Impact modifier compositions and applications thereof

A polypropylene composition with specific styrenic block copolymers and polyolefin blends addresses the balance of impact resistance, clarity, and stiffness, enhancing mechanical properties and flow in polypropylene compositions.

JP2024166147APending Publication Date: 2024-11-28クレイトン·ポリマーズ·ネーデルラント·ベー·フェー
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024079181
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2024-05-15
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing polypropylene compositions lack a balance of improved impact resistance, clarity, high stiffness, tensile strength, and flow properties when using styrenic block copolymers as impact modifiers.

Method used

A polypropylene composition comprising a blend of polypropylene homopolymer, first and second hydrogenated styrenic block copolymers, and a polyolefin copolymer, with specific block compositions and ratios, to enhance impact resistance and maintain clarity, stiffness, and flow properties.

Benefits of technology

The composition achieves a 5-10% increase in impact strength, 5% increase in stiffness, and minimal reduction in clarity, while maintaining good flow properties, outperforming traditional polypropylene compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166147000001
    Figure 2024166147000001
  • Figure 2024166147000002
    Figure 2024166147000002
  • Figure 2024166147000003
    Figure 2024166147000003
Patent Text Reader

Abstract

To provide an improved polypropylene composition with SBCs having improved impact resistance and a good balance of transparency, high stiffness, tensile strength, flow properties, etc.SOLUTION: A polyolefin composition is disclosed comprising: (A) a polypropylene homopolymer; (B) an impact modifier containing (a) a first hydrogenated styrenic block copolymer (first HSBC), and (b) at least one polymer selected from (i) a second hydrogenated styrenic block copolymer (second HSBC) and (ii) a polyolefin copolymer; and (C) up to 25 wt. % of at least an additive. Each of the first and second HSBCs prior to the hydrogenation has a vinyl content of 70 to 95 wt.% and 0 to 50 wt.%, respectively. The impact modifier has a weight ratio of the first HSBC to the at least one polymer between 1:10 and 10:1. The polyolefin composition shows improved impact resistance and a balance of transparency and other mechanical properties.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to impact modifiers, their process for preparation and their use in polyolefin compositions. [Background technology]

[0002] Polyolefin-based polymers and compositions thereof are used in large quantities. Among polyolefins, polypropylene compositions have many applications, including packaging materials, machine parts, automobile parts, electrical appliances, etc. Such compositions need to have better mechanical properties, flexibility, scratch resistance, processability, heat resistance, etc. for the desired end use. Impact resistance is an important property that the compositions should have in order to compete with engineering thermoplastics.

[0003] Impact modifiers such as rubbery materials have been used to improve the impact resistance of compositions containing polypropylene. By incorporating rubbery materials, impact resistance can be achieved at the expense of reduced stiffness, flowability, transparency, etc. Styrenic block copolymer (SBC)-based impact modifiers have been used to improve the impact resistance of polyolefin compositions. Summary of the Invention [Problem to be solved by the invention]

[0004] There remains a need to provide improved polypropylene compositions having an SBC that has improved impact resistance and a good balance of clarity, high stiffness, tensile strength, flow properties, and the like. [Means for solving the problem]

[0005] Summary of the Invention In one aspect, the present disclosure relates to a polyolefin composition comprising, consisting essentially of, or consisting of: (A) 65-99 wt. % polypropylene homopolymer having a melt flow rate (MFR) of 0.25-100 dg / min measured at 230° C. under 2.16 kg load according to ASTM D1238; (B) (a) a first hydrogenated styrenic block copolymer (first HSBC) and (b) 1-35 wt. % impact modifier consisting essentially of at least one polymer selected from (i) a second hydrogenated styrenic block copolymer (second HSBC) and (ii) a polyolefin copolymer (POLC); and (C) up to 25 wt. % of at least an additive, based on the total weight of the polyolefin composition. The first HSBC has a block A and a block B. Each block A, prior to hydrogenation, is a polymer block of a vinyl aromatic monomer and each block B is a polymer block of a conjugated diene monomer. Block B has a vinyl content of 70-95 wt. % based on the total weight of polymerized conjugated diene monomers in block B. The second HSBC has a block A' and a block B'. ​​Each block A' before hydrogenation is a polymer block of a vinyl aromatic monomer and each block B' is a polymer block of a conjugated diene monomer. Block B' has a vinyl content of 0-50 wt. % based on the total weight of polymerized conjugated diene monomers in block B'. ​​The polyolefin copolymer has a vinyl content of 0.850-0.920 g / cm measured according to ASTM D792. 3 and a melt index (MI) measured according to ASTM D1238 at 190°C under a 2.16 kg load of 0.5 to 100 dg / min. The weight ratio of (a) to (b) is 1:10 to 10:1. When the at least one polymer is a second HSBC, at least one of the first HSBC or the second HSBC has a polystyrene content (PSC) of 15 to 50 wt.%.

