Method of manufacturing pre-cured tread
By using a precisely sized precure tread vulcanization mold and a polyester film to prevent rubber protrusion and adhesion, the method addresses the issues of material waste and defective products in precure tread manufacturing, achieving cost reduction and improved yield.
Patent Information
- Application Number
- JP2023082349
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing methods for manufacturing precure treads result in excessive extruded rubber, leading to increased material costs and defective products due to bare formation and rubber marks, which deteriorate yield.
A method involving a precure tread vulcanization mold with specific dimensions and a polyester film to prevent excessive rubber protrusion and adhesion during vulcanization, ensuring the green tread fits accurately and the film prevents direct contact with the mold.
Reduces material costs and improves yield by minimizing excessive rubber discard and rubber marks on the precure tread, enhancing the manufacturing process efficiency.
Smart Images

Figure 2024165824000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a precured tread. [Background technology]
[0002] A retread tire is constructed by vulcanizing and bonding a vulcanized precured tread having a tread pattern to a base tire.
[0003] Patent Document 1 discloses embedding canvas in the surface of the green tread that is to be vulcanized and bonded to the base tire, vulcanizing the precured tread, and removing the canvas when attaching the precured tread to the base tire, thereby eliminating the need to buff the precured tread. Patent Document 2 discloses manufacturing a precured tread by stacking an upper layer made of an abrasion-resistant rubber composition and a lower layer made of a rubber composition with good self-adhesiveness. Patent Document 3 discloses forming an engagement-capable cavity in the bottom of the precured tread and attaching a peelable polymer film to the bottom surface including the cavity. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-057871 [Patent Document 2] Japanese Patent Application Publication No. 60-247547 [Patent Document 3] European Patent No. 2199110 Summary of the Invention [Problem to be solved by the invention]
[0005] When the green tread is vulcanized in a precured tread vulcanization mold, in order to prevent bare spots in the vulcanized precured tread, the volume of the green tread may be set to have a larger margin than the volume required to fill the precured tread vulcanization mold.
[0006] As a result, a lot of rubber protrudes from the vulcanized precured tread, and much of the protruding rubber is discarded, which increases material costs. Furthermore, a lot of the protruding rubber may remain in the precured tread vulcanization mold, and in this case, the remaining protruding rubber remains as a rubber defect on the precured tread that is next vulcanized in the same vulcanization mold, making it a defective product and causing a decrease in yield.
[0007] An object of the present invention is to provide a method for producing a precured tread that enables reduction in material costs and improvement in yield while suppressing the occurrence of bare spots. [Means for solving the problem]
[0008] One aspect of the present invention is A method for manufacturing a precured tread to be attached to an outer peripheral surface of a base tire to form a retread tire, comprising: preparing a precured tread vulcanization mold for vulcanizing and molding a precured tread, the precured tread having a mold shoulder width corresponding to a shoulder width of the retread tire and a mold length longer than a circumferential length of the base tire; The green tread is vulcanized and molded using the precured tread vulcanizing mold. Contains The green tread is The green tread width, which is the length corresponding to the tire axial direction of the retread tire, is ±5 mm relative to the mold shoulder width, The green tread length, which is the length corresponding to the tire circumferential direction of the retread tire, is ±25 mm relative to the mold length plus 30 mm, The mass is ±0.4 kg relative to the weight obtained by adding 0.8 kg to the mass of the precured tread, which is the mass excluding the protruding rubber formed when the green tread is vulcanized and molded using the precured tread vulcanization mold. A method for producing a precured tread is provided.
[0009] According to the present invention, since the green tread is an appropriate size for the precured tread vulcanization mold, the occurrence of bare spots in the vulcanized precured tread is suppressed, while the formation of excessive protruding rubber is suppressed. As a result, the amount of protruding rubber that is discarded is reduced, and material costs can be reduced. Furthermore, since the remaining of the protruding rubber in the mold is suppressed, the occurrence of defective products in which the protruding rubber forms rubber defects on the subsequent precured tread is suppressed. Therefore, since an excessively large green tread is not prepared, the material costs required for the production of the precured tread are reduced, and the yield of the precured tread production is improved.
[0010] In addition, during the vulcanization molding, a film that prevents the precured tread from adhering to the precured tread vulcanization mold may be interposed between the back surface of the green tread, which is opposite to the surface that constitutes the ground contact surface after vulcanization molding, and the precured tread vulcanization mold.
