Stretched product

A bimodal molecular weight distributed polyethylene composition, produced with a co-supported metallocene catalyst, addresses the challenge of balancing mechanical strength and processability in ultra-high molecular weight polyethylene, resulting in stretched products with enhanced properties for diverse applications.

JP2024166532APending Publication Date: 2024-11-29TOSOH CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023082689
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing polyethylene compositions, particularly ultra-high molecular weight polyethylene, face challenges in achieving a balance between improved mechanical strength and processability, especially in stretching processes, leading to difficulties in molding and extrusion due to high molecular weight and low fluidity.

Method used

A polyethylene composition with a bimodal molecular weight distribution, comprising ethylene resin with specific melt flow rates and density, combined with ultra-high molecular weight polyethylene, is produced using a co-supported metallocene catalyst system, allowing for enhanced stretching processability and mechanical properties.

Benefits of technology

The composition achieves a balanced tensile strength and processability, enabling the production of stretched products with improved mechanical properties and reduced thickness, suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166532000001
    Figure 2024166532000001
  • Figure 2024166532000002
    Figure 2024166532000002
  • Figure 2024166532000003
    Figure 2024166532000003
Patent Text Reader

Abstract

To provide a stretched product which is converted into a polyethylene composition of polyethylene and a high-molecular-weight ethylenic resin having a bimodal molecular weight, and thereby is excellent in tensile characteristics such as stretching workability, tensile braking stress and elastic modulus.SOLUTION: A stretched product made of a polyethylene composition contains an ethylenic resin having an HLMFR at a temperature of 190°C and a load of 21.6 kg of 0.01 to 100 g / 10 min and a bimodal elution curve measured by GPC, and polyethylene having an MFR at a temperature of 190°C and a load of 2.16 kg of 0.01 to 10 g / 10 min and a density of 930 to 980 kg / m3.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a specific stretched product, and more specifically, to a stretched product which can improve the stretch processability and the mechanical strength of a molded product, and which is expected to reduce the thickness of the molded product and extend the life of the molded product. [Background technology]

[0002] Polyethylene is a resin used in a wide range of applications, and in order to make it suitable for each application, technologies have been proposed to control the molecular weight distribution and composition by combining two or more resin components, thereby improving various physical properties and appearance. For example, an increase in higher molecular weight components improves mechanical strength but decreases moldability, while an increase in lower molecular weight components decreases mechanical strength but improves moldability.

[0003] As a method for combining two or more types of polyethylene components, there have been proposed a method in which each component is polymerized and then blended by melt kneading or dry blending, a method in which multi-stage polymerization is carried out continuously, a method in which two or more types of polyethylene components are simultaneously produced by adding a plurality of transition metal catalysts to a polymerization system, a method in which a combination of these is carried out, etc. In addition, a resin modifier has also been proposed (see, for example, Patent Document 1) that is blended with a target material to modify the physical properties, appearance, etc. of the target material.

[0004] In the drawing, spinning, blow molding, injection molding, inflation molding, and extrusion molding of polyethylene, materials with good moldability and physical properties are generally required. In recent years, there has been a demand for lighter weight and thinner walls to reduce costs, but at the same time, there is a demand for excellent mechanical strength.

[0005] Ultra-high molecular weight polyethylene, which has attracted attention in recent years (see, for example, Patent Documents 2 and 3), has an extremely high molecular weight equivalent to a viscosity average molecular weight (hereinafter sometimes referred to as Mv) of 1 million or more, and therefore has excellent impact resistance, self-lubrication, abrasion resistance, weather resistance, chemical resistance, dimensional stability, etc., and has high physical properties comparable to those of engineering plastics. For this reason, attempts have been made to apply it to uses such as sheets, films, high-strength fibers, sliding members, lining materials, line parts in the food industry, machine parts, artificial joints, sporting goods, microporous membranes, and separators by various molding methods.

[0006] However, because of its high molecular weight, ultra-high molecular weight polyethylene has extremely low fluidity when melted, and it is difficult to mold it by kneading and extrusion like ordinary polyethylene, which has a molecular weight in the range of several tens of thousands to about 300,000.Therefore, ultra-high molecular weight polyethylene is molded by various methods, such as direct sintering of the polymer powder obtained by polymerization, compression molding, molding using a ram extruder in which extrusion molding is performed while intermittently compressing, and extrusion molding into a sheet, film, or fiber shape in a state where it is uniformly mixed with a plasticizer, and in some cases, stretching it and then removing the solvent.

[0007] In order to improve the moldability of ultra-high molecular weight polyethylene and its mixability with other resins, a method of adding low molecular weight polyethylene has been proposed (see, for example, Patent Documents 4 and 5), and an ultra-high molecular weight polyethylene exhibiting a specific melting behavior has been proposed (see, for example, Patent Document 6). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2017-179304 A [Patent Document 2] Patent No. 4868853 [Patent Document 3] Patent No. 6405888 [Patent Document 4] Patent No. 4173444 [Patent Document 5] Patent No. 7071966 [Patent Document 6] JP 2021-172716 A Summary of the Invention [Problem to be solved by the invention]

[0009] However, although the modified material proposed in Patent Document 1 was effective in improving processability to a certain extent, further improvement was required in terms of improving mechanical strength.

[0010] Moreover, Patent Documents 2 and 3 merely propose ultra-high molecular weight polyethylene, and have problems with moldability. The proposals in Patent Documents 4 to 6 also only improve the processability of ultra-high molecular weight polyethylene, and still have problems with versatility.

[0011] Therefore, there has been a demand for the development of stretched products that have excellent mechanical properties without impairing the processability, particularly the stretch processability, of general-purpose resins. [Means for solving the problem]

[0012] Means for Solving the Problems The present inventors have conducted intensive studies to solve the above problems and have found that a polyethylene composition comprising an ethylene-based resin and a polyethylene having specific melting properties and molecular weight configuration has excellent stretch processability and can give a stretched product having excellent tensile properties such as tensile stress at break and elastic modulus, thereby completing the present invention.

[0013] That is, the present invention relates to: (1) an ethylene-based resin having a high melt flow rate (HLMFR) of 0.01 to 100 g / 10 min at a temperature of 190° C. and a load of 21.6 kg in accordance with JIS 6922-2:1997 and a bimodal elution curve measured by gel permeation chromatography; and (2) an ethylene-based resin having a melt flow rate (MFR) of 0.01 to 10 g / 10 min at a temperature of 190° C. and a load of 2.16 kg in accordance with JIS 6922-2:1997 and a density of 930 to 980 kg / m as measured according to JIS K6922-1 (1997). 3 The present invention relates to a stretched product characterized by being made of a polyethylene composition containing a polyethylene of the formula:

[0014] The present invention will be described in detail below.

[0015] The stretched product of the present invention is (1) an ethylene-based resin (C) having a melt flow rate (hereinafter sometimes referred to as HLMFR) of 0.01 to 100 g / 10 min at a temperature of 190° C. and a load of 21.6 kg in accordance with JIS 6922-2:1997 and a bimodal elution curve measured by gel permeation chromatography (hereinafter sometimes referred to as GPC); and (2) an ethylene-based resin (C) having a melt flow rate (hereinafter sometimes referred to as MFR) of 0.01 to 10 g / 10 min at a temperature of 190° C. and a load of 2.16 kg in accordance with JIS 6922-2:1997 and a density of 930 to 980 kg / m2 measured according to JIS K6922-1 (1997). 3The stretched product is a polyethylene composition (e) containing a polyethylene (d) of the formula: The ethylene-based resin (c) may be a bimodal ethylene-based resin having a relatively high molecular weight that exhibits melting behavior and a bimodal elution curve measured by GPC that exhibits two peaks, and examples of the ethylene homopolymer and ethylene-α-olefin copolymer are available. Examples of the α-olefin include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, etc., and ethylene homopolymer is preferred because the stretched product has excellent tensile properties. Similarly, examples of the polyethylene (d) include ethylene homopolymer and ethylene-α-olefin copolymer, and examples of the α-olefin include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, etc., and ethylene homopolymer is preferred because the stretched product has excellent tensile properties.

