Rapid hardening mortar composition
The fast-hardening mortar composition with hydraulic cement, aggregate, and amorphous aluminum hydroxide, enhanced by alkali metal carbonate or lime, addresses the issues of fluidity and self-supporting properties, ensuring rapid strength development and preventing collapse during 3D printing.
Patent Information
- Application Number
- JP2023082431
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing mortar compositions for 3D printing lack sufficient fluidity and self-supporting properties, leading to collapse during layering and curing times that are too long for certain structures.
A fast-hardening mortar composition containing hydraulic cement, aggregate, water, and amorphous aluminum hydroxide, optionally with alkali metal carbonate or lime, achieving flow values of 100 to 120 mm before impact and 135 to 250 mm after impact, ensuring extrudability and early strength development.
The composition maintains shape after extrusion from a 3D printer nozzle and achieves early strength within 10 minutes, preventing collapse and enabling rapid layering without structural failure.
Smart Images

Figure 2024165871000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a fast-setting mortar composition mainly used in the fields of civil engineering and construction, and more particularly to a fast-setting mortar composition suitable for use in 3D printers. [Background technology]
[0002] In recent years, the use of 3D printers to build houses and structures and manufacture structural components has been considered in the field of architecture and a wide range of other fields. The material used in this case is basically mortar, which is made of hydraulic cement, aggregate, and water. In other words, hydraulic cement alone shrinks significantly after hardening, causing defects such as cracks, so materials with aggregate added are used.
[0003] The construction of a model using a 3D printer is carried out by extruding mortar from the nozzle of the 3D printer onto a bed (table) according to modeling data created by a computer, forming a hardened layer of the extruded mortar, and then extruding more mortar from the nozzle onto this hardened layer, repeatedly extruding and hardening the mortar to successively stack hardened layers in the height direction. For this reason, mortar for 3D printers is required to be soft enough to be extruded from the nozzle of the 3D printer, self-supporting so that it can maintain its shape after extrusion, and not to be crushed or disintegrated even if more mortar is stacked on top of it.
[0004] For this reason, for example, Patent Document 1 proposes a material that contains hydraulic cement, aggregate, water, a specific dispersant, a thickener, a retarder, amorphous calcium aluminosilicate, gypsum, and short fibers, and has excellent self-supporting properties and strength development.
[0005] Furthermore, as materials that impart hardening acceleration performance, Patent Document 2 discloses a hardening material that is mixed with a main liquid containing lime and water to harden the main liquid, the hardening material being characterized by containing dry aluminum hydroxide gel (amorphous aluminum hydroxide) and an alkali metal carbonate, as well as a hardening material liquid and a chemical liquid for soil stabilization. Furthermore, Patent Document 3 describes, as a comparative example, that the viscosity of the cement slurry is increased by adding amorphous aluminum hydroxide to a mixture of cement and water. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2018-140906 A [Patent Document 2] Patent Publication No. 2021-42088 [Patent Document 3] JP 2001-348257 A Summary of the Invention [Problem to be solved by the invention]
[0007] Patent Document 1 proposes a material that has excellent self-supporting properties and strength development due to the inclusion of various additives, but the curing time of the examples shown therein is 25 minutes or more, making it unsuitable for use in situations where the material is prone to collapse after being layered, such as in sloped structures, and an even faster curing time is desired. Patent Document 2 describes an example in which a hardening agent containing amorphous aluminum hydroxide is mixed with a main liquid, causing the mixture to gel in about 10 seconds after mixing. However, this material is intended for ground improvement, does not contain aggregate, does not require self-supporting, and is related to a hydraulic cement slurry (liquid) with a large amount of water relative to the cement, and although it describes that the mixture gels in about 10 seconds, there is no description of the hardness of the chemical solution after gelation. Patent Document 3 describes how adding amorphous aluminum hydroxide increases the viscosity of a slurry of cement and water, but makes no mention of the process by which the slurry becomes hard enough to withstand being crushed when layered using a 3D printer.
