Negative photosensitive resin composition, dry film, cured product, and electronic component

A controlled ratio of acid crosslinkable groups in a polyhydroxyamide-based resin composition improves substrate adhesion and elongation, addressing peeling and cracking issues, enabling fine patterns for semiconductor applications.

JP2024165942APending Publication Date: 2024-11-28TAIYO HOLDINGS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023082552
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing negative photosensitive resin compositions used for semiconductor applications suffer from insufficient elongation and adhesion to substrates, leading to issues such as peeling and cracking of the cured products.

Method used

A negative photosensitive resin composition incorporating a polyhydroxyamide compound, a photoacid generator, a crosslinking agent with an acid crosslinkable group, and a polyrotaxane, where the ratio of acid crosslinkable groups to the total hydroxyl groups is carefully controlled to enhance elongation and adhesion.

Benefits of technology

The composition provides cured products with excellent elongation and adhesion to substrates, enabling the formation of fine and high aspect ratio patterns, suitable for semiconductor devices and printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165942000001
    Figure 2024165942000001
  • Figure 2024165942000002
    Figure 2024165942000002
  • Figure 2024165942000003
    Figure 2024165942000003
Patent Text Reader

Abstract

To provide a negative photosensitive resin composition which can give a cured product excellent in elongation and excellent in adhesion to a substrate.SOLUTION: The negative photosensitive resin composition contains (A) a polyhydroxyamide compound containing a structural unit represented by formula (1), (B) a photoacid generator, (C) a crosslinking agent containing acid-crosslinkable groups, and (D) a polyrotaxane in which a cyclic molecule is modified with a graft chain having a hydroxy group at a terminal. The ratio of the number of moles of the acid-crosslinkable groups contained in the (C) to the total number of moles of hydroxy groups contained in the (A) and the hydroxy group at the terminal of the graft chain of the (D) is less than 1.5.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative photosensitive resin composition, a dry film, a cured product, and an electronic component. [Background technology]

[0002] Photosensitive resin compositions containing polybenzoxazole precursors exhibit excellent properties such as insulating properties, heat resistance, and mechanical strength, and are therefore widely used as insulating films in various fields such as semiconductors and electronic components.

[0003] In the past, there has been a demand for higher integration of semiconductor elements in response to the demand for higher performance and smaller size of electronic components and electrical equipment. In recent years, in order to meet these demands, technologies for higher performance and smaller size in the field of semiconductor element packaging, such as wafer level packaging (WLP), have been developed, and there is an increasing demand for finer pattern formation (resolution) in the insulating film used in the redistribution layer.

[0004] Regarding negative-type photosensitive resin compositions that enable the formation of fine patterns, negative-type photosensitive resin compositions containing a polyhydroxyamide compound as a polybenzoxazole precursor have been proposed (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2001-125267 A [Patent Document 2] JP 2008-033159 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0006] However, when the above-mentioned negative photosensitive resin composition is used, the cured product formed from the composition has insufficient elongation and adhesion to a substrate, and there is a risk of problems such as peeling or cracking of the cured product.

[0007] An object of the present disclosure is to provide a negative-type photosensitive resin composition capable of producing a cured product having excellent elongation and adhesion to a substrate. Another object of the present disclosure is to provide a cured product using the negative-type photosensitive resin composition, and electronic parts such as printed wiring boards and semiconductor elements using the same. [Means for solving the problem]

[0008] The present inventors have found that the above-mentioned problems can be solved by blending a polyrotaxane (hereinafter also referred to as a "specific polyrotaxane") in which a cyclic molecule is modified by a graft chain having a hydroxy group at an end into a negative photosensitive resin composition containing a polyhydroxyamide compound containing a structural unit represented by formula (1) described below (hereinafter also referred to as a "specific polyhydroxyamide compound"), a photoacid generator, and a crosslinking agent containing an acid crosslinking group (hereinafter also referred to as a "specific crosslinking agent") such that the number of moles of the acid crosslinking group of the specific crosslinking agent relative to the total number of moles of the hydroxy groups of the specific polyhydroxyamide compound and the number of moles of the hydroxy groups at the ends of the graft chains of the specific polyrotaxane falls within a predetermined range, and have completed the present invention.

[0009] The gist of the present invention is as follows. [1] (A) a polyhydroxyamide compound containing a structural unit represented by the following formula (1): (B) a photoacid generator, (C) a crosslinking agent containing an acid crosslinking group, and (D) a polyrotaxane having a cyclic molecule modified with a graft chain having a hydroxyl group at its terminal, the ratio of the number of moles of the acid crosslinkable groups contained in (C) to the sum of the number of moles of the hydroxy groups contained in (A) and the number of moles of the hydroxy groups at the graft chain terminals of (D) is less than 1.5; A negative photosensitive resin composition. [ka] (In the formula, R 1 is a divalent organic group, R 2 is a tetravalent organic group.

[0010] [2] The negative photosensitive resin composition according to [1], wherein the amount of the (D) is 3 to 30 parts by mass per 100 parts by mass of the (A).

[0011] [3] The negative photosensitive resin composition according to [2], wherein the amount of the (D) is 3 to 10 parts by mass per 100 parts by mass of the (A).

[0012] [4] The negative photosensitive resin composition according to any one of [1] to [3], wherein the acid crosslinkable group is an alkoxymethyl group, a methylol group, or an epoxy group.

[0013] [5] The negative photosensitive resin composition according to any one of [1] to [4], wherein (B) is an oxime sulfonate compound.

[0014] [6] The negative type photosensitive resin composition according to any one of [1] to [5], further comprising (E) a basic compound.

[0015] [7] A dry film comprising a resin layer formed from the negative photosensitive resin composition according to any one of [1] to [6].

[0016] [8] A cured product of the negative photosensitive resin composition according to any one of [1] to [6].

[0017] [9] An electronic component having the cured product according to [8]. Effect of the Invention

[0018] According to the disclosed technique, it is possible to provide a negative type photosensitive resin composition that can give a cured product that has excellent elongation and adhesion to a substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, embodiments of the present disclosure will be described in detail. In this specification, the expression "a to b" in the description of a numerical range means a to b, unless otherwise specified.

