Fiber mat

The described method enhances fiber sheet strength by fusing thermoplastic fine fibers using light irradiation, addressing the strength challenges of fine fibers without hydrogen bonds, suitable for applications like flexible copper clad laminates.

JP2024166409AActive Publication Date: 2024-11-28MURATA MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024163326
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-07-26
Filing Date
2024-09-20
Publication Date
2024-11-28
Estimated Expiration
2042-03-25

AI Technical Summary

Technical Problem

Existing methods for producing fiber sheets with fine fibers face challenges in achieving sufficient strength, especially with chemical fibers lacking hydrogen bonds, as they either require costly solvent recovery or result in deteriorated electrical properties when using binders, and calendering methods struggle with peeling fine fibers from the mesh.

Method used

A method involving dispersing thermoplastic fine fibers in a dispersion medium, forming a mat on a support, and fusing the fibers using light irradiation to enhance strength, particularly using liquid crystal polymer powder with a high melting point and aspect ratio, ensuring fusion only on the surface layers to maintain air permeability.

Benefits of technology

The method produces a fiber mat with high breaking strength, enabling applications like flexible copper clad laminates without compromising electrical properties or requiring high-melting-point materials for the support.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166409000001_ABST
    Figure 2024166409000001_ABST
Patent Text Reader

Abstract

To provide a fiber mat containing fine fibers and having a high strength.SOLUTION: There is provided a fiber mat that is composed of fine fibers having a thermoplastic property, and is configured in that: a first main surface is provided on one side in a thickness direction, and a second main surface is provided on the other side in the thickness direction; and the fine fibers are fused on the first main surface side and are provided so as to be releasable from a support body that supports the second main surface.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fiber mat. [Background technology]

[0002] As a conventional method for producing a fiber sheet (fiber mat), JP 2013-076196 A (Patent Document 1) discloses a method for producing a fiber sheet using a papermaking method. Specifically, the method discloses a method in which a fiber suspension in which fibers are dispersed is supplied onto a papermaking wire, and the fibers are deposited on the papermaking wire to form a fiber sheet on the papermaking wire. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-076196 A Summary of the Invention [Problem to be solved by the invention]

[0004] 2. Description of the Related Art In recent years, fiber sheets such as nonwoven fabrics have been used in a wide variety of applications, including as filters, adsorbents, heat insulating materials, and also as printed wiring board materials by incorporating epoxy resins therein.

[0005] The finer the fibers constituting the fiber sheet, the thinner the fiber sheet and the more the thickness variation can be suppressed. In addition, there is a demand for improved filter performance in fiber sheets, and it is expected that fiber sheets will be manufactured using fine fibers in order to increase the specific surface area and reduce the pore size to capture fine particles.

[0006] The mainstream techniques for making fibers into sheets (mats) are the coater method and the papermaking method, but as the fibers become thinner and their specific surface area increases, the amount of solvent required to wet the fibers increases. For this reason, solvent recovery methods such as the papermaking method are more cost-effective.

[0007] When fibers having hydrogen bonds, such as pulp, are made into paper using a papermaking method, the fibers in the formed fiber mat acquire strength through hydrogen bonds by dehydrating and drying the paper after it is made.

[0008] However, in the case of chemical fibers that do not have hydrogen bonds, the only way to bond them is through entanglement between the fibers, and it is difficult to obtain sufficient strength for handling, especially for short fibers such as fine fibers. Therefore, a method of adding a binder substance to the fiber mat to give it strength can be considered, but in this case, the electrical properties and heat resistance of the fiber mat are deteriorated, and the performance as a fiber mat is deteriorated.

[0009] As another widely used method, a technique is used in which the fibers are heated and pressed with a calendar to bond them together and provide strength. However, when heat-bonding with a calendar, it is necessary to peel off the fiber mat from the mesh or papermaking wire. When fine, particularly ultrashort fibers are used, the fiber mat does not have enough strength to withstand peeling.

[0010] If the calendering process is performed without peeling, the fiber mat will become integrated with the mesh or papermaking wire, making it impossible to peel it off. In addition, the mesh or papermaking wire must be made of a material with a higher melting point than the fibers used for papermaking, and when using fine fibers made of high-melting resin such as liquid crystal polymer (LCP), there are no inexpensive materials available that can meet this requirement.

[0011] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a fiber mat that contains fine fibers and has high strength. [Means for solving the problem]

[0012] A method for producing a fiber mat according to the present disclosure includes dispersing thermoplastic fine fibers in a dispersion medium and forming the dispersed fine fibers into a mat on a support. The mat forming step includes papermaking the fine fibers onto the support to form a fiber mat, and irradiating a first main surface of the fiber mat located on the opposite side to the support with light. In the step of irradiating the first main surface of the fiber mat with light, the fine fibers located on the first main surface side are fused.

[0013] In the method for producing a fiber mat based on the present disclosure, the fine fibers may have a melting point higher than that of the support.

[0014] In the method for producing a fiber mat based on the present disclosure, it is preferable that pulsed light is irradiated in the light irradiating step.

[0015] In the method for producing a fiber mat according to the present disclosure, the mat-forming step may further include a step of peeling the fiber mat, the first main surface of which has been irradiated with light, from the support, and irradiating a second main surface of the fiber mat, which is located on the opposite side to the first main surface, with light. In this case, it is preferable that the fine fibers located on the second main surface side are fused in the step of irradiating the second main surface of the fiber mat with light.

[0016] In the method for producing a fiber mat based on the present disclosure, liquid crystal polymer powder may be used as the fine fibers.

[0017] In the fiber mat manufacturing method based on the present disclosure, it is preferable to use as the liquid crystal polymer powder short fiber particles having an aspect ratio, which is the ratio of the longitudinal length to the fiber diameter, of 10 to 500 times and including a fiber portion having an average diameter of 2 μm or less.