[0008] In view of the problems with the conventional technology described above, the present invention aims to provide a fast-hardening mortar composition that is fluid immediately after preparation, soft enough to be extruded from the nozzle of a 3D printer, and self-supporting after extrusion, and will not collapse or crumble even if a material is layered on top of it within 10 minutes. [Means for solving the problem]
[0009] The present invention includes the following aspects [1] to [3].
[0010] [1] A rapid-setting mortar composition comprising hydraulic cement, aggregate, water, and amorphous aluminum hydroxide, the rapid-setting mortar composition having a flow value immediately after preparation of the rapid-setting mortar composition before impact of 100 to 120 mm and a flow value after impact of 135 to 250 mm as measured in a flow test specified in JIS R5201:2015. [2] The fast-hardening mortar composition according to [1], further comprising an alkali metal carbonate. [3] The fast-hardening mortar composition according to [1] or [2], further comprising lime. Effect of the Invention
[0011] According to the present invention, a fast-hardening mortar composition can be provided which is soft and fluid immediately after preparation, allowing it to be extruded from the nozzle of a 3D printer, and which can stand on its own while maintaining its shape after extrusion. It then hardens in about 10 minutes, and does not crumble even if cement mortar is layered on top at an early stage, making it suitable for additive manufacturing using a 3D printer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below.
[0013] [Component composition of fast-hardening mortar composition] The rapid-setting mortar composition of the present invention contains hydraulic cement, aggregate, water, and amorphous aluminum hydroxide. The rapid-setting mortar composition of the present invention may further contain an alkali metal carbonate, lime, and other additives. Each component will be described below.
[0014] (hydraulic cement) Examples of hydraulic cement include ordinary, early strength, super early strength, moderate heat and white Portland cement, blast furnace cement, silica cement, mixed cement such as fly ash cement, fine particle cement, ultrafine particle cement, ultra-ultrafine particle cement, granulated blast furnace slag, and alumina cement. Hydraulic cement also includes pozzolanic reactive substances, which exhibit hydraulic properties due to the presence of lime. Examples of such pozzolanic reactive substances include silica fume, fly ash, and activated kaolin. The hydraulic cement may be contained in a single type or in a combination of two or more types.
[0015] (aggregate) The aggregate is not particularly limited, but examples thereof include silica sand of various sizes such as No. 3, No. 4, No. 5, No. 6, No. 7, No. 8, etc., lightweight aggregates such as fly ash balloons and shirasu balloons, Toyoura sand, etc. The aggregate may be contained in a single type or in a combination of two or more types. The particle size of the aggregate is preferably 0.1 to 3 mm, more preferably 0.2 to 1 mm, and even more preferably 0.3 to 0.7 mm, in terms of 50% particle size. If the particle size of the aggregate is equal to or greater than the lower limit, it is preferable from the viewpoint of increasing the fluidity and strength even with the same amount of water, and if it is equal to or less than the upper limit, it is preferable from the viewpoint of easily maintaining the shape.
[0016] In the fast-setting mortar composition of the present invention, the content of the aggregate is preferably 50 to 500 parts by mass, more preferably 100 to 300 parts by mass, relative to 100 parts by mass of hydraulic cement. If the content of the aggregate is equal to or more than the lower limit, it is preferable from the viewpoint of suppressing shrinkage of the cement and suppressing cracks, and if it is equal to or less than the upper limit, it is preferable from the viewpoint of increasing strength.
[0017] (water) Examples of water include tap water, industrial water, groundwater, river water, seawater, etc. Among these, tap water and industrial water are preferred in order to fully exert the effects of the present invention.
[0018] In the fast-setting mortar composition of the present invention, the content of water is preferably 0.2 to 1.5, more preferably 0.5 to 1.0, in terms of the ratio of water to cement (water / cement ratio). If the water / cement ratio is equal to or more than the lower limit, it is preferable from the viewpoint of increasing fluidity. On the other hand, if it is equal to or less than the upper limit, it is preferable from the viewpoint of increasing strength.