[0016] The ethylene-based resin (iii) has (1) an HLMFR of 0.01 to 100 g / 10 min and exhibits melt fluidity. If it is less than 0.01 g / 10 min, the melt fluidity is poor and the processability when stretched is poor. On the other hand, if it is more than 100 g / 10 min, the stretched product has poor mechanical properties.

[0017] The ethylene resin (iii) constituting the stretched product of the present invention is an ethylene polymer having a bimodal molecular weight distribution, and preferably contains a specific ultra-high molecular weight polyethylene component (i) as a specific component, since the stretched product has an excellent balance between processability and tensile properties. In this case, the bimodal molecular weight distribution is preferably one in which the elution curve measured by GPC has two peaks, and when the elution curve is expressed as a differential molecular weight distribution (x-axis: Log[M], y-axis: differential distribution value) and the peaks are divided into two normal distributions (normal distribution of ultra-high molecular weight polyethylene component (i) and normal distribution of polyethylene component (ii)) according to the following formula (i), it satisfies (2-1) to (2-3). f(x)=a×(1 / (2π(σ 2 )) (1 / 2) ) exp(-((x-μ) 2 ) / (2(σ 2 ))) Formula (i) (Here, a is the peak intensity, σ is the standard deviation, x is the variable, and μ is the mean.) (2-1) The ultra-high molecular weight polyethylene component (a) (hereinafter may be referred to as component (a)) represented as the high molecular weight peak component has an Mw of 900,000 to 5,000,000 and a molecular weight distribution represented by Mw / Mn of 2.0 to 5.0, (2-2) The polyethylene component (b) (hereinafter may be referred to as component (b)) represented as the low molecular weight peak component has an Mw of 10,000 to 500,000 and Mw / Mn of 2.0 to 5.0, and (2-3) the component (a) / component (b) (weight ratio) is greater than 5 / 95 and less than 80 / 20, and it is particularly preferable that the component (a) / component (b) (weight ratio) is 10 / 90 to 50 / 50.

[0018] When the ethylene-based resin (iii) is one in which the ultra-high molecular weight component (i) and the low molecular weight component (ii) coexist in a specific ratio, when blended with polyethylene, the component (i) can be highly dispersed, making it possible to highly modify the tensile properties of the stretched product without impairing the appearance.

[0019] In order to obtain a stretched product having a particularly excellent balance between dispersibility in polyethylene and improved mechanical properties, the ethylene-based resin (C) preferably has (3) Mw / Mn, calculated as linear polyethylene as measured by GPC, of ​​4.0 or more and less than 50, and particularly preferably 4.0 or more and 30 or less.

[0020] In addition, since the components (A) and (B) are different from a simple blend in which they are independently dispersed, it is preferable that the ethylene-based resin (C) has a single-peak crystal melting peak (hereinafter sometimes referred to as Tm1) in the first scan measured using a differential scanning calorimeter (hereinafter sometimes referred to as DSC) by heating from 0°C to 230°C at a heating rate of 10°C / min (hereinafter sometimes referred to as 1st scan).

[0021] The ethylene-based resin (iii) constituting the stretched product of the present invention may be any resin as long as it satisfies the above-mentioned characteristics. In particular, it is preferable that the resin is produced using a metallocene-based catalyst, since it is easy to control the molecular weight and molecular weight distribution and to produce an (ultra)high molecular weight resin. Among these, examples of a method for producing the ethylene-based resin (iii) having both components (i) and (ii) include a method using a co-supported catalyst in which two or more types of metallocene complexes are supported on a carrier as the catalyst system, and a method using a multi-stage polymerization of two or more stages.

[0022] The polymerization method of the ethylene-based resin (iii) may be, for example, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method, a slurry polymerization method, etc., among which, the slurry polymerization method is preferable since it enables the production of an ethylene-based resin with a regular particle shape. The solvent used in the slurry polymerization method may be any organic solvent that is generally used, for example, benzene, toluene, xylene, pentane, hexane, heptane, etc., and liquefied gases such as isobutane and propane, and olefins such as 1-butene and 1-hexene can also be used as the solvent.

[0023] The production catalyst used to produce the ethylene-based resin (iii) may be any catalyst capable of producing the ethylene-based resin. For example, in the case of multi-stage polymerization, a metallocene catalyst obtained from at least a transition metal compound (A-1), an organically modified clay modified with an aliphatic salt (B), and an organoaluminum compound (C) may be used. For example, in the case of a co-supported catalyst method, a metallocene catalyst obtained from at least a transition metal compound (A-1), a transition metal compound (A-2), an organically modified clay modified with an aliphatic salt (B), and an organoaluminum compound (C) may be used.

[0024] Examples of the transition metal compound (A-1) include a transition metal compound having a (substituted) cyclopentadienyl group and a (substituted) fluorenyl group, a transition metal compound having a (substituted) cyclopentadienyl group and a (substituted) indenyl group, and a transition metal compound having a (substituted) indenyl group and a (substituted) fluorenyl group. In this case, examples of the transition metal include zirconium and hafnium. Among these, a zirconium compound having a (substituted) cyclopentadienyl group and an amino group-substituted fluorenyl group and a hafnium compound having a (substituted) cyclopentadienyl group and an amino group-substituted fluorenyl group are preferred, as they enable efficient production of an ethylene-based resin suitable for use as a stretched product.

[0025] More specifically, for example, diphenylmethylene(1-indenyl)(9-fluorenyl)zirconium dichloride, diphenylmethylene(1-indenyl)(2,7-di-t-butyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(4-phenyl-1-indenyl)(2,7-di-t-butyl-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(2-(dimethylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(2-(dimethylamino)-9-fluorenyl)zirconium dichloride, )(2-(diethylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(2-(dibenzylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(2,7-bis(dimethylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(2,7-bis(diethylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(2,7-bis (dibenzylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(4-(dimethylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(4-(diethylamino)-9-fluorenyl)zirconium dichloride, diphenylsilanediyl(cyclopentadienyl)(4-(dibenzylamino)-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dimethylamino)-9-fluorenyl)zirconium dichloride diphenylmethylene(cyclopentadienyl)(2-(diethylamino)-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(diisopropylamino)-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dibenzylamino)-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(diethylamino)-7-ethyl-9-fluorenyl)zirconium dichloride,Diphenylmethylene(cyclopentadienyl)(2-(diisopropylamino)-7-ethyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dibenzylamino)-7-ethyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dimethylamino)-7-n-propyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(diethylamino)-7-n-propyl-9-fluorenyl)zirconium dichloride diphenylmethylene(cyclopentadienyl)(2-(diisopropylamino)-7-n-propyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dibenzylamino)-7-n-propyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dimethylamino)-7-isopropyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(diphenylmethylene)(cyclopentadienyl)(2-(diphenylmethylene)(cyclopentadienyl) diphenylmethylene(cyclopentadienyl)(2-(diisopropylamino)-7-isopropyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dibenzylamino)-7-isopropyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dimethylamino)-7-n-butyl-9-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2-(dimethylamino)-7-n-butyl-9-fluorenyl)zirconium dichloride Examples of zirconium compounds include diphenylmethylene(cyclopentadienyl)(2-(diisopropylamino)-7-t-butyl-9-fluorenyl)zirconium dichloride and diphenylmethylene(cyclopentadienyl)(2-(dibenzylamino)-7-t-butyl-9-fluorenyl)zirconium dichloride; zirconium compounds in which the dichloro form of these compounds is replaced with a dimethyl form, a diethyl form, a dihydro form, a diphenyl form or a dibenzyl form; and hafnium compounds in which the zirconium of these compounds is replaced with hafnium.