[0006] In a second embodiment, the polyolefin composition exhibits, when compared to a polyolefin composition in the absence of the impact modifier, (i) a >5% increase in flexural secant modulus at 1° C., and (ii) a <10% decrease in permeability measured at a sample thickness of 1.6 mm, or (iii) a >10% increase in Charpy notched impact measured at 0° C., and (iv) a <5% decrease in permeability measured at a sample thickness of 1.6 mm, or (v) a >5% increase in Charpy notched impact measured at 21° C., and (vi) a <5% decrease in permeability measured at a sample thickness of 1.6 mm, or (vii) a >5% increase in Charpy notched impact measured at 21° C., and (viii) a <5% increase in Flexural Secant Modulus measured at 1° C., and (viii) a <5% decrease in Permeability measured at a sample thickness of 1.6 mm, or (viv) a <5% increase in Flexural Secant Modulus measured at 1.6 mm, and (vv) a <5% increase in Flexural Secant Modulus measured at 1.6 mm, and (vvi ... vi) <10% decrease in transmission measured at 1.6 mm sample thickness, or (vii) >10% increase in notched Izod impact measured at 21°C, and (viii) <5% decrease in transmission measured at 1.6 mm sample thickness, or (ix) >10% increase in yield strain, and (x) <5% decrease in transmission measured at 1.6 mm sample thickness, or (xi) >5% increase in elongation at break, and (xii) <5% decrease in transmission measured at 1.6 mm sample thickness. 1% flexural secant modulus is measured according to ASTM D790. Notched Charpy impact measured at 0°C and notched Charpy impact measured at 21°C are both according to ASTM D610. Notched Izod impact is measured at 21°C according to ISO 180. Yield strain is measured according to ISO 527-2. Elongation at break is measured according to ISO 527-2. Permeability is measured according to ASTM D1003.

[0007] In a third embodiment, the at least one polymer is a second hydrogenated styrenic block copolymer.

[0008] In a fourth embodiment, each block A and A′ independently has a molecular weight (M) of 1 to 40 kg / mol, measured according to ASTM 5296. p ). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The following terms are used throughout this specification:

[0010] "Consisting essentially of" means that the claimed composition contains primarily the specified material, with the allowance for additional components that do not materially affect the novel characteristics or function of the claimed invention, and if present, the amount of additional components is <30%, or <20%, or <10%.

[0011] "At least one of [a group, e.g., A, B, and C]" or "any of [a group, e.g., A, B, and C]" means a single member from the group, more than one member from the group, or a combination of members from the group. For example, at least one of A, B, and C includes, for example, A only, B only, or C only, as well as A and B, A and C, B and C; or A, B and C, or any other combination of A, B, and C.

[0012] A list of embodiments presented as "A, B, or C" should be interpreted as including the embodiments A only, B only, C only, "A or B," "A or C," "B or C," or "A, B, or C."

[0013] The "polystyrene content" or PSC of a block copolymer refers to the weight percent of polymerized vinyl aromatic monomer, such as styrene, in the block copolymer and is calculated by dividing the sum of the molecular weights of all vinyl aromatic units by the total molecular weight of the block copolymer. PSC can be determined using any suitable method, such as proton nuclear magnetic resonance (NMR).

[0014] "Vinyl content" refers to the content of conjugated diene monomers that polymerize via 1,2-addition in the case of butadiene, or 3,4-addition in the case of isoprene, resulting in monosubstituted olefin or vinyl groups adjacent to the polymer backbone. Vinyl content can be measured by nuclear magnetic resonance spectroscopy (NMR).

[0015] "Molecular weight" or Mw refers to the molecular weight (kg / mol) of the polystyrene equivalent of a polymer block or block copolymer. Mw can be measured by gel permeation chromatography (GPC) using polystyrene calibration standards, such as measured according to ASTM 5296. The GPC detector can be an ultraviolet or refractive index detector or a combination thereof. The chromatograph is calibrated using commercially available polystyrene molecular weight standards. The Mw of a polymer measured using a GPC so calibrated is the molecular weight of the polystyrene equivalent or apparent molecular weight. Mw as expressed herein is measured at the peak of the GPC trace, commonly referred to as the "peak molecular weight" of the polystyrene equivalent, and M p It is shown as:

[0016] A "bimodal" molecular weight of a polymer refers to two or more peaks of different molecular weights that are readily distinguishable in a plot of (x) molecular weight as a function of (y) relative percentage of polymers exhibiting a given molecular weight, such as that obtained by gel permeation chromatography (GPC) analysis of the polymer.