[0019] (Amorphous Aluminum Hydroxide) In the present invention, the amorphous aluminum hydroxide includes all amorphous aluminum hydroxides. Examples of amorphous aluminum hydroxide include dried aluminum hydroxide gel powder and aluminum sludge generated in anodizing. Among these, from the viewpoint of high activity, dry aluminum hydroxide gel powder is preferred.
[0020] Dry aluminum hydroxide gel is a compound with the chemical composition Al(OH)3·mH2O, and is amorphous aluminum hydroxide. Examples of dry aluminum hydroxide gel powder include those used in medical antacids and ulcer healing agents in the Japanese Pharmacopoeia, but for industrial use, dry aluminum hydroxide gel powder used as an adsorbent is preferred. The aluminum oxide content of the dry aluminum hydroxide gel powder is preferably 45% or more, more preferably 50% or more. If the aluminum oxide content is 45% or more, the reactivity is high and the rapid hardening property is excellent. The particle size of the dry aluminum hydroxide gel powder is preferably 40 to 120 μm, more preferably 60 to 100 μm, as determined by a laser diffraction scattering method. If the median size is equal to or greater than the lower limit, the particles are less likely to fly around, improving the handling properties. On the other hand, if the median size is equal to or less than the upper limit, the particles are prevented from settling, and the reactivity is increased, resulting in excellent rapid curing properties.
[0021] In the rapid-setting mortar composition of the present invention, the content of amorphous aluminum hydroxide is preferably 10 to 0.2 parts by mass, more preferably 5 to 0.5 parts by mass, and even more preferably 3 to 1 part by mass, relative to 100 parts by mass of hydraulic cement. If the content of amorphous aluminum hydroxide is equal to or more than the above lower limit, it is preferable in that the rapid-setting effect of amorphous aluminum hydroxide can be sufficiently obtained, and if it is equal to or less than the above upper limit, it is preferable in that the effect of maintaining fluidity immediately after preparation can be sufficiently obtained.
[0022] (alkali metal carbonate) The alkali metal carbonate is a component that further imparts rapid hardening properties when combined with amorphous aluminum hydroxide, which imparts rapid hardening properties.
[0023] Examples of the alkali metal carbonate include carbonates of alkali metals such as Li2CO3, Na2CO3, K2CO3, etc. Only one type of alkali metal carbonate may be contained, or two or more types may be contained in combination.
[0024] When the rapid-setting mortar composition of the present invention contains an alkali metal carbonate, the content of the alkali metal carbonate is preferably in the range of 0.5 to 2 in terms of mass ratio to the amorphous aluminum hydroxide. The total content of the amorphous aluminum hydroxide and the alkali metal carbonate is preferably 0.2 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and even more preferably 1 to 2 parts by mass, per 100 parts by mass of hydraulic cement. That is, due to the synergistic effect of improving the rapid hardening property by using amorphous aluminum hydroxide in combination with an alkali metal carbonate, the amount of these compounds can be smaller than that when amorphous aluminum hydroxide is used alone.
[0025] (lime) Lime is a component that imparts further rapid hardening properties when combined with amorphous aluminum hydroxide, which already imparts rapid hardening properties, and even in a combination of amorphous aluminum hydroxide, alkali metal carbonate, and lime, rapid hardening properties can be imparted with a small amount of amorphous aluminum hydroxide.
[0026] Lime takes the form of calcium hydroxide (Ca(OH)2) in water, and examples include slaked lime (Ca(OH)2) and quicklime (CaO). Among these, slaked lime is preferred because it is easy to handle.
[0027] The Blaine value of lime is 6000~30000 cm 2 / g is preferable, and 8000 to 20000 cm 2 If the Blaine value of lime is equal to or higher than the lower limit, the rapid hardening property is improved. On the other hand, if the Blaine value is equal to or lower than the upper limit, the viscosity of the rapid hardening mortar composition is reduced and aggregation is less likely to occur when mixed with water. The lime may be contained in a single type or in a combination of two or more types.