[0018] The fiber mat according to the present disclosure is made of fine fibers having thermoplasticity and has a first main surface on one side in a thickness direction. In the fiber mat, the fine fibers are fused on the first main surface side.

[0019] In the fiber mat based on the present disclosure, it is preferable that the breaking strength is 45 cN / 20 mm or more.

[0020] In the fiber mat according to the present disclosure, the fine fibers may be liquid crystal polymer powder.

[0021] In the fiber mat based on the present disclosure, it is preferable that the liquid crystal polymer powder is a short fiber particle having an aspect ratio, which is the ratio of the longitudinal length to the fiber diameter, of 10 to 500 times and includes a fiber portion having an average diameter of 2 μm or less. Effect of the Invention

[0022] According to the present invention, it is possible to provide a fiber mat which contains fine fibers and has high strength. [Brief description of the drawings]

[0023] [Figure 1] 3 is a scanning electron microscope photograph showing an enlarged view of a first main surface of a fiber mat according to an embodiment. [Diagram 2] 2 is a scanning electron microscope photograph showing a cross section in a thickness direction of a fiber mat according to an embodiment. [Diagram 3] FIG. 2 is a flow diagram showing a manufacturing process of a fiber mat according to an embodiment. [Figure 4] FIG. 2 is a diagram showing a matting step for matting liquid crystal polymer powder in the process for producing a fiber mat. [Diagram 5] FIG. 13 is a diagram showing a step of irradiating a second surface of the fiber mat with light. [Figure 6] FIG. 2 is a diagram showing evaluation conditions and evaluation results in Example 1, Example 2, and a comparative example. [Figure 7]FIG. 13 is a diagram showing evaluation conditions and evaluation results in Examples 3 and 4. [Figure 8] FIG. 1 is a graph showing the breaking strength in Examples 1 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In the following preferred embodiments, the same or common parts are designated by the same reference characters in the drawings, and the description thereof will not be repeated.

[0025] <Fiber mat> The fiber mat 30 according to the present embodiment is made of fine fibers having thermoplastic properties, specifically, it is made of liquid crystal polymer powder in which liquid crystal polymer is finely pulverized and fiberized. The liquid crystal polymer used in the liquid crystal polymer powder is, for example, a thermotropic liquid crystal polymer. Furthermore, the molecules of the liquid crystal polymer have a negative thermal expansion coefficient in the axial direction of the molecular axis and a positive thermal expansion coefficient in the radial direction of the molecular axis. The liquid crystal polymer according to the present embodiment does not have an amide bond.

[0026] The fiber mat 30 according to this embodiment has a plate-like shape, and has a first main surface 31 (see FIG. 4) and a second main surface 32 (see FIG. 4) facing each other in the thickness direction.

[0027] Fig. 1 is a scanning electron microscope photograph showing an enlarged view of a first main surface of a fiber mat according to an embodiment. Fig. 2 is a scanning electron microscope photograph showing a cross section in the thickness direction of a fiber mat according to an embodiment. In Fig. 2, the area surrounded by a dashed line is a first surface layer portion R1 of the fiber mat 30 located on the first main surface side.

[0028] As shown in the region surrounded by the dashed lines in FIG. 1 and FIG. 2, in the fiber mat 30 according to the embodiment, the liquid crystal polymer powder is fused on the first main surface 31 side. That is, the liquid crystal polymer powder is fused in the first surface layer portion R1 of the fiber mat 30 located on the first main surface 31 side. On the other hand, the liquid crystal polymer powder is not fused in the intermediate layer portion R2 located closer to the center in the thickness direction than the first main surface 31 side. As a result, the fiber mat 30 has a density gradient from the first main surface 31 side to the center in the thickness direction. Specifically, the density on the first main surface 31 side in the thickness direction is greater than the density on the center side.

[0029] As described later, the liquid crystal polymer powder located on the second main surface 32 side may also be fused. That is, the liquid crystal polymer powder may also be fused in the second surface layer portion of the fiber mat 30 located on the second main surface 32 side.

[0030] As described above, the liquid crystal polymer powder is fused at least on the first main surface 31 side so as to have a density gradient in the thickness direction, thereby improving the strength of the fiber mat 30. When the liquid crystal polymer powder is fused on both the first main surface 31 side and the second main surface 32 side, the strength of the fiber mat 30 can be further improved.

[0031] The breaking strength of the fiber mat 30 is preferably 45 cN / 20 mm or more, and more preferably 50 cN / 20 mm or more. Furthermore, the breaking strength of the fiber mat 30 may be 115 cN / 20 mm or more, or 350 cN / 20 mm or more.

[0032] The breaking strength of the fiber mat 30 can be measured using an autograph (AG-XDplus manufactured by Shimadzu Corporation). In this case, the width of the fiber mat 30 at the time of measurement is set to 20 mm.

[0033] The overall basis weight of the fiber mat 30 is approximately 30 to 40 g / m 2The overall density of the fiber mat 30 is, for example, 0.30 to 0.60 g / cm 3 and the density increases as the fused area of ​​the liquid crystal powder polymer in the thickness direction increases.

[0034] The thickness of the fiber mat 30 is about 50 to 100 μm, and the thickness decreases as the fused region of the liquid crystal polymer powder in the thickness direction becomes larger.

[0035] <Film> The fiber mat 30 is pressed to be used as a film (more specifically, a liquid crystal polymer film). The liquid crystal polymer film may have a metal foil such as a copper foil bonded to at least one surface, or may have the metal foil bonded to both surfaces. In this case, the liquid crystal polymer film according to this embodiment can be used as a laminated molded product, for example, as FCCL (Flexible Copper Clad Laminates) on which a circuit can be formed by a subtractive method.

