Toner

The toner with specific resin particles addresses the durability and cleaning performance issues in high-speed printing by forming a protective layer that stabilizes the blocking layer, preventing charging roller contamination and image defects in varying environments.

JP2024165834APending Publication Date: 2024-11-28CANON KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023082367
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing toners with PET structures and black pigments face challenges in maintaining cleaning performance and durability in high-speed printing, particularly in low-temperature, low-humidity environments, leading to charging roller contamination and image defects.

Method used

A toner formulation with specific resin particles having a repeating structure, a brightness value of 90 to 120, an average equivalent circle diameter of 0.5 to 3.0 μm, and a content of 5 to 40 particles per 100 toner particles, which forms a protective layer to prevent toner slipping through the cleaning blade and maintains a stable blocking layer.

Benefits of technology

The toner effectively prevents charging roller contamination and image defects by maintaining a stable blocking layer, ensuring consistent image quality and durability even in challenging environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165834000001
    Figure 2024165834000001
  • Figure 2024165834000002
    Figure 2024165834000002
  • Figure 2024165834000003
    Figure 2024165834000003
Patent Text Reader

Abstract

To provide a toner that contains resin having a PET structure and a black pigment, and that, even if a large amount of printing is performed for a long period, can prevent dirt on a charging roller due to poor cleaning and an image defect resulting therefrom, in a low temperature and low humidity environment and a normal temperature and normal humidity environment, and exhibits good image density.SOLUTION: A toner includes toner particles containing a pigment, resin particles, and an external additive. The resin particles have a specific luminance average value and average equivalent circle diameter. The luminance average value of the toner particles is within a specific range. The pigment is a black pigment. The content of the resin particles is within a specific range. The toner particles and the resin particles each have a PET structure on its surface. In a load displacement curve obtained by micro compression measurement of the resin particles, 90 number% or more of the resin particles do not have a breaking point within a load range of 0-10 mN.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to toners for use in imaging processes such as electrophotography. [Background technology]

[0002] In recent years, the speed of copiers and printers has increased and their environmental stability has been improved, and there is a demand for toners that provide stable image quality even during high-speed printing and when the usage environment changes, such as low temperature and low humidity, or high temperature and high humidity. Furthermore, apart from the performance of printers, social awareness of the preservation of the global environment is increasing, and it is necessary to consider using environmentally friendly materials for printer materials such as toner. Polyethylene terephthalate (PET) is a plastic material that is widely used in the world, and PET is one of the plastic materials that can reduce waste plastic because there are established methods for recycling it after use and recycled materials can be used as raw materials.

[0003] In the electrophotographic method, a latent image carrier is first charged by various means and exposed to light to form an electrostatic latent image on the surface of the latent image carrier. The electrostatic latent image is then developed with toner to form a toner image, which is then transferred to a transfer material such as paper, and the toner image is fixed on the transfer material by applying heat and pressure to obtain a copy or print. In such an image forming process, the toner remaining on the surface of the latent image carrier after the toner image is transferred must be removed (cleaned) by some method.

[0004] As a method for cleaning the toner remaining on the latent image carrier, a method in which the edge of a cleaning blade made of an elastic material such as urethane rubber is brought into contact with the surface of the latent image carrier is widely used. Increasing the contact pressure of the cleaning blade improves the cleaning performance, but it also increases the likelihood of chipping of the blade, wear of the latent image carrier, and abnormal noise due to chatter vibration of the blade. Increasing the process speed to increase the printing speed increases the likelihood of the above-mentioned problems. In other words, it tends to be difficult to achieve both cleaning performance and durability of the components in high-speed copying machines and printers. Furthermore, when PET is used as a constituent material of the toner binder, it has a higher glass transition temperature Tg and is harder than commonly used toner binder materials. Therefore, it is more durable for embedding external additives, but a clear interface is likely to form between the binder and the internal additive material of the toner, especially the black pigment carbon black, which is the starting point for cracking and chipping of the toner. Toner with cracks and chips is more likely to be supplied to the cleaning unit, which has a significant negative impact on the cleaning member.

[0005] This phenomenon is particularly noticeable in high-speed copying machines and printers, and therefore a toner with further improved cleaning properties is required. To address the above-mentioned problems, for example, Patent Document 1 proposes a toner containing both positively charged lubricant particles and negatively charged lubricant particles. It is disclosed that the positively charged lubricant particles and the negatively charged lubricant particles are placed on the latent image portion and the non-latent image portion of the surface of the latent image carrier, respectively, and therefore exhibit good cleaning properties regardless of the image coverage. Patent Document 2 discloses that by incorporating at least two types of strontium titanate microparticles having different particle sizes as an external additive, a blocking layer is formed in the cleaning portion, thereby improving the cleaning properties of the toner. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2017-219823 A [Patent Document 2] JP 2019-184795 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, even when such measures are used, there is still room for improvement in the durability and stability of the cleaning portion of a toner containing a resin having a PET structure and a black pigment in high-speed copying machines and printers.

[0008] The present disclosure aims to provide a toner that solves the above problems. Specifically, the present disclosure is directed to a toner that contains a resin having a PET structure and a black pigment, which can suppress charging roller contamination due to poor cleaning and the resulting image defects in a low-temperature, low-humidity environment and in a normal-temperature, normal-humidity environment, even when performing a large amount of printing over a long period of time, and further shows good image density. [Means for solving the problem]

[0009] The present disclosure relates to a toner including toner particles containing a pigment, resin particles, and an external additive, the resin particles have an average brightness of 90 to 120 based on monochrome 256 gradations, and an average equivalent circular diameter of 0.5 to 3.0 μm; the toner particles have an average brightness of 40 to 80 based on monochrome 256 gradations; the pigment is a black pigment, the content of the resin particles in the toner is 5 to 40 per 100 toner particles, The toner particles have a resin having a repeating structure represented by the following formula (1) on the surface thereof, The resin particles have a resin having a repeating structure represented by the following formula (1) on the surface thereof, In the load-displacement curve obtained by microcompression measurement of the resin particles, The toner is such that 90% or more by number of the resin particles do not have a breaking point within a load range of 0 to 10 mN. [ka] Effect of the Invention

[0010] According to the present disclosure, a toner containing a resin having a PET structure and a black pigment can be provided that can suppress charging roller contamination due to poor cleaning and resulting image defects in both low temperature and low humidity environments and normal temperature and normal humidity environments, even when performing large volume printing over a long period of time, and that also exhibits good image density. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present disclosure will be described in more detail below with reference to embodiments thereof, but is not limited thereto. In addition, the description of "XX or more and YY or less" or "XX to YY" representing a numerical range means a numerical range including a lower limit and an upper limit as endpoints, unless otherwise specified. When a numerical range is described in stages, the upper limit and the lower limit of each numerical range can be arbitrarily combined.

[0012] The present disclosure relates to a toner including toner particles containing a pigment, resin particles, and an external additive, the resin particles have an average brightness of 90 to 120 based on monochrome 256 gradations, and an average equivalent circular diameter of 0.5 to 3.0 μm; the toner particles have an average brightness of 40 to 80 based on monochrome 256 gradations; the pigment is a black pigment, the content of the resin particles in the toner is 5 to 40 per 100 toner particles, The toner particles have a resin having a repeating structure represented by the following formula (1) on the surface thereof, The resin particles have a resin having a repeating structure represented by the following formula (1) on the surface thereof, In the load-displacement curve obtained by microcompression measurement of the resin particles, The toner is such that 90% or more by number of the resin particles do not have a breaking point within a load range of 0 to 10 mN. [ka]

[0013] In the present disclosure, the toner particles have a resin having a repeating structure of the structure shown in formula (1) on the surface. Furthermore, the toner has an average brightness of 90 to 120 and an average equivalent circle diameter of 0.5 to 3.0 μm, and contains resin particles having the repeating structure of the structure shown in formula (1). With such a toner, a toner having excellent durability even in a high-speed process and good cleaning properties over a long period of printing can be obtained. The present inventors consider the mechanism by which such effects are obtained to be as follows.

[0014] In order to prevent toner and external additives from slipping through the cleaning blade, it is effective to maintain the deposition layer of the external additives (hereinafter also referred to as a blocking layer) formed at the contact area between the latent image carrier surface and the cleaning blade (hereinafter also referred to as the cleaning blade nip area) without collapsing.

[0015] The main component of the material that forms the blocking layer is an external additive supplied from the toner. A stable blocking layer is maintained by the constant supply of external additive from the toner during printing. However, if the blocking layer collapses or a gap appears due to some factor, the supplied external additive and toner will slip through the cleaning blade nip and adhere to the charging roller (hereinafter also referred to as the C roller). When the deposits accumulate on the C roller and the electrical resistance of the surface changes, the transfer of charge to the latent image carrier will not be performed normally, resulting in image defects such as streaks and unevenness.

[0016] Toners that contain PET resin as a binder resin are highly resistant to surface deterioration and are highly resistant to changes in surface properties caused by continuous printing. However, as mentioned above, PET tends to harden, and clear interfaces tend to form between the pigments dispersed inside, especially carbon black, and the PET, and when force is applied during printing, the toner particles can crack starting from the interface. The cracked toner particles become irregularly shaped particles with their interiors exposed. Such particles have strong adhesion to the latent image carrier, so after development, they penetrate into the cleaning blade nip without being transferred. Irregular particles that strongly adhere to the latent image carrier cannot be easily collected, and they attack the blocking layer in the cleaning blade nip. This causes the blocking layer to not be stably maintained, causing gaps and crumbling, allowing toner and external additives to slip through. As a result, the material that has slipped through accumulates on the C roller, causing image defects such as streaks and unevenness. It is believed that this will occur.

[0017] The present inventors have found that the above-mentioned problems can be suppressed by using toner particles having a resin having a repeating structure represented by formula (1), and resin particles having a repeating structure represented by formula (1) and an average brightness value of 90 to 120 based on monochrome 256 gradations and an average equivalent circle diameter of 0.5 to 3.0 μm.

[0018] The resin particles have a repeating structure of the structure shown in formula (1), and the toner particles also have a repeating structure of the structure shown in formula (1). In other words, the resin particles have a similar composition to the toner particle surface, so the charging characteristics are equivalent to those of the toner particles. Therefore, when the toner is developed, the resin particles are also developed on the latent image carrier in the same manner. However, since the developed resin particles have a small particle size, they have a high adhesion to the latent image carrier and are not transferred, remaining, and are efficiently supplied to the cleaning blade nip. The resin particles supplied to the cleaning blade nip have a smaller particle size than the toner.

[0019] In general, the van der Waals force and electrostatic adhesion force become stronger as the particle size becomes smaller. Therefore, the adhesion force between the resin particles and the latent image carrier becomes stronger, so that the resin particles are sent out before the toner particles, and are positioned in front of the blocking layer, where they remain. The resin particles that remain in front of the blocking layer become a protective layer, and it is believed that the broken toner particles that are involved in the destruction of the blocking layer are prevented from penetrating into the blocking layer in front of the layer, thereby maintaining a stable blocking layer and good cleaning properties. As a result, it is believed that the occurrence of image defects such as streaks and uneven density can be suppressed.

[0020] The brightness, circle equivalent diameter, and resin particle content of the toner are values ​​obtained by measuring under the analysis conditions described below using a flow type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation), and are indices that represent the degree of light scattering of the toner. In general, the brightness of a toner decreases when it contains a colorant.

[0021] The average brightness value of the toner particles based on monochrome 256 gradations is 40 to 80, which means that the black pigment is sufficiently present in the toner particles. The average brightness value of the toner particles is preferably 40 to 75, and more preferably 50 to 70. In contrast, the average brightness value of the resin particles based on monochrome 256 gradations is 90 to 120. An average brightness value of 90 or more means that the amount of black pigment present in the resin particles is small. The average brightness value of the resin particles is preferably 95 to 120, and more preferably 100 to 115. The average brightness value can be controlled by the amount of pigment, etc.

[0022] If the resin particles remain in front of the blocking layer for a long time, the force applied to each resin particle accumulates, making the resin particles more likely to break. However, since the resin particles are nearly transparent with an average brightness value in the range of 90 to 120, there are almost no other components dispersed inside, and there are almost no interfaces inside the particles. Therefore, the resin particles are not easily broken, and in the load-displacement curve obtained by the measurement and analysis described below, 90% or more of the resin particles do not have a breaking point in the load range of 0 to 10 mN.