[0011] According to this configuration, by performing vulcanization molding through the film, the precured tread formed by vulcanization molding of the green tread is prevented from adhering to the precured tread vulcanization mold. Furthermore, the film also prevents the protruding rubber from adhering to the precured tread vulcanization mold, thereby preventing the occurrence of rubber defects during the subsequent vulcanization molding.
[0012] The film may be a polyester film.
[0013] According to this configuration, the film has resistance to the high temperature and high pressure conditions present during vulcanization molding of the precured tread, and therefore the film can effectively exert the above-mentioned effect of inhibiting adhesion of the precured tread and protruding rubber to the precured tread vulcanization mold.
[0014] The width of the film may be 150% or more and 210% or less of the green tread width.
[0015] According to this configuration, the film is sufficiently wide relative to the green tread, so that the protruding rubber formed by vulcanization is prevented from going around the film from the outside in the width direction and reaching the precured tread vulcanization mold side. This prevents the protruding rubber from adhering to the precured tread vulcanization mold, so that the occurrence of rubber abnormalities is more reliably prevented. Effect of the Invention
[0016] According to the method for producing a precured tread of the present invention, it is possible to reduce material costs and improve yields while suppressing the occurrence of bare spots. [Brief description of the drawings]
[0017] [Figure 1] 1 is a perspective view of a retread tire according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a perspective view of a precured tread used in the retread tire of FIG. 1 . [Diagram 3] FIG. [Figure 4] FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] A method for producing a precured tread according to one embodiment of the present invention will now be described with reference to the accompanying drawings. Note that the following description is merely exemplary in nature and is not intended to limit the present invention, its applications, or its uses.
[0019] Fig. 1 is a perspective view of a retread tire 1 (also called a reclaimed tire) having a precured tread 20 formed by a manufacturing method for a precured tread according to a first embodiment of the present invention. In Fig. 1, the precured tread 20 is shown in a partially broken state. As shown in Fig. 1, the retread tire 1 is a tire for trucks, buses, or light trucks, and is generally formed by vulcanizing and adhering in a vulcanizer the precured tread 20, which has been vulcanized and molded in advance, to the outer circumferential surface 11 of a base tire 10 from which the worn old tread has been removed.
[0020] Fig. 2 is a perspective view of the precured tread 20. As shown in Fig. 2, the precured tread 20 is a strip-shaped member having a pattern formed thereon and a front surface 21 that constitutes the contact surface in the retread tire 1, and a back surface 22 that is located on the opposite side and is attached to the outer circumferential surface 11 of the base tire 10. The precured tread 20 according to this embodiment is a square shoulder in which the front surface 21 and a pair of widthwise side surfaces 23 are connected by corners 24.
[0021] The precured tread 20 has a precured tread width W1, which is the dimension between a pair of corners 4 and the width in the direction corresponding to the tire axial direction, equal to the retread tire width W0 (see FIG. 1), which is the dimension in the tire axial direction at the contact patch of the retread tire 1 (i.e., shoulder width). On the other hand, the precured tread 20 has a precured tread length L1, which is the length corresponding to the tire circumferential direction, longer than the base tire circumference L0 (see FIG. 1), which is the dimension in the tire circumferential direction of the base tire 10. In other words, the precured tread 20 is prepared to be longer than the base tire circumference L0, and is cut to fit the length of the base tire circumference L0 before use.
[0022] Fig. 3 is an exploded perspective view of a precured tread vulcanizing mold 40 for vulcanizing and molding the precured tread 20. Fig. 3 also shows the green tread 30 that is vulcanized and molded in the precured tread vulcanizing mold 40 to become the precured tread 20, and a film 44. As shown in Fig. 3, the precured tread vulcanizing mold 40 has a pattern molding mold 41, a hot plate upper mold 42 located above the pattern molding mold 41, and a hot plate lower mold 43 located below the pattern molding mold 41.
[0023] The pattern molding die 41 has a cavity 41a that opens upward, and a bottom surface 41c of the cavity 41a has bones 41b for transferring a tread pattern to the green tread 30. That is, the green tread 30 is vulcanized in the cavity 41a to form the precured tread 20. In this embodiment, the pattern molding die 41 extends in an elongated shape in a direction corresponding to the tire circumferential direction by combining a plurality of segments 45 in the longitudinal direction.
