Moisture-curable polyurethane resin composition, adhesive, and laminate
A moisture-curable polyurethane resin composition with a urethane prepolymer and monoesterified compound addresses adhesion and texture issues in water-repellent fabrics, enhancing adhesion and film strength in functional clothing.
Patent Information
- Application Number
- JP2024004464
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2024-01-16
- Publication Date
- 2024-11-28
AI Technical Summary
Existing urethane adhesives face challenges in achieving excellent adhesion to water-repellent fabrics while maintaining texture and film strength in moisture-permeable and waterproof functional clothing, due to the inhibitory effect of low surface energy water repellents and issues with adhesive application methods.
A moisture-curable polyurethane resin composition containing a urethane prepolymer with an isocyanate group, derived from a polyol and polyisocyanate, incorporating a monoesterified product of a compound with three hydroxyl groups to enhance adhesion and reduce surface energy differences.
The composition achieves excellent adhesion to water-repellent fabrics and maintains texture, with improved film strength and reduced adhesive application impact on fabric texture.
Smart Images

Figure 2024166059000001 
Figure 2024166059000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a moisture-curable polyurethane resin composition, an adhesive, and a laminate. [Background technology]
[0002] Moisture-permeable, waterproof functional clothing, which has both moisture permeability and waterproofness, is a structure in which a moisture-permeable film is bonded to a fabric with an adhesive, and as the adhesive, a urethane-based adhesive is generally used because of its good adhesion to both the moisture-permeable film and the fabric. Among the urethane-based adhesives, the amount of use of solvent-free moisture-curable polyurethane resin compositions is gradually increasing due to recent global regulations on solvent emissions and residual solvents (see, for example, Patent Document 1).
[0003] On the other hand, water-repellent fabrics are used for waterproof functional fabrics, which are made by soaking the fabric in a water-repellent agent and drying it to make them water-repellent. Conventionally, fluorine-based water-repellents have been used as water-repellents. However, with the global restrictions on the use of fluorine, the movement to eliminate fluorine has accelerated, in addition to switching from C8 fluorine to C6 fluorine, and long-chain alkyl-based C0 and silicon-based water-repellents are being used as raw materials for fluorine-alternative water-repellents. These water-repellents are low-surface energy materials, so they exhibit the water-repellency required for waterproof functional clothing, but they also cause adhesion inhibition of adhesives. If the adhesive is applied to a moisture-permeable film and then laminated to a non-water-repellent fabric, and the water-repellent treatment is performed after the composite is formed, the above-mentioned adhesion inhibition is not caused, but there is a problem in that the number of processes increases. On the other hand, when using water-repellent fabric, the adhesive applied to the film does not exhibit sufficient adhesion when laminated, so a method of increasing the amount of adhesive is considered, but this has a negative effect on the texture because it is used for clothing. Generally, there is a manufacturing method in which an adhesive is applied to a water-repellent fabric and then a moisture-permeable film is attached to it, but applying the adhesive to the fabric can cause the adhesive to soak into the fabric, adversely affecting the texture. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-202608 A Summary of the Invention [Problem to be solved by the invention]
[0005] The problem to be solved by the present invention is to provide a moisture-curable polyurethane resin composition that has excellent adhesion to fabrics (particularly water-repellent fabrics) and excellent texture. [Means for solving the problem]
[0006] The present invention provides a moisture-curable polyurethane hot-melt resin composition containing a urethane prepolymer (i) having an isocyanate group, which is a reaction product of a polyol (A) and a polyisocyanate (B), wherein the polyol (A) contains, as an essential component, a monoester (a1) of a compound having three hydroxyl groups.
[0007] The present invention also provides an adhesive comprising the moisture-curable polyurethane resin composition. The present invention also provides a laminate comprising at least a substrate (i) and a cured product of the moisture-curable polyurethane resin composition. Effect of the Invention
[0008] The moisture-curable polyurethane hot-melt resin composition of the present invention not only has an excellent texture, but also has excellent adhesion to various fabrics, including water-repellent fabrics. The moisture-curable polyurethane hot-melt resin composition also provides excellent film strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The moisture-curable polyurethane hot-melt resin composition used in the present invention is a reaction product of a polyol (A) containing a specific compound and a polyisocyanate (B), and contains a urethane prepolymer (i) having an isocyanate group.