[0026] Examples of the transition metal compound (A-2) include a transition metal compound having a (substituted) cyclopentadienyl group and a (substituted) fluorenyl group, a transition metal compound having a (substituted) cyclopentadienyl group and a (substituted) indenyl group, and a transition metal compound having a (substituted) indenyl group and a (substituted) indenyl group.

[0027] More specifically, dimethylsilanediylbis(cyclopentadienyl)zirconium dichloride, diethylsilanediylbis(cyclopentadienyl)zirconium dichloride, dicyclohexylsilanediylbis(cyclopentadienyl)zirconium dichloride, diphenylsilanediylbis(cyclopentadienyl)zirconium dichloride, dimethylsilanediylbis(methylcyclopentadienyl)zirconium dichloride, diethylsilanediylbis(methylcyclopentadienyl)zirconium dichloride, dicyclohexylsilanediylbis(cyclopentadienyl)zirconium dichloride, Silanediylbis(methylcyclopentadienyl)zirconium dichloride, diphenylsilanediylbis(methylcyclopentadienyl)zirconium dichloride, dimethylsilanediylbis(2,4-dimethylcyclopentadienyl)zirconium dichloride, diethylsilanediylbis(2,4-dimethylcyclopentadienyl)zirconium dichloride, dicyclohexylsilanediylbis(2,4-dimethylcyclopentadienyl)zirconium dichloride, diphenylsilanediylbis(2,4-dimethylcyclopentadienyl)zirconium dichloride silanediyl[(cyclopentadienyl)(indenyl)]zirconium dichloride, dimethylsilanediyl[(cyclopentadienyl)(indenyl)]zirconium dichloride, diethylsilanediyl[(cyclopentadienyl)(indenyl)]zirconium dichloride, dicyclohexylsilanediyl[(cyclopentadienyl)(indenyl)]zirconium dichloride, diphenylsilanediyl[(cyclopentadienyl)(indenyl)]zirconium dichloride, dimethylsilanediyl[(cyclopentadienyl)(4,7-dimethylindenyl)]zirconium dichloride silanediyl[(cyclopentadienyl)(4,7-dimethylindenyl)]zirconium dichloride, dicyclohexylsilanediyl[(cyclopentadienyl)(4,7-dimethylindenyl)]zirconium dichloride, diphenylsilanediyl[(cyclopentadienyl)(4,7-dimethylindenyl)]zirconium dichloride, dimethylsilanediyl[(cyclopentadienyl)(2,4,7-trimethylindenyl)]zirconium dichloride, diethylsilanediyl[(cyclopentadienyl)(2,4,7-trimethylindenyl)]zirconium dichloride, dicyclohexylsilanediyl[(cyclopentadienyl)(2,4,7-trimethylindenyl)]zirconium dichloride, diphenylsilanediyl[(cyclopentadienyl)(2,4,7-trimethylindenyl)]zirconium dichloride, bis(indenyl)zirconium dichloride, isopropylidenebis(indenyl)zirconium dichloride, (methyl)(phenyl)methylenebis(indenyl)zirconium dichloride, diphenyl Phenylmethylene bis(indenyl)zirconium dichloride, ethylene bis(indenyl)zirconium dichloride, isopropylidene bis(2-methylindenyl)zirconium dichloride, (methyl)(phenyl)methylene bis(2-methylindenyl)zirconium dichloride, diphenylmethylene bis(2-methylindenyl)zirconium dichloride, ethylene bis(2-methylindenyl)zirconium dichloride, isopropylidene bis(tetrahydroindenyl)zirconium dichloride , (methyl)(phenyl)methylenebis(tetrahydroindenyl)zirconium dichloride, diphenylmethylenebis(tetrahydroindenyl)zirconium dichloride, ethylenebis(tetrahydroindenyl)zirconium dichloride, isopropylidene(cyclopentadienyl)(fluorenyl)zirconium dichloride, (methyl)(phenyl)methylene(cyclopentadienyl)(fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride dichloride, ethylene(cyclopentadienyl)(fluorenyl)zirconium dichloride, isopropylidene(cyclopentadienyl)(2,7-di-t-butyl-fluorenyl)zirconium dichloride, (methyl)(phenyl)methylene(cyclopentadienyl)(2,7-di-t-butyl-fluorenyl)zirconium dichloride, diphenylmethylene(cyclopentadienyl)(2,7-di-t-butyl-fluorenyl)zirconium dichloride, ethylene(cyclopentadienyl)(2,7-di-t-butyl-fluorenyl)zirconium dichloride; zirconium compounds in which the dichloro form of these compounds is replaced with a dimethyl form, a diethyl form, a dihydro form, a diphenyl form, or a dibenzyl form; and hafnium compounds in which the zirconium of these compounds is replaced with hafnium.

[0028] Examples of the organically modified clay (B) modified with an aliphatic salt include N,N-dimethyl-behenylamine hydrochloride, N-methyl-N-ethyl-behenylamine hydrochloride, N-methyl-Nn-propyl-behenylamine hydrochloride, N,N-dioleyl-methylamine hydrochloride, N,N-dimethyl-behenylamine hydrofluoride, N-methyl-N-ethyl-behenylamine hydrofluoride, N-methyl-Nn-propyl-behenylamine hydrofluoride, N,N-dioleyl-methylamine hydrofluoride, N,N-dimethyl-behenyl ... behenylamine hydrobromide, N-methyl-N-ethyl-behenylamine hydrobromide, N-methyl-Nn-propyl-behenylamine hydrobromide, N,N-dioleyl-methylamine hydrobromide, N,N-dimethyl-behenylamine hydroiodide, N-methyl-N-ethyl-behenylamine hydroiodide, N-methyl-Nn-propyl-behenylamine hydroiodide, N,N-dioleyl-methylamine hydroiodide, N,N-dimethyl-behenylamine sulfate, N-methyl-N-ethyl-behenylamine sulfate aliphatic amine salts such as N-methyl-Nn-propyl-behenylamine sulfate and N,N-dioleyl-methylamine sulfate; P,P-dimethyl-behenylphosphine hydrochloride, P,P-diethyl-behenylphosphine hydrochloride, P,P-dipropyl-behenylphosphine hydrochloride, P,P-dimethyl-behenylphosphine hydrofluoride, P,P-diethyl-behenylphosphine hydrofluoride, P,P-dipropyl-behenylphosphine hydrofluoride, P,P-dimethyl-behenylphosphine hydrobromide, P,P- Examples of the clay modified with an aliphatic salt include aliphatic phosphonium salts such as diethyl-behenylphosphine hydrobromide, P,P-dipropyl-behenylphosphine hydrobromide, P,P-dimethyl-behenylphosphine hydroiodide, P,P-diethyl-behenylphosphine hydroiodide, P,P-dipropyl-behenylphosphine hydroiodide, P,P-dimethyl-behenylphosphine sulfate, P,P-diethyl-behenylphosphine sulfate, and P,P-dipropyl-behenylphosphine sulfate.