[0024] The cavity 41a corresponds to the shape of the precured tread 20. That is, the mold length L2, which is the length of the cavity 41a in the direction corresponding to the tire circumferential direction, is equal to the precured tread length L1 (see FIG. 2). Also, the mold shoulder width W2, which is the length of the bottom surface 41c of the cavity 41a in the direction corresponding to the tire axial direction, is equal to the precured tread width W1 (see FIG. 2). In other words, the mold shoulder width W2 corresponds to the length of the ground contact surface of the precured tread 20 to be vulcanized in the tire axial direction, and corresponds to the length of the tire ground contact surface between a pair of corners 24 (see FIG. 2) of the precured tread 20.
[0025] The hot plate upper mold 42 applies heat required for vulcanization from above to the green tread 30 during vulcanization. The hot plate upper mold 42 seals the cavity 41a at the upper opening. The hot plate lower mold 43 applies heat required for vulcanization from below to the green tread 30 through the pattern molding die 41 during vulcanization.
[0026] In this embodiment, a film 44 is interposed between the pattern molding die 41 and the hot plate mold 42. The film 44 is made of a material that can withstand the temperature and pressure during vulcanization, and is made of polyester in this embodiment. The film 44 prevents the green tread 30 from directly contacting the hot plate mold 42 during vulcanization molding, thereby preventing the green tread 30 (or the precured tread 20 after vulcanization) from adhering to the hot plate mold 42.
[0027] The green tread 30 is a strip-shaped unvulcanized rubber member having a predetermined thickness, for example, extruded from a die (not shown). The green tread 30 has a front surface 31 that constitutes the ground contact surface after vulcanization molding, and a back surface 32 that is attached to the base tire 10 after vulcanization molding. The green tread 30 is set in the cavity 41a so that the front surface 31 is located on the lower side and the back surface 32 is located on the upper side.
[0028] The green tread 30 has a green tread width W3, which is the length in the direction corresponding to the tire axial direction, and a green tread length L3, which is the length in the direction corresponding to the tire circumferential direction, which are set based on the size of the cavity 41a of the pattern molding die 41. Specifically, the green tread width W3 is the length on the surface 31, and is set to a length of ±5 mm relative to the die shoulder width W2. The green tread length L3 is set to a length obtained by adding 30 mm to the die length L2 and adding ±25 mm (i.e., adding 5 mm to 55 mm relative to the die length L2).
[0029] Furthermore, the green tread 30 has a green tread width W3 and a green tread length L3 set as described above, and is set so that the mass G2 is ±0.4 kg (i.e., 0.4 kg or more and 1.2 kg or less added to the mass G1) obtained by adding 0.8 kg to the mass G1 of the precured tread 20. This allows the green tread 30 to be set to an appropriate thickness T3 so as to satisfy the size and mass in a plan view.
[0030] The film 44 has a film width W4, which is the length in the direction corresponding to the tire axial direction, and a film length L4, which is the length in the direction corresponding to the tire circumferential direction, which are set based on the size of the green tread 30. Specifically, the film width W4 is set to a length that is 150% or more and 210% or less of the green tread width W3. The film length L4 is set to a length that is 105% or more and 120% or less of the green tread length L4.
[0031] For example, the retread tire 1 according to this embodiment may be for trucks and buses and may have tire sizes of, for example, 245 / 70R19.5, 265 / 70R19.5, 10R22.5, 11R22.5, 235 / 70R22.5, 12R22.5, 275 / 70R22.5, 275 / 80R22.5, and 295 / 80R22.5.
[0032] As an example, the mold shoulder width W2 may be 190 mm or more and 250 mm or less, and the mold length L2 may be 2800 mm or more and 3500 mm or less. The green tread width W3 may be 185 mm or more and 255 mm or less, and the green tread length L3 may be 2805 mm or more and 3555 mm or less. The film width W4 may be 390 mm, and the film length L4 may be 4000 mm. The film 44 is cut to fit the green tread length L4 before use.
[0033] Next, a method for manufacturing the precured tread 20 will be described with reference to Fig. 4. In Fig. 4, the green tread 30, the precured tread 20, and the precured tread vulcanization mold 40 are simply shown in cross section perpendicular to the direction corresponding to the tire circumferential direction.
