Laminate and cured product made by curing the same
A laminate with a bisphenol A polycarbonate base layer and a curable resin layer addresses the trade-off between hardness and moldability, providing excellent three-dimensional formability and resistance for complex surfaces.
Patent Information
- Application Number
- JP2023174113
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2023-10-06
- Publication Date
- 2024-11-28
AI Technical Summary
Thermoformable films face a trade-off between hardness and moldability, with existing laminates lacking sufficient three-dimensional formability for complex surfaces.
A laminate comprising a base layer of bisphenol A polycarbonate with a specific glass transition temperature range and a curable resin layer containing a (meth)acryloyl polymer with controlled acrylic equivalent, along with optional acrylic and inorganic particles, to enhance hardness and three-dimensional moldability.
The laminate achieves high hardness and excellent three-dimensional formability, allowing for seamless molding on uneven surfaces without cracking, and resulting in a cured product with enhanced scratch resistance and chemical resistance.
Smart Images

Figure 2024166027000001 
Figure 2024166027000002 
Figure 2024166027000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate and a cured product obtained by curing the laminate. [Background technology]
[0002] Thermoforming films (also called functional films or decorative films) are suitably used to impart desired properties (for example, scratch resistance, chemical resistance, design, etc.) to the surface of a molded article.
[0003] When applying a thermoforming film to a molded product, various molding methods are used, such as vacuum molding, compressed air molding, film insert molding, in-mold molding, and three-dimensional decoration (TOM) molding.
[0004] When a molded product is to be given a characteristic such as scratch resistance, the thermoforming film is required to have a high hardness. Therefore, the thermoforming film is formed into a laminate having a hard coat layer formed by curing a resin. However, the higher the hardness of the thermoforming film, the lower the moldability and the less the conformability to the molded product. In other words, the thermoforming film has a trade-off relationship between hardness and moldability.
[0005] Conventionally, methods for achieving both hardness and moldability of a thermoforming film have been studied. For example, Patent Document 1 describes an invention relating to a thermoforming sheet formed by laminating at least three layers in this order: layer A containing a polycarbonate resin, layer B containing an acrylic resin, and layer C formed from an uncured product of an acrylate-based active energy ray-curable resin composition. In this case, the glass transition temperature (Tg) of layer A is 100°C or higher and 145°C or lower.
[0006] Patent Document 1 describes that, according to the invention, high moldability can be achieved by leaving layer C, which corresponds to the hard coat layer, in an uncured state when applied to a molded article, and that a hard coat layer with high hardness can be obtained by curing layer C by post-exposure to active energy rays after applying the thermoforming sheet to the molded article (after molding). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2021-146687 A Summary of the Invention [Problem to be solved by the invention]
[0008] The thermoforming film described in Patent Document 1 is able to achieve both hardness and formability, but there is room for improvement in three-dimensional formability. Therefore, the present invention provides a laminate having excellent hardness and three-dimensional formability. [Means for solving the problem]
[0009] The present invention is, for example, as follows.
[0010] [1] A substrate layer (a), A curable resin layer (b) containing a (meth)acryloyl polymer having an acrylic equivalent of 200 to 600 g / mol; A laminate comprising: The base layer (a) contains 96% by mass or more of bisphenol A polycarbonate based on the total mass of the base layer (a), The intermediate glass transition temperature (Tmg) of the substrate layer (a) is 100 to 140°C. [2] The bisphenol A polycarbonate is a polycarbonate obtained by mixing bisphenol A, a carbonate binder, and a compound represented by the following formula (1): [ka] [In the above formula (1), R 1 is an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms, R 2 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may be substituted with a halogen atom or an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms which may be substituted with a halogen atom, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 12 carbon atoms. The laminate according to the above item [1], which is a polycarbonate obtained by reacting with a monohydric phenol end terminator represented by the following formula: [3] The laminate according to the above [2], wherein the monohydric phenol end terminator represented by the formula (1) includes at least one selected from the group consisting of 2-hexyldecyl parahydroxybenzoate, hexadecyl parahydroxybenzoate, dodecyl parahydroxybenzoate, and 2-ethylhexyl parahydroxybenzoate. [4] The (meth)acryloyl polymer is represented by the following formula (2): [ka] [In the above formula (2), m is a single bond or an alkylene group having 1 to 4 carbon atoms; n is hydrogen or an alkyl group having 1 to 4 carbon atoms; p is a single bond or an alkylene group having 1 to 2 carbon atoms; q is hydrogen or an alkyl group having 1 to 12 carbon atoms which may be substituted with at least one substituent selected from the group consisting of an epoxy group, a hydroxyl group, and a (meth)acryloyl group. The laminate according to any one of the above [1] to [3], which contains a repeating unit represented by the following formula: [5] The (meth)acryloyl polymer is represented by the following formulas (2-a) to (2-c): [ka] The laminate according to the above [4], comprising at least one repeating unit represented by the following formula: [6] The laminate according to any one of the above [1] to [5], wherein the (meth)acryloyl polymer has an acrylic equivalent of 200 to 500 g / mol. [7] The laminate according to any one of the above [1] to [6], wherein the curable resin layer (b) further contains a leveling agent. [8] The laminate according to the above [7], wherein the leveling agent comprises a fluorine-based leveling agent. [9] The laminate according to any one of the above [1] to [8], wherein the curable resin layer (b) further contains inorganic particles.
[10] The laminate according to the above [9], wherein the inorganic particles have an average particle size of 20 to 60 nm.
[11] The laminate according to any one of the above [1] to
[10] , wherein the curable resin layer (b) further contains a light stabilizer.
[12] The laminate according to any one of the above [1] to
[11] , wherein the curable resin layer (b) further contains a polymerization inhibitor.
[13] The laminate according to any one of the above [1] to
[12] , wherein the curable resin layer (b) has a thickness of 5 μm or more.
[14] Further comprising an acrylic layer (c), The laminate according to any one of the above [1] to
[13] , wherein the base layer (a), the acrylic layer (c), and the curable resin layer (b) are laminated in this order.
[15] The laminate according to the above
[14] , wherein the thickness of the acrylic layer (c) is 20 μm or more.
[16] The laminate according to any one of the above [1] to
[15] , which is used for vacuum forming.
[17] The laminate according to any one of the above [1] to
[16] , which is used in TOM molding.
[18] A cured product obtained by curing the laminate according to any one of the above [1] to
[17] . Effect of the Invention
[0011] According to the present invention, a laminate having excellent hardness and three-dimensional formability is provided, which allows it to be suitably molded, for example, by three-dimensional decoration (TOM) molding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described in detail.
[0013] 1.Laminate The laminate according to the present invention includes a base layer (a) and a curable resin layer (b) containing a (meth)acryloyl polymer having an acrylic equivalent of 200 to 600 g / mol. The base layer (a) contains 96% by mass or more of bisphenol A polycarbonate based on the total mass of the base layer (a). The intermediate glass transition temperature (Tmg) of the base layer (a) is 100 to 140°C.
[0014] The laminate has excellent hardness and three-dimensional moldability. Specifically, the laminate includes a curable resin layer (b), i.e., an uncured resin layer (b), and has a predetermined structure, so that the laminate has excellent moldability, particularly three-dimensional moldability. In addition, after molding the laminate, the curable resin layer (b) is cured to form a cured film, and the cured product obtained from the laminate has high hardness.
[0015] In this specification, the term "intermediate glass transition temperature (Tmg)" refers to a value obtained by analyzing a DSC curve obtained by differential scanning calorimetry (DSC). Specifically, when the intersection point of line A and tangent B of line A extending the low-temperature side baseline of the DSC curve to the high-temperature side, line B tangent to the inflection point, and line C extending the high-temperature side baseline to the low-temperature side are defined as the start glass transition temperature (Tig) and the tangent of tangent B and line C are defined as the end glass transition temperature (Teg), the intermediate point between the start glass transition temperature (Tig) and the end glass transition temperature (Teg) is the intermediate glass transition temperature (Tmg). In general, glass transition temperature refers to the start glass transition temperature (Tig), which is lower than the intermediate glass transition temperature (Tmg). The intermediate glass transition temperature (Tmg) is measured by the method described in the Examples.
[0016] In one embodiment, the laminate according to the present invention is used for vacuum forming. Vacuum forming is a forming method in which forming is performed under vacuum conditions, and may include in-mold forming, total-or-three-dimensional (TOM) forming, and the like. When a laminate including the curable resin layer (b) is applied to a molded article (when molding), it is preferable not to cause curing of the curable resin layer (b) during molding, but to cure the curable resin layer (b) after molding. However, when molding is performed under vacuum conditions, radicals are generated from oxygen atoms and the like contained in the curable resin layer (b), which may cause unintended curing of the curable resin layer (b) during vacuum molding, and as a result, cracks may occur in the curable resin layer (b) after molding. According to the laminate of the present invention, even when molding is performed under vacuum conditions, the laminate can be formed without generating cracks, and the occurrence of cracks in the curable resin layer (b) of the laminate can be prevented.