[0017] The present disclosure relates to a polyolefin composition comprising, consisting essentially of, or consisting of (A) a polypropylene homopolymer, (B) an impact modifier consisting essentially of at least one polymer selected from (a) a first hydrogenated styrenic block copolymer (first HSBC) and (b) i) a second hydrogenated styrenic block copolymer (second HSBC) and ii) a polyolefin copolymer (POLC), and (C) optional additives. The polyolefin composition exhibits improved impact resistance and a good balance of clarity, high stiffness, tensile strength, and flow properties.

[0018] (Polypropylene homopolymer) Polypropylene homopolymer is polypropylene homopolymer (e.g., isotactic, syndiotactic, atactic, etc.) produced via any process known in the art. Polypropylene homopolymer can be obtained from virgin or recycled sources, and if produced for the first time, can be based on petroleum or biosources.

[0019] In an embodiment, polypropylene blends are used in the polyolefin composition, for example, blends of polypropylene with random ethylene or butene copolymers of propylene, or crystalline random copolymers of ethylene and propylene in combination with rubbery ethylene-propylene copolymers. Polypropylene copolymers can be used, including copolymers of propylene with copolymerizable comonomers, such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-octene, or one or more conjugated or non-conjugated dienes. The comonomers can range from 0.05 to 40, or 0.5 to 30, or 1 to 20, or 5 to 30 weight percent, based on the total weight of the polypropylene copolymer.

[0020] In an embodiment, the polypropylene homopolymer is bimodal or multimodal in terms of molecular weight and has a molecular weight (M p ).

[0021] In an embodiment, the polypropylene homopolymer has a melting temperature (T m ).

[0022] In an embodiment, the polypropylene homopolymer has a crystallinity of 20-70%, or 25-65%, or 30-60%, or 35-55%, or >35%, or >40%, or >50%, as measured by Differential Scanning Calorimetry (DSC) heat of fusion according to ASTM F2625.

[0023] In an embodiment, the polypropylene homopolymer has a melt flow rate (MFR) of <400, or <300, or <200, or 5-100, or 0.25-100, or 0.25-75, or 0.50-70, or 15-65, or 20-40 dg / min at 230° C. with a 2.16 kg load, measured according to ASTM D1238.

[0024] In embodiments, the polypropylene homopolymer is used in an amount of 65-99, or 70-99, or 70-95, or 75-99, or 75-90 weight percent, based on the total weight of the polyolefin composition.

[0025] (Impact Modifier) The impact modifier comprises, consists essentially of, or consists of (a) a first HSBC having a vinyl content of 70-95 wt% before hydrogenation, and (b) at least one polymer selected from i) a second HSBC having a vinyl content of 0-50 wt% before hydrogenation, and ii) a POLC, in a weight ratio of first HSBC to the at least one polymer of 1:10-10:1, or 1:8-8:1, or 1:5-5:1, or 1:2-2:1.

[0026] (Hydrogenated styrenic block copolymer (HSBC)) The first HSBC and the second HSBC (if present) are independently obtained by hydrogenation of an SBC precursor which is either a linear, branched or radial block copolymer having at least one block A or A' and at least one block B or B'.

[0027] In embodiments, the SBC precursors are prepared by anionic polymerization using techniques known in the art. Other methods such as cationic polymerization can also be employed. Anionic polymerization initiators are generally organometallic compounds, such as organolithium compounds, such as ethyl-, propyl-, isopropyl-, n-butyl-, sec-butyl-, tert-butyl-, phenyl-, hexylbiphenyl-, hexamethylenedi-, butadienyl-, isoprenyl-, 1,1-diphenylhexyllithium or polystyryllithium. The amount of initiator required is calculated based on the molecular weight to be achieved and is generally 0.002-5 wt.% based on the amount of monomers to be polymerized. Suitable solvents for polymerization include aliphatic, cycloaliphatic or aromatic hydrocarbons having 4-12 carbon atoms, such as pentane, hexane, heptane, cyclopentane, cyclohexane, methylcyclohexane, decalin, isooctane, benzene, alkylbenzenes, such as toluene, xylene, ethylbenzene and mixtures thereof. Termination of the polymer chain can be achieved by quenching with a proton donor or a compound that has a leaving group that can be displaced by a carbanionic polymer chain.

[0028] In embodiments, the SBC precursor is ABA, BAB, ABAB, ABABA, (AB) n , (AB) n (A), (ABA) n , (ABA) n X, (AB) n X, (BAB) n X, (ABAB) n X, (ABABA) n X, A'-B'-A', B'-A'-B', A'-B'-A'-B', A'-B'-A'-B'-A', (A'-B') n , (A'-B') n (A'), (A'-B'-A') n , (A'-B'-A') n X, (A'-B') n X, (B'-A'-B') n X, (A'-B'-A'-B') nX, (A'-B'-A'-B'-A') n X or mixtures thereof; where n is an integer from 2 to 30; and X is the residue of a coupling agent. Each block A and A' may be the same or different and is independently derived from a vinyl aromatic monomer, and each block B and B' may be the same or different and is independently derived from a conjugated diene monomer.