[0034] 4(a), first, there is prepared a green tread 30. The green tread 30 is a strip-shaped unvulcanized rubber member having a predetermined thickness, which is extruded from, for example, a die (not shown).
[0035] Next, as shown in Fig. 4(b), a precured tread vulcanizing mold 40 is prepared, and the green tread 30 is set in the precured tread vulcanizing mold 40. Specifically, the green tread 30 is set in the pattern molding mold 41 so that the front surface 31 is located on the lower side and the back surface 32 is located on the upper side in the cavity 41a. Furthermore, a film 44 is interposed between the green tread 30 and the hot plate upper mold 42.
[0036] Next, as shown in Fig. 4(c), the hot plate upper die 42 and the hot plate lower die 43 are hydraulically clamped in the vertical direction and then released, and this bumping cycle (30 seconds) is repeated multiple times to align the green tread 30 with the cavity 41a and remove air that may be present between the green tread 30 and the cavity 41a. For example, in this embodiment, the clamping hydraulic pressure is set to 14.7 MPa or more and 16.9 MPa or less so that the surface pressure generated on the green tread 30 by clamping is about 2.94 MPa. In this embodiment, two cycles of bumping are performed.
[0037] 4(d), the green tread 30 is vulcanized for about 25 minutes under conditions of, for example, about 165° C. in a precured tread vulcanizing mold 40. At this time, a part of the rubber of the green tread 30 protrudes to the outside of the cavity 41a through the mating surface of the precured tread vulcanizing mold 40, i.e., between the pattern molding mold 41 and the film 44, and is vulcanized as protruding rubber 25.
[0038] Next, as shown in Fig. 4(e), the hot plate mold 42 is moved upward to open the precured tread vulcanization mold 40, and the precured tread 20 having the protruding rubber 25 is taken out. Here, in the precured tread vulcanization mold 40, a film 44 is interposed between the green tread 30 and the hot plate mold 42. Since the film 44 is sufficiently wide compared to the green tread 30, the protruding rubber 25 does not extend beyond the film 44 from the outside in the width direction to the upper side of the film 44, and is prevented from contacting and adhering to the hot plate mold 42. As a result, the precured tread 20 is taken out with the protruding rubber 25 still connected.
[0039] Finally, as shown in FIG. 4( f ), the protruding rubber 25 is cut off with a cutter 46 to produce the precured tread 20 .
[0040] The method for producing the precured tread 20 according to this embodiment has the following advantages.
[0041] (1) The manufacturing method of Precure Tread 20 is as follows: A method for manufacturing a precured tread 20 to be attached to an outer peripheral surface 11 of a base tire 10 to form a retread tire 1, comprising: preparing a precured tread vulcanization mold 40 for vulcanizing and molding a precured tread 20, the precured tread having a mold shoulder width W2 corresponding to a retread tire width W0 of a retread tire 1 and a mold length L2 longer than a base tire circumference L0 of a base tire 10; The green tread 30 is vulcanized and molded by a precured tread vulcanizing mold 40. Contains Green Tread 30 is The green tread width W3, which is the length corresponding to the tire axial direction of the retread tire 1, is ±5 mm with respect to the mold shoulder width W2, The green tread length L3, which is the length corresponding to the tire circumferential direction of the retread tire 1, is ±25 mm with respect to the length obtained by adding 30 mm to the mold length L2, The mass G3 is ±0.4 kg relative to the weight obtained by adding 0.8 kg to the mass G2 of the precured tread 20, which is the mass excluding the protruding rubber 25 formed when the green tread 30 is vulcanized and molded by the precured tread vulcanizing mold 40.
[0042] As a result, since the green tread 30 is an appropriate size for the precured tread vulcanizing mold 40, the occurrence of bare spots in the vulcanized precured tread 20 is suppressed, while the formation of excessive protruding rubber 25 is suppressed. As a result, the amount of protruding rubber 25 that is discarded is reduced, so that material costs can be reduced. Furthermore, since the remaining of the protruding rubber 25 in the precured tread vulcanizing mold 40 is suppressed, the occurrence of defective products in which the protruding rubber 25 is formed as a rubber defect in the precured tread 20 that is subsequently vulcanized and molded is suppressed. Therefore, since an excessively large green tread 30 is not prepared, material costs are reduced, and the occurrence of defective products caused by the protruding rubber 25 is suppressed, so that the yield is improved.