[0017] In one embodiment, the laminate according to the present invention is used in three-dimensional decoration (TOM) molding. Three-dimensional decoration (TOM) molding includes (1) a vacuum process in which a lower chamber with an open top in which a molded product having a textured surface is placed, an upper chamber with an open bottom in which a heater is placed, and the laminate according to the present invention sandwiched between the lower chamber and the upper chamber are made airtight and then placed under vacuum conditions, (2) a heating process in which the laminate is heated using the heater, (3) a contact process in which the molded product having the texture is brought into contact with the heated laminate, (4) an upper chamber de-vacuum process in which the upper chamber is placed under atmospheric pressure, and (5) a lower chamber de-vacuum process in which the lower chamber is placed under atmospheric pressure. That is, in three-dimensional decoration (TOM) molding, a laminate is heated under vacuum conditions to soften it, and then a molded product is pushed up from the bottom of the laminate to bring them into contact (the laminate is tightly laminated by the molded product due to its own weight), and the upper chamber is placed under atmospheric pressure to create a pressure difference and apply pressure from the upper chamber to the lower chamber to complete the lamination. This allows for the production of a three-dimensional decorated molded product that includes a molded product with an uneven surface and a laminate placed on the uneven surface. The TOM molding may further include an upper chamber pressurizing step of introducing compressed air into the upper chamber after the upper chamber de-vacuuming step, and may further include a trimming step of removing a part of the laminate placed on the uneven surface and a curing step of curing the laminate after the lower chamber de-vacuuming step. When using a conventional laminate, when attempting to perform three-dimensional decoration (TOM) molding, the laminate cannot be laminated with high conformity to a molded product having an uneven surface, and even if it can be laminated, cracks may occur in the laminate. However, according to the laminate of the present invention, it is possible to laminate with high conformity to a molded product having an uneven surface, and cracks are unlikely to occur in the obtained laminate. That is, the laminate of the present invention has excellent three-dimensional moldability. In addition, according to the laminate having the configuration of the present invention, a cured product having high hardness can be obtained.
[0018] <Base material layer (a)> The substrate layer (a) contains bisphenol A polycarbonate. The substrate layer (a) may further contain other resins, plasticizers, additives, and the like.
[0019] [Bisphenol A polycarbonate] Bisphenol A polycarbonate is a resin that contains structural units derived from bisphenol A (BPA) in an amount of 80 mass% or more, preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 97 mass% or more, and particularly preferably 98 to 100 mass%, based on the mass of all structural units of bisphenol A polycarbonate excluding the terminal structures.
[0020] In one embodiment, the bisphenol A type polycarbonate is preferably a polycarbonate obtained by reacting bisphenol A, a carbonate binder, and a monohydric phenol end terminator represented by the following formula (1). [ka]
[0021] (Bisphenol A) Bisphenol A (BPA) is represented by the following formula: [ka]
[0022] (Compounds that derive other building blocks) The bisphenol A polycarbonate may be formed by further reacting a compound that derives other structural units. By using the compound that derives the other structural units, the physical properties of the bisphenol A polycarbonate (e.g., the mid-glass transition temperature (Tmg), the viscosity average molecular weight, etc.) can be adjusted.
[0023] The compound from which the other structural units are derived is a polymerizable compound other than bisphenol A, and examples thereof include bisphenol compounds other than bisphenol A and organosiloxanes.
[0024] Bisphenol compounds other than bisphenol A include bis(4-hydroxyphenyl)methane (bisphenol F: BPF), bis(2-hydroxyphenyl)methane, 2,4'-dihydroxydiphenylmethane, bis(4-hydroxy-3-methylphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane (bisphenol E: BPE), 1,1-bis(4-hydroxy-3-methylphenyl)ethane, 2,2-bis(4-hydroxy-3-methylphenyl)propane (bisphenol C: BPC), 2,2-bis(4-hydroxy-3-isopropylphenyl)propane (bisphenol G: BPG), 2,2-bis(4-hydroxyphenyl)butane (bisphenol B: BPB), 2,2-bis(4-hydroxy-3-t-butylphenyl)propane, 5,5'-(1-methylethylidene)-bis[1,1'-(bisphenyl)-2-ol]propane (bisphenol PH: BPPH), 1,1-bis(4-hydroxyphenyl)-2-methylpropane (bisphenol IBTD), 2,2-bis(4-hydroxyphenyl)-4-methylpentane (bisphenol MIBK), 1,1-bis(4-hydroxyphenyl)-2-ethylhexane (bisphenol IOTD), 1,1-bis(4-hydroxyphenyl)decane, 1,1-bis(4-hydroxyphenyl)cyclohexane (bisphenol Z: BPZ), 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (bisphenol TMC), 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)cycloundecane, 1,1-bis(4-hydroxyphenyl)cyclododecane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane (bisphenol AP: BPAP), bis(4-hydroxyphenyl)diphenylmethane (bisphenol BP;BPBP), bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)ether, bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenylsulfone, bis(2-hydroxyphenyl)sulfone, bis(4-hydroxy-3-methylphenyl)sulfonebis(4-hydroxyphenyl)ketone, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-hydroxy-3-ethylphenyl)fluorene, 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisphenol, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisphenol, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, and the like.;
[0025] Examples of the organosiloxane include α,ω-bis[3-(o-hydroxyphenyl)propyl]polydimethylsiloxane, α,ω-bis[3-(o-hydroxyphenyl)propyl]polydimethyldiphenyl random copolymerized siloxane, and the like.
[0026] The compounds from which the other structural units are derived may be used alone or in combination of two or more kinds.
[0027] The amount of the compound that derives other structural units added is preferably 50 mol or less, and more preferably 0.1 to 40 mol, per mol of bisphenol A.
[0028] (carbonate binder) Carbonate binders include, but are not limited to, carbonyl compounds such as phosgene, triphosgene, carbon monoxide, carbon dioxide, and carbonic acid diesters.
[0029] Examples of the carbonic acid diester include dialkyl carbonate compounds such as dimethyl carbonate, diethyl carbonate, and di-tert-butyl carbonate, and substituted diphenyl carbonates such as diphenyl carbonate, di-p-tolyl carbonate, phenyl-p-tolyl carbonate, and di-p-chlorophenyl carbonate.
[0030] Among these, the carbonate binder preferably contains at least one of phosgene, triphosgene, diphenyl carbonate, and substituted diphenyl carbonate, and more preferably contains at least one of phosgene and diphenyl carbonate. The carbonate binder may be used alone or in combination of two or more kinds.
[0031] (Monohydric phenol end-capping agent represented by formula (1)) The monohydric phenol end terminator represented by formula (1) has a function of adjusting the intermediate glass transition temperature (Tmg) of bisphenol A polycarbonate, and the like. [ka]
[0032] In the above formula (1), R 1 is an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms, R 2 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may be substituted with a halogen atom or an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms which may be substituted with a halogen atom, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 12 carbon atoms. In this specification, the "alkyl group" and the "alkenyl group" may be linear or branched, but are preferably linear.
[0033] More preferably, the monohydric phenol end terminator represented by formula (1) is represented by the following general formula (1-a): [ka]
[0034] In the above formula (1-a), R 1 is an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms.
[0035] R in formula (1) or formula (1-a) 1 It is more preferable that the number of carbon atoms in R is within a specific numerical range. 1 The upper limit of the number of carbon atoms in R is preferably 36, more preferably 22, and particularly preferably 18. 1 The lower limit of the number of carbon atoms is preferably 8, and more preferably 12.
[0036] R 1 When the upper limit of the carbon number of R is appropriate, the monohydric phenol end terminator represented by formula (1) tends to have high solubility in organic solvents, which is preferable from the viewpoints of increasing the productivity during the production of bisphenol A type polycarbonate resin and increasing the transparency of the bisphenol A type polycarbonate resin. 1 When the carbon number of R is 36 or less, a bisphenol A type polycarbonate resin having high transparency can be obtained, and the productivity in producing the bisphenol A type polycarbonate resin is high and economical. 1 When the carbon number is 22 or less, the monohydric phenol end terminator represented by formula (1) has particularly excellent solubility in organic solvents, and can extremely increase the productivity in producing bisphenol A type polycarbonate resin, thereby improving the economic efficiency.
[0037] R 1 If the lower limit of the carbon number is appropriate, the glass transition point of the bisphenol A polycarbonate resin is not too high, and the resin has favorable thermoformability. 1When a monohydric phenol end terminator represented by formula (1), in which R is an alkyl group having 16 carbon atoms, is used, the intermediate glass transition temperature, melt fluidity, moldability, drawdown resistance, and solvent solubility of the monohydric phenol end terminator represented by formula (1) during production of the bisphenol A type polycarbonate resin are excellent, and this is particularly preferable as the end terminator used for the bisphenol A type polycarbonate resin in the present invention.
[0038] In one embodiment, R in formula (1) or formula (1-a) 1 is preferably dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, or octadecyl, more preferably tetradecyl, pentadecyl, hexadecyl, heptadecyl, or 2-hexyldecyl, and even more preferably hexadecyl or 2-hexyldecyl.