[0020] 1. Negative-type photosensitive resin composition The negative type photosensitive resin composition of the present disclosure contains (A) a polyhydroxyamide compound having a structural unit represented by the following formula (1) ((A) specific polyhydroxyamide compound), (B) a photoacid generator, (C) a crosslinking agent containing an acid crosslinkable group ((C) specific crosslinking agent), and (D) a polyrotaxane in which a cyclic molecule is modified with a graft chain having a hydroxy group at an end ((D) specific polyrotaxane).

[0021] 1-1.(A) Specific polyhydroxyamide compounds (A) The specific polyhydroxyamide compound contains a structural unit represented by the following formula (1): [ka] (In the formula, R 1 is a divalent organic group, R 2 is a tetravalent organic group.

[0022] R in formula (1) 1 is not particularly limited as long as it is a divalent organic group, and examples thereof include an alkylene group, a cycloalkylene group, an arylene group, a heteroarylene group, a ketone group, an ester group, an amide group, etc., and may be a combination of two or more of these, or a combination of one or more of these with an ether group, a thioether group, a sulfonyl group, a sulfinyl group, etc. The divalent organic group may have a fluorine atom as a substituent. Here, the organic group refers to a functional group containing at least one carbon atom.

[0023] For example, R 1may be a divalent aromatic hydrocarbon group having a skeleton such as benzene, naphthalene, perylene, biphenyl, diphenyl ether, diphenyl sulfone, diphenylpropane, diphenylhexafluoropropane, or benzophenone, or a divalent aliphatic hydrocarbon group having a skeleton such as butane or cyclobutane. From the viewpoint of forming fine and high aspect ratio patterns of negative photosensitive resin compositions, R 1 The number of carbon atoms of R is preferably 4 to 30. 1 Examples include the following: [ka] (where A is a single bond, -CH 2 -, -O-, -CO-, -S-, -SO 2 -, -NHCO-, -C(CF 3 ) 2 - or -C(CH 3 ) 2 -It is.)

[0024] (A) A specific polyhydroxyamide compound has multiple R 1 If it contains multiple R 1 may be the same or different.

[0025] R in formula (1) 2 is not particularly limited as long as it is a tetravalent organic group, and can be, for example, a tetravalent residue having a skeleton of an alkane, a cycloalkane, an arene, a heteroarene, etc. These residues may have an ether group, a thioether group, a ketone group, a sulfonyl group, a sulfinyl group, an ester group, an amide group, etc., and may have a fluorine atom as a substituent. For example, R 2 is preferably a tetravalent aromatic hydrocarbon group having a skeleton such as benzene, biphenyl, diphenyl ether, diphenyl thioether, benzophenone, diphenylmethane, diphenylpropane, diphenylhexafluoropropane, diphenyl sulfoxide, diphenyl sulfone, etc. These may have a fluorine atom as a substituent.

[0026] From the viewpoint of forming a fine and high aspect ratio pattern of the negative photosensitive resin composition, a preferable R 2 Examples include the following: [ka] (In the formula, a is an integer of 0 to 3, and preferably 0.)

[0027] (A) A specific polyhydroxyamide compound has multiple R 2 If it contains multiple R 2 may be the same or different.

[0028] The terminal structure of the specific polyhydroxyamide compound (A) is not particularly limited, and examples thereof include terminal structures having functional groups such as amino groups, alcoholic hydroxyl groups, phenolic hydroxyl groups, acid anhydride groups, carboxyl groups, and isocyanate groups. From the viewpoint of solubility in a developer, the terminal structure is preferably a carboxyl group or a phenolic hydroxyl group, and more preferably a phenolic hydroxyl group. The terminal structure may be introduced by a terminal blocking agent.

[0029] The weight average molecular weight (Mw) of the (A) specific polyhydroxyamide compound is not particularly limited and can be from 2,000 to 20,000, and from the viewpoint of forming a fine pattern with a high aspect ratio, it is preferably from 3,000 to 15,000. The number average molecular weight (Mn) of the (A) specific polyhydroxyamide compound is preferably from 1,000 to 10,000, and more preferably from 1,500 to 6,000. The polydispersity index (PDI) of the (A) specific polyhydroxyamide compound is preferably from 1.5 to 4.0, and more preferably from 1.5 to 3.5.

[0030] In this specification, the weight average molecular weight and the number average molecular weight are values ​​measured by gel permeation chromatography (GPC) (GL7700 manufactured by GL Science) and converted into standard polystyrene. Specific measurement conditions are as follows. Column: TSKgel αM (Tosoh Corporation) Column temperature: 40℃ Eluent composition: 100mmol / L H 3 PO 4 (H 3 PO 4 85% aqueous solution was used as the raw material) and NMP solution containing 10mmol / L LiBr Eluent flow rate: 0.5mL / min Calibration standard: Polystyrene Detector wavelength: 260nm and 300nm Detector temperature: Room temperature Baseline range at analysis: 15 to 40 minutes Molecular weight calculation range during analysis: 20 to 35 minutes In this specification, the polydispersity index (PDI) is calculated by the following formula (4). PDI=Mw / Mn (4)

[0031] The hydroxyl equivalent of the specific polyhydroxyamide compound (A) is not particularly limited from the viewpoint of forming a fine pattern with a high aspect ratio, but may be, for example, 100 to 400 g / eq, preferably 150 to 350 g / eq, and more preferably 200 to 300 g / eq. In the present disclosure, the hydroxyl equivalent of the polyhydroxyamide compound means a theoretical hydroxyl equivalent calculated from the number average molecular weight measured by the above-mentioned method and the molecular weight of the repeating unit structure.

[0032] The specific polyhydroxyamide compound (A) may be used alone or in any combination of two or more kinds in any ratio.