[0043] (2) In addition, during vulcanization molding, a film is interposed between the back surface 32 of the green tread 30, which is opposite the front surface 31 that constitutes the contact surface after vulcanization molding, and the hot plate mold 42 of the precured tread vulcanization mold 40, to prevent the precured tread 20 from sticking to the hot plate mold 42. As a result, by performing vulcanization molding through the film 44, the precured tread 20 obtained by vulcanization molding is prevented from adhering to the hot plate mold 42 of the precured tread vulcanization mold 40. Furthermore, since the adhesion of the protruding rubber 25 to the hot plate mold 42 is also prevented, the occurrence of rubber abnormalities during the subsequent vulcanization molding is prevented.
[0044] (3) Also, the film 44 is a polyester film. As a result, the film 44 has resistance to the high temperature and high pressure conditions present during vulcanization molding of the precured tread 20, and therefore the film 44 can effectively exert the above-mentioned effect of inhibiting adhesion of the precured tread 20 and the protruding rubber 25 to the precured tread vulcanization mold 40.
[0045] (4) The film width W4 is 150% or more and 210% or less of the green tread width W3. As a result, since the film 44 is sufficiently wide with respect to the green tread 30, the protruding rubber 25 formed by vulcanization is prevented from wrapping around the film 44 from the outside in the width direction and reaching the hot plate upper die 42 side of the precured tread vulcanization mold 40. This prevents the protruding rubber 25 from adhering to the hot plate upper die 42, so that the occurrence of rubber abnormalities is more reliably prevented.
[0046] The method for producing the precured tread according to the present invention is not limited to the configuration of the above embodiment, and various modifications are possible. EXAMPLES
[0047] The size of the green tread 30 (W3, L3, G3), the presence or absence of the film 44, and the number of bumping were varied (Comparative Examples 1 to 6, Examples 1 to 3), under which the green tread 30 was vulcanized in a precured tread vulcanizing mold 40, and the occurrence of defects in the obtained precured tread 20 was evaluated.
[0048] As shown in Table 1, in Comparative Examples 1 to 3, one or more of the above conditions do not satisfy the numerical ranges of the above embodiment.
[0049] Specifically, in Comparative Example 1, the green tread width W3 is −6 mm relative to the mold shoulder width W2, which is below the lower limit of the numerical range of W3, and the green tread length L3 is +5 mm relative to the mold length L2, which is the lower limit of the numerical range of L3. Therefore, the mass G3 of the green tread 30 is +0.3 kg relative to the mass G2 of the precured tread 20, which is below the lower limit of the numerical range of G3.
[0050] In Comparative Example 2, the green tread width W3 is +6 mm relative to the mold shoulder width W2, exceeding the upper limit of the numerical range of W3, and the green tread length L3 is +55 mm relative to the mold length L2, which is the upper limit of the numerical range of L3. Therefore, the mass G3 of the green tread 30 is +1.3 kg relative to the mass G2 of the precured tread 20, exceeding the upper limit of the numerical range of G3.
[0051] In Comparative Example 3, the green tread length L3 is +3 mm with respect to the mold length L2 and is below the lower limit of the numerical range of L3, but the green tread width W3 and mass G3 are within the numerical ranges.
[0052] In Comparative Example 4, the green tread length L3 is +60 mm with respect to the mold length L2, exceeding the upper limit of the numerical range of L3, but the green tread width W3 and mass G3 are within the numerical ranges.
[0053] In both Comparative Examples 5 and 6, the green tread size was within the numerical range, but in Comparative Example 5, vulcanization molding was performed without interposing the film 44, and in Comparative Example 6, only one cycle of bumping was performed. In Comparative Examples 1 to 5, two cycles of bumping were performed. In Comparative Examples 1 to 4 and 6, vulcanization molding was performed with the film 44 interposed.
[0054] As shown in Table 2, Examples 1 to 3 satisfy the numerical range of the above embodiment. All of Examples 1 to 3 were vulcanization molded with the film 44 interposed therebetween, and two cycles of bumping were performed.