[0029] The clay compound constituting the organically modified clay (B) may be any compound as long as it belongs to the category of clay compounds. In general, the organically modified clay (B) is formed by stacking many layers called silicate layers, which are composed of a tetrahedral sheet of silica tetrahedrons connected in two dimensions and an octahedral sheet of alumina octahedrons or magnesia octahedrons connected in two dimensions in a 1:1 or 2:1 ratio. The Si in some of the silica tetrahedra is replaced by Al, the Al in the alumina octahedrons by Mg, and the Mg in the magnesia octahedrons by Li, etc., resulting in a lack of positive charges within the layers and the layers as a whole being negatively charged. In order to compensate for this negative charge, Na is introduced between the layers. + Or Ca 2+ As the clay compound, there are natural or synthetic products such as kaolinite, talc, smectite, vermiculite, mica, brittle mica, and malachite, and these can be used, among which smectite is preferred because of its ease of availability and ease of organic modification, and among smectites, hectorite or montmorillonite is even more preferred.

[0030] The organically modified clay (B) can be obtained by introducing the aliphatic salt between the layers of the clay compound to form an ion complex. When preparing the organically modified clay (B), it is preferable to select conditions of a clay compound concentration of 0.1 to 30% by weight and a treatment temperature of 0 to 150°C. The aliphatic salt may be prepared as a solid and dissolved in a solvent for use, or a solution of the aliphatic salt may be prepared by chemical reaction in a solvent and used as is. As for the reaction ratio of the clay compound and the aliphatic salt, it is preferable to use an equivalent or greater amount of aliphatic salt relative to the exchangeable cations of the clay compound. Examples of the treatment solvent that can be used include aliphatic hydrocarbons such as pentane, hexane, and heptane; aromatic hydrocarbons such as benzene and toluene; alcohols such as ethyl alcohol and methyl alcohol; ethers such as ethyl ether and n-butyl ether; halogenated hydrocarbons such as methylene chloride and chloroform; acetone; 1,4-dioxane; tetrahydrofuran; water, and the like. It is preferable to use alcohols or water alone or as one component of the solvent.

[0031] In addition, the particle size of the organically modified clay (B) constituting the production catalyst is not limited, and is preferably 1 to 100 μm, since it is excellent in efficiency during catalyst preparation and efficiency during ethylene-based resin production. There is also no limit to the method of adjusting the particle size, and large particles may be crushed to an appropriate particle size, small particles may be granulated to an appropriate particle size, or crushing and granulation may be combined. In addition, the particle size may be adjusted either on the clay before organic modification or on the organically modified clay after modification.

[0032] As the organoaluminum compound (C), any compound that belongs to the category called an organoaluminum compound can be used, and examples thereof include alkylaluminum such as trimethylaluminum, triethylaluminum, and triisobutylaluminum.

[0033] The proportions of the transition metal compounds (A-1) and (A-2) (hereinafter, the transition metal compounds (A-1) and (A-2) are collectively referred to as component (A)), the organically modified clay (B) (hereinafter, also referred to as component (B)), and the organoaluminum compound (C) (hereinafter, also referred to as component (C)) constituting the production catalyst are not subject to any restrictions as long as they can be used as a production catalyst. In particular, in order to provide a production catalyst capable of efficiently producing the ethylene-based resin (C), the molar ratio per metal atom of component (A) to component (C) is preferably in the range of component (A):component (C)=100:1 to 1:100,000, and more preferably in the range of 1:1 to 1:10,000. Furthermore, the weight ratio of component (A) to component (B) is preferably component (A):component (B)=10:1 to 1:10000, and more preferably in the range of 3:1 to 1:1000.

[0034] Regarding the preparation method of the production catalyst, any method may be used as long as it is possible to prepare a production catalyst containing the (A) component, the (B) component, and the (C) component, and for example, a method of mixing the (A), (B), and (C) components in a solvent inert to the respective components, or using the monomer to be polymerized as a solvent, can be mentioned. In addition, there is no restriction on the order in which these components are reacted, and there is no restriction on the temperature and time of this treatment. In addition, it is also possible to prepare a production catalyst using two or more kinds of each of the (A), (B), and (C) components.

[0035] The polymerization conditions such as polymerization temperature, polymerization time, polymerization pressure, and monomer concentration when producing the ethylene resin (iii) can be arbitrarily selected, and among them, it is preferable to carry out the polymerization at a polymerization temperature of 0 to 100°C, for a polymerization time of 10 seconds to 20 hours, and at a polymerization pressure of normal pressure to 100 MPa. It is also possible to adjust the molecular weight by using hydrogen or the like during the polymerization. The polymerization can be carried out by any method such as a batch method, a semi-continuous method, or a continuous method, and it is also possible to carry out the polymerization in two or more stages by changing the polymerization conditions. The polymer particles obtained after the polymerization is completed can be separated and recovered from the polymerization solvent by a conventionally known method, and dried to obtain the product.

[0036] The polyethylene (iv) constituting the stretched product of the present invention has an MFR of 0.01 to 10 g / 10 min and a density of 930 to 980 kg / m 3 Examples of such polyethylene include those mentioned above, and among them, high density polyethylene is preferable, and an example of such polyethylene is Nipolon Hard (trade name, manufactured by Tosoh Corporation). 3 On the other hand, if the MFR exceeds 10 g / 10 min or the density is less than 930 g / m 3 If it is less than this, the stretchability and / or mechanical properties will be poor.

[0037] The blending amount when blending into the polyethylene composition (e) constituting the stretched product of the present invention is arbitrary as long as excellent tensile properties as a stretched product are exhibited. In particular, since an excellent balance between the mechanical properties and processability is achieved, it is preferable for the polyethylene composition (e) to contain 1 to 100 parts by weight of the ethylene resin (c) per 100 parts by weight of the polyethylene (d), and particularly preferably 5 to 50 parts by weight.

[0038] The polyethylene composition (e) constituting the stretched product of the present invention may be prepared by any method, and examples of the method include a method in which 1 to 100 parts by weight of an ethylene-based resin (c) is blended with 100 parts by weight of polyethylene (d) and, if necessary, additives usually used in polyolefins, such as a weather resistance stabilizer, a heat resistance stabilizer, an antistatic agent, an antislip agent, an antiblocking agent, an antifogging agent, a lubricant, a pigment, a nucleating agent, a plasticizer, an antioxidant, an antioxidant, an ultraviolet absorber, a neutralizing agent, a surfactant, a slip agent, and an inorganic or organic filler, and then blended and kneaded by a kneading machine or the like. The conditions for this may be any as long as it enables the formation of a polyethylene composition (E). For example, the ethylene-based resin (C) and polyethylene (D), and optionally other additives, may be heated, melted, and kneaded using a single-screw or twin-screw melt kneader or the like at a temperature in the range of 190°C to 250°C for about 20 to 30 seconds. The mixture may then be cut into granular pellets and used as a material for molding a uniaxially or multiaxially stretched product.