[0033] 1-2.(B) Photoacid generator (B) photoacid generator is not particularly limited as long as it generates an acid by irradiation (exposure) of radiation. For example, diazomethane compounds, onium salt compounds, sulfonimide compounds, disulfone compounds, sulfonic acid derivative compounds, nitrobenzyl compounds, benzoin tosylate compounds, iron arene complexes, halogen-containing triazine compounds, acetophenone derivative compounds, cyano group-containing oxime sulfonate compounds, etc. can be mentioned. (B) photoacid generator can adjust the solubility of the photosensitive resin composition in an alkaline developer.

[0034] From the viewpoint of forming a fine pattern with a high aspect ratio, the photoacid generator (B) is preferably an oxime sulfonate compound, which, when irradiated (exposed) to radiation, breaks the sulfonate ester bond and generates sulfonic acid.

[0035] The oxime sulfonate compound is preferably a cyano group-containing oxime sulfonate compound, and particularly preferably one having a structure represented by the following formula (2). [ka] X in the formula (2) is not particularly limited, and examples thereof include a hydrocarbon group (e.g., an alkyl group, an alkenyl group, an alkynyl group, an aryl group, etc.) and a halogen atom (e.g., a chlorine atom, a fluorine atom, etc.). The hydrocarbon group may have a substituent. Here, the hydrocarbon group may be any of linear, branched, and cyclic, and may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. X is preferably a linear or branched hydrocarbon group having 1 to 4 carbon atoms. When X is a halogen atom, it is preferably a chlorine atom or a fluorine atom.

[0036] In formula (2), m represents an integer of 0 to 3, and is preferably 0 or 1. When m is 2 or 3, multiple Xs may be the same or different.

[0037] R in Equation (2) 3is not particularly limited, and may be, for example, a hydrogen atom, a hydrocarbon group, an organic group including a ketone group, or a halogen atom. The hydrocarbon group (e.g., an alkyl group, an alkenyl group, an alkynyl group, an aryl group, etc.) may be unsubstituted or may be substituted with a halogen atom. The hydrocarbon group is preferably a straight-chain, branched-chain or cyclic group having 1 to 20 carbon atoms, and more preferably a straight-chain, branched-chain or cyclic group having 1 to 10 carbon atoms. The halogen atom is preferably a chlorine atom or a fluorine atom.

[0038] Commercially available oxime sulfonate compounds include Irgacure PAG103, Irgacure PAG108, Irgacure PAG121, and Irgacure PAG203 manufactured by BASF.

[0039] As the (B) photoacid generator, a sulfonium salt compound, an iodonium salt compound, a naphthalimide compound, a diazonium salt compound, an onium salt compound, a sulfonate compound, a carboxylate compound, a nitrobenzyl ester compound, an N-oxyimide sulfonate compound, and the like can also be used.

[0040] (B) The photoacid generator may be used alone or in any combination of two or more kinds in any ratio.

[0041] 1-3. (C) Crosslinking agent containing acid crosslinking group The (C) crosslinking agent containing an acid crosslinkable group (hereinafter also referred to as "(C) specific crosslinking agent") is not particularly limited as long as it is an agent that reacts with the hydroxy groups of the (A) specific polyhydroxyamide compound and the hydroxy groups (particularly the hydroxy groups on the graft chains) of the (D) specific polyrotaxane by the action of the acid generated by the (B) photoacid generator to form a crosslinked structure.

[0042] (C) Examples of the acid crosslinkable group of the specific crosslinking agent include an alkoxymethyl group (e.g., a methoxymethyl group, etc.), a methylol group (-CH 2—OH), epoxy, oxetane, episulfide, etc., and preferred are methoxymethyl and methylol groups.

[0043] (C) The specific crosslinking agent preferably contains a heterocycle from the viewpoint of obtaining a cured product having excellent elongation and adhesion to a substrate. The heterocycle is not particularly limited, and contains one or more heteroatoms such as boron, nitrogen, oxygen, phosphorus, sulfur, antimony, arsenic, bismuth, selenium, silicon, tellurium, and tin, and contains a 3-, 4-, 5-, 6-, 7-, or 8-membered saturated or unsaturated ring. From the viewpoint of obtaining a cured product having excellent elongation and adhesion to a substrate, the heterocycle is preferably a nitrogen-containing heterocycle, and more preferably a heterocycle containing multiple nitrogen atoms. Specifically, compounds having a triazine structure such as hexamethylolmelamine and hexamethoxymethylmelamine, compounds having a guanamine structure such as tetramethylolbenzoguanamine and tetramethoxymethylbenzoguanamine, compounds having a glycoluril structure such as tetramethylolglycoluril and tetramethoxyglycoluril, and compounds having an imidazolidinone structure such as 1,3-bis(methoxymethyl)-2-imidazolidinone are more preferred. Among these, compounds having a triazine structure containing a triazine ring and compounds having a guanamine structure are preferably used from the viewpoint of obtaining a cured product having excellent elongation and adhesion to a substrate.

[0044] (C) As the specific crosslinking agent, an epoxy compound, an oxetane compound, an episulfide compound, etc. can also be used.

[0045] (C) The specific crosslinking agent may be used alone or in any combination of two or more in any ratio.

[0046] 1-4.(D) Polyrotaxane with cyclic molecules modified by graft chains having hydroxyl groups at the termini In the negative type photosensitive resin composition of the present disclosure, when irradiated with radiation (exposure), the photoacid generator (B) generates an acid, which causes the specific crosslinking agent (C) to react with the hydroxyl group of the specific polyhydroxyamide compound (A) and the hydroxyl group on the graft chain of the specific polyrotaxane (D) to generate a crosslinked structure. The crosslinked structure includes a structure in which the specific polyhydroxyamide compounds (A) are bonded together via the specific polyrotaxane (D), and forms flexible crosslinking points, which is presumed to provide excellent elongation to the cured product obtained from the composition and improve adhesion to the substrate.

[0047] Polyrotaxane is a compound having a linear molecule that includes multiple cyclic molecules in a skewered shape, and a blocking group that is arranged at the end of the linear molecule and prevents the cyclic molecules from detaching. In polyrotaxane, the cyclic molecules can move freely on the linear molecule, but the blocking group prevents them from escaping from the linear molecule. (D) In ​​a specific polyrotaxane, the cyclic molecules are modified by graft chains that have hydroxyl groups at their ends.