[0023] Here, the break point of the toner particles or resin particles is defined as follows: Here, the toner particles or resin particles are simply referred to as particles. Breaking point: Among the maximum points in the load-displacement curve in the microcompression measurement of a particle, the point at which the load amount at that maximum point is the smallest is defined as the breaking point. Maximum point: In the load-displacement curve of the displacement amount D and the load P, the point where the particle begins to deform (the first point of the first group of measurement points in the group of measurement points where the displacement increases monotonically continuously over a displacement of at least 0.3 μm) is taken as the starting point. Then, at the measurement points after the starting point, The point where the ratio of the change in load P to the load (dP / dD) is 0 is defined as point A. If dP / dD is positive over a displacement of at least 0.1 μm up until just before point A, and dP / dD is negative over a displacement of at least 0.1 μm from just after point A, then point A is defined as the maximum point.

[0024] In order to make the proportion of resin particles that do not have a breaking point within a load range of 0 to 10 mN 90% by number or more, for example, a method of reducing the amount of components other than the resin inside the resin particles, such as by satisfying the above-mentioned brightness range, can be mentioned. In addition, it can also be controlled by the resin composition, that is, the monomer composition, and it can be easily achieved by incorporating the structure represented by formula (1) into the resin composition.

[0025] The fact that the resin particles are less likely to break prevents the resin particles themselves from becoming irregularly shaped particles that attack the blocking layer, and makes it easier for them to become a protective layer that protects the blocking layer. By making the average equivalent circle diameter of the resin particles 3.0 μm or less, the protective layer is formed on the blocking layer side of the toner particles, improving the maintenance of the blocking layer and cleaning performance. In addition, by making the average equivalent circle diameter of the resin particles 0.5 μm or more, it is possible to prevent the resin particles from penetrating and integrating with the blocking layer. The average equivalent circle diameter of the resin particles is preferably 0.8 to 2.2 μm, and more preferably 1.0 to 2.0 μm.

[0026] The content of the resin particles in the toner is 5 to 40 per 100 toner particles. By having the content of the resin particles be 5 or more, a protective layer that prevents the intrusion of irregularly shaped particles can be formed in front of the blocking layer in the cleaning nip, and it is believed that good cleaning performance can be maintained. As a result, it is believed that the occurrence of image defects such as streaks and uneven density can be suppressed. On the other hand, by having the content of the resin particles be 40% by number or less, it is possible to prevent a decrease in image density. The content of the resin particles in the toner is preferably 7 to 30 particles, and more preferably 12 to 18 particles, per 100 toner particles.

[0027] The toner particles have a resin having a repeating structure of the structure represented by the following formula (1) on the surface. The resin particles have a resin having a repeating structure of the structure represented by the following formula (1) on the surface. The repeating structure of the structure represented by formula (1) is, for example, a polyethylene terephthalate structure (PET structure). That is, it is preferable that the toner particles and the resin particles contain a resin having a PET structure on the surface. The structure represented by formula (1) is formed, for example, by condensation of ethylene glycol and terephthalic acid. [ka]

[0028] An example of the toner particles and resin particles having a resin having a repeating structure of the structure represented by formula (1) on the surface thereof is a toner particle or resin particle having a polyester resin, which is a condensation polymer of a monomer mixture containing ethylene glycol and terephthalic acid, on the surface thereof. More specifically, the toner particles and resin particles preferably contain a polyester resin having a PET structure consisting of ethylene glycol and terephthalic acid. For the PET-containing polyester resin, ethylene glycol and terephthalic acid may be used as monomers during resin synthesis, or recycled PET oligomers produced by recycling may be used.

[0029] In the monomer mixture, it is preferable to use, as a monomer other than ethylene glycol and terephthalic acid, for example, the following carboxylic acid components and alcohol components. Examples of the carboxylic acid component include terephthalic acid, isophthalic acid, phthalic acid, fumaric acid, maleic acid, cyclohexanedicarboxylic acid, and trimellitic acid. Examples of the alcohol component include bisphenol A, hydrogenated bisphenol, an ethylene oxide adduct of bisphenol A, a propylene oxide adduct of bisphenol A, glycerin, trimethylolpropane, and pentaerythritol.

[0030] Among these, preferred acid monomer components include terephthalic acid, isophthalic acid, succinic acid, adipic acid, fumaric acid, trimellitic acid, etc. More preferred are terephthalic acid, isophthalic acid, and trimellitic acid. Among these, preferred alcohol components include ethylene oxide adducts of bisphenol A (e.g., 1-5 mol adducts), propylene oxide adducts of bisphenol A (e.g., 1-5 mol adducts), etc.

[0031] The content of ethylene glycol in the monomer mixture is preferably 3 to 30 mass%, more preferably 5 to 20 mass%. The content of terephthalic acid in the monomer mixture is preferably 20 to 45 mass%, more preferably 20 to 30 mass%. The content of an alkylene oxide adduct of bisphenol A (e.g., propylene oxide or 1 to 5 mol ethylene oxide adduct) in the monomer mixture is preferably 30 to 65 mass%, more preferably 40 to 60 mass%. Of the resin components contained in the toner particles and resin particles, the content of the polyester resin is preferably 50 to 100% by mass, more preferably 80 to 100% by mass, and further preferably 90 to 100% by mass.

[0032] The resin particles have a m / z 341 normalized intensity of 2.50×10 calculated by the following formula (A) in time-of-flight secondary ion mass spectrometry under the following condition (2). -4 ~1.00×10 -2 It is preferable that: m / z 341 normalized intensity = (ion intensity of the peak detected at m / z = 341) / (total ion intensity from m / z = 0.5 to 1850) (A)

[0033] In addition, the resin particles have a m / z 341 normalized intensity of 2.50×10 calculated by formula (A) in time-of-flight secondary ion mass spectrometry under the following condition (3): -4 ~1.00×10 -2 It is preferable that:

[0034] Condition (2): Primary ion species: Bi 3++ ,Accelerating voltage: 30kV, Measurement mode: Positive, Negative, Measurement range: m / z=0.5~1850, Raster size: 300×300μm / 256×256pixel, Measurement time: 180 seconds Condition (3): After performing sputtering with Ar-GCIB under the following conditions, measurement is performed under the above condition (2). Ar-GCIB conditions Acceleration voltage: 5 kV Current: 6.5nA Raster size: 600 x 600 μm Irradiation time: 5sec / cycle Sputtering time: 500 seconds

[0035] In the analysis using a time-of-flight secondary ion mass spectrometer, the peak detected at m / z=341 under condition (2) was composed of three monomers: terephthalic acid, ethylene glycol, and terephthalic acid. The detection of this peak indicates that the resin contains a PET resin structure, and the normalized intensity of m / z341 is 2.50 × 10 -4 ~1.00×10 -2By so doing, the charging characteristics due to the inclusion of the PET resin become more stable, and the charging characteristics tend to be similar to those of the toner particles. The normalized intensity at m / z 341 under condition (2) is preferably 0.0015 to 0.0035, and more preferably 0.0020 to 0.0030. The normalized intensity of m / z 341 under condition (2) can be increased by increasing the contents of terephthalic acid and ethylene glycol in the resin composition, and can be decreased by decreasing the contents of terephthalic acid and ethylene glycol in the resin composition.

[0036] Furthermore, analysis under condition (3) confirmed that the PET resin structure was present not only on the surface but also inside. The normalized intensity of m / z 341 under condition (3) was 2.50×10 -4 ~1.00×10 -2 By setting the above range, the blocking layer can be protected from cracking in the cleaning nip area with sufficient hardness and can be highly durable. The m / z 341 normalized intensity under the condition (3) is preferably 0.0010 to 0.0030, and more preferably 0.0015 to 0.0025.

[0037] The m / z 341 normalized intensity under condition (3) can be increased by using the same resin from the surface to the interior, and can be decreased by using a gradient structure or a core-shell structure in which a resin with a lower polarity than the PET-containing resin on the surface is placed inside.

[0038] When particles contained in the toner having a circular equivalent diameter of 0.5 to 3.0 μm are considered as microparticles, the content of resin particles in the microparticles is preferably 60 to 100% by number, and more preferably 65 to 80% by number.

[0039] The fine particles include toner particles having a small particle size in addition to the resin particles having the above-mentioned specific average brightness value. Such fine toner particles may contain a pigment. Resin fine particles such as toner particles containing a pigment tend to break at the interface with the pigment. Resin fine particles containing a pigment are also located in the same place as resin particles in the cleaning nip due to their high adhesive force derived from their particle size, but they tend to break easily, so that irregularly shaped fine particles may be generated. If the resin particles are 60% or more by number, the resin particles that break in the cleaning nip can be suppressed, and cleaning performance can be maintained better.

[0040] The toner preferably contains 10 to 40% by number, and more preferably 10 to 20% by number, of microparticles out of the total of toner particles and resin particles (including the above-mentioned microparticles). When the content is 10% by number or more, a sufficient amount of resin particles that protect the blocking layer in the cleaning nip can be contained, whereas when the content is 40% by number or less, a decrease in image density can be more easily suppressed. The amount of the fine particles described above can be controlled by setting conditions in the toner classification process and the amount of resin particles added in the external addition process.

[0041] The toner particles may contain a binder resin. The binder resin preferably contains a polyester resin, and more preferably contains a polyester resin having a PET structure as a resin having a repeating structure represented by the following formula (1) described above. The resin particles preferably contain a polyester resin. Resins used for the binder resin and resin particles are not particularly limited other than polyester resin, and the following known resins can be used in combination.

[0042] Specifically, styrene-based copolymers such as polystyrene, styrene-propylene copolymer, styrene-vinyltoluene copolymer, styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-butyl acrylate copolymer, styrene-octyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, styrene-butyl methacrylate copolymer, styrene-octyl methacrylate copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-maleic acid copolymer, and styrene-maleic acid ester copolymer, polyacrylic acid ester, polymethacrylic acid ester, and polyvinyl acetate can be used, and a plurality of these can be used in combination.

[0043] The binder resin contains a polyester resin, and preferably contains 3 to 30% by mass (more preferably 5 to 20% by mass) of a structure corresponding to ethylene glycol and 20 to 45% by mass (more preferably 20 to 30% by mass) of a structure corresponding to terephthalic acid as components constituting the polyester resin. By containing 3% by mass or more of ethylene glycol and 20% by mass or more of terephthalic acid, it is possible to maintain a charge more stably, and toner particle deformation and surface deterioration due to continuous printing can be further suppressed. In addition, by containing 30% by mass or less of ethylene glycol and 45% by mass or less of terephthalic acid, it is possible to suppress the influence of humidity and maintain environmental stability at a higher level.

[0044] In addition, in a load-displacement curve obtained by microcompression measurement of toner particles, it is preferable that 80% or more of the toner particles have a breaking point in the load range of 0 mN to 10 mN. When the toner particles have the above-mentioned PET structure, the breaking point is likely to occur. Therefore, it is considered that the fact that 80% or more of the toner particles have a breaking point indicates that the majority of the toner particles have a PET structure. Therefore, the charging characteristics become more uniform and the electrophotographic characteristics become more stable.

[0045] There is no particular restriction on the means for making the resin particles exist in the toner. For example, when toner particles are produced by a pulverization method, a suspension polymerization method, or an emulsion aggregation method, the resin particles can be made to exist in the toner by mixing the resin particles with the toner particles prior to the external addition step.

[0046] In the suspension polymerization method, it is possible to form resin particles by generating small particles that do not contain pigments, for example by increasing the rotation speed during suspension, while in the emulsion aggregation method, it is possible to form resin particles by generating small particles that do not contain pigments, for example by using a resin with a high acid value during aggregation. In addition, for toner particles produced by any of the methods, after the toner particles are produced and dried, the toner particles and resin particles may be mixed using the same device as in the external addition, so that the resin particles are present in the toner. During the external addition, the toner particles, resin particles, and external additive may be mixed.

[0047] It is preferable that the toner contains compound A and compound B which are eluted in methanol when the toner is subjected to an elution treatment under the elution condition A described below. Dissolution condition A: At 25° C., 10 times the mass of the toner is used in methanol (JIS K8891 equivalent), and the toner is stirred for 10 hours at a rotor speed of 200 rpm using a stirring device.

[0048] In addition, when the supernatant obtained by centrifuging the eluate in which Compound A and Compound B were eluted in methanol under the following centrifugation condition A was analyzed by liquid chromatography ESI / MS under the following analysis condition A, The compound A contained in the supernatant is ionized as a cation and detected, The compound B contained in the supernatant is preferably detected as an anion. Centrifugation condition A: Rotation is performed for 30 minutes at 25° C., a rotation radius of 10.1 cm, and a rotation speed of 3,500 rpm. Analysis condition A: Sheath Gas: 10 (arb. unit.), Aux Gas: 5 (arb. unit.), spray voltage: 5 kV, capillary temperature: 275°C. Ionized substances are detected as cations under the conditions of capillary voltage: 35 V, tube lens voltage: 110 V, and ionized substances are detected as anions under the conditions of capillary voltage: -35 V, tube lens voltage: -110 V.

