixed liquid prepared in step (ii), the amount of the silicone rubber spherical particles is in the range of 0.1 to 25 parts by mass relative to 100 parts by mass of the core particles, and the amount of the cationic surfactant is in the range of 0.02 to 0.9 parts by mass relative to 100 parts by mass of water.

2. 2. The method for producing composite particles according to claim 1, wherein the core particles are made of at least one of inorganic particles and organic particles.

3. 3. The method for producing composite particles according to claim 1, wherein the silicone rubber spherical particles have a rubber hardness in the range of 5 to 95 as measured by a Type A durometer specified in JIS K6253.

Citation Information

Patent Citations

  • Composite particle containing polyorganosiloxane and its production

    JP1997208644A

  • Composite particle, method for producing the same and cosmetic product

    JP2011001332A

  • Method for producing composite particle

    JP2013035758A

  • Composite particles, method for preparing the same and cosmetic composition

    US20100330132A1

  • Production of emulsion type silicone composition and silicone fine particle

    JP1991281536A