[0039] The stretched product of the present invention can be prepared by any method, for example, by preparing the polyethylene composition (e) described above and then stretching it, or by blending polyethylene (d), an ethylene-based resin (c), and other additives and stretching it as is. Examples of the method include a method of forming various structures such as films, sheets, fibers, and strands by various molding methods such as roll molding, inflation molding, calendar molding, extrusion molding, compression molding, injection molding, and blow molding, and subjecting them to a stretching step such as tenter stretching, roll stretching, and rolling, and a method of subjecting a molten polyethylene composition (e) to melt stretching and blow stretching to form a stretched product. The stretch ratio when forming a stretched product can be appropriately selected depending on the purpose, and can be, for example, 2 to 20 times, preferably 2 to 10 times. Also, uniaxial stretching, multiaxial stretching, simultaneous stretching, and successive stretching can be appropriately selected.

[0040] Since the stretched product of the present invention is particularly excellent in improving heat resistance, it is preferable that the difference (Tmd-Tm0) between the crystalline melting peak temperature (Tm0) of the raw sheet before stretching and the crystalline melting peak temperature (Tmd) of the stretched product is 5° C.≦Tmd-Tm0. The crystalline melting peak temperature can be measured by DSC as the crystalline melting peak temperature in the 1st scan when the temperature is raised from 0° C. to 230° C. at a heating rate of 10° C. / min (1st scan).

[0041] The stretched product of the present invention has an excellent balance between mechanical properties and processability, and can be used as various structural materials such as uniaxially oriented sheets, biaxially oriented sheets, uniaxially oriented films, biaxially oriented films, stretched tapes, stretched fibers, stretched yarns, and the like, as well as stretch-blown containers. Effect of the Invention

[0042] The stretched product can improve the stretch processability and the mechanical strength of the molded article, and is expected to enable the molded article to be made thinner and have a longer life, and is therefore expected to be applicable to a variety of uses. EXAMPLES

[0043] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to these examples as long as the gist of the present invention is not exceeded.

[0044] Unless otherwise specified, the reagents used were either commercially available or synthesized according to known methods.

[0045] The organically modified clay was pulverized using a jet mill (product name: CO-JET SYSTEM α MARK III, manufactured by Seishin Enterprise Co., Ltd.), and the particle size after pulverization was measured using a Microtrack particle size distribution measuring device (product name: MT3000, manufactured by Nikkiso Co., Ltd.) using ethanol as a dispersant.

[0046] The preparation of the catalyst for production, the production of the ethylene resin, and the purification of the solvent were all carried out under an inert gas atmosphere. The hexane solution (20 wt%) of triisobutylaluminum manufactured by Toso Finechem Co., Ltd. was used.

[0047] Furthermore, various physical properties of the ethylene resin and polyethylene were measured by the methods shown below.

[0048] ~Measurement of intrinsic viscosity ([η])~ The measurements were performed using an Ubbelohde viscometer, decahydronaphthalene as a solvent, at 135° C., and an ethylene resin concentration of 0.005 wt %.

[0049] ~Measurement of Mw and Mn~ Measurements were performed using an ultra-high temperature GPC (SSC-7110, manufactured by Senshu Scientific Co., Ltd.) equipped with a column (TSKgel GMHHR-H(S)HT, manufactured by Tosoh Corporation) with 1-chloronaphthalene as the eluent at a column temperature of 210°C, a sample concentration of 0.5 mg / ml, and an injection volume of 0.2 ml. The molecular weight calibration curve was calibrated using a standard polystyrene sample, and Mw and Mn were converted to linear polyethylene.

[0050] ~MFR~ The melt flow rate was measured at a temperature of 190° C. under a load of 2.16 kg in accordance with JIS6922-2:1997.

[0051] ~HLMFR~ The melt flow rate was measured at a temperature of 190° C. and a load of 21.6 kg in accordance with JIS6922-2:1997.

[0052] ~Measurement of thermal melting of ethylene resin~ Using a DSC (product name: DSC6220 manufactured by SII NanoTechnology, Inc.), the temperature was raised from 0°C to 230°C at a heating rate of 10°C / min (1st scan), and the crystal melting peak (Tm1) and heat of fusion (ΔH1) of the 1st scan were measured.

[0053] Furthermore, various physical properties of the stretched product were measured by the methods shown below.

[0054] ~Tensile properties~ The stretched material was cut into a 3 cm long strip and the 1% tensile modulus and tensile breaking stress of the test piece were measured at 25° C. and 50 mm / min using a tensile tester (manufactured by BALDWIN (product name) UTM-2.5T-PL).

[0055] ~Stretching ratio~ The stretch ratio was evaluated based on the stretch ratio (DRset) calculated from the chuck movement distance during stretching and the stretch ratio (DRexp) calculated from the change in cross-sectional area before and after stretching. The smaller the difference between DRset and DRexp, the more uniform the stretching was, and stretch processability was evaluated to be excellent when 0.8≦DRset / DRexp≦1.3.

[0056] ~Measurement of thermal melting of stretched material~ Using a DSC (manufactured by SII Nano Technology Co., Ltd., product name: DSC6220), the temperature was raised from 0°C to 230°C at a heating rate of 10°C / min (1st scan), and the crystal melting peak (Tm) and heat of fusion (ΔH) of the 1st scan were measured. The amount of polyethylene sample was 6 mg. The Tm of the original roll was Tm0, and the Tm of the stretched product was Tmd. If the difference between Tm0 and Tmd (Tmd-Tm0) was 5°C or less than Tmd-Tm0, the stretching was deemed to have a high effect of improving heat resistance.

[0057] Preparation Example 1 (1) Preparation of organically modified clay 300 ml of industrial alcohol (manufactured by Japan Alcohol Sales Co., Ltd., (trade name) Ekinen F-3) and 300 ml of distilled water were placed in a 1-liter flask, 15.0 g of concentrated hydrochloric acid and 42.4 g (120 mmol) of dimethylbehenylamine (manufactured by Lion Specialty Chemicals, (trade name) Lipomin DM22D) were added, and the mixture was heated to 45°C to disperse 100 g of synthetic hectorite (manufactured by BYK Additives Limited, (trade name) Laponite RDS), and then the mixture was heated to 60°C and stirred for 1 hour while maintaining the temperature. After filtering the slurry, it was washed twice with 600 ml of hot water at 60°C and dried in a dryer at 85°C for 12 hours to obtain 125 g of organically modified clay. This organically modified clay was pulverized in a jet mill to a median diameter of 10 μm.

[0058] (2) Preparation of catalyst suspension for production After replacing the air in a 300 ml flask equipped with a thermometer and reflux condenser with nitrogen, 25.0 g of the organically modified clay obtained in (1) and 108 ml of hexane were added, followed by 0.628 g of diphenylmethylene(cyclopentadienyl)(2-diethylamino-9-fluorenyl)zirconium dichloride and 142 ml of a hexane solution of 20 wt% triisobutylaluminum, and the mixture was stirred at 60°C for 3 hours. After cooling to 45°C, the supernatant was removed and washed twice with 200 ml of hexane, and then 200 ml of hexane was added to obtain a suspension of a catalyst for production (solid weight content: 12.5 wt%).

[0059] Preparation Example 2 (1) Preparation of organically modified clay The same procedure as in Preparation Example 1 was followed.