[0010] The polyol (A) contains a monoester (a1) of a compound having three hydroxyl groups as an essential component in order to obtain excellent adhesion to fabrics (especially water-repellent fabrics) and texture. By grafting the monoester (a1) having a hydrophobic functional group to the urethane prepolymer (i), the polymer itself becomes more hydrophobic, and the difference in surface energy with respect to an adherend having low surface energy becomes smaller, thereby exhibiting excellent adhesion, particularly to water-repellent fabrics. Furthermore, excellent adhesion can be obtained without applying a large amount, which also contributes to excellent texture.
[0011] The monoester (a1) of the compound having three hydroxyl groups is obtained by esterifying one hydroxyl group of the compound having three hydroxyl groups with a monocarboxylic acid. As the compound having three hydroxyl groups, for example, glycerin, trimethylolpropane, polypropylene polyol having three hydroxyl groups, 1,2,4-butanetriol, etc. can be used. Among these, glycerin, trimethylolpropane, or polypropylene polyol having three hydroxyl groups is preferred from the viewpoint of obtaining even better adhesion to water-repellent fabrics. As the monocarboxylic acid, for example, one having an alkyl group with 8 to 22 carbon atoms can be used, and the number of carbon atoms is preferably 14 to 22 from the viewpoint of obtaining even better adhesion to water-repellent fabrics.
[0012] The amount of the monoester (a1) used is preferably 0.5 to 15.0% by mass, more preferably 1.0 to 10.0% by mass, in the polyol (A) in order to obtain even better adhesion to water-repellent fabrics.
[0013] The polyol (A) may be any other polyol in addition to the monoester (a1). Examples of the other polyols include polyether polyols, polyester polyols, polycarbonate polyols, polyacrylic polyols, and polybutadiene polyols. These polyols may be used alone or in combination of two or more. Among these, it is preferable to use polyether polyols and / or polyester polyols, since they provide even better flexibility and adhesiveness.
[0014] As the polyether polyol, for example, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, etc. can be used. These polyols may be used alone or in combination of two or more. The polyether polyol may be derived from plants. As the plant-derived polyether polyol, for example, "Bio PTMG" manufactured by Mitsubishi Chemical Corporation, "Bio PTG" manufactured by Hodogaya Chemical Co., Ltd., and biomass polypropylene glycol manufactured by Vithal Castor Polyols can be obtained as commercial products. When the polyether polyol is used, the amount of use is preferably 20 to 60 mass % in the polyol (A) from the viewpoint of obtaining even more excellent flexibility and adhesiveness.
[0015] As the polyester polyol, for example, a reaction product of a compound having two or more hydroxyl groups and a polybasic acid can be used. As the compound having two or more hydroxyl groups, for example, ethylene glycol, diethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, pentanediol, 2,4-diethyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, hexanediol, neopentyl glycol, hexamethylene glycol, glycerin, trimethylolpropane, bisphenol A, bisphenol F, and alkylene oxide adducts thereof can be used. As the polybasic acid, for example, adipic acid, glutaric acid, pimelic acid, suberic acid, dimer acid, sebacic acid, undecanedicarboxylic acid, hexahydroterephthalic acid, phthalic acid, phthalic anhydride, isophthalic acid, terephthalic acid, etc. can be used. When the polyester polyol is used, the amount used is preferably 40 to 70% by mass in the polyol (A) in terms of obtaining even better mechanical strength and adhesiveness.
[0016] The number average molecular weight of the other polyol is, for example, 500 to 100,000. The number average molecular weight of the other polyol indicates a value measured by gel permeation chromatography (GPC).
[0017] As the polyisocyanate (B), aromatic polyisocyanates such as polymethylene polyphenyl polyisocyanate, diphenylmethane diisocyanate, carbodiimide-modified diphenylmethane diisocyanate isocyanate, xylylene diisocyanate, phenylene diisocyanate, tolylene diisocyanate, and naphthalene diisocyanate; aliphatic or alicyclic polyisocyanates such as hexamethylene diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and tetramethylxylylene diisocyanate can be used. These polyisocyanates may be used alone or in combination of two or more. Among these, aromatic polyisocyanates are preferred, and diphenylmethane diisocyanate is more preferred, in view of obtaining even better reactivity and adhesion to fabric.
[0018] The amount of the polyisocyanate (B) used is preferably from 5 to 40 mass %, more preferably from 10 to 30 mass %, based on the total mass of the raw materials constituting the urethane prepolymer (i).