[0049] Compound A and compound B, which can be extracted into methanol and ionized, are highly polar components that exist near the surface and play a role in supporting the charging properties of the toner. The fact that compound A was detected on the cation side and compound B on the anion side in ESI / MS analysis indicates that some compounds have a tendency to have positive charging properties and others have a tendency to have negative charging properties.

[0050] By containing compound A and compound B in the toner, both positive and negative components are present, which means that the negative components tend to cause negative charging, and the positive components tend to cause leakage. The structure shown in formula (1) has high polarity and is easily charged. The presence of compound A and compound B, which play a role in supporting the charging characteristics, near the surface stabilizes the retention of negative charge, and prevents overcharging of the toner due to leakage from the positive components. By preventing the toner from being overcharged, the adhesive force can be reduced, so that the amount of residual toner supplied to the cleaning nip can be reduced, and the cleaning performance can be maintained more satisfactorily.

[0051] In order to incorporate Compound A into the toner, it is preferable to use a material that does not bond to the binder resin of the toner and exists independently, such as a surfactant having a repeating structure of ethylene oxide.

[0052] Preferably, compound A includes at least one compound selected from the group consisting of polyoxyethylene lauryl ether, polyoxyethylene hexadecyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene dodecyl ether, polyoxyethylene sorbitan monooleate ether, polyoxyethylene styryl phenyl ether, polyoxyethylene (2) lauryl ether sodium sulfate, polyoxyethylene lauryl ether sodium acetate, and the like.

[0053] Compound A is preferably at least one compound selected from the group consisting of an ethylene oxide adduct of a linear aliphatic alcohol having 8 to 16 carbon atoms (more preferably 10 to 14) and sodium polyoxyethylene lauryl ether acetate, and is more preferably an ethylene oxide adduct of lauryl alcohol.

[0054] There is no particular limitation on the method of addition, but for example, when a toner is produced by an emulsion aggregation method, Compound A may be added in any step of preparing a colorant dispersion, a release agent dispersion, a resin particle dispersion, or the like, or in a step of washing the toner. Compound A is preferably added when preparing each dispersion, such as a colorant dispersion, a release agent dispersion, or a resin particle dispersion. Compound A is also preferably added to a mixture when preparing these aggregated particles (i.e., in a dispersion step).

[0055] In order to incorporate compound B into the toner, it is preferable to use a material that does not bond with the binder resin of the toner and exists independently. For example, an anionic surfactant can be preferably used. Compound B is preferably an aliphatic soap such as sodium stearate or sodium laurate, sodium lauryl sulfate, or (linear or branched) dodecylbenzene. The compound B is preferably at least one compound selected from the group consisting of sodium sulfonate, sodium polyoxyethylene (2) lauryl ether sulfate, etc. Compound B is preferably linear or branched sodium dodecylbenzenesulfonate.

[0056] There is no particular limitation on the method of addition, but for example, when a toner is manufactured by an emulsion aggregation method, the above-mentioned compound may be added in any step of preparing a colorant dispersion, a release agent dispersion, a resin particle dispersion, or the like, or in a step of washing the toner. It is preferable to add compound B when preparing each dispersion, such as a colorant dispersion, a release agent dispersion, or a resin particle dispersion. It is also preferable to add compound B to the mixture when preparing these aggregated particles (i.e., in the dispersion step).

[0057] The method for producing the toner is not particularly limited, and any method such as a suspension polymerization method, a solution suspension method, an emulsion aggregation method, or a pulverization method may be used. In particular, a production method using an emulsion aggregation method is preferably used. That is, it is preferable that the toner particles are emulsion aggregation toner particles. This is preferable from the viewpoint of ease of production, including the fact that a surfactant is generally used in the process of forming the toner.

[0058] As mentioned above, in the production of toner by emulsion aggregation, the components to be contained can be mixed as emulsion particles and aggregated to produce a toner, so it is easy to introduce the necessary components and to design and manufacture a highly functional toner. However, since the emulsion particles are aggregated to form particles, the shape of the original emulsion particles may remain on the surface or inside. In such cases, the toner particles are prone to cracking starting from these cracks, so the cleaning performance improvement according to the present disclosure is more likely to be effective.

[0059] Each component constituting the toner and the method for producing the toner will be described in more detail. <Binding resin> The toner particles may have a binder resin. Examples of the binder resin include polyester resin, vinyl resin, and other binder resins such as the following resins or polymers: styrene acrylic resin, polyester resin, epoxy resin, polyurethane resin, polyamide resin, cellulose resin, polyether resin, mixed resins or composite resins thereof. The binder resin is preferably a polyester resin, a styrene-acrylic resin or a hybrid resin thereof, and more preferably a polyester resin, because it is inexpensive, easily available and has excellent low-temperature fixing properties.

[0060] The polyester resin can be obtained by selecting and combining suitable compounds from polyvalent carboxylic acids, polyols, hydroxycarboxylic acids, etc., and synthesizing them using a conventionally known method such as an ester exchange method or a polycondensation method. For example, the following polycarboxylic acids and polyols may be used in the above-mentioned monomer mixture.

[0061] Polycarboxylic acids are compounds containing two or more carboxy groups in one molecule. Among them, dicarboxylic acids are compounds containing two carboxy groups in one molecule and are preferably used.

[0062] Examples of dicarboxylic acids include oxalic acid, succinic acid, glutaric acid, maleic acid, adipic acid, β-methyladipic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, fumaric acid, citraconic acid, diglycolic acid, cyclohexane-3,5-diene-1,2-carboxylic acid, hexahydroterephthalic acid, malonic acid, pimelic acid, suberic acid, phthalic acid, isophthalic acid, and terephthalic acid. Examples of the carboxylic acid include tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-carboxyphenylacetic acid, p-phenylene diacetic acid, m-phenylene diacetic acid, o-phenylene diacetic acid, diphenylacetic acid, diphenyl-p,p'-dicarboxylic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-1,5-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, anthracene dicarboxylic acid, and cyclohexane dicarboxylic acid.

[0063] Examples of polyvalent carboxylic acids other than dicarboxylic acids include trimellitic acid, trimesic acid, pyromellitic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, pyrene tricarboxylic acid, pyrene tetracarboxylic acid, itaconic acid, glutaconic acid, n-dodecyl succinic acid, n-dodecenyl succinic acid, isododecyl succinic acid, isododecenyl succinic acid, n-octyl succinic acid, n-octenyl succinic acid, etc. These may be used alone or in combination of two or more.

[0064] A polyol is a compound containing two or more hydroxyl groups in one molecule. Among them, a diol is a compound containing two hydroxyl groups in one molecule, and is preferably used. Specifically, ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,14-eicosanediol, didecanediol, tetra ... Examples of suitable bisphenols include propylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,4-butenediol, neopentyl glycol, 1,4-cyclohexanediol, polytetramethylene glycol, hydrogenated bisphenol A, bisphenol A, bisphenol F, bisphenol S, and alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts of the above bisphenols.

[0065] Of these, preferred are terephthalic acid, isophthalic acid, trimellitic acid, an ethylene oxide adduct of bisphenol A (for example, a 1-5 mol adduct), and a propylene oxide adduct of bisphenol A (for example, a 1-5 mol adduct).

[0066] Examples of trivalent or higher polyols include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, hexamethylolmelamine, hexaethylolmelamine, tetramethylolbenzoguanamine, tetraethylolbenzoguanamine, sorbitol, trisphenol PA, phenol novolac, cresol novolac, and alkylene oxide adducts of the above trivalent or higher polyphenols. These may be used alone or in combination of two or more. The polyester resin may be a polyester resin containing a urea group. It is preferable that the carboxyl group of the polyester resin, such as the terminal, is not capped.

[0067] Examples of the styrene-acrylic resin include homopolymers made of the following polymerizable monomers, copolymers obtained by combining two or more of these, and mixtures thereof. Styrenic monomers such as styrene, α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, p-methoxystyrene and p-phenylstyrene; Methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate (Meth)acrylic monomers such as acrylate, iso-propyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-amyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, dimethyl phosphate ethyl (meth)acrylate, diethyl phosphate ethyl (meth)acrylate, dibutyl phosphate ethyl (meth)acrylate and 2-benzoyloxyethyl (meth)acrylate, (meth)acrylonitrile, 2-hydroxyethyl (meth)acrylate, (meth)acrylic acid, maleic acid; Vinyl ether monomers such as vinyl methyl ether and vinyl isobutyl ether; vinyl ketone monomers such as vinyl methyl ketone, vinyl ethyl ketone and vinyl isopropenyl ketone; Polyolefins such as ethylene, propylene, and butadiene.

[0068] The styrene acrylic resin may use a polyfunctional polymerizable monomer as required. Examples of the polyfunctional polymerizable monomer include diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 2,2'-bis(4-((meth)acryloxydiethoxy)phenyl)propane, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, divinylbenzene, divinylnaphthalene, and divinyl ether. In order to control the degree of polymerization, it is also possible to further add a known chain transfer agent and polymerization inhibitor.

[0069] Examples of the polymerization initiator for obtaining the styrene-acrylic resin include organic peroxide-based initiators and azo-based polymerization initiators. Examples of the organic peroxide initiator include benzoyl peroxide, lauroyl peroxide, di-α-cumyl peroxide, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, bis(4-t-butylcyclohexyl)peroxydicarbonate, 1,1-bis(t-butylperoxy)cyclododecane, t-butylperoxymaleic acid, bis(t-butylperoxy)isophthalate, methyl ethyl ketone peroxide, tert-butylperoxy-2-ethylhexanoate, diisopropyl peroxycarbonate, cumene hydroperoxide, 2,4-dichlorobenzoyl peroxide, and tert-butylperoxypivalate.

[0070] Examples of the azo polymerization initiator include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, azobismethylbutyronitrile, and 2,2'-azobis-(methyl isobutyrate).

[0071] Furthermore, a redox initiator, which is a combination of an oxidizing substance and a reducing substance, can also be used as the polymerization initiator. Oxidizing substances include inorganic peroxides such as hydrogen peroxide, persulfates (sodium, potassium and ammonium salts) and oxidizing metal salts such as tetravalent cerium salts. Reducing substances include reducing metal salts (divalent iron salts, monovalent copper salts, and trivalent chromium salts), Examples of reducing sulfur compounds include ammonia, lower amines (amines having from 1 to 6 carbon atoms, such as methylamine and ethylamine), amino compounds such as hydroxylamine, sodium thiosulfate, sodium hydrosulfite, sodium hydrogensulfite, sodium sulfite, and sodium formaldehyde sulfoxylate, lower alcohols (having from 1 to 6 carbon atoms), ascorbic acid or a salt thereof, and lower aldehydes (having from 1 to 6 carbon atoms).

[0072] The polymerization initiator is selected with reference to its 10-hour half-life temperature and is used alone or in combination. The amount of polymerization initiator added varies depending on the desired degree of polymerization, but is generally 0.5 to 20.0 parts by mass per 100.0 parts by mass of polymerizable monomer.

[0073] The binder resin may contain a crystalline polyester, for example, a condensation polymer of an aliphatic diol and an aliphatic dicarboxylic acid. It is preferably a condensation polymer of an aliphatic diol having from 2 to 12 carbon atoms and an aliphatic dicarboxylic acid having from 2 to 12 carbon atoms. Examples of the aliphatic diol having from 2 to 12 carbon atoms include the following compounds: 1,2-ethanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, etc.

[0074] Aliphatic diols having a double bond can also be used, such as the following compounds: 2-butene-1,4-diol, 3-hexene-1,6-diol, and 4-octene-1,8-diol.

[0075] Examples of aliphatic dicarboxylic acids having 2 to 12 carbon atoms include the following compounds: oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, lower alkyl esters and acid anhydrides of these aliphatic dicarboxylic acids.

[0076] Among these, sebacic acid, adipic acid, 1,10-decanedicarboxylic acid, and lower alkyl esters and acid anhydrides thereof are preferred. These may be used alone or in combination of two or more.

[0077] Aromatic dicarboxylic acids can also be used. Examples of aromatic dicarboxylic acids include the following compounds: terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, and 4,4'-biphenyldicarboxylic acid. Among these, terephthalic acid is preferred because of its ease of availability and the ease of forming a polymer with a low melting point.

[0078] A dicarboxylic acid having a double bond can also be used. The dicarboxylic acid having a double bond can be preferably used to suppress hot offset during fixing, since the double bond can be utilized to crosslink the entire resin. Such dicarboxylic acids include fumaric acid, maleic acid, 3-hexenedioic acid, and 3-octenedioic acid. In addition, lower alkyl esters and acid anhydrides thereof are also included. Among these, fumaric acid and maleic acid are more preferred.

[0079] The method for producing the crystalline polyester is not particularly limited, and the crystalline polyester can be produced by a general polyester polymerization method in which a dicarboxylic acid component and a diol component are reacted. For example, the crystalline polyester can be produced by a direct polycondensation method or an ester exchange method, which are selected depending on the type of monomer.