[0029] In embodiments, the coupling agent comprises a di- or polyfunctional compound such as divinylbenzene, aliphatic or araliphatic hydrocarbon halides such as 1,2-dibromoethane, bis(chloromethyl)benzene, silicon tetrachloride, dialkyl- or diaryl silicon dichlorides, alkyl- or aryl silicon trichlorides, tin tetrachloride, alkyl silicon methoxides, alkyl silicon ethoxides, polyfunctional aldehydes such as terephthalic dialdehyde, ketones, esters, anhydrides, or epoxides, etc. In embodiments, the coupling agent is selected from methyltrimethoxysilane (MTMS), methyltriethoxysilane (MTES), tetramethoxysilane (TMOS), dimethyl adipate, gamma-glycidoxypropyltrimethoxysilane, and mixtures thereof.

[0030] In embodiments, the vinyl aromatic monomer is selected from the group consisting of styrene, para-methylstyrene, para-ethylstyrene, para-n-propylstyrene, para-iso-propylstyrene, para-n-butylstyrene, para-sec-butylstyrene, para-iso-butylstyrene, para-t-butylstyrene, isomers of para-decylstyrene, isomers of para-dodecylstyrene, ortho-substituted styrenes, meta-substituted styrenes, alpha-methylstyrene, 1,1-diphenylethylene, and mixtures thereof.

[0031] In an embodiment, the conjugated diene monomer is selected from the group consisting of isoprene, 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 1-phenyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 3-butyl-1,3-octadiene, farnesene, myrcene, piperylene, cyclohexadiene, and mixtures thereof.

[0032] In embodiments, each block A and A' has a molecular weight (M p ) independently.

[0033] In embodiments, block B has a vinyl content of ≧70 or >72 or >75 or 70-95 or 70-85 or 75-90 or 70-80 weight percent, based on the total weight of polymerized conjugated diene monomers in block B.

[0034] In embodiments, block B' has a vinyl content of ≦50, or 0 to 50, or 0 to 45, or <45 weight percent, based on the total weight of polymerized conjugated diene monomers in block B'.

[0035] In an embodiment, each block B and B′ has a molecular weight (M p ) independently.

[0036] In an embodiment, the first HSBC has a polystyrene content (PSC) of 5-50, or 10-45, or 5-40, or 10-40, or 5-35, or 10-35 wt.%, based on the total weight of the first HSBC.

[0037] In embodiments having an impact modifier comprising both a first HSBC and a second HSBC, the second HSBC independently has a polystyrene content (PSC) of 5-50, or 10-45, or 5-40, or 10-40, or 5-35, or 10-35 wt.%, based on the total weight of the second HSBC. Further, the polystyrene content (PSC) in at least one of the first HSBC or second HSBC is 15-50, or 15-35, or 18-40 wt.%, based on the total weight of the first HSBC or second HSBC, respectively.

[0038] In embodiments, each first HSBC and second HSBC (if present) independently has a molecular weight (M) of 10 to 500, or 20 to 300, or 50 to 250, or 20 to 240, or 40 to 220 kg / mol. p ).

[0039] In an embodiment, each first HSBC and second HSBC (if present) independently has a melt flow rate (MFR) at 230° C. under 2.16 kg load of at least 1 dg / min or >2 or >4 or >5 or 1-40 or 2-30 or 4-35 or 5-35 dg / min, measured according to ASTM D 1238.

[0040] In an embodiment, each of the first HSBC and second HSBC (if present) has a coupling efficiency (CE) of >60%, or >65%, or >70%, or 60-98%, or 65-95%.

[0041] In an embodiment, the first HSBC has a diblock content of <15, or <12, or <10, or 1-15, or 1-10 wt.%, based on the total weight of the first HSBC.

[0042] In an embodiment, each first HSBC and second HSBC (if present) is independently functionalized with at least one functional group, such as, for example, a hydroxyl group, an amino group, a carboxyl group, an acid anhydride group, an epoxy group, an isocyanate group, and a silanol group.

[0043] (Polyolefin Copolymer (POLC)) The POLC is selected from the group consisting of polyolefin elastomers (POE), polyolefin plastomers (POP), and mixtures thereof.

[0044] In an embodiment, the POE is selected from ethylene-α-olefin copolymers (EOC), propylene-α-olefin copolymers (POC), and mixtures thereof. EOC is a copolymer of ethylene and at least one C3-C 20 It may be a copolymer with an α-olefin and may contain ethylene in an amount of >50 or >60 or >70 or >80 or >90 or 50-90 wt.% based on the total weight of the EOC. In an embodiment, the POC is a copolymer of propylene and at least one C3-C 20 Copolymers with α-olefins, the POC contains propylene in an amount of >50 or >60 or >70 or >80 or >90 or 50-90 wt %, based on the total weight of the POC.