[0019] The hot-melt urethane prepolymer (i) is obtained by reacting the polyol (A) with the polyisocyanate (B), and has an isocyanate group that can form a crosslinked structure by reacting with moisture present in the air or in the substrate to which the moisture-curable polyurethane hot-melt resin composition is applied.
[0020] The hot-melt urethane prepolymer (i) can be produced, for example, by adding the polyisocyanate (B) to a reaction vessel containing the polyol (A) and reacting them under conditions in which the isocyanate groups of the polyisocyanate (B) are in excess of the hydroxyl groups of the polyol (A).
[0021] In producing the hot-melt urethane prepolymer (i), the equivalent ratio (isocyanate group / hydroxyl group) of the isocyanate group in the polyisocyanate (B) to the hydroxyl group in the polyol (A) is preferably 1.1 to 5, and more preferably 1.5 to 3, in order to obtain even better adhesion to fabrics.
[0022] The isocyanate group content (hereinafter abbreviated as "NCO%) of the hot-melt urethane prepolymer (i) obtained by the above method is preferably 1.5 to 10, more preferably 2 to 6, in view of obtaining even better adhesiveness. The NCO% of the hot-melt urethane prepolymer (i) is a value measured by potentiometric titration in accordance with JIS K1603-1:2007.
[0023] The moisture-curable polyurethane hot-melt resin composition used in the present invention contains the urethane prepolymer (i) as an essential component, but may contain other additives as necessary.
[0024] Examples of the other additives that can be used include light resistance stabilizers, curing catalysts, tackifiers, plasticizers, stabilizers, fillers, dyes, pigments, fluorescent brighteners, silane coupling agents, waxes, thermoplastic resins, etc. These additives may be used alone or in combination of two or more.
[0025] Next, the laminate of the present invention will be described.
[0026] The laminate of the present invention comprises at least a base material (i) and a cured product of the moisture-curable polyurethane hot-melt resin composition.
[0027] Examples of the fabric (i) that can be used include fiber substrates such as nonwoven fabrics, woven fabrics, knitted fabrics, etc. made of polyester fibers, polyethylene fibers, nylon fibers, acrylic fibers, polyurethane fibers, acetate fibers, rayon fibers, polylactic acid fibers, cotton, hemp, silk, wool, glass fibers, carbon fibers, and blends thereof; nonwoven fabrics impregnated with resins such as polyurethane resin; nonwoven fabrics further provided with a porous layer; and resin substrates.
[0028] In addition, the present invention shows excellent adhesion even when the above-mentioned fabric (i) is subjected to a water-repellent treatment (hereinafter, abbreviated as "water-repellent fabric"). In the present invention, the "water repellency" of the water-repellent fabric is grade 4 or higher in the water repellency test (spray test) of JIS L 1092:2020.
[0029] In the JIS L 1092:2020 water repellency test (spray test), a test specimen of approximately 200 mm x 200 mm is attached to the test specimen holding frame without creating wrinkles, and the center of the spray is aligned with the center of the holding frame, and the vertical direction of the test specimen is aligned so that it is parallel to the water flow and tilted at 45°. 250 ml of water adjusted to a temperature of 20 ± 3°C is sprayed onto the test specimen fixed to the holding frame for 25 to 30 seconds, and after spraying, excess water droplets are removed. After wiping off the water droplets remaining on the surface of the test specimen, the wetness of the test specimen is compared with a comparison sample in a wet state specified by JIS and judged as grade 1 to 5.
[0030] Grade 5: No water droplets separating, no traces left after wiping Grade 4: Water droplets separate, no traces left after wiping Grade 3: No penetration when dripped, traces left after wiping Grade 2: Permeation after dripping Grade 1: Complete penetration
[0031] Examples of a method for applying the moisture-curable polyurethane hot-melt resin composition include methods using a roll coater, a knife coater, a spray coater, a gravure roll coater, a comma coater, a T-die coater, an applicator, a dispenser, and the like.
[0032] After the moisture-curable polyurethane hot-melt resin composition is applied, it can be dried and cured by a known method.
[0033] The thickness of the cured product of the moisture-curable urethane hot-melt resin composition is, for example, in the range of 5 to 300 μm.