[0055] Specifically, in Example 1, the green tread width W3 is -5 mm relative to the mold shoulder width W2, and the green tread length L3 is +5 mm relative to the mold length L2, and are set at the lower limit of the numerical range of W3 and L3. Therefore, the mass G3 of the green tire is +0.4 kg relative to the mass G2 of the precured tread 20, which is the lower limit of the numerical range of G3.
[0056] In Example 2, the green tread width W3 is equal to the mold shoulder width W2, and the green tread length L3 is +30 mm relative to the mold length L2, and is set in the center of the numerical range of W3 and L3. Therefore, the mass G3 of the green tire is +0.8 kg relative to the mass G2 of the precured tread 20, which is in the center of the numerical range of G3.
[0057] In Example 3, the green tread width W3 is +5 mm relative to the mold shoulder width W2, and the green tread length L3 is +55 mm relative to the mold length L2, and are set at the upper limit of the numerical range of W3 and L3. Therefore, the mass G3 of the green tire is +1.2 kg relative to the mass G2 of the precured tread 20, which is in the middle of the numerical range of G3.
[0058] [Table 1]
[0059] [Table 2]
[0060] As shown in Table 1, at least one of the green tread width W3, green tread length L3, and mass G3 is below the lower limit of the respective numerical range, and thus the rubber volume is insufficient in Comparative Examples 1 and 3, resulting in bare spots.Also, at least one of the green tread width W3, green tread length L3, and mass G3 is above the upper limit of the respective numerical range, and thus the rubber volume is excessive in Comparative Examples 2 and 4, and thus a large amount of protruding rubber is formed, resulting in the occurrence of rubber marks caused by the protruding rubber.
[0061] In addition, in Comparative Example 5, in which vulcanization molding was performed without the interposition of a film, the green tread 30 or the vulcanization molded precured tread 20 tended to stick to the hot plate mold 42, resulting in the occurrence of rubber abnormalities in the precured tread subsequently vulcanized and molded using the same precured tread vulcanization mold 40.
[0062] As shown in Table 2, in Examples 1 to 3, the green tread width W3, green tread length L3, and mass G3 were all within their respective numerical ranges, so the volume of the green tread 30 was appropriate and no bare spots or rubber marks occurred. [Explanation of symbols]
[0063] 1 Retread tires 10 Tires 11 Outer surface 20 Precure Tread 25 Rubber band 30 Green Tread 40 Precure tread vulcanization mold 41 Pattern forming mold 41a Cavity 42 Hot plate top mold 43 Hot plate lower mold 44 Film W2 Mold shoulder width W3 Green tread width W4 Film width L2 mold length L3 Green tread length G1 Precure Tread's mass G2 Green Tread Mass
Claims
1. A method for manufacturing a precured tread to be attached to an outer peripheral surface of a base tire to form a retread tire, comprising: preparing a precured tread vulcanization mold for vulcanizing and molding a precured tread, the precured tread having a mold shoulder width corresponding to a shoulder width of the retread tire and a mold length longer than a circumferential length of the base tire; The green tread is vulcanized and molded using the precured tread vulcanizing mold. Contains The green tread is The green tread width, which is the length corresponding to the tire axial direction of the retread tire, is ±5 mm with respect to the mold shoulder width, A green tread length, which is a length corresponding to a tire circumferential direction of the retread tire, is ±25 mm relative to the mold length plus 30 mm, The mass is ±0.4 kg relative to the weight obtained by adding 0.8 kg to the mass of the precured tread, which is the mass excluding the protruding rubber formed when the green tread is vulcanized and molded in the precured tread vulcanization mold. A method for producing precure tread.
2. In the vulcanization molding, a film is interposed between a back surface of the green tread, which is opposite to a surface that constitutes a ground contact surface after vulcanization molding, and the precured tread vulcanization mold, to prevent the precured tread from sticking to the precured tread vulcanization mold. A method for producing the precured tread according to claim 1.
3. The film is a polyester film. A method for producing the precured tread according to claim 2.
4. The width of the film is 150% or more and 210% or less of the green tread width. A method for producing the precured tread according to claim 2 or 3.
Citation Information
Patent Citations
Retreaded tire and methods of preparation
EP2199110A2
Manufacture of precured tread for renewed tire
JP1985247547A
Manufacture of precured tread for retreated tire and manufacture of retreated tire using the same
JP1997057871A