[0045] In an embodiment, the POLC is a copolymer of ethylene and at least one C3-C6 olefin selected from propylene, isobutylene, 1-butene, 1-hexene, 1-pentene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. 20 It is a copolymer with α-olefin.

[0046] The EOC can be selected from ethylene / butene (EB) copolymers, ethylene / hexene-1 copolymers, ethylene / octene copolymers, ethylene / α-olefin / diene modified (EAODM) interpolymers (e.g., ethylene / propylene / diene modified (EPDM) interpolymers, ethylene / propylene / octene terpolymers, and the like), and ethylene / propylene copolymers.

[0047] Examples of POCs include copolymers such as propylene / ethylene, propylene / 1-butene, propylene / 1-hexene, propylene / 4-methyl-1-pentene, propylene / 1-octene, propylene / ethylene / 1-butene, propylene / ethylene / ENB, propylene / ethylene / 1-hexene, propylene / ethylene / 1-octene, propylene / styrene, and propylene / ethylene / styrene.

[0048] In an embodiment, the POE is C4 to C 18 It further comprises a diolefin and / or an alkenylbenzene.

[0049] In an embodiment, the POLC is produced in a process that uses a catalyst selected from the group consisting of a metallocene catalyst (or constrained geometry) or a Ziegler-Natta catalyst.

[0050] In an embodiment, the POLC comprises two polyolefin copolymer fractions, POLC-1 and POLC-2, in suitable amounts, for example, 1:10 to 10:1 or 1:5 to 5:1. The POLC may have a bimodal molecular weight distribution. In an embodiment, the POLC composition has a weight ratio (M w-HMW / M w-LMW The ratio is 20 to 60, 25 to 50, or 30 to 40.

[0051] In an embodiment, the POLC has a viscosity of 0.850 to 0.920, or 0.853 to 0.915, 0.855 to 0.910, or 0.852 to 0.905 g / cm, measured according to ASTM D792. 3 has a density of

[0052] In an embodiment, the POLC has a melt index at 190° C. under 2.16 kg load of 0.5-100, or 1-80, or 5-70, or 5-50, or 5-40 dg / min, measured according to ASTM D1238.

[0053] In an embodiment, the POLC has a molecular weight (M p ).

[0054] In embodiments, the POLC has a polydispersity index (M w / M n ).

[0055] In embodiments, the POLC has a glass transition temperature (T g ).

[0056] In embodiments, the POLC has a melting point of >20°C, or >30°C, or 20-140°C, or 25-130°C, or 30-125°C.

[0057] (Polyolefin Composition) In an embodiment, the polyolefin composition contains the impact modifier in an amount of 1-35, or 1-30, or 5-30, or 10-30, or 5-25 wt %, based on the total weight of the polyolefin composition.

[0058] In an embodiment, the polyolefin composition comprises, based on the total weight of the composition, 65-99 wt. % of a polypropylene homopolymer; 1-35 wt. % of an impact modifier comprising a first HSBC and a second HSBC in a weight ratio of 1:10 to 10:1 or a first HSBC and a POLC in a weight ratio of 1:10 to 10:1; and up to 25 wt. % of optional additives.

[0059] (Optional Additives) The optional additives are selected from the group consisting of activators, curing agents, stabilizers, neutralizing agents, thickening agents, coalescing agents, slip agents, mold release agents, antimicrobial agents, surfactants, antioxidants, antiozonants, color changing pH indicators, plasticizers, tackifiers, film forming additives, dyes, pigments, UV stabilizers, UV absorbers, catalysts, fillers, other resins, redox couples, fibers, flame retardants, viscosity modifiers, wetting agents, degassing agents, toughening agents, adhesion promoters, colorants, heat stabilizers, light stabilizers, lubricants, flow control agents, anti-drip agents, anti-blocking agents, antistatic agents, processing aids, stress relief additives, foaming agents, foam nucleating agents, weld line strength promoters, and mixtures thereof.

[0060] Examples of fillers include sand, talc, dolomite, calcium carbonate, clay, silica, mica, wollastonite, feldspar, aluminum silicate, alumina, hydrated alumina, glass beads, glass microspheres, ceramic microspheres, thermoplastic microspheres, baryte, wood flour, glass fiber, wood fiber, carbon fiber, and mixtures thereof. The fillers can be surface treated before being added to the polyolefin composition.

[0061] In embodiments, the additives used in the polyolefin composition are up to 25 wt%, or 0.5-25, or 0.5-20, or 1-15, or 0.5-10, or >0.5, or <20 wt%, based on the total weight of the polyolefin composition.