[0080] The content of the crystalline polyester is preferably 1.0 parts by mass or more and 30.0 parts by mass or less, and more preferably 3.0 parts by mass or more and 25.0 parts by mass or less, relative to 100 parts by mass of the binder resin.

[0081] The peak temperature of the maximum endothermic peak of the crystalline polyester measured using a differential scanning calorimeter (DSC) is preferably 50.0° C. or more and 100.0° C. or less, and from the viewpoint of low-temperature fixability, more preferably 60.0° C. or more and 90.0° C. or less.

[0082] The molecular weight of the binder resin is preferably such that the peak molecular weight Mp is 5000 or more and 100000 or less, and more preferably such that the peak molecular weight Mp is 10000 or more and 40000 or less. The glass transition temperature Tg of the binder resin is preferably 40° C. or more and 70° C. or less.

[0083] <Crosslinking agent> In order to control the molecular weight of the binder resin constituting the toner particles, a crosslinking agent may be added during polymerization of the polymerizable monomer. For example, ethylene glycol dimethacrylate, ethylene glycol diacrylate, diethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol dimethacrylate, triethylene glycol diacrylate, neopentyl glycol dimethacrylate, neopentyl glycol diacrylate, divinylbenzene, bis(4-acryloxypolyethoxyphenyl)propane, ethylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butanediol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol #200, #400, #600 diacrylates, dipropylene glycol diacrylate, polypropylene glycol diacrylate, polyester type diacrylate (MANDA Nippon Kayaku), and the above acrylates are methacrylated. Something that has been converted into a relate. The amount of the crosslinking agent added is preferably 0.001 parts by mass or more and 15,000 parts by mass or less based on 100 parts by mass of the polymerizable monomer.

[0084] <Release agent> The toner may contain a known wax as a releasing agent. Specific examples include petroleum waxes such as paraffin wax, microcrystalline wax, and petrolatum and their derivatives, montan wax and its derivatives, hydrocarbon waxes produced by the Fischer-Tropsch process and their derivatives, polyolefin waxes such as polyethylene and polypropylene and their derivatives, and natural waxes such as carnauba wax and candelilla wax and their derivatives. Derivatives also include oxides, block copolymers with vinyl monomers, and graft modified products. Other examples include alcohols such as higher aliphatic alcohols, fatty acids such as stearic acid and palmitic acid or their acid amides, esters and ketones, hydrogenated castor oil and its derivatives, vegetable waxes and animal waxes. These can be used alone or in combination.

[0085] Among these, polyolefin, Fischer-Tropsch hydrocarbon wax, or petroleum wax is preferably used since it tends to improve the developing property and transfer property. Note that these waxes may contain an antioxidant within a range that does not affect the properties of the toner. In addition, from the viewpoint of phase separation with respect to the binder resin or crystallization temperature, preferred examples include higher fatty acid esters such as behenyl behenate and dibehenyl sebacate. Ester wax can also be suitably used as a plasticizer.

[0086] The content of the release agent is preferably 1.0 part by mass or more and 30.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin. The melting point of the release agent is preferably from 30° C. to 120° C., more preferably from 60° C. to 100° C. By using a release agent having a melting point of from 30° C. to 120° C., the release effect is efficiently exerted and a wider fixing area is secured.

[0087] <Plasticizer> In order to improve the sharp melting property of the toner, it is preferable to use a crystalline plasticizer. The plasticizer is not particularly limited, and any of the known plasticizers used in toners such as those described below can be used. Esters of monohydric alcohols and fatty carboxylic acids, such as behenyl behenate, stearyl stearate, and palmityl palmitate, or esters of monohydric carboxylic acids and fatty alcohols; esters of dihydric alcohols and fatty carboxylic acids, such as ethylene glycol distearate, dibehenyl sebacate, and hexanediol dibehenate, or esters of dihydric carboxylic acids and fatty alcohols; esters of trihydric alcohols and fatty carboxylic acids, such as glycerol tribehenate, or esters of trihydric carboxylic acids and fatty alcohols; pentaerythritol tetrastearate esters of tetrahydric alcohols and aliphatic carboxylic acids, such as pentaerythritol tetrapalmitate, or esters of tetrahydric carboxylic acids and aliphatic alcohols; esters of hexahydric alcohols and aliphatic carboxylic acids, such as dipentaerythritol hexastearate, dipentaerythritol hexapalmitate, or esters of hexahydric carboxylic acids and aliphatic alcohols; esters of polyhydric alcohols and aliphatic carboxylic acids, such as polyglycerin behenate, or esters of polyhydric carboxylic acids and aliphatic alcohols; and natural ester waxes, such as carnauba wax and rice wax. These may be used alone or in combination.

[0088] <Coloring agent> The toner particles have a pigment as a colorant. The pigment contains a black pigment. Carbon black is typically used as the black pigment. The black pigment preferably contains carbon black. As described above, by using a black pigment such as carbon black, a clear interface is likely to be formed between the carbon black and the resin, which is likely to cause cracking and chipping of the toner. In the present disclosure, even when such a toner is used, good cleaning performance can be maintained. The pigment is preferably used in an amount of 1.0 part by mass or more and 20.0 parts by mass or less, and more preferably 2.0 parts by mass or more and 10.0 parts by mass or less, relative to 100.0 parts by mass of the binder resin.

[0089] <Charge control agents and charge control resins> The toner particles may contain a charge control agent or a charge control resin. Any known charge control agent can be used as the charge control agent, and a charge control agent that has a high triboelectric charging speed and can stably maintain a constant triboelectric charge amount is particularly preferred. Furthermore, when the toner particles are produced by a suspension polymerization method, a charge control agent that has low polymerization inhibition and is substantially free of solubilized matter in an aqueous medium is particularly preferred.

[0090] Examples of toners that control the toner to be negatively charged include monoazo metal compounds, acetylacetone metal compounds, aromatic oxycarboxylic acids, aromatic dicarboxylic acids, oxycarboxylic and dicarboxylic acid-based metal compounds, aromatic oxycarboxylic acids, aromatic mono- and polycarboxylic acids and their metal salts, anhydrides, esters, phenol derivatives such as bisphenol, urea derivatives, metal-containing salicylic acid-based compounds, metal-containing naphthoic acid-based compounds, boron compounds, quaternary ammonium salts, calixarenes, and charge control resins.

[0091] The charge control resin may be a polymer or copolymer having a sulfonic acid group, a sulfonate group, or a sulfonate ester group. As the polymer having a sulfonic acid group, a sulfonate group, or a sulfonate ester group, a polymer containing a sulfonic acid group-containing acrylamide monomer or a sulfonate group-containing methacrylamide monomer in a copolymerization ratio of 2% by mass or more is preferable, and a polymer containing a sulfonic acid group-containing methacrylamide monomer in a copolymerization ratio of 5% by mass or more is more preferable.

[0092] The charge control resin preferably has a glass transition temperature (Tg) of 35° C. or more and 90° C. or less, a peak molecular weight (Mp) of 10,000 or more and 30,000 or less, and a weight average molecular weight (Mw) of 25,000 or more and 50,000 or less. When used, it is possible to impart preferable triboelectric charging characteristics without affecting the thermal characteristics required for the toner particles. Furthermore, when the charge control resin contains a sulfonic acid group, for example, the dispersibility of the charge control resin itself in the polymerizable monomer composition and the dispersibility of the colorant are improved, and the coloring power, transparency, and triboelectric charging characteristics can be further improved. These charge control agents or charge control resins may be added alone or in combination of two or more kinds. The amount of the charge control agent or charge control resin added is preferably 0.01 parts by mass or more and 20.0 parts by mass or less, and more preferably 0.5 parts by mass or more and 10.0 parts by mass or less, relative to 100.0 parts by mass of the binder resin.

[0093] <Method of manufacturing toner particles> The toner particles preferably have a core particle containing a binder resin and a shell on the surface of the core particle. The method for producing the toner particles is not particularly limited and may be a known method, such as a kneading and grinding method or a wet production method. From the viewpoints of uniform particle size, shape controllability, and ease of obtaining toner particles with a core-shell structure, the wet production method is preferred. Examples of the wet production method include a suspension polymerization method, a dissolution suspension method, an emulsion polymerization aggregation method, and an emulsion aggregation method, and the emulsion aggregation method is more preferred from the viewpoint of ease of controlling the shape of the toner particles.

[0094] In the emulsion aggregation method, first, a dispersion of each material such as binder resin particles and colorant is prepared. The obtained dispersion of each material is dispersed and mixed by adding a dispersion stabilizer as necessary. Then, an aggregating agent is added to aggregate the particles to the desired toner particle size, and then or simultaneously with the aggregation, the resin particles are fused together. If necessary, the shape is controlled by heat to form toner particles.

[0095] Here, the binder resin particles can be composite particles formed of a plurality of layers, each of which is made of two or more layers of resins with different compositions. For example, they can be manufactured by emulsion polymerization, mini-emulsion polymerization, phase inversion emulsification, or a combination of several manufacturing methods. When an internal additive is contained in the toner particles, the resin particles may contain the internal additive, or a dispersion of internal additive particles consisting of only the internal additive may be separately prepared, and the internal additive particles may be aggregated together with the resin particles when the internal additive particles are aggregated. In addition, resin particles with different compositions can be added at different times during aggregation and aggregated to produce toner particles with different layer configurations. After the resin particles containing the binder resin are aggregated to form a core portion, the resin particles containing the shell resin can be added at different times and aggregated to form a shell portion.

[0096] The toner particles may have a shell. The resin for the shell may be the same as or different from the binder resin. The amount of the resin for the shell (shell content) is preferably 1.0 to 10.0 parts by mass, more preferably 2.0 to 7.0 parts by mass, relative to 100 parts by mass of the binder resin contained in the core particles. For example, a polyester resin having a repeating structure of formula (1) may be used as the resin for the shell. When the shell has a repeating structure of formula (1), It is preferable to use a polyester resin having a repeat structure.

[0097] In this case, the method for producing the toner preferably includes the following steps. (1) a dispersion and mixing step of preparing a binder resin microparticle dispersion liquid containing a binder resin and a colorant microparticle dispersion liquid containing a pigment, and mixing them to obtain a mixed dispersion liquid; (2) an aggregation step of aggregating the binder resin fine particles and the colorant fine particles contained in the obtained mixed dispersion to form aggregates; (3) a shell formation step of further adding resin fine particles containing a resin for a shell to the dispersion containing the aggregates to aggregate them and form aggregates having a shell; and (4) A fusion step of heating the aggregates to fuse them together The resulting fused particles can be cooled to obtain toner particles.

[0098] In addition, during the step (4) or after the steps (1) to (4), the following step (5) is carried out: (5) A spheronization step in which the agglomerates are heated at a higher temperature. It is preferred that the compound has the formula:

[0099] After the step (5), the following steps (6) and (7) may be included. (6) An annealing step of heating and holding the fused particles at a temperature equal to or higher than the crystallization temperature or glass transition temperature of the binder resin. (7) A step of cooling the fused particles at a cooling rate of 0.1° C. / sec or more to obtain toner particles.

[0100] The following can be used as the dispersion stabilizer. As the surfactant, a known cationic surfactant, anionic surfactant, or nonionic surfactant can be used. Examples of inorganic dispersion stabilizers include tricalcium phosphate, magnesium phosphate, zinc phosphate, aluminum phosphate, calcium carbonate, magnesium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, bentonite, silica, and alumina. Examples of the organic dispersion stabilizer include polyvinyl alcohol, gelatin, methyl cellulose, methylhydroxypropyl cellulose, ethyl cellulose, sodium salt of carboxymethyl cellulose, and starch.

[0101] As the flocculant, in addition to a surfactant having a polarity opposite to that of the surfactant used in the dispersion stabilizer described above, an inorganic salt or a divalent or higher inorganic metal salt can be suitably used. In particular, an inorganic metal salt is preferred because it is easy to control the flocculation property and the toner charge property by ionizing a polyvalent metal element in an aqueous medium. Specific examples of preferred inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, iron chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyiron chloride, polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. Among these, aluminum salts and their polymers are particularly preferred. In general, in order to obtain a sharper particle size distribution, the valence of the inorganic metal salt is preferably divalent rather than monovalent, and more preferably trivalent or more than divalent, and even if the valence is the same, inorganic metal salt polymers are more suitable. From the viewpoint of high definition and high resolution of images, the weight average particle size (D4) of the toner particles is preferably 3.0 μm or more and 10.0 μm or less, more preferably 5.0 μm or more and 8.0 μm or less, and even more preferably 6.0 μm or more and 7.0 μm or less.