[0028] When the rapid-setting mortar composition of the present invention contains lime, the content of lime is preferably in the range of 0.2 to 2 in terms of mass ratio to the amorphous aluminum hydroxide. The total content of the amorphous aluminum hydroxide and lime is preferably 0.2 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and even more preferably 1 to 2 parts by mass, per 100 parts by mass of hydraulic cement. That is, due to the synergistic effect of improving the rapid hardening property by using amorphous aluminum hydroxide in combination with lime, the amount of these ingredients can be less than when amorphous aluminum hydroxide is used alone. In particular, when the rapid-setting mortar composition of the present invention contains an alkali metal carbonate and lime together with amorphous aluminum hydroxide, due to the synergistic effect of these three components in improving the rapid-setting property, the total content of amorphous aluminum hydroxide, alkali metal carbonate and lime is preferably 0.2 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and even more preferably 1 to 2 parts by mass, per 100 parts by mass of hydraulic cement.
[0029] (alkali metal hydroxides) The rapid-setting mortar composition of the present invention can further increase the rapid-setting property by further containing an alkali metal hydroxide. Examples of the alkali metal hydroxide include LiOH, NaOH, and KOH. The alkali metal hydroxide may be contained alone or in combination of two or more kinds.
[0030] When the rapid-setting mortar composition of the present invention contains an alkali metal hydroxide, the content of the alkali metal hydroxide is preferably in the range of 0.2 to 1 in terms of mass ratio to the amorphous aluminum hydroxide.
[0031] (alkali metal silicate) The rapid-hardening mortar composition of the present invention can further increase the rapid-hardening property by further containing an alkali metal silicate. Examples of the alkali metal silicate include lithium silicate, sodium silicate, and potassium silicate. The alkali metal silicate may be contained alone or in combination of two or more kinds.
[0032] Examples of alkali metal silicates include aqueous solutions, granular products, and powder products of alkali metal orthosilicates, alkali metal sesquisilicates, alkali metal metasilicates, alkali metal silicates No. 1, alkali metal silicates No. 2, alkali metal silicates No. 3, and alkali metal silicates No. 4. Among these, alkali metal orthosilicates with high alkalinity are preferred from the viewpoint of their high effect of increasing reactivity, and sodium orthosilicate is more preferred.
[0033] When the rapid-setting mortar composition of the present invention contains an alkali metal silicate, the content of the alkali metal silicate is preferably in the range of 0.2 to 1 in terms of mass ratio to the amorphous aluminum hydroxide.
[0034] (Other additives) The fast-hardening mortar composition of the present invention may further contain a thickener as another additive. Examples of thickeners include cellulose ethers such as methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, hydroxyethyl ethyl cellulose, and carboxymethyl cellulose; acrylic polymers such as polyacrylamide, sodium polyacrylate, polyacrylamide-sodium polyacrylate copolymers, and partial hydrolysates of polyacrylamide; and water-soluble polymers such as polyvinyl alcohol, polyethylene oxide, sodium alginate, casein, and natural polysaccharide derivatives. These thickeners may be contained alone or in combination of two or more kinds.
[0035] Furthermore, the fast-hardening mortar composition of the present invention may contain additives such as a defoamer, a hardening retarder, and a water reducing agent.
[0036] Examples of the defoaming agent include higher alcohol-based, alkylphenol-based, diethylene glycol-based, dibutyl phthalate-based, water-insoluble alcohol-based, tributyl phosphate-based, polyglycol-based, silicone-based, and polyether-based defoaming agents such as ethylene oxide-propylene oxide copolymers. These defoaming agents may be contained alone or in combination of two or more.
[0037] As the water-reducing agent, it is preferable to use a high-performance water-reducing agent with excellent water-reducing performance, and examples thereof include water-reducing agents mainly composed of naphthalene sulfonate-formaldehyde condensate, lignin sulfonate or its derivatives, melamine formalin condensate (sulfonate, (modified) methylol), polycarboxylic acid, aminosulfonic acid, and polyether. Here, the "main component" refers to a component that usually accounts for 50% by mass or more of the total, preferably 70% by mass or more, and more preferably 90% to 100% by mass. These water reducing agents may be contained alone or in combination of two or more.