[0034] In addition, when the moisture-curable polyurethane hot melt resin composition of the present invention is used as an adhesive for moisture-permeable waterproof functional clothing, the moisture-curable polyurethane hot melt resin composition is preferably intermittently applied by a gravure roll coater or a dispenser, and the fabric (i) is bonded to a known moisture-permeable film. In such a case, the thickness of the cured product of the moisture-curable polyurethane hot melt resin composition is, for example, in the range of 5 to 50 μm. EXAMPLES
[0035] The present invention will now be described in more detail with reference to examples.
[0036] [Example 1] Into a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux condenser, 41 parts by mass of polypropylene glycol (number average molecular weight: 1,000, hereinafter abbreviated as "PEt-1"), 33 parts by mass of polypropylene glycol (number average molecular weight: 2,000, hereinafter abbreviated as "PEt-2"), 55 parts by mass of polyester polyol (reaction product of 1,6-hexanediol and orthophthalic acid, number average molecular weight: 2,000, hereinafter abbreviated as "PEs-1"), and 20 parts by mass of terpolyol (a reaction product of neopentyl glycol and orthophthalic acid, number average molecular weight: 1,000, hereinafter abbreviated as "PEt-2"), 39 parts by mass of polyester polyol (a reaction product of 1,6-hexanediol and sebacic acid, number average molecular weight: 3,500, hereinafter abbreviated as "PEs-3"), and 16 parts by mass of decanoic acid monoester of trimethylolpropane were mixed and heated under reduced pressure at 100 ° C. to dehydrate the water content to 0.05 mass % or less. Next, after cooling to 90 ° C., 49 parts by mass of diphenylmethane diisocyanate melted at 70 ° C. was added, the temperature was raised to 110 ° C., and the mixture was reacted for 3 hours until the isocyanate group content became constant, to obtain a urethane prepolymer, which was a moisture-curable polyurethane hot melt resin composition.
[0037] [Example 2] In a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux condenser, 16 parts by mass of PEt-1, 65 parts by mass of PEt-2, 35 parts by mass of PEs-1, 35 parts by mass of PEs-2, 47% by mass of PEs-3, and 6 parts by mass of glycerin stearic acid monoester were mixed and heated under reduced pressure at 100 ° C. to dehydrate the water content to 0.05% by mass or less. Next, after cooling to 90 ° C., 53 parts by mass of diphenylmethane diisocyanate melted at 70 ° C. was added, the temperature was raised to 110 ° C., and the mixture was reacted for 3 hours until the isocyanate group content became constant, to obtain a urethane prepolymer, which was used as a moisture-curable polyurethane hot melt resin composition.
[0038] [Example 3] In a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux condenser, 65 parts by mass of PEt-2, 31 parts by mass of PEs-1, 49 parts by mass of PEs-2, 49 parts by mass of polyester polyol (a reaction product of 1,6-hexanediol and adipic acid, number average molecular weight: 4,500, hereinafter abbreviated as "PEt-4"), and 10 parts by mass of stearic acid monoester of trimethylolpropane were mixed and heated under reduced pressure at 100 ° C. to dehydrate the water content to 0.05% by mass or less. Next, after cooling to 90 ° C., 57 parts by mass of diphenylmethane diisocyanate melted at 70 ° C. was added, the temperature was raised to 110 ° C., and the mixture was reacted for 3 hours until the isocyanate group content became constant, to obtain a urethane prepolymer, which was a moisture-curable polyurethane hot melt resin composition.
[0039] [Example 4] In a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux condenser, 53 parts by mass of PEtPEt-1, 53 parts by mass of PEt-2, 55 parts by mass of PEs-1, 20 parts by mass of PEs-2, 39 parts by mass of PEs-3, and 4 parts by mass of glycerin stearic acid monoester were mixed and heated under reduced pressure at 100 ° C. to dehydrate until the water content was 0.05 mass% or less. Next, after cooling to 90 ° C., 68 parts by mass of diphenylmethane diisocyanate melted at 70 ° C. was added, the temperature was raised to 110 ° C., and the mixture was reacted for 3 hours until the isocyanate group content became constant, to obtain a urethane prepolymer, which was used as a moisture-curable polyurethane hot melt resin composition.
