Melting bag for hot melt adhesive, hot melt sheet using the same, and hot melt laminate
The melt bag and hot melt laminate, using styrenic elastomer and hydrogenated petroleum resin, address compatibility and workability issues in hot melt adhesive packaging, enhancing crush resistance and deformation ease while reducing environmental impact.
Patent Information
- Application Number
- JP2024163473
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-03
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2043-11-22
AI Technical Summary
Conventional hot melt adhesive packaging bags face issues with compatibility and workability, leading to blocking, crushing, and inefficient filling due to mismatched properties between the bag and the adhesive, resulting in environmental and operational inefficiencies.
A melt bag composed of a styrenic elastomer and a tackifier, specifically a fully or partially hydrogenated petroleum resin, with a softening point of 50°C or higher and a film thickness of 25 to 500 μm, providing crush resistance and ease of deformation, and a hot melt sheet and laminate designed for improved compatibility.
The solution enhances packaging workability with crush resistance and ease of deformation, ensuring compatibility with hot melt adhesives, reducing environmental impact and improving operational efficiency.
Smart Images

Figure 2024166411000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to melt bags, hot melt sheets, and hot melt laminates used to package hot melt adhesives. [Background technology]
[0002] Hot melt adhesives are melted and bonded to objects, and then cooled down, and the adhesive function is immediately apparent, so the advantage of not needing a curing period has been rediscovered, and their use in packaging and industrial applications is expanding. In response to recent social changes that emphasize reducing the burden on the environment, the advantage of not needing a solvent or drying process during use has also been rediscovered, and their use is continuing to expand.
[0003] As the range of application of hot melt expands, there is a demand for improved workability. In the summer, hot melt blocks stick together (blocking), and when removing them from the packed cardboard boxes, etc., they become huge blocks, which significantly reduces workability. Therefore, hot melts that are sticky at room temperature in particular are packed, transported, and stored in a state wrapped in release paper or release film, which is peeled off and discarded when the hot melt is used, but the disposal of these release materials has also come to be seen as an environmental burden.
[0004] Therefore, a specification called a melting bag was developed in which hot melt is packaged in a hard material and the hot melt is melted while still packaged when it is used (Patent Document 1). This avoids the environmental burden of disposing of the release material, and also eliminates the work of peeling off the release material every time a lump of hot melt is melted, dramatically improving work efficiency.
[0005] In recent years, measures have been taken to prevent blocking by increasing the strength of the melting bag (Patent Document 2) or embossing the shape (Patent Document 3). However, these methods have a large deviation from the properties of the hot melt content, and the compatibility between the melting bag and the hot melt in the melting furnace is insufficient, resulting in a problem that the mixed melt supplied to the coating head does not have the designed ratio. In addition, because the strength of the melting bag is too high, when a mass of hot melt adhesive wrapped in the melting bag is packed in a cardboard box or the like, the mass cannot change shape, resulting in a low-density package that does not meet the desired filling amount. However, if the strength of the melting bag is made extremely weak in order to impart ease of deformation, the mass will break during packaging, causing the hot melt adhesive to come out to the surface, resulting in a problem of blocking between the masses. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2004-002581 A [Patent Document 2] International Publication No. 2014 / 194087 [Patent Document 3] JP 2019-065164 A Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, an object of the present invention is to provide a melting bag for hot melt adhesives which has superior workability during packaging, such as shatter resistance and ease of deformation, and which also has excellent compatibility with the contents during use, as well as a hot melt sheet and a hot melt laminate using the same. [Means for solving the problem]
[0008] The present inventors have conducted intensive research to solve the above problems and have completed the present invention. . That is, an embodiment of the present invention is a melt bag containing a styrene-based elastomer (A) and a tackifier (C), wherein the tackifier (C) contains at least one of a fully hydrogenated petroleum resin and a partially hydrogenated petroleum resin.
[0009] Another embodiment of the present invention is the melt bag described above, which has a softening point of 50° C. or higher.
[0010] Another embodiment of the present invention is the melt bag, wherein the thickness is 25 to 500 μm.
[0011] Another embodiment of the present invention is the melt bag described above, wherein the styrene-based elastomer (A) has a weight average molecular weight of 300,000 or less.