[0102] (Method of producing resin particles) The resin particles are preferably produced by the emulsion aggregation method, similar to the toner particles. Resin particles can be obtained by aggregating a binder resin particle dispersion liquid containing a polyester resin and, if necessary, a colorant particle dispersion liquid. The aggregation time can be controlled so as to obtain the above-mentioned average equivalent circle diameter by the same means as in the production of toner particles.

[0103] <Toner manufacturing method> If necessary, external additives such as various organic or inorganic fine particles may be added to the toner particles. Other external additives include, for example, inorganic oxide fine particles such as silica fine particles, alumina fine particles, and titanium oxide fine particles, inorganic stearic acid compound fine particles such as aluminum stearate fine particles and zinc stearate fine particles, and inorganic titanic acid compound fine particles such as strontium titanate and zinc titanate. These can be used alone or in combination of two or more. The external additive preferably contains silica fine particles. These inorganic particles are preferably gloss-treated with a silane coupling agent, a titanium coupling agent, a higher fatty acid, a silicone oil, etc., to improve heat resistance and storage stability and environmental stability. The BET specific surface area of ​​the external additive is 10 m 2 / g or more 450m 2 It is preferable that the molecular weight is not more than 1 / g.

[0104] The BET specific surface area can be determined by a low-temperature gas adsorption method using a dynamic constant pressure method in accordance with the BET method (preferably the BET multipoint method). For example, a specific surface area measuring device (product name: Gemini 2375 Ver. 5.0, manufactured by Shimadzu Corporation) is used to adsorb nitrogen gas onto the surface of a sample, and the BET multipoint method is used to measure the BET specific surface area (m 2 / g) can be calculated.

[0105] The total content of these various external additives is preferably 0.05 parts by mass or more and 5 parts by mass or less, more preferably 0.1 parts by mass or more and 3 parts by mass or less, and even more preferably 1.0 parts by mass or more and 2.0 parts by mass or less, relative to 100 parts by mass of the toner particles. Also, various external additives may be used in combination.

[0106] The mixer for adding the external additive to the toner particles is not particularly limited, and any known mixer can be used, regardless of whether it is a dry or wet type. Examples include FM Mixer (manufactured by Nippon Coke & Engineering Co., Ltd.), Super Mixer (manufactured by Kawata Corporation), Nobilta (manufactured by Hosokawa Micron Corporation), and Hybridizer (manufactured by Nara Machinery Co., Ltd.). In order to control the coating state of the external additive, the toner can be prepared by adjusting the rotation speed, processing time, and water temperature and amount of water in the jacket of the external addition device.

[0107] In addition, sieving devices used to sift out coarse particles after external addition include Ultrasonic (manufactured by Koei Sangyo Co., Ltd.); Resonaseave, Gyroshifter (Tokuju Kogyo Co., Ltd.); Vibrasonic System (manufactured by Dalton Co., Ltd.); Soniclean (manufactured by Shinto Kogyo Co., Ltd.); Turbo Screener (manufactured by Turbo Kogyo Co., Ltd.); Microshifter (manufactured by Makino Sangyo Co., Ltd.), etc.

[0108] The methods for measuring the physical properties of the toner and each material will be described below. <Measurement of average brightness and average equivalent circle diameter of toner particles and resin particles> The average brightness value and average circle equivalent diameter of the toner particles and resin particles are measured using a flow type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation) under the measurement and analysis conditions during the calibration work. The brightness is based on monochrome 256 gradations (0 to 255) (brightness 0: dark, brightness 255: light). The specific measurement method is as follows. First, 20 mL of ion-exchanged water from which solid impurities have been removed is placed in a glass container. 0.2 mL of a solution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made from nonionic surfactants, anionic surfactants, and organic builders, manufactured by Wako Pure Chemical Industries) diluted 3 times by mass with ion-exchanged water is added as a dispersant. Add 0.02 g of the measurement sample, disperse it for 2 minutes using an ultrasonic disperser, and prepare a dispersion for measurement. At this time, cool the dispersion appropriately so that the temperature is 10°C or higher and 40°C or lower. As the ultrasonic disperser, use a tabletop ultrasonic cleaner disperser "VS-150" (manufactured by Vervoclear) with an oscillation frequency of 50 kHz and an electrical output of 150 W. Put a specified amount of ion-exchanged water in the water tank, and add 2 mL of the above-mentioned Contaminon N to this water tank.

[0109] For the measurement, the flow type particle image analyzer equipped with "LUCPLFLN" (magnification 20x, numerical aperture 0.40) is used as the objective lens, and particle sheath "PSE-900A" (manufactured by Sysmex Corporation) is used as the sheath liquid. The dispersion liquid prepared according to the above procedure is introduced into the flow type particle image analyzer, and 2000 toner particles and resin particles are measured in HPF measurement mode and total count mode. From the results, the average brightness value and average circle equivalent diameter of the toner particles and resin particles are calculated.

[0110] When toner particles or resin particles are available as the measurement sample, they can be measured separately. When toner is used as the measurement sample, measurements can be made as follows. The average brightness of toner particles can be obtained by setting the range of equivalent circle diameters in analysis mode to the range of equivalent circle diameters of toner particles (for example, 4.0 μm to 10.0 μm). The average brightness of resin particles can be obtained by setting the range of equivalent circle diameters in analysis mode to the range of equivalent circle diameters of resin particles (for example, 0.5 μm to 3.0 μm). The average equivalent circular diameter of the toner particles can be obtained by setting the range of the average brightness in the analysis mode to the range of the brightness of the toner particles (for example, 40 to 80). The average equivalent circular diameter of the resin particles can be obtained by setting the range of the average brightness in the analysis mode to the range of the brightness of the resin particles (for example, 90 to 120). The range of the equivalent circular diameter and the range of brightness of the toner particles and the range of the equivalent circular diameter and the range of brightness of the resin particles can be understood, for example, from the particle size distribution and brightness of the toner particles and the resin particles measured from the toner.

[0111] Before starting the measurement, standard latex particles (e.g., Duke Science Automatic focus adjustment is performed using "RESEARCH AND TEST PARTICLES Latex Microsphere Suspensions 5200A" manufactured by tific (diluted with ion-exchanged water). After that, it is preferable to perform focus adjustment every 2 hours from the start of measurement. In the examples of the present application, a flow-type particle image analyzer that has been calibrated by Sysmex Corporation and has a calibration certificate issued by Sysmex Corporation was used.

[0112] <Measurement of resin particle content per 100 toner particles> The content of resin particles in a toner based on the number of particles per 100 toner particles can be measured by the following method. In measuring the average equivalent circle diameter of resin particles using toner as the measurement sample, a frequency table is displayed, and the count number A of particles included in the range of equivalent circle diameters of resin particles (e.g., 0.5 μm to 3.0 μm) and the range of brightness of resin particles (e.g., 90 to 120) is measured. Furthermore, the count number B of all particles is measured, and BA is defined as the count number of toner particles. The content of resin particles can be calculated from the obtained count number A of resin particles and count number BA of toner particles.

[0113] <Measurement of the content of resin particles in microparticles> The content (percentage by number) of resin particles in the fine particles in the toner is measured as follows. In the measurement of the toner by the flow type particle image analyzer, in the same manner as in the measurement of the average brightness and the average equivalent circle diameter, the brightness is set to the range of brightness of the resin particles (for example, 90 to 120) in the analysis of the measurement results, and a frequency table is displayed. Then, when the equivalent circle diameter is 0. The number of counted particles having a size of 5 μm or more and 3.0 μm or less is defined as the "number of counted resin particles among fine particles." On the other hand, the count number of particles having a circle equivalent diameter of 0.5 μm to 3.0 μm is defined as the “microparticle count number.” The content ratio of resin particles in the microparticles can be calculated from the obtained “microparticle count number” and the “resin particle count number in the microparticles.”

[0114] <Measurement of the content of fine particles in the total of toner particles and resin particles> The content ratio (number %) of microparticles in the total of toner particles and resin particles is measured as follows: The content can be measured from the above-mentioned resin particle count number A, toner particle count number BA, and "microparticle count number."

[0115] <Micro-compression measurement of toner particles and resin particles> The breaking points of the toner particles and resin particles in the load range of 0 to 10 mN can be confirmed from the load displacement curve obtained by microcompression measurement. Specifically, a microparticle crushing force measuring device "NS-A100" (manufactured by Nano Seeds Co., Ltd.) is used. The specific method for measuring the load displacement curve is as follows. The measurement environment is maintained at 25.0°C by the attached temperature control device. After applying toner to the sample stage, the temperature is set as mentioned above and maintained for 10 minutes or more before measurement.

[0116] The measurement is performed using a flat indenter with a force of 0.014 mN / μm that is attached to the device. The indenter pressure is set to 30 μm, and the indenter movement speed is set to 0.2 μm / s. Setting this test load makes it possible to measure up to the region where the particles undergo plastic deformation, and makes it possible to measure under conditions close to the stress experienced during the developing and fixing processes. The number of indentation data is set to 3001. As particles to be measured, toner particles or resin particles present alone on the measurement screen of the microscope attached to the device are selected, and measurements are carried out on 100 random particles. The percentage of particles with a breaking point is calculated from the measurements of the 100 particles.

[0117] During the measurement, toner particles and resin particles in the toner can be distinguished from each other based on the appearance of a microscope image: transparent particles are resin particles, and black particles are toner particles.

[0118] The analysis is performed using the "A100 strain analysis graph creation tool" that comes with the "NS-A100" microparticle crushing force measuring device. The presence or absence of a breaking point in the load range of 0 to 10 mN can be confirmed from the obtained load-displacement curve. The breaking point is defined as follows:

[0119] Break point definition: Among the maximum points in the load displacement curve in the microcompression measurement of toner particles or resin particles, the point at which the load amount at the maximum point is the smallest is defined as the breaking point.

[0120] Definition of local maximum: In the load-displacement curve of the displacement amount D and the load P, the point where the toner particle or resin particle starts to deform (the first point in the first group of measurement points where the displacement increases continuously and monotonically over a displacement of at least 0.3 μm) is defined as the starting point. Then, among the measurement points after the starting point, the point where the ratio of the change in the load P to the displacement amount D (dP / dD) is 0 is defined as point A. If dP / dD is positive over a displacement of at least 0.1 μm until just before point A, and dP / dD is negative over a displacement of at least 0.1 μm from just after point A, then point A is defined as the maximum point.

[0121] <Analysis of the structure of resin contained in toner particles and resin particles using a time-of-flight secondary ion mass spectrometer> The structure of the resin constituting the surface of the toner particles and the resin particles is analyzed and the normalized intensity is calculated by a time-of-flight secondary ion mass spectrometer (TOF-SIMS). The equipment and measurement conditions used are shown below. The measurement is carried out on a mixture of toner particles and resin particles from which external additives such as silica have been removed by the following method. (Removal of external additives) Add 160 g of sucrose (Kishida Chemical) to 100 mL of ion-exchanged water and dissolve in a hot water bath to prepare a concentrated sucrose solution. Place 31 g of the concentrated sucrose solution and 6 mL of Contaminon N (a 10% by weight aqueous solution of a neutral detergent for cleaning precision measuring instruments, pH 7, consisting of a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) in a centrifuge tube to prepare a dispersion. Add 1 g of toner to this dispersion and break up the toner clumps with a spatula or the like. The centrifuge tube is shaken for 30 minutes in a shaker (Iwaki Sangyo Co., Ltd., "KM Shaker") at 350 reciprocations per minute. After shaking, the solution is transferred to a glass tube for a swing rotor (50 mL) and centrifuged at 58.33 S in a centrifuge (H-9R; Kokusan Co., Ltd.). -1 After centrifugation, the toner particles and resin particles are present in the top layer in the glass tube, and external additives such as silica are present in the aqueous solution side in the bottom layer. The toner particles and resin particles in the top layer are collected and filtered, and washed with 2 L of ion-exchanged water heated to 40° C., and the washed toner particles and resin particles are taken out.

[0122] Using toner particles and resin particles from which external additives have been removed, measurements are carried out under the following conditions. Measurement device: nanoTOF II (product name, manufactured by ULVAC-PHI, Inc.) Primary ion species: Bi 3++ Acceleration voltage: 30kV Primary ion current: 0.05pA Repetition rate: 8.2kHz Raster mode: Unbunch Raster size: 300μm×300μm Measurement range: m / z=0.5~1850 Measurement mode: Positive, Negative Neutralization gun: Used Measurement time: 180 seconds Sample preparation: Toner particles or resin particles are fixed on an indium sheet. Sample pretreatment: None Using ULVAC-PHI's standard software (TOF-DR), the image is checked to confirm the peaks in the range of m / z=0.5-1850 at the points corresponding to the resin particles and the points corresponding to the toner particles. The peak at m / z193 is due to the ethylene glycol-terephthalic acid dimer structure, and the peak at m / z341 is due to the terephthalic acid-ethylene glycol-terephthalic acid trimer structure, and these peaks indicate that the resin contains a PET structure containing the repeating structure of formula (1) as a component. In addition, the m / z 341 normalized intensity of the resin particles can be calculated by dividing the intensity of the target ion peak by the total ion intensity from m / z 0.5 to 1850 (the above formula (A)). The arithmetic average value of 10 points corresponding to the resin particles and 10 points corresponding to the toner particles is used. By checking the peaks at m / z=193 and m / z=341 in this measurement, it is possible to determine whether the toner particles or resin particles being measured have a resin having a repeating structure represented by formula (1) on their surface. Furthermore, by checking the peak at m / z=385, it is possible to confirm up to tetramers, and it is possible to determine whether the measurement sample has a repeating structure of formula (1).