[0038] Examples of the hardening retarder include organic carboxylic acids (salts), such as oxycarboxylic acids such as citric acid, gluconic acid, tartaric acid, malic acid, lactic acid, glucoheptonic acid, oxymalonic acid, mucic acid, glucuronic acid, and lactobionic acid, and alkali metal salts (lithium salt, sodium salt, potassium salt, etc.) and ammonium salts of these oxycarboxylic acids. Examples of the hardening retarder include aminocarboxylic acids such as glutamic acid, and alkali metal salts (lithium salt, sodium salt, potassium salt, etc.) and ammonium salts of these aminocarboxylic acids. Among these, oxycarboxylic acids and / or their salts are preferred from the viewpoint of the rise in gel strength immediately after gelation, and citric acid, sodium salt of citric acid, gluconic acid, and sodium salt of gluconic acid are particularly preferred. These cure retarders may be contained alone or in combination of two or more.
[0039] Furthermore, the fast-setting mortar composition of the present invention may contain a sulfate such as sodium sulfate, potassium sulfate, or aluminum sulfate as a sulfate ion source. Furthermore, the fast-hardening mortar composition of the present invention may contain fibers. The inclusion of fibers can suppress the occurrence of cracks due to the shrinkage or movement of the material. Examples of fibers include polyvinyl alcohol fibers, polypropylene fibers, polyethylene fibers, polyester fibers, aramid fibers, glass fibers, steel fibers, and carbon fibers. The length of the fibers is preferably 0.1 to 40 mm, more preferably 1 to 30 mm, and even more preferably 3 to 10 mm. Longer fibers are preferable from the viewpoint of improving the crack generation suppression performance, while shorter fibers are preferable from the viewpoint of increasing the flowability. Furthermore, clay minerals such as toticlay and bentonite may be contained. The inclusion of clay minerals increases the thixotropy, making it easier to extrude and improving the shape retention performance after extrusion.
[0040] [Mortar flow value before and after impact] The fast-setting mortar composition of the present invention is characterized in that the flow values before and after impact measured in the flow test specified in JIS R5201:2015 (Physical testing methods for cement) for the fast-setting mortar composition immediately after preparation are specific values as follows: Here, "the rapid-setting mortar composition immediately after preparation" refers to the rapid-setting mortar composition of the present invention immediately after all of the components constituting the rapid-setting mortar composition are mixed, and "immediately" refers to within 10 seconds after all of the components are mixed. There is no particular restriction on the order of mixing the materials when preparing the rapid-setting mortar composition of the present invention, but generally, as shown in the examples below, the composition is prepared by adding and mixing amorphous aluminum hydroxide, which is a minor component, to a mixture (mortar) of hydraulic cement, aggregate, and water, and therefore "immediately after preparation" usually means immediately after adding and mixing amorphous aluminum hydroxide to a mixture (mortar) of hydraulic cement, aggregate, and water. It is preferable that other additives are mixed in advance into the mixture (mortar) of hydraulic cement, aggregate, and water. Usually, the mixture of hydraulic cement, aggregate, and other additives is kneaded with water to prepare the mortar. As for alkali metal carbonate, since its fluidity decreases when mixed with hydraulic cement, it is usually added and mixed together with amorphous aluminum hydroxide to a mixture of hydraulic cement, aggregate, and water, and therefore the time immediately after addition and mixing is immediately after preparation. As for lime, since the fluidity does not decrease when it is mixed with hydraulic cement, it may be mixed in advance into the mixture (mortar) of hydraulic cement, aggregate, and water, or it may be mixed together with amorphous aluminum hydroxide gel. From the viewpoint of improving mixing, it is preferable to mix it in advance into the mixture (mortar) of hydraulic cement, aggregate, and water. As for alkali metal hydroxides and alkali metal silicates, their fluidity decreases when they are mixed with hydraulic cement, and therefore they are usually added and mixed together with amorphous aluminum hydroxide to a mixture of hydraulic cement, aggregate, and water, and therefore the time immediately after addition and mixing is immediately after preparation. The flow value can be measured using a commercially available flow value measuring device specified in JIS R5201:2015 (Physical testing methods for cement).