[0012] Another embodiment of the present invention is the melt bag, which is for packaging hot melt adhesive.
[0013] Another embodiment of the present invention is a mass in which a hot melt adhesive is packaged in a melt bag, the melt bag being the mass described above.
[0014] Another embodiment of the present invention is the above lump, wherein the difference between the softening point of the hot melt adhesive and the softening point of the melting bag is within 50°C.
[0015] Another embodiment of the present invention is a hot melt sheet which is a sheet-shaped product of the above-mentioned lump.
[0016] Another embodiment of the present invention is the hot melt sheet having a thickness of 25 μm, which is fixed to an inclined plate with an inclination angle of 30 degrees, and a steel ball (1 / 32 to 32 / 32 inch) is rolled onto the sample with a run-up of 10 cm and a glue surface of 10 cm, and the diameter number (ball tack) of the ball that stops near the center of the glue surface is 4 or more.
[0017] Another embodiment of the present invention is a hot melt laminate comprising the hot melt sheet and an adherend disposed in this order. Effect of the Invention
[0018] According to the present invention described above, it is possible to provide a melting bag for hot melt adhesives which has superior workability during packaging, such as crush resistance and ease of deformation, and which also has excellent compatibility with the contents during use, as well as a hot melt sheet and a hot melt laminate using the same. [Brief description of the drawings]
[0019] [Figure 1] FIG. 2 is a schematic cross-sectional view partially showing the lump of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The melt bag, hot melt sheet, and hot melt laminate used to package the hot melt adhesive of the present invention will be described in more detail below, but are not limited thereto. The melting bag containing the hot melt adhesive is called a lump. Note that the term "hot melt adhesive" includes hot melt pressure sensitive adhesives. In this specification, a numerical range specified by using "~" includes the numerical values before and after "~" as the lower and upper limit values. In this specification, hot melt adhesives may be abbreviated as "hot melt". Unless otherwise noted, the various components appearing in this specification may be used independently as a single type or as a combination of two or more types. Moreover, unless otherwise specified, "parts" and "%" represent "parts by mass" and "% by mass", respectively.
[0021] <Melting bag> The melt bag of the present invention is used for packaging hot melt adhesives, but is not limited thereto as long as it can contribute technically to articles other than hot melt adhesives. The melting bag contains a styrene-based elastomer (A) and a tackifier (C). A material (resin composition) containing the styrene-based elastomer (A) and the tackifier (C) is heated and melted, and a film can be formed (manufactured) by a known method.
[0022] The softening point of the melting bag is preferably 50° C. or higher as a lower limit, more preferably 60° C. or higher, even more preferably 70° C. or higher, and particularly preferably 80° C. or higher as a lower limit. The softening point is preferably 150° C. or lower, more preferably 130° C. or lower, even more preferably 110° C. or lower, and particularly preferably 100° C. or lower as an upper limit. By having the softening point within the above range, crush resistance and blocking resistance are easily exhibited. The softening point is measured in accordance with JIS K-2207 (petroleum asphalt) 6.4 Softening point test method (ring and ball method).
[0023] The thickness of the melting bag is preferably 25 to 500 μm, more preferably 50 to 500 μm, further preferably 50 to 300 μm, and particularly preferably 50 to 200 μm. By keeping the thickness within the above range, it is easy to achieve both crush resistance and ease of deformation.
[0024] The amount of volatile organic compounds (VOCs) contained in the melting bag is preferably 3% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, and preferably substantially free. By keeping the amount of VOCs within the above range, the melting bag is easily adapted to applications where hygiene is important, such as the food and medical industries.
[0025] ≪Resin composition≫ In the present invention, the resin composition refers to a material for forming a melt bag, and contains a styrene-based elastomer (A) and a tackifier (C). It is preferable that the resin composition further contains a process oil (B). The inclusion of the process oil (B) is preferable because it provides excellent compatibility and ease of deformation.