[0060] (2) Preparation of catalyst suspension for production After replacing the air in a 300 ml flask equipped with a thermometer and a reflux condenser with nitrogen, 25.0 g of the organically modified clay obtained in (1) and 108 ml of hexane were added, followed by 0.669 g of diphenylmethylene(cyclopentadienyl)(2,7-di-t-butyl-9-fluorenyl)zirconium dichloride and 142 ml of a hexane solution of 20 wt% triisobutylaluminum, and the mixture was stirred at 60°C for 3 hours. After cooling to 45°C, the supernatant was removed and washed twice with 200 ml of hexane, and then 200 ml of hexane was added to obtain a suspension of a catalyst for production (solid weight content: 12.5 wt%).

[0061] Preparation Example 3 (1) Preparation of organically modified clay In a 1-liter flask, 300 ml of industrial alcohol (product name Ekinen F-3, manufactured by Japan Alcohol Sales Co., Ltd.) and 300 ml of distilled water were added, and 15.0 g of concentrated hydrochloric acid and dioleylmethylamine ((C 18 H 35 )2(CH3)N, 63.7g (120mmol) of (Lipomin MO, manufactured by Lion Specialty Chemicals Co., Ltd.) was added and heated to 45℃, after which 100g of synthetic hectorite (Laponite RD, manufactured by BYK Co., Ltd.) was dispersed, and the temperature was raised to 60℃ and stirred for 1 hour while maintaining the temperature. After filtering the slurry, it was washed twice with 600ml of water at 60℃ and dried in a dryer at 85℃ for 12 hours to obtain 130g of organically modified clay. This organically modified clay was pulverized in a jet mill to a median diameter of 15μm.

[0062] (2) Preparation of catalyst suspension for production After replacing the air in a 300 ml flask equipped with a thermometer and a reflux condenser with nitrogen, 25.0 g of the organically modified clay obtained in (1) and 108 ml of hexane were added, followed by the addition of 0.392 g (1 mmol) of bis(indenyl)zirconium dichloride and 142 ml of a 20 wt% hexane solution of triisobutylaluminum, and stirring for 3 hours at 60°C. After cooling to room temperature, the supernatant was removed and washed twice with 220 ml of hexane, followed by the addition of 220 ml of hexane to obtain a suspension of a catalyst for production (solid weight content: 12.0 wt%).

[0063] Manufacturing Example 1 As described below, a bimodal polyethylene ethylene-based resin (III-1) was produced by two-stage polymerization in which the polymerization of component (III-1) was successively carried out after the polymerization of component (III-1). The ethylene-based resin (III-1) had an HLMFR of 2.3 g / 10 min and an [η] of 6.5 dl / g.

[0064] Manufacturing of component (A-1) 6 liters of hexane, 5.5 ml of a hexane solution of 20 wt% triisobutylaluminum, and 2.50 g (equivalent to 310 mg of solid content) of the suspension of the production catalyst obtained in Preparation Example 1 were added to a 10-liter autoclave, and the temperature was raised to 60°C. Ethylene was continuously fed so that the ethylene partial pressure could be maintained at 0.80 MPa, and slurry polymerization was carried out for 1 hour. 100 g of ethylene was consumed during the polymerization in terms of polyethylene, and the [η] of component (A-1) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 22 dl / g.

[0065] Manufacture of component (B-1) and ethylene resin (C-1) After polymerizing component (a-1), ethylene was continuously fed so that the ethylene partial pressure was maintained at 0.50MPa at 60°C, and hydrogen was intermittently added so that the hydrogen concentration in the gas phase of the autoclave was 4500ppm, and slurry polymerization was carried out for 9 hours to polymerize component (b-1), thereby producing ethylene-based resin (c-1), which is an ethylene homopolymer. During the polymerization, 900g of ethylene was consumed in terms of polyethylene, and the [η] of component (b-1) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 2.0dl / g.

[0066] Manufacturing Example 2 As described below, a bimodal polyethylene ethylene-based resin (III-2) was produced by two-stage polymerization in which the polymerization of component (III-2) was successively carried out after the polymerization of component (III-2). The ethylene-based resin (III-2) had an HLMFR of 0.08 g / 10 min and an [η] of 7.5 dl / g.

[0067] Manufacturing of component (A-2) In a 10-liter autoclave, 6 liters of hexane, 5.5 ml of a hexane solution of 20 wt% triisobutylaluminum, and 2.50 g (equivalent to 310 mg of solid content) of the suspension of the production catalyst obtained in Preparation Example 1 were added, and the temperature was raised to 60°C. Ethylene was continuously fed so that the ethylene partial pressure could be maintained at 0.80 MPa, and slurry polymerization was carried out for 2 hours. During the polymerization, 200 g of ethylene was consumed in terms of polyethylene, and the [η] of component (A-2) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 22 dl / g.

[0068] Manufacture of component (B-2) and ethylene resin (B-2) After polymerizing component (a-2), ethylene was continuously fed so that the ethylene partial pressure was maintained at 0.50MPa at 60°C, and hydrogen was intermittently added so that the hydrogen concentration in the gas phase of the autoclave was 4500ppm, and slurry polymerization was carried out for 8 hours to polymerize component (b-2), thereby producing ethylene-based resin (c-2), which is an ethylene homopolymer. During the polymerization, 800g of ethylene was consumed in terms of polyethylene, and the [η] of component (b-2) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 2.0dl / g.

[0069] Production Example 3 As described below, an ethylene resin (III-3), which is a bimodal polyethylene, was produced by two-stage polymerization in which the polymerization of component (III-3) was successively carried out after the polymerization of component (III-3). The ethylene polymer (III-3) had an HLMFR of 3.1 g / 10 min and an [η] of 4.1 dl / g.

[0070] Manufacturing of component (A-3) 6 liters of hexane, 5.5 ml of a hexane solution of 20 wt% triisobutylaluminum, and 2.50 g (equivalent to 310 mg of solid content) of the suspension of the production catalyst obtained in Preparation Example 2 were added to a 10-liter autoclave, and the temperature was raised to 70°C. Ethylene was continuously fed so that the ethylene partial pressure could be maintained at 0.80 MPa, and slurry polymerization was carried out for 1 hour. During the polymerization, 200 g of ethylene was consumed in terms of polyethylene, and the [η] of component (A-3) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 10 dl / g.

[0071] Manufacture of component (B-3) and ethylene resin (B-3) After polymerizing component (a-3), ethylene was continuously fed so that the ethylene partial pressure was maintained at 0.87MPa at 60°C, and hydrogen was intermittently added so that the hydrogen concentration in the gas phase of the autoclave was 4500ppm, and slurry polymerization was carried out for 4 hours to polymerize component (b-3), thereby producing ethylene-based resin (c-3), which is an ethylene homopolymer. During the polymerization, 800g of ethylene was consumed in terms of polyethylene, and the [η] of component (b-3) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 2.0dl / g.

[0072] Production Example 4 As described below, a bimodal polyethylene ethylene resin (III-4) was produced by two-stage polymerization in which the polymerization of component (III-4) was successively carried out after the polymerization of component (III-4). The ethylene resin (III-4) had an HLMFR of 7.2 g / 10 min and an [η] of 3.2 dl / g.

[0073] Manufacturing of component (A-4) In a 10-liter autoclave, 6 liters of hexane, 5.5 ml of a hexane solution of 20 wt% triisobutylaluminum, and 2.50 g (equivalent to 310 mg of solid content) of the suspension of the production catalyst obtained in Preparation Example 2 were added, and the temperature was raised to 70°C. Ethylene was continuously fed so that the ethylene partial pressure could be maintained at 0.80 MPa, and slurry polymerization was carried out for 0.5 hours. 100 g of ethylene was consumed during the polymerization in terms of polyethylene, and the [η] of component (A-4) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 10 dl / g.

[0074] Manufacture of component (B-4) and ethylene resin (B-4) After polymerization of component (a-4), ethylene was continuously fed so that the ethylene partial pressure was maintained at 0.87MPa at 60°C, and hydrogen was intermittently added so that the hydrogen concentration in the gas phase of the autoclave was 4500ppm, and slurry polymerization was carried out for 4.5 hours to polymerize component (b-4), thereby producing ethylene-based resin (c-4), which is an ethylene homopolymer. During the polymerization, 900g of ethylene was consumed in terms of polyethylene, and the [η] of component (b-4) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 2.0dl / g.

[0075] Production Example 5 As described below, a bimodal polyethylene ethylene resin (III-5) was produced by two-stage polymerization in which the polymerization of component (III-5) was successively carried out after the polymerization of component (III-5). The ethylene resin (III-5) had an HLMFR of 0.23 g / 10 min and an [η] of 6.6 dl / g.

[0076] Manufacturing of component (A-5) In a 10-liter autoclave, 6 liters of hexane, 5.5 ml of a hexane solution of 20 wt% triisobutylaluminum, and 2.50 g (equivalent to 310 mg of solid content) of the suspension of the production catalyst obtained in Preparation Example 2 were added, and the temperature was raised to 70°C. Ethylene was continuously fed so that the ethylene partial pressure could be maintained at 0.80 MPa, and slurry polymerization was carried out for 2.5 hours. During the polymerization, 500 g of ethylene was consumed in terms of polyethylene, and the [η] of component (A-5) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 10 dl / g.

[0077] Manufacture of components (Ro-5) and ethylene-based resins (Ha-5) After polymerization of component (a-5), ethylene was continuously fed so that the ethylene partial pressure was maintained at 0.87MPa at 60°C, and hydrogen was intermittently added so that the hydrogen concentration in the gas phase of the autoclave was 4500ppm, and slurry polymerization was carried out for 2.5 hours to polymerize component (b-5), thereby producing ethylene-based resin (c-5), which is an ethylene homopolymer. During the polymerization, 500g of ethylene was consumed in terms of polyethylene, and the [η] of component (b-5) calculated from the relationship with the hydrogen concentration in the system during the polymerization reaction was 2.0dl / g.

[0078] Production Example 6 In a 10-liter autoclave, 6 liters of hexane, 5.5 ml of a hexane solution of 20 wt% triisobutylaluminum, and 2.50 g (corresponding to 310 mg of solid content) of the suspension of the catalyst for production obtained in Preparation Example 3 were added, and the temperature was raised to 85°C. Ethylene was continuously fed so that the ethylene partial pressure could be maintained at 0.90 MPa, and hydrogen was intermittently added so that the hydrogen concentration in the gas phase of the autoclave was 100 ppm, and slurry polymerization was carried out for 1.5 hours to produce polyethylene, an ethylene homopolymer. The polyethylene had MFR=0.68 g / 10 min, HLMFR=10 g / 10 min, and [η]=2.4 dl / g.

[0079] [Table 1]

[0080] Example 1 500 g of the ethylene-based resin (H-1) obtained in Production Example 1, polyethylene (manufactured by Tosoh Corporation, (product name) Nipolon Hard 5110 (MFR = 0.9 g / 10 min, density = 961 kg / m 3 500g of NH5110 (hereinafter sometimes referred to as NH5110) and 2g of an antioxidant (BASF, (trade name) Irganox B225) were dry-blended, and then melt-kneaded at 220°C, 30 rpm, and a discharge rate of 0.8 kg / h using a twin-screw extruder (Toyo Seiki Seisakusho, (trade name) Labo Plastomill Parallel Twin-screw Extruder 2D25S) to obtain composition (E-1). The MFR of composition (E-1) was 0.11 g / 10 min.

[0081] 15 g of the obtained composition (E-1) was press molded for 5 minutes at 180° C. and 10 MPa using a high-temperature 50 ton automatic press (manufactured by Shinto Metal Industries Co., Ltd.), and then cooled for 5 minutes at 25° C. and 10 MPa. The obtained pressed sheet was cut into a length of 6 cm and a width of 1 cm to prepare a raw sheet for stretching.

[0082] The prepared raw fabric was stretched 9 times at a stretching speed of 100 mm / min in a thermostatic chamber at a temperature of 90°C using an automatic tensile tester with a thermostatic chamber (manufactured by Toyo Seiki Seisakusho, product name VG-1G), and after stretching, it was air-cooled to obtain a stretched product (H-1).

[0083] The stretched product (F-1) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 6.6 GPa and 406 MPa, respectively.

[0084] Example 2 A stretched product (F-2) was obtained in the same manner as in Example 1, except that the stretching was performed 10 times in a thermostatic bath at a temperature of 120° C. and at a stretching speed of 100 mm / min.

[0085] The stretched product (F-2) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 7.2 GPa and 428 MPa, respectively.

[0086] Example 3 A stretched product (F-3) was obtained in the same manner as in Example 1, except that the film was stretched 11 times in a thermostatic bath at a temperature of 130° C. and at a stretching speed of 100 mm / min.

[0087] The stretched product (F-3) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 7.3 GPa and 346 MPa, respectively.

[0088] Example 4 A stretched product (F-4) was obtained in the same manner as in Example 1, except that the film was stretched 6 times at a stretching speed of 100 mm / min in a thermostatic bath at a temperature of 120°C.

[0089] The stretched product (F-4) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 4.4 GPa and 297 MPa, respectively.

[0090] Example 5 A stretched product (F-5) was obtained in the same manner as in Example 1, except that 500 g of the ethylene-based resin (F-2) obtained in Production Example 2 was stretched 11 times at a stretching speed of 100 mm / min in a constant temperature bath at a temperature of 120°C.

[0091] The stretched product (F-5) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 8.2 GPa and 434 MPa, respectively.

[0092] Example 6 A stretched product (F-6) was obtained in the same manner as in Example 1, except that 100 g of the ethylene resin (F-2) obtained in Production Example 2 and 900 g of polyethylene (NH5110) were stretched 9 times at a stretching speed of 100 mm / min in a thermostatic bath at a temperature of 120°C.

[0093] The stretched product (F-6) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 5.3 GPa and 323 MPa, respectively.

[0094] [Table 2]

[0095] Example 7 A stretched product (F-7) was obtained in the same manner as in Example 1, except that 500 g of the ethylene-based resin (F-3) obtained in Production Example 3 was stretched 9 times at a stretching speed of 100 mm / min in a constant temperature bath at a temperature of 120°C.

[0096] The stretched product (F-7) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 6.0 GPa and 369 MPa, respectively.

[0097] Example 8 A stretched product (F-8) was obtained in the same manner as in Example 1, except that 40 g of the ethylene-based resin (F-4) obtained in Production Example 4 and 960 g of polyethylene (NH5110) were stretched 5 times at a stretching speed of 100 mm / min in a thermostatic bath at a temperature of 120°C.

[0098] The stretched product (F-8) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 4.1 GPa and 314 MPa, respectively.

[0099] Example 9 500 g of the ethylene-based resin (H-2) obtained in Production Example 2, polyethylene (manufactured by Tosoh Corporation, (product name) Nipolon Hard 06S81A (MFR = 1.0 g / 10 min, density = 952 kg / m 3 A stretched product (H-9) was obtained in the same manner as in Example 1, except that 500 g of NH06S81A (hereinafter sometimes referred to as NH06S81A) was stretched 11 times in a thermostatic bath at a temperature of 125° C. and a stretching speed of 100 mm / min.