[0123] The points corresponding to the resin particles and the points corresponding to the toner particles are distinguished from each other by the following method. Separately, the TOF-SIMS measurement sample is checked under an optical microscope, and the measurement range is marked by a method such as a laser marker, and an image of the measurement range is obtained. The transparent particles in the optical microscope image are resin particles, and the black particles are toner particles. If necessary, the brightness can be calculated based on the obtained image to confirm that it is within a predetermined range. Next, the sample is subjected to TOF-SIMS measurement, and the TOF-SIMS image is compared with the image obtained by an optical microscope to distinguish between resin particles and toner particles, thereby obtaining the target spectrum.

[0124] <Method for measuring normalized intensity of m / z 341 under condition (3)> Normally, TOF-SIMS is a surface analysis method, and the data in the depth direction is about 1 nm. Therefore, the strength inside the resin particles is measured after sputtering the resin particles with an argon gas cluster ion beam (Ar-GCIB) and scraping the surface. The toner particles and resin particles from which the external additives have been removed by the above method are sputtered under the following condition (3), and then the resin particles are measured under the same conditions as those in the above <Analysis of the structure of the resin contained in the toner particles and resin particles by a time-of-flight secondary ion mass spectrometer>. The obtained m / z 341 normalized intensity is the m / z 341 normalized intensity under condition (3). m / z 341 normalized intensity = (ion intensity of the peak detected at m / z = 341) / (total ion intensity from m / z = 0.5 to 1850) (A)

[0125] The sputtering conditions (3) are as follows: Ar-GCIB conditions Acceleration voltage: 5 kV Current: 6.5nA Raster size: 600 x 600 μm Irradiation time: 5sec / cycle Sputtering time: 500 seconds

[0126] <Identification of resin components and measurement of weight ratios using nuclear magnetic resonance spectroscopy (NMR)> Add 1 mL of deuterated chloroform to 20 mg of toner particles or resin particles, and measure the NMR spectrum of the protons of the dissolved resin. From the obtained NMR spectrum, the molar ratio and mass ratio of each monomer can be calculated, and the content of the constituent monomer units of the resin, such as polyester resin, can be obtained. The content ratio of each monomer component in the binder resin can also be calculated. For example, as a monomer for polyester resin, a peak derived from terephthalic acid appears at approximately 8.0 ppm, a peak derived from ethylene glycol appears at approximately 4.7 ppm, a peak derived from bisphenol appears at approximately 6.8 ppm, and a peak derived from styrene appears at approximately 7.1 ppm. Therefore, the molar ratio and mass ratio of each monomer can be calculated based on the integral ratio of the peaks of each monomer that makes up the resin. NMR device: JEOL RESONANCE ECX500 Observed nucleus: Proton Measurement mode: Single pulse Base peak: TMS

[0127] <Method of measuring weight average particle size (D4) of toner> The weight-average particle diameter (D4) of the toner is calculated as follows. The measurement device used is a precision particle size distribution measurement device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (Beckman Coulter, Inc.). The measurement will be performed using an effective number of measurement channels of 25,000. The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter). Before carrying out the measurements and analyses, the dedicated software is set up as follows. In the "Change standard measurement method (SOMME)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particle 10.0 μm" (Beckman Coulter). Press the "Threshold / Noise level measurement button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement." In the "Pulse to particle size conversion setting" screen of the dedicated software, the bin interval is set to logarithmic particle size, the particle size bin is set to 256 particle size bins, and the particle size range is set to 2 μm to 60 μm.

[0128] The specific measurement method is as follows. (1) Pour about 200 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, remove dirt and air bubbles from inside the aperture tube using the "Aperture Tube Flush" function of the dedicated software. (2) About 30 mL of the electrolyte solution is placed in a 100 mL flat-bottom glass beaker, and about 0.3 mL of a dilution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted about three times by mass with ion-exchanged water is added as a dispersant. (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetra150" (manufactured by Nikkaki Bios Co., Ltd.) with two built-in oscillators with an oscillation frequency of 50 kHz and a phase difference of 180 degrees, and an electrical output of 120 W. Pour about 3.3 L of ion-exchanged water into the water tank of the ultrasonic disperser, and add about 2 mL of Contaminon N to the water tank. (4) Set the beaker from (2) in the beaker fixing hole of the ultrasonic disperser, and operate the ultrasonic disperser. Then, adjust the height position of the beaker so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, the electrolytic solution (5) in which the toner is dispersed is dropped into the round-bottom beaker (1) placed in the sample stand, and the measurement concentration is adjusted to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle size (D4).

[0129] <Method for confirming that compound A is contained and that compound A is detected as a cation and compound B as an anion> The method of confirming that the compound A and the compound B are contained may be a method using liquid chromatography ESI / MS (electrospray ionization mass spectrometry), 1 Known analytical methods such as H nuclear magnetic resonance spectroscopy can be used. In the present disclosure, an analytical method using liquid chromatography ESI / MS is used. The analytical method is described below. The sample is prepared by using a toner under the dissolution condition A described below, and then separated into a solid content and a supernatant liquid under the centrifugation condition A. The supernatant obtained by the above adjustment is supplied to the liquid chromatograph ESI / MS analyzer described below, and ESI / MS analysis is carried out under analysis condition A.

[0130] Dissolution condition A: At 25°C, 10 times the mass of methanol (JISK8891 equivalent) is used for 10 g of toner, and a multi-stirrer (KSS-8; AS ONE Corporation) is used as the stirring device, and stirring is performed for 10 hours at 200 rpm. A triangle rotor (001.440; AS ONE Corporation) with total length x side length: 40 x 14 mm is used for stirring.

[0131] Centrifugation condition A: Rotation is performed for 30 minutes at 25° C., a rotation radius of 10.1 cm, and a rotation speed of 3500 rpm. As the centrifugation device, a centrifuge (H-9R; manufactured by Kokusan Co., Ltd.) can be used.

[0132] Measurement device: Ultimate3000 (Thermo Fisher Scientific) Mass spectrometer: LCQ Fleet (manufactured by Thermo Fisher Scientific) Analysis condition A: Under the following conditions, ionized materials are detected as cations under the capillary voltage of 35 V and tube lens voltage of 110 V, and ionized materials are detected as anions under the capillary voltage of -35 V and tube lens voltage of -110 V, and MS spectra of the cations and anions are obtained. Ionization method: Electrospray Ionization (ESI) Sheath Gas: 10 (arb. unit.) Aux Gas: 5 (arb. unit.) Spray voltage: 5kV Capillary temperature: 275℃ Mobile phase: Methanol (JISK8891 standard equivalent) Column: Not used (no stationary phase) Flow rate: 1ml / min Injection volume: 10μl Chromatogram detector: UV detector MS acquisition time: 5min MS measurement range: 50-1500 m / z EXAMPLES

[0133] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is in no way limited thereto. "Parts" used in the examples are by weight unless otherwise specified.

[0134] An example of toner production will now be described. <Production Example of Polyester Resin 1> A reaction vessel equipped with a stirrer, a thermometer, a nitrogen inlet tube, a dehydration tube, and a pressure reducing device was charged with 26.5 parts of terephthalic acid, 0.7 parts of isophthalic acid, 46.9 parts of a propylene oxide 2 mol adduct of bisphenol A, 5.0 parts of an ethylene oxide 2 mol adduct of bisphenol A, and 15.9 parts of ethylene glycol, and heated to a temperature of 130°C while stirring. Then, 0.52 parts of di(2-ethylhexanoate)tin was added as an esterification catalyst relative to 100.0 parts of the total amount of the monomers, and the temperature was raised to 200°C, and polycondensation was performed until the desired molecular weight was obtained. Furthermore, 5.0 parts of trimellitic anhydride was added to obtain an amorphous polyester resin 1.

[0135] <Production Example of Polyester Resin 2> Polyester resin 2 was obtained in the same manner as polyester resin 1, except that the ratio of each monomer component was changed to the following ratio. Terephthalic acid: 23.4 parts Isophthalic acid: 2.7 parts Trimellitic acid: 5 parts Bisphenol A-propylene oxide 2.2 mole adduct: 55.5 parts Bisphenol A-ethylene oxide 2.2 mole adduct: 4.8 parts Ethylene glycol: 8.8 parts Tin di(2-ethylhexanoate): 0.5 parts

[0136] <Production Example of Polyester Resin 3> Polyester resin 3 was obtained in the same manner as polyester resin 1, except that the ratio of each monomer component was changed to the following ratio. Terephthalic acid: 33.9 parts Trimellitic acid: 6.1 parts Bisphenol A-propylene oxide 2.2 mole adduct: 26.4 parts Ethylene glycol: 33.6 parts Tin di(2-ethylhexanoate): 0.5 parts

[0137] <Production Example of Polyester Resin 4> Polyester resin 4 was obtained in the same manner as polyester resin 1, except that the ratio of each monomer component was changed to the following ratio. Terephthalic acid: 52.7 parts Trimellitic acid: 1.1 parts Bisphenol A-propylene oxide 2.2 mole adduct: 52.7 parts Bisphenol A-ethylene oxide 2.2 mole adduct: 14.9 parts Tin di(2-ethylhexanoate): 0.5 parts

[0138] <Preparation of Polyester Resin Particle Dispersion 1> Polyester resin 1: 200 parts Ion-exchanged water: 500 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted, and then 0.1 mol / L sodium bicarbonate was added while thoroughly stirring at 7800 rpm using a homogenizer (IKA: Ultra Turrax T50) to make the pH greater than 7.0. Thereafter, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the mixture, thereby obtaining polyester resin particle dispersion 1. The particle size distribution of this polyester resin particle dispersion 1 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the polyester resin particles contained was 0.25 μm, and no coarse particles exceeding 1 μm were observed.

[0139] <Preparation of Polyester Resin Particle Dispersion 4> Polyester resin particle dispersion 4 was obtained in the same manner as in Production Example of Polyester resin particle dispersion 1, except that Polyester resin 1 was changed to Polyester resin 4. The particle size distribution of this polyester resin particle dispersion was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the polyester resin particles contained was 0.25 μm, and no coarse particles exceeding 1 μm were observed.

[0140] <Preparation example of wax particle dispersion> -500 parts deionized water Wax (behenyl behenate, melting point: 72.1°C) 250 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted. While thoroughly stirring at 7,800 rpm using a homogenizer (IKA Ultra Turrax T50), 0.1 mol / L sodium bicarbonate was added to adjust the pH to greater than 7.0. Thereafter, a mixed solution of 5 parts of sodium dodecylbenzenesulfonate and 245 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the wax particles. The particle size distribution of the wax particles contained in this wax particle dispersion was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number-average particle size of the wax particles contained was 0.35 μm, and no coarse particles exceeding 1 μm were observed.

[0141] <Preparation example of colorant particle dispersion> Carbon black Nipex35 (Orion Engineered Carbons) 100 Department Sodium dodecylbenzenesulfonate 5 parts -Ion-exchanged water 400 parts The above was mixed and dispersed using a sand grinder mill. The particle size distribution of the colorant particles contained in this colorant particle dispersion was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number-average particle size of the colorant particles contained was 0.2 μm, and no coarse particles exceeding 1 μm were observed.

[0142] <Production Example of Toner Particle 1> Polyester resin particle dispersion 1: 500 parts Colorant particle dispersion: 50 parts Wax particle dispersion: 50 parts Fatty alcohol alkylene oxide adduct (fatty alcohol type: lauryl alcohol, fatty alcohol parts: 190 parts, ethylene oxide parts: 310 parts) 5 parts A reactor (1-liter flask, anchor blade with baffle) was charged with polyester resin particle dispersion 1, wax particle dispersion, and aliphatic alcohol alkylene oxide adduct, and mixed uniformly. Meanwhile, a colorant particle dispersion was mixed uniformly in a 500 mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise while stirring the obtained mixed dispersion to form aggregated particles. After the dropwise addition was completed, the system was replaced with nitrogen, and the mixture was maintained at 50° C. for 1 hour and then at 55° C. for 30 minutes. 20 parts of polyester resin particle dispersion was added thereto at a ratio of 1:1, and the mixture was maintained for another 30 minutes, after which the pH was adjusted to 9.0 using a 5% aqueous sodium hydroxide solution.