[0041] (Flow value before impact) In the flow test specified in JIS R5201:2015, before 15 strikes in 15 seconds, i.e., at zero strikes, the spread of the mortar at the bottom when the flow cone is lifted vertically (diameter: the average value of the direction recognized as the maximum and its right angle) is measured. When this value is 100 to 120 mm, it becomes possible to self-support while maintaining the shape after extrusion from the nozzle of the 3D printer. From the viewpoint of self-support, the flow value before striking is preferably 100 to 120 mm.
[0042] (Mortar flow value after impact) In the flow test specified in JIS R5201:2015, the handle is rotated 15 times in 15 seconds (15 impacts) as specified, and the flow table is raised and lowered to measure the spread of the specified amount of mortar (diameter: the average value in the direction recognized as maximum and at a right angle thereto). When this value is 135 to 250 mm, fluidity is ensured and extrusion from the nozzle of a 3D printer is possible. From the viewpoint of fluidity, the flow value after impact is preferably 135 to 250 mm.
[0043] [Method for preparing fast-hardening mortar composition] The above-mentioned components can be mixed to prepare the fast-setting mortar composition of the present invention by adding the components in desired amounts to a general mixer and mixing them together. The mixer may be fixed in a factory or on a construction site, or may be mounted on a mixer truck. It is preferable that each component is thoroughly mixed.
[0044] [Effects] According to the present invention, a fast-setting mortar composition is obtained which contains hydraulic cement, aggregate, water, and amorphous aluminum hydroxide, and in measurement of the flow value specified in JIS R5201 immediately after preparation, the flow value before impact is 100 to 120 mm and the flow value after impact is 135 to 250 mm. This means that immediately after mixing, the composition is soft enough to be extruded from the nozzle of a 3D printer, but quickly develops high strength after extrusion. Furthermore, by containing an alkali metal carbonate or lime together with amorphous aluminum hydroxide, or by containing an alkali metal carbonate and lime, a fast-hardening mortar composition that develops high strength more quickly can be obtained.
[0045] That is, since the flow value after impact is 135 to 250 mm, the fast-hardening mortar composition of the present invention can be extruded from the nozzle of a 3D printer. Furthermore, since the flow value before impact is 100 to 120 mm, it is possible to maintain the shape after extrusion. After extrusion, strength can be developed quickly due to the action of amorphous aluminum hydroxide, and further alkali metal carbonate and / or lime. EXAMPLES
[0046] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to these examples.
[0047] [material] Hydraulic cement: Ordinary Portland cement (manufactured by UBE Mitsubishi Cement Co., Ltd.) Aggregate: Tohoku silica sand No. 5 (50% particle size: approx. 0.525 mm) Water: Tap water Amorphous aluminum hydroxide: dried aluminum hydroxide gel powder (median diameter: 84 μm) (product name: AD200P (manufactured by Tomita Pharmaceutical Co., Ltd.)) Alkali metal carbonate: Soda ash (anhydrous sodium carbonate) (product name: Soda ash light (manufactured by Tokuyama Corporation)) Lime: Special grade slaked lime (Blaine value: 12000 cm 2 / g) (Product name: Special slaked lime (manufactured by Ube Material Industries, Ltd.))
[0048] [Method for preparing fast-hardening mortar composition] The hydraulic cement and sand were mixed and mixed with water and stirred with a spoon until homogenous. Additives such as amorphous aluminum hydroxide were added in powder form to the obtained mortar, and the mixture was stirred with a spoon for 10 seconds (the stirring time includes the time required for transferring the mixture to a cup and transferring the liquid).
[0049] [Method of measuring consistency] The prepared fast-hardening mortar composition was placed in a 500 mL disc cup with the top cut off, and the needle was dropped into a penetrometer (a JIS K 2220-2013-specified consistency meter and an optional cone were used) 10 minutes after the start of mixing (however, 25 minutes in Comparative Example 1) to measure the consistency. The consistency measurement 10 minutes after the start of mixing is a measurement that simulates the state after extrusion from the nozzle of a 3D printer. The criteria for judging the results were as follows: If the consistency is 100 or more: × If the consistency is less than 100: 〇
[0050] [Flow value measurement before impact] In the flow value measurement method specified in JIS R5201:2015, the rapid-setting mortar composition immediately after preparation (the rapid-setting mortar composition after stirring with the above-mentioned spoon for 10 seconds) was packed into a flow cone, and the diameter of the contact area between the rapid-setting mortar composition and the flow table when the flow cone was removed vertically from the top was measured.