[0040] [Example 5] In a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux condenser, 48 parts by mass of PEs-2, 10 parts by mass of PEs-3, 133 parts by mass of polyester polyol (a reaction product of diethylene glycol and sebacic acid, number average molecular weight: 2,000, hereinafter abbreviated as "PEs-5"), and 13 parts by mass of decanoic acid monoester of glycerin were mixed and heated under reduced pressure at 100 ° C. to dehydrate the water content to 0.05% by mass or less. Next, after cooling to 90 ° C., 37 parts by mass of diphenylmethane diisocyanate melted at 70 ° C. was added, the temperature was raised to 110 ° C., and the mixture was reacted for 3 hours until the isocyanate group content became constant, to obtain a urethane prepolymer, which was a moisture-curable polyurethane hot melt resin composition.
[0041] [Example 6] In a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux condenser, 69 parts by mass of PEt-2, 24 parts by mass of PEs-1, 43 parts by mass of PEs-2, 43 parts by mass of PEs-4, and 24 parts by mass of behenic acid monoester of glycerin were mixed and heated under reduced pressure at 100 ° C. to dehydrate until the water content was 0.05 mass% or less. Next, after cooling to 90 ° C., 54 parts by mass of diphenylmethane diisocyanate melted at 70 ° C. was added, the temperature was raised to 110 ° C., and the mixture was reacted for 3 hours until the isocyanate group content became constant, to obtain a urethane prepolymer, which was used as a moisture-curable polyurethane hot melt resin composition.
[0042] [Example 7] In a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux condenser, 31 parts by mass of PEt-1, 41 parts by mass of PEt-2, 31 parts by mass of PEs-1, 45 parts by mass of PEs-2, 49 parts by mass of PEs-4, and 8 parts by mass of behenic acid monoester of trimethylolpropane were mixed and heated under reduced pressure at 100 ° C. to dehydrate the water content to 0.05% by mass or less. Next, after cooling to 90 ° C., 64 parts by mass of diphenylmethane diisocyanate melted at 70 ° C. was added, the temperature was raised to 110 ° C., and the mixture was reacted for 3 hours until the isocyanate group content became constant, to obtain a urethane prepolymer, which was a moisture-curable polyurethane hot melt resin composition.
[0043] [Example 8] In Example 1, 41 parts by mass of PEt-1 was changed to a biomass polypropylene glycol (number average molecular weight: 1,000) manufactured by Vithal Castor Polyols, and 33 parts by mass of PEt-2 was changed to a biomass polypolypropylene glycol (number average molecular weight: 2,000) manufactured by Vithal Castor Polyols. A moisture-curable polyurethane hot-melt resin composition was obtained in the same manner as in Example 1.
[0044] [Comparative Example 1] In a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux condenser, 75 parts by mass of PEt-2, 31 parts by mass of PEs-1, 49 parts by mass of PEs-2 and 49 parts by mass of PEs-4 were mixed and heated under reduced pressure at 100 ° C. to dehydrate until the water content was 0.05 mass% or less. Next, after cooling to 90 ° C., 48 parts by mass of diphenylmethane diisocyanate melted at 70 ° C. was added, the temperature was raised to 110 ° C., and the mixture was reacted for 3 hours until the isocyanate group content became constant, to obtain a urethane prepolymer, which was used as a moisture-curable polyurethane hot melt resin composition.
[0045] [Method for measuring number average molecular weight] The number average molecular weights of the polyols used in the examples and comparative examples are values measured by gel permeation chromatography (GPC) under the following conditions.
[0046] Measurement equipment: High-speed GPC equipment (Tosoh Corporation "HLC-8220GPC") Column: The following columns manufactured by Tosoh Corporation were used, connected in series. "TSKgel G5000" (7.8mm I.D. x 30cm) x 1 "TSKgel G4000" (7.8mm I.D. x 30cm) x 1 "TSKgel G3000" (7.8mm I.D. x 30cm) x 1 "TSKgel G2000" (7.8mmI.D. x 30cm) x 1 Detector: RI (differential refractometer) Column temperature: 40℃ Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Injection volume: 100 μL (sample concentration 0.4% by mass in tetrahydrofuran solution) Standard sample: A calibration curve was prepared using the following standard polystyrene.
[0047] (Standard polystyrene) "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation
[0048] [Method for evaluating adhesion to fabric] The moisture-curable polyurethane hot-melt resin compositions obtained in the Examples and Comparative Examples were melted at 100°C, and then coated with a gravure roll coater (coating amount: 17.5±5 g / m 2 ) was used to intermittently coat a moisture permeable film (DIC CRISBON S-517 processed into a 15μm film), which was then bonded to water-repellent fabric 1 (a polyester fabric (Japan Standards Association, weft / weft: 75D / 36f-FDY, basis weight: 71.8g / m2) treated with a water repellent agent (Nicca Chemical Co., Ltd., Neoseed NR-8800) with a water repellency of grade 5; hereafter abbreviated as "fabric 1") and water-repellent fabric 2 (a polyester fabric (Japan Standards Association, weft / weft: 75D / 36f-FDY, basis weight: 71.8g / m2) treated with a water repellent agent (Nicca Chemical Co., Ltd., Neoseed NR-7080) with a water repellency of grade 5; hereafter abbreviated as "fabric 2"), and left for 24 hours in an atmosphere at a temperature of 23°C and a humidity of 50% to obtain processed fabrics. Each of the processed fabrics obtained was cut to a width of 1 inch, and the peel strength was measured using a Tensilon (Orientec Co., Ltd. Tensilon multipurpose machine "RTC-1210A") at a crosshead speed of 200 mm / min, and evaluated as follows. "T": 6N / cm or more. "F": Less than 6N / cm.
[0049] [How to evaluate texture] The processed fiber obtained in the above [Method for evaluating adhesion to fabric] was cut into a piece 1 inch wide and 8 cm long. Using a precision universal testing machine (Shimadzu Corporation's "Autoflaf AG-1"), the test piece was folded in half and attached so that 5 cm of the folded part was rounded and protruding from the top of the clamping jig. A flat indenter was pressed into the test piece at a test speed of 10 mm / min, and the stress at the time of 5 mm displacement was measured and evaluated as follows. “T”; 100mN or less "F": Over 100mN
[0050] [Film property evaluation method] The moisture-curable polyurethane hot melt resin compositions obtained in the examples and comparative examples were melted at 100°C, and then coated on flat release paper ("EK-100D" manufactured by Lintec Corporation) to a thickness of 30 μm using a roll coater, and left for 24 hours in an atmosphere of 23°C and 50% humidity to obtain a film. The obtained film was cut into strips of 5 mm width and 50 mm length, and was stretched using a precision universal testing machine "Autograph AG-NX" (manufactured by Shimadzu Corporation) under an environment of chuck distance of 40 mm, tensile speed of 10 mm / sec, temperature of 23°C, and humidity of 50%, to measure the stress when stretched 100%, and evaluated as follows. "T": Less than 10 MPa. "F": 10MPa or more.
[0051] [Table 1]
[0052] [Table 2]
[0053] It has been found that the moisture-curable polyurethane hot-melt resin composition of the present invention has excellent adhesion to water-repellent fabrics, texture, and film properties.
[0054] On the other hand, Comparative Example 1, which is an embodiment in which the monoesterified product (a1) was not used, was evaluated as being poor in terms of adhesiveness to the fabric.
Claims
1. A moisture-curable polyurethane hot-melt resin composition comprising a urethane prepolymer (i) having an isocyanate group, the urethane prepolymer (i) being a reaction product of a polyol (A) and a polyisocyanate (B), A moisture-curable polyurethane hot-melt resin composition, characterized in that the polyol (A) contains a monoester (a1) of a compound having three hydroxyl groups as an essential component.
2. The moisture-curable polyurethane hot melt resin composition according to claim 1, wherein the monoester (a1) has a structure derived from a monocarboxylic acid having 8 to 22 carbon atoms.
3. 2. The moisture-curable polyurethane hot-melt resin composition according to claim 1, wherein the compound having three hydroxyl groups is glycerin, trimethylolpropane, or a polypropylene polyol having three hydroxyl groups.
4. The moisture-curable polyurethane hot melt resin composition according to claim 1, wherein the amount of the monoester (a1) used is 0.5 to 15.0 mass% in the polyol (A).
5. 2. The moisture-curable polyurethane hot-melt resin composition according to claim 1, wherein the polyol (A) further contains a polyether polyol and / or a polyester polyol.
6. An adhesive comprising the moisture-curable polyurethane hot-melt resin composition according to claim 1.
7. A laminate comprising at least a substrate (i) and a cured product of the moisture-curable polyurethane hot melt resin composition according to claim 1.
8. 8. The laminate according to claim 7, wherein the fabric (i) is a water-repellent fabric.
Citation Information
Patent Citations
Sheet material
JP2017202608A