[0143] The temperature was then raised to 90°C and held for 30 minutes. The temperature was then lowered to 63°C and held for 3 hours to form fused particles. The reaction was carried out in a nitrogen atmosphere. After the specified time had elapsed, the temperature was lowered at a rate of 0.5°C per minute until it reached room temperature. After cooling, the reaction product was subjected to solid-liquid separation under a pressure of 0.4 MPa in a 10 L pressure filter to obtain a toner cake. Then, ion-exchanged water was added to the pressure filter until it was filled with water, and the mixture was washed under a pressure of 0.4 MPa. The mixture was further washed in the same manner for a total of three times. After that, the mixture was subjected to solid-liquid separation under a pressure of 0.4 MPa, and then fluidized bed drying was performed at 45°C to obtain toner particles 1 having a weight average particle size (D4) of 6.4 μm.

[0144] <Production Example of Toner Particle 2> Toner particles 2 were obtained in the same manner as in the production example of toner particles 1, except that the aliphatic alcohol alkylene oxide adduct was changed to sodium dodecylbenzenesulfonate.

[0145] <Production Example of Toner Particle 6> Toner particles 6 were obtained in the same manner as in the production example of toner particles 1, except that polyester resin 1 was changed to polyester resin 4.

[0146] <Production Example of Toner Particle 3> Polyester resin 1: 100.0 parts Wax (behenyl behenate, melting point: 72.1°C): 6.0 parts Carbon black Nipex35 (Orion Engineered Carbons): 10 parts Monoazo dye iron complex (T-77, manufactured by Hodogaya Chemical Co., Ltd.): 2.0 parts The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for a rotation time of 5 minutes, the mixture was kneaded in a twin-screw kneader (PCM-30, manufactured by Ikegai Corporation) set at a temperature of 130°C. The kneaded mixture was cooled to 25°C and coarsely crushed to 1 mm or less in a hammer mill to obtain a coarsely crushed product. The coarsely crushed product was finely crushed in a mechanical crusher (T-250, manufactured by Turbo Kogyo Co., Ltd.). The product was classified using a multi-division classifier utilizing the Coanda effect to obtain toner particles 3 having a weight average particle size (D4) of 7.2 μm.

[0147] <Production Examples of Toner Particles 4 and 5> Toner particles 4 and 5 were obtained in the same manner as in the production example of toner particles 3, except that polyester resin 2 was used in place of polyester resin 1 for toner particles 4, and polyester resin 3 was used in toner particles 5. The physical properties are shown in Table 1.

[0148] [Table 1] In the table, the particle size indicates the weight average particle size (D4), and the average brightness value is the average brightness value based on monochrome 256 gradations.

[0149] <Production Example of Resin Particle 1> Polyester resin particle dispersion 1: 500 parts Ion-exchanged water: 160 parts Polyester resin particle dispersion 1 and ion-exchanged water were uniformly mixed in a reactor (1-liter flask, baffled anchor blade), and 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise while stirring to form aggregated particles. After the dropwise addition was completed, the system was replaced with nitrogen and the temperature was raised to 55° C. The formed aggregated particles were appropriately checked using a Coulter Multisizer III, and the weight average particle size (D4) was about 1.5 When aggregated particles of 1 μm in size were formed, the pH was adjusted to 9.0 using a 5% aqueous sodium hydroxide solution.

[0150] The temperature was then raised to 90°C and held for 30 minutes. The temperature was then lowered to 63°C and held for 3 hours to form fused particles. The reaction was carried out in a nitrogen atmosphere. After the specified time had elapsed, the temperature was lowered at a rate of 0.5°C per minute until it reached room temperature. After cooling, solid-liquid separation was performed using a pressure filter, and washing with ion-exchanged water was performed a total of three times, followed by fluidized bed drying at 45° C. to obtain resin particles 1 having a weight average particle size (D4) of about 1.5 μm.

[0151] <Production Example of Resin Particles 2> A 5L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introduction device was charged with an aqueous surfactant solution in which 4 parts by mass of sodium dodecylbenzenesulfonate was dissolved in 3040 parts by mass of ion-exchanged water. Further, a polymerization initiator solution in which 10 parts by mass of potassium persulfate was dissolved in 400 parts by mass of ion-exchanged water was added, and the liquid temperature was raised to 75°C. 530 parts by mass of styrene, 200 parts by mass of n-butyl acrylate, and 16 parts by mass of n-octyl mercaptan were added thereto, and polymerization was carried out by heating and stirring for 2 hours, to prepare a styrene-acrylic resin particle dispersion. Styrene acrylic resin particle dispersion: 800 parts Polyester resin particle dispersion 1: 50 parts The styrene-acrylic resin particle dispersion was transferred to a reactor (1-liter flask, baffled anchor blade), and 0.5 parts of an aluminum sulfate aqueous solution (solid content) was added dropwise while stirring to form aggregated particles. After the dropping was completed, the system was replaced with nitrogen and the temperature was raised to 55° C. The formed aggregated particles were appropriately checked using a Coulter Multisizer III, and when aggregated particles having a weight average particle size (D4) of about 1.2 μm were formed, polyester resin particle dispersion liquid 1 was added, and after keeping for another 30 minutes, the pH was adjusted to 9.0 using a 5% aqueous sodium hydroxide solution.

[0152] The temperature was then raised to 90°C and held for 30 minutes. The temperature was then lowered to 63°C and held for 3 hours to form fused particles. The reaction was carried out in a nitrogen atmosphere. After the specified time had elapsed, the temperature was lowered at a rate of 0.5°C per minute until it reached room temperature. After cooling, solid-liquid separation was performed using a pressure filter, and washing with ion-exchanged water was performed a total of three times, followed by fluidized bed drying at 45° C. to obtain resin particles 2 having a weight average particle size (D4) of about 1.8 μm.

[0153] <Production Examples of Resin Particles 3, 4, and 5> Resin particles 3, 4, and 5 were obtained in the same manner as in the production example of resin particles 1, except that polyester resin particle dispersion 2 was used for resin particles 3, polyester resin particle dispersion 3 was used for resin particles 4, and polyester resin particle dispersion 4 was used for resin particles 5 instead of polyester resin particle dispersion 1. The physical properties are shown in Table 2.

[0154] <Production Example of Resin Particles 6> In a production example of resin particles 1, polyester resin particle dispersion 1 and ion-exchanged water were uniformly mixed in a reactor (1-liter flask, baffled anchor blade), and 0.5 parts of an aluminum sulfate aqueous solution (solid content) were dropped while stirring to form aggregated particles. After the dropwise addition was completed, the system was purged with nitrogen and the temperature was raised to 55° C. The formed aggregated particles were appropriately checked using a Coulter Multisizer III, and when aggregated particles having a weight average particle size (D4) of about 2.5 μm were formed, the pH was adjusted to 9.0 using a 5% aqueous sodium hydroxide solution. The temperature was then raised to 90°C and held for 60 minutes. After that, the temperature was lowered to 63°C and held for 4 hours. The reaction was carried out in a nitrogen atmosphere, and after the specified time had elapsed, the mixture was cooled to room temperature at a rate of 0.5°C per minute. After cooling, solid-liquid separation was performed using a pressure filter, and washing with ion-exchanged water was performed a total of three times, followed by fluidized bed drying at 45° C. to obtain resin particles 6 having a weight average particle size (D4) of about 2.5 μm.

[0155] <Production Example of Resin Particles 7> Resin particles 7 were obtained in the same manner as in the production example of resin particles 1, except that 0.18 parts by mass of the colorant particle dispersion was added.

[0156] <Production Example of Resin Particle 8> Resin particles 8 were obtained in the same manner as in the production example of resin particles 1, except that 0.20 parts by mass of the colorant particle dispersion was added. [Table 2] The average brightness value is based on 256 monochrome gradations.

[0157] <Toner 1 Manufacturing Example> Resin particles 1 (2 parts) and silica particles (RX200: primary average particle size 12 nm, HMDS treatment, manufactured by Nippon Aerosil Co., Ltd.) (1.5 parts) were externally added and mixed with the toner particles 1 (100.0 parts) obtained above using an FM10C (manufactured by Nippon Coke and Engineering Co., Ltd.). The external addition conditions were as follows: the lower blade was set to A0 blade, the gap with the deflector wall was set to 20 mm, the amount of toner particles charged was 2.0 kg, and the rotation speed was 66.6 s. -1 The external addition time was 10 minutes, and the cooling water temperature was 20°C and the flow rate was 10 L / min. Thereafter, the mixture was sieved through a mesh having an opening of 200 μm to obtain Toner 1. The formulation and physical properties of the obtained Toner 1 are shown in Tables 3 and 4.

[0158] <Production example of toner 2 to 20> In the manufacturing example of Toner 1, the type of toner particles, the type of resin particles and the amount of addition are shown in Table 3. Except for the above changes, toners 2 to 20 were obtained in the same manner. The physical properties of toners 2 to 20 obtained are shown in Tables 3 and 4. [Table 3] The amount of resin particles is the amount relative to 100 parts by mass of toner particles. The average brightness is the average brightness based on monochrome 256 gradations. In the columns for the presence of toner particle formula (1) and the presence of resin particle formula (1), "present" is recorded when the toner particle has a resin having a repeating structure of the structure represented by formula (1) on its surface, and "absent" is recorded when the resin does not have the surface. In the column for compound A, when the analysis was performed under the above-mentioned analytical condition A, if compound A was ionized and detected as a cation, it was marked "Y," and if it was not detected, it was marked "N." In the column for compound B, when the analysis was performed under the above-mentioned analytical condition A, if compound B was ionized and detected as an anion, it was marked "Y," and if it was not detected, it was marked "N."

[0159] [Table 4] In the table, "Fine particle ratio in toner" is the ratio of fine particles (number %) to the total of toner particles and resin particles. "Resin particle amount in toner" is the resin particle content (number) per 100 toner particles. "Resin particle ratio in fine particles" is the ratio of resin particles (number %) in fine particles. In the table, in the column of "resin particle break point", if the ratio of resin particles without a break point in the load displacement curve obtained by microcompression measurement of resin particles in the load range of 0 to 10 mN is 90% or more by number, it is recorded as "none". On the other hand, if the ratio of resin particles without the break point is less than 90% by number, it is recorded as "present". In the column of "Toner particle break point", if the ratio of toner particles having a break point in a load displacement curve obtained by microcompression measurement of toner particles in a load range of 0 to 10 mN is 80% or more by number, it is recorded as "Yes". On the other hand, if the ratio of toner particles having the break point is less than 80% by number, it is recorded as "No".

[0160] The obtained toner was subjected to the following evaluations. <Image evaluation> The image evaluation was performed using a speed-up device that was partially modified from a commercially available color laser printer (HP LaserJet Enterprise Color M555dn, manufactured by HP). The printer was modified so that it could operate even with only one color process cartridge installed. The toner was removed from the black cartridge and replaced with 100 g of the toner to be evaluated, and the evaluation was performed.

[0161] [Image quality evaluation under normal temperature and humidity conditions] For the purpose of testing the image quality of the toner, density and fog in a normal temperature and humidity environment (25° C. / 65% RH) were evaluated by the following method. Canon color laser copier paper (A4: 81.4 g / m2) under normal temperature and humidity conditions. 2 (Unless otherwise specified, hereafter, this paper is assumed to be used) images with a print rate of 1.0% were printed on a 1000-ink cartridge with a 2-second break every two prints, for a total of 2000 prints per day. After printing 2000 prints, the fogging on the drum of the cartridge was taped off and evaluated, and solid and halftone images were printed.

[0162] Fog was measured using a reflection densitometer (TOKYO DENSHOKU CORP., REFLECTOMETER MODEL TC-6DS). The fog density (%) was calculated by taking the worst reflection density of the white background of the tape as Ds and the average reflection density of the paper of the taped part as Dr (Ds-Dr). Measurements were performed using three types of filters: green, amber, and blue, and the worst value was recorded as the fog density. The fog density was evaluated according to the following criteria: C or higher was considered to be good. Evaluation criteria A: Fog density less than 0.5% B: Fog density 0.5% or more and less than 1.5% C: Fog density 1.5% or more and less than 3.0% D: Fog density 3.0% or more

[0163] Image density was measured at five points using a color reflection densitometer (X-Rite404A) and the average value was calculated. Evaluation rank was based on the following criteria. C or higher was judged as good. A: 1.2 or higher B: 1.1 or more and less than 1.2 C: 1.0 or more and less than 1.1 D: Less than 1.0

[0164] Halftone density unevenness caused by C roller contamination due to poor cleaning was evaluated according to the following criteria. The halftone density unevenness caused by C roller contamination evaluated here is unevenness that occurs over the entire length in a width of 2 cm or more from the edge. The image density becomes darker in areas where the C roller is contaminated. The density of the edge and center of the image was measured using a color reflection densitometer (X-Rite404A), and the difference in density was taken as the unevenness value. A grade of C or above was judged to be good. Evaluation criteria A: Density unevenness less than 0.02% B: Density unevenness: 0.02% or more, less than 0.05% C: Density unevenness: 0.05% or more, but less than 0.10% D: Density unevenness 0.10% or more

[0165] [Cleaning ability in low temperature and low humidity environments] The cleaning ability in a low temperature and low humidity environment (10° C. / 15% RH) was evaluated by the following method. In a low temperature and low humidity environment, 1,000 images with a print rate of 1.0% were printed per day with a 2 second break between every two images, for a total of 2,000 images. After printing 2,000 images, the cartridge was used to continuously print three all-black images and one all-white image, for a total of four images, and finally a halftone image was printed. In this evaluation method, if the cleaning ability of the toner is reduced, a streak-like image defect (vertical black streak) occurs in an all-white image after outputting an all-black image due to poor cleaning (toner slip-through).