[0048] The linear molecule is not particularly limited as long as it has a functional group that penetrates the opening of the cyclic molecule and can react with the block group. For example, polyalkylene glycols such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; polybutadiene diol, polyisoprene diol, polyisobutylene diol, poly(acrylonitrile-butadiene) diol, hydrogenated polybutadiene diol, polyethylene diol, and polypropylene diol, terminal hydroxyl group polyolefins; polycaprolactone diol, polylactic acid, polyethylene adipate, polybutylene adipate, polyethylene terephthalate, and polybutylene terephthalate, polyesters; terminal functional polysiloxanes such as terminal silanol type polydimethylsiloxane; terminal amino group polyethylene glycol, terminal amino group polypropylene glycol, and terminal amino group polybutadiene, terminal amino group chain polymers; and trifunctional or more multifunctional chain polymers having three or more of the above functional groups in one molecule. Among these, polyethylene glycol and amino-terminated polyethylene glycol are preferably used from the viewpoint of ease of synthesis of polyrotaxane. The weight average molecular weight of the linear molecule can be 1,000 to 100,000, and is preferably 2,000 to 50,000. From the viewpoint of achieving superior elongation of the cured product and adhesion to a substrate, it is more preferably 2,000 to 15,000.

[0049] The blocking group is not particularly limited as long as it can be bonded to the terminal functional group of the linear molecule and is sufficiently bulky so that the cyclic molecule does not leave the linear molecule. For example, dinitrophenyl group, cyclodextrin group, adamantyl group, trityl group, fluoresceinyl group, pyrenyl group, anthracenyl group, main chain or side chain of a polymer having a number average molecular weight of 1,000 to 1,000,000, etc. can be mentioned. The blocking groups at both ends may be the same or different.

[0050] The cyclic molecule is not particularly limited as long as the linear molecule can penetrate the opening. For example, cyclodextrins, crown ethers, cryptands, macrocyclic amines, calixarenes, cyclophanes, etc. are included. Cyclodextrins are compounds in which multiple glucose molecules are linked in a ring shape with α-1,4-bonds. α-cyclodextrin, β-cyclodextrin, and γ-cyclodextrin are more preferred.

[0051] (D) In ​​a specific polyrotaxane, a cyclic molecule is modified by a graft chain having a hydroxy group at the end. For example, it is preferable that a hydroxy group is bonded to the cyclic molecule by a graft chain composed of a polyester. From the viewpoint of compatibility with other components and solubility in organic solvents, the polyester is more preferably an aliphatic polyester, such as polylactic acid, polyglycolic acid, poly3-hydroxybutyrate, poly4-hydroxybutyrate, poly(3-hydroxybutyrate / 3-hydroxyvalerate), poly(ε-caprolactone), etc., and among them, poly(ε-caprolactone) is more preferable. The cyclic molecule may be entirely or partially modified with a graft chain having a hydroxy group at its terminal.

[0052] The hydroxyl value of the (D) specific polyrotaxane can be 20 to 200 mgKOH / g, and is preferably 50 to 150 mgKOH / g. In the present disclosure, the hydroxyl value of the polyrotaxane refers to the amount of active hydroxyl groups measured in accordance with JIS K0070-1992. In the (D) specific polyrotaxane, the hydroxyl group at the end of the graft chain is the active hydroxyl group.

[0053] Preferred specific polyrotaxanes (D) include the following: [ka] In formula (5), The thick line indicates the cyclodextrin structure. The dashed lines represent polyalkylene glycol chains. R a is an alkylene group having 1 to 18 carbon atoms, R b is an alkylene group having 1 to 18 carbon atoms, R c is an alkylene group having 1 to 10 carbon atoms, Rd is a monovalent organic group having an adamantyl group. Re is a monovalent organic group having an adamantyl group, p is 1 or greater, q is 1 or greater; r is greater than or equal to 1.

[0054] (D) The specific polyrotaxane may be a single one or a combination of two or more kinds in any ratio.

[0055] 1-5.(E) Basic compounds The negative type photosensitive resin composition of the present disclosure preferably contains a (E) basic compound from the viewpoints of improving dissolution contrast and resolution, and improving the stability of the coating film during the waiting time from when the photosensitive resin composition is applied until when it is exposed to light.

[0056] (E) The basic compound is not particularly limited, and examples thereof include amine compounds such as trimethylamine, diethylamine, triethylamine, di-n-propylamine, tri-n-propylamine, tri-n-pentylamine, tribenzylamine, diethanolamine, triethanolamine, n-hexylamine, n-heptylamine, n-octylamine, n-nonylamine, ethylenediamine, N,N,N',N'-tetramethylethylenediamine, tetramethylenediamine, hexamethylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylether, 4,4'-diaminobenzophenone, and 4,4'-diaminodiphenylamine; formamide, N-methylformamide, N,N-dimethylformamide, and amine compounds such as dimethylformamide, diethyl ... Examples of the compound include amide compounds such as cetoamide, N-methylacetamide, N,N-dimethylacetamide, propionamide, and benzamide; lactams such as pyrrolidone and N-methylpyrrolidone; urea compounds such as methylurea, 1,1-dimethylurea, 1,3-dimethylurea, 1,1,3,3-tetramethylurea, and 1,3-diphenylurea; nitrogen-containing heterocyclic compounds such as imidazole, benzimidazole, 4-methylimidazole, 8-oxyquinoline, acridine, purine, pyrrolidine, piperidine, 2,4,6-tri(2-pyridyl)-S-triazine, piperazine, 1,4-dimethylpiperazine, 1,4-diazabicyclo[2.2.2]octane, and pyridine; and morpholine compounds such as morpholine and 4-methylmorpholine.

[0057] The (E) basic compound may be used alone or in any combination of two or more kinds in any ratio.