[0036] <Method of manufacturing fiber mat> 3 is a flow diagram showing a manufacturing process of a fiber mat. Referring to FIG. 3, the manufacturing method of the fiber mat according to the present embodiment will be described.

[0037] As shown in FIG. 3, the method for manufacturing a fiber mat in this embodiment includes, as a pre-process (S10), a coarse grinding process (S11), a fine grinding process (S12), a coarse particle removal process (S13), and a fiberization process (S14), in that order, and further includes, as a post-process (S20) following the pre-process (S10), a dispersion process (S21) and a mat-forming process (S22).

[0038] <Pre-process> In the coarse grinding step (S12), which is the first step of the pre-step (S10), a molded liquid crystal polymer is first prepared as a raw material. Examples of molded liquid crystal polymers include uniaxially oriented pellet-shaped, biaxially oriented film-shaped, or powder-shaped liquid crystal polymers. From the viewpoint of production cost, the molded liquid crystal polymer is preferably a pellet-shaped or powder-shaped liquid crystal polymer, which is less expensive than a film-shaped liquid crystal polymer, and more preferably a pellet-shaped liquid crystal polymer. In this embodiment, the molded liquid crystal polymer preferably does not include a liquid crystal polymer directly molded into a fiber shape by electrospinning or melt-blowing. However, the molded liquid crystal polymer may include a liquid crystal polymer processed into a fiber shape by crushing a pellet-shaped liquid crystal polymer or a powder-shaped liquid crystal polymer.

[0039] Next, the molded liquid crystal polymer is coarsely pulverized to obtain a coarsely pulverized liquid crystal polymer. For example, the molded liquid crystal polymer is coarsely pulverized with a cutter mill to obtain a coarsely pulverized liquid crystal polymer. The particle size of the coarsely pulverized liquid crystal polymer is not particularly limited as long as it can be used as a raw material for the fine pulverization process described later. The maximum particle size of the coarsely pulverized liquid crystal polymer is, for example, 3 mm or less.

[0040] The method for producing a liquid crystal polymer film in this embodiment does not necessarily have to include the coarse pulverization step (S11). For example, if the liquid crystal polymer molded product can be used as a raw material for the fine pulverization step, the liquid crystal polymer molded product may be directly used as a raw material for the fine pulverization step.

[0041] Next, in the fine pulverization step (S12), the coarsely pulverized liquid crystal polymer is dispersed in liquid nitrogen and pulverized to obtain granular finely pulverized liquid crystal polymer. In the fine pulverization step (S12), the coarsely pulverized liquid crystal polymer dispersed in liquid nitrogen is pulverized using media. The media is, for example, beads. In the fine pulverization step (S12), it is preferable to use a bead mill, which has relatively few technical problems, from the viewpoint of handling liquid nitrogen. An example of a device that can be used in the fine pulverization step (S12) is the liquid nitrogen bead mill "LNM-08" manufactured by IMEX.

[0042] In the fine grinding step (S12) of this embodiment, the grinding method of grinding the liquid crystal polymer in a state of being dispersed in liquid nitrogen is different from the conventional freeze grinding method. The conventional freeze grinding method is a method of grinding the raw material to be ground while pouring liquid nitrogen onto the raw material to be ground and the grinding device body, but most of the liquid nitrogen has evaporated at the time the raw material to be ground is ground. In other words, in the conventional freeze grinding method, most of the raw material to be ground is not dispersed in liquid nitrogen at the time the raw material to be ground is ground.

[0043] In the conventional freeze-pulverization method, the heat of the raw material to be pulverized itself, the heat generated by the pulverization device, and the heat generated by the pulverization of the raw material to be pulverized vaporize the liquid nitrogen in an extremely short time. Therefore, in the conventional freeze-pulverization method, the raw material being pulverized inside the pulverization device is at a temperature much higher than the boiling point of liquid nitrogen, which is -196°C. In other words, in the conventional freeze-pulverization method, pulverization is performed under conditions where the temperature inside the pulverization device is usually between -100°C and 0°C. In the conventional freeze-pulverization method, even if as much liquid nitrogen as possible is supplied, the temperature inside the pulverization device is at its lowest about -150°C.

[0044] Therefore, in the conventional freeze-pulverization method, for example, when uniaxially oriented pellet-shaped liquid crystal polymer or coarsely pulverized pellet-shaped liquid crystal polymer is pulverized, the pulverization proceeds along a plane approximately parallel to the axial direction of the molecular axis of the liquid crystal polymer, so that a fibrous liquid crystal polymer having a very large aspect ratio and a fiber diameter much larger than 3 μm is obtained. That is, even if uniaxially oriented pellet-shaped liquid crystal polymer or coarsely pulverized pellet-shaped liquid crystal polymer is pulverized in the conventional freeze-pulverization method, the granular finely pulverized liquid crystal polymer used in the present embodiment cannot be obtained.

[0045] In this embodiment, the raw material to be pulverized is pulverized in a state dispersed in liquid nitrogen, so that the raw material can be pulverized in a state that is even more cooled than in the conventional freeze-pulverization method. Specifically, the raw material to be pulverized can be pulverized at a temperature lower than −196° C., which is the boiling point of liquid nitrogen. When the raw material to be pulverized at a temperature lower than −196° C. is pulverized, the raw material to be pulverized progresses as brittle fracture of the raw material to be pulverized is repeated. As a result, even when a uniaxially oriented liquid crystal polymer is pulverized, for example, not only does the fracture progress on a plane approximately parallel to the axial direction of the molecular axis of the liquid crystal polymer, but also brittle fracture progresses along a plane intersecting the axial direction, so that a granular finely pulverized liquid crystal polymer can be obtained.

[0046] In the fine pulverization step (S12), the liquid crystal polymer, which has been broken into particles through brittle fracture in liquid nitrogen, is continuously subjected to impacts with media or the like while in an embrittled state, so that multiple fine cracks are formed from the outer surface to the inside of the liquid crystal polymer obtained in the fine pulverization step (S12).

[0047] The pulverized liquid crystal polymer particles obtained in the pulverization step (S12) preferably have a D50 of 100 μm or less, more preferably 50 μm or less, as measured by a particle size distribution measuring device using a laser diffraction scattering method, which can prevent the pulverized liquid crystal polymer particles from clogging the nozzle in the fiberization step described below.

[0048] Next, in the coarse particle removing step (S13), coarse particles are removed from the granular pulverized liquid crystal polymer obtained in the pulverizing step (S12). For example, by sieving the granular pulverized liquid crystal polymer with a mesh, granular pulverized liquid crystal polymer under the sieve is obtained, and the granular liquid crystal polymer on the sieve is removed, so that the coarse particles contained in the granular pulverized liquid crystal polymer can be removed. The type of mesh may be appropriately selected, and examples of the mesh include meshes with a mesh size of 100 μm. The mesh size can be appropriately changed according to the fiber length of the liquid crystal polymer powder to be obtained. For example, a mesh with a mesh size of about 5 μm to 50 μm may be used. In addition, the manufacturing method of the liquid crystal polymer powder according to this embodiment does not necessarily have to include the coarse particle removing step (S13).

[0049] Next, in the fiberization step (S14), the granular liquid crystal polymer is crushed by a wet high-pressure crushing device to obtain a liquid crystal polymer powder. In the fiberization step (S14), the finely pulverized liquid crystal polymer is first dispersed in a dispersion medium for the fiberization step. The finely pulverized liquid crystal polymer to be dispersed does not need to have coarse particles removed, but it is preferable that the coarse particles have been removed. Examples of the dispersion medium for the fiberization step include water, ethanol, methanol, isopropyl alcohol, toluene, benzene, xylene, phenol, acetone, methyl ethyl ketone, diethyl ether, dimethyl ether, hexane, or a mixture thereof.

[0050] Then, the finely pulverized liquid crystal polymer dispersed in the dispersion medium for the fiberization process, i.e., the finely pulverized liquid crystal polymer in a slurry state, is passed through the nozzle under high pressure. By passing through the nozzle at high pressure, the shear force or collision energy due to the high-speed flow in the nozzle acts on the liquid crystal polymer, and the granular finely pulverized liquid crystal polymer is crushed, so that the fiberization of the liquid crystal polymer progresses, and a liquid crystal polymer powder that can be used in a subsequent process can be obtained. From the viewpoint of applying a high shear force or high collision energy, it is preferable that the nozzle diameter of the nozzle is as small as possible within a range in which the finely pulverized liquid crystal polymer does not clog in the nozzle. Since the particle diameter of the granular finely pulverized liquid crystal polymer in this embodiment is relatively small, the nozzle diameter in the wet high-pressure crushing device used in the fiberization process can be made small. The nozzle diameter is, for example, 0.2 mm or less.

[0051] In this embodiment, as described above, a plurality of fine cracks are formed in the granular finely pulverized liquid crystal polymer powder. Therefore, the dispersion medium penetrates into the finely pulverized liquid crystal polymer through the fine cracks by pressurization in the wet high-pressure crushing device. Then, when the slurry-like finely pulverized liquid crystal polymer passes through the nozzle and is placed under normal pressure, the dispersion medium that penetrates into the finely pulverized liquid crystal polymer expands in a short time. The dispersion medium that penetrates into the finely pulverized liquid crystal polymer expands, and destruction proceeds from the inside of the finely pulverized liquid crystal polymer. Therefore, fiberization proceeds to the inside of the finely pulverized liquid crystal polymer, and the liquid crystal polymer molecules are separated into domain units in which they are aligned in one direction. Thus, in the fiberization process in this embodiment, by defibrating the granular finely pulverized liquid crystal polymer obtained in the finely pulverized process in this embodiment, a liquid crystal polymer powder having a lower content of aggregates and in the form of fine short fibers can be obtained, compared to the liquid crystal polymer powder obtained by crushing the granular liquid crystal polymer obtained by the conventional freeze-pulverization method.

[0052] In the fiberization step (S14) in this embodiment, the finely pulverized liquid crystal polymer may be crushed multiple times with a wet high-pressure crushing device to obtain a liquid crystal polymer powder. It is preferable that the number of times of crushing with the wet high-pressure crushing device is small. The number of times of crushing with the wet high-pressure crushing device may be, for example, 5 times or less.

[0053] The obtained liquid crystal polymer powder is used as a raw material in the subsequent steps. Here, the liquid crystal polymer powder as fine fibers will be described in detail.

[0054] The liquid crystal polymer powder contains at least a fiber portion. The fiber portion is a short fiber-like particle having an aspect ratio, which is the ratio of the longitudinal length to the fiber diameter, of 10 to 500 times and an average diameter of 2 μm or less. A liquid crystal polymer powder containing such a fine short fiber-like fiber portion having an aspect ratio of 10 to 500 times and an average diameter of 2 μm or less cannot be produced by a conventionally known production method.

[0055] For example, liquid crystal polymer powder containing a fiber portion with an aspect ratio of 10 to 500 cannot be produced only by the electrospinning method, which is a method for producing ultrafine continuous long fibers. It is possible to cut the continuous long fiber liquid crystal polymer ultrafine long fiber produced by the electrospinning method into short fibers after spinning. However, there is a limit to how short the continuous long fiber liquid crystal polymer ultrafine long fiber, which has an extremely small fiber diameter and an aspect ratio of approximately infinity, can be cut. After cutting the continuous long fiber liquid crystal polymer ultrafine long fiber produced by the electrospinning method, the liquid crystal polymer ultrafine long fiber has an aspect ratio of more than 500.

[0056] The average diameter of the fiber portion is the average value of the fiber diameters of a plurality of fibrous particles constituting the fiber portion. Thus, the liquid crystal polymer powder according to this embodiment contains fine fibrous particles. The fiber diameter can be measured from image data of the fibrous particles obtained when observing the fibrous particles with a scanning electron microscope.

[0057] The aspect ratio of the fibrous portion is preferably equal to or less than 300, and more preferably equal to or less than 100. The average diameter of the fibrous portion is preferably equal to or less than 1 μm.

[0058] The fiber portion may be included in the liquid crystal polymer powder as an aggregate portion in which fibrous particles are aggregated. In addition, the axial direction of the liquid crystal polymer molecules constituting the fiber portion and the longitudinal direction of the fiber portion are the same. In the manufacturing method of the fiber mat according to the present embodiment, since the liquid crystal polymer powder is manufactured through the above-mentioned fiberization process, the axial direction of the liquid crystal polymer molecules is strongly oriented along the longitudinal direction of the fiber portion due to the destruction between the multiple domains formed by the liquid crystal polymer molecules being bundled.

[0059] The liquid crystal polymer powder preferably contains substantially non-fibrous aggregates at a content of 20% or less. More preferably, the liquid crystal polymer powder does not contain aggregates. The content of aggregates is evaluated by the number of aggregates relative to the number of aggregates contained in the liquid crystal polymer powder. In this embodiment, when the liquid crystal polymer powder is placed on a flat surface, aggregates having a maximum height of more than 10 μm are aggregates, and aggregates having a maximum height of 10 μm or less are fibrous.

[0060] The lump portion may be included in the liquid crystal polymer powder as an aggregate portion containing lump particles. The lump portion is a liquid crystal polymer powder that is not substantially fibrous. The lump portion may have a flat outer shape.

[0061] In this embodiment, the liquid crystal polymer powder can have a D50 value of, for example, 13 μm or less, as measured by particle size measurement using a particle size distribution measuring device based on a laser diffraction scattering method.

[0062] The liquid crystal polymer powder used as a raw material in the subsequent process is not limited to that produced in the above-mentioned previous process.

[0063] <Post-process> Next, the post-process (S20) will be described. In the dispersion process (S21), which is the first process of the post-process (S20), the liquid crystal polymer powder is dispersed in a dispersion medium to form a slurry. Since the liquid crystal polymer powder in the form of fine short fibers is used, the liquid crystal polymer powder can be dispersed in a high-viscosity dispersion medium, and a homogeneous fiber mat can be produced.

[0064] The dispersion medium used in the dispersion step (S21) may be water, ethanol, a mixture of these, etc. By using such a dispersion medium, the cost of the dispersion medium can be reduced, and the fiber mat can be produced at low cost.

[0065] It is considered that the longitudinal direction of the fiber portion in the liquid crystal polymer powder dispersed in the dispersion medium is not oriented in a specific direction in the dispersion medium.

[0066] Next, in the mat-forming step (S22), the slurry liquid crystal polymer powder is formed into a liquid crystal polymer fiber mat by a papermaking method. In the papermaking method, the dispersion medium used in the dispersion step can be recovered and reused, and the fiber mat can be produced at low cost.

[0067] 4 is a diagram showing a matting step for matting the liquid crystal polymer powder in the fiber mat manufacturing process. The matting step will be described in detail with reference to FIG.

[0068] 4, the mat-forming step uses a papermaking machine 100. The papermaking machine 100 includes a supply roller 15 that supplies the microporous sheet 10, a take-up roller (not shown) that collects the microporous sheet 10, a papermaking wire 20, transport rollers 25 and 26, a storage section 40 that stores a dispersion medium 41 in which the liquid crystalline polymer powder is dispersed, a heating device 50, and a light irradiation device 60.

[0069] The papermaking wire 20 is, for example, a papermaking mesh of about 80 to 100 mesh. That is, the papermaking wire 20 has a pore size of about 150 μm to 180 μm. The papermaking wire 20 is transported by transport rollers 25 and 26 arranged in the transport direction. The transport roller 26 is disposed downstream of the transport roller 25. The papermaking wire 20 is transported by the transport rollers 25 and 26 so as to pass through the storage section 40.

[0070] The supply roller 15 supplies the microporous sheet 10 onto the papermaking wire 20. The microporous sheet 10 functions as a support for supporting the liquid crystalline polymer powder. The microporous sheet 10 placed on the papermaking wire 20 is transported by the papermaking wire 20 to pass through the storage section 40. The microporous sheet 10 that has passed through the storage section 40 is peeled off from the papermaking wire 20 and taken up by a take-up roller.

[0071] The microporous sheet 10 has a finer mesh than the papermaking wire 20. The microporous sheet 10 preferably has a mesh size of approximately 157 or more. In other words, the microporous sheet 10 preferably has a pore size of approximately 100 μm or less. This makes it possible to collect the fine liquid crystal polymer powder dispersed in the dispersion medium.

[0072] More preferably, the microporous sheet 10 has a pore size of about 5 μm to 50 μm. If the pore size of the microporous sheet 10 is too small, the drainage is poor and the time required for dehydration is long. On the other hand, if the pore size of the microporous sheet 10 is too large, it is difficult to collect the fine fibers (fine liquid crystal polymer powder), resulting in a poor yield.

[0073] When a microporous sheet 10 having a variation in pore size is selected, the texture of the formed fiber mat is affected, so when high uniformity is required for the fiber mat, a mesh that is periodically woven in a reticulated pattern is preferred. In other words, it is preferable to use a mesh for the microporous sheet 10 in which the pore size is uniform and the pores are not distributed unevenly.

[0074] For example, a woven mesh having a pore size of 50 μm or less can be used as the microporous sheet 10. As the woven mesh, for example, one made of synthetic fibers such as polyester can be used.

[0075] The microporous sheet 10 may have a basis weight of 15 g / m. 2 The following wet-laid nonwoven fabrics may be used. As the wet-laid nonwoven fabric, one made of microfibers may be used. The microfibers are made of synthetic fibers such as polyester.

[0076] The heating device 50 is disposed downstream of the storage section 40 in the conveying direction. The heating device 50 heats and dries the liquid crystal polymer powder 30 that has been woven onto the microporous sheet 10. As a result, a fiber mat is formed on the microporous sheet 10.

[0077] The light irradiation device 60 is disposed downstream of the heating device 50 in the conveying direction. The light irradiation device 60 irradiates light toward the fiber mat formed on the microporous sheet 10. The light irradiation device 60 may be, for example, a flash lamp.

[0078] The light irradiation device 60 preferably irradiates pulsed light. Since the pulsed light is absorbed by the surface (first main surface 31) of the fiber mat, the support (microporous sheet 10) supporting the fiber mat is not deteriorated by light irradiation. Therefore, a material having a lower melting point than the fiber mat can be used as the support, and the range of support options is expanded. In addition, since the fiber mat can be prevented from fusing to the support, the support can be reused repeatedly. As the light irradiation device 60, PulseForge (registered trademark) 1300 manufactured by NovaCentrix can be adopted.

[0079] The mat-forming step (S21) includes a paper-making step, a peeling step, a drying step, and a light irradiation step. In the mat-forming step (S21), first, in the paper-making step, the dispersed liquid crystal polymer powder is papered into the microporous sheet 10. Specifically, the microporous sheet 10 supplied onto the papermaking wire 20 is conveyed by the papermaking wire 20 and passes through the storage section 40. At this time, the liquid crystal polymer powder dispersed in the dispersion medium 41 stored in the storage section 40 is papered into the microporous sheet 10.

[0080] Next, in a peeling step, the microporous sheet formed by weaving up the dispersed liquid crystal polymer powder is peeled off from the papermaking wire 20. Specifically, the microporous sheet 10 is wound up by a winding roller, thereby transporting the microporous sheet 10 in a direction different from that of the papermaking wire 20. The papermaking wire 20 may be transported in a direction different from that of the microporous sheet 10 by a transport roller 26.

[0081] Next, in a drying step, the liquid crystal polymer powder laid on the microporous sheet 10 is heated and dried by a heater 50. As a result, a fiber mat 30 made of the liquid crystal polymer is formed on the microporous sheet 10.

[0082] Next, in the light irradiation step, the first main surface 31 of the fiber mat 30 located on the opposite side to the side on which the microporous sheet 10 is located is irradiated with light. This causes the liquid crystal polymer powder located on the first main surface 31 side to fuse together. As a result, the strength of the fiber mat 30 is improved, and the fiber mat 30 can be carried to the next step without being damaged.

[0083] Furthermore, since only the liquid crystal polymer powder located in the surface layer on the first main surface 31 side is fused, the density of the entire fiber mat 30 is low, which makes it possible to ensure high breathability and high collection efficiency.

[0084] The fiber mat 30 after light irradiation is placed on the microporous sheet 10 and then wound up by the winding roller in the winding process.

[0085] Fig. 5 is a diagram showing a step of irradiating the second surface of the fiber mat with light. As shown in Fig. 5, the mat-forming step may further include a step of peeling the fiber mat 30, the first main surface 31 of which has been irradiated with light, from the microporous sheet 10, and irradiating the second main surface 32 of the fiber mat 30 located on the opposite side to the side where the first main surface 31 is located with light. In this step, the fine fibers located on the second main surface 32 side are fused by light irradiation from a light irradiation device 61. The light irradiation device 61 may be the same as the light irradiation device 60 described above. When irradiating with light, the fiber mat 30 is irradiated while being transported.

[0086] When the liquid crystal polymer powder is fused on both the first main surface 31 side and the second main surface 32 side, the strength of the fiber mat 30 can be further improved.

[0087] Furthermore, when the fiber mat 30 is peeled off from the microporous sheet 10, since the liquid crystal polymer powder is fused on the first main surface 31 side and the fiber mat 30 has sufficient strength, the fiber mat 30 can be peeled off without being damaged.

[0088] <Film manufacturing method> Next, the fiber mat 30 is peeled off from the microporous sheet 10, and the fiber mat 30 is hot-pressed to obtain a liquid crystal polymer film. The thickness of the liquid crystal polymer film becomes thinner than that of the fiber mat 30 by the hot-pressing process.

[0089] In the hot pressing step, the fiber mat 30 is hot pressed together with, for example, copper foil. This allows the hot pressing step to also serve as a step of bonding the liquid crystal polymer film and the copper foil together, so that the liquid crystal polymer film with the copper foil bonded thereto can be obtained at low cost. Note that, when heating is performed for a long time in the hot pressing step, it is preferable to hot press the fiber mat 30 in a vacuum.

[0090] In the hot pressing step, the hot pressing is preferably performed at a temperature about 5°C to 15°C lower than the melting point of the liquid crystal polymer constituting the liquid crystal polymer powder. If the hot pressing is performed at a temperature about 5°C to 15°C lower than the endothermic peak temperature, the sintering of the liquid crystal polymers is facilitated.

[0091] In the hot pressing step, a polyimide film, a PTFE film, or a composite sheet made of a reinforcing material such as a glass fiber fabric and a heat-resistant resin may be sandwiched between the press machine used in the hot pressing step and the fiber mat 30 as a release film. In place of the polyimide film, an additional copper foil may be sandwiched between the press machine and the fiber mat 30. This makes it possible to obtain a liquid crystal polymer film having copper foil bonded to both sides. The liquid crystal polymer film having copper foil bonded to both sides can be used as a double-sided copper-clad FCCL.

[0092] If necessary, the metal foil bonded to the liquid crystal polymer film may be removed by etching, etc. This provides a liquid crystal polymer film free of any metal foil bonded thereto.

[0093] <Experimental Example> The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. In the experimental examples, fiber mats 30 according to Examples 1 to 4 were prepared, and the basis weight, thickness, density, and breaking strength were measured for Examples 1 and 2, and the breaking strength was measured for Examples 3 and 4. The breaking strength was measured using an autograph (AG-XDplus, manufactured by Shimadzu Corporation) after preparing a fiber mat 30 having a width of 20 mm.

[0094] Fig. 6 is a diagram showing the evaluation conditions and evaluation results in Examples 1 and 2, and Comparative Example. Fig. 7 is a diagram showing the evaluation conditions and evaluation results in Examples 3 and 4. Fig. 8 is a diagram showing the breaking strength in Examples 1 to 4.

[0095] Example 1 In Example 1, first, pellet-shaped liquid crystal polymer was charged into a cutter mill device as a raw liquid crystal polymer molding and coarsely pulverized. In Example 1, a liquid crystal polymer having a melting point of 315°C and an absorptivity of 60% at a wavelength of 500 nm was used. The coarsely pulverized film-shaped liquid crystal polymer was discharged from a discharge hole with a diameter of 3 mm provided in the cutter mill device to obtain a coarsely pulverized liquid crystal polymer.

[0096] Next, the coarsely pulverized liquid crystal polymer was finely pulverized in a liquid nitrogen bead mill (LNM-08, manufactured by Imex Co., Ltd.). In the pulverization in the liquid nitrogen bead mill, the vessel volume was set to 0.8 L, zirconia beads with a diameter of 5 mm were used as media, the amount of media input was set to 500 mL, 30 g of the coarsely pulverized liquid crystal polymer was input, and the pulverization process was performed for 120 minutes at a rotation speed of 2000 rpm. In the liquid nitrogen bead mill, the coarsely pulverized liquid crystal polymer was dispersed in liquid nitrogen and subjected to a wet pulverization process. In this way, the coarsely pulverized liquid crystal polymer was pulverized in the liquid nitrogen bead mill to obtain a granular finely pulverized liquid crystal polymer.

[0097] Next, the finely pulverized liquid crystal polymer was wet classified using a mesh with an opening of 100 μm to remove the coarse particles contained in the finely pulverized liquid crystal polymer, and the finely pulverized liquid crystal polymer that passed through the mesh was collected. In Example 1, a mesh with an opening of 100 μm was used, but a mesh with an opening smaller than the mesh may also be used for classification.

[0098] Next, the finely pulverized liquid crystal polymer from which the coarse particles had been removed was dispersed in a 20 wt% ethanol aqueous solution. The ethanol slurry in which the finely pulverized liquid crystal polymer was dispersed was repeatedly crushed five times using a wet high-pressure crushing device under conditions of a nozzle diameter of 0.2 mm and a pressure of 200 MPa to form fibers. The wet high-pressure crushing device used was Starburst HJP-25060 manufactured by Sugino Machine. As a result, a liquid crystal polymer powder dispersed in an ethanol aqueous solution was obtained.

[0099] Next, the necessary amounts of water and ethanol were added to prepare 2.2 g of liquid crystal polymer powder per 30 L of 50 wt% ethanol aqueous solution, and the slurry liquid crystal polymer powder was formed into a fiber mat 30 by a papermaking method. A square sheet machine 2555 manufactured by Kumagai Riki Co., Ltd. was used as the papermaking machine, and the liquid crystal polymer powder dispersed in the dispersion medium was papered on a microporous sheet of polyester mesh with a pore size of 11 μm.

[0100] Subsequently, the fiber mat 30 was formed into a microporous sheet by heating and drying at a temperature of 100°C using a hot air dryer. The fiber mat 30 had a basis weight of 35 g / m 2 That was about it.

[0101] Next, a plurality of fiber mats 30 were prepared, and the first main surface 31 of each fiber mat 30 was irradiated with light by changing the voltage conditions of a light irradiation device (PulseForge (registered trademark) 1300 manufactured by NovaCentrix). The voltages were 230 V, 250 V, and 270 V, and the pulse length was 3.5 ms.

[0102] The fiber mat 30 irradiated with light under these conditions was peeled off from the microporous sheet, and the basis weight, thickness, density, and breaking strength of the fiber mat 30 of Example 1 were measured using a thickness measuring device (digital linear gauge DG-525H (manufactured by Ono Seiki Co., Ltd.)), a density measuring device, or by conducting a tensile test, etc.

[0103] In Example 1, the basis weight, thickness, density, and breaking strength of the mat irradiated with light at 230 V were 33.9 g / m 2 , 95.3μm, 0.36g / cm 3 , 50cN / 20mm.

[0104] In Example 1, the basis weight, thickness, density, and breaking strength of the mat irradiated with light at 250 V were 34.2 g / m 2 , 84.1μm, 0.41g / cm 3 , 130cN / 20mm.

[0105] In Example 1, the basis weight, thickness, density, and breaking strength of the mat irradiated with light at 270 V were 34 g / m 2 , 79.2μm, 0.43g / cm 3 , 350cN / 20mm.

[0106] Example 2 In Example 2, a fiber mat 30 was prepared in a manner similar to that of Example 1, and the second main surface 32 located on the opposite side to the first main surface 31 was also irradiated with light with the same energy as that of Example 1. That is, in Example 2, the fiber mat 30 with the first main surface 31 irradiated with light was peeled off from the microporous sheet, and then the second main surface 32 was irradiated with light. The voltage of the light irradiating device (NovaCentrix PulseForge (registered trademark) 1300) when irradiating the second main surface 32 with light was 230V, 250V, and 270V, and the pulse length was 3.5 ms, as in Example 1. The basis weight, thickness, density, and breaking strength of the fiber mat 30 according to Example 2 were also measured in the same manner as in Example 1.

[0107] In Example 2, the basis weight, thickness, density, and breaking strength of the mat in which both the first main surface 31 and the second main surface 32 were irradiated with light at 230 V were 33.9 g / m 2 , 92.8μm, 0.37g / cm 3 , 120cN / 20mm.

[0108] In Example 2, the basis weight, thickness, density, and breaking strength of the mat in which both the first main surface 31 and the second main surface 32 were irradiated with light at 250 V were 34.2 g / m 2 , 78.5μm, 0.44g / cm 3 , 380cN / 20mm.

[0109] In Example 2, the basis weight, thickness, density, and breaking strength of the mat in which both the first main surface 31 and the second main surface 32 were irradiated with light at 270 V were 34 g / m 2 , 65μm, 0.52g / cm 3 , 720cN / 20mm.

[0110] (Comparative Example) The Comparative Example is different from Example 1 in that the light irradiation step is omitted in the matting step. That is, the fiber mat of the Comparative Example is not irradiated with light on the surface (first main surface) as compared with the fiber mat 30 of Example 1, and the fibers on the surface are not melted.

[0111] In this case, the basis weight, thickness, density and breaking strength of the mat are 34.2 g / m 2 , 105.2μm, 0.33g / cm 3 , 19.8cN / 20mm.

[0112] Example 3 In Example 3, the liquid crystal polymer used had a melting point of 315° C. and an absorptivity of 70% at a wavelength of 500 nm. Other than the above, the fiber mat 30 was obtained in the same manner as in Example 1.

[0113] In Example 3, the breaking strengths of the mats irradiated with light at 230 V, 250 V, and 270 V were 400 cN / 20 mm, 830 cN / 20 mm, and 1720 cN / 20 mm, respectively.

[0114] Example 4 In Example 4, the liquid crystal polymer used had a melting point of 315° C. and an absorptivity of 70% at a wavelength of 500 nm. Other than the above, the fiber mat 30 was obtained in the same manner as in Example 2.

[0115] In Example 4, the breaking strengths of the mats irradiated with light at 230 V, 250 V, and 270 V were 930 cN / 20 mm, 1690 cN / 20 mm, and 2410 cN / 20 mm, respectively.

[0116] As described above, it was confirmed that each fiber mat 30 had sufficient strength (breaking strength) in comparison with the comparative example in all of Examples 1 to 4. It was also confirmed that by increasing the voltage during light irradiation, the amount of fused liquid crystal polymer powder increased, and the thickness decreased, but the density and breaking strength increased.

[0117] Furthermore, it was confirmed that the breaking strength was further increased by irradiating the second main surface 32 with light in addition to the first main surface 31 as in Examples 2 and 4. In addition, by comparing Examples 1 and 2 with Examples 3 and 4, it was confirmed that the breaking strength was further increased by using a liquid crystal polymer powder with high absorptivity.

[0118] <Other Modifications> In the above-mentioned embodiment and examples, the fine fibers are liquid crystal polymer powder, but the fine fibers are not limited to liquid crystal polymer powder. As the fine fibers, chemical fibers that do not have hydrogen bonds may be used as long as they have thermoplasticity, as described above.

[0119] In the above-mentioned embodiment and examples, the support on which the fine fibers are woven is a microporous sheet, but the present invention is not limited to this. The microporous sheet may be omitted and the papermaking wire 20 may be used as the support. In this case, the fine fibers may have a fiber length greater than the pore size of the papermaking wire 20, and may have a fiber length of 200 μm or less. Furthermore, the fine fibers may have a fiber length of 1 mm or less.

[0120] The above-mentioned embodiments and examples of the present invention are illustrative in all respects and are not restrictive. The scope of the present invention is defined by the claims, and includes all modifications within the meaning and scope of the claims. [Explanation of symbols]

[0121] 10 microporous sheet, 15 supply roller, 20 papermaking wire, 25, 26 transport rollers, 30 fiber mat, 31 first main surface, 32 second main surface, 40 storage section, 41 dispersion medium, 50 heating device, 60 light irradiation device, 100 papermaking machine.

Claims

1. It is made up of fine thermoplastic fibers. A first main surface is provided on one side in a thickness direction, and a second main surface is provided on the other side in the thickness direction. The fine fibers are fused on the first main surface side, A fiber mat provided so as to be releasable from a support supporting the second main surface.

2. In the thickness direction, a density gradient is provided from the first main surface side to the central portion side of the fiber mat, The density of the first main surface side is higher than the density of the central portion side, The overall density of the fiber mat is between 0.30 and 0.52 g / cm 3 2. The fiber mat of claim 1, wherein

3. 3. The fiber mat according to claim 1, having a breaking strength of 45 cN / 20 mm or more.

4. The fiber mat according to claim 1 , wherein the fine fibers are liquid crystal polymer powder.

5. The fiber mat according to claim 4, wherein the liquid crystal polymer powder is a short fiber-like particle having an aspect ratio, which is the ratio of the longitudinal length to the fiber diameter, of 10 to 500 times, and includes a fiber portion having an average diameter of 2 μm or less.

Citation Information

Patent Citations

  • High performance paper comprising fibril of thermotropic liquid crystal polymer

    JP1985239600A

  • Bulky nonwoven fabric and its production

    JP1992136295A

  • Nonwoven fabric for printing base material

    JP2003096687A

  • Fiber sheet

    JP2013159882A

  • Liquid crystal polymer powder and method for producing same

    WO2021060255A1