[0100] The stretched product (F-9) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 4.4 GPa and 329 MPa, respectively.

[0101] Example 10 A stretched product (F-10) was obtained in the same manner as in Example 1, except that 500 g of the ethylene-based resin (F-5) obtained in Production Example 5 and 500 g of the polyethylene obtained in Production Example 6 were stretched 11 times at a stretching speed of 100 mm / min in a constant temperature bath at a temperature of 125°C.

[0102] The stretched product (F-10) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 4.5 GPa and 363 MPa, respectively.

[0103] [Table 3]

[0104] Comparative Example 1 A stretched product (H-11) was obtained in the same manner as in Example 1, except that 1000 g of polyethylene (NH5110) and 2 g of an antioxidant (manufactured by BASF, (product name) Irganox B225) were stretched 4 times at a stretching speed of 100 mm / min in a thermostatic bath at a temperature of 120°C.

[0105] The stretched product (F-11) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 4.7 GPa and 284 MPa, respectively.

[0106] Comparative Example 2 Using 40 g of ultra-high molecular weight polyethylene (Mitsui Chemicals, Inc., product name Million 030S) and 960 g of polyethylene (NH5110), an attempt was made to stretch the material 3 times at a stretching rate of 100 mm / min in a thermostatic bath at a temperature of 120°C, but the material broke at a stretching ratio of about 2 times, and no stretched product was obtained.

[0107] Comparative Example 3 A stretched product (H-12) was obtained in the same manner as in Example 1, except that 1000 g of polyethylene (NH06S81A) and 2 g of an antioxidant (manufactured by BASF, (product name) Irganox B225) were stretched 3 times at a stretching speed of 100 mm / min in a thermostatic bath at a temperature of 125°C.

[0108] The stretched product (F-12) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 2.6 GPa and 239 MPa, respectively.

[0109] Comparative Example 4 A stretched product (H-13) was obtained in the same manner as in Example 1, except that 1000 g of the polyethylene obtained in Production Example 6 and 2 g of an antioxidant (manufactured by BASF, (product name) Irganox B225) were stretched 4 times in a thermostatic bath at a temperature of 125°C and a stretching speed of 100 mm / min.

[0110] The stretched product (F-13) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 3.2 GPa and 288 MPa, respectively.

[0111] Comparative Example 5 Polyethylene (manufactured by Tosoh Corporation, product name Nipolon Hard 8D01A (MFR = 0.05 g / 10 min, density = 957 kg / m 3 A stretched product (H-14) was obtained in the same manner as in Example 1, except that 1000 g of NH8D01A (hereinafter sometimes referred to as NH8D01A) and 2 g of an antioxidant (manufactured by BASF, (product name) Irganox B225) were used and stretched to 11 times at a stretching speed of 100 mm / min in a thermostatic bath at a temperature of 120°C.

[0112] The stretched product (F-14) thus obtained was subjected to a tensile test, and as a result, the 1% tensile modulus and the tensile breaking stress were 5.4 GPa and 286 MPa, respectively.

[0113] Comparative Example 6 500 g of the ethylene resin (H-1) obtained in Production Example 1 and polyethylene (manufactured by Tosoh Corporation, (product name) Nipolon Hard 2000 (MFR = 15 g / 10 min, density = 960 kg / m 3 ), hereinafter sometimes referred to as NH2000), was weighed and an attempt was made to stretch it 3 times at a stretching rate of 100 mm / min in a thermostatic bath at 120°C. However, it broke at a stretching ratio of about 2 times, and no stretched product was obtained.

[0114] Comparative Example 7 500 g of the ethylene resin (H-1) obtained in Production Example 1 and polyethylene (manufactured by Tosoh Corporation, (trade name) Petrothene 176 (MFR = 1.0 g / 10 min, density = 924 kg / m 3 ), hereinafter sometimes referred to as P2000), was weighed at 500 g and an attempt was made to stretch it 3 times at a stretching rate of 100 mm / min in a thermostatic bath at 120° C., but it broke at a stretching ratio of about 2 times, and no stretched product was obtained.

[0115] [Table 4] [Industrial Applicability]

[0116] The stretched product of the present invention can improve the stretch processability and the mechanical strength of the molded article, and is expected to enable the molded article to be made thinner and have a longer life.

Claims

1. (1) An ethylene-based resin having a melt flow rate (HLMFR) of 0.01 to 100 g / 10 min at a temperature of 190° C. and a load of 21.6 kg in accordance with JIS 6922-2:1997 and a bimodal elution curve measured by gel permeation chromatography; and a melt flow rate (MFR) of 0.01 to 10 g / 10 min at a temperature of 190° C. and a load of 2.16 kg in accordance with JIS 6922-2:1997 and a density of 930 to 980 kg / m as measured according to JIS K6922-1 (1997). 3 A stretched product comprising a polyethylene composition comprising a polyethylene of formula (I).

2. 2. The stretched product according to claim 1, wherein the ethylene-based resin satisfies the following characteristic (2): (2) The elution curve measured by gel permeation chromatography has two peaks, and when the elution curve is expressed as a differential molecular weight distribution (x-axis: Log [M], y-axis: differential distribution value) and the peak is divided into two normal distributions according to the following formula (i), the following (2-1) to (2-3) are satisfied: f(x)=a×(1 / (2π(σ 2 )) (1/2) ) exp(-((x-μ) 2 ) / (2(σ 2 ))) Formula (i) (Here, a is the peak intensity, σ is the standard deviation, x is the variable, and μ is the average.) (2-1): The weight average molecular weight, calculated as linear polyethylene, based on the peak on the high molecular weight side is 900,000 to 5,000,000, and the molecular weight distribution, expressed as weight average molecular weight / number average molecular weight, is 2.0 to 5.

0. (2-2): The weight average molecular weight, calculated based on the peak on the low molecular weight side, is 10,000 to 500,000 in terms of linear polyethylene, and the molecular weight distribution is 2.0 to 5.

0. (2-3): The weight ratio of the high molecular weight peak to the weight ratio of the low molecular weight peak is greater than 5 / 95 and smaller than 80 / 20.

3. 3. The stretched product according to claim 1, wherein the ethylene-based resin also satisfies the following characteristic (3): (3) The molecular weight distribution, calculated as standard polyethylene, measured by gel permeation chromatography is 4.0 or more and less than 50.

4. 3. The stretched product according to claim 1, wherein the ethylene-based resin also satisfies the following characteristic (4): (4): The crystal melting peak (Tm) in the first scan measured using a differential scanning calorimeter by heating from 0° C. to 230° C. at a heating rate of 10° C. / min (1st scan) is single-peaked.

5. 3. The stretched product according to claim 1, which is a stretched sheet having a 1% tensile modulus of elasticity measured at 23° C. of 4.0 GPa or more and a tensile breaking strength of 300 MPa or more.

6. 3. The stretched product according to claim 1, wherein the ethylene-based resin is an ethylene homopolymer.

Citation Information

Patent Citations

  • JP1973068853A

  • Thermal transfer type sheet

    JP1989005888A

  • Modifier for polyethylene resin, manufacturing method of polyethylene resin composition using the same and manufacturing method of molded body

    JP2017179304A

  • Ultra high molecular weight polyethylene

    JP2021172716A

  • polyethylene resin composition

    JP4173444B2