[0058] 1-6.(F) Inorganic filler The negative photosensitive resin composition of the present disclosure may contain an inorganic filler. The inorganic filler is not particularly limited, and a conventionally known inorganic filler may be used, for example, silica, aluminum hydroxide, alumina, aluminum nitride, boron nitride, glass powder, magnesium carbonate, barium sulfate, barium titanate, hydrotalcite, etc. These may be used alone or in combination in any ratio. From the viewpoint of excellent insulation reliability and low thermal expansion coefficient of the negative photosensitive resin composition, it is preferable to use silica, and it is particularly preferable to use spherical silica.

[0059] The volume average particle size (D50) of the inorganic filler can be 1.0 μm or less, preferably 500 nm or less, and particularly preferably 100 nm or less. The volume average particle size of the inorganic filler can be measured by a laser diffraction method.

[0060] 1-7.Solvent The negative photosensitive resin composition of the present disclosure may contain a solvent. The solvent is not particularly limited, and examples thereof include 2-methoxy-1-methylethyl acetate (PGMEA), 4-methyl-2-pentanone, γ-butyrolactone, N-methylpyrrolidone, N-methylcaprolactam, dimethyl sulfoxide, tetramethylurea, pyridine, dimethyl sulfone, hexamethyl sulfoxide, ethyl acetate, butyl acetate, ethyl lactate, methyl 3-methoxypropionate, methyl 2-methoxypropionate, ethyl 3-methoxypropionate, ethyl 2-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 2-ethoxypropionate, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ... Examples of the ethyl alcohol include methyl ethyl ether, propylene glycol dimethyl ether, dipropylene glycol dimethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, carbitol acetate, ethyl cellosolve acetate, cyclohexanone, cyclopentanone, methyl ethyl ketone, methyl isobutyl ketone, and 2-heptanone. These can be used alone or in combination of a plurality of them at any ratio. Among them, γ-butyrolactone or cyclopentanone is preferred from the viewpoint of excellent affinity with each component in the negative photosensitive resin composition. In addition, cyclopentanone is particularly preferred from the viewpoint of excellent solvent removability during drying of the negative photosensitive resin composition and compatibility with the edge rinse process in semiconductor manufacturing. The solvent may be used alone or in any combination of two or more in any ratio.

[0061] 1-8.Other ingredients The negative photosensitive resin composition of the present disclosure may contain other components as long as the effects of the present disclosure are not impaired. As the other components, known components that can be contained in negative photosensitive resin compositions can be used, and examples of such components include adhesion agents, surfactants, plasticizers, thermal acid generators, sensitizers, leveling agents, colorants, fibers, fine particles, and phenolic compounds.

[0062] The surfactant is not particularly limited, and examples thereof include fluorosurfactants, silicon-based surfactants, etc. Commercially available fluorosurfactants include the "Megafac" series manufactured by DIC Corporation (e.g., Megafac F-281, F-477, F-553, F-554, F-555, F-556, F-557, F-558, F-559, F-560, F-561, F-563, F-569, etc.). Examples of commercially available silicone surfactants include the BYK Surface Conditioner series (e.g., BYK-302, BYK-307, BYK-310, BYK-322, BYK-323, BYK-326, BYK-331, BYK-332, BYK-333, BYK-348, BYK-349, BYK-377, BYK-378, BY-3455, BYK-3760, etc.). These may be used alone or in any combination of two or more in any ratio.

[0063] 2. Negative-type photosensitive resin composition The negative type photosensitive resin composition of the present disclosure can be obtained by mixing any components including (A) a specific polyhydroxyamide compound, (B) a photoacid generator, (C) a specific crosslinking agent, (D) a specific polyrotaxane, and (E) a basic compound. The mixing of each component can be performed under heating as necessary.

[0064] The amount of the specific polyhydroxyamide compound (A) may be 50 to 80% by mass, assuming that the total mass of the solid content of the negative photosensitive resin composition is 100% by mass. Here, the solid content mass in this specification refers to the mass of the residue after the volatile components have been completely evaporated.

[0065] The blending amount of (B) the photoacid generator can be 0.5 to 20 parts by mass, and preferably 1 to 10 parts by mass, per 100 parts by mass of (A) the specific polyhydroxyamide compound in the negative photosensitive resin composition.

[0066] The number of moles of hydroxyl groups contained in the specific polyhydroxyamide compound (A) in the negative photosensitive resin composition of the present disclosure (X A ) and (D) the mole number of hydroxyl groups on the graft chain of a particular polyrotaxane (X D ) the mole number (X C ) ratio ((Xc / (X A +X D ) is less than 1.5. The lower limit of the ratio is, for example, 0.1 or more, preferably 0.3 or more, and more preferably 0.5 or more. When the ratio is within this range, the cured product produced by irradiation (exposure) with radiation can be imparted with excellent elongation and adhesion to the substrate.

[0067] (D) The mole number of hydroxyl groups on the graft chain of a specific polyrotaxane (X D ) is the number of moles (X) contained in a specific polyhydroxyamide compound (A) A ) can be set to 0.001 to 0.20, and preferably 0.01 to 0.15.

[0068] The amount of the specific polyrotaxane (D) blended is preferably 3 to 30 parts by mass, and more preferably 3 to 10 parts by mass, per 100 parts by mass of the specific polyhydroxyamide compound (A), from the viewpoint of providing excellent elongation to the cured product. When the amount of the specific polyrotaxane (D) is 10 parts by mass or less, it becomes easier to suppress the generation of development residues in unexposed areas after the negative photosensitive resin composition is developed, and it becomes possible to form a fine pattern with a high aspect ratio.

[0069] The amount of the basic compound (E) added may be 0.01 to 0.50 parts by mass, and preferably 0.08 to 0.40 parts by mass, relative to 100 parts by mass of the specific polyhydroxyamide compound (A) in the negative photosensitive resin composition. By setting the amount in this range, it becomes easier to suppress the occurrence of development residues in unexposed areas after the negative photosensitive resin composition is developed.

[0070] The amount of the inorganic filler (F) added may be 1 to 50 parts by mass, and preferably 10 to 40 parts by mass, per 100 parts by mass of the specific polyhydroxyamide compound (A) in the negative photosensitive resin composition. By setting the amount in this range, the cured product of the negative photosensitive resin composition can have a low thermal expansion coefficient while maintaining the developability of the negative photosensitive resin composition.