[0026] <Styrene-based elastomer (A)> Styrene-based elastomer (A) is a type of thermoplastic elastomer. Thermoplastic elastomers are elastic materials that have the same properties as vulcanized rubber at room temperature, and at high temperatures, they are polymeric materials that can be molded using existing molding machines, just like ordinary thermoplastic resins. Thermoplastic elastomers have both elastic rubber components (soft segments: soft phase) in the molecules and molecular restraint components (hard segments: hard phase) to prevent plastic deformation, so they have properties between rubber and plastic. Styrene elastomers generally have a polystyrene block and a rubber middle block, with the polystyrene portion forming a physical crosslink (domain) and becoming the crosslinking point, and the middle rubber block giving the product rubber elasticity. The middle soft segment includes polybutadiene (B), polyisoprene (I) and polyolefin elastomers (ethylene-propylene (EP), ethylene-butylene (EB), butylene-butadiene (BB)), and the hard Depending on the arrangement of the segments with polystyrene (S), they are divided into linear type and branched type (radial type).
[0027] Styrene-based elastomers include styrene-butadiene-styrene block copolymer (hereinafter sometimes abbreviated as SBS), styrene-ethylene-butylene-styrene block copolymer, etc. Examples of such block copolymers include styrene-ethylene-propylene-styrene block copolymers (hereinafter abbreviated as SEBS), styrene-ethylene-propylene-styrene block copolymers (hereinafter abbreviated as SEPS), styrene-isoprene-styrene block copolymers (hereinafter abbreviated as SIS), and styrene-butylene-butadiene-styrene block copolymers (hereinafter abbreviated as SBBS).
[0028] The styrene content of the styrene elastomer (A) is preferably 10 to 50% by mass, more preferably 15 to 45% by mass, and even more preferably 20 to 40% by mass. When the styrene content is within this range, it becomes easier to balance the strength that exhibits crush resistance and the flexibility that exhibits ease of deformation. The styrene content is the content (mass%) of styrene in 100% by mass of the styrene elastomer.
[0029] The weight average molecular weight (Mw) of the styrene-based elastomer (A) is preferably 10,000 to 300,000, more preferably 50,000 to 200,000, further preferably 80,000 to 150,000, and particularly preferably 100,000 to 150,000. By setting the molecular weight within the above range, it is easy to achieve both crush resistance and ease of deformation. The weight average molecular weight is a value calculated as polystyrene by measuring by gel permeation chromatography (GPC).
[0030] The content of the styrene-based elastomer (A) is preferably 5 to 70 mass%, more preferably 10 to 60 mass%, and even more preferably 10 to 50 mass%, based on 100 mass% of the resin composition. By containing the styrene-based elastomer (A) in the above range, it is easy to achieve both crush resistance and ease of deformation.
[0031] <Process oil (B)> Process oil (B) is generally used as a plasticizer for rubber, thermoplastic elastomers, etc. It is a process oil produced in so-called oil refineries, etc., and is roughly classified into paraffinic process oil, aromatic process oil, and naphthenic process oil. Process oil is a mixture of paraffin chains, aromatic rings, and naphthenic rings, and is classified as paraffinic process oil when the paraffin chain carbon of the total carbon is 50% or more by weight, aromatic process oil when the aromatic carbon of the total carbon is 30% or more by weight, and naphthenic process oil when the naphthenic ring carbon of the total carbon is 30% or more by mass.
[0032] The content of the process oil (B) is preferably 5 to 90 mass%, more preferably 10 to 80 mass%, further preferably 15 to 70 mass%, particularly preferably 20 to 60 mass%, based on 100 mass% of the resin composition. By containing the process oil (B) in the above range, the ease of deformation is excellent.
[0033] <Tackifier (C)> The tackifier (C) contains at least one of fully hydrogenated petroleum resin and partially hydrogenated petroleum resin. By containing at least one of fully hydrogenated petroleum resin and partially hydrogenated petroleum resin, the tackifier has excellent crush resistance. Since fully hydrogenated petroleum resin and partially hydrogenated petroleum resin do not have aromatic rings that increase affinity between molecules, they are thought to be less prone to blocking.
[0034] The tackifier (C) is a relatively low molecular weight polymer with a molecular weight of several hundred to several thousand. It exhibits liquid or solid properties at room temperature, and adding the tackifier imparts fluidity and tackiness and improves adhesive strength. In the present invention, there are no particular limitations as long as it is a solid at room temperature. When it is a solid at room temperature, it has excellent resistance to shattering, but when used as a hot melt, it plays an important role in boosting adhesive strength, which is its original function. Examples of fully hydrogenated petroleum resins include the Arcon P series manufactured by Arakawa Chemical Industries, Ltd., and examples of partially hydrogenated petroleum resins include the Arcon M series manufactured by Arakawa Chemical Industries, Ltd.
