Molded body containing polycarbonate-polyorganosiloxane copolymer
A polycarbonate-polyorganosiloxane copolymer with specific structural units addresses the flexibility and transparency issues of polycarbonate and acrylic resins, offering a molded article with enhanced mechanical and optical properties.
Patent Information
- Application Number
- JP2024152747
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2017-12-28
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polycarbonate resins offer superior mechanical strength and moldability but are inferior in flexibility, while acrylic resins, though flexible and transparent, lack mechanical strength and moldability.
A molded article containing a polycarbonate-polyorganosiloxane copolymer with specific structural units, where the polyorganosiloxane block content is between 20% to 70% by mass, and durometer hardness of 25 to 72, achieving both flexibility and transparency.
The copolymer provides a molded article with excellent flexibility and transparency, suitable for various applications requiring both properties, including optical and mechanical durability.
Smart Images

Figure 2024166227000001 
Figure 2024166227000002 
Figure 2024166227000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a molded article which contains a polycarbonate-polyorganosiloxane copolymer and has flexibility and excellent transparency.
[0002] There is a demand for flexible resin molded products that can be attached to various shapes and can be deformed and processed according to various designs, such as lighting covers for street lamps and optical lenses. In these applications, flexibility as well as transparency and mechanical properties are required. As such a resin, acrylic resins have been widely studied from the viewpoints of high transparency and optical properties (Patent Document 1). Although acrylic resins are excellent in transparency and flexibility, they have the disadvantages of being inferior in mechanical strength, moldability, and handleability. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2003-277574 A Summary of the Invention [Problem to be solved by the invention]
[0004] Although polycarbonate-based resins are superior in mechanical strength and moldability to acrylic-based resins, they tend to be inferior in terms of flexibility. An object of the present invention is to provide a molded article which contains a polycarbonate-polyorganosiloxane copolymer and has both excellent flexibility and transparency. [Means for solving the problem]
[0005] The present inventors have found that by including a polycarbonate-polyorganosiloxane copolymer (hereinafter sometimes abbreviated as PC-POS copolymer) having specific structural units and satisfying specific conditions, a molded article having flexibility and excellent transparency can be obtained. That is, the present invention relates to the following [1] to
[10] .
[0006] [1] A molded article comprising a polycarbonate block (A-1) having a repeating unit represented by the following general formula (I) and a polyorganosiloxane block (A-2) having a repeating unit represented by the following general formula (II), wherein the content of the polyorganosiloxane block (A-2) is 20% by mass or more and 70% by mass or less, and wherein the molded article has a durometer hardness of 25 or more and 72 or less by a type D durometer measured in accordance with JIS K 6253-3:2012. [ka] [In the formula, R 1 and R 2 each independently represents a halogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. X represents a single bond, an alkylene group having 1 to 8 carbon atoms, an alkylidene group having 2 to 8 carbon atoms, a cycloalkylene group having 5 to 15 carbon atoms, an arylene group having 6 to 12 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, a fluorenediyl group, an arylalkylene group having 7 to 15 carbon atoms, an arylalkylidene group having 7 to 15 carbon atoms, -S-, -SO-, -SO2-, -O-, or -CO-. R 3 and R 4 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. a and b each independently represent an integer of 0 to 4.] [2] The molded article according to the above [1], wherein the content of the unit represented by the following general formula (III) in the polyorganosiloxane block (A-2) is 0.1 mol % or less. [ka] [In the formula, R 33 and R 34 R each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. 31 R represents an alkylene group having 1 to 8 carbon atoms, an alkylidene group having 2 to 8 carbon atoms, a cycloalkylene group having 5 to 15 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, an arylene group having 6 to 12 carbon atoms, a fluorenediyl group, an arylalkylene group having 7 to 15 carbon atoms, or an arylalkylidene group having 7 to 15 carbon atoms. 35 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. t represents the average chain length of the polyorganosiloxane.] [3] The molded article according to [1] or [2] above, wherein the number of repetitions of the polyorganosiloxane block (A-2) is 10 or more and less than 90. [4] The molded article according to any one of the above [1] to [3], wherein the polyorganosiloxane block (A-2) contains a unit represented by at least one of the following general formulas (II-I) to (II-III): [ka] [In the formula, R 3 ~R 6 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms; 3 ~R 6 may be the same or different. Y is -R 7 O-, -R 7 COO-, -R 7 NH-, -R 7 NR 8 -, -COO-, -S-, -R 7 COO-R 9 -O-, or -R 7 OR 10The R represents —O—, and a plurality of Y's may be the same or different. 7 R represents a single bond, a linear, branched or cyclic alkylene group, an aryl-substituted alkylene group, a substituted or unsubstituted arylene group, or a diarylylene group. 8 R represents an alkyl group, an alkenyl group, an aryl group, or an aralkyl group. 9 R represents a diarylene group. 10 represents a linear, branched or cyclic alkylene group, or a diarylene group. β represents a divalent group derived from a diisocyanate compound, or a divalent group derived from a dicarboxylic acid or a dicarboxylic acid halide. n represents the chain length of the polyorganosiloxane, n-1, p and q each represent an integer of 1 or more that indicates the number of repetitions of the polyorganosiloxane unit, and the sum of p and q is n-2.]
[0007] [5] The molded article according to any one of the above [1] to [4], wherein the polyorganosiloxane block (A-2) is represented by the following general formula (V): [ka] [In the formula, R 3 ~R 6 and n-1 are the same as those described in the above general formulas (II-I) to (II-III). 15 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms.] [6] The molded article according to any one of the above [1] to [5], wherein the polycarbonate-polyorganosiloxane copolymer (A) has a viscosity average molecular weight of 10,000 or more and 23,000 or less. [7] The molded article according to any one of the above [1] to [6], wherein the molecular weight distribution of the polycarbonate-polyorganosiloxane copolymer (A) is 2.1 or more and 3.9 or less. [8] The molded article according to any one of the above [1] to [7], which has a total light transmittance at a thickness of 2 mm of 75% or more, as measured in accordance with JIS K 7361-1:1997. [9] The molded article according to any one of the above [1] to [8], which is an optical member.
[10] Flexible displays, light guide plates, housings, water-repellent and oil-repellent films, optical adhesives, switch covers, heat sealants, waterproofing materials, sealants, connectors, adapters, smartphone covers, lenses, eyeglass and sunglasses parts, optical fiber parts, cushioning materials for car batteries, wiper blades, convex mirrors, side mirrors, rearview mirrors, lamp covers, bumpers, windows, exterior materials, interior materials, sound-absorbing materials, steering wheel covers, sensor covers, watch parts, stationery, cosmetic containers, aquariums for raising aquatic organisms, shoe soles, cups, nail art, toys, artificial bait, suction cups, cooking utensils such as steamers, clothing, silicone wipes The molded article according to any one of the above [1] to [8], which is at least one selected from a cleaning sheet, a remote control cover, an umbrella, a metal container lining, a building material cover, a door, a window, a glass interlayer, a tent, a mirror, a show window case, a vinyl greenhouse, a medical device housing, an infusion bag, an infusion tube, a syringe, a baby bottle, a mask, a face band, a filter part, a vibration-damping part, a robot housing, a drone housing, a shield, a bulletproof shield, a sports cushion, an airplane window, a resin compatibilizer, a lighting cover, a light guide, a light guiding panel, a lighting unit, a prism panel, a flat lens, a Fresnel lens, a microlens array, and a collimator lens. Effect of the Invention
[0008] According to the present invention, a molded article containing a polycarbonate-polyorganosiloxane copolymer and having both excellent flexibility and transparency can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The molded article containing the polycarbonate-polyorganosiloxane copolymer of the present invention will be described in detail below. In this specification, the preferred definitions can be adopted arbitrarily, and it can be said that a combination of preferred definitions is more preferable. In this specification, the description "XX to YY" means "XX or more and YY or less."
[0010] The molded article of the present invention comprises a polycarbonate block (A-1) consisting of a repeating unit represented by the following general formula (I) and a polyorganosiloxane block (A-2) containing a repeating unit represented by the following general formula (II), and is characterized in that it comprises a polycarbonate-polyorganosiloxane copolymer (A) in which the content of the polyorganosiloxane block (A-2) is 20% by mass or more and 70% by mass or less, and has a durometer hardness of 25 or more and 72 or less by a type D durometer measured in accordance with JIS K 6253-3:2012.
[0011] [ka]
[0012] [In the formula, R 1 and R 2 each independently represents a halogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. X represents a single bond, an alkylene group having 1 to 8 carbon atoms, an alkylidene group having 2 to 8 carbon atoms, a cycloalkylene group having 5 to 15 carbon atoms, an arylene group having 6 to 12 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, a fluorenediyl group, an arylalkylene group having 7 to 15 carbon atoms, an arylalkylidene group having 7 to 15 carbon atoms, -S-, -SO-, -SO2-, -O-, or -CO-. R 3 and R 4 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. a and b each independently represent an integer of 0 to 4.]
[0013] The polycarbonate-polyorganosiloxane copolymer (A) contained in the molded article of the present invention will be described below. First, the polycarbonate block (A-1) represented by the general formula (I) will be described in detail. In the above general formula (I), R 1 and R 2 The halogen atoms each independently represent include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. R 1and R 2 Examples of the alkyl groups each independently represent include methyl, ethyl, n-propyl, isopropyl, various butyl groups (the term "various" refers to both linear and branched butyl groups, and the same applies below), various pentyl groups, and various hexyl groups. 1 and R 2 The alkoxy groups each independently represent include those in which the alkyl moiety is the above-mentioned alkyl group.
[0014] Examples of the alkylene group represented by X include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, and a hexamethylene group, and an alkylene group having 1 to 5 carbon atoms is preferable. Examples of the alkylidene group represented by X include an ethylidene group and an isopropylidene group. Examples of the cycloalkylene group represented by X include a cyclopentanediyl group, a cyclohexanediyl group, and a cyclooctanediyl group, and an alkylene group having 5 to 10 carbon atoms is preferable. Examples of the arylene group represented by X include a phenylene group, a naphthylene group, and a biphenylene group. Examples of the cycloalkylidene group represented by X include a cyclohexylidene group, a 3,5,5-trimethylcyclohexylidene group, and a 2-adamantylidene group, and an alkylidene group having 5 to 10 carbon atoms is preferable, and an alkylidene group having 5 to 8 carbon atoms is more preferable. The aryl moiety of the aryl alkylene group represented by X includes aryl groups having 6 to 14 ring carbon atoms, such as a phenyl group, a naphthyl group, a biphenyl group, and an anthryl group. The aryl moiety of the aryl alkylidene group represented by X includes aryl groups having 6 to 14 ring carbon atoms, such as a phenyl group, a naphthyl group, a biphenyl group, and an anthryl group.
[0015] a and b each independently represent an integer of 0 to 4, preferably 0 to 2, and more preferably 0 or 1. Among these, those in which a and b are 0 and X is a single bond or an alkylene group having 1 to 8 carbon atoms, or those in which a and b are 0 and X is an alkylidene group, particularly an isopropylidene group, are preferred. The polycarbonate block (A-1) may contain a plurality of types of polycarbonate blocks. When the polycarbonate block (A-1) contains a plurality of types of polycarbonate blocks, it is preferable from the viewpoint of transparency that a and b are 0, and X is an isopropylidene group accounts for preferably 90 mass % or more, more preferably 90.9 mass % or more, even more preferably 93.3 mass % or more, particularly preferably 95 mass % or more, and most preferably 100 mass %.
[0016] Next, the polyorganosiloxane block (A-2) represented by the general formula (II) will be described in detail. In the above general formula (II), R 3 or R 4 The halogen atoms each independently represent include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. 3 or R 4 Examples of the alkyl groups each independently represent include methyl, ethyl, n-propyl, isopropyl, various butyl groups, various pentyl groups, and various hexyl groups. 3 or R 4 The alkoxy group represented by each independently is exemplified by those in which the alkyl group moiety is the above-mentioned alkyl group. 3 or R 4 Examples of the aryl group that each independently represents include a phenyl group and a naphthyl group. R 3 and R 4 are preferably all hydrogen atoms, alkyl groups having 1 to 6 carbon atoms, alkoxy groups having 1 to 6 carbon atoms, or aryl groups having 6 to 12 carbon atoms, and more preferably all methyl groups.
[0017] The polyorganosiloxane block containing the repeating unit represented by general formula (II) preferably has units represented by the following general formulas (II-I) to (II-III). [ka] [In the formula, R 3 ~R 6 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms; 3 ~R 6 may be the same or different. Y is -R 7 O-, -R 7 COO-, -R 7 NH-, -R 7 NR 8 -, -COO-, -S-, -R 7 COO-R 9 -O-, or -R 7 OR 10 The R represents —O—, and a plurality of Y's may be the same or different. 7 R represents a single bond, a linear, branched or cyclic alkylene group, an aryl-substituted alkylene group, a substituted or unsubstituted arylene group, or a diarylene group. 8 R represents an alkyl group, an alkenyl group, an aryl group, or an aralkyl group. 9 R represents a diarylene group. 10 represents a linear, branched or cyclic alkylene group, or a diarylene group. β represents a divalent group derived from a diisocyanate compound, or a divalent group derived from a dicarboxylic acid or a dicarboxylic acid halide. n represents the average chain length of the polyorganosiloxane, n-1, p and q each represent an integer of 1 or more that indicates the number of repetitions of the polyorganosiloxane unit, and the sum of p and q is n-2.]
[0018] R 3 ~R 6 The halogen atoms each independently represent include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. 3 ~R6 Examples of the alkyl groups each independently represent include methyl, ethyl, n-propyl, isopropyl, various butyl groups, various pentyl groups, and various hexyl groups. 3 ~R 6 The alkoxy group represented by each independently is exemplified by those in which the alkyl group moiety is the above-mentioned alkyl group. 3 ~R 6 Examples of the aryl group that each independently represents include a phenyl group and a naphthyl group. R 3 ~R 6 is preferably a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. R in general formula (II-I), (II-II) and / or (II-III) 3 ~R 6 are preferably all methyl groups.
[0019] Y indicates -R 7 O-, -R 7 COO-, -R 7 NH-, -R 7 NR 8 -, -R 7 COO-R 9 -O- or -R 7 OR 10 R in -O- 7 The linear or branched alkylene group represented by the formula (I) is an alkylene group having 1 to 8 carbon atoms, preferably 1 to 5 carbon atoms, and the cyclic alkylene group is a cycloalkylene group having 5 to 15 carbon atoms, preferably 5 to 10 carbon atoms.
[0020] R 7 The aryl-substituted alkylene group represented by may have a substituent such as an alkoxy group or an alkyl group on the aromatic ring, and its specific structure can be, for example, the structure of the following general formula (i) or (ii). When the aryl-substituted alkylene group is present, the alkylene group is bonded to Si. [ka] (In the formula, c represents a positive integer, and is usually an integer of 1 to 6.)
[0021] R 7 , R 9 and R 10 The diarylene group represented by the formula (I) is a group in which two arylene groups are linked directly or via a divalent organic group, and specifically, -Ar 1 -W-Ar 2 - is a group having a structure represented by Ar 1 and Ar 2 represents an arylene group, and W represents a single bond or a divalent organic group. The divalent organic group represented by W is, for example, an isopropylidene group, a methylene group, a dimethylene group, or a trimethylene group. R 7 , Ar 1 and Ar 2 Examples of the arylene group represented by the formula (1) include arylene groups having 6 to 14 ring carbon atoms, such as a phenylene group, a naphthylene group, a biphenylene group, and an anthrylene group. These arylene groups may have any substituent, such as an alkoxy group or an alkyl group. R 8 The alkyl group represented by the formula (I) is a straight or branched group having 1 to 8 carbon atoms, preferably 1 to 5 carbon atoms. The alkenyl group is a straight or branched group having 2 to 8 carbon atoms, preferably 2 to 5 carbon atoms. The aryl group is a phenyl group, a naphthyl group, etc. The aralkyl group is a phenylmethyl group, a phenylethyl group, etc. R 10 The linear, branched or cyclic alkylene group represented by R 7 is the same as:
[0022] Y is preferably -R 7 O- and R 7 is an aryl-substituted alkylene group, particularly a residue of a phenolic compound having an alkyl group, and more preferably an organic residue derived from allylphenol or an organic residue derived from eugenol. With respect to p and q in formula (II-II), it is preferable that p=q. β represents a divalent group derived from a diisocyanate compound or a divalent group derived from a dicarboxylic acid or a dicarboxylic acid halide, and examples thereof include divalent groups represented by the following general formulas (iii) to (vii).
[0023] [ka]
[0024] The PC-POS copolymer (A) contained in the molded article of the present invention more preferably contains a polyorganosiloxane block (A-2) represented by the following structural formula. [ka] [In the formula, R 3 ~R 6 and n are the same as those defined in the above general formulas (II-I) to (II-III). 15 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms.]
[0025] The number of repetitions of the polyorganosiloxane block (A-2) in the PC-POS copolymer is preferably 10 or more and less than 90. More specifically, it is preferably 10 or more, more preferably 15 or more, particularly preferably 20 or more, and preferably less than 90, more preferably 80 or less, even more preferably 60 or less, even more preferably 45 or less, even more preferably 40 or less, particularly preferably less than 40. The number of repetitions is calculated by nuclear magnetic resonance (NMR) measurement. By setting the number of repetitions of the polyorganosiloxane block (A-2) within the above range, it is possible to achieve both excellent transparency and flexibility, and to suppress peeling after the production of a molded product.
[0026] The PC-POS copolymer (A) contained in the molded article of the present invention requires that the content of the polyorganosiloxane block (A-2) is 20% by mass or more and 70% by mass or less. By making the content of the polyorganosiloxane block (A-2) in the PC-POS copolymer 20% by mass or more, a copolymer with excellent flexibility can be obtained. If the content of the polyorganosiloxane block (A-2) is 70% by mass or less, the copolymer does not have significant tackiness and can maintain the shape of a flexible molded article. The content of the polyorganosiloxane block (A-2) in the PC-POS copolymer (A) contained in the molded article of the present invention is preferably 30 mass% or more, more preferably 40 mass% or more, even more preferably 45 mass% or more, and preferably 65 mass% or less, more preferably 60 mass% or less, even more preferably 55 mass% or less.
[0027] The viscosity average molecular weight of the PC-POS copolymer contained in the molded product of the present invention is preferably 10,000 or more and 23,000 or less. The viscosity average molecular weight (Mv) can be adjusted by using a molecular weight regulator (terminal terminator) or by adjusting the reaction conditions. By setting the viscosity average molecular weight in the above range, the copolymer has excellent moldability, and melt fracture of the molded product can be further suppressed, which is preferable. The viscosity average molecular weight (Mv) is more preferably 12,000 or more, even more preferably 14,000 or more, even more preferably 16,000 or more, and more preferably 21,500 or less, even more preferably 20,500 or less, even more preferably 19,500 or less, even more preferably 18,500 or less, and particularly preferably 18,000 or less. If the viscosity average molecular weight is 10,000 or more, sufficient strength of the molded product can be obtained. The viscosity average molecular weight (Mv) is a value calculated from the intrinsic viscosity [η] of a methylene chloride solution at 20° C. using the Schnell formula below.
[0028]
number
[0029] The weight average molecular weight (Mw) of the PC-POS copolymer of the present invention is preferably 40,000 or less. When the weight average molecular weight (Mw) is within the above range, a PC-POS copolymer having excellent flexibility can be obtained. The weight average molecular weight (Mw) of the PC-POS copolymer is more preferably 37,000 or less, further preferably 35,000 or less, and even more preferably 30,000 or less. In addition, the weight average molecular weight (Mw) is preferably 20,000 or more, and more preferably 23,000 or more.
[0030] The PC-POS copolymer (A) contained in the molded article of the present invention preferably has a molecular weight distribution (Mw / Mn) of 2.1 or more and 3.9 or less. When the molecular weight distribution Mw / Mn of the PC-POS copolymer is in the above range, non-uniformity due to asymmetric flow and phase separation during molding is suppressed, and a molded article having high transparency and easy control of flexibility is obtained, which is preferable. The above molecular weight distribution Mw / Mn of the PC-POS copolymer (A) is more preferably 2.3 or more, even more preferably 2.4 or more, still more preferably 2.5 or more, still more preferably 2.7 or more, particularly preferably 2.8 or more, and more preferably 3.5 or less, even more preferably 3.0 or less, particularly preferably 2.9 or less.
[0031] The PC-POS copolymer (A) can be produced by known production methods such as an interfacial polymerization method (phosgene method), a pyridine method, and an ester exchange method. In particular, when an interfacial polymerization method is adopted in which a polyorganosiloxane is added to a reaction system in which a dihydric phenol and a carbonate precursor are polymerized and copolymerized, the separation process between an organic phase containing the PC-POS copolymer and an aqueous phase containing unreacted materials and catalyst residues is facilitated, and the organic phase containing the PC-POS copolymer and the aqueous phase are easily separated in each washing process by alkali washing, acid washing, and pure water (ion-exchanged water) washing, and the PC-POS copolymer can be obtained efficiently, which is preferable. For example, the method described in JP-A-2014-80462 can be referred to as a method for producing a PC-POS copolymer.
[0032] Specifically, the polycarbonate oligomer and polyorganosiloxane, which have been previously prepared as described below, are dissolved in a non-water-soluble organic solvent (such as methylene chloride), an aqueous alkaline compound solution (such as an aqueous sodium hydroxide solution) of a dihydric phenol compound (such as bisphenol A) is added, and an interfacial polycondensation reaction is carried out in the presence of a terminal terminator (monohydric phenol such as p-tert-butylphenol) using a tertiary amine (such as triethylamine) or a quaternary ammonium salt (such as trimethylbenzylammonium chloride) as a polymerization catalyst. The PC-POS copolymer can also be produced by copolymerizing a polyorganosiloxane, a dihydric phenol, and phosgene, a carbonate ester, or a chloroformate.
[0033] When the PC-POS copolymer (A) contained in the molded article of the present invention is produced, for example, by reacting a polycarbonate oligomer with a polyorganosiloxane raw material in an organic solvent and then reacting it with a dihydric phenol, from the viewpoint of transparency of the obtained PC-POS copolymer, the solid weight (g / L) of the polycarbonate oligomer in 1 L of the mixed solution of the organic solvent and the polycarbonate oligomer is preferably in the range of 200 g / L or less, more preferably 180 g / L or less, and even more preferably 170 g / L or less. The transparency of the obtained copolymer is improved as the solids weight (g / L) of the polycarbonate oligomer in 1 L of the mixed solution of the organic solvent and the polycarbonate oligomer is lower, so there is no particular lower limit, but from the viewpoint of efficiently producing a PC-POS copolymer, the solids weight (g / L) is preferably 20 g / L or more, more preferably 30 g / L or more, and even more preferably 40 g / L or more.
[0034] As the polyorganosiloxane raw material, those represented by the following general formula (1), (2) and / or (3) can be used. [ka]
[0035] In the above formula, R 3 ~R 6 , Y, β, n-1, p and q are as described above, and specific examples and preferred ones are also as described above. Z represents a hydrogen atom or a halogen atom, and multiple Zs may be the same or different.
[0036] For example, examples of the polyorganosiloxane represented by general formula (1) include compounds represented by the following general formulas (1-1) to (1-11). [ka]
[0037] In the above general formulas (1-1) to (1-11), R 3 ~R 6 , n and R 8 is as defined above, and the preferred values are also the same. c represents a positive integer, and is usually an integer of 1 to 6. Among these, from the viewpoint of ease of polymerization, the phenol-modified polyorganosiloxane represented by the above general formula (1-1) is preferred. From the viewpoint of ease of availability, α,ω-bis[3-(o-hydroxyphenyl)propyl]polydimethylsiloxane, which is one of the compounds represented by the above general formula (1-2), and α,ω-bis[3-(4-hydroxy-3-methoxyphenyl)propyl]polydimethylsiloxane, which is one of the compounds represented by the above general formula (1-3), are preferred.
[0038] Alternatively, the polyorganosiloxane raw material may be one having the following general formula (4): [ka]
[0039] In the above formula, R 3 and R 4 is the same as above. The average chain length of the polyorganosiloxane block represented by the general formula (4) is (r×m), and the range of (r×m) is the same as n above. When the above (4) is used as the polyorganosiloxane raw material, the polyorganosiloxane block (A-2) preferably has a unit represented by the following general formula (II-IV).
[0040] [ka] [R in the formula 3 , R 4 , r and m are as defined above.
[0041] The polyorganosiloxane block (A-2) may have a structure represented by the following general formula (II-V). [ka] [In the formula, R 18 ~R 21 R is independently a hydrogen atom or an alkyl group having 1 to 13 carbon atoms. 22 Q is an alkyl group having 1 to 6 carbon atoms, a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 14 carbon atoms. 2 is a divalent aliphatic group having 1 to 10 carbon atoms. n-1 represents the number of repeating polyorganosiloxane blocks, and the range is as described above.]
[0042] In general formula (II-V), R 18 ~R 21 Examples of the alkyl group having 1 to 13 carbon atoms that R each independently represents include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, various butyl groups, various pentyl groups, various hexyl groups, various heptyl groups, various octyl groups, a 2-ethylhexyl group, various nonyl groups, various decyl groups, various undecyl groups, various dodecyl groups, and various tridecyl groups. 18 ~R 21 is preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and more preferably a methyl group.
[0043] R 22 Examples of the alkyl group having 1 to 6 carbon atoms represented by R include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, various butyl groups, various pentyl groups, and various hexyl groups. 22 Examples of the halogen atom represented by R include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. 22 The alkoxy group having 1 to 6 carbon atoms represented by R 1 may be one in which the alkyl group moiety is the above-mentioned alkyl group. 22 Examples of the aryl group having 6 to 14 carbon atoms include a phenyl group, a toluyl group, a dimethylphenyl group, and a naphthyl group. Among the above, R 22 is preferably a hydrogen atom or an alkoxy group having 1 to 6 carbon atoms, more preferably a hydrogen atom or an alkoxy group having 1 to 3 carbon atoms, and even more preferably a hydrogen atom.
[0044] Q 2 The divalent aliphatic group having 1 to 10 carbon atoms represented by is preferably a linear or branched divalent saturated aliphatic group having 1 to 10 carbon atoms. The number of carbon atoms in the saturated aliphatic group is preferably 1 to 8, more preferably 2 to 6, even more preferably 3 to 6, and still more preferably 4 to 6. The repeat number n-1 is as described above.
[0045] A preferred embodiment of the structural unit (II-V) is a structure represented by the following formula (II-VI). [ka] [In the formula, n-1 is the same as above.]
[0046] The polyorganosiloxane block (A-2) represented by the above general formula (II-V) or (II-VI) can be obtained by using a polyorganosiloxane raw material represented by the following general formula (5) or (6). [ka] [In the formula, R 18~R 22 , Q 2 , and n-1 are as defined above.] [ka] [In the formula, n-1 is as defined above.]
[0047] The method for producing the polyorganosiloxane is not particularly limited.For example, according to the method described in JP-A-11-217390, cyclotrisiloxane and disiloxane are reacted in the presence of an acid catalyst to synthesize α,ω-dihydrogenorganopentasiloxane, and then, in the presence of a catalyst for hydrosilylation reaction, the α,ω-dihydrogenorganopentasiloxane is subjected to an addition reaction with a phenolic compound (e.g., 2-allylphenol, 4-allylphenol, eugenol, 2-propenylphenol, etc.), etc., to obtain crude polyorganosiloxane. According to the method described in Japanese Patent No. 2662310, octamethylcyclotetrasiloxane and tetramethyldisiloxane are reacted in the presence of sulfuric acid (acid catalyst), and the resulting α,ω-dihydrogenorganopolysiloxane is subjected to an addition reaction with a phenolic compound or the like in the presence of a hydrosilylation catalyst in the same manner as described above to obtain a crude polyorganosiloxane. The α,ω-dihydrogenorganopolysiloxane can be used by appropriately adjusting its chain length n depending on the polymerization conditions, or a commercially available α,ω-dihydrogenorganopolysiloxane can be used. Specifically, the hydrosilylation catalyst described in Japanese Patent Publication No. 2016-098292 can be used.
[0048] Polycarbonate oligomers can be produced by reacting a dihydric phenol with a carbonate precursor such as phosgene or triphosgene in an organic solvent such as methylene chloride, chlorobenzene, chloroform, etc. When producing polycarbonate oligomers using the transesterification method, they can also be produced by reacting a dihydric phenol with a carbonate precursor such as diphenyl carbonate.
[0049] As the dihydric phenol, it is preferable to use a dihydric phenol represented by the following general formula (viii). [ka] [In the formula, R 1 , R 2 , a, b and X are as defined above.]
[0050] Examples of the dihydric phenol represented by the general formula (viii) include bis(hydroxyphenyl)alkanes such as 2,2-bis(4-hydroxyphenyl)propane [bisphenol A], bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, and 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 4,4'-dihydroxydiphenyl, bis(4-hydroxyphenyl)cycloalkane, bis(4-hydroxyphenyl)oxide, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)sulfone, bis(4-hydroxyphenyl)sulfoxide, and bis(4-hydroxyphenyl)ketone. These dihydric phenols may be used alone or in combination of two or more. Among these, bis(hydroxyphenyl)alkane dihydric phenols are preferred, and bisphenol A is more preferred. When bisphenol A is used as the dihydric phenol, the resulting copolymer is a PC-POS copolymer in which X is an isopropylidene group and a=b=0 in the above general formula (i).
[0051] Examples of dihydric phenols other than bisphenol A include bis(hydroxyaryl)alkanes, bis(hydroxyaryl)cycloalkanes, dihydroxyaryl ethers, dihydroxydiaryl sulfides, dihydroxydiaryl sulfoxides, dihydroxydiaryl sulfones, dihydroxydiphenyls, dihydroxydiarylfluorenes, dihydroxydiaryladamantanes, etc. These dihydric phenols may be used alone or in combination of two or more.
[0052] Examples of bis(hydroxyaryl)alkanes include bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, bis(4-hydroxyphenyl)phenylmethane, bis(4-hydroxyphenyl)diphenylmethane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, bis(4-hydroxyphenyl)naphthylmethane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)propane, 2,2-bis(4-hydroxy-3-bromophenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3-chlorophenyl)propane, 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane, and 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane.
[0053] Examples of bis(hydroxyaryl)cycloalkanes include 1,1-bis(4-hydroxyphenyl)cyclopentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,5,5-trimethylcyclohexane, 2,2-bis(4-hydroxyphenyl)norbornane, 1,1-bis(4-hydroxyphenyl)cyclododecane, etc. Examples of dihydroxyaryl ethers include 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethylphenyl ether, etc.
[0054] Examples of dihydroxydiaryl sulfides include 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfide, etc. Examples of dihydroxydiaryl sulfoxides include 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide, etc. Examples of dihydroxydiaryl sulfones include 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfone, etc.
[0055] Examples of dihydroxydiphenyls include 4,4'-dihydroxydiphenyl, etc. Examples of dihydroxydiarylfluorenes include 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, etc. Examples of dihydroxydiaryladamantanes include 1,3-bis(4-hydroxyphenyl)adamantane, 2,2-bis(4-hydroxyphenyl)adamantane, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, etc.
[0056] Examples of dihydric phenols other than those mentioned above include 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisphenol, 10,10-bis(4-hydroxyphenyl)-9-anthrone, and 1,5-bis(4-hydroxyphenylthio)-2,3-dioxapentane.
[0057] In order to adjust the molecular weight of the resulting PC-POS copolymer, a terminal terminator (molecular weight regulator) can be used. Examples of the terminal terminator include monohydric phenols such as phenol, p-cresol, p-tert-butylphenol, p-tert-octylphenol, p-cumylphenol, p-nonylphenol, m-pentadecylphenol, and p-tert-amylphenol. These monohydric phenols may be used alone or in combination of two or more.
[0058] After the above-mentioned interfacial polycondensation reaction, the mixture is left to stand for an appropriate period to separate into an aqueous phase and an organic solvent phase [separation step], the organic solvent phase is washed (preferably with a basic aqueous solution, an acidic aqueous solution, and water in that order) [washing step], and the resulting organic phase is concentrated [concentration step] and dried [drying step], thereby obtaining the PC-POS copolymer (A) contained in the molded article of the present invention.
[0059] In the PC-POS copolymer (A) contained in the molded article of the present invention, the content of the unit represented by the following general formula (III) in the polyorganosiloxane block (A-2) is preferably 0.1 mol % or less. [ka] [In the formula, R 33 and R 34 R each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. 31 R represents an alkylene group having 1 to 8 carbon atoms, an alkylidene group having 2 to 8 carbon atoms, a cycloalkylene group having 5 to 15 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, an arylene group having 6 to 12 carbon atoms, a fluorenediyl group, an arylalkylene group having 7 to 15 carbon atoms, or an arylalkylidene group having 7 to 15 carbon atoms. 35 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. t represents the average chain length of the polyorganosiloxane.]
[0060] By controlling the content of the block represented by the above general formula (III) to 0.1 mol % or less, precise control can be exercised between the raw material polyorganosiloxane used in the production of the PC-POS copolymer and the chain length of the copolymer, thereby making it possible to obtain a molded article having the desired high flexibility and transparency. Specifically, by employing the above-mentioned interfacial polymerization method, a PC-POS copolymer having a content of the block represented by the above general formula (III) of 0.1 mol % or less can be obtained. The PC-POS copolymer (A) contained in the molded product of the present invention theoretically cannot contain the block represented by the above general formula (III) from the synthesis procedure, and the content thereof is substantially 0.0 mol %.
[0061] The content of the block represented by the general formula (III) in the PC-POS copolymer (A) is 13 Quantitative determination is performed based on the peak of C-NMR. The specific quantitative method is shown in the Examples. The lower limit of quantification for this quantitative method is 13 The baseline signal-to-noise ratio of the C-NMR chart indicates that the concentration is less than 0.1 mol%. In the region less than 0.1 mol%, quantitative determination is impossible, but semi-quantitative determination is possible. When semi-quantitative determination is performed, a relative comparison of the peak heights corresponding to (III) is performed. If a relative comparison of the peak heights is difficult, the lower limit for semi-quantitative determination can be further lowered by increasing the number of integrations to improve the signal-to-noise ratio. The content of the block represented by the above general formula (III) in the PC-POS copolymer (A) contained in the molded product of the present invention, as determined by the above-mentioned quantitative method or semi-quantitative method, is more preferably 0.08 mol % or less, even more preferably 0.05 mol % or less, and particularly preferably substantially 0.0 mol %.
[0062] In the conventional synthesis method, a mixture of a bisphenol monomer and a polyorganosiloxane monomer or a polyorganosiloxane is reacted with a polymerization-active phosgene gas. Therefore, even if the amount of the block represented by the above general formula (III) is reduced by improving the method of adding phosgene gas and the contact time, the contact between a plurality of polyorganosiloxane monomer molecules and the polymerization-active phosgene gas is unavoidable, and it is impossible to substantially reduce the amount of the block represented by the general formula (III) to 0.0 mol%. On the other hand, in the method for synthesizing the PC-POS copolymer contained in the molded product of the present invention, a bisphenol monomer is reacted with phosgene gas in advance to synthesize a bisphenol monomer or a bisphenol polycarbonate oligomer having chloroformate structures at both ends, and then a polymerization inactive polyorganosiloxane monomer or a polymerization inactive polyorganosiloxane monomer and a polymerization inactive bisphenol monomer are reacted with the bisphenol monomer having polymerization active chloroformate groups at both ends or the bisphenol polycarbonate oligomer having polymerization active chloroformate groups at both ends, so that the above general formula (III) cannot be substantially produced.
[0063] The resulting PC-POS copolymer can be melt-kneaded to obtain raw material pellets. In this case, other additives may be added during preparation of the raw material pellets within a range that does not impair the effects of the present invention. Examples of other additives include antioxidants, ultraviolet absorbers, release agents, reinforcing materials, fillers, elastomers for improving impact resistance, dyes, pigments, antistatic agents, resins other than polycarbonate, etc., and the amount of each additive can be appropriately selected at an appropriate ratio.
[0064] The melt kneading can be carried out by premixing using a commonly used device such as a ribbon blender or drum tumbler, followed by using a Henschel mixer, a Banbury mixer, a single screw extruder, a twin screw extruder, a multi-screw extruder, a co-kneader, etc. The heating temperature during kneading is usually appropriately selected within the range of 240° C. to 320° C. For this melt kneading, it is preferable to use an extruder, particularly a vent-type extruder.
[0065] <Molded body> The molded article of the present invention can be produced by injection molding, injection compression molding, extrusion molding, blow molding, press molding, vacuum molding, foam molding, etc., using the above melt-kneaded polycarbonate-polyorganosiloxane copolymer or the obtained pellets as a raw material. In particular, the molded article of the present invention is preferably a molded article obtained by using pellets of the above PC-POS copolymer (A) obtained by melt-kneading.
[0066] The molded article of the present invention is characterized by having both excellent flexibility and transparency. Each of these properties will be described in detail below.
[0067] The flexibility is described in detail below. The molded product of the present invention is required to have a durometer hardness of 25 or more and 72 or less using a type D durometer, which is measured in accordance with JIS K 6253-3:2012 by the method described in the Examples. Durometer hardness is an index showing indentation hardness. In order to obtain a molded body having high flexibility while maintaining a certain degree of mechanical strength, the type D durometer hardness must be within the above range. The molded body of the present invention containing the specific PC-POS copolymer (A) has excellent flexibility, so that it can be used as a lighting cover without using a packing member, and can be used for a light guide of a complex shape, and the ease of construction can be dramatically improved. Furthermore, even in the case of an optical member having a void structure with an undercut draft angle inside, it can be integrally molded without performing an internal cutting process, so it can be suitably used for a collimator lens. Due to its excellent transparency and flexibility, it is used in home appliances such as substrates, light guide plates, and housings for flexible displays, as well as water- and oil-repellent films, optical adhesives, switch covers, heat sealants, waterproofing materials, sealants, connectors, adapters, and smartphone covers; optical applications include lenses, eyeglass and sunglasses parts, and optical fiber parts; in the automotive industry, cushioning materials for on-board batteries, wiper blades, convex mirrors, side mirrors, rearview mirrors, lamp covers, bumpers, windows, glass intermediate layers, exterior materials, interior materials, sound-absorbing materials, steering wheel covers, and sensor covers; and in everyday items such as watch parts, letterpress, and other materials. The silicone rubber can be suitably used in stationery, cosmetic containers, tanks for raising aquatic organisms, shoe soles, cups, nail art, toys, artificial bait, suction cups, cooking utensils such as steamers, clothing, silicone wiping sheets, remote control covers, umbrellas, metal container linings, etc.; in the field of building materials, building material covers, doors, windows, glass intermediate layers, tents, mirrors, show window cases, vinyl greenhouses, etc.; in the field of medical equipment, medical device housings, infusion bags, infusion tubes, syringes, baby bottles, masks, face bands, filter parts, etc.; and in other fields, vibration damping parts, robot housings, drone housings, shields, bulletproof shields, sports cushions, airplane windows, resin compatibilizers, etc.
[0068] The molded article of the present invention has a durometer hardness of more preferably 30 or more, further preferably 40 or more, and more preferably 70 or less, further preferably 68 or less, as measured by a type D durometer. Depending on the application of the molded article of the present application, the preferred range of durometer hardness may change. For example, when used in an application that emphasizes flexibility, the durometer hardness is more preferably 28 or more and more preferably 33 or less. When used in an application that emphasizes mechanical strength, the durometer hardness is more preferably 60 or more and more preferably 65 or less. When used in an application that emphasizes both flexibility and mechanical strength, the durometer hardness is more preferably 45 or more and more preferably 50 or less.
[0069] Depending on the shape of the molded product, the durometer hardness may not be measured, but in that case, the molded product is melted once and molded again into a shape that allows the durometer hardness to be measured, so that the durometer hardness can be measured. The molding conditions in this case are the same as those of the molding method described in the examples. As the raw material for obtaining such a molded body, those obtained by cutting, disassembling, breaking, etc. a molded body or a member containing a molded body can be used.
[0070] The transparency will be described in detail. The molded article of the present invention preferably has a total light transmittance of 75% or more at a thickness of 2 mm, measured in accordance with JIS K 7361-1:1997. By making the total light transmittance 75% or more under the above conditions, the molded article has excellent transparency and can be suitably used as the above-mentioned optically transparent member. The total light transmittance at a thickness of 2 mm of the molded article of the present invention is more preferably 85% or more, further preferably 89% or more, even more preferably 90% or more, still further preferably 91% or more, and particularly preferably 92% or more.
[0071] The molded article of the present invention can be used as an optical member or a transparent member, and specifically, for flexible displays, light guide plates, housings, water-repellent and oil-repellent films, optical pressure sensitive adhesives, switch covers, heat sealants, waterproofing materials, sealants, connectors, adapters, smartphone covers, lenses, eyeglass and sunglasses parts, optical fiber parts, cushioning materials for in-vehicle batteries, wiper blades, convex mirrors, side mirrors, rearview mirrors, lamp covers, bumpers, windows, exterior materials, interior materials, sound absorbing materials, steering wheel covers, sensor covers, watch parts, stationery, cosmetic containers, aquariums for raising aquatic organisms, shoe soles, cups, nail art, toys, artificial bait, and suction cups. The present invention can be suitably used in at least one selected from cooking utensils such as steamers, clothing, silicone wipes, remote control covers, umbrellas, metal container linings, building material covers, doors, windows, glass interlayers, tents, mirrors, show window cases, vinyl greenhouses, medical device housings, infusion bags, infusion tubes, syringes, baby bottles, masks, face bands, filter parts, vibration damping parts, robot housings, drone housings, shields, bulletproof shields, sports cushions, airplane windows, resin compatibilizers, lighting covers, light guides, light guiding panels, lighting units, prism panels, flat lenses, Fresnel lenses, microlens arrays, and collimator lenses. EXAMPLES
[0072] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples. The characteristic values and evaluation results in each example were determined according to the following procedures.
[0073] (1) Polydimethylsiloxane chain length and content The ratio was calculated from the integral ratio of the methyl groups of polydimethylsiloxane measured by NMR. In this specification, polydimethylsiloxane may be abbreviated as PDMS. <Quantitative method for determining the chain length of polydimethylsiloxane> 1 H-NMR measurement conditions NMR device: JEOL RESONANCE ECA500 Probe: 50TH5AT / FG2 Observation range: -5 to 15 ppm Observation center: 5 ppm Pulse repetition time: 9 seconds Pulse width: 45° NMR sample tube: 5φ Sample size: 30-40mg Solvent: deuterated chloroform Measurement temperature: room temperature Number of times accumulated: 256 In the case of allylphenol-terminated polydimethylsiloxane A: The integral value of the methyl group of the dimethylsiloxane part observed around δ-0.02 to 0.5 B: Integral value of methylene group of allylphenol observed around δ2.50~2.75 Polydimethylsiloxane chain length = (A / 6) / (B / 4) In the case of eugenol-terminated polydimethylsiloxane A: The integral value of the methyl group of the dimethylsiloxane part observed around δ-0.02 to 0.5 B: Integral value of methylene group of eugenol observed around δ2.40~2.70 Polydimethylsiloxane chain length = (A / 6) / (B / 4)
[0074] <Method for quantifying polydimethylsiloxane content> Quantitative method for determining the amount of polydimethylsiloxane copolymerized in PTBP-terminated polycarbonate copolymerized with allylphenol-terminated polydimethylsiloxane NMR device: JEOL RESONANCE ECA500 Probe: 50TH5AT / FG2 Observation range: -5 to 15 ppm Observation center: 5 ppm Pulse repetition time: 9 seconds Pulse width: 45° Number of times accumulated: 256 NMR sample tube: 5φ Sample size: 30-40mg Solvent: deuterated chloroform Measurement temperature: room temperature A: Integral value of the methyl group of the BPA part observed around δ1.5-1.9 B: The integral value of the methyl group of the dimethylsiloxane part observed around δ-0.02 to 0.3 C: Integral value of the butyl group in the p-tert-butylphenyl moiety observed around δ1.2~1.4 a=A / 6 b=B / 6 c=C / 9 T=a+b+c f=a / T×100 g=b / T×100 h=c / T×100 TW=f×254+g×74.1+h×149 PDMS (wt%) = g × 74.1 / TW × 100
[0075] <Method for quantifying the amount of block represented by formula (III)> 13 C-NMR measurement conditions NMR device: JEOL RESONANCE ECA500 Probe: C5HPD / FG probe Observation range: -25 to 225 ppm Observation center: 100 ppm Pulse repetition time: 4 seconds Pulse width: 45° NMR sample tube: 10φ Sample size: 250-300mg Solvent: deuterated chloroform Measurement temperature: room temperature Number of times: 10,000
[0076] Measured under the above conditions 13 In a C-NMR chart, the area A of the signal peak of the carbonate bond of the block represented by formula (III) detected at 150.9 ppm using tetramethylsilane (TMS) as the standard, and the area B of the signal peak at 152.1 ppm detected as an overlap of the signals of the carbonate bond of the block represented by formula (Ia) and the block represented by formula (III-a) are calculated from the formula A / (A+B) (unit: mol%). The lower limit of quantification for this method is: 13 The concentration was calculated to be less than 0.1 mol% based on the signal-to-noise ratio of the baseline of the C-NMR chart. [ka] [ka] [In the above formula, R 1 ,R 2 ,R 31 ~R 35 , X, a, b and t are as defined above.
[0077] (2) Viscosity average molecular weight The viscosity average molecular weight (Mv) was calculated by the following formula (Schnell formula) using the intrinsic viscosity [η] obtained by measuring the viscosity of a methylene chloride solution at 20° C. using an Ubbelohde viscometer.
number
[0078] (3) Weight average molecular weight, molecular weight distribution The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) were measured under the following conditions using a high-speed GPC device HLC-8220GPC (manufactured by Tosoh Corporation) and calculated based on a general-purpose calibration curve prepared using molecular weight standards. Column temperature: 40℃ Columns: TSK-GEL GHXL-L, TSK-GEL G4000HXL, TSK-GEL G2000HXL (manufactured by Tosoh Corporation) Mobile phase solvent: Tetrahydrofuran Flow rate: 1.0ml / min Detector: RI Injection concentration: 10mg / 10ml Injection amount: 0.1ml Molecular weight standard sample: Polycarbonate 18,050 (Idemitsu Kosan Co., Ltd., molecular weight error ±5% / 17,148-18,953), Polycarbonate 18,100 (Idemitsu Kosan Co., Ltd., molecular weight error ±5% / 17,200-19,100)
[0079] (4) Durometer hardness The type A durometer hardness was measured under a load of 1 kg using a rubber hardness tester ESA type (manufactured by Elastron Co., Ltd.) and a constant pressure load device EDL-1 (manufactured by Elastron Co., Ltd.) in accordance with JIS K 6253-3:2012 Type A and ISO7619 Type A. The type D durometer hardness was measured under a load of 5 kg using a rubber hardness tester ESD type (manufactured by Elastron Co., Ltd.) and a constant pressure load tester EDL-1 special type (with oil damper, manufactured by Elastron Co., Ltd.) in accordance with JIS K 6253-3:2012 Type D and ISO7619 Type D.
[0080] (5) Total light transmittance The haze was measured at a thickness of 2 mm using a haze meter NDH 5000 (manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K 7361-1:1997.
[0081] <Production of polycarbonate oligomer> Sodium dithionite of 2000 ppm relative to bisphenol A (BPA) (to be dissolved later) was added to a 5.6% by mass aqueous solution of sodium hydroxide. BPA was dissolved in this so that the BPA concentration was 13.5% by mass, and an aqueous solution of sodium hydroxide of BPA was prepared. This aqueous solution of sodium hydroxide of BPA was continuously passed through a tubular reactor with an inner diameter of 6 mm and a tube length of 30 m at flow rates of 40 L / hr, methylene chloride at 15 L / hr, and phosgene at 4.0 kg / hr. The tubular reactor had a jacket, and cooling water was passed through the jacket to keep the temperature of the reaction solution below 40°C. The reaction liquid leaving the tubular reactor was continuously introduced into a 40 L baffled tank reactor equipped with a swept-back blade, where an aqueous sodium hydroxide solution of BPA was added at a flow rate of 2.8 L / hr, a 25% by mass aqueous sodium hydroxide solution at 0.07 L / hr, water at 17 L / hr, and a 1% by mass aqueous triethylamine solution at 0.64 L / hr to carry out the reaction. The reaction liquid overflowing from the tank reactor was continuously withdrawn and allowed to stand to separate and remove the aqueous phase, and the methylene chloride phase was collected. The polycarbonate oligomer thus obtained had a concentration of 341 g / L and a chloroformate group concentration of 0.71 mol / L.
[0082] Manufacturing Example 1 A 1 L separable flask equipped with a baffle plate and a mechanical stirrer with a stirring blade was charged with 185 mL of the polycarbonate oligomer solution (PCO) produced as described above, 445 mL of methylene chloride, 30.3 g of allylphenol-terminated polydimethylsiloxane with an average chain length n = 37, and 0.104 mL (0.75 mmol) of triethylamine (TEA), and to this was added a previously prepared sodium hydroxide aqueous solution A (NaOHaq) (sodium hydroxide 1.9 g (47 mmol), ion-exchanged water 22 mL) under stirring, and the polycarbonate oligomer and allylphenol-terminated PDMS were reacted for 20 minutes. Next, previously prepared sodium hydroxide aqueous solution B [BisP-AP (Honshu Chemical Industry Co., Ltd.): 4.8 g (16 mmol), sodium hydroxide: 2.9 g (73 mmol), ion-exchanged water: 42 mL, sodium hyposulfite (Na2S2O4): 0.006 g (0.038 mmol)] was further added, and polymerization was allowed to proceed for 20 minutes. To the obtained polymerization solution, a methylene chloride solution of p-tert-butylphenol (PTBP: manufactured by DIC Corporation) [PTBP: 1.5 g (10.0 mmol) dissolved in 10 mL of methylene chloride] and an aqueous sodium hydroxide solution of BPA C [bisphenol A: 7.4 g (26 mmol), NaOH: 5.2 g (131 mmol) and Na2S2O4: 0.006 g (0.038 mmol) dissolved in 77 mL of ion-exchanged water] were added and the polymerization reaction was carried out for 20 minutes. After the polymerization was completed, the reaction mixture was transferred to a separatory funnel and allowed to stand to separate into an organic phase and an aqueous phase, and the organic phase was transferred to another separatory funnel, where it was washed with 100 mL of 0.03 mol / L NaOH aqueous solution and 100 mL of 0.2 mol / L hydrochloric acid, and then repeatedly washed with ion-exchanged water until the electrical conductivity of the aqueous phase after washing was 10 μS / m or less. The organic layer obtained after washing was transferred to a tray and dried overnight at 48°C in an explosion-proof dryer (under nitrogen atmosphere) to obtain a sheet-like PC-POS copolymer. This sheet-like PC-POS copolymer was cut to obtain a flake-like PC-POS copolymer (a1). Details of the PC-POS copolymer are shown in Table 1-1.
[0083] Manufacturing Example 2 The amount of allylphenol-terminated polydimethylsiloxane was 40.4 g, the sodium hydroxide aqueous solution A was prepared by dissolving 1.9 g (47 mmol) of NaOH in 22 mL of ion-exchanged water, the sodium hydroxide aqueous solution B was prepared by dissolving 4.8 g (20 mmol) of BisP-B, 2.9 g (73 mmol) of NaOH, and 0.031 g (0.20 mmol) of Na2S2O4 in 42 mL of ion-exchanged water, and the sodium hydroxide aqueous solution C was prepared by dissolving 3 g (10 mmol) of BPA, 5.2 g (131 mmol) of NaOH, and 0.031 g (0.20 mmol) of Na2S2O4 in 77 mL of ion-exchanged water. The PC-POS copolymer (a6) was obtained by the same production as in Production Example 1. Details of the PC-POS copolymer are shown in Table 1-1.
[0084] Production Example 3 A PC-POS copolymer (a2) was obtained by carrying out the same production as in Production Example 1, except that the amount of allylphenol-terminated polydimethylsiloxane was 40.4 g, and a solution of 3.0 g (10 mmol) of bisphenol A, 5.2 g (131 mmol) of NaOH, and 0.006 g (0.038 mmol) of Na2S2O4 dissolved in 77 mL of ion-exchanged water was used as the sodium hydroxide aqueous solution C. Details of the PC-POS copolymer are shown in Table 1-1.
[0085] Production Example 4 As the allylphenol-terminated polydimethylsiloxane, 43.0 g of allylphenol-terminated polydimethylsiloxane with an average chain length n = 23 was used. As the sodium hydroxide aqueous solution A, a solution obtained by dissolving 3.7 g (94 mmol) of NaOH in 43 mL of ion-exchanged water was used. As the sodium hydroxide aqueous solution B, 5.5 g (19 mmol) of BisP-AP (manufactured by Honshu Chemical Industry Co., Ltd.) and 2.3 g (57 mmol) of NaOH were used. A PC-POS copolymer (a10) was obtained by carrying out the same production as in Production Example 1, except that a mixture of 33 mL of ion-exchanged water and 0.031 g (0.196 mmol) of Na2S2O4 was used, and that a solution of 2.5 g (8.7 mmol) of bisphenol A, 1.9 g (46.3 mmol) of NaOH, and 0.031 g (0.196 mmol) of Na2S2O4 dissolved in 27 mL of ion-exchanged water was used as the sodium hydroxide aqueous solution C of BPA. Details of the PC-POS copolymer are shown in Table 1-1.
[0086] Production Example 5 As the allylphenol-terminated polydimethylsiloxane, 46.0 g of allylphenol-terminated polydimethylsiloxane with an average chain length n = 63 was used. As the sodium hydroxide aqueous solution A, a solution obtained by dissolving 2.2 g (55.9 mmol) of NaOH in 26 mL of ion-exchanged water was used. As the sodium hydroxide aqueous solution B, 5.8 g (20 mmol) of BisP-AP (manufactured by Honshu Chemical Industry Co., Ltd.) and 2.4 g (60 mmol) of NaOH were used. A PC-POS copolymer (a14) was obtained by carrying out the same production as in Production Example 1, except that a mixture of 35 mL of ion-exchanged water and 0.031 g (0.196 mmol) of Na2S2O4 was used, and that a solution of 6.6 g (22.6 mmol) of bisphenol A, 3.2 g (80.9 mmol) of NaOH, and 0.031 g (0.196 mmol) of Na2S2O4 dissolved in 47 mL of ion-exchanged water was used as the sodium hydroxide aqueous solution C of BPA. Details of the PC-POS copolymer are shown in Table 1-1.
[0087] Production Example 6 The amount of allylphenol-terminated polydimethylsiloxane was 62.0 g, and the sodium hydroxide aqueous solution A was prepared by dissolving 3.1 g (77 mmol) of NaOH in 35 mL of ion-exchanged water, the sodium hydroxide aqueous solution B was prepared by dissolving 6.0 g (21 mmol) of BisP-AP, 2.5 g (62 mmol) of NaOH, and 0.031 g (0.20 mmol) of Na2S2O4 in 36 mL of ion-exchanged water, and the sodium hydroxide aqueous solution C was prepared by dissolving 4.0 g (14 mmol) of bisphenol A, 2.3 g (58 mmol) of NaOH, and 0.031 g (0.20 mmol) of Na2S2O4 in 34 mL of ion-exchanged water. The PC-POS copolymer (a3) was obtained by the same production as in Production Example 1. Details of the PC-POS copolymer are shown in Table 1-1.
[0088] Production Example 7 The amount of allylphenol-terminated polydimethylsiloxane was 77.0 g, and the sodium hydroxide aqueous solution A was prepared by dissolving 3.5 g (87 mmol) of NaOH in 40 mL of ion-exchanged water, the sodium hydroxide aqueous solution B was prepared by dissolving 6.0 g (21 mmol) of BisP-AP, 2.5 g (62 mmol) of NaOH, and 0.031 g (0.20 mmol) of Na2S2O4 in 36 mL of ion-exchanged water, and the sodium hydroxide aqueous solution C was prepared by dissolving 2.9 g (10 mmol) of bisphenol A, 1.9 g (48 mmol) of NaOH, and 0.031 g (0.20 mmol) of Na2S2O4 in 28 mL of ion-exchanged water. The PC-POS copolymer (a4) was obtained by the same production as in Production Example 1. Details of the PC-POS copolymer are shown in Table 1-1.
[0089] Production Example 8 PC-POS copolymer (a5) was obtained by carrying out the same production as in Production Example 1, except that the amount of allylphenol-terminated polydimethylsiloxane was 96.0 g, the sodium hydroxide aqueous solution A was prepared by dissolving 4.0 g (100 mmol) of NaOH in 46 mL of ion-exchanged water, the sodium hydroxide aqueous solution B was prepared by dissolving 7.7 g (27 mmol) of BisP-AP, 4.7 g (118 mmol) of NaOH, and 0.031 g (0.20 mmol) of Na2S2O4 in 69 mL of ion-exchanged water, and the sodium hydroxide aqueous solution C was not added. Details of the PC-POS copolymer are shown in Table 1-1.
[0090] Production Example 9 The amount of allylphenol-terminated polydimethylsiloxane was 4.0 g, the sodium hydroxide aqueous solution A was prepared by dissolving 1.5 g (38 mmol) of NaOH in 18 mL of ion-exchanged water, 1.8 g (12.0 mmol) of PTBP was used, the sodium hydroxide aqueous solution C was prepared by dissolving 13.2 g (45 mmol) of bisphenol A, 6.3 g (159 mmol) of NaOH, and 0.031 g (0.20 mmol) of Na2S2O4 in 93 mL of ion-exchanged water, and the sodium hydroxide aqueous solution B was not added. The PC-POS copolymer (a9) was obtained by the same production as in Production Example 1. Details of the PC-POS copolymer are shown in Table 1-2.
[0091] Manufacturing Example 10 The amount of allylphenol-terminated polydimethylsiloxane was 23.0 g, the sodium hydroxide aqueous solution A was prepared by dissolving 2.0 g (50.8 mmol) of NaOH in 23 mL of ion-exchanged water, 1.8 g (12.0 mmol) of PTBP was used, the sodium hydroxide aqueous solution C was prepared by dissolving 11.7 g (40.4 mmol) of bisphenol A, 5.8 g (146.0 mmol) of NaOH, and 0.031 g (0.20 mmol) of Na2S2O4 in 85 mL of ion-exchanged water, and the sodium hydroxide aqueous solution B was not added. The PC-POS copolymer (a12) was obtained by the same production as in Production Example 1. Details of the PC-POS copolymer are shown in Table 1-2.
[0092] Manufacturing Example 11 The allylphenol-terminated polydimethylsiloxane having an average chain length n=63 was used as 30.0 g, the sodium hydroxide aqueous solution A was prepared by dissolving 1.8 g (45 mmol) of NaOH in 21 mL of ion-exchanged water, 1.8 g (12.0 mmol) of PTBP was used, the sodium hydroxide aqueous solution C was prepared by dissolving 12.3 g (43 mmol) of bisphenol A, 6.1 g (151 mmol) of NaOH, and 0.031 g (0.20 mmol) of Na2S2O4 in 89 mL of ion-exchanged water, and the sodium hydroxide aqueous solution B was not added. The PC-POS copolymer (a8) was obtained by the same production as in Production Example 1. Details of the PC-POS copolymer are shown in Table 1-2.
[0093] Manufacturing Example 12 The amount of allylphenol-terminated polydimethylsiloxane was 55 g, the sodium hydroxide aqueous solution A was prepared by dissolving 2.9 g (72.1 mmol) of NaOH in 33 mL of ion-exchanged water, 1.8 g (12.0 mmol) of PTBP was used, the sodium hydroxide aqueous solution C was prepared by dissolving 9.3 g (32.0 mmol) of bisphenol A, 5.0 g (124.7 mmol) of NaOH, and 0.031 g (0.20 mmol) of Na2S2O4 in 73 mL of ion-exchanged water, and the sodium hydroxide aqueous solution B was not added. The PC-POS copolymer (a13) was obtained by the same production as in Production Example 1. Details of the PC-POS copolymer are shown in Table 1-2.
[0094] Manufacturing Example 13 The amount of allylphenol-terminated polydimethylsiloxane was 78.0 g, 3.5 g (87 mmol) of NaOH was dissolved in 40 mL of ion-exchanged water as the sodium hydroxide aqueous solution A, 1.8 g (12.0 mmol) of PTBP was used, 7.5 g (26 mmol) of bisphenol A, 4.4 g (109 mmol) of NaOH, and 0.031 g (0.20 mmol) of Na2S2O4 were dissolved in 70 mL of ion-exchanged water as the sodium hydroxide aqueous solution C, and the sodium hydroxide aqueous solution B was not added. The PC-POS copolymer (a7) was obtained by the same production as in Production Example 1. Details of the PC-POS copolymer are shown in Table 1-2.
[0095] [Table 1]
[0096] [Table 2]
[0097] Examples 1 to 12, Comparative Example 1 The PC-POS copolymer obtained in each manufacturing example was molded using a vacuum press (manufactured by Imoto Manufacturing, manual hydraulic vacuum heating press). 7.0 g of resin was placed in a mold with a length of 5 cm, a width of 5 cm, and a thickness of 2 mm, and the surface in contact with the resin was sandwiched between mirror-finished aluminum plates, and the molded product was placed in a vacuum press, and the pressure inside the vacuum press tank was reduced to -0.1 MPa or less relative to atmospheric pressure. The molded product was then heated to the molding temperature shown in Tables 2-1 and 2-2. After the molding temperature was reached, the press pressure was increased to 2 MPa and heated for 2 minutes. The press pressure was then increased over 3 minutes, and molding was performed while maintaining the pressure at 15 MPa for 5 minutes. After molding, the molded product was returned to atmospheric pressure, and then removed and cooled to room temperature. The molded product was then peeled off from the mirror-finished aluminum plate to obtain a measurement sample with a length of 5 cm, a width of 5 cm, and a thickness of 2 mm. The evaluation results of the PC-POS copolymer are shown in Tables 2-1 and 2-2.
[0098] [Table 3]
[0099] [Table 4] [Industrial Applicability]
[0100] According to the present invention, a molded article having both excellent flexibility and transparency can be obtained. The molded article of the present invention can be used as an optically transparent member, specifically, flexible displays, light guide plates, housings, water-repellent and oil-repellent films, optical adhesives, switch covers, heat sealants, waterproofing materials, sealants, connectors, adapters, smartphone covers, lenses, eyeglass and sunglasses parts, optical fiber parts, cushioning materials for automotive batteries, wiper blades, curved mirrors, side mirrors, rearview mirrors, lamp covers, bumpers, windows, exterior materials, interior materials, sound-absorbing materials, handle covers, sensor covers, watch parts, stationery, cosmetic containers, aquariums for raising aquatic organisms, shoe soles, cups, nail art, toys, artificial bait, suction cups, The material can be suitably used in at least one selected from cooking utensils such as steamers, clothing, silicone wiping sheets, remote control covers, umbrellas, metal container linings, building material covers, doors, windows, glass interlayers, tents, mirrors, show window cases, vinyl greenhouses, medical device housings, infusion bags, infusion tubes, syringes, baby bottles, masks, face bands, filter parts, vibration-damping parts, robot housings, drone housings, shields, bulletproof shields, sports cushions, airplane windows, resin compatibilizers, lighting covers, light guides, light guiding panels, lighting units, prism panels, flat lenses, Fresnel lenses, microlens arrays, and collimator lenses.
Claims
[Claim 1] A molded article comprising a polycarbonate block (A-1) having a repeating unit represented by the following general formula (I) and a polyorganosiloxane block (A-2) having a repeating unit represented by the following general formula (II), in which the content of the polyorganosiloxane block (A-2) is 20% by mass or more and 70% by mass or less, and having a durometer hardness of 25 or more and 72 or less by a type D durometer measured in accordance with JIS K 6253-3:2012. 【Chemistry 1】 [In the formula, R 1 and R 2 each independently represents a halogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. X represents a single bond, an alkylene group having 1 to 8 carbon atoms, an alkylidene group having 2 to 8 carbon atoms, a cycloalkylene group having 5 to 15 carbon atoms, an arylene group having 6 to 12 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, a fluorenediyl group, an arylalkylene group having 7 to 15 carbon atoms, an arylalkylidene group having 7 to 15 carbon atoms, -S-, -SO-, -SO 2 represents -, -O- or -CO-. 3 and R 4 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. a and b each independently represent an integer of 0 to 4.