[0071] A cured product formed from the negative photosensitive resin composition of the present disclosure exhibits good elongation and excellent adhesion to a substrate (for example, a silicon substrate, etc.). In addition, by using the negative type photosensitive resin composition of the present disclosure, it is also possible to form a fine pattern with a high aspect ratio. Specifically, the negative type photosensitive resin composition of the present disclosure can make the line / space (L / S) in the pattern of a semiconductor circuit or a circuit board less than 4 μm / 4 μm, and can also make it 3.0 μm / 3.0 μm or less, or even 2.0 μm / 2.0 μm or less. In addition, the aspect ratio (line height / line width) can be made 1.5 or more, and can also be made 3.0 or more.

[0072] 3. Dry film The dry film of the present disclosure includes a substrate and a resin layer formed on the substrate using the negative photosensitive resin composition of the present disclosure. In addition, a protective film may be further laminated on the surface of the resin layer to protect the resin layer.

[0073] The substrate is not particularly limited, but examples thereof include metal foils such as copper foil; and polyester films such as polyimide films, polyethylene terephthalate (PET) films, and polyethylene naphthalate (PEN) films.

[0074] The protective film is not particularly limited, but polyethylene film, polytetrafluoroethylene film, polypropylene film, paper, etc. can be used. It is preferable to select a protective film in which the adhesive strength between the protective film and the resin layer is lower than that between the substrate and the resin layer. In order to make the adhesive strength between the protective film and the resin layer lower than that between the substrate and the resin layer, a protective film having a release treatment applied to its surface can be used.

[0075] The thickness of the resin layer is not particularly limited, but can be 1 to 150 μm depending on the application. The resin layer can be obtained, for example, by applying a negative photosensitive resin composition onto a substrate, adjusting the thickness of the resin layer using a comma coater, a blade coater, a lip coater, a rod coater, a squeeze coater, a reverse coater, a transfer roll coater, a gravure coater, a spray coater, or the like, and drying the resin layer.

[0076] 4.Cured product The cured product of the present disclosure is obtained by curing the resin layer of the negative photosensitive resin composition or dry film of the present disclosure. The cured product may be a patterned cured product. Examples of the method for producing the patterned cured product include the following method.

[0077] 4-1. Dry coating film formation process The dry coating film forming step is a step of applying the negative photosensitive resin composition of the present disclosure onto a substrate to form a coating film, and then drying the coating film. In the dry coating film forming step, a resin layer of a dry film can be transferred onto the substrate to form a dry coating film on the substrate.

[0078] The method of applying the negative photosensitive resin composition onto a substrate is not particularly limited, and examples thereof include a method of applying using a spin coater, a bar coater, a blade coater, a curtain coater, a screen printer, etc., a spray application method using a spray coater, an inkjet method, etc. The thickness of the applied film is not particularly limited, and can be, for example, 10 μm or less, 5 μm or less, or 3 μm or less. By reducing the film thickness, finer L / S patterning is possible while maintaining the aspect ratio of the pattern.

[0079] The method for drying the coating film is not particularly limited, and examples thereof include air drying, heat drying in an oven or a hot plate, vacuum drying, etc. Conditions for heat drying are, for example, a heating temperature of 70 to 140° C. and a drying time of 1 to 30 minutes.

[0080] The transfer of the resin layer of the dry film onto the substrate is preferably carried out under pressure and heat using a vacuum laminator, etc. The heating temperature can be, for example, 60 to 100°C.

[0081] The substrate is not particularly limited, and may be, for example, a printed wiring board on which a circuit is formed, a flexible printed wiring board, or a wafer on which a semiconductor element is formed.

[0082] 4-2. Exposure process The exposure step is a step in which the dried coating film formed in the dry coating film forming step is irradiated with radiation through a photomask capable of forming a desired pattern, thereby sensitizing the photoacid generator (B) in the exposed area and generating active species. If patterning is not required, there is no need to use a photomask. Alternatively, a pattern may be directly drawn with a laser using a direct drawing device.

[0083] The wavelength of the radiation is such that the photoacid generator (B) can be activated, and in order to perform fine patterning, the maximum wavelength is preferably 410 nm or less. The irradiation energy can be adjusted depending on the thickness of the formed dry coating film, and is, for example, 10 to 1000 mJ / cm. 2As the exposure light source, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, a KRF laser, or the like can be used.

[0084] 4-3.PEB process The Post Exposure Bake (PEB) process is a process in which the dried coating film exposed in the exposure process is heat-treated to impart development resistance to the exposed portion of the dried coating film (hereinafter, sometimes abbreviated as the exposed portion). In the PEB process, a crosslinking reaction between a specific polyhydroxyamide compound (A) or a specific polyrotaxane (D) and a specific crosslinking agent (C) proceeds in the exposed portion using an acid generated by a photoacid generator (B) as an active species, and the exposed portion becomes insoluble in a developer. The heating temperature in the PEB process can be 90 to 150°C, and the heating time can be 0.5 to 10 minutes. Heating can be performed by a known method such as a hot plate or a heating furnace.

[0085] 4-4.Developing process The developing step is a step in which the dried coating film heated in the PEB step is treated with a developer to dissolve and remove the unexposed areas of the dried coating film in the developer, thereby obtaining a patterned coating film. As the developing method, a known method can be used, for example, a rotary spray method, a paddle method, a dipping method accompanied by ultrasonic treatment, etc.

[0086] The developer may be a known one, and examples of the developer include aqueous solutions of inorganic alkalis such as sodium hydroxide, sodium carbonate, sodium silicate, and aqueous ammonia, organic amines such as ethylamine, diethylamine, triethylamine, and triethanolamine, and quaternary ammonium salts such as tetramethylammonium hydroxide and tetrabutylammonium hydroxide, etc. If necessary, a water-soluble organic solvent such as methanol, ethanol, and isopropyl alcohol, or a surfactant may be added.

[0087] After the treatment with the developer, the coating film can be washed with a rinse liquid as necessary to obtain a patterned coating film. The rinse liquid is not particularly limited, and examples thereof include pure water, methanol, ethanol, isopropyl alcohol, etc. These can be used alone or in combination in any ratio.

[0088] 4-5. Post-development heating process The post-development heating step is a step of heating the patterned coating film formed in the development step to complete the curing of the patterned coating film and obtain a cured patterned coating film (cured product). The heating temperature can be 150 to 240°C, and the heating time can be 1 to 120 minutes. Heating can be performed by a known method such as a hot plate or an inert oven, and heating is preferably performed under a nitrogen atmosphere.

[0089] 5. Uses of negative-type photosensitive resin compositions The negative type photosensitive resin composition of the present disclosure can be suitably used as a material for forming a display device, a semiconductor element, an electronic component, an optical component, a building material, etc. Examples of materials for forming a semiconductor element include a resist material, a buffer coat film, and an insulating film for a rewiring layer of a wafer level package (WLP). Since a cured product formed from the negative type photosensitive resin composition of the present disclosure exhibits good elongation and excellent adhesion, the negative type photosensitive resin composition of the present disclosure can be preferably used in a rewiring layer formation process using a damascene method. Examples of materials for forming electronic components include a printed wiring board, an interlayer insulating film, and a wiring coating film. EXAMPLES

[0090] The present disclosure will be described in more detail using examples, but the present disclosure is not limited to the examples.

[0091] The components used in the examples and comparative examples are as follows.

[0092] (a) Polyhydroxyamide compound [ka] The polyhydroxyamide compound of the above formula was prepared as follows. In a 500 mL flask equipped with a stirrer and a thermometer, 14.93 g (44.39 mmol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP) and 2.45 g (22.42 mmol) of 3-aminophenol were stirred and dissolved in 79 g of N-methylpyrrolidone (NMP). The flask was then immersed in an ice bath, and while keeping the temperature in the flask at 0-5°C, 16.41 g (55.61 mmol) of 4,4'-oxybis(benzoyl chloride) (DEDC) was added as a solid over a period of 10 minutes, and the mixture was stirred in an ice bath for 30 minutes. After stirring at room temperature for 18 hours, the solution was poured into a large amount of ion-exchanged water, and the precipitate was collected. The obtained solid was dissolved in 79 g of ethyl acetate. 17 g of anion-exchange resin (Organo Corporation Amberlyst B-20) was added thereto, and the mixture was stirred vigorously for 1 hour. The stirred solution was concentrated, then poured into a large amount of ion-exchanged water, and the precipitate was collected. The precipitated solid was collected and dried under reduced pressure to obtain a polyhydroxyamide compound (a) having a hydroxyl group at each end. The resulting polyhydroxyamide compound (a) had a weight average molecular weight (Mw) of 9,222, a number average molecular weight (Mn) of 3,561, a polydispersity index (PDI) of 2.6, and a phenolic hydroxyl group equivalent of 252 g / eq.

[0093] (b) Photoacid generator Irgacure PAG103 (BASF oxime sulfonate compound) [ka]

[0094] (c) Crosslinking agent MW-390 (Hexamethoxymethylmelamine compound manufactured by Nippon Carbide Industries Co., Ltd.)

[0095] (d-1) Polyrotaxane (SH1300P, manufactured by ASM Co., Ltd.; molecular weight of the axis: 11,000; total molecular weight (representative value): 180,000; hydroxyl value (mgKOH / g) (representative value): 85) (d-2) Polyrotaxane (SH2400P, manufactured by ASM Co., Ltd.; axis molecular weight 20,000, total molecular weight (representative value) 400,000, hydroxyl value (mgKOH / g) (representative value) 76) [ka]

[0096] (e) Basic compounds Triethanolamine (TEA)

[0097] Surfactant: BYK-310 (BYK-Chemie, silicone surfactant)

[0098] Solvent: Cyclopentanone (Tokyo Chemical Industry Co., Ltd.)

[0099] <Preparation of negative type photosensitive resin composition> Each component was mixed in the amount (parts by mass) shown in Table 1, and dissolved and adjusted in a solvent so that the concentration of non-volatile components in the varnish was 30%, thereby obtaining a varnish of a negative photosensitive resin composition for each of the Examples and Comparative Examples. From the amounts of the raw materials of the negative photosensitive resin composition, (a) the number of moles of hydroxyl groups contained in the polyhydroxyamide compound (Xa), the number of moles of hydroxyl groups at the graft chain terminals of the polyrotaxane (d-1) or (d-2) (Xd), and (c) the number of moles of acid crosslinking groups contained in the crosslinking agent (Xc) were converted to calculate Xc / (Xa+Xd) and Xd / Xa. The calculated values ​​are shown in Table 1.

[0100] The varnishes obtained in each of the Examples and Comparative Examples were subjected to the following evaluations. The results of the evaluations are shown in Table 1.

[0101] <Young's modulus, tensile strength, elongation at break> Cured films for evaluation of Young's modulus, tensile strength, and elongation at break were prepared as follows. The varnish of each Example and Comparative Example was applied to a silicon substrate using a spin coater so that the thickness after curing was 10 μm, and then dried on a hot plate at 90° C. for 180 seconds to obtain a dried coating film of each Example and Comparative Example. The obtained dried coating film was exposed to UV light (wavelength 365 nm) so that the exposure amount was 1000 mJ, and then heated in an inert oven at 220° C. for 1 hour to obtain a cured film. The obtained cured film was subjected to a pressure cooker (PCT) test (conditions: 1 hour treatment under conditions of temperature 121° C. and humidity 100%), and after peeling from the substrate, the cured film was formed into a strip of length 70 mm x width 5 mm to obtain a cured film for evaluation. The Young's modulus, tensile strength, and breaking elongation were measured using the obtained cured film for evaluation. The measurement conditions were as follows. Young's modulus was calculated from the average slope in the stress range of 5 to 10 MPa in the stress-strain curve obtained from the tensile test, and breaking strength was calculated from the stress when the sample broke in the tensile test, and breaking elongation was calculated from the following formula, with the stress being the stress when the sample broke in the tensile test, and the breaking elongation being the elongation until the sample broke in the tensile test. Each measurement value was calculated as the average value of the measurements obtained by performing the same tensile test five times. [Measurement conditions] Testing machine: Tensile testing machine EZ-SX (manufactured by Shimadzu Corporation) Chuck distance: 50mm Test speed: 1mm / min Elongation calculation: (tensile travel distance / chuck distance) x 100