[0035] As long as the tackifier (C) contains at least one of a fully hydrogenated petroleum resin and a partially hydrogenated petroleum resin, other tackifier resins can also be used in combination. Other tackifier resins are broadly classified into natural resin-based and synthetic resin-based. Natural resin-based resins include rosin-based resins and terpene-based resins, while synthetic resin-based resins include unhydrogenated petroleum-based resins, phenol-based resins, and xylene-based resins. It is preferable to use synthetic resin-based resins from the viewpoint of crush resistance.
[0036] The content of the tackifier (C) is preferably from 0 to 50 mass%, more preferably from 0 to 45 mass%, and even more preferably from 5 to 40 mass%, based on 100 mass% of the resin composition. By containing the tackifier (C) in the above range, it is easy to achieve both crush resistance and ease of deformation while adjusting the amount of the process oil (B).
[0037] To the extent that the problem of the present invention can be solved, waxes such as polyethylene wax, polypropylene wax, Fischer-Tropsch wax, paraffin wax, and microcrystalline wax, α-methylstyrene resin, and other thermoplastic elastomers can be used as components contained in the resin composition that forms the melt bag. Other examples of thermoplastic elastomers include olefin-based, urethane-based, polyester-based, polyamide-based, and 1,2-butadiene-based elastomers. If necessary, antioxidants, age resistors, etc. may be added to prevent thermal deterioration and thermal decomposition.
[0038] [Production of resin composition] The resin composition can be prepared by compounding and mixing the above-mentioned materials while heating in a known manner. Diluting the composition with an organic solvent increases workability, but places restrictions on application, so it is preferable to avoid using organic solvents whenever possible.
[0039] <Lump> The lump is a hot melt adhesive packaged in a melting bag. The weight is preferably 10 g to 5000 g. If the weight is within the above range, it is easy to handle and has excellent workability in terms of the number of times it can be filled, which is preferable. The thickness of the melting bag can be appropriately adjusted depending on the weight. After forming (manufacturing) the melt bag, a mass can be obtained by filling it with hot melt adhesive so that as little air as possible gets in. From the viewpoint of energy efficiency, this process is preferably cooled immediately after forming the film or carried out underwater.
[0040] (Hot melt adhesive) For example, when the hot melt adhesive is intended for adhesive applications, it is preferable that the resin system contains a styrene-based elastomer, which is easy to exhibit various adhesive properties. As the styrene-based elastomer, the material used in the resin composition for manufacturing the melt bag described above can be used as it is. In terms of compatibility in a melting furnace, it is more preferable to use the same type of material as the resin composition. Specifically, it is preferable to contain a styrene-based elastomer (A), a process oil (B), and a tackifier (C). The types of the styrene-based elastomer (A), the process oil (B) and the tackifier (C) can be appropriately selected depending on the application of the hot melt. For example, for recycling purposes, a tackifier with a high acid value of 100 mgKOH / g or more is preferred since it is required to be releasable by an alkaline aqueous solution. Also, for environmentally friendly products, a tackifier with a high biomass degree of 80% or more is preferred.
[0041] The softening point of the hot melt adhesive is preferably 40° C. to 110° C., more preferably 50° C. to 100° C., and even more preferably 60° C. to 90° C. A hot melt adhesive having a softening point within the above range exhibits tackiness at room temperature, and therefore has excellent compatibility with melting bags while enjoying the advantages of being made into a mass, and also easily exhibits cohesive force when used as a hot melt.
[0042] The softening point of the hot melt adhesive is preferably within 70° C. of the softening point of the melting bag, more preferably within 50° C., even more preferably within 30° C., and particularly preferably within 20° C. The difference between the softening point of the hot melt adhesive and the softening point of the melting bag is within the above range, resulting in excellent compatibility between the two.
[0043] <Hot melt sheet> The hot melt sheet is a sheet-shaped product of a lump, which can be produced by melting the lump in a melting furnace and forming it into a sheet by any coating method.
[0044] The coating method is not particularly limited, but any known method can be used. Examples include the open wheel method, the closed gun method, and the direct coat method. When removability is important depending on the application, the open wheel method and the direct coat method are preferred. The thickness of the hot melt sheet varies depending on the application, but is generally in the range of 10 μm to 1000 μm.
[0045] The ball tack of the hot melt sheet is not particularly limited, but is preferably 4 or more for label applications such as food packaging. A ball tack of 4 or more is preferable because sufficient adhesive strength can be obtained.
[0046] <Hot melt laminate> The hot melt laminate is a laminate in which a hot melt sheet and an adherend are arranged in this order. There are no particular limitations on the manufacturing method, but it can be obtained by (a) a method in which a hot melt is applied to the release-treated surface of a release-treated film to prepare a hot melt sheet with a release film, and an adherend is laminated on the surface of the hot melt layer, (b) a method in which a hot melt is directly applied to the adherend, and the release-treated surface of the release-treated film is laminated on the surface of the hot melt layer, or (c) a method in which the release film is peeled off from the laminate obtained by (a) or (b), and an adherend is further laminated on the surface of the hot melt layer.
[0047] (adherent) The adherend is not particularly limited, but plastic, nonwoven fabric, and paper can be suitably used. Examples of plastics include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), acrylic resins such as polymethyl methacrylate (PMMA), and other plastic materials such as polycarbonate, triacetyl cellulose, polysulfone, polyarylate, and polycycloolefin. Examples of nonwoven fabrics include nonwoven fabrics made of hydrophilic fibers such as cotton and rayon, and nonwoven fabrics made of synthetic resin fibers that have been subjected to a hydrophilic treatment. Examples of paper include Yupo paper, coated paper, wood-free paper, and cardboard. The adherends may be used alone or in combination of two or more kinds.
[0048] There are no particular limitations on the uses of hot melt laminates, but examples include food labels, hygiene products such as diapers and sanitary products, and bonding materials used in computers, cameras, and medical equipment. . EXAMPLES
[0049] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited thereto. In the examples, unless otherwise specified, "parts" means "parts by mass", "%" means "% by mass", and "RH" means relative humidity. The blending amounts in the tables are in parts by mass. Note that blanks in the tables indicate that no blending was performed.
[0050] [Weight average molecular weight] The weight average molecular weight (Mw) was measured using a GPC "LC-GPC system" manufactured by Shimadzu Corporation. The weight average molecular weight (Mw) can be determined by conversion using polystyrene with a known molecular weight as a standard substance. Device name: Shimadzu Corporation, LC-GPC system "Prominence" Column: Four GMHXL columns manufactured by Tosoh Corporation and one HXL-H column manufactured by Tosoh Corporation were connected together. Mobile phase solvent: Tetrahydrofuran Flow rate: 1.0ml / min Column temperature: 40℃
[0051] The abbreviations used in Tables 1 to 4 are as follows: [Styrene-based elastomer (A)] G1642: Kraton G1642 (Kraton Polymers, styrene content: 2 1% by mass, weight average molecular weight: 124,000) G1650: Kraton G1650 (Kraton Polymers, styrene content: 3 0% by mass, weight average molecular weight: 96,000) A1536: Kraton A1536 (Kraton Polymers, styrene content: 4 2% by mass, weight average molecular weight: 135,000) G1726: Kraton G1726 (Kraton Polymers, styrene content: 30% by mass, weight average molecular weight: 46,000)
[0052] [Process oil (B)] PW-90: Diana Process PW-90 (Idemitsu Kosan, paraffin-based process oil)
[0053] [Tackifier (C)] P-100: Alcon P-100 (Arakawa Chemical Co., Ltd., fully hydrogenated petroleum resin, softening point: 100°C) M-100: Alcon M-100 (Arakawa Chemical Co., Ltd., partially hydrogenated petroleum resin, softening point: 100°C) Haritac F (Harima Chemicals, hydrogenated rosin type, acid value: 170 mg KOH / g, softening point: 80°C)
[0054] [wax] Sasol H1 (manufactured by Sasol Chemical Industries, Fischer-Tropsch wax, softening point: 112°C) Sasol C80 (manufactured by Sasol Chemical Industries, Fischer-Tropsch wax, softening point: 88°C)
[0055] [Other thermoplastic elastomers] LDPE: Low density polyurethane (melting peak temperature 107℃, density 0.919g / cm 3 ) EVA: Ethylene-vinyl acetate copolymer (vinyl acetate content 28% by mass)
[0056] [Other tackifiers] Petokol 120: Petokol 120 (manufactured by Tosoh Corporation, non-hydrogenated petroleum resin, softening point: 120°C)
[0057] Example 1 <Production of Resin Composition P-1> In a stainless steel beaker equipped with a stirrer, 30 parts of wax: Sasol H1 and 20 parts of PW-90 as process oil (B) were added and heated to melt. Heating was performed carefully so that the contents were at 130 to 150 ° C. After melting, stirring was performed to obtain a homogeneous molten liquid, and then 10 parts of G1642 as a styrene-based elastomer (A) was added to the molten liquid while maintaining the temperature at 130 to 150 ° C and continuing to stir. After the addition was completed, the mixture was heated and stirred at a temperature of 130 to 150 ° C to completely melt G1642. Then, 40 parts of tackifier (C): P-100 was added to obtain a molten homogeneous mixture, which was then cooled to produce a resin composition P-1.
[0058] <Manufacture of hot melt adhesive Q-1> In a stainless steel beaker equipped with a stirrer, 5 parts of wax: Sasol C80 and 40 parts of PW-90 as process oil (B) were added and heated to melt. Heating was performed carefully so that the contents would reach 130 to 150°C. After melting, stirring was performed to obtain a homogeneous molten liquid, and then 25 parts of G1726 as a styrene-based elastomer (A) was added to the molten liquid while maintaining the temperature at 130 to 150°C and continuing to stir. After the addition was completed, the mixture was heated and stirred at a temperature of 130 to 150°C to completely melt G1726. Then, 30 parts of Haritac F was added as a tackifier (C) to obtain a homogeneous molten mixture, which was then cooled to produce hot melt adhesive Q-1. <Production of melt bag and lump 1> Next, resin composition P-1 was placed in a melt bag molding machine and set to form a melt bag with a thickness of 200 μm under the condition of a temperature of 100° C. 500 g of hot melt adhesive Q-1 was extruded toward the molten film while being heated, and molded so as to encase it in water. After cooling in the water as it is, lump 1 was obtained.
[0059] <Manufacturing of hot melt sheets> The obtained lump 1 was melted for 1 hour in a melting furnace heated to 160°C, and coated onto the release agent layer of a heavy release film so that the thickness of the sheet after formation was 25 µm to form a hot melt sheet. Next, the release agent layer of a light release film was bonded to this hot melt layer to obtain a hot melt sheet.
[0060] (Examples 2 to 20, Comparative Examples 1 and 2) Hot melt adhesives (Q-2 to 6) were produced in the same manner as in Example 1, except that the compositions and amounts (parts by mass) were changed to those shown in Table 1. Resin compositions (P-2 to 20, P'-1, 2) were produced in the same manner as in Example 1, except that the compositions and amounts (parts by mass) were changed to those shown in Tables 2 to 4. Subsequently, in the same manner as in Example 1, the lumps and hot melt sheets of Examples 2 to 20 and Comparative Examples 1 and 2 were obtained by filling the hot melt into a melting bag. In Tables 1 to 4, hot melt is abbreviated as HM, styrene-based elastomer as elastomer, process oil as oil, tackifier as TF, and wax as WAX.
[0061] [Table 1]
[0062] [Table 2]
[0063] [Table 3]
[0064] [Table 4]
[0065] <Ball tuck> The resulting hot melt sheet was prepared to a size of 25 mm wide and 250 mm long. The light release film was removed from the hot melt sheet and it was fixed to an inclined plate with an inclination angle of 30 degrees, and the heavy release film was removed to place the adhesive side facing up. A PET film for the runway was attached to the top, and a steel ball (1 / 32 to 32 / 32 inches) was rolled over the sample with a runway of 10 cm and an adhesive surface of 10 cm, and the diameter number of the ball that stopped near the center of the adhesive surface was recorded.