[0039] In one embodiment, R in formula (1) 2 are each independently preferably hydrogen, a halogen atom, methyl, ethyl, propyl, isopropyl, butyl, t-butyl, or phenyl, more preferably hydrogen, a fluorine atom, a chlorine atom, methyl, ethyl, or phenyl, and further preferably hydrogen, a fluorine atom, a chlorine atom, methyl, or ethyl. 2 is preferably hydrogen.
[0040] In one embodiment, the monohydric phenol end-terminator represented by formula (1) preferably includes at least one selected from the group consisting of 2-hexyldecyl parahydroxybenzoate, hexadecyl parahydroxybenzoate, dodecyl parahydroxybenzoate, and 2-ethylhexyl parahydroxybenzoate, more preferably includes at least one of 2-hexyldecyl parahydroxybenzoate and hexadecyl parahydroxybenzoate, and further preferably includes 2-hexyldecyl parahydroxybenzoate.
[0041] The monohydric phenol end terminator represented by the above formula (1) may be used alone or in combination of two or more kinds.
[0042] The amount of the monohydric phenol end terminator represented by formula (1) used is preferably 0.02 to 0.07 mol, and more preferably 0.025 to 0.06 mol, per 1 mol of bisphenol A.
[0043] The amount of the monohydric phenol end terminator represented by formula (1) used is preferably 0.02 to 0.07 mol, and more preferably 0.025 to 0.06 mol, per 1 mol of the carbonate binder.
[0044] (Other end terminators) The bisphenol A polycarbonate may be formed by further reacting with another end terminator. The other end terminator is a end terminator other than the monohydric phenol end terminator represented by formula (1), and is preferably an end terminator having no unsaturated group. By using the other end terminator, the physical properties (e.g., mid-glass transition temperature (Tmg), viscosity average molecular weight, etc.) of the bisphenol A polycarbonate can be adjusted.
[0045] Other end terminators include those derived from monohydric phenol compounds.
[0046] Examples of the monohydric phenol compound include phenol, p-cresol, o-cresol, 2,4-xylenol, p-tert-butylphenol, p-hexylphenol, p-heptylphenol, p-octylphenol, p-cumylphenol, etc. These monohydric phenol compounds may be used alone or in combination of two or more kinds.
[0047] The amount of the other terminal terminator used is preferably 0.5 mol or less, more preferably 0.2 mol or less, and even more preferably 0.1 mol or less, per mol of the terminal terminator represented by formula (1).
[0048] The amount of the other terminal terminator used is preferably 0.02 to 0.07 mol, and more preferably 0.025 to 0.06 mol, per 1 mol of bisphenol A.
[0049] The intermediate glass transition temperature (Tmg) of the bisphenol A polycarbonate is preferably 100 to 140° C., more preferably 125 to 140° C., even more preferably 128 to 140° C., and still more preferably 128 to 135° C. If the intermediate glass transition temperature (Tmg) of the bisphenol A polycarbonate is in the above range, it is preferable because it is easy to control the intermediate glass transition temperature (Tmg) of the base layer (a).
[0050] The viscosity average molecular weight of the bisphenol A type polycarbonate is preferably 14000 or more, more preferably 16000 or more, even more preferably 20000 or more, particularly preferably 24000 or more, and very preferably 26000 or more. The viscosity average molecular weight of the bisphenol A type polycarbonate is preferably 40000 or less, more preferably 38000 or less, even more preferably 36000 or less, particularly preferably 34000 or less, and very preferably 32000 or less. In one embodiment, the viscosity average molecular weight of the bisphenol A type polycarbonate is preferably 14000 to 40000, more preferably 16000 to 38000, even more preferably 18000 to 36000, particularly preferably 20000 to 34000, and very preferably 24000 to 32000. In this specification, the "viscosity average molecular weight" is measured by the method described in the examples. When the bisphenol A type polycarbonate is a mixture of two or more kinds of bisphenol A type polycarbonate having different molecular weights, the viscosity average molecular weight after mixing is used.
[0051] The content of bisphenol A polycarbonate is 96% by mass or more, more preferably 98% by mass or more, and even more preferably 100% by mass, based on the total mass of the base layer (a).
[0052] [Plasticizer] The base layer (a) may further contain a plasticizer, which has the function of adjusting the intermediate glass transition temperature (Tmg) of the base layer.
[0053] The plasticizer is not particularly limited, but examples thereof include polyesters, polyethers, aromatic phosphonate compounds, and aromatic ester compounds.
[0054] Examples of the polyester include aliphatic polyesters such as polycaprolactone (PCL); and aromatic polyesters such as polyethylene terephthalate modified resins and polycaprolactone polyethylene terephthalate modified resins.
[0055] Examples of the polycaprolactone polyethylene terephthalate modified resin include glycol modified polyethylene terephthalate (PETG) and glycol modified polycyclohexylene dimethylene terephthalate (PCTG). PETG is a PET (containing terephthalic acid units as dicarboxylic acid units and ethylene glycol units as glycol units) in which some of the ethylene glycol units have been replaced with 1,4-cyclohexanedimethanol units. The content of 1,4-cyclohexanedimethanol units is preferably less than 50 mol %, more preferably 30 to 40 mol %, based on the total glycol units. PCTG is a copolymer in which some of the glycol units in PCT (dicarboxylic acid units, i.e., terephthalic acid units and glycol units, i.e., 1,4-cyclohexanedimethanol units) are replaced with glycol units. The content of the glycol units is preferably less than 50 mol%, more preferably 30 to 40 mol%, based on the total glycol units.
[0056] The number average molecular weight of the polyester is preferably from 10,000 to 100,000, and more preferably from 20,000 to 60,000. In this specification, the value of "number average molecular weight" is measured by gel permeation chromatography.
[0057] The polyether may be a polyether having at least one selected from the group consisting of ethylene glycol unit, propylene glycol unit, butylene glycol unit, trimethylene glycol unit, and tetramethylene glycol unit.Specifically, the polyether may be a homopolymer or a copolymer, and if it is a copolymer, it may be any of random copolymerization, alternating copolymerization, block copolymerization, graft copolymerization, and combinations thereof.Specific examples of polyether include polyethylene glycol, polypropylene glycol, polybutylene butylene glycol, and block copolymers of polyethylene glycol and polypropylene glycol. The number average molecular weight of the polyether is preferably 500-4,000, more preferably 600-3,000, and further preferably 800-2,000.
[0058] Examples of the aromatic phosphonate compound include triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, 2-ethylhexyl diphenyl phosphate, tert-butylphenyl diphenyl phosphate, bis-(tert-butylphenyl)phenyl phosphate, tris-(tert-butylphenyl)phosphate, isopropylphenyl diphenyl phosphate, bis-(isopropylphenyl)diphenyl phosphate, tris-(isopropylphenyl)phosphate, resorcinol bis-diphenyl phosphate, resorcinol poly(di-2,6-xylyl)phosphate, resorcinol bis-dixylenyl phosphate, bisphenol A bis-diphenyl phosphate, biphenyl bis-diphenyl phosphate, etc. The molecular weight of the aromatic phosphonate compound is preferably 200 to 1000, more preferably 400 to 800.
[0059] Examples of aromatic ester compounds include diethylene glycol dibenzoate, glyceryl tribenzoate, trimethylolpropane tribenzoate, pentaerythritol tetrabenzoate, etc. The molecular weight of the aromatic ester compound is preferably 200 to 1000, and more preferably 400 to 800.
[0060] Among the above, the plasticizer preferably contains polyester or an aromatic phosphonate compound, more preferably contains polyester, further preferably contains at least one of polycaprolactone (PCL), glycol-modified polyethylene terephthalate (PETG), and glycol-modified polycyclohexylene dimethylene terephthalate (PCTG), and particularly preferably contains polycaprolactone (PCL). The above plasticizers may be used alone or in combination of two or more kinds.
[0061] The content of the plasticizer is preferably 4% by mass or less, more preferably 3% by mass or less, and even more preferably 0.1 to 2% by mass, based on the total mass of the base layer (a). When the content of the plasticizer is 4% by mass or less, the base layer (a) can contain bisphenol A polycarbonate at a content of 96% by mass or more.
[0062] [Additives] The base layer (a) may further contain additives. The additives are not particularly limited, and examples thereof include polycarbonates other than bisphenol A polycarbonates, antioxidants, ester exchange inhibitors, release agents, heat stabilizers, flame retardants, flame retardant assistants, ultraviolet absorbers, colorants, antistatic agents, fluorescent brighteners, antifogging agents, flow improvers, plasticizers, dispersants, antibacterial agents, antiblocking agents, impact improvers, sliding improvers, hue improvers, acid trapping agents, etc. These additives may be used alone or in combination of two or more.
[0063] The content of the additive is preferably 4% by mass or less, more preferably 3% by mass or less, and even more preferably 0.1 to 2% by mass, based on the total mass of the base layer (a). When the content of the additive is 4% by mass or less, the base layer (a) can contain bisphenol A type polycarbonate in a content of 96% by mass or more.