[0102] <Cross-cut after curing and peel after curing> Evaluation substrates for post-cure crosscut and post-cure peel were prepared as follows. The varnish of each Example and Comparative Example was applied to a silicon substrate using a spin coater so that the thickness after curing was 10 μm, and then dried on a hot plate at 90° C. for 180 seconds to obtain a dried coating film of each Example and Comparative Example. The resulting dried coating film was exposed to UV light (wavelength 365 nm) at an exposure dose of 1000 mJ over the entire surface, and then heated in an inert oven at 220° C. for 1 hour to obtain an evaluation substrate with a cured film formed on the surface. Using a cross-cut test guide CCJ-1 (manufactured by COTEC), a total of 100 squares of 1 mm x 1 mm were created with a cutter knife in 10 rows and 10 columns on the cured film of the evaluation substrate. The number of squares that remained without peeling after creation is shown in Table 1 as the result of the cross-cut test after curing. Next, tape peeling was performed (conditions: in accordance with JIS K 5600-5-6:1999). The number of pieces that remained unpeeled is shown in Table 1 as the results of the peel test after curing.

[0103] <Solubility of unexposed areas> A substrate for evaluating the solubility of the unexposed area was prepared as follows. The varnish of each Example and Comparative Example was applied onto a silicon substrate using a spin coater so that the thickness after drying would be 3 μm, and then dried on a hot plate at 90° C. for 180 seconds to obtain a substrate for solubility evaluation in which a dried coating film was formed on the silicon substrate. The solubility evaluation substrate was immersed in a 2.38% tetramethylammonium hydroxide (TMAH) aqueous solution for 1 minute, then removed and the surface on which the dried coating film was formed was observed. The presence or absence of residue in the unexposed areas was visually observed.

[0104] [Table 1]

[0105] As shown in Table 1, the negative photosensitive resin compositions of the examples provide cured products with excellent elongation and adhesion to the substrate. For Examples 1 to 4 and 6, no residue was observed in the unexposed areas, and the compositions are also excellent in terms of developability.

[0106] <Patterning test> The negative photosensitive resin compositions of Examples 1, 4 and 6 were used to carry out the following patterning test, and it was confirmed that patterns were formed normally up to L / S of 2 / 2 μm. The varnish of each Example and Comparative Example was applied to a silicon wafer using a spin coater so that the film thickness after curing was 3.0 μm, and then dried using a hot plate at 90 ° C for 3 minutes to obtain a dried coating film of the negative photosensitive resin composition of each Example and Comparative Example. This dried coating film was exposed to a test pattern with L / S of 1 / 1 μm, 2 / 2 μm, 3 / 3 μm, 4 / 4 μm, and 5 / 5 μm (exposure amount 100 mJ) using a contact exposure machine (UVE-251S + EL-100 (Minaei Electric Manufacturing Co., Ltd.)), and post-exposure baking (PEB) was performed for 60 seconds at 120 ° C on a hot plate. Thereafter, the film was developed for 30 seconds using a 2.38% TMAH aqueous solution, rinsed with ultrapure water for 30 seconds, and spin-dried for 30 seconds to obtain a sample having a pattern. Each sample was cut so that a cross section perpendicular to the longitudinal direction of the pattern could be observed. The cut surface of the pattern was observed using a scanning electron microscope (10,000x magnification) to confirm whether the patterning was normal or not. Samples in which each pattern was patterned vertically without falling were judged to be normal. [Industrial Applicability]

[0107] According to the disclosed technology, a negative photosensitive resin composition capable of producing a cured product having excellent elongation is provided, and a cured product using the negative photosensitive resin composition, and electronic components using the same, such as printed wiring boards and semiconductor elements, are also provided. The disclosed technology enables the formation of sufficiently highly integrated circuits, and has high industrial applicability.

Claims

1. (A) a polyhydroxyamide compound containing a structural unit represented by the following formula (1): (B) a photoacid generator, (C) a crosslinking agent containing an acid crosslinkable group, and (D) a polyrotaxane having a cyclic molecule modified by a graft chain having a hydroxy group at its terminal, the ratio of the number of moles of the acid crosslinking groups contained in (C) to the sum of the number of moles of the hydroxy groups contained in (A) and the number of moles of the hydroxy groups at the graft chain ends of (D) is less than 1.5; A negative photosensitive resin composition. [Formula 1] (In the formula, R 1 is a divalent organic group, R 2 is a tetravalent organic group.

2. 2. The negative photosensitive resin composition according to claim 1, wherein the amount of the (D) is 3 to 30 parts by mass relative to 100 parts by mass of the (A).

3. 3. The negative photosensitive resin composition according to claim 2, wherein the amount of the (D) is 3 to 10 parts by mass relative to 100 parts by mass of the (A).

4. 2. The negative photosensitive resin composition according to claim 1, wherein the acid crosslinkable group is an alkoxymethyl group, a methylol group, or an epoxy group.

5. The negative photosensitive resin composition according to claim 1, wherein the (B) is an oxime sulfonate compound.

6. The negative photosensitive resin composition according to claim 1 , further comprising (E) a basic compound.

7. A dry film comprising a resin layer formed from the negative type photosensitive resin composition according to any one of claims 1 to 6.

8. A cured product of the negative photosensitive resin composition according to any one of claims 1 to 6.

9. An electronic component comprising the cured product according to claim 8.

Citation Information

Patent Citations

  • Negative type photosensitive resin composition, method for producing pattern and electronic parts

    JP2001125267A

  • Negative photosensitive resin composition, method for producing patterned cured film, and electronic component

    JP2008033159A