[0166] The cleaning performance was evaluated according to the following criteria: C or above was evaluated as good. Evaluation criteria In the case of an all-white image after outputting five all-black images, A: No streaky image defects are observed B: 1 to 3 tiny streak-like defects less than 1 mm wide are observed. C: 4 to 10 tiny streak-like defects less than 1 mm wide are observed. D: 11 or more minute streak defects less than 1 mm in width are observed, or streak defects 1 mm or more in width are observed.

[0167] Furthermore, if contamination of the C roller accumulates, it appears as density unevenness in the halftone image. Halftone density unevenness caused by C roller contamination due to poor cleaning was evaluated according to the following criteria. The halftone density unevenness evaluated here is unevenness that occurs over the entire length in a width of 2 cm or more from the edge. The image density becomes higher in areas where the C roller is contaminated. The density of the edge and center of the image was measured using a color reflection densitometer (X-Rite404A), and the density difference was taken as the unevenness value. A grade of C or above was considered good. Evaluation criteria A: Density unevenness less than 0.02% B: Density unevenness: 0.02% or more, less than 0.05% C: Density unevenness: 0.05% or more, but less than 0.10% D: Density unevenness 0.10% or more

[0168] [Examples 1 to 15] In Examples 1 to 15, the above evaluations were carried out using toners 1 to 15, respectively. The evaluation results are shown in Table 5.

[0169] [Comparative Examples 1 to 5] In Comparative Examples 1 to 5, the above evaluations were carried out using toners 16 to 20, respectively. The evaluation results are shown in Table 5.

[0170] [Table 5]

[0171] In Examples 1 to 15, good results were obtained in all evaluation items. On the other hand, in Comparative Examples 1 and 3 to 5, the results were inferior to those of the Examples in the evaluation item of cleaning ability. In Comparative Example 2, the results were inferior to those of the Examples in image density.

[0172] From the above results, according to the present disclosure, when a toner containing a resin having a PET structure and a black pigment is used, even when a large amount of printing is performed over a long period of time, contamination of the charging roller due to poor cleaning and the resulting image defects can be suppressed in low temperature and low humidity environments and in normal temperature and normal humidity environments.

[0173] The present disclosure relates to the following configurations. (Configuration 1) A toner comprising toner particles containing a pigment, resin particles, and an external additive, the resin particles have an average brightness of 90 to 120 based on monochrome 256 gradations, and an average equivalent circular diameter of 0.5 to 3.0 μm; the toner particles have an average brightness of 40 to 80 based on monochrome 256 gradations; the pigment is a black pigment, the content of the resin particles in the toner is 5 to 40 per 100 toner particles, The toner particles have a resin having a repeating structure represented by the following formula (1) on the surface thereof, The resin particles have a resin having a repeating structure represented by the following formula (1) on the surface thereof, In the load-displacement curve obtained by microcompression measurement of the resin particles, The toner is characterized in that 90% or more by number of the resin particles do not have a breaking point within a load range of 0 to 10 mN. TIFF2024165834000009.tif31153 (Configuration 2) In a time-of-flight secondary ion mass spectrometry of the resin particles under the following condition (2), the normalized intensity at m / z 341 calculated by the following formula (A) is 2.50×10 -4 ~1.00×10 -2 and In a time-of-flight secondary ion mass spectrometry analysis of the resin particles under the following condition (3), the normalized intensity at m / z 341 calculated by the following formula (A) is 2.50×10 -4 ~1.00×10 -2 2. The toner according to claim 1, m / z 341 normalized intensity = (ion intensity of the peak detected at m / z = 341) / (total ion intensity from m / z = 0.5 to 1850) (A) Condition (2): Primary ion species: Bi 3++ ,Accelerating voltage: 30kV, Measurement mode: Positive, Negative, Measurement range: m / z=0.5~1850, Raster size: 300×300μm / 256×256pixel, Measurement time: 180 seconds Condition (3): After performing sputtering with Ar-GCIB under the following conditions, perform measurement under said conditions (2). Ar-GCIB conditions Acceleration voltage: 5 kV Current: 6.5nA Raster size: 600 x 600 μm Irradiation time: 5sec / cycle Sputtering time: 500 seconds (Configuration 3) 3. The toner according to claim 1 or 2, wherein the content of the resin particles in the fine particles is 60 to 100% by number when the particles having a circle-equivalent diameter of 0.5 to 3.0 μm contained in the toner are regarded as fine particles. The toner described. (Configuration 4) When particles having a circular equivalent diameter of 0.5 to 3.0 μm contained in the toner are considered as microparticles, The toner according to any one of configurations 1 to 3, wherein the toner contains the fine particles in an amount of 10 to 40% by number of the total of the toner particles and the resin particles. (Configuration 5) the toner particles contain a binder resin, The binder resin contains a polyester resin, The binder resin contains, as a component constituting the polyester resin, Contains 3 to 30 mass% of a structure corresponding to ethylene glycol, 5. The toner according to any one of configurations 1 to 4, which contains 20 to 45% by mass of a structure corresponding to terephthalic acid. (Configuration 6) In the load-displacement curve obtained by microcompression measurement of the toner particles, The toner according to any one of configurations 1 to 5, wherein 80% by number or more of the toner particles have a breaking point within a load range of 0 mN to 10 mN. (Configuration 7) The toner contains compound A and compound B which are eluted in methanol when the toner is subjected to an elution treatment under the following elution condition A, The supernatant obtained by centrifuging the eluate in which the compound A and the compound B were eluted in the methanol under the following centrifugation condition A was analyzed by liquid chromatography ESI / MS under the following analysis condition A. The compound A contained in the supernatant is ionized as a cation and detected, The toner according to any one of configurations 1 to 6, wherein the compound B contained in the supernatant is detected as an anion. Dissolution condition A: At 25° C., 10 times the mass of the toner is used in methanol (JIS K8891 equivalent), and the toner is stirred for 10 hours at a rotor speed of 200 rpm using a stirring device. Centrifugation condition A: Rotation is performed for 30 minutes at 25° C., a rotation radius of 10.1 cm, and a rotation speed of 3,500 rpm. Analysis condition A: Sheath Gas: 10 (arb. unit.), Aux Gas: 5 (arb. unit.), spray voltage: 5 kV, capillary temperature: 275°C. Ionized substances are detected as cations under the conditions of capillary voltage: 35 V, tube lens voltage: 110 V, and ionized substances are detected as anions under the conditions of capillary voltage: -35 V, tube lens voltage: -110 V. (Configuration 8) The compound A is at least one compound selected from the group consisting of an ethylene oxide adduct of a linear aliphatic alcohol having 8 to 16 carbon atoms and sodium polyoxyethylene lauryl ether acetate, The toner according to configuration 7, wherein the compound B is linear or branched sodium dodecylbenzenesulfonate. (Configuration 9) The toner according to any one of configurations 1 to 8, wherein the toner particles are emulsion aggregation toner particles. (Configuration 10) 10. The toner according to any one of configurations 1 to 9, wherein the black pigment comprises carbon black.

Claims

1. A toner comprising toner particles containing a pigment, resin particles, and an external additive, the resin particles have an average brightness of 90 to 120 based on monochrome 256 gradations, and an average equivalent circular diameter of 0.5 to 3.0 μm; the toner particles have an average brightness value of 40 to 80 based on monochrome 256 gradations; the pigment is a black pigment, the content of the resin particles in the toner is 5 to 40 per 100 toner particles, The toner particles have a resin having a repeating structure represented by the following formula (1) on the surface thereof, The resin particles have a resin having a repeating structure represented by the following formula (1) on the surface thereof, In the load-displacement curve obtained by microcompression measurement of the resin particles, The toner is characterized in that 90% or more by number of the resin particles do not have a breaking point within a load range of 0 to 10 mN.

2. In a time-of-flight secondary ion mass spectrometry analysis of the resin particles under the following condition (2), the normalized intensity at m / z 341 calculated by the following formula (A) is 2.50×10 -4 ~1.00 x 10 -2 and In a time-of-flight secondary ion mass spectrometry analysis of the resin particles under the following condition (3), the normalized intensity at m / z 341 calculated by the following formula (A) is 2.50×10 -4 ~1.00 x 10 -2 The toner according to claim 1 , m / z 341 normalized intensity=(ion intensity of the peak detected at m / z=341) / (total ion intensity at m / z=0.5 to 1850) (A) Condition (2): Primary ion species: Bi 3++ , Acceleration voltage: 30 kV, Measurement mode: Positive, Negative, Measurement range: m / z = 0.5 to 1850, Raster size: 300 x 300 μm / 256 x 256 pixels, Measurement time: 180 seconds Condition (3): After performing sputtering with Ar-GCIB under the following conditions, measurement is performed under the same conditions (2). Ar-GCIB conditions Acceleration voltage: 5 kV Current: 6.5nA Raster size: 600 x 600 μm Irradiation time: 5sec / cycle Sputtering time: 500 seconds

3. 3. The toner according to claim 1, wherein when particles having an equivalent circle diameter of 0.5 to 3.0 μm contained in the toner are considered as microparticles, a content ratio of the resin particles in the microparticles is 60 to 100% by number.

4. When particles having a circular equivalent diameter of 0.5 to 3.0 μm contained in the toner are considered as microparticles, 3. The toner according to claim 1, wherein the toner contains the fine particles in an amount of 10 to 40% by number of the total of the toner particles and the resin particles.

5. the toner particles contain a binder resin, The binder resin contains a polyester resin, The binder resin contains, as a component constituting the polyester resin, Contains 3 to 30% by mass of a structure corresponding to ethylene glycol, 3. The toner according to claim 1, which contains 20 to 45% by mass of a structure corresponding to terephthalic acid.

6. In the load-displacement curve obtained by microcompression measurement of the toner particles, 3. The toner according to claim 1, wherein 80% or more by number of the toner particles have a breaking point within a load range of 0 mN to 10 mN.

7. The toner contains compound A and compound B which are soluble in methanol when the toner is subjected to an elution treatment under the following elution condition A, The supernatant obtained by centrifuging the eluate in which the compound A and the compound B were eluted in methanol under the following centrifugation condition A was analyzed by liquid chromatography ESI / MS under the following analysis condition A. The compound A contained in the supernatant is ionized as a cation and detected, 3. The toner according to claim 1, wherein the compound B contained in the supernatant is detected as an anion. Dissolution condition A: At 25° C., methanol (equivalent to JIS K8891 standard) in an amount 10 times the mass of the toner is used, and the toner is stirred for 10 hours at a rotor speed of 200 rpm using a stirring device. Centrifugation condition A: Rotation was performed at 25° C., a rotation radius of 10.1 cm, and a rotation speed of 3,500 rpm for 30 minutes. Analysis condition A: Sheath gas: 10 (arb. unit), Aux gas: 5 (arb. unit), spray voltage: 5 kV, capillary temperature: 275° C., ionized substances are detected as cations under the conditions of capillary voltage: 35 V, tube lens voltage: 110 V, and ionized substances are detected as anions under the conditions of capillary voltage: −35 V, tube lens voltage: −110 V.

8. The compound A is at least one compound selected from the group consisting of an ethylene oxide adduct of a linear aliphatic alcohol having 8 to 16 carbon atoms and sodium polyoxyethylene lauryl ether acetate, The toner according to claim 7, wherein the compound B is linear or branched sodium dodecylbenzenesulfonate.

9. The toner of claim 1 or 2, wherein said toner particles are emulsion aggregation toner particles.

10. The toner of claim 1 or 2, wherein the black pigment comprises carbon black.

Citation Information

Patent Citations

  • Toner for electrostatic charge image development

    JP2017219823A

  • Toner for electrostatic charge image development and two-component developer for electrostatic charge image development

    JP2019184795A