[0051] [Measurement of flow value after impact] In the flow value measurement method specified in JIS R5201:2015, the handle was turned 15 times in 15 seconds for the fast-setting mortar composition immediately after preparation (the fast-setting mortar composition after stirring with the above-mentioned spoon for 10 seconds), and the flow table was moved up and down to measure the spread (diameter) of the specified amount of mortar.
[0052] [Examples 1 to 6 and Comparative Examples 1 to 3] The fast-hardening mortar compositions prepared according to the formulations shown in Table 1 were subjected to measurement and evaluation of consistency and flow value. The results are shown in Table 1.
[0053] [Table 1]
[0054] The following can be seen from Table 1:
[0055] It is clear from Comparative Example 1 that the mortar not containing additives such as amorphous aluminum hydroxide had a high consistency even 25 minutes after preparation, and was so hard that it would collapse when stacked. In contrast, by mixing amorphous aluminum hydroxide as in Example 1, the material is soft enough to be extruded through the nozzle of a 3D printer immediately after mixing, yet hard enough to maintain its shape after extrusion, and within 10 minutes it has hardened enough that it will not collapse even if layered on top. In Examples 2 and 3, by adding soda ash in addition to amorphous aluminum hydroxide, the total amount of amorphous aluminum hydroxide and soda ash added was the same as or less than the amount of amorphous aluminum hydroxide added in Example 1, and thus the mixture became hard enough 10 minutes after preparation that it would not collapse even if stacked on top of one another. Also, although the hardness after 10 minutes was harder than that of amorphous aluminum hydroxide alone, the flow value after impact was large, and it is clear that the fluidity immediately after mixing was better than that of Example 1, which used amorphous aluminum hydroxide alone. In Example 4, when slaked lime was added in addition to amorphous aluminum hydroxide, the material became hard enough that it would not collapse even if a layer was placed on top of it after 10 minutes, despite the small amount of amorphous aluminum hydroxide. In Example 5, soda ash and hydrated lime were added to the amorphous aluminum hydroxide, and even with a smaller amount of amorphous aluminum hydroxide, it became hard enough that it would not collapse even when stacked on top after 10 minutes. In Comparative Examples 2 and 3, amorphous aluminum hydroxide was contained in mortar with a large amount of water, but the flow value before impact was large and the shape could not be maintained after being extruded from the nozzle. In Comparative Example 4, the mortar had a low water content, and although the shape was maintained from the flow value before striking, there was no significant change in the flow value after striking, which indicates that it was difficult to extrude from the nozzle. [Industrial Applicability]
[0056] The fast-hardening mortar composition of the present invention has excellent initial fluidity (injectability), early hardening, and self-supporting properties, and is useful as a cement mortar composition for 3D printers in the construction of civil engineering works, buildings, etc.
Claims
1. A rapid-setting mortar composition comprising hydraulic cement, aggregate, water, and amorphous aluminum hydroxide, the rapid-setting mortar composition having a flow value immediately after preparation, measured in a flow test specified in JIS R5201:2015, of 100 to 120 mm before impact and a flow value of 135 to 250 mm after impact.
2. The fast-hardening mortar composition according to claim 1, further comprising an alkali metal carbonate.
3. The fast-hardening mortar composition according to claim 1 or 2, further comprising lime.
Citation Information
Patent Citations
Cement admixture capsule
JP2001348257A
Three-dimensional modeling cement composition for construction, and three-dimensional modeling method for construction
JP2018140906A
Quick setting admixture, quick setting admixture solution, chemical solution for soil stabilization, manufacturing method of chemical solution thereof, and ground stabilization method
JP2021042088A
Cited By
Castable refractories and precast blocks
JP7834229B1