[0062] In an embodiment, the polyolefin composition comprises talc in an amount of 0.5 to 15, or 1 to 10, or 3 to 12 wt %, based on the total weight of the polyolefin composition.

[0063] In an embodiment, the polyolefin composition further comprises an impact modifier other than the impact modifiers mentioned above. Examples include ethylene propylene diene (EPDM) monomer, ethylene-propylene (EPM) monomer, ethylene-propylene rubber (EPR), elastomeric polyolefin (POE), ethylene and propylene based copolymers and terpolymers, nitrile-butadiene rubber (NBR), isobutylene (IB), chlorinated rubber, chlorinated polyethylene (CM), isoprene, ethylene-butene, mixtures and derivatives thereof. The other impact modifiers, if present, are in an amount of 0-10 or 0.5-8 or 1-5 or >1 or <10 wt. %, based on the total weight of the polyolefin composition.

[0064] (Method of preparing impact modifier) The compositions can be prepared by dry blending or dry blending and melt extruding into pellets using suitable amounts of the ingredients. Dry blending and melt mixing can be carried out in a single or twin screw extruder.

[0065] (Polyolefin composition / processing method for molded products) The polyolefin compositions can be processed according to methods known in the art, where the components are combined and blended by melt mixing / extrusion into pellets and then formed into molded articles by known techniques such as injection molding, stretch blow molding, overmolding, rotomolding, thermoforming, casting, extrusion, profile extrusion and blow molding.

[0066] In embodiments, the polyolefin composition is compounded at a temperature of 80-250°C, 100-240°C, 120-220°C, or 150-230°C. The various components can be added and compounded together in any order or simultaneously. In some embodiments, the additives are added as a premixed masterbatch. The masterbatch is conveniently formed by melt compounding techniques.

[0067] (Properties of polyolefin composition) The polyolefin composition is characterized by having a good balance of properties among flexibility, impact resistance, rigidity, transparency, tensile strength, flow properties, and anisotropy for forming molded articles.

[0068] A polyolefin composition comprising A) 65-99 wt. % of a polypropylene homopolymer, B) 1-35 wt. % of an impact modifier comprising a first HSBC and a second HSBC in a weight ratio of 1:10 to 10:1, or a first HSBC and a POLC in a weight ratio of 1:10 to 10:1, and C) up to 25 wt. % of an additive, based on the total weight of the polyolefin composition, has at least one of the following properties: 28-75 or 28-72 or 29-70 or >28 or >30 or <50 kJ / m, all measured according to ASTM D610 2 Charpy notched impact at 21°C; 3-20 or 3-18 or 3-15 or >2 or <15 kJ / m 2 Charpy notched impact at 0°C; and 3 to 10 or 3 to 8 or 3 to 6 or >3 or <8 kJ / m 2 Charpy notched impact at -20°C.

[0069] 15-50 or 16-45 or 17-42 or >18 or <40 kJ / m, all measured according to ISO 180 2 notched Izod impact at 21°C; and 2 to 10 or 2 to 8 or 3 to 7 or >2 or <8 kJ / m 2 Notched Izod impact at -20°C.

[0070] >55% or >60% or >63% or 50-100%, 52-95% transmission; and <100% or <98% or 85-99 or 88-98% haze, all measured according to ASTM D1003 on a 3 mm sample thickness.

[0071] >70% or >75% or 70-100%, 75-95% transmission; and <95% or <90% or <85% or <80% or 60-95% or 60-90% or 60-85%, all measured in accordance with ASTM D1003 on a sample thickness of 1.6 mm.

[0072] Flexural secant modulus at 1% of 700-1200 or 800-1100 or 830-1150 or >800 or >820 or <1150 MPa measured in accordance with ASTM D790.

[0073] Flexural strength of 25-50 or 25-45 or 26-42 or >25 or <40 MPa, measured according to ASTM D790.

[0074] Tensile modulus measured according to ISO 527-2 of 900-1600 or 920-1550 or 940-1500 or >930 or <1550 MPa.

[0075] A yield stress of 20-35 or 21-32 or 20-30 or >20 or <30 MPa, measured according to ISO 527-2.

[0076] Yield strain of 5-18% or 6-15% or >5% or <15%, measured according to ISO 527-2.

[0077] Elongation at break measured according to ISO 527-2 of 100-400% or 110-370% or 120-350% or >110% or <350%.