[0066] <Easy to deform> The ease of deformation (deformability) of the obtained lump was evaluated using a rubber hardness tester Type A (a durometer hardness tester manufactured by Shimadzu Corporation) The evaluation criteria were as follows: [Evaluation Criteria] ◎: Measurement scale is 20 points or less, excellent. ○: Measurement scale is between 20 and 30 points, good. △: Measurement scale is between 30 and 40 points, no practical problems. ×: The measurement scale is over 40 points, which is problematic for practical use.
[0067] <Crush resistance> A release film was laid on a small piece of cardboard, molten hot melt adhesive was poured onto it, and it was allowed to cool naturally and harden to produce a block of hot melt adhesive with a flat surface. A melting bag (10 cm square, 200 μm thick) was layered on top of the resulting block of hot melt adhesive, and a melting bag (10 cm square, 200 μm thick) and a block of hot melt adhesive were layered on top of that in that order to produce a block of hot melt adhesive / melting bag / / melting bag / block. A laminate of hot melt in a rock shape was prepared. A 10 kg weight was placed on the laminate, and it was stored at 40°C for 24 hours. After cooling in air, the melted bags were peeled apart by hand to evaluate the shatter resistance. The evaluation criteria were as follows: [Evaluation Criteria] ◎: No peeling sound or peeling strength, excellent. Good: Slight peeling sound, some peeling strength, good. △: Blocking occurred, but the molten bag did not break even when peeled off, and there was no problem in practical use. ×: Blocking occurred and the melted bag would break when peeled off, which would be problematic in practical use.
[0068] <compatibility> A white melting bag was prepared by mixing 1% by mass of titanium oxide with respect to the total mass of the melting bag, and this was used to prepare a white mass. The compatibility of the white melting bag and the hot melt adhesive in the melting furnace when preparing a hot melt sheet from the obtained white mass was evaluated based on the white unevenness of the hot melt sheet. The evaluation criteria are as follows. [Evaluation Criteria] ◎: No color unevenness, excellent. ◯: Good, with some color unevenness in some areas. △: Although color unevenness was observed overall, there was no remaining melted part in the melting bag, and there was no problem in practical use. ×: Color unevenness was observed overall, and melted bags remained. Problematic for practical use.
[0069] From the results in Tables 2 to 4, the aggregates of Examples 1 to 20 were excellent in workability during packaging and transportation, such as crush resistance and ease of deformation, and furthermore, the melting bags had excellent compatibility with the contents when used. On the other hand, the aggregates of Comparative Examples 1 and 2 did not satisfy all of the above characteristics. [Explanation of symbols]
[0070] 1 Melting Bag 2. Hot melt adhesives
Claims
1. Contains a styrene-based elastomer (A) and a tackifier (C), A melt bag in which the tackifier (C) contains at least one of a fully hydrogenated petroleum resin and a partially hydrogenated petroleum resin.
2. 2. The melt bag of claim 1 having a softening point of 50° C. or higher.
3. The melt bag according to claim 1 or 2, wherein the membrane thickness is 25 to 500 μm.
4. 3. The melt bag according to claim 1, wherein the styrene-based elastomer (A) has a weight average molecular weight of 300,000 or less.
5. 3. The melt bag according to claim 1 or 2, for packaging hot melt adhesives.
6. A mass in which a hot melt adhesive is packaged in a melt bag, the melt bag being the melt bag according to claim 1 or 2.
7. 7. The mass according to claim 6, wherein the difference between the softening point of the hot melt adhesive and the softening point of the melting bag is within 50°C.
8. A hot melt sheet which is a sheet-shaped product of the lump according to claim 6.
9. The hot melt sheet according to claim 8, wherein a hot melt sheet having a thickness of 25 μm is fixed to an inclined plate with an inclination angle of 30 degrees, a steel ball (1 / 32 to 32 / 32 inches) is rolled on the sample with a run-up of 10 cm and a glue surface of 10 cm, and the ball that stops near the center of the glue surface has a diameter number (ball tack) of 4 or more.
10. A hot melt laminate comprising the hot melt sheet according to claim 8 and an adherend, disposed in this order.
Citation Information
Patent Citations
Material and method for packaging hot melt adhesive
JP2002362661A
Method for packaging hot-melt adhesive-like plastic materials
JP2008518851A
Hot melt adhesive
JP2019119811A
Film suitable for melted bag and melted bag
JP2004002581A
Thermoplastic resin film, melting bag and packaged hot melt adhesive
JP2019065164A