[0064] [Configuration of base layer (a)] The intermediate glass transition temperature (Tmg) of the substrate layer (a) is 100 to 140° C., preferably 110 to 140° C., more preferably 120 to 140° C., even more preferably 120 to 135° C., and particularly preferably 125 to 135° C. The intermediate glass transition temperature (Tmg) of the substrate layer (a) can be controlled by appropriately adjusting the structure of the bisphenol A polycarbonate (for example, the content of structural units derived from bisphenol A (BPA), the types and contents of other structural units, the type of end terminator used, the viscosity average molecular weight, etc.), the type and content of the plasticizer added to the substrate layer (a), etc.
[0065] The thickness of the base layer (a) is preferably 10 to 800 μm, more preferably 20 to 500 μm, and even more preferably 30 to 400 μm. In one embodiment, the thickness of the base layer (a) is preferably 20 to 140 μm, more preferably 30 to 120 μm, and even more preferably 60 to 120 μm. In another embodiment, the thickness of the base layer (a) is preferably 140 to 500 μm, more preferably 150 to 400 μm, even more preferably 180 to 300 μm, and particularly preferably 180 to 260 μm.
[0066] The Charpy impact strength of the base layer (a) is 30 kJ / m 2 It is preferable that the concentration is 45 kJ / m or more. 2 In this specification, the "Charpy impact strength" is measured by the method described in the Examples.
[0067] <Curable resin layer (b)> The curable resin layer (b) contains a (meth)acryloyl polymer having an acrylic equivalent of 200 to 600 g / mol. Since the curable resin layer (b) is in an uncured state, when the laminate according to the present invention is to be molded, it has excellent three-dimensional moldability. Therefore, when three-dimensional molding is performed, the curable resin layer (b) is easy to follow, and cracks are unlikely to occur in the curable resin layer (b) after molding. In addition, the cured product obtained by curing the laminate has high hardness, and may have high scratch resistance, chemical resistance, etc. In this specification, "(meth)acryloyl" means methacryloyl and / or acryloyl. Similarly, "(meth)acrylic" and "(meth)acrylate" mean methacrylic and / or acrylic, methacrylate and / or acrylate.
[0068] [(Meth)acryloyl polymer] The (meth)acryloyl polymer preferably contains a repeating unit represented by the following formula (2).
[0069] [ka]
[0070] In the above formula (2), m is a single bond or an alkylene group having 1 to 4 carbon atoms, preferably methylene or ethylene, and more preferably methylene.
[0071] n is hydrogen or an alkyl group having 1 to 4 carbon atoms, preferably hydrogen, methyl, or ethyl, more preferably hydrogen or methyl, and further preferably hydrogen.
[0072] p is a single bond or an alkylene group having 1 to 2 carbon atoms, preferably a single bond or methylene, and more preferably a single bond.
[0073] q is hydrogen or an alkyl group having 1 to 12 carbon atoms which may be substituted with at least one substituent selected from the group consisting of an epoxy group, a hydroxyl group, and a (meth)acryloyl group, is preferably an alkyl group having 1 to 4 carbon atoms which may be substituted with at least one substituent selected from the group consisting of an epoxy group and a (meth)acryloyl group, and is more preferably an alkyl group having 1 to 2 carbon atoms which may be substituted with at least one substituent selected from the group consisting of an epoxy group and a (meth)acryloyl group.
[0074] In one embodiment, the (meth)acryloyl polymer preferably contains at least one of the repeating units represented by the following formulas (2-a) to (2-c).
[0075] [ka]
[0076] The content of the repeating unit represented by formula (2-a) is preferably from 30 to 85 mol %, and more preferably from 40 to 80 mol %, based on the total number of moles of the (meth)acryloyl polymer.
[0077] The content of the repeating unit represented by formula (2-b) is preferably from 5 to 30 mol %, and more preferably from 10 to 25 mol %, based on the total number of moles of the (meth)acryloyl polymer.
[0078] The content of the repeating unit represented by formula (2-c) is preferably from 10 to 40 mol %, and more preferably from 10 to 35 mol %, based on the total number of moles of the (meth)acryloyl polymer.
[0079] The above-mentioned (meth)acryloyl polymers may be used alone or in combination of two or more kinds.
[0080] The molar ratio of the repeating unit represented by formula (2-a) to the repeating unit represented by formula (2-b) is preferably 4.5-5.5:1.5-2.5. The molar ratio of the repeating unit represented by formula (2-a) to the repeating unit represented by formula (2-c) is preferably 4.5-5.5:2.5-3.5. The molar ratio of the repeating unit represented by formula (2-b) to the repeating unit represented by formula (2-c) is preferably 1.5-2.5:2.5-3.5.
[0081] The acrylic equivalent of the (meth)acryloyl polymer is 200 to 600 g / mol, and from the viewpoint of increasing the hardness of the cured product, it is preferably 200 to 500 g / mol, more preferably 200 to 400, and even more preferably 200 to 300. In this specification, the (meth)acrylic equivalent (g / mol) means the molecular weight per one (meth)acryloyl group, and can be calculated by the method described in the Examples.
[0082] The weight average molecular weight of the (meth)acryloyl polymer is preferably 5,000 to 200,000, more preferably 10,000 to 150,000, further preferably 15,000 to 100,000, and particularly preferably 20,000 to 50,000. In this specification, the "weight average molecular weight" is calculated by the method described in the Examples.
[0083] The content of the (meth)acryloyl polymer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 60 to 100% by mass, and particularly preferably 60 to 90% by mass, based on the total mass of the curable resin layer (b).
[0084] [Multifunctional acrylate compounds] The curable resin layer (b) may further contain a polyfunctional acrylate compound. The polyfunctional acrylate compound can improve the hardness of the cured product by reacting with, for example, a (meth)acryloyl group, an epoxy group, a hydroxyl group, or the like, contained in the (meth)acryloyl polymer. In this specification, the term "polyfunctional" means two or more functional groups, preferably three or more functional groups, more preferably three to eight functional groups, and even more preferably three to six functional groups.
[0085] The polyfunctional acrylate compound is not particularly limited, but examples thereof include pentaerythritol triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.
[0086] The content of the polyfunctional acrylate compound is preferably 70% by mass or less, more preferably 50% by mass or less, and even more preferably 30% by mass or less, based on the total content of the (meth)acryloyl polymer and the polyfunctional acrylate compound.
[0087] [Inorganic particles] The curable resin layer (b) may further contain inorganic particles, which can improve the hardness and scratch resistance of the cured product.
[0088] The inorganic particles are not particularly limited, but examples thereof include silica, alumina, titania, zirconia, diamond, and the like.
[0089] The inorganic particles may be surface-treated. By surface-treating the inorganic particles, they can be dispersed in a stable state in the curable resin layer (b). In this case, the surface treatment agent used is not particularly limited, but silane compounds, alcohols, amines, carboxylic acids, sulfonic acids, phosphonic acids, etc. can be used. These surface treatment agents may be used alone or in combination of two or more. By the surface treatment, a polymerizable group (preferably a vinyl group or a (meth)acrylic group) can be introduced onto the inorganic particle surface.
[0090] The above-mentioned inorganic particles may be used alone or in combination of two or more kinds.
[0091] The average particle size of the inorganic particles is preferably 5 to 95 nm, more preferably 8 to 70 nm, and from the viewpoint of improving the scratch resistance of the obtained cured product, is further preferably 20 to 60 nm, and particularly preferably 30 to 60 nm. In this specification, the "particle size" means the maximum distance between two points on the outer surface of the particle. The "average particle size" is measured by the method described in the Examples.
[0092] The content of the inorganic particles is preferably from 5 to 60% by mass, more preferably from 10 to 50% by mass, and further preferably from 20 to 40% by mass, based on the total mass of the curable resin layer (b).
[0093] [Leveling agent] The curable resin layer (b) may further contain a leveling agent, which has functions such as leveling properties (making the coating film flat and smooth) and improving the fingerprint wiping properties, stain resistance, and abrasion resistance of the cured product.
[0094] The leveling agent is not particularly limited, but examples thereof include fluorine-based leveling agents and silicone-based leveling agents.
[0095] The fluorine-based leveling agent can be a compound having a perfluoropolyether bond.The fluorine-based leveling agent can be a commercially available product, such as Megafac RS-56, RS-75, RS-76-E, RS-76-NS, RS-78, RS-90 (manufactured by DIC Corporation), KY-1203, X-71-1203E, KY-1207, KY-1211 (manufactured by Shin-Etsu Chemical Co., Ltd.), Optool UD120 (manufactured by Daikin Industries, Ltd.), Ftergent 710FL, 220P, 208G, 601AD, 602A, 650A, 228P, 240GFTX-218 (manufactured by Neos Co., Ltd.).
[0096] Examples of the silicone-based leveling agent include acrylic group-containing polyether-modified polydimethylsiloxane, etc. As the silicone-based leveling agent, commercially available products can be used, such as BYK-UV3500 and BYK-UV3505 (manufactured by BYK-Chemie Japan Co., Ltd.).
[0097] Among these, the leveling agent preferably contains a fluorine-based leveling agent from the viewpoint of improving the ease of wiping off fingerprints from the cured product, etc. The above-mentioned leveling agents may be used alone or in combination of two or more kinds.
[0098] The content of the leveling agent is preferably 0.001 to 10 mass %, more preferably 0.001 to 5 mass %, further preferably 0.01 to 4 mass %, and particularly preferably 0.1 to 3 mass %, relative to the total mass of the curable resin layer (b).
[0099] [Photopolymerization initiator] The curable resin layer (b) may further contain a photopolymerization initiator. The photopolymerization initiator has a function of promoting a curing reaction when curing the curable resin layer (b).
[0100] Examples of photopolymerization initiators include, but are not limited to, 1-hydroxycyclohexyl-phenyl-ketone (Irgacure 184), 2-hydroxy-2-methyl-1-phenyl-propan-1-one (Irgacure 1173), 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (Irgacure TPO), bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Irgacure 819), 2,2'-dimethoxy-2-phenylacetophenone (Irgacure 651), oligo(2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone (Esacure ONE), 1-hydroxycyclohexyl-phenyl ketone (Omnirad Among these, the photopolymerization initiator preferably contains at least one of oligo(2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone (EsacureONE) and 1-hydroxycyclohexyl-phenyl ketone (Omnirad 184) from the viewpoint of increasing heat resistance, and more preferably contains 1-hydroxycyclohexyl-phenyl ketone (Omnirad 184). The above-mentioned photopolymerization initiators may be used alone or in combination of two or more kinds.
[0101] The content of the photopolymerization initiator is preferably 1 to 10 mass %, more preferably 1 to 6 mass %, even more preferably 2 to 5 mass %, and particularly preferably 2 to 4 mass %, relative to the total mass of the curable resin layer (b).
[0102] [Light stabilizer] The curable resin layer (b) may further contain a light stabilizer. The light stabilizer has a function of improving the weather resistance of the cured product.
[0103] The light stabilizer is not particularly limited, but may be a hindered amine light stabilizer.
[0104] Hindered amine light stabilizers include bis(1-undecaneoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate (ADK STAB LA-81), tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate (ADK STAB LA-52), tetrakis(2,2,6,6-tetramethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate (ADK STAB LA-57), 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate (ADK STAB LA-82), Examples of such compounds include bis(2,2,6,6-tetramethyl-1-octyloxy-4-piperidyl)sebacate (Tinuvin 123), bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate (Tinuvin 770DF), and bis(1,2,2,6,6-pentamethyl-4-piperidyl)-((3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl)methyl)butyl malonate (Tinuvin 144).
[0105] Among these, the light stabilizer preferably contains a hindered amine light stabilizer. The above light stabilizers may be used alone or in combination of two or more kinds.
[0106] The content of the light stabilizer is preferably 0.1 to 15 mass %, more preferably 0.1 to 7 mass %, even more preferably 0.3 to 5 mass %, and particularly preferably 0.3 to 3 mass %, relative to the total mass of the curable resin layer (b).
[0107] [Polymerization inhibitor] The curable resin layer (b) may further contain a polymerization inhibitor. The polymerization inhibitor has a function of suppressing a polymerization reaction of the curable resin layer (b) caused by light, heat, etc., and improving the storage stability of the laminate.
[0108] The polymerization inhibitor is not particularly limited, but examples thereof include phenothiazine, mequinol (4-methoxyphenol), hydroquinone, 2-hydroxynaphthoquinone, N-isopropyl-N'-phenyl-p-phenylenediamine, 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, 2,2,6,6-tetramethyl-4-oxopiperidine-1-oxyl, and 2-mercaptobenzimidazole.
[0109] Among these, the polymerization inhibitor preferably contains at least one of phenothiazine, mequinol, and hydroquinone, and more preferably contains phenothiazine. The above-mentioned polymerization inhibitors may be used alone or in combination of two or more kinds.
[0110] The content of the polymerization inhibitor is preferably from 0.001 to 5 mass %, more preferably from 0.01 to 4 mass %, and further preferably from 0.01 to 3 mass %, based on the total mass of the curable resin layer (b).
[0111] [Additives] The curable resin layer (b) may further contain an additive.
[0112] The additives are not particularly limited, but include heat stabilizers, antioxidants, flame retardants, flame retardant assistants, ultraviolet absorbers, release agents, colorants, antistatic agents, fluorescent brighteners, antifogging agents, flow improvers, plasticizers, dispersants, antibacterial agents, etc. These additives may be used alone or in combination of two or more.
[0113] [Configuration of curable resin layer (b)] The curable resin layer (b) is in an uncured state, and for example, the (meth)acryloyl polymer has a polymerizable functional group (such as a (meth)acryloyl group, an epoxy group, or a hydroxyl group). The curable resin layer (b) is easy to conform and is less likely to crack after molding, so that it has excellent three-dimensional moldability. However, for example, within a range that does not impair the effects of the present invention, the (meth)acryloyl polymer in the curable resin layer (b) may have a crosslinked structure due to a part of the (meth)acryloyl group undergoing a curing reaction during the molding process.
[0114] The thickness of the curable resin layer (b) is preferably 1 μm or more, more preferably 3 μm or more, and from the viewpoint of increasing hardness, is further preferably 5 μm or more, particularly preferably 5 to 30 μm, and most preferably 5 to 10 μm.
[0115] <Acrylic layer (c)> The laminate may further include an acrylic layer (c). The acrylic layer (c) has a function of improving the impact resistance of the laminate and a function of improving the hardness of the cured product.
[0116] In one embodiment, the laminate preferably includes a base layer (a), an acrylic layer (c), and a curable resin layer (b) laminated in this order. By disposing the acrylic layer (c) between the base layer (a) and the curable resin layer (b), the adhesion between the base layer (a) and the curable resin layer (b) can be improved.
[0117] The acrylic layer (c) preferably contains a (meth)acrylic resin.
[0118] [(Meth)acrylic resin] The (meth)acrylic resin is not particularly limited as long as it is a polymer of a (meth)acrylic acid ester. Examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate.
[0119] The (meth)acrylic resin may be a homopolymer or a copolymer.
[0120] Among these, the (meth)acrylic resin preferably contains polymethyl methacrylate (PMMA) resin from the viewpoints of high transparency, excellent moldability, etc. The above-mentioned (meth)acrylic resins may be used alone or in combination of two or more kinds.
[0121] The content of the (meth)acrylic resin is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 90 to 100% by mass, based on the total mass of the acrylic layer (c).
[0122] [Additives] The acrylic layer (c) may further contain an additive.
[0123] The additives are not particularly limited, and examples thereof include ultraviolet absorbers, antioxidants, coloring inhibitors, inorganic particles, etc. These additives may be used alone or in combination of two or more kinds. [Structure of acrylic layer (c)] The thickness of the acrylic layer (c) is preferably 5 μm or more, more preferably 10 μm or more, and from the viewpoint of increasing the hardness of the cured product, is further preferably 20 μm or more, particularly preferably 30 μm or more, very preferably 30 to 80 μm, and most preferably 40 to 60 μm.
[0124] 2. Manufacturing method of laminate According to one aspect of the present invention, there is provided a method for producing a laminate.
[0125] In one embodiment, the method for producing a laminate includes a step (1-1) of forming a base layer (a) from a first resin composition, and a step (2-1) of forming a curable resin layer (b) from a second resin composition on the base layer (a).
[0126] In this case, instead of step (1-1), a step (1-2) of co-extruding the first resin composition and the third resin composition to form a precursor including the base layer (a) and the acrylic layer (c) may be included. When the step (1-2) is included, instead of step (2-1), a step (2-2) of forming a curable resin layer (b) from the second resin composition on the acrylic layer (c) on the precursor is included.
[0127] In this case, the first resin composition contains bisphenol A type polycarbonate. The second resin composition contains a (meth)acryloyl polymer having an acrylic equivalent of 200 to 600 g / mol. The third resin composition contains a (meth)acrylic resin.
[0128] Each step will be described below.
[0129] <Process (1-1)> The step (1-1) is a step of forming a substrate layer (a) from a first resin composition.
[0130] [First resin composition] The first resin composition contains bisphenol A polycarbonate. In addition, the first resin composition may further contain a plasticizer, an additive, and the like.
[0131] The bisphenol A polycarbonate, plasticizer, and additives used are as described above.
[0132] The composition of the first resin composition is appropriately adjusted so that the substrate layer (a) has a desired structure.
[0133] [Method of forming base layer (a)] The method for forming the base layer (a) is not particularly limited, but it is preferable to extrude the first resin composition.
[0134] The melting temperature of the first resin composition is not particularly limited, but is preferably from 230 to 320°C, and more preferably from 260 to 300°C.
[0135] The cooling temperature of the first resin composition is not particularly limited, but is preferably from 50 to 200°C, and more preferably from 70 to 150°C.
[0136] <Process (1-2)> The step (1-2) is a step of co-extruding the first resin composition and the third resin composition to form a precursor including the base layer (a) and the acrylic layer (c).
[0137] [First resin composition] The first resin composition used is the same as that used in step (1-1).
[0138] [Third resin composition] The third resin composition contains a (meth)acrylic resin. The third resin composition may further contain other additives and the like.
[0139] The composition of the third resin composition is appropriately adjusted so that the acrylic layer (c) has a desired structure.
[0140] [Method of forming precursor] The precursor is formed by co-extruding the first resin composition and the third resin composition, thereby forming a precursor including the base layer (a) and the acrylic layer (c).
[0141] The melting temperature and cooling temperature of the first resin composition are the same as those in the step (1-1).
[0142] The melting temperature of the third resin composition is not particularly limited, but is preferably from 200 to 280°C, and more preferably from 210 to 260°C.
[0143] The cooling temperature of the third resin composition is not particularly limited, but is preferably from 50 to 200°C, and more preferably from 70 to 150°C.
[0144] <Process (2-1)> The step (2-1) is a step of forming a curable resin layer (b) from a second resin composition on the base layer (a) formed in the step (1-1).
[0145] [Second resin composition] The second resin composition contains a (meth)acryloyl polymer having an acrylic equivalent of 200 to 600 g / mol. The second resin composition may further contain a polyfunctional acrylate compound, inorganic particles, a leveling agent, a photopolymerization initiator, a light stabilizer, a polymerization inhibitor, an additive, a dilution solvent, etc.
[0146] The dilution solvent is not particularly limited, but examples thereof include acetone, methyl ethyl ketone, cyclohexanone, etc. These dilution solvents may be used alone or in combination of two or more kinds.
[0147] The composition of the second resin composition is appropriately adjusted so that the curable resin layer (b) has a desired structure.
[0148] [Method of forming curable resin layer (b)] The method for forming the curable resin layer (b) is not particularly limited, but is preferably a method in which the second resin composition is applied onto the substrate layer (a).
[0149] Examples of the method for applying the second resin composition include spray coating, spin coating, bar coating, gravure coating, and die coating.
[0150] The coating film formed by application is preferably dried. For example, the dilution solvent that may be contained in the second resin composition is evaporated by drying, and the curable resin layer (b) can be obtained.
[0151] The drying temperature for the coating is preferably from 50 to 200°C, and more preferably from 70 to 150°C.
[0152] <Process (2-2)> Step (2-2) is a step of forming a curable resin layer (b) from a second resin composition on the acrylic layer (c) in the precursor formed in step (1-2), and can be performed in the same manner as step (2-1).
[0153] 3.Cured product According to one embodiment of the present invention, a cured product is provided. The cured product is obtained by curing the above-mentioned laminate. In this specification, "curing of the laminate" means curing the curable resin layer (b) of the laminate to obtain a cured film. Also, "cured film" means a cured film (single layer film) obtained by curing the curable resin layer (b). Furthermore, "cured product" means a laminate of two or more layers including each layer (such as the base layer (a)) derived from the laminate in addition to the cured film.
[0154] In one embodiment, the cured product includes a substrate layer (a) and a cured film of the curable resin layer (b). In another embodiment, the cured product includes a base layer (a), a cured film of the curable resin layer (b), and an acrylic layer (c). The cured product is preferably laminated in the order of the base layer (a), the acrylic layer (c), and the cured film of the curable resin layer (b). In this case, the configurations of the base layer (a) and the acrylic layer (c) are usually the same as those in the laminate.
[0155] The cured film of the curable resin layer (b) has high hardness. As a result, the cured product can have high scratch resistance, chemical resistance, etc. In one embodiment, the cured product can have high fingerprint wiping properties, weather resistance, adhesion, etc.
[0156] Since the cured product can be used as a thermoforming film (functional film, decorative film), it is preferable that the cured product is molded so as to cover the surface of a molded article. That is, in one embodiment, a thermoforming film-containing molded article is provided, which includes a molded article and the cured product according to the present invention arranged on the surface of the molded article.
[0157] The molded article is not particularly limited, but is preferably a molded article having an uneven surface. Examples of the molded article include goggles, sinks, organs, beds, and vehicle housings.
[0158] In a preferred embodiment, the molded article is a molded article having a concave-convex surface, and the laminate is three-dimensionally decorated (TOM) molded onto the molded article, thereby providing a three-dimensionally decorated molded article comprising a molded article having a concave-convex surface and a laminate arranged on the concave-convex surface.
[0159] 4. Manufacturing method of the cured product According to one aspect of the present invention, there is provided a method for producing a cured product. The method for producing a cured product includes a curing step of curing the above-mentioned laminate. The method for producing a cured product may further include a molding step of three-dimensionally molding the laminate onto a surface of a molded article.
[0160] [Molding process] The molding step is a step of three-dimensionally molding the laminate on the surface of the molded article. Since the curable resin layer (b) of the laminate is in an uncured state, the laminate has high three-dimensional moldability. As a result, even when three-dimensional molding is performed, the laminate has high conformability and is less likely to crack after molding.
[0161] (molded product) The molded article is not particularly limited, but for example, the above-mentioned molded articles are used.
[0162] (Laminate) As the laminate, the one described above is used.
[0163] (Three-dimensional molding) An example of three-dimensional molding is three-dimensional decoration (TOM) molding. As described above, the three-dimensional decoration (TOM) molding process includes the following steps: (1) a vacuum process in which a lower chamber that is open at the top and in which a molded product having a textured surface is placed, an upper chamber that is open at the bottom and in which a heater is placed, and the laminate of the present invention sandwiched between the lower chamber and the upper chamber are made airtight and then placed under vacuum conditions; (2) a heating process in which the laminate is heated using the heater; (3) a contact process in which the molded product having texture is brought into contact with the heated laminate; (4) an upper chamber de-vacuum process in which the upper chamber is placed under atmospheric pressure conditions; and (5) a lower chamber de-vacuum process in which the lower chamber is placed under atmospheric pressure conditions. In addition, the method may further include an upper chamber pressurizing step of introducing compressed air into the upper chamber after the upper chamber de-vacuuming step, and a trimming step of removing a part of the laminate disposed on the uneven surface after the lower chamber de-vacuuming step.
[0164] [Curing process] The curing step is a step of curing the laminate, more specifically, a step of curing the curable resin layer (b) in the laminate by a curing reaction to obtain a cured film of the curable resin layer (b).
[0165] The curing reaction is not particularly limited, but is preferably carried out by irradiation with active energy rays.
[0166] Examples of the active energy rays include ultraviolet rays, electron beams, and radiation, and ultraviolet rays are preferable.
[0167] The amount of irradiation of the active energy rays is not particularly limited, but is preferably 100 to 5000 mJ / cm as the cumulative exposure amount at an ultraviolet wavelength of 365 nm. 2 is preferably 300 to 3000 mJ / cm 2 It is more preferable that: EXAMPLES
[0168] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.
[0169] 1. Raw materials (1) Polycarbonate resin T-1380: Bisphenol A (BPA) type polycarbonate resin using parahydroxybenzoic acid hexadecyl ester (p-HBAHE) as the end-capping agent (manufactured by Mitsubishi Gas Chemical Co., Ltd., viscosity average molecular weight: 25,500, Tig: 126°C, Tmg: 131°C) T-1300: Bisphenol A (BPA) type polycarbonate resin using parahydroxybenzoic acid hexadecyl ester (p-HBAHE) as the end-capping agent (manufactured by Mitsubishi Gas Chemical Company, Inc., viscosity average molecular weight: 30,500, Tig: 132°C, Tmg: 136°C) S-1000: Bisphenol A (BPA) type polycarbonate resin using para-tertiary butylphenol (pt-BPh) as the end-capping agent (manufactured by Mitsubishi Engineering Plastics Corporation, viscosity average molecular weight: 25,000, Tig: 147°C, Tmg: 151°C) FPC-0330: Bisphenol C (BPC) type polycarbonate resin using para-tertiary butylphenol (pt-BPh) as the end-capping agent (manufactured by Mitsubishi Gas Chemical Company, Inc., viscosity average molecular weight: 32,000, Tig: 123°C, Tmg: 126°C)
[0170] The structures of parahydroxybenzoic acid hexadecyl ester (p-HBAHE) and para-tertiary butylphenol (pt-BPh) are as follows: [ka]
[0171] (2) Plasticizers Plaxel H1P: Polycaprolactone (PCL) (manufactured by Daicel Corporation) SKYGREEN® J2003: PCTG (glycol-modified polycyclohexylene dimethylene terephthalate) (SK Chemicals, a polyester in which 80 mol% of the ethylene glycol, the raw material for PET, has been replaced with cyclohexanedimethanol) PX200: Resorcinol poly(di-2,6-xylyl) phosphate (manufactured by Daihachi Chemical Industry Co., Ltd.)
[0172] (3) PMMA (polymethyl methacrylate) resin Delpet 80HD: PMMA resin (manufactured by Asahi Kasei Corporation, methyl methacrylate (MMA): methyl acrylate = 99% by mass: 1% by mass, weight average molecular weight: 124,600)
[0173] (4) Curable resin raw material SMP-360A: Acryloyl group-containing polymer (Kyoeisha Chemical Co., Ltd., acrylic equivalent 360 g / mol) SMP-220A: Acryloyl group-containing polymer (Kyoeisha Chemical Co., Ltd., acrylic equivalent 220 g / mol) SMP-550A: Acryloyl group-containing polymer (Kyoeisha Chemical Co., Ltd., acrylic equivalent: 550 g / mol) PGM-AC4130Y: Nanosilica (Nissan Chemical Co., Ltd., average particle size 45 nm, surface acrylic treatment, PGM dispersion) MEK-AC2140Z: Nanosilica (Nissan Chemical Co., Ltd., average particle size 12 nm, surface acrylic treatment, MEK dispersion) MEK-AC5140Z: Nanosilica (Nissan Chemical Co., Ltd., average particle size 80 nm, surface acrylic treatment, MEK dispersion) Omnirad 184: Photoinitiator (IGM RESINS BV) ADK STAB LA-81: Hindered amine light stabilizer (manufactured by ADEKA Corporation) Phenothiazine (PTZ): Polymerization inhibitor (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) RS-90: Fluorine-based leveling agent (DIC Corporation) BYK-UV3500: Silicone leveling agent (manufactured by BYK)
[0174] 2.Measurement method (1) Glass transition temperature The glass transition temperature (Tg) of each resin and resin composition was measured by carrying out two cycles of heating and cooling according to the differential scanning calorimetry (DSC) measurement conditions below, and measuring the glass transition temperature during the second heating cycle. The intersection point between a straight line (line A) extending the low-temperature side baseline to the high-temperature side and the tangent to the inflection point (tangent B) was determined as the initial glass transition temperature (Tig). The intersection point between a straight line (line C) extending the high-temperature side baseline to the low-temperature side and the tangent to the inflection point (tangent B) was determined as the final glass transition temperature (Teg). The midpoint between the initial glass transition temperature (Tig) and the final glass transition temperature (Teg) was determined as the intermediate glass transition temperature (Tmg).
[0175] Measurement start temperature: 30℃ Heating rate: 10℃ / min Achieved temperature: 250℃ The temperature drop rate was 20° C. / min. Measurement equipment: Differential scanning calorimeter "DSC7020" (Hitachi High-Tech Science Corporation)
[0176] (2) Viscosity average molecular weight The viscosity average molecular weight was calculated from Schnell's viscosity equation. Specifically, first, the intrinsic viscosity [η] (unit: dL / g) of the resin was measured using methylene chloride as a solvent. The temperature was set at 25°C. The specific viscosity [η] at each solution concentration [C] (g / dL) was measured using an Ubbelohde viscometer. sp The intrinsic viscosity was calculated from the obtained specific viscosity value and concentration according to the following formula.
number
[0177] Next, the viscosity average molecular weight [Mv] is calculated using Schnell's viscosity formula, i.e., η = 1.23 × 10 -4 Mv 0.83 Calculated from.
[0178] (3) Weight average molecular weight The weight average molecular weight (Mw) was measured by gel permeation chromatography. Specifically, the gel permeation chromatography apparatus used was an LC-20AD system (manufactured by Shimadzu Corporation), and the column was connected to an LF-804 (manufactured by Shodex). The column temperature was set to 40°C. The RI detector used was an RID-10A (manufactured by Shimadzu Corporation). Chloroform was used as the eluent, and a calibration curve was created using standard polystyrene (manufactured by Tosoh Corporation).
[0179] (4) Acrylic equivalent The acrylic equivalent was calculated using the formula "molecular weight / number of (meth)acryloyl groups".
[0180] (5) Average particle diameter The average particle diameter was determined by randomly selecting 30 inorganic particles observed with a transmission electron microscope (TEM), determining the maximum distance between two points on the outer surface of each particle as the particle diameter, and then calculating the average of these distances.
[0181] (6) Charpy impact strength The Charpy impact strength of the substrate layer (a) was measured in accordance with JIS K 7111-1:2012. Specifically, the polycarbonates and plasticizers used in Examples 1 to 22 and Comparative Examples 1 to 8 were melt-kneaded at a cylinder temperature of 260°C using a vented twin-screw injection molding machine (Sodick's "PE-100", intermeshing co-rotating twin-screw diameter 29 mm, plunger diameter 28 mm) and molded bodies (test pieces) measuring 80 mm in length, 10 mm in width, and 3 mm in thickness were produced at a mold temperature of 70°C. Then, a notched Charpy impact test was performed in accordance with JIS K7111-1:2012 to measure the Charpy impact strength. The unit is kJ / m. 2 As shown in.
[0182] 3. Manufacturing of laminates [Example 1] A laminate was produced in which a substrate layer (a), an acrylic layer (c), and a curable resin layer (b) were laminated in this order. (1) Preparation of a laminate (precursor) of a base layer (a) and an acrylic layer (c) Polycarbonate resin T-1380 was melt-kneaded at a cylinder temperature of 280° C. using a vented twin-screw extruder TEX30α (manufactured by The Japan Steel Works, Ltd.) with a screw diameter of 32 mm and a screw L / D of 31.5, and pellets were obtained by strand cutting.
[0183] Using the pellets and PMMA (polymethyl methacrylate) resin Delpet 80HD, a laminate (precursor) of a base material layer (a) and an acrylic layer (c) was produced. Specifically, a multi-layer extrusion device having a single screw extruder with a shaft diameter of 32 mm, a single screw extruder with a shaft diameter of 65 mm, a feed block connected to all the extruders, and a 650 mm wide T-die connected to the feed block was used, and PMMA resin (Delpet 80HD) was continuously introduced into the single screw extruder with a shaft diameter of 32 mm at a cylinder temperature of 240° C., and the pellets were continuously introduced into the single screw extruder with a shaft diameter of 65 mm at a cylinder temperature of 280° C., and extruded. At this time, the discharge amounts of the PMMA resin and the pellets were controlled so that the thickness of the acrylic layer (c) of the PMMA resin was 35 μm, and the thickness of the base layer (a) of the pellets was 90 μm, respectively. The feed block connected to all extruders was equipped with two-type, two-layer distribution pins, and the laminar flow was laminated and extruded into a sheet through a T-die. The sheet was then cooled while transferring a mirror surface using three mirror-finished rolls set at temperatures of 100°C, 90°C, and 120°C from the upstream side, to produce a laminate (precursor) consisting of a base layer (a) containing T-1380, a polycarbonate resin, and an acrylic layer (c) containing Delpet 80HD, a PMMA resin.
[0184] (2) Manufacturing of laminates Of the laminate (precursor) of the base material layer (a) and the acrylic layer (c), the curable resin layer (b) was formed on the acrylic layer (c) to produce a laminate.
[0185] 70 parts by weight of SMP-360A, an acryloyl group-containing polymer, 30 parts by weight of PGM-AC4130Y, a nanosilica, 3 parts by weight of Omnirad 184, a photopolymerization initiator, 1 part by weight of RS-90, a fluorine-based leveling agent, and cyclohexanone, a dilution solvent, were mixed by stirring to obtain a curable resin composition. At this time, cyclohexanone was added in an amount such that the solid content concentration of the curable resin composition was 25% by weight.
[0186] Of the laminate of the base layer (a) and the acrylic layer (c), the curable resin composition was applied onto the acrylic layer (c) with a bar coater so that the film thickness after drying would be 4 μm, and the resulting coating film was dried for 3 minutes at 130° C. to form the curable resin layer (b). In this way, a laminate in which the base layer (a), the acrylic layer (c), and the curable resin layer (b) were laminated in this order was produced.
[0187] [Examples 2 to 20] A laminate having a base layer (a), an acrylic layer (c), and a curable resin layer (b) laminated in this order was produced in the same manner as in Example 1, except that the types and amounts of raw materials used and the thickness of each layer were changed as shown in Tables 1-1 and 1-2.
[0188] [Example 21] A laminate of a substrate layer (a) and a curable resin layer (b) was produced.
[0189] (1) Preparation of a monolayer film consisting of a substrate layer (a) Using pellets of T-1380, a polycarbonate resin obtained in the same manner as in Example 1, a single-layer film consisting of a base layer (a) was produced. Specifically, a T-die melt extruder consisting of a twin-screw extruder TEX30α with a barrel diameter of 32 mm and a screw L / D of 31.5 (manufactured by Nippon Steel Works, Ltd.) equipped with a vent was used. Under the conditions of a discharge rate of 10 Kg / h, a screw rotation speed of 63 rpm, and a cylinder temperature of 280°C, the pellets were continuously introduced and extruded. They were extruded into a sheet shape using a T-die connected to the extruder and cooled while transferring the mirror surface with three mirror-finished rolls set at temperatures of 120°C, 120°C, and 120°C from the upstream side, thereby obtaining a single-layer film composed of a base material layer (a) containing T-1380, a polycarbonate resin.
[0190] (2) Manufacture of laminate A curable resin layer (b) was formed on the base material layer (a) in the same manner as in Example 1 so as to have the composition described in Table 1, and a laminate in which the base material layer (a) and the curable resin layer (b) were laminated was manufactured.
[0191] [Example 22, Comparative Examples 1 to 8] Except that the types of raw materials used, their amounts used, and the thicknesses of each layer were changed as shown in Table 1-3, a laminate in which a base material layer (a), an acrylic layer (c), and a curable resin layer (b) were laminated in this order, or a laminate in which a base material layer (a) and a curable resin layer (b) were laminated was manufactured in the same manner as in Example 1 or Example 21.
Table 1-1
Table 1-2
Table 1-3
[0192] <TOM moldability> TOM molding was performed using the laminate, and the followability and cracks were evaluated.
[0193] The laminate was cut to a size of 330 mm x 330 mm, and the adhesive layer was attached to the base layer (a) side. A spare lens for safety goggles (manufactured by TRUSCO: product number TSG-005SP) was used as the adherend. The laminate with the adhesive layer and the adherend were set in the upper and lower boxes of a TOM molding machine NGF-0709-S (manufactured by Fuse Vacuum Co., Ltd.), and the pressure inside the upper and lower boxes was reduced to 0.1 kPa, and the laminate with the adhesive layer was heated to 140°C or 150°C. Then, compressed air of 0.3 MPa was introduced only into the upper box to obtain a TOM molded body.
[0194] The conformability of the TOM compact was evaluated as follows. The evaluation was performed by five experts and judged by majority vote. The results are shown in Table 2 below. ◯: The laminate conforms to the shape of the adherend. △: The laminate does not conform to the shape of the adherend. ×: The laminate does not conform to the shape of the adherend.
[0195] The cracks in the TOM compacts were evaluated as follows. The evaluation was carried out by five experts and judged by majority vote. The results are shown in Table 2 below. ◯: No cracks in the laminate △: Fine cracks are observed on the surface of the laminate. ×: Large cracks are observed in the laminate.
[0196] <Pencil hardness> The laminate was cured and the resulting cured product was evaluated for pencil strength.
[0197] The cured product was prepared as follows. That is, the curable resin layer (b) of the laminate was irradiated with ultraviolet light using a conveyor-type UV irradiator ECS-401GX (manufactured by Eye Graphics Co., Ltd.). At this time, the ultraviolet light irradiation was 700 mJ / cm 2 (UV illuminometer manufactured by Oak Corporation, measuring wavelength 360 nm) As a result, a cured product was produced in which the curable resin layer (b) of the laminate was cured.
[0198] The pencil hardness of the cured product of the curable resin layer (b) was measured according to the conditions of JIS K 5600-5-4:1999, and was evaluated based on the hardest pencil that did not cause scratches. The results are shown in Table 2 below.
[0199] The pencil hardness increases in the following order: 6B, 5B, 4B, 3B, 2B, B, HB, F, H, 2H, 3H, 4H, 5H, 6H, 7H, 8H, and 9H.
[0200] <Chemical resistance> The chemical resistance of the cured product obtained by curing the laminate was evaluated. The cured product used was the same as that produced for the evaluation of pencil hardness.
[0201] Neutrogena SPF70 (a sunscreen containing homosalate, octocrylene, octisalate, and avobenzone) was applied to the surface of the cured product of the curable resin layer (b) and allowed to stand at 80°C for 1 hour. The surface was then washed with a neutral detergent, and the appearance was evaluated according to the following criteria. The results are shown in Table 2 below. ○: No abnormality on the surface ×: Whitening is observed on the surface.
[0202] <Scratch resistance> The scratch resistance of the cured product obtained by curing the laminate was evaluated. The cured product used was the same as that produced for the evaluation of pencil hardness.
[0203] The surface of the cured curable resin layer (b) is coated with #0000 steel wool at 100 gf / cm 2 The surface was scratched by moving it back and forth 15 times under a pressure of 1000 mm. The appearance after scratching was evaluated according to the following criteria. The results are shown in Table 2 below. ◎: No scratches are visible 〇: Very slight scratches △: Some scratches are visible ×: Scratches are visible all over the surface
[0204] <Weather-resistant adhesion> The laminate was cured and the cured product obtained was evaluated for weather resistance and adhesion. The cured product used was the same as that produced for the evaluation of pencil hardness.
[0205] The surface of the cured product of the curable resin layer (b) was irradiated with light under the following conditions. Equipment: SUV-W161 (manufactured by Iwasaki Electric Co., Ltd.) Light source: Metal halide lamp Test environment: 63℃ (black panel temperature), 50% RH Illuminance: 50mW / cm 2 (wavelength 365nm) Irradiation cycle: 24 hours (continuous irradiation)
[0206] After irradiation, the surface of the cured product of the curable resin layer (b) was evaluated for weather resistance adhesion according to the following criteria in accordance with JIS K5600-5-6: 1999. The results are shown in Table 2 below. ◎: The edges of the cut are completely smooth and there is no peeling on any of the lattices. ○: Peeling occurred in less than 40% of the squares ×: Peeling occurred in 40% or more of the squares.
[0207] <Fingerprint wipe-off ability> The laminate was cured and the cured product obtained was evaluated for its fingerprint wiping ability. The cured product used was the same as that produced for the evaluation of pencil hardness.
[0208] A fingerprint was left on the surface of the cured product of the curable resin layer (b). The fingerprint was then wiped off with a cloth, and the ease of wiping off the fingerprint was evaluated according to the following criteria. The results are shown in Table 2 below. ○: Fingerprints disappeared after 2 to 4 wipes. △: Fingerprints disappeared after 5 wipings. ×: Fingerprints disappeared after wiping six or more times.
[0209] [Table 2]
[0210] From the results in Table 2, it was found that the laminates of Examples 1 to 22 were excellent in three-dimensional moldability. In addition, it was found that the cured products obtained by curing the laminates of Examples 1 to 22 had high hardness.
Claims
1. A substrate layer (a); a curable resin layer (b) containing a (meth)acryloyl polymer having an acrylic equivalent of 200 to 600 g / mol; A laminate comprising: The substrate layer (a) contains 96% by mass or more of bisphenol A polycarbonate based on the total mass of the substrate layer (a), The intermediate glass transition temperature (Tmg) of the substrate layer (a) is 100 to 140°C.
2. The bisphenol A polycarbonate is a polycarbonate obtained by mixing bisphenol A, a carbonate binder, and a compound represented by the following formula (1): 【Chemistry 1】 [In the above formula (1), R 1 is an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms, R 2 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may be substituted with a halogen atom or an aryl group having 6 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms which may be substituted with a halogen atom, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 12 carbon atoms.
2. The laminate according to claim 1, which is a polycarbonate obtained by reacting a monohydric phenol end terminator represented by the formula:
3. 3. The laminate according to claim 2, wherein the monohydric phenol end terminator represented by formula (1) comprises at least one selected from the group consisting of parahydroxybenzoic acid 2-hexyldecyl ester, parahydroxybenzoic acid hexadecyl ester, parahydroxybenzoic acid dodecyl ester, and parahydroxybenzoic acid 2-ethylhexyl ester.
4. The (meth)acryloyl polymer is represented by the following formula (2): 【Chemistry 2】 [In the above formula (2), m is a single bond or an alkylene group having 1 to 4 carbon atoms; n is hydrogen or an alkyl group having 1 to 4 carbon atoms; p is a single bond or an alkylene group having 1 to 2 carbon atoms; q is hydrogen or an alkyl group having 1 to 12 carbon atoms which may be substituted with at least one substituent selected from the group consisting of an epoxy group, a hydroxyl group, and a (meth)acryloyl group. The laminate according to claim 1 , comprising a repeating unit represented by:
5. The (meth)acryloyl polymer is represented by the following formulas (2-a) to (2-c): 【Chemistry 3】 The laminate according to claim 4 , comprising at least one repeating unit represented by:
6. 2. The laminate according to claim 1, wherein the (meth)acryloyl polymer has an acrylic equivalent of 200 to 500 g / mol.
7. The laminate of claim 1 , wherein the curable resin layer (b) further comprises a leveling agent.
8. The laminate according to claim 7 , wherein the leveling agent comprises a fluorine-based leveling agent.
9. The laminate according to claim 1 , wherein the curable resin layer (b) further comprises inorganic particles.
10. The laminate according to claim 9, wherein the inorganic particles have an average particle size of 20 to 60 nm.
11. The laminate according to claim 1 , wherein the curable resin layer (b) further comprises a light stabilizer.
12. The laminate according to claim 1 , wherein the curable resin layer (b) further comprises a polymerization inhibitor.
13. The laminate according to claim 1 , wherein the curable resin layer (b) has a thickness of 5 μm or more.
14. Further comprising an acrylic layer (c), The laminate according to claim 1 , wherein the base layer (a), the acrylic layer (c), and the curable resin layer (b) are laminated in this order.
15. The laminate according to claim 14, wherein the acrylic layer (c) has a thickness of 20 μm or more.
16. The laminate according to claim 1 , which is used for vacuum forming.
17. The laminate according to claim 1 , which is used in TOM molding.
18. A cured product obtained by curing the laminate according to any one of claims 1 to 17.
Citation Information
Patent Citations
Thermoforming sheet, decorative sheet, and molding using them
JP2021146687A