[0078] In an embodiment, the polyolefin composition has the following balanced properties compared to the polyolefin composition in the absence of the impact modifier: (i) an increase of >5% in the bending secant modulus at 1 mm, and (ii) a decrease of <10% in the transmittance measured at a sample thickness of 1.6 mm, or (iii) a >10% increase in Charpy notched impact measured at 0°C, and (iv) a <5% decrease in transmittance measured at a sample thickness of 1.6 mm, or (v) an increase of >5% in Charpy notched impact measured at 21°C, and (vi) a decrease of <10% in transmittance measured at a sample thickness of 1.6 mm, or (vii) an increase in notched Izod impact of >10% measured at 21°C; and (viii) a decrease in transmittance of <5% measured at a sample thickness of 1.6 mm; or (ix) an increase in yield strain of >10%, and (x) a decrease in transmittance measured at a sample thickness of 1.6 mm of <5%, or (xi) an increase in elongation at break of >5%, and (xii) a decrease in transmittance measured at a sample thickness of 1.6 mm of <5%. and the transmittance property is measured in accordance with ASTM D1003.

[0079] (Uses of polyolefin compositions) The polyolefin compositions can be used to make a variety of molded articles through injection blow molding, injection molding, extrusion blow molding (EBM), coextrusion, cast film extrusion, blown film extrusion, injection stretch blow molding (ISBM), rotational molding, thermoforming, heat bonding, foam blow molding, pultrusion, calendar molding, additive manufacturing, or other known processing methods.

[0080] Hollow molded articles can be formed from the polyolefin compositions by either continuous or intermittent extrusion blow molding. In embodiments, hollow molded articles include bottles, containers, fuel tanks, drums, etc. Other molded articles include furniture, signs, wheels, toys, and garden items.

[0081] The polyolefin compositions can be used in plumbing, packaging applications, films, geomembranes, roofing applications, pond liners, caps and barriers, as well as multi-layer polyolefin sheets or films, containers and core layers of household products, medical moldings, bottles and caps. The polyolefin compositions can be used in automotive applications, such as interior trim, interior cladding, door panels, instrument panels, fascias, liftgates and consoles, etc.

[0082] In embodiments, the polyolefin composition is used to prepare textile fibers, which are then used to form spunbond fibers, staple fibers, multifilament yarns, knitted fabrics, woven fabrics, or nonwoven fabrics. EXAMPLES

[0083] The following examples are intended to be non-limiting.

[0084] Ingredients used in the examples include: PP-1 is a polypropylene homopolymer manufactured by Borealis with a MFR of 20 dg / min at 230° C. with a 2.16 kg load.

[0085] POLC-1 is 0.857g / cm 3 Density at 10dg / min, MI at 190℃ / 2.16kg, T at -58℃ g and an ethylene-octene copolymer having a melting temperature of 38°C.

[0086] POLC-2 is 0.868g / cm 3 Density at 10dg / min, MI at 190℃ / 2.16kg, T at -62℃ g and an ethylene-octene copolymer having a melting temperature of 121°C.

[0087] POLC-3 is 0.900g / cm 3 and an MI (190°C / 2.16 kg) of 10 dg / min.

[0088] The composition details of the first HSBC and the second HSBC are shown in Table 1. SEBS stands for poly(styrene-ethylene / butylene-styrene) and SEP stands for poly(styrene-ethylene / propylene).

[0089] [Table 1]

[0090] (Examples 1 to 34) The polyolefin compositions were prepared by dry blending the components and then compounding in a 25 mm twin screw extruder using a batch size of 5 lbs. The melt temperature was maintained at about 245°C. Test specimens for various measurements were prepared by injection molding with a hold time of around 6 seconds and a cooling time of about 30 seconds. The polyolefin compositions and mechanical properties of Examples 1-34 are shown in Tables 2-6.

[0091] [Table 2]

[0092] [Table 3]

[0093] [Table 4]

[0094] [Table 5]

[0095] [Table 6]

[0096] As used herein, the term "comprising" means including the elements or steps identified following the term, but any such elements or steps are not exhaustive and embodiments may include other elements or steps. Although the terms "comprising" and "including" have been used herein to describe various aspects, the terms "consisting essentially of" and "consisting of" can be used and are disclosed in place of "comprising" and "including" to provide more specific aspects of the disclosure.

Claims

1. (A) 65 to 99 weight percent polypropylene homopolymer, said polymer having a melt flow rate of 0.25 to 100 dg / min measured at 230° C. under 2.16 kg load according to ASTM D1238; (B) 1 to 35 weight percent of an impact modifier consisting essentially of: (a) a first hydrogenated styrenic block copolymer having a block A and a block B, each block A is a polymer block of a vinyl aromatic monomer; a first hydrogenated styrenic block copolymer, each block B being a polymer block of a conjugated diene monomer, said block B having a vinyl content of 70 to 95 weight percent, based on the total weight of polymerized conjugated diene monomer in said block B; (b) at least one polymer selected from: (i) a second hydrogenated styrenic block copolymer having a block A′ and a block B′, each block A' is a polymer block of a vinyl aromatic monomer; a second hydrogenated styrenic block copolymer, each block B' being a polymer block of a conjugated diene monomer, said block B' having a vinyl content of 0 to 50 weight percent, based on the total weight of polymerized conjugated diene monomer in said block B'; and (ii) 0.850 to 0.920 g / cm3 measured in accordance with ASTM D792 3 and a melt index of 0.5 to 100 dg / min measured at 190° C. under a 2.16 kg load according to ASTM D1238. wherein the weight ratio of (a) to (b) is from 1:10 to 10:1; and (C) up to 25 wt. %, based on the total weight of the polyolefin composition, of at least one additive A polyolefin composition comprising: A polyolefin composition, wherein when said at least one polymer is said second hydrogenated styrenic block copolymer, at least one of said first and said second hydrogenated styrenic block copolymers has a polystyrene content of 15 to 50 weight percent.

2. The polyolefin composition, when compared to a polyolefin composition in the absence of the impact modifier, (i) a >5% increase in bending secant modulus at 1%, and (ii) a <10% decrease in transmission, or (iii) an increase in Charpy notched impact measured at 0° C. of >10%; and (iv) a decrease in permeability of <5%, or (v) an increase in Charpy notched impact measured at 21° C. of >5%; and (vi) a decrease in permeability of <10%, or (vii) an increase in notched Izod impact measured at 21° C. of >10%, and (viii) a decrease in transmission of <5%, or (ix) an increase in yield strain of >10%, and (x) a decrease in permeability of <5%, or (xi) an increase in elongation at break of >5%, and (xii) a decrease in transmittance of <5%. having The 1% bending secant modulus is measured in accordance with ASTM D790; The Charpy notched impact measured at 0° C. and the Charpy notched impact measured at 21° C. are both measured in accordance with ASTM D610; The notched Izod impact is measured at 21° C. according to ISO 180; The yield strain is measured according to ISO 527-2; The elongation at break is measured according to ISO 527-2; The transmittance is measured according to ASTM D1003 at a sample thickness of 1.6 mm; The polyolefin composition of claim 1.

3. 3. The polyolefin composition of claim 1 or 2, wherein said at least one polymer is a second hydrogenated styrenic block copolymer.

4. Each block A and A' independently has a molecular weight (M) of 1 to 40 kg / mol, measured according to ASTM 5296. p 3. The polyolefin composition according to claim 1 or 2, wherein

5. 3. The polyolefin composition according to claim 1, wherein said block B has a vinyl content of 70 to 85% by weight and said block B' has a vinyl content of 0 to 45% by weight.

6. 3. The polyolefin composition according to claim 1, wherein one of the first and second hydrogenated styrenic block copolymers has a polystyrene content of 15 to 50 wt.%, and the other has a polystyrene content of 5 to 50 wt.%.

7. 3. The polyolefin composition of claim 1 or 2, wherein the first hydrogenated styrenic block copolymer has a diblock content of <15 wt.%.

8. 3. The polyolefin composition of claim 1 or 2, wherein said at least one polymer is a polyolefin copolymer.

9. The polyolefin copolymer has a viscosity of 0.853 to 0.915 g / cm 3 The polyolefin composition of claim 8 having a density of

10. The polyolefin composition of claim 8, wherein said polyolefin copolymer has a melt index of 5 to 50 dg / min, measured at 190° C. under a 2.16 kg load.

11. The polyolefin copolymer is a copolymer of ethylene and at least one C selected from propylene, isobutylene, 1-butene, 1-hexene, 1-pentene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, and mixtures thereof. 3 ~C 20 The polyolefin composition of claim 8 which is a copolymer with an α-olefin.

12. The polyolefin composition comprises: 28-75 kJ / m at 21°C 2 , 3 to 20 kJ / m at 0°C 2 , and 3 to 10 kJ / m at -20°C 2 Charpy notched impact measured according to ASTM D610, and 15-50 kJ / m at 21°C 2 , and 2 to 10 kJ / m at -20°C 2 Notched Izod impact measured according to ISO 180 The polyolefin composition according to claim 1 or 2, having

13. 3. The polyolefin composition according to claim 1 or 2, wherein said polyolefin composition has a transmission of >70% and a haze of <95%, each measured according to ASTM D1003 at a sample thickness of 1.6 mm.

14. The polyolefin composition comprises: 1% bending secant modulus from 700 to 1200 MPa; and Bending strength of 25 to 50 MPa 3. The polyolefin composition according to claim 1 or 2, wherein the polyolefin composition has at least one of the following properties:

15. The polyolefin composition comprises: A tensile modulus of 900 to 1600 MPa; Yield stress of 20 to 35 MPa, Yield strains between 5 and 18%, and Elongation at break: 100-400% 3. The polyolefin composition according to claim 1 or 2